Method for manufacturing photonic crystal gallium nitride light-emitting element, and lighting device

The method of epitaxial growth and reactive ion etching on a sapphire substrate efficiently forms photonic crystals on GaN layers, addressing the challenge of narrowing light directivity and enhancing luminous efficiency in gallium nitride light emitting devices without lenses or costly mold changes.

WO2024237194A1PCT designated stage expired Publication Date: 2024-11-21NITRIDE SEMICON +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017392
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-10
Filing Date
2024-05-10
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Current methods for forming photonic crystals on gallium nitride (GaN) layers in light emitting devices are inefficient, making it difficult to narrow the directivity angle of emitted light without using expensive lenses and requiring costly mold changes for adjustments.

Method used

A method involving epitaxial growth of n-type and p-type gallium nitride layers on a sapphire substrate, followed by electron beam lithography and inductively coupled plasma reactive ion etching to form a photonic crystal structure on the GaN layer, allowing for efficient formation of holes at desired intervals and diameters, thereby creating a photonic crystal gallium nitride light emitting device.

Benefits of technology

This approach enables reliable formation of photonic crystals on GaN layers, narrowing the directivity angle of emitted light and significantly increasing luminous efficiency without the need for lenses or costly mold changes, while allowing for flexible specification adjustments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017392_21112024_PF_FP_ABST
    Figure JP2024017392_21112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a method for obtaining a photonic crystal GaN light-emitting element by efficiently forming a photonic crystal on a GaN layer that constitutes a light-emitting element. This method comprises: a step in which an n-type GaN layer (12), an MQW layer (14), and a p-type GaN layer (16) are epitaxially grown in sequence on a sapphire substrate (10) to form an epitaxial structure; a step in which a p-type electrode, a metal substrate, and a support substrate are formed on the p-type GaN layer (16); a step in which the top and bottom of the epitaxial structure are inverted; a step in which the sapphire substrate (10) is peeled to expose the n-type GaN layer (12) at a surface; a step in which a photonic crystal is formed on the surface of the n-type GaN layer (12) exposed at the surface by electron beam drawing and inductively coupled plasma reactive ion etching; and a step in which an n-electrode (24) is formed.
Need to check novelty before this filing date? Find Prior Art

Description

Photonic crystal gallium nitride light emitting device manufacturing method and lighting device

[0001] The present invention relates to a method for manufacturing a photonic crystal gallium nitride light emitting device.

[0002] In order to narrow the beam angle of light emitted from a light-emitting diode (LED) chip using gallium nitride (GaN), it has been considered to mount a lens on the LED device to collect the light and narrow the beam angle.

[0003] However, with lenses, even a slight change in directionality requires changing the mold, which increases costs.In addition, for ultraviolet and deep ultraviolet light, quartz lenses are used to take into account lens absorption, which makes the lenses expensive.

[0004] Therefore, as a method of concentrating light and narrowing the directivity without mounting a lens on an LED device, a method of forming photonic crystals with holes on the order of several hundred nanometers at a pitch of several hundred nanometers on the surface of an LED chip is being considered.

[0005] Patent Document 1 describes an invention relating to a gallium nitride photonic crystal and a manufacturing method thereof. Specifically, the invention aims to provide a nitride semiconductor with reduced dislocation density over a wide region and good crystallinity during epitaxial growth, and to provide high-performance gallium nitride semiconductor devices, gallium nitride semiconductor substrates, and gallium nitride photonic crystals with high yields, and describes a method for manufacturing the same, comprising the steps of forming a gallium nitride semiconductor layer on a substrate, forming an array of trenches in the gallium nitride semiconductor layer, and performing a heat treatment in a nitrogen-containing atmosphere to deform at least two or more adjacent trenches among the plurality of trenches, thereby forming continuous cavities within the gallium nitride semiconductor layer corresponding to the positions of the deformed trenches, and forming a gallium nitride semiconductor device on the gallium nitride semiconductor layer having the cavities.

[0006] Furthermore, Patent Document 2 describes a photonic crystal light-emitting diode having an object of providing a photonic crystal light-emitting diode that is resistant to deterioration over a long period of time and has high energy efficiency and light-emitting efficiency, in which three layers, namely a first semiconductor layer, an active layer, and a second semiconductor layer, are stacked in this order, with a first electrode electrically connected to the first semiconductor layer and a second electrode electrically connected to the second semiconductor layer, in which voids penetrating at least the first semiconductor layer and the active layer out of the three layers are arranged two-dimensionally periodically to form a photonic crystal structure, and the first electrode covers the first semiconductor layer except for the voids and a first non-current injection region surrounding the voids.

[0007] JP 2004-111766 A JP 2011-54828 A

[0008] However, when a light emitting element such as an LED is made of gallium nitride (GaN), a technique for forming a photonic crystal in a GaN layer has not yet been established.

[0009] An object of the present invention is to provide a method for obtaining a photonic crystal GaN light-emitting device by efficiently forming a photonic crystal in a GaN layer that constitutes a light-emitting device, and a lighting device.

[0010] the n-type gallium nitride layer is exposed to the surface by etching the n-type gallium nitride layer exposed to the surface, and a thickness of the n-type gallium nitride layer is adjusted. The present invention provides a method for manufacturing a photonic crystal gallium nitride light-emitting device, the method comprising the steps of: epitaxially growing an n-type gallium nitride layer, a multiple quantum well layer, and a p-type gallium nitride layer, successively, on a sapphire substrate to form an epitaxial structure; forming a p-type electrode on the p-type gallium nitride layer; forming a metal substrate and a support substrate on the p-type electrode; inverting the epitaxial structure so that the support substrate is on the bottom and the sapphire substrate is on the top; peeling off the sapphire substrate located at the top by the inversion step to expose the n-type gallium nitride layer to the surface;

[0011] In one embodiment of the present invention, the step of forming the photonic crystal comprises the steps of: performing a hydrophobic treatment on the surface of the n-type gallium nitride layer; applying a resist to the surface of the n-type gallium nitride layer; irradiating the resist with an electron beam to pattern it; and removing the resist with chlorine gas by inductively coupled plasma reactive ion etching.

[0012] Another embodiment of the present invention includes the step of growing a buffer layer and an undoped gallium nitride layer in that order on the sapphire substrate before growing the n-type gallium nitride layer on the sapphire substrate.

[0013] In yet another embodiment of the present invention, the photonic crystal gallium nitride light emitting device has an emission wavelength of 380 nm to 390 nm.

[0014] The present invention also provides an illumination device comprising a photonic crystal gallium nitride light-emitting element manufactured by the above manufacturing method, and an illumination optical system that irradiates an object with light from the photonic crystal gallium nitride light-emitting element.

[0015] According to the present invention, it is possible to reliably form photonic crystals in the GaN layer that constitutes a gallium nitride (GaN) light-emitting device. This makes it possible to narrow the directivity of light emitted from the light-emitting device. It is also possible to increase the luminous efficiency of the gallium nitride light-emitting device.

[0016] FIG. 1 is a schematic cross-sectional view (1) showing a manufacturing method of an embodiment; FIG. 2 is a schematic cross-sectional view (3) showing a manufacturing method of an embodiment; FIG. 4 is a schematic cross-sectional view (4) showing a manufacturing method of an embodiment; FIG. 5 is a schematic cross-sectional view (5) showing a manufacturing method of an embodiment; FIG. 6 is a schematic cross-sectional view (6) showing a manufacturing method of an embodiment; FIG. 7 is a schematic cross-sectional view (7) showing a manufacturing method of an embodiment; FIG. 8 is a schematic cross-sectional view (8) showing a manufacturing method of an embodiment; FIG. 9 is a schematic cross-sectional view (90) showing a manufacturing method of an embodiment; FIG. 10 is a schematic cross-sectional view (100) showing a manufacturing method of an embodiment. FIG. 1 is a diagram showing the configuration of an illumination device and an exposure device of an embodiment; FIG. 2 is a diagram showing the configuration of a light source unit; FIG. 2 is an SEM image after electron beam writing of an embodiment; FIG. 3 is an SEM image after etching by inductively coupled plasma reactive ion etching of an embodiment, where (a) is an SEM image of the inner diameter of the hole and (b) is an SEM image of the outer diameter of the hole; FIG. 3 is a cross-sectional SEM image of a hole of an embodiment; FIG. 4 is a perspective view of a GaN wafer of an embodiment. 8 is an enlarged view of a portion of FIG. 7. It is a diagram showing the probe measurement results of a reference chip. It is a diagram showing the probe measurement results of an LED chip (PhC-formed chip) of an embodiment. It is a diagram showing the integrating sphere measurement results of the reference and the PhC-formed chip. It is an emission spectrum diagram of the reference and the PhC-formed chip. It is an IV characteristic diagram of the reference and the PhC-formed chip. It is an IL characteristic diagram of the reference and the PhC-formed chip. It is a diagram showing the directional characteristic measurement results of the reference. It is a diagram showing the directional characteristic measurement results of the PhC-formed chip.

[0017] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.

[0018] The basic principle of this embodiment is that, when forming a photonic crystal in a GaN layer that constitutes a GaN light-emitting device, the etching rate of the GaN layer that has been subjected to electron beam (EB) lithography and inductively coupled plasma reactive ion etching varies greatly depending on the structure and crystallinity of the substrate and the GaN layer. In consideration of this, the GaN layer is grown on a sapphire substrate rather than growing the GaN layer on a Si substrate or the like, and photonic crystals are formed on the GaN layer thus grown by electron beam (EB) lithography and inductively coupled plasma reactive ion etching.

[0019] The present inventors have found that, compared to a GaN layer grown on a Si substrate, a GaN layer grown on a sapphire substrate has a significantly higher etching rate by electron beam (EB) lithography and inductively coupled plasma reactive ion etching, and that holes can be formed at desired intervals and with desired diameters on the surface of the GaN layer extremely efficiently, thereby forming a photonic crystal.

[0020] 1A to 1J are cross-sectional views schematically showing a method for manufacturing a photonic crystal GaN light-emitting device (LED) according to this embodiment.

[0021] As shown in FIG. 1A, a low-temperature buffer layer (not shown) and an undoped GaN (u-GaN) layer (not shown) are deposited on a sapphire substrate 10 using a metalorganic chemical vapor deposition (MOCVD) apparatus, and an n-GaN layer (n-type GaN layer) 12, a multiple quantum well (MQW) layer 14, and a p-GaN layer (p-type GaN layer) 16 are sequentially deposited thereon to grow an epitaxial structure that emits light at 385 nm (380 to 390 nm).

[0022] More specifically, the n-GaN layer 12 is composed of an (AlInGaN) / (InGaN;Si) n-SLS (superlattice structure) layer and a (GaN;Si) contact layer, where (GaN;Si) indicates Si-doped GaN.

[0023] The multiple quantum well (MQW) layer 14 is composed of an MQW layer of (InGaN / AlGaN).

[0024] More specifically, the p-GaN layer 16 is composed of a p-GaN (GaN; Mg) contact layer and an (AlGaN; Mg / GaN; Mg) p-SLS (super lattice structure) layer.

[0025] In this embodiment, the term "GaN layer" does not necessarily mean a single layer having a GaN composition, but means a single layer or multiple layers having a composition containing GaN, such as AlInGaN, InGaN, or AlGaN. In short, it means a single layer or multiple layers containing GaN as the main component.

[0026] The emission wavelength of the epitaxial layer in this embodiment is 385 nm. When a wavelength longer than this is used, although the basic epitaxial structure is the same, the Al content of the (InGaN / AlInGaN) MQW light-emitting layer 14 is made larger and the In content is made smaller for 385 nm than for wavelengths longer than this, due to the relationship of band gap energy.

[0027] Next, as shown in Fig. 1B, a p-electrode (p-type electrode: ITO or the like) and a metal reflective film (Ag or the like) are vapor-deposited on the epitaxial structure layer that emits light at 385 nm. In Fig. 1B, the p-electrode and the metal reflective film are collectively shown as p-electrode and reflective film 18.

[0028] Next, as shown in FIG. 1C, a metal substrate (CuW, CuMo, etc.) 20 is bonded onto the p-electrode and the metal reflective film 18 .

[0029] 1D, a support substrate (sapphire, Si substrate, etc.) 22 is bonded onto the metal substrate 20. The layered structure shown in FIG. 1D is, from the bottom up, sapphire substrate 10 / n-GaN layer 12 / MQW layer 14 / p-GaN layer 16 / p-electrode and reflective film 18 / metal substrate 20 / support substrate 22.

[0030] 1E, the epitaxial structure of FIG. 1D is flipped 180° upside down, with the sapphire substrate 10 positioned at the top, and the sapphire substrate 10 is peeled off (lifted off) with a laser to expose the n-GaN layer 12. That is, the layered structure obtained by flipping the epitaxial structure of FIG. 1D 180° upside down is, in order from the bottom, a support substrate 22 / metal substrate 20 / p-electrode and reflective film 18 / p-GaN layer 16 / MQW layer 14 / n-GaN layer 12 / sapphire substrate 10, and the topmost sapphire substrate 10 (and buffer layer) is peeled off (lifted off) to expose the n-GaN layer 12 on the top surface.

[0031] Next, as shown in Fig. 1F, the n-GaN layer 12 on the surface is etched. Specifically, the total thickness of the epitaxial structure is adjusted by dry etching to 1050 µm. Note that the total thickness of the epitaxial structure is not limited to this and can be optimized depending on the emission wavelength.

[0032] 1G, a photonic crystal (PhC) is formed on the surface of the n-GaN layer 12 whose thickness has been adjusted by dry etching, as will be described in more detail later.

[0033] Next, as shown in FIG. 1H, trenches are formed from the surface of the n-GaN layer 12 down to the metal substrate 20 to separate the epitaxial structure.

[0034] Next, as shown in FIG. 1I, n-electrodes (n-type electrodes) 24 are formed on the n-GaN layer 12 in each of the separated regions.

[0035] Finally, as shown in FIG. 1J, the support substrate 22 is peeled off and diced to manufacture LED chips (V-chip structure LED chips: vertical LED chips in which electrodes are arranged in a vertical structure).

[0036] The method for manufacturing the photonic crystal shown in FIG. 1G will now be described in more detail.

[0037] Photonic crystals (PhCs) are formed by developing a pattern in a resist by electron beam (EB) lithography and then etching by inductively coupled plasma reactive ion etching. Therefore, prior to forming the photonic crystal, it is necessary to set the EB lithography conditions and the etching conditions for inductively coupled plasma reactive ion etching.

[0038] <Etching Conditions> The etching rate may vary depending on the type of substrate to be laminated on the Si substrate, sapphire substrate, etc., and on the structure and crystallinity of GaN.

[0039] Therefore, a GaN wafer with an emission wavelength of 385 nm grown on a sapphire substrate was rinsed and then dried for 2 minutes at 120° C. After that, a treatment (HMDS treatment) was performed to make the GaN wafer surface hydrophobic, and a UV resist was applied to a thickness of 950 nm using a spin coater, followed by pre-baking at 90° C. for 90 seconds.

[0040] Next, a 100um x 100um pattern was printed using a high-speed maskless exposure device at 150mJ / cm 2 The resist was formed by the above process, post-baked at 110° C. for 90 seconds, and developed.

[0041] A GaN wafer coated with UV resist was etched for 10 minutes using an inductively coupled plasma reactive ion etching system with chlorine gas (30 sccm). The etching depth was measured using a UV stylus profilometer, resulting in a depth of 789.05 nm. The etching rate was 78.9 nm / min.

[0042] On the other hand, when the etching rate was confirmed by the same method using a GaN wafer with an emission wavelength of 385 nm grown on a Si substrate, the etching rate was found to be 16 nm / min. That is, GaN layer grown on sapphire substrate: etching rate = 78.9 nm / min GaN layer grown on Si substrate: etching rate = 16 nm / min It was confirmed that, although it is relatively difficult to form photonic crystals in a GaN layer using a Si substrate, a GaN layer grown on a sapphire substrate, that is, as in this embodiment, first grows a GaN layer on the sapphire substrate 10, then turns it upside down to remove the sapphire substrate 10, and then etches the GaN layer on the metal substrate 20 by inductively coupled plasma reactive ion etching, it is possible to efficiently form photonic crystals in the GaN layer at a significantly high etching rate.

[0043] Next, an illumination device including a GaN light emitting device manufactured by the manufacturing method shown in the above embodiment and an exposure device including the illumination device will be described with reference to FIGS.

[0044] Fig. 2 is a diagram showing the configuration of an exposure apparatus equipped with an illumination device IU using a GaN light-emitting element manufactured by the manufacturing method according to the embodiment described above as a light source. Fig. 3A is a plan view showing the configuration of a light source unit 120 that supplies exposure light to the illumination device IU, and Fig. 3B is a diagram showing the internal configuration of the light source unit 120 and the output optical system 130.

[0045] In FIG. 2, the illumination device IU includes a first focusing optical system 140 that focuses the exposure light from the light source unit 120 via the output optical system 130, a fly-eye lens FEL onto which the exposure light from the first focusing optical system 140 is incident, and a second focusing optical system 160 that focuses the exposure light from the fly-eye lens FEL and illuminates a reticle REI as an illuminated surface.

[0046] The exposure apparatus also includes an illumination unit IU and a projection optical system PO that forms an image of a pattern on a reticle illuminated by the illumination unit IU onto a wafer as an exposed substrate.

[0047] Next, the light source unit 120 and the output optical system 130 will be described with reference to FIG.

[0048] In FIG. 3A, the light source unit 120 includes a plurality of LED (Light Emitting Diode) chips 123 (5 × 5 in FIG. 3A) arranged on a substrate 121, for example. These LED chips are GaN light-emitting elements manufactured by the manufacturing method of the above-described embodiment. The number of LED chips 123 may be changed as needed. Each of the plurality of LED chips 123 has a light-emitting portion 231, and the peak wavelength of light emitted from this light-emitting portion 231 is in the range of 380 to 390 nm. In other words, the light-emitting portion 231 is an ultraviolet LED (UVLED). More preferably, the peak wavelength of the light emitted from the light-emitting portion 231 is 385 nm. The light-emitting surface of the light-emitting portion 231 may be square, rectangular, hexagonal, or other polygonal. The LED chips 123 may be arranged on, for example, a heat sink, rather than on a substrate.

[0049] The configuration of the light source unit 120 and the output optical system 130 will be described with reference to Fig. 3(B). In Fig. 3(B), the two directions in which the LED chips 123 are arranged are defined as the X direction and the Y direction. The X direction and the Y direction are orthogonal to each other. The direction orthogonal to the X direction and the Y direction is defined as the Z direction. The Z direction substantially coincides with the traveling direction of the light emitted from the light-emitting unit 231. Note that Fig. 3(B) shows only four LED chips 123 lined up in a row along the Y direction for clarity of the drawing.

[0050] As shown in FIG. 3B , the output optical system 130 includes multiple magnifying optical systems for forming magnified images of the light-emitting portions 231 of the LED chips 123. Each magnifying optical system is arranged to correspond to the arrangement of the LED chips 123, and is a double-telecentric optical system that magnifies and projects the light-emitting portions 231 at a magnification ratio. While FIG. 3B illustrates each magnifying optical system of the output optical system 130 as consisting of two positive lenses, the number of lenses constituting the magnifying optical system is not limited to two. The magnifying optical system may also be configured as a reflective system or a catadioptric system. Instead of or in addition to the magnifying optical system, the output optical system 130 may include a 1x optical system or a reduction optical system.

[0051] 2 and 3 , each magnifying optical system of the output optical system 130 forms a magnified image of the light-emitting unit 231 near the final optical element of the output optical system 130. As a result, a plurality of light source images that are densely arranged are located near the final optical element of the output optical system 130.

[0052] Returning to FIG. 2, each component of the illumination device IU will be described.

[0053] The first focusing optical system 140 is arranged so that its front focal point is located at or near the position of the light source image formed by the light source unit 120 and the output optical system 130, and provides Koehler illumination to the incident surface of the fly's eye lens FEL.

[0054] The fly-eye lens FEL is formed by, for example, arranging a plurality of lens elements having positive refractive power in a dense array vertically and horizontally so that their optical axes are parallel to the reference optical axis AX. Each lens element constituting the fly-eye lens FEL has a rectangular cross section similar to the shape of the illumination field to be formed on the reticle REI (and consequently the shape of the exposure area to be formed on the wafer W).

[0055] Therefore, the light beam incident on the fly-eye lens FEL is wavefront-split by the multiple lens elements, and one light source image is formed on or near the rear focal plane (exit surface) of each lens element. That is, a substantial surface light source, i.e., a secondary light source, consisting of multiple light source images is formed on or near the rear focal plane (exit surface) of the fly-eye lens FEL.

[0056] Here, when focusing on one lens element of the fly-eye lens FEL, a plurality of light source images formed by the light source unit 120 and the output optical system 130 are formed on or near the rear focal plane (exit surface) of this one lens element, and these plurality of light source images are distributed in an area having a similar shape to the area where the plurality of LED chips 123 are arranged. For this reason, the area where the plurality of LED chips 123 are arranged and the cross section of each lens element of the fly-eye lens FEL may have a similar shape to each other.

[0057] The light beam from the secondary light source formed on or near the rear focal plane (exit surface) of the fly-eye lens FEL is incident on the aperture stop 150 arranged nearby. In this embodiment, the rear focal plane (exit surface) of the fly-eye lens FEL and the LED chip array surface of the light source unit 120 are optically conjugate.

[0058] The aperture stop 150 is disposed at a position that is optically nearly conjugate with the entrance pupil plane of the projection optical system PO, and has a variable opening for defining the range that contributes to illumination from the secondary light source. The exposure light from the secondary light source that passes through the aperture stop 150 is subjected to the focusing action of the second focusing optical system 160, and then superimposes and illuminates a reticle REI on which a predetermined pattern is formed.

[0059] The exposure light from the reticle REI illuminated by the illumination device IU (exposure light passing through a pattern located within the illumination field on the reticle REI) is incident on the projection optical system PO, which forms an image of the pattern of the reticle REI on the wafer W as the substrate to be exposed. As a result, the pattern of the reticle REI is exposed onto the exposure area of ​​the wafer W. The projection magnification of the projection optical system PO may be a reduction magnification, an enlargement magnification, or an equal magnification. The projection optical system PO may also be a refractive optical system, a reflective optical system, or a catadioptric optical system.

[0060] A GaN wafer with an emission wavelength of 385 nm was rinsed and then dried for 2 minutes at 120° C. Thereafter, a treatment (HMDS treatment) was performed to make the wafer surface hydrophobic, and EB resist was applied to a thickness of 500 nm using a spin coater, followed by pre-baking at 180° C. for 3 minutes.

[0061] Next, a high-speed, high-precision electron beam lithography system was used to measure the exposure dose (μC / cm 2 The dose (μC / cm) of the nine conditions was changed. 2 ) were 150, 160, 170, 180, 190, 200, 210, 220, and 230, respectively.

[0062] After development, the hole diameter was confirmed using a scanning electron microscope (SEM). As a result, the relationship between the exposure dose (Dose amount) and the hole diameter was: Dose amount: 150 → 293.3 nm Dose amount: 160 → 296.00 nm Dose amount: 170 → 309.33 nm Dose amount: 180 → 314.67 nm Dose amount: 190 → 320.00 nm Dose amount: 200 → 325.33 nm Dose amount: 210 → 330.67 nm Dose amount: 220 → 338.67 nm Dose amount: 230 → 352.00 nm It was confirmed that there is a positive correlation between the exposure dose and the hole diameter.

[0063] From the results of the above EB lithography conditions, a high-speed, high-precision electron beam lithography system was used, and a 140 μC / cm 2 After development, the hole diameter was confirmed by SEM.

[0064] Figure 4 shows an SEM image after development, which confirmed that holes with diameters in the range of 286-292 nm were formed.

[0065] Next, etching was performed using an inductively coupled plasma reactive ion etching apparatus with chlorine gas (30 sccm), and after EB resist removal, the hole diameters were confirmed using an SEM. As a result, it was confirmed that the outer diameter was 262 to 269 nm, the inner diameter was 213 to 220 nm, and the taper angle was sufficiently suppressed to 70 to 80 degrees.

[0066] Figure 5 shows SEM images after etching using an inductively coupled plasma reactive ion etching system. Figure 5(a) is an SEM image of the inner diameter, and Figure 5(b) is an SEM image of the outer diameter. It was confirmed that holes on the order of several hundred nanometers were formed at a pitch of several hundred nanometers on the surface of the GaN wafer, and that a photonic crystal had been formed.

[0067] Figure 6 shows an SEM image of the cross section of a GaN wafer after etching with an inductively coupled plasma reactive ion etching apparatus. The taper angle of the holes that make up the photonic crystal is 70 to 80 degrees. In order to narrow the beam angle of the light emitted from the LED chip, it is desirable that the holes that make up the photonic crystal are not tapered, that is, that the taper angle be 90 degrees. In this embodiment, however, good results were obtained with a taper angle of 70 to 80 degrees.

[0068] Fig. 7 shows a perspective view of the appearance of a GaN wafer on which photonic crystals are formed, and Fig. 8 shows an enlarged view of a portion of the wafer. It was confirmed that the illumination light (fluorescent light in the room and halogen light from the microscope) illuminating the GaN wafer was trapped in the area where the photonic crystals were formed, making the area brighter than other areas.

[0069] 9 and 10 show the results of measuring the electrical characteristics of a reference chip and an LED chip (a chip with PhC formed) of this embodiment using a prober. The reference chips shown in FIG. 9 are LED chips without photonic crystals formed in the GaN layer, and there are a total of 10 LED chips, A1 to A10, located at different positions on the wafer. The LED chips of this embodiment shown in FIG. 10 are LED chips with photonic crystals (PhC) formed in the GaN layer, and there are a total of 11 LED chips, B1 to B11, located at different positions on the wafer. Both the reference chip and the PhC-formed chip have good electrical properties, but when the half-width (WH) and light output (Po) of the reference chip A1 and the PhC chip are compared, for example, the following is obtained: <Reference chip A1> Half-width WH = 16.87 (nm) Light output Po = 166.86 (mW) <PhC-formed chip B1> Half-width WH = 11.55 (nm) Light output Po = 445.70 (mW) The LED chip of this embodiment has a significantly reduced half-width and a significantly increased light output compared to the reference chip, with an average half-width WH reduction of approximately 5.9 nm and an increase in light output Po of approximately 2.68 times.

[0070] Figure 11 shows the results of integrating sphere measurements of the reference chip and the LED chip (PhC-formed chip) of this embodiment. Each chip was mounted on an aluminum substrate and its characteristics were measured using an integrating sphere. Figure 11(A) shows the measurement results at a forward current IF of 500 mA, and Figure 11(B) shows the measurement results at IF of 700 mA.

[0071] When the reference chips (A1 to A3) and the PhC-formed chips (B4 to B6) were compared, the LED chips of this embodiment gave results similar to the measurement results using a prober shown in Figures 9 and 10, compared to the reference chips.

[0072] Figures 12, 13, and 14 show the emission spectra, IV characteristics, and IL characteristics of the reference chips (A1 to A3) and the PhC-formed chips (B4 to B6), respectively. Figure 12(A) shows the emission spectrum of the reference chips (A1 to A3), and Figure 12(B) shows the emission spectrum of the PhC-formed chips (B4 to B6). Figures 13 and 14 are similar. Note that the IL characteristics in Figure 14 are plotted with the intensity of IF (100 mA) set to 1. As shown in Figure 12, the emission spectra are almost similar for the reference and PhC-formed chips. Furthermore, as shown in Figure 13, the IV characteristics are good for both the reference and PhC-formed chips.

[0073] On the other hand, as shown in Figure 14, the IL characteristics of the chip with PhC formation suppressed the output decrease when the current increased compared to the reference. This is thought to be due to the reduced heat generation caused by the improved external quantum efficiency (EQE).

[0074] 15 and 16 show the directional characteristic measurement results of the reference chips (A1 to A3) and the PhC-formed chips (B4 to B6), respectively. It was confirmed that the directional characteristics were imparted, and in this embodiment, a tendency for the intensity to increase with dispersion in four directions was observed for the PhC-formed chips.

[0075] As described above, according to this embodiment, a photonic crystal can be manufactured by forming holes on the order of several hundred nanometers at a pitch of several hundred nanometers on the surface of a GaN layer grown on a sapphire substrate. This makes it possible to provide directionality to the LED chip alone without using a lens, eliminating the need to create a mold and reducing costs. Furthermore, the light-emitting efficiency of the LED chip can be increased by more than two times compared to when a photonic crystal is not formed, and output reduction when current increases can be suppressed, allowing for flexible response to specification changes.

[0076] 10 sapphire substrate, 12 n-GaN layer, 14 MQW layer, 16 p-GaN layer, 18 p-electrode and reflective film, 20 metal substrate, 22 support substrate, 24 n-electrode.

Claims

1. A method for manufacturing a photonic crystal gallium nitride light-emitting device, comprising: forming an epitaxial structure by epitaxially growing, in order, an n-type gallium nitride layer, a multiple quantum well layer, and a p-type gallium nitride layer on a sapphire substrate; forming a p-type electrode on the p-type gallium nitride layer; forming a metal substrate and a support substrate on the p-type electrode; inverting the epitaxial structure so that the support substrate is on the bottom and the sapphire substrate is on the top; peeling off the sapphire substrate located at the top by the inversion step to expose the n-type gallium nitride layer on the surface; etching the n-type gallium nitride layer exposed on the surface to adjust its thickness; forming a photonic crystal on the etched surface of the n-type gallium nitride layer using electron beam lithography and inductively coupled plasma reactive ion etching; forming an n-type electrode on the n-type gallium nitride layer; and peeling off the support substrate.

2. The method for manufacturing a photonic crystal gallium nitride light-emitting device as described in claim 1, wherein the step of forming the photonic crystal comprises the steps of: performing a hydrophobic treatment on the surface of the n-type gallium nitride layer; applying a resist to the surface of the n-type gallium nitride layer; irradiating the resist with an electron beam to perform drawing; and removing the resist with chlorine gas by inductively coupled plasma reactive ion etching.

3. The method for manufacturing a photonic crystal gallium nitride light-emitting device according to claim 1, comprising the step of growing a buffer layer and an undoped gallium nitride layer, in that order, on the sapphire substrate before growing the n-type gallium nitride layer on the sapphire substrate.

4. A method for producing a photonic crystal gallium nitride light-emitting device according to any one of claims 1 to 3, wherein the emission wavelength of the photonic crystal gallium nitride light-emitting device is 380 nm to 390 nm.

5. An illumination device comprising: a photonic crystal gallium nitride light-emitting element manufactured by the manufacturing method described in any one of claims 1 to 3; and an illumination optical system that irradiates an object with light from the photonic crystal gallium nitride light-emitting element.

Citation Information

Patent Citations

  • Gallium nitride-based semiconductor device and its manufacturing method

    JP2004111766A

  • Photonic-crystal light-emitting diode

    JP2011054828A

  • High-power and high-brightness LED (Light Emitting Diode) chip

    CN202259401U

  • Light emitting device and fabrication method thereof

    JP2007305998A

  • Pyramidal photonic crystal light emitting device

    US20080121912A1