Foamable adhesive sheet and method for producing article

The foamable adhesive sheet with a foaming agent in one layer and without in the other, and a specific tensile shear test, addresses the brittleness and peeling issues, ensuring strong adhesion and durability of the second layer to the base material.

WO2024237232A1PCT designated stage expired Publication Date: 2024-11-21DAI NIPPON PRINTING CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017640
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2024-05-13
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Foam adhesive sheets with adhesive layers on both sides, where one layer contains a foaming agent and the other does not, face issues with the non-foamed layer becoming hard and brittle upon curing, leading to peeling and potential insulation or product failure under shear stress.

Method used

A foamable adhesive sheet with a first adhesive layer containing a foaming agent and a second adhesive layer without a foaming agent, designed to undergo a tensile shear adhesive strength test, ensuring cohesive failure of the first layer and appropriate hardness of the second layer, with a stress-strain curve slope between 3% to 5% strain at 0.20 MPa or less.

Benefits of technology

This configuration enhances the adhesion and durability of the second adhesive layer to the base material, preventing peeling and excessive load on other layers, while maintaining suitable hardness and adhesiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017640_21112024_PF_FP_ABST
    Figure JP2024017640_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure provides a foamable adhesive sheet having a first adhesive layer, a base material, and a second adhesive layer in the stated order. The first adhesive layer contains a first curable adhesive agent and a foaming agent. The second adhesive layer contains a second curable adhesive agent but does not contain a foaming agent. When a tensile shear adhesive strength test method is performed on the foamable adhesive sheet after being foamed and cured, the sheet is fractured in a manner that causes cohesive fracturing of the first adhesive layer after being foamed and cured. In a stress-strain curve obtained when a tensile shear adhesive strength test method is performed on the second adhesive layer after being cured, the slope of an approximate straight line in an interval of strain from 3% to 5% is at most 0.20 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Foamable adhesive sheet and method for manufacturing article

[0001] The present disclosure relates to a foamable adhesive sheet and a method for producing an article using the same.

[0002] Adhesives for bonding two members together are used in a variety of fields, and many bonding methods are known.

[0003] In recent years, it has been proposed to use adhesive sheets containing a foaming agent (foamable adhesive sheets) instead of liquid adhesives (see, for example, Patent Documents 1 and 2).

[0004] Patent No. 6274540 JP 2021-197888 A

[0005] Known examples of foamable adhesive sheets include foamable adhesive sheets having adhesive layers on both sides of a substrate, and it has been proposed that one adhesive layer be a foamed layer containing a foaming agent and the other adhesive layer be a non-foamed layer not containing a foaming agent (see, for example, Patent Documents 1 and 2).

[0006] One example of a method for bonding two components using a foamable adhesive sheet is to place a foamable adhesive sheet between the two components and then foam and cure the foamable adhesive sheet to bond the two components. However, when a foamable adhesive sheet has adhesive layers on both sides of a substrate, with one adhesive layer being a foamed layer and the other being a non-foamed layer, the hardness of the cured adhesive layer varies depending on whether or not it contains a foaming agent. Non-foamed adhesive layers tend to become hard and brittle upon curing. Therefore, after foaming and curing the foamable adhesive sheet, the cured second adhesive layer may peel off from the substrate. If the cured second adhesive layer peels off from the substrate and becomes foreign matter, and this foreign matter adheres to the component, it may lead to product failure or, if the foamable adhesive sheet has insulating properties, to poor insulation. Furthermore, after foaming and curing the foamable adhesive sheet, shear stress may be applied, causing excessive loads on layers other than the second adhesive layer, leading to failure.

[0007] The present disclosure has been made in consideration of the above-mentioned circumstances, and has as its main object to provide a foamable adhesive sheet in which the second adhesive layer has good adhesion to the substrate and durability after curing.

[0008] One embodiment of the present disclosure provides a foamable adhesive sheet having, in this order, a first adhesive layer, a substrate, and a second adhesive layer, wherein the first adhesive layer contains a first curable adhesive and a foaming agent, and the second adhesive layer contains a second curable adhesive but no foaming agent, and when the foamable adhesive sheet after foaming and curing is subjected to a tensile shear bond strength test method, the failure mode is cohesive failure of the first adhesive layer after foaming and curing, and when the second adhesive layer after curing is subjected to a tensile shear bond strength test method, the slope of the approximate straight line in the section from 3% strain to 5% strain in the stress-strain curve obtained is 0.20 MPa or less.

[0009] Another embodiment of the present disclosure provides a method for manufacturing an article, comprising: a placement step of placing the above-mentioned foamable adhesive sheet between a first member and a second member; and a bonding step of foaming and curing the foamable adhesive sheet to bond the first member and the second member together.

[0010] The present disclosure has the effect of providing a foamable adhesive sheet in which the second adhesive layer has good adhesion to the substrate after curing and good durability.

[0011] FIG. 1 is a schematic cross-sectional view showing an example of a foamable adhesive sheet according to the present disclosure. FIG. 2 is a schematic cross-sectional view illustrating a method for testing tensile shear bond strength for a second adhesive layer after curing. FIG. 3 is a schematic cross-sectional view illustrating a method for testing tensile shear bond strength for a first adhesive layer after foaming and curing. FIG. 4 is a schematic cross-sectional view illustrating a method for testing tensile shear bond strength for a first adhesive layer after foaming and curing. FIG. 5 is a graph illustrating an example of a stress-strain curve. FIG. 6 is a schematic cross-sectional view illustrating a method for testing tensile shear bond strength for a foamable adhesive sheet after foaming and curing. FIG. 7 is a schematic cross-sectional view showing another example of a foamable adhesive sheet according to the present disclosure. FIG. 8 is a schematic cross-sectional view showing an example of a method for manufacturing an article according to the present disclosure.

[0012] Embodiments of the present disclosure will be described below with reference to the drawings and the like. However, the present disclosure can be implemented in many different forms and should not be construed as being limited to the description of the embodiments exemplified below. Furthermore, to clarify the explanation, the drawings may show the width, thickness, shape, etc. of each part schematically compared to the actual form, but these are merely examples and do not limit the interpretation of the present disclosure. Furthermore, in this specification and each drawing, elements similar to those described above with reference to the previous drawings may be designated by the same reference numerals, and detailed descriptions may be omitted as appropriate.

[0013] In this specification, when describing a mode in which another component is placed on a certain component, the term "above" or "below" is used, unless otherwise specified, to include both a case in which another component is placed directly above or below a certain component so as to be in contact with the component, and a case in which another component is placed above or below a certain component with another component interposed therebetween. Also, in this specification, when describing a mode in which another component is placed on the surface of a certain component, the term "on the surface side" or "on the surface" is used, unless otherwise specified, to include both a case in which another component is placed directly above or below a certain component so as to be in contact with the component, and a case in which another component is placed above or below a certain component with another component interposed therebetween.

[0014] In this specification, the term "sheet" also includes a member called a "film." In addition, the term "film" also includes a member called a "sheet." In addition, the numerical ranges in this specification are ranges of average values.

[0015] The foamable adhesive sheet and article manufacturing method according to the present disclosure will be described in detail below.

[0016] A. Foamable Adhesive Sheet The foamable adhesive sheet according to the present disclosure comprises a first adhesive layer, a substrate, and a second adhesive layer, in this order; the first adhesive layer contains a first curable adhesive and a foaming agent; the second adhesive layer contains a second curable adhesive but no foaming agent; when the foamable adhesive sheet after foaming and curing is subjected to a tensile shear bond strength test method, the failure mode is cohesive failure of the first adhesive layer after foaming and curing; and when the second adhesive layer after curing is subjected to a tensile shear bond strength test method, the slope of the approximate straight line in the section from 3% strain to 5% strain in the stress-strain curve obtained is 0.20 MPa or less.

[0017] FIG. 1 is a schematic cross-sectional view illustrating an example of a foamable adhesive sheet according to the present disclosure. As shown in FIG. 1, the foamable adhesive sheet 10 comprises a first adhesive layer 1, a substrate 2, and a second adhesive layer 3, in that order. The first adhesive layer 1 contains a first curable adhesive and a foaming agent. The second adhesive layer 3 contains a second curable adhesive but no foaming agent. Furthermore, when the foamable adhesive sheet after foaming and curing is subjected to a tensile shear bond strength test, the failure mode is cohesive failure of the first adhesive layer after foaming and curing. Furthermore, in the stress-strain curve obtained when the tensile shear bond strength test is performed on the cured second adhesive layer, the slope of the approximation line in the section from 3% strain to 5% strain falls within a predetermined range.

[0018] In the present disclosure, the first adhesive layer contains a foaming agent. Therefore, when a foamable adhesive sheet is used to bond two components, the foamable adhesive sheet is foamed and cured, and the gap between the two components is filled with the foamed and cured foamable adhesive sheet, thereby bonding the two components. Therefore, the thickness of the foamable adhesive sheet before foaming and curing can be made thinner than the gap between the two components, improving the ease of insertion of the foamable adhesive sheet. Furthermore, in the present disclosure, the second adhesive layer does not contain a foaming agent, so the surface of the foamable adhesive sheet facing the second adhesive layer does not have any irregularities due to the foaming agent. If the surface of the foamable adhesive sheet had irregularities due to the foaming agent, the protrusions on the surface of the foamable adhesive sheet would likely catch on the component. However, because the surface of the foamable adhesive sheet facing the second adhesive layer does not have any irregularities due to the foaming agent, the surface of the foamable adhesive sheet facing the second adhesive layer is prevented from getting caught on the component. This improves the ease of insertion of the foamable adhesive sheet. For example, the foamable adhesive sheet can be smoothly inserted into the gap between two components. Alternatively, after placing the foamable adhesive sheet in the hole or groove of one component, the other component can be smoothly inserted into the gap. Alternatively, the other component and the foamable adhesive sheet can be smoothly inserted into the hole or groove of one component. Furthermore, the surface of the foamable adhesive sheet facing the second adhesive layer can be caught on the component, preventing the foaming agent from falling off and the second adhesive layer from being scraped. Therefore, the abrasion resistance of the second adhesive layer can be improved.

[0019]

[0013] Note that although the first adhesive layer contains a foaming agent, only one of the two adhesive layers contains a foaming agent, which prevents the surface of the foamable adhesive sheet from getting caught on a member, compared to when both adhesive layers contain a foaming agent. Furthermore, when a second member is inserted into the gap after placing the foamable adhesive sheet in a hole or groove in a first member, by arranging the foamable adhesive sheet so that the surface of the foamable adhesive sheet facing the first adhesive layer faces the first member and the surface of the foamable adhesive sheet facing the second adhesive layer faces the second member, it is possible to prevent the surface of the foamable adhesive sheet facing the second adhesive layer from getting caught on the second member when inserting the second member into the gap after placing the foamable adhesive sheet in a hole or groove in the first member. Furthermore, when inserting the second member and the foamable adhesive sheet into a hole or groove in the first member, by arranging the foamable adhesive sheet so that the surface of the foamable adhesive sheet facing the first adhesive layer faces the second member and the surface of the foamable adhesive sheet facing the second adhesive layer faces the first member, it is possible to prevent the surface of the foamable adhesive sheet facing the second adhesive layer from getting caught on the first member when inserting the second member and the foamable adhesive sheet into the hole or groove in the first member.

[0020] Furthermore, in the present disclosure, because the second adhesive layer does not contain a foaming agent, the cured second adhesive layer does not have bubbles due to the foaming agent. In other words, after the foamable adhesive sheet has foamed and cured, the surface of the cured second adhesive layer does not have any irregularities due to bubbles. Therefore, when two components are bonded using a foamable adhesive sheet, the contact area between the cured second adhesive layer and the components is increased. This improves the thermal conductivity between the two components. For example, when a foamable adhesive sheet is used to bond the stator core and coil of a rotor stator, the thermal conductivity between the stator core and coil can be increased, improving heat dissipation.

[0021] In the present disclosure, since the first adhesive layer contains a foaming agent and the second adhesive layer does not, the cured second adhesive layer tends to be harder and more brittle than the foamed and cured first adhesive layer. Therefore, after the foamed and cured foamable adhesive sheet, the cured second adhesive layer is likely to peel off from the substrate, which could result in the generation of foreign matter. Furthermore, after the foamed and cured foamable adhesive sheet, if shear stress is applied, excessive load may be applied to layers other than the second adhesive layer, leading to breakage. Here, for the cured second adhesive layer, if the slope of the approximate line is large, the cured second adhesive layer tends to be hard; if the slope of the approximate line is small, the cured second adhesive layer tends to be soft. For the cured second adhesive layer, if the slope of the approximate line is below a predetermined value, the cured second adhesive layer will have an appropriate hardness. Therefore, the difference between the hardness of the cured second adhesive layer and the hardness of the foamed and cured first adhesive layer can be reduced. Therefore, after the foamable adhesive sheet has foamed and cured, the adhesion of the cured second adhesive layer to the substrate can be improved, thereby suppressing the generation of foreign matter.Furthermore, after the foamable adhesive sheet has foamed and cured, when shear stress is applied, excessive load on layers other than the second adhesive layer can be suppressed, improving the durability of the foamable adhesive sheet after foaming and curing.

[0022] On the other hand, if the slope of the approximate straight line for the cured second adhesive layer is below a predetermined value, there is a concern that the cured second adhesive layer will become too soft, resulting in a decrease in the adhesiveness of the second adhesive layer after curing. In contrast, in the present disclosure, when the foamable adhesive sheet is subjected to a tensile shear adhesive strength test method, the failure mode is cohesive failure of the first adhesive layer after foaming and curing. Therefore, it can be said that the adhesiveness of the second adhesive layer after curing is high. Furthermore, the adhesiveness of the first adhesive layer after foaming and curing is also high.

[0023] Therefore, by using the foamable adhesive sheet of the present disclosure, the quality and reliability of the product can be improved.

[0024] There are various known methods for testing adhesive strength, including tensile shear adhesive strength testing, tensile adhesive strength testing, peel adhesive strength testing, and flexural adhesive strength testing. Generally, tensile shear adhesive strength is often used to evaluate adhesive properties. When two components are bonded together, the joint is subjected to stresses such as tensile stress, compressive stress, and shear stress. However, when one component is bonded to a hole or groove in the other component, it is believed that shear stress acts primarily on the joint. Therefore, in this disclosure, the tensile shear adhesive strength testing method is used to evaluate physical properties.

[0025] The configuration of the foamable adhesive sheet according to the present disclosure will be described below.

[0026] 1. Physical Properties of the Foamable Adhesive Sheet In the present disclosure, in the stress-strain curve obtained when the cured second adhesive layer is subjected to a tensile shear adhesive strength test, the slope of the approximation line in the section from 3% strain to 5% strain is 0.20 MPa or less, or may be 0.15 MPa or less, or may be 0.10 MPa or less. When the slope is within the above range, the cured second adhesive layer has an appropriate hardness. Therefore, the difference between the hardness of the cured second adhesive layer and the hardness of the foamed and cured first adhesive layer can be reduced. Therefore, after the foamed and cured foamable adhesive sheet, peeling of the cured second adhesive layer from the substrate can be suppressed, thereby suppressing the generation of foreign matter. Furthermore, after the foamed and cured foamable adhesive sheet, excessive load on layers other than the second adhesive layer can be suppressed, improving the durability of the foamed and cured foamable adhesive sheet. Furthermore, the slope is, for example, 0.05 MPa or more, or may be 0.07 MPa or more, or may be 0.10 MPa or more. If the gradient is within the above range, the second adhesive layer after curing has an appropriate hardness, and therefore the adhesiveness of the second adhesive layer after curing is high. Specifically, the gradient may be 0.05 MPa or more and 0.20 MPa or less, or 0.07 MPa or more and 0.15 MPa or less.

[0027] In the present disclosure, the difference between the slope of the approximate straight line in the section from 3% to 5% strain in the stress-strain curve obtained when the first adhesive layer after foaming and curing is subjected to a tensile shear bond strength test method and the slope of the approximate straight line in the section from 3% to 5% strain in the stress-strain curve obtained when the second adhesive layer after curing is subjected to a tensile shear bond strength test method is preferably 0.20 MPa or less, but may also be 0.15 MPa or less, or 0.10 MPa or less. When the difference in slope is within the above range, the difference in hardness between the second adhesive layer after curing and the first adhesive layer after foaming and curing is small. Therefore, after the foamable adhesive sheet is foamed and cured, the second adhesive layer after curing is prevented from peeling from the substrate, thereby preventing the generation of foreign matter. Furthermore, after the foamable adhesive sheet is foamed and cured, excessive load on layers other than the second adhesive layer is prevented, improving the durability of the foamable adhesive sheet after foaming and curing. Furthermore, the difference in the slopes is, for example, 0.05 MPa or more, may be 0.07 MPa or more, or may be 0.10 MPa or more. If the difference in the slopes is within the above range, the second adhesive layer after curing will have an appropriate hardness, and the adhesiveness of the second adhesive layer after curing will be high. Specifically, the difference in the slopes may be 0.05 MPa or more and 0.20 MPa or less, or 0.07 MPa or more and 0.15 MPa or less.

[0028] The tensile shear bond strength test for the cured second adhesive layer is performed according to JIS K6850:1999, which corresponds to ISO 4587, using the following method. First, a 12.5 mm x 25 mm second adhesive layer is prepared. For example, if the adhesive composition used in the second adhesive layer of the foamable adhesive sheet or its composition is known, the second adhesive layer can be formed using that adhesive composition or by preparing an adhesive composition with that composition. Alternatively, the composition of the second adhesive layer of the foamable adhesive sheet can be analyzed, and an adhesive composition with that composition can be prepared to form the second adhesive layer. Known methods can be used to analyze the composition of the second adhesive layer. The thickness of the second adhesive layer is the same as that of the second adhesive layer of the foamable adhesive sheet. Furthermore, as shown in FIG. 2, two metal plates 31a and 31b, each 1.6 mm thick, 25 mm wide, and 100 mm long, are prepared. For example, cold-rolled steel plate SPCC-SD can be used as the metal plate. A spacer 32 is placed at a predetermined distance from one end of one metal plate 31a. The thickness of the spacer 32 is at least 15 μm less than the thickness of the second adhesive layer and at most the thickness of the second adhesive layer. The thickness of the spacer 32 is adjusted, for example, by stacking multiple sheets of Kapton adhesive tape (manufactured by Teraoka Seisakusho Co., Ltd.). Next, the second adhesive layer 3 is placed between the spacers 32, and the other metal plate 31b is placed so that one end overlaps the other and secured with clips or adhesive tape such as Kapton tape to obtain a test specimen. Next, the second adhesive layer of the test specimen is cured. The curing conditions are adjusted appropriately depending on the second curable adhesive contained in the second adhesive layer. Next, the tensile shear bond strength test method is performed on the cured test specimen in accordance with JIS K6850:1999. The measurement conditions are a tensile speed of 10 mm / min, a grip distance of 100 mm, room temperature (23°C), and humidity of 50% RH. As the tensile tester, for example, Tensilon RTF1350 manufactured by A&D Co., Ltd. can be used.

[0029] Furthermore, the tensile shear bond strength test method for the first adhesive layer after foaming and curing is performed in accordance with JIS K6850:1999, which corresponds to ISO 4587, using the following method. First, a first adhesive layer measuring 12.5 mm x 25 mm is prepared. For example, if the adhesive composition used in the first adhesive layer of the foamable adhesive sheet or its composition is known, the first adhesive layer can be formed using that adhesive composition or by preparing an adhesive composition with that composition. Alternatively, the composition of the first adhesive layer of the foamable adhesive sheet can be analyzed, and an adhesive composition with that composition can be prepared to form the first adhesive layer. Known methods can be used to analyze the composition of the first adhesive layer. The thickness of the first adhesive layer is the same as that of the first adhesive layer of the foamable adhesive sheet. Furthermore, as shown in FIG. 3, two metal plates 31a and 31b, each 1.6 mm thick, 25 mm wide, and 100 mm long, are prepared. For example, cold-rolled steel plate SPCC-SD can be used as the metal plate. A spacer 32 is placed at one end of one metal plate 31a with a predetermined gap between them. The thickness of the spacer 32 is set appropriately depending on the foaming ratio of the first adhesive layer. For example, as shown in FIG. 4, a foamable adhesive sheet 10 is placed between a first member 20a and a second member 20b, and then, although not shown, the foamable adhesive sheet 10 is foamed and cured to bond the first member 20a and the second member 20b. If the distance d1 between the first member 20a and the second member 20b is known, the gap d2 after the foamable adhesive sheet 10 is placed between the first member 20a and the second member 20b is first calculated. The gap d2 is calculated by subtracting the thickness t1 of the foamable adhesive sheet 10 from the distance d1. Next, the thickness of the spacer 32 is determined based on the thickness of the first adhesive layer and the gap d2. The thickness of the spacer 32 is calculated by adding the thickness of the first adhesive layer to the gap d2. The thickness of the spacer 32 may be within ±5% of the sum of the thickness of the first adhesive layer and the gap d2. On the other hand, if the distance d1 between the first member 20a and the second member 20b is unknown, the expansion ratio of the first adhesive layer is first determined. The expansion ratio here refers to the expansion ratio when the first adhesive layer is foamed and cured without being sandwiched between any members.The expansion ratio of the first adhesive layer can be determined by foaming and curing the foamable adhesive sheet without sandwiching it between any other components. In this case, the thickness of the spacer 32 is at least (thickness of the first adhesive layer) × (expansion ratio of the first adhesive layer) × 0.3 and at most (thickness of the first adhesive layer) × (expansion ratio of the first adhesive layer) × 0.8. However, the thickness of the spacer 32 must be at least the thickness of the first adhesive layer. The thickness of the spacer 32 is adjusted, for example, by stacking multiple sheets of Kapton adhesive tape (manufactured by Teraoka Seisakusho Co., Ltd.). Next, the first adhesive layer 1 is placed between the spacers 32, and the other metal plate 31b is placed so that one end overlaps the other and secured with clips or adhesive tape such as Kapton tape to obtain a test specimen. Next, the first adhesive layer of the test specimen is foamed and cured. The foaming and curing conditions are adjusted appropriately depending on the first curable adhesive and foaming agent contained in the first adhesive layer. Next, the tensile shear bond strength test method is performed on the foamed and cured test specimen in accordance with JIS K6850:1999. The measurement conditions are a tensile speed of 10 mm / min, a gripping distance of 100 mm, a room temperature (23° C.), and a humidity of 50% RH. As the tensile tester, for example, a Tensilon RTF1350 manufactured by A&D Co., Ltd. can be used.

[0030] The stress-strain curve is a plot of the relationship between shear stress and strain obtained in the above-mentioned tensile shear bond strength test method, with strain (%) on the horizontal axis and shear stress (MPa) on the vertical axis, as shown in Figures 5(a) and (b). The strain is the increase in the distance between the grippers divided by the length of the first adhesive layer or the second adhesive layer, i.e., 12.5 mm. Figure 5(b) is an enlarged view of Figure 5(a).

[0031] In the stress-strain curve obtained by the above-mentioned tensile shear bond strength test method, the approximate straight line in the section from 3% strain to 5% strain is obtained by linearly approximating the curve in the section from 3% strain to 5% strain using the least squares method. The slope of the approximate straight line is then calculated. The above-mentioned tensile shear bond strength test method is performed three times, and the average value of the three measurements is used as the slope of the approximate straight line.

[0032] In the stress-strain curve obtained by the above-mentioned tensile shear bond strength test method, the initial slope is the slope in the elastic region. Therefore, in the present disclosure, the initial slope is adopted. Furthermore, in the stress-strain curve, shear stress tends to be unstable in the section below 3% strain. Therefore, in the present disclosure, the slope in the section from 3% strain to 5% strain is adopted as the initial slope.

[0033] Methods for controlling the slope of the above approximate straight line for the second adhesive layer after curing include, for example, adjusting the composition of the second adhesive layer and adjusting the drying conditions when forming the second adhesive layer.

[0034] In the method of adjusting the composition of the second adhesive layer, as described below, by incorporating flexible particles into the second adhesive layer, the hardness of the second adhesive layer after curing tends to be reduced, and the slope of the above-mentioned approximate straight line tends to be smaller. Furthermore, in a second adhesive layer containing an epoxy resin and a curing agent, if the number of functional groups of the epoxy resin is the same, by reducing the molecular weight of the epoxy resin, the hardness of the second adhesive layer after curing tends to be reduced, and the slope of the above-mentioned approximate straight line tends to be smaller. Furthermore, in a second adhesive layer containing an epoxy resin and a curing agent, by reducing the content of a multifunctional epoxy resin, the crosslink density after curing decreases, and therefore the hardness of the second adhesive layer after curing tends to be reduced, and the slope of the above-mentioned approximate straight line tends to be smaller.

[0035] In the present disclosure, when a foamable adhesive sheet is subjected to a tensile shear adhesive strength test method after foaming and curing, the failure mode is cohesive failure of the first adhesive layer after foaming and curing. If the failure mode is cohesive failure of the first adhesive layer after foaming and curing, it can be said that the second adhesive layer after curing has a higher strength than the first adhesive layer after foaming and curing.

[0036] The tensile shear adhesive strength test for the foamed and cured foam adhesive sheet is performed according to the following method, which conforms to JIS K6850:1999, which corresponds to ISO 4587. First, a foam adhesive sheet measuring 12.5 mm x 25 mm is prepared. As shown in FIG. 6, two metal plates 31a and 31b, each 1.6 mm thick, 25 mm wide, and 100 mm long, are prepared. For example, cold-rolled steel plate SPCC-SD can be used as the metal plates. A spacer 32 is placed at one end of one of the metal plates 31a, with a predetermined distance between them. The thickness of the spacer 32 is appropriately set depending on the foaming ratio of the first adhesive layer. For example, as shown in FIG. 4 , a foamable adhesive sheet 10 is placed between a first member 20a and a second member 20b, and then, although not shown, foamed and cured to bond the first member 20a and the second member 20b. If the distance d1 between the first member 20a and the second member 20b is known, the thickness of the spacer 32 is set to the distance d1. The thickness of the spacer 32 may be within ±5% of the distance d1. On the other hand, if the distance d1 between the first member 20a and the second member 20b is unknown, the foaming ratio of the first adhesive layer is first determined. The foaming ratio here refers to the foaming ratio when the first adhesive layer is foamed and cured without being sandwiched between any other members. The foaming ratio of the first adhesive layer can be determined by foaming and curing the foamable adhesive sheet without being sandwiched between any other members. In this case, the thickness of the spacer 32 must be equal to or greater than {(thickness of the foamable adhesive sheet) - (thickness of the first adhesive layer)} + ​​(thickness of the first adhesive layer) x (expansion ratio of the first adhesive layer) x 0.3, and equal to or less than {(thickness of the foamable adhesive sheet) - (thickness of the first adhesive layer)} + ​​(thickness of the first adhesive layer) x (expansion ratio of the first adhesive layer) x 0.8. However, the thickness of the spacer 32 must be equal to or greater than the thickness of the foamable adhesive sheet. The thickness of the spacer 32 is adjusted by stacking multiple sheets of Kapton adhesive tape manufactured by Teraoka Seisakusho Co., Ltd. Next, a foamable adhesive sheet 10 is placed between the spacers 32, and the other metal plate 31b is placed so that one tip overlaps the other and fixed with a clip or adhesive tape such as Kapton tape to obtain a test specimen. Next, the first adhesive layer of the test specimen is foamed and cured, and the second adhesive layer is cured.The foaming and curing conditions are adjusted appropriately depending on the first curable adhesive and foaming agent contained in the first adhesive layer and the second curable adhesive contained in the second adhesive layer. Next, the test piece after foaming and curing is subjected to a tensile shear bond strength test method in accordance with JIS K6850:1999. The measurement conditions are a tensile speed of 10 mm / min, room temperature (23°C), and humidity of 50% RH. For example, a Tensilon RTF1350 manufactured by A&D Co., Ltd. can be used as a tensile tester. Next, the fracture surface of the test piece is visually observed.

[0037] The failure mode being cohesive failure of the first adhesive layer after foaming and curing means that the cohesive failure rate within the first adhesive layer after foaming and curing is 90% or more. The cohesive failure rate is the ratio of the area of ​​the cohesive failure portion within the first adhesive layer to the total adhesive area. The above tensile shear bond strength test method is performed three times, and the cohesive failure rate is the average value of the three measurements.

[0038] The foamable adhesive sheet of the present disclosure preferably has high adhesiveness after foaming and curing. The shear bond strength may be, for example, 2.1 MPa or more, or 2.3 MPa or more, at 23°C. Furthermore, the shear bond strength may be, for example, 0.27 MPa or more, 0.55 MPa or more, or 0.58 MPa or more, at 200°C. For example, a high-strength acrylic foam adhesive tape that does not require heating has a shear bond strength of approximately 1 MPa to 2 MPa at room temperature and lacks heat resistance at 200°C. Therefore, if the shear bond strength is within the above range at 23°C, it has advantages in terms of strength. Furthermore, if the shear bond strength is within the above range at 200°C, it can be used in applications requiring heat resistance around automobile engines or similar.

[0039] The shear adhesive strength of the foamable adhesive sheet after foaming and curing was measured by the tensile shear adhesive strength test method described above, and was defined as the maximum shear stress at break.

[0040] The foamable adhesive sheet of the present disclosure preferably has good shape retention. The bending moment based on JIS P8125-2:2017, which corresponds to ISO 2493, is, for example, 3 gf·cm or more, and may be 5 gf·cm or more. On the other hand, the bending moment may be, for example, less than 40 gf·cm, and may be less than 30 gf·cm. Conventionally, adhesive sheets generally have a high bending moment to improve their shape retention and ease of insertion into narrow gaps. In contrast, the inventors of the present disclosure have discovered that shape retention can be ensured by modifying the shape, and that a high bending moment has other drawbacks, so taking other characteristics into consideration, it is preferable that the bending moment be within the above range. If the bending moment is smaller than the above range, shape retention may be difficult even with measures such as folding. Furthermore, if the bending moment is larger than the above range, the shape will return to its original state after folding, requiring heating or creases during folding. Heating reduces the sheet life, and striations can reduce the insulation properties of that area.

[0041] The foamable adhesive sheet of the present disclosure preferably has high electrical insulation after foaming and curing. The breakdown voltage based on JIS C2107:2011, which corresponds to IEC 60454-2, is preferably 1 kV or higher, and more preferably 3 kV or higher. Having the breakdown voltage within the above range enables application for rust prevention and around copper wires. Furthermore, the foamable adhesive sheet of the present disclosure preferably has a thermal conductivity after foaming and curing of 0.1 W / mK or higher, and more preferably 0.15 W / mK or higher. Having the thermal conductivity within the above range allows for the miniaturization of components and promotes the curing reaction during heating.

[0042] 2. First Adhesive Layer The first adhesive layer in the present disclosure is disposed on one surface of the substrate and contains a first curable adhesive and a foaming agent.

[0043] (1) Physical Properties of the First Adhesive Layer The first adhesive layer in the present disclosure is preferably substantially non-tacky. Specifically, the tackiness of the first adhesive layer is preferably less than 0.1 N, and may be 0.05 N or less, or may be 0.02 N or less. When the tackiness of the first adhesive layer is within the above range, the first adhesive layer becomes substantially non-tacky (tack-free). In addition, the slipperiness of the first adhesive layer is improved, which can improve the insertability of the foamable adhesive sheet.

[0044] Here, the tackiness of the first adhesive layer is measured by a probe tack test. Specifically, a cylindrical stainless steel probe with a diameter of 5 mm is pressed against the surface of the first adhesive layer of the foamable adhesive sheet under conditions of a temperature of 23±5°C and a humidity of 50±30% RH at a load of 0.1 N and a speed of 30 mm / min, and after holding for 1.0 second, it is peeled off at a speed of 30 mm / min, and the load at the time of peeling is measured. This measurement is performed five times, and the average value is taken as the tackiness. As a probe tackiness tester, for example, a tackiness tester "TAC-II" manufactured by RHESCA can be used.

[0045] In the present disclosure, methods for controlling the tackiness of the first adhesive layer include, for example, adjusting the composition of the first adhesive layer. Specifically, the tackiness of the first adhesive layer can be reduced by using an epoxy resin that is solid at room temperature or a curing agent that is solid at room temperature in the first adhesive layer containing an epoxy resin and a curing agent. Furthermore, the tackiness of the first adhesive layer can be reduced by including an epoxy resin with a high softening temperature or an epoxy resin with a high weight-average molecular weight in the first adhesive layer containing an epoxy resin and a curing agent. For example, the tackiness of the first adhesive layer can be reduced by including multiple epoxy resins with different softening temperatures in the first adhesive layer, i.e., by including one epoxy resin and another epoxy resin with a softening temperature of 25°C or higher and 10°C or higher than the softening temperature of the first epoxy resin. Furthermore, for example, the tackiness of the first adhesive layer can be reduced by including multiple epoxy resins with different weight-average molecular weights in the first adhesive layer. That is, the first adhesive layer can include one epoxy resin and another epoxy resin with a weight-average molecular weight of 370 or more that is 300 or more greater than that of the first epoxy resin. More specifically, the tackiness of the first adhesive layer can be reduced by including a first epoxy resin with a low softening temperature and low molecular weight and a second epoxy resin with a high softening temperature and high molecular weight, as described below, in the first adhesive layer containing an epoxy resin and a curing agent. The tackiness of the first adhesive layer can also be reduced by including an acrylic resin that is compatible with the epoxy resin, as described below, in the first adhesive layer containing an epoxy resin and a curing agent.

[0046] Here, non-tacky is generally used mainly to mean low adhesive strength. In the present disclosure, "substantially non-tacky" means that the tack is less than 0.1 N.

[0047] "Adhesion" is a concept that is included in "adhesion." The two are sometimes distinguished in that "adhesion" is used to mean a temporary adhesive phenomenon, while "adhesion" is used to mean a substantially permanent adhesive phenomenon (Iwanami Shoten Physics and Chemistry Dictionary, 5th Edition). "Adhesion" and "adhesive strength" refer to the property of adhering by pressure and the adhesive strength at that time.

[0048] In this specification, unless otherwise specified, the terms "adhesion of the adhesive layer" and "adhesion strength of the adhesive layer" refer to the adhesion and adhesive strength of the adhesive layer before curing. In addition, in this specification, unless otherwise specified, the terms "adhesion of the adhesive layer" and "adhesion strength of the adhesive layer" refer to the adhesion and adhesive strength of the adhesive layer after curing.

[0049] (2) Material for the First Adhesive Layer (a) First Curable Adhesive The first curable adhesive contained in the first adhesive layer in the present disclosure can be a curable adhesive generally used in adhesive layers of adhesive sheets. Examples of the first curable adhesive include heat-curable adhesives and light-curable adhesives. Among these, heat-curable adhesives are preferred. Heat-curable adhesives can be applied even when the component does not have transparency, such as a metal component.

[0050] Examples of the first curable adhesive include epoxy resin adhesives, acrylic resin adhesives, phenol resin adhesives, unsaturated polyester resin adhesives, alkyd resin adhesives, urethane resin adhesives, and thermosetting polyimide resin adhesives.

[0051] The first curable adhesive is preferably an epoxy resin adhesive. That is, the first curable adhesive preferably contains an epoxy resin and a curing agent. In general, epoxy resin adhesives produce hard and tough cured films, making them suitable for bonding hard material components such as metal and glass components. Furthermore, epoxy resin adhesives generally have excellent heat resistance, insulating properties, chemical resistance, etc., and exhibit little shrinkage upon curing, making them suitable for a wide range of applications.

[0052] Furthermore, when the first curable adhesive is an epoxy resin adhesive, the first curable adhesive preferably further contains an acrylic resin that is compatible with the epoxy resin. By using an acrylic resin that is compatible with the epoxy resin, the toughness of the first adhesive layer can be increased, thereby improving the adhesiveness after foaming and curing.

[0053] Hereinafter, an example in which the first curable adhesive is an epoxy resin adhesive will be described.

[0054] (i) Epoxy Resin The epoxy resin in the present disclosure is a compound that has at least one epoxy group or glycidyl group and cures by a crosslinking polymerization reaction in combination with a curing agent. The epoxy resin also includes a monomer having at least one epoxy group or glycidyl group.

[0055] The epoxy resin can be any epoxy resin commonly used in the adhesive layer of an adhesive sheet. In particular, the curable adhesive preferably contains, as the epoxy resin, a first epoxy resin having a softening temperature of 50°C or higher and an epoxy equivalent of 5,000 g / eq or less, and a second epoxy resin having a softening temperature higher than that of the first epoxy resin and a weight-average molecular weight of 20,000 or more. By using a combination of the first epoxy resin and the second epoxy resin, an adhesive sheet with good adhesion and blocking resistance after foaming and curing can be obtained. Furthermore, the tackiness (tackiness) of the first adhesive layer can be reduced, resulting in an adhesive sheet with good slip properties.

[0056] For example, when only improving adhesiveness after foaming and curing is desired, it is more effective to use a low molecular weight (low epoxy equivalent) epoxy resin than a high molecular weight (high epoxy equivalent) epoxy resin. However, when a low molecular weight (low epoxy equivalent) epoxy resin is used, for example, when the adhesive sheet is wound into a roll, the low molecular weight (low epoxy equivalent) epoxy resins tend to assimilate with each other, resulting in blocking.

[0057] In contrast, when a first epoxy resin having a relatively low softening temperature (relatively high crystallinity) and a low molecular weight (low epoxy equivalent weight) is used, the first epoxy resin rapidly melts and changes into a low-viscosity liquid when heated to a temperature above its softening temperature. This facilitates improved adhesiveness after foaming and curing. Meanwhile, the first epoxy resin has relatively high crystallinity, which can suppress blocking compared to epoxy resins with relatively low crystallinity or no crystallinity. However, using only the first epoxy resin may result in insufficient blocking suppression or excessive tackiness of the first adhesive layer. Therefore, by further using a second epoxy resin having a relatively high softening temperature (relatively low crystallinity) and a high molecular weight, the blocking suppression effect can be improved and the tackiness of the first adhesive layer can be reduced.

[0058] (i-1) First Epoxy Resin The first epoxy resin has a softening temperature of 50°C or higher and an epoxy equivalent of 5000 g / eq or lower. The first epoxy resin has a relatively low softening temperature (relatively high crystallinity) compared to the second epoxy resin described below. The first epoxy resin has relatively high crystallinity and a low molecular weight, which makes it easy to improve adhesion and blocking resistance after foaming and curing. Furthermore, the first epoxy resin has a low molecular weight, which allows for a high crosslink density, resulting in a first adhesive layer with excellent mechanical strength, chemical resistance, and curing properties. Furthermore, the first epoxy resin is preferably an epoxy resin that is solid at room temperature (23°C).

[0059] The softening temperature of the first epoxy resin is usually 50° C. or higher, and may be 55° C. or higher, or 60° C. or higher. On the other hand, the softening temperature of the first epoxy resin is, for example, 150° C. or lower. The softening temperature is measured by the ring and ball method in accordance with JIS K7234:1986.

[0060] The epoxy equivalent of the first epoxy resin is, for example, 5000 g / eq or less, and may be 3000 g / eq or less, 1000 g / eq or less, or 600 g / eq or less. On the other hand, the epoxy equivalent of the first epoxy resin is, for example, 90 g / eq or more, 100 g / eq or more, or 110 g / eq or more. The epoxy equivalent is the number of grams of resin containing 1 gram equivalent of epoxy groups. The epoxy equivalent is measured by a method in accordance with JIS K7236:2009, which corresponds to ISO 3001 (Plastics - Epoxy compounds - Determination of epoxy equivalent).

[0061] The first epoxy resin may be a monofunctional epoxy resin, a difunctional epoxy resin, a trifunctional epoxy resin, or a tetrafunctional or higher functional epoxy resin.

[0062] The weight-average molecular weight (Mw) of the first epoxy resin is usually smaller than the weight-average molecular weight (Mw) of the second epoxy resin described below. The Mw of the first epoxy resin is, for example, 6,000 or less, and may be 4,000 or less, or 3,000 or less. On the other hand, the Mw of the first epoxy resin is, for example, 400 or more. Mw is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).

[0063] The melt viscosity of the first epoxy resin at 150°C is, for example, 0.005 Pa·s or more, or may be 0.015 Pa·s or more, 0.03 Pa·s or more, 0.05 Pa·s or more, or 0.1 Pa·s or more. If the melt viscosity is too low, good foaming properties may not be obtained. Furthermore, if the melt viscosity of the first epoxy resin is too low (if the crystallinity of the first epoxy resin is too high), the resulting first adhesive layer may have high tackiness. This is presumably because if the melt viscosity of the first epoxy resin is too low (if the crystallinity of the first epoxy resin is too high), its crystallinity is significantly reduced when it is mixed with the second epoxy resin or the acrylic resin, thereby reducing the Tg of the entire adhesive composition. On the other hand, the melt viscosity of the first epoxy resin at 150°C is, for example, 10 Pa·s or less, or may be 5 Pa·s or less, or 2 Pa·s or less. If the melt viscosity is too high, the resulting first adhesive layer may have reduced uniformity. The melt viscosity is measured in accordance with JIS K6862:1984, which corresponds to ISO 2555 (Resins in the liquid state or as emulsions or dispersions—Determination of Brookfield RV viscosity), using a Brookfield-type single-cylinder rotational viscometer and a thermocell for heating the solution.

[0064] Next, the composition of the first epoxy resin will be described. Examples of the first epoxy resin include aromatic epoxy resins, aliphatic epoxy resins, alicyclic epoxy resins, and heterocyclic epoxy resins. Specific examples of the first epoxy resin include bisphenol-type epoxy resins, novolac-type epoxy resins, and modified epoxy resins. Examples of the bisphenol-type epoxy resin include bisphenol A-type epoxy resins and bisphenol F-type epoxy resins. Examples of the novolac-type epoxy resin include bisphenol A novolac-type epoxy resins and cresol novolac-type epoxy resins. Examples of the modified epoxy resin include urethane-modified epoxy resins and rubber-modified epoxy resins. Other specific examples include biphenyl-type epoxy resins, stilbene-type epoxy resins, triphenolmethane-type epoxy resins, alkyl-modified triphenolmethane-type epoxy resins, triazine-nucleus-containing epoxy resins, dicyclopentadiene-modified phenol-type epoxy resins, naphthalene-type epoxy resins, glycol-type epoxy resins, and pentaerythritol-type epoxy resins. The first epoxy resin may be one type or two or more types.

[0065] Bisphenol A epoxy resins can exist in a liquid state or a solid state at room temperature depending on the number of repeating units in the bisphenol skeleton. Bisphenol A epoxy resins having, for example, 2 to 10 bisphenol skeletons in the main chain are solid at room temperature. Bisphenol A epoxy resins are particularly preferred because they can improve heat resistance.

[0066] In particular, the first epoxy resin is preferably a bisphenol A novolac epoxy resin represented by the following general formula (1).

[0067]

[0068] In general formula (1), R 1 is C m H 2m (m is 1 or more and 3 or less), and R 2 and R 3 are each independently C p H2p+1 (p is 1 or more and 3 or less), and n is 0 or more and 10 or less.

[0069] In general formula (1), R 1 m in is 1, that is, R 1 Ha-CH 2 Similarly, R 2 and R 3 p in is 1, that is, R 2 and R 3 Ha-CH 3 Furthermore, the hydrogen bonded to the benzene ring in general formula (1) may be substituted with other elements or other groups.

[0070] The content of the first epoxy resin, relative to 100 parts by mass of the resin component contained in the first adhesive layer, may be, for example, 1 part by mass or more, 3 parts by mass or more, 5 parts by mass or more, 10 parts by mass or more, 15 parts by mass or more, or 25 parts by mass or more. If the content of the first epoxy resin is too low, the adhesiveness and blocking resistance after foaming and curing may be reduced. On the other hand, the content of the first epoxy resin, relative to 100 parts by mass of the resin component contained in the first adhesive layer, may be, for example, 90 parts by mass or less, 80 parts by mass or less, 70 parts by mass or less, 60 parts by mass or less, 50 parts by mass or less, or 40 parts by mass or less. If the content of the first epoxy resin is too high, the contents of the second epoxy resin and acrylic resin may be relatively low, which may make it difficult to balance blocking resistance, adhesion of the first adhesive layer to the substrate, and adhesiveness after foaming and curing.

[0071] (i-2) Second Epoxy Resin The second epoxy resin has a softening temperature higher than that of the first epoxy resin and a weight-average molecular weight of 20,000 or more. The second epoxy resin has a relatively high softening temperature (relatively low crystallinity) compared to the first epoxy resin described above. The second epoxy resin has relatively low crystallinity and a high molecular weight, which makes it easy to improve blocking resistance. Furthermore, the second epoxy resin has relatively low crystallinity and a high molecular weight, which can suppress an increase in adhesion (tackiness) caused by the first epoxy resin. In addition, the second epoxy resin is preferably an epoxy resin that is solid at room temperature (23°C).

[0072] The weight average molecular weight (Mw) of the second epoxy resin is usually larger than the weight average molecular weight (Mw) of the first epoxy resin. The Mw of the second epoxy resin is usually 20,000 or more, or may be 30,000 or more, or may be 35,000 or more. On the other hand, the Mw of the second epoxy resin is, for example, 100,000 or less.

[0073] The epoxy equivalent of the second epoxy resin may be greater than, less than, or the same as the epoxy equivalent of the first epoxy resin. The epoxy equivalent of the second epoxy resin is, for example, 4000 g / eq or more, 5000 g / eq or more, or 6000 g / eq or more. On the other hand, the epoxy equivalent of the second epoxy resin is, for example, 20000 g / eq or less.

[0074] The second epoxy resin may be a monofunctional epoxy resin, a difunctional epoxy resin, a trifunctional epoxy resin, or a tetrafunctional or higher functional epoxy resin.

[0075] The softening temperature of the second epoxy resin is usually higher than that of the first epoxy resin. The difference between the two temperatures is, for example, 10°C or higher, and may be 20°C or higher, or 30°C or higher. The softening temperature of the second epoxy resin is, for example, 80°C or higher, and may be 90°C or higher. On the other hand, the softening temperature of the second epoxy resin is, for example, 180°C or lower.

[0076] The structure of the second epoxy resin is the same as that of the first epoxy resin described above, and therefore will not be described here.

[0077] The content of the second epoxy resin, relative to 100 parts by mass of the resin component contained in the first adhesive layer, may be, for example, 10 parts by mass or more, 15 parts by mass or more, 20 parts by mass or more, 25 parts by mass or more, 30 parts by mass or more, 35 parts by mass or more, 40 parts by mass or more, or 45 parts by mass or more. If the content of the second epoxy resin is too low, blocking resistance may be reduced. On the other hand, the content of the second epoxy resin, relative to 100 parts by mass of the resin component contained in the first adhesive layer, may be, for example, 90 parts by mass or less, 85 parts by mass or less, 80 parts by mass or less, or 75 parts by mass or less. If the content of the second epoxy resin is too high, the contents of the first epoxy resin and acrylic resin may be relatively low, which may make it difficult to balance blocking resistance, adhesion of the first adhesive layer to the substrate, and adhesion after foaming and curing.

[0078] The proportion of the first epoxy resin relative to the total of the first epoxy resin and the second epoxy resin is, for example, 5% by mass or more, or alternatively 10% by mass or more, or 15% by mass or more, or alternatively 20% by mass or more, while the proportion of the first epoxy resin is, for example, 80% by mass or less, or alternatively 75% by mass or less, or alternatively 60% by mass or less.

[0079] Furthermore, the total proportion of the first epoxy resin and the second epoxy resin to all epoxy resins contained in the first adhesive layer is, for example, 50% by mass or more, or may be 70% by mass or more, or 90% by mass or more, or may be 100% by mass.

[0080] (ii) Acrylic Resin The acrylic resin in the present disclosure is a resin compatible with epoxy resin. Because acrylic resin is compatible with epoxy resin, it is easy to improve the toughness of the first adhesive layer. As a result, the adhesion of the first adhesive layer to the substrate can be improved. Furthermore, improved toughness of the adhesive layer can improve adhesion after foaming and curing. Furthermore, it is thought that the acrylic resin acts as a compatibilizer for the foaming agent (e.g., a foaming agent whose shell portion is an acrylonitrile copolymer resin), uniformly dispersing and foaming, thereby improving adhesion after foaming and curing. Furthermore, the compatibility of the acrylic resin with the epoxy resin can maintain high hardness of the surface of the first adhesive layer. On the other hand, if the acrylic resin is incompatible with the epoxy resin, a flexible portion is formed on the surface of the first adhesive layer, making the interface with the adherend less slippery and reducing workability.

[0081] The acrylic resin in the present disclosure is compatible with the epoxy resin. Here, compatibility of the acrylic resin with the epoxy resin can be confirmed, for example, by observing the cross section of the first adhesive layer of the adhesive sheet with a scanning electron microscope (SEM) or a transmission electron microscope (TEM) to see if micron-sized islands are present. More specifically, the average particle size of the islands is preferably 1 μm or less. In particular, the average particle size of the islands may be 0.5 μm or less, or even 0.3 μm or less. A large number of samples, for example, 100 or more, is preferred. The area to be observed is within a range of 100 μm × 100 μm, or, if the average thickness of the first adhesive layer is 100 μm or less, within a range of the average thickness × 100 μm.

[0082] The weight-average molecular weight (Mw) of the acrylic resin is, for example, 50,000 or more, or may be 70,000 or more, or even 100,000 or more. The first epoxy resin has relatively high crystallinity, which can result in a low melt viscosity (or dynamic viscoelasticity) when heated, potentially causing shrinkage during curing after foaming (between the end of foaming of the foaming agent and the curing of the adhesive composition). However, by using an acrylic resin with a certain molecular weight, it is possible to prevent the melt viscosity from becoming too low, making it less likely for shrinkage to occur during curing after foaming. Meanwhile, the Mw of the acrylic resin is, for example, 1,500,000 or less. The weight-average molecular weight of the acrylic resin is measured by GPC (eluent: THF, standard: PS, sample: 20 μL, flow rate: 1 mL / min, column temperature: 40°C).

[0083] The glass transition temperature (Tg) of the acrylic resin is, for example, 90° C. or higher, and may be 100° C. or higher. On the other hand, the Tg of the acrylic resin is, for example, 180° C. or lower. Tg is measured by a differential scanning calorimeter (DSC) in accordance with JIS K7121:2012, which corresponds to ISO 3146.

[0084] The acrylic resin has a storage modulus (E') of 1 x 10 at the foaming initiation temperature. 6 A low E' at the foaming initiation temperature can improve fluidity and provide good foaming properties. On the other hand, E' at the foaming initiation temperature can be, for example, 1 x 10 5 The foaming initiation temperature is a temperature that varies depending on the type of foaming agent. When two or more foaming agents are used, the foaming initiation temperature is the temperature at which the main foaming reaction begins.

[0085] The acrylic resin has a storage modulus (E') of 1 x 10 at the curing initiation temperature. 5Pa or more. As described above, shrinkage may occur during curing after foaming (from the time when foaming of the foaming agent is completed until the adhesive composition is cured). However, if E' at the curing initiation temperature is large, shrinkage can be suppressed and good shape retention can be obtained. The curing initiation temperature varies depending on the type of curing agent. When two or more curing agents are used as the curing agent, the initiation temperature of the main curing reaction is taken as the curing initiation temperature.

[0086] The acrylic resin has an average storage modulus (E') of 1 x 10 at temperatures between 0°C and 100°C. 6 The average value of E' before foaming may be high, which allows for good blocking resistance. On the other hand, the average value of the storage modulus (E') at temperatures of 0°C or higher and 100°C or lower may be, for example, 1 x 10 8 Pa or less.

[0087] The storage modulus (E') of the acrylic resin is measured by a dynamic viscoelasticity measurement method in accordance with JIS K7244-1:1998. The measurement conditions are as follows: attachment mode: compression mode, frequency: 1 Hz, temperature: -30°C to 200°C, and temperature rise rate: 10°C / min. The device that can be used is a solid viscoelasticity analyzer "RSA-III" manufactured by TA Instruments.

[0088] The acrylic resin may have a polar group, such as an epoxy group, a hydroxyl group, a carboxyl group, a nitrile group, or an amide group.

[0089] The acrylic resin may be a homopolymer of an acrylic acid ester monomer, a mixed component containing two or more of the above homopolymers, or a copolymer of two or more acrylic acid ester monomers, a component containing one or more copolymers. The acrylic resin may also be a mixed component of the above homopolymer and the above copolymer. The "acrylic acid" acrylic acid ester monomer also includes the concept of methacrylic acid. Specifically, the acrylic resin may be a mixture of a methacrylate polymer and an acrylate polymer, or an acrylic acid ester polymer such as acrylate-acrylate, methacrylate-methacrylate, or methacrylate-acrylate. Of these, it is preferable that the acrylic resin contain a copolymer of two or more acrylic acid ester monomers (a (meth)acrylic acid ester copolymer).

[0090] Examples of the monomer component constituting the (meth)acrylic acid ester copolymer include the monomer components described in JP 2014-065889 A. The monomer component may have the polar group described above. Examples of the (meth)acrylic acid ester copolymer include an ethyl acrylate-butyl acrylate-acrylonitrile copolymer, an ethyl acrylate-acrylonitrile copolymer, and a butyl acrylate-acrylonitrile copolymer. Note that "acrylic acid" such as methyl acrylate and ethyl acrylate also includes "methacrylic acid" such as methyl methacrylate and ethyl methacrylate.

[0091] The (meth)acrylic acid ester copolymer is preferably a block copolymer, and more preferably an acrylic block copolymer such as a methacrylate-acrylate copolymer. Examples of (meth)acrylates constituting the acrylic block copolymer include methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, and benzidyl acrylate. In these examples, "acrylic acid" also includes "methacrylic acid."

[0092] Specific examples of methacrylate-acrylate copolymers include acrylic copolymers such as methyl methacrylate-butyl acrylate-methyl methacrylate (MMA-BA-MMA) copolymer, which also includes block copolymers of polymethyl methacrylate-polybutyl acrylate-polymethyl methacrylate (PMMA-PBA-PMMA).

[0093] The acrylic copolymer may have no polar groups, or may be a modified product in which the above-mentioned polar groups have been partially introduced. The modified product is highly compatible with epoxy resins, thereby further improving adhesion.

[0094] Among these, the acrylic resin is preferably a (meth)acrylic acid ester copolymer having a first polymer portion having a glass transition temperature (Tg) of 10° C. or lower and a second polymer portion having a glass transition temperature (Tg) of 20° C. or higher. Such a (meth)acrylic acid ester copolymer has the first polymer portion that becomes a soft segment and the second polymer portion that becomes a hard segment.

[0095] The manifestation of the above-mentioned effect can be presumed as follows: By using an acrylic resin having both a soft segment and a hard segment, such as the above-mentioned (meth)acrylic acid ester copolymer, the hard segment contributes to heat resistance, and the soft segment contributes to toughness or flexibility, so that a first adhesive layer having good heat resistance, toughness, and flexibility can be obtained.

[0096] At least one of the first polymer portion and the second polymer portion contained in the (meth)acrylic acid ester copolymer has compatibility with epoxy resins. When the first polymer portion has compatibility with epoxy resins, flexibility can be increased. Furthermore, when the second polymer portion has compatibility with epoxy resins, cohesion and toughness can be increased.

[0097] When either the first polymer portion or the second polymer portion is incompatible with the epoxy resin, the (meth)acrylic acid ester copolymer has a compatible portion, which is a polymer portion that is compatible with the epoxy resin, and an incompatible portion, which is a polymer portion that is incompatible with the epoxy resin. In this case, when the (meth)acrylic acid ester copolymer is added to an adhesive composition, the compatible portion is compatible with the epoxy resin, and the incompatible portion is incompatible with the epoxy resin, causing fine phase separation. As a result, a fine sea-island structure is formed. The sea-island structure varies depending on the type of (meth)acrylic acid ester copolymer, the compatibility of the first polymer portion and the second polymer portion contained in the (meth)acrylic acid ester copolymer, and whether or not modification by introduction of polar groups has been performed, and examples include a sea-island structure in which the compatible portions of the cured epoxy resin and the (meth)acrylic acid ester copolymer are the sea and the incompatible portions of the (meth)acrylic acid ester copolymer are the islands, a sea-island structure in which the incompatible portions of the (meth)acrylic acid ester copolymer are the sea and the compatible portions of the cured epoxy resin and the (meth)acrylic acid ester copolymer are the islands, and a sea-island structure in which the (meth)acrylic acid ester copolymer is the sea and the cured epoxy resin is the islands. The presence of such a sea-island structure makes it easier to disperse stress, thereby preventing interfacial failure and achieving excellent adhesion after foaming and curing.

[0098] The (meth)acrylic acid ester copolymer is preferably a block copolymer, and particularly preferably an A-B-A block copolymer in which a compatible portion is polymer block A and an incompatible portion is polymer block B. Furthermore, an A-B-A block copolymer in which a first polymer portion is an incompatible portion and a second polymer portion is a compatible portion, with the first polymer portion being polymer block B and the second polymer portion being polymer block A, is preferred. By using such an A-B-A block copolymer as the acrylic resin, in a case where a sea-island structure is formed in which the compatible portion of the cured epoxy resin and the (meth)acrylic acid ester copolymer is a sea and the incompatible portion of the (meth)acrylic acid ester copolymer is an island, the island portions can be made smaller. Furthermore, in a case where a sea-island structure is formed in which the incompatible portion of the (meth)acrylic acid ester copolymer is a sea and the compatible portion of the cured epoxy resin and the (meth)acrylic acid ester copolymer is an island, or in a case where the (meth)acrylic acid ester copolymer is a sea and the cured epoxy resin is an island, the sea portions can be made smaller.

[0099] The (meth)acrylic acid ester copolymer may be a modified product in which the above-mentioned polar group is introduced into a part of the first polymer segment or the second polymer segment.

[0100] The Tg of the first polymer portion contained in the (meth)acrylic acid ester copolymer is 10°C or lower, and may be in the range of -150°C or higher and 10°C or lower, -130°C or higher and 0°C or lower, or -110°C or higher and -10°C or lower.

[0101] The Tg of the first polymer portion is calculated using the following formula based on the Tg(K) of each homopolymer described in "POLYMER HANDBOOK, Third Edition" (published by John Wiley & Sons, Inc.): 1 / Tg(K)=W 1 / Tg 1 +W 2 / Tg 2 +...+W n / Tg n W n : mass fraction of each monomer Tg n: Tg (K) of the homopolymer of each monomer, and publicly available values ​​such as those in the Polymer Handbook (3rd Ed., J. Brandrup and E. H. Immergut, Wiley Interscience) may be used. The same applies to the Tg of the second polymer portion described below.

[0102] The first polymer portion contained in the (meth)acrylic acid ester copolymer may be either a homopolymer or a copolymer, but is preferably a homopolymer. The monomer component and polymer component constituting the first polymer portion may be any monomer component and polymer component that can give a first polymer portion having a Tg within a predetermined range, and examples thereof include acrylate monomers such as butyl acrylate, 2-ethylhexyl acrylate, isononyl acrylate, and methyl acrylate, other monomers such as vinyl acetate, acetal, and urethane, polar group-containing monomers containing the above-mentioned polar groups, and copolymers such as EVA.

[0103] The Tg of the second polymer portion contained in the (meth)acrylic acid ester copolymer is 20°C or higher, and may be in the range of 20°C or higher and 150°C or lower, 30°C or higher and 150°C or lower, or 40°C or higher and 150°C or lower.

[0104] The second polymer portion contained in the (meth)acrylic acid ester copolymer may be either a homopolymer or a copolymer, but is preferably a homopolymer. The monomer component constituting the second polymer portion may be any monomer component capable of obtaining a second polymer portion having a Tg within a predetermined range, and examples thereof include acrylic acid ester monomers such as methyl methacrylate, other monomers such as acrylamide, styrene, vinyl chloride, amide, acrylonitrile, cellulose acetate, phenol, urethane, vinylidene chloride, methylene chloride, and methacrylonitrile, and polar group-containing monomers containing the above-mentioned polar groups.

[0105] A specific example of the (meth)acrylic acid ester copolymer having the first polymer portion and the second polymer portion is the above-mentioned MMA-BA-MMA copolymer.

[0106] The content of the acrylic resin, relative to 100 parts by mass of the resin component contained in the first adhesive layer, may be, for example, 1 part by mass or more, 3 parts by mass or more, 5 parts by mass or more, 7 parts by mass or more, or 10 parts by mass or more. If the content of the acrylic resin is too low, the adhesion of the first adhesive layer to the substrate and the adhesion after foaming and curing may be reduced. On the other hand, the content of the acrylic resin, relative to 100 parts by mass of the resin component contained in the first adhesive layer, may be, for example, 60 parts by mass or less, 50 parts by mass or less, 40 parts by mass or less, 35 parts by mass or less, or 30 parts by mass or less. If the content of the acrylic resin is too high, the contents of the first epoxy resin and the second epoxy resin may be relatively low, which may make it difficult to balance blocking resistance, adhesion of the first adhesive layer to the substrate, and adhesion after foaming and curing.

[0107] (iii) Curing Agent The curing agent in the present disclosure is appropriately selected depending on the type of the first curing adhesive. When the first curing adhesive is, for example, an epoxy resin adhesive, a curing agent generally used in epoxy resin adhesives can be used as the curing agent. The curing agent is preferably solid at 23°C. A curing agent that is solid at 23°C can extend storage stability (pot life) compared to a curing agent that is liquid at 23°C. The curing agent may also be a latent curing agent. The curing agent may also be a curing agent that undergoes a curing reaction due to heat or a curing agent that undergoes a curing reaction due to light. The curing agents may be used alone or in combination of two or more types.

[0108] The reaction initiation temperature of the curing agent is, for example, 110°C or higher, and may be 130°C or higher. If the reaction initiation temperature is too low, the reaction will start early, and curing will occur with low flexibility and fluidity of the resin component, making it difficult to achieve uniform curing. On the other hand, the reaction initiation temperature of the curing agent is, for example, 200°C or lower. If the reaction initiation temperature is too high, the resin component may deteriorate. Note that when a highly heat-resistant resin such as a phenolic resin is used in addition to the epoxy resin, the resin component will deteriorate less, and the reaction initiation temperature of the curing agent may be, for example, 300°C or lower. The reaction initiation temperature of the curing agent can be determined by differential scanning calorimetry (DSC).

[0109] Specific examples of the curing agent include imidazole-based curing agents, phenol-based curing agents, amine-based curing agents, acid anhydride-based curing agents, isocyanate-based curing agents, and thiol-based curing agents.

[0110] Examples of imidazole-based curing agents include imidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-isopropylimidazole, 2-phenylimidazole, carboxylic acid salts of imidazole compounds, and adducts with epoxy compounds. Furthermore, it is preferable that the imidazole-based curing agent has a hydroxyl group. Crystallization occurs due to hydrogen bonding between the hydroxy groups, so the reaction initiation temperature tends to be high.

[0111] Examples of phenolic curing agents include phenolic resins. Further, examples of phenolic resins include resol-type phenolic resins and novolac-type phenolic resins. From the viewpoint of adhesion of the first adhesive layer to the substrate, phenolic-type novolac resins having a Tg of 110°C or less are particularly preferred. Furthermore, phenolic curing agents and imidazole-type curing agents may be used in combination. In this case, it is preferable to use an imidazole-type curing agent as a curing catalyst.

[0112] The phenolic resin is preferably a biphenyl type from the viewpoint of heat resistance. The phenolic resin may also be a resin in which the phenol nucleus is modified. By modifying the phenol nucleus, for example, it is possible to further improve heat resistance.

[0113] Examples of amine-based curing agents include aliphatic amines, aromatic amines, alicyclic amines, and polyamidoamines. Examples of aliphatic amines include diethylenetriamine (DETA), triethylenetetramine (TETA), and metaxylylenediamine (MXDA). Examples of aromatic amines include diaminodiphenylmethane (DDM), m-phenylenediamine (MPDA), and diaminodiphenylsulfone (DDS). In addition, examples of amine-based curing agents that can be used include dicyandiamide-based curing agents such as dicyandiamide (DICY), organic acid dihydrazide-based curing agents, amine adduct-based curing agents, and ketimine-based curing agents.

[0114] Examples of acid anhydride curing agents include alicyclic acid anhydrides (liquid acid anhydrides) and aromatic acid anhydrides. Examples of alicyclic acid anhydrides (liquid acid anhydrides) include hexahydrophthalic anhydride (HHPA) and methyltetrahydrophthalic anhydride (MTHPA). Examples of aromatic acid anhydrides include trimellitic anhydride (TMA), pyromellitic anhydride (PMDA), and benzophenonetetracarboxylic dianhydride (BTDA).

[0115] The isocyanate curing agent may, for example, be a blocked isocyanate.

[0116] Examples of thiol-based curing agents include ester-bonded thiol compounds, aliphatic ether-bonded thiol compounds, and aromatic ether-bonded thiol compounds.

[0117] The content of the curing agent is, for example, 1 part by mass or more and 40 parts by mass or less, based on 100 parts by mass of the resin component contained in the first adhesive layer. For example, when an imidazole-based curing agent is used as the main component of the curing agent, the content of the curing agent is preferably, for example, 1 part by mass or more and 15 parts by mass or less, based on 100 parts by mass of the resin component contained in the first adhesive layer. On the other hand, when a phenol-based curing agent is used as the main component of the curing agent, the content of the curing agent is preferably, for example, 5 parts by mass or more and 40 parts by mass or less, based on 100 parts by mass of the resin component contained in the first adhesive layer. Note that using an imidazole-based curing agent or a phenol-based curing agent as the main component of the curing agent means that the mass proportion of the imidazole-based curing agent or the phenol-based curing agent is the highest in the curing agent.

[0118] (b) Foaming Agent The foaming agent contained in the first adhesive layer of the present disclosure may be a foaming agent generally used in adhesive layers of adhesive sheets. The foaming agent may be a foaming agent that undergoes a foaming reaction when exposed to heat or when exposed to light.

[0119] The foaming initiation temperature of the foaming agent is preferably equal to or higher than the softening temperature of the base of the curable adhesive, such as an epoxy resin, and equal to or lower than the activation temperature of the curing reaction of the base of the curable adhesive, such as an epoxy resin. The foaming initiation temperature of the foaming agent is, for example, 70°C or higher, and may be 100°C or higher. If the foaming initiation temperature is too low, the reaction may start early, causing foaming to occur in a state where the flexibility and fluidity of the resin component are low, making it difficult to achieve uniform foaming. On the other hand, the foaming initiation temperature of the foaming agent is, for example, 210°C or lower. If the foaming initiation temperature is too high, the resin component may deteriorate.

[0120] The softening temperature of the base resin of the curable adhesive such as epoxy resin is measured by the ring and ball method specified in JIS K7234:1986.

[0121] Examples of the blowing agent include organic blowing agents and inorganic blowing agents. Examples of the organic blowing agent include azo blowing agents such as azodicarbonamide (ADCA), azobisformamide, and azobisisobutyronitrile, fluorinated alkane blowing agents such as trichloromonofluoromethane, hydrazine blowing agents such as paratoluenesulfonylhydrazide, semicarbazide blowing agents such as p-toluenesulfonylsemicarbazide, triazole blowing agents such as 5-morpholyl-1,2,3,4-thiatriazole, and N-nitroso blowing agents such as N,N-dinitrosoterephthalamide. On the other hand, examples of the inorganic blowing agent include ammonium carbonate, ammonium bicarbonate, ammonium nitrite, ammonium borohydride, and azides.

[0122] Alternatively, a microcapsule type foaming agent may be used as the foaming agent. The microcapsule type foaming agent preferably has a core made of a thermal expansion agent such as hydrocarbon and a shell made of a resin such as acrylonitrile copolymer.

[0123] The average particle size of the foaming agent may be, for example, 7 μm or more, 10 μm or more, 13 μm or more, or 17 μm or more. On the other hand, the average particle size of the foaming agent is preferably equal to or less than the average thickness of the first adhesive layer, and may be, for example, 44 μm or less, 30 μm or less, or 24 μm or less.

[0124] The average particle size of the foaming agent is the particle size at 50% of the cumulative value in the particle size distribution determined by laser diffraction scattering. To measure the average particle size of the foaming agent, the first adhesive layer is dissolved in a solvent to separate the foaming agent. The solvent is not particularly limited as long as it can dissolve components other than the foaming agent contained in the first adhesive layer. It is appropriately selected depending on the type of first curable adhesive contained in the first adhesive layer. For example, a solvent used in the adhesive composition used to form the first adhesive layer can be used. Specifically, methyl ethyl ketone, ethyl acetate, toluene, etc. can be used.

[0125] The content of the foaming agent may be, for example, 0.5 parts by mass or more, 2 parts by mass or more, 3 parts by mass or more, 4 parts by mass or more, or 5 parts by mass or more, based on 100 parts by mass of the resin component contained in the first adhesive layer. On the other hand, the content of the foaming agent may be, for example, 25 parts by mass or less, 20 parts by mass or less, or 15 parts by mass or less, based on 100 parts by mass of the resin component contained in the first adhesive layer. If the content of the foaming agent is too low, the expansion ratio of the first adhesive layer will be small, which may not be able to sufficiently fill the gap between the two components, resulting in reduced adhesive strength after foaming and curing. On the other hand, if the content of the foaming agent is too high, the content of the first curable adhesive will be relatively low, which may result in reduced cohesive strength and reduced adhesive strength after foaming and curing.

[0126] (c) Other Components In the present disclosure, for example, when the first curable adhesive is an epoxy resin adhesive, the first adhesive layer may contain only an epoxy resin and an acrylic resin as resin components, or may further contain other resins such as urethane resins.

[0127] The total ratio of the first epoxy resin, the second epoxy resin and the acrylic resin to the resin components contained in the first adhesive layer is, for example, 70% by mass or more, or may be 80% by mass or more, or 90% by mass or more, or may be 100% by mass.

[0128] The content of the resin component contained in the first adhesive layer is, for example, 60% by mass or more, or may be 70% by mass or more, or 80% by mass or more, or may be 90% by mass or more.

[0129] The first adhesive layer may contain, as needed, for example, a silane coupling agent, a filler, an antioxidant, a light stabilizer, an ultraviolet absorber, a lubricant, a plasticizer, an antistatic agent, a crosslinking agent, and a colorant. Examples of the silane coupling agent include epoxy-based silane coupling agents. Examples of the filler include inorganic fillers such as calcium carbonate, aluminum hydroxide, magnesium hydroxide, antimony trioxide, zinc borate, molybdenum compounds, and titanium dioxide. Examples of the antioxidant include phenol-based antioxidants and sulfur-based antioxidants.

[0130] (3) Configuration of the First Adhesive Layer The thickness of the first adhesive layer is not particularly limited, but is preferably equal to or greater than the average particle size of the foaming agent. The thickness of the first adhesive layer is, for example, 10 μm or more, or may be 15 μm or more, or may be 20 μm or more. If the first adhesive layer is too thin, it may be difficult to obtain sufficient adhesion to the substrate and adhesion after foaming and curing. On the other hand, the thickness of the first adhesive layer is, for example, 200 μm or less, or may be 150 μm or less, or may be 100 μm or less. If the first adhesive layer is too thick, the surface quality may be deteriorated.

[0131] Here, the thickness of the first adhesive layer is a value measured from a cross section of the adhesive sheet in the thickness direction as observed with a transmission electron microscope (TEM), a scanning electron microscope (SEM), or a scanning transmission electron microscope (STEM), and is the average value of the thicknesses at 10 randomly selected locations. The same method for measuring the average thickness of other layers of the foamable adhesive sheet applies.

[0132] The first adhesive layer can be foamed at an expansion ratio of, for example, 1.5 times or more and 15 times or less. The expansion ratio may be, for example, 3.5 times or more, 4 times or more, or 4.5 times or more. The expansion ratio may be, for example, 9 times or less, 8.5 times or less, or 8 times or less. If the expansion ratio is too small, the gap between the two components may not be sufficiently filled, and the adhesiveness after foaming and curing may be reduced. If the expansion ratio is too large, the porosity of the first adhesive layer after foaming and curing may be large, which may reduce the adhesiveness after foaming and curing.

[0133] Here, the expansion ratio is calculated by the following formula: Expansion ratio (times) = thickness of the first adhesive layer after foaming and curing / thickness of the first adhesive layer before foaming and curing

[0134] The first adhesive layer may be a continuous layer or a discontinuous layer. Examples of discontinuous layers include stripes and dots. The surface of the first adhesive layer may have an uneven shape such as an embossed shape.

[0135] The first adhesive layer can be formed, for example, by applying an adhesive composition containing the first curable adhesive and a foaming agent, etc., followed by removing the solvent. Examples of application methods include roll coating, reverse roll coating, transfer roll coating, gravure coating, gravure reverse coating, comma coating, rod coating, blade coating, bar coating, wire bar coating, die coating, lip coating, and dip coating.

[0136] The adhesive composition may or may not contain a solvent. In this specification, the term "solvent" is used in a broad sense to include not only a strict solvent (a solvent that dissolves a solute) but also a dispersion medium. The solvent contained in the adhesive composition is volatilized and removed when the adhesive composition is applied and dried to form the first adhesive layer.

[0137] The adhesive composition can be obtained by mixing the above-mentioned components and, if necessary, kneading and dispersing them. As a mixing and dispersing method, a general kneading disperser, such as a two-roll mill, a three-roll mill, a pebble mill, a tron ​​mill, a Szegvari attritor, a high-speed impeller disperser, a high-speed stone mill, a high-speed impact mill, a desper, a high-speed mixer, a ribbon blender, a co-kneader, an intensive mixer, a tumbler, a blender, a desperzer, a homogenizer, or an ultrasonic disperser can be used.

[0138] 3. Second Adhesive Layer The second adhesive layer in the present disclosure is disposed on the surface of the substrate opposite to the first adhesive layer, contains a second curable adhesive, and is substantially free of a foaming agent.

[0139] (1) Physical Properties of the Second Adhesive Layer The second adhesive layer in the present disclosure is preferably substantially non-tacky. The tackiness of the second adhesive layer is the same as that of the first adhesive layer.

[0140] (2) Materials for the Second Adhesive Layer (a) Second Curable Adhesive The second curable adhesive contained in the second adhesive layer in the present disclosure is the same as the first curable adhesive used in the first adhesive layer.

[0141] (b) Other Components The other components contained in the second adhesive layer in the present disclosure are the same as the other components used in the first adhesive layer.

[0142] The second adhesive layer may contain soft particles. When the second adhesive layer contains soft particles, the slope of the approximate line tends to be smaller. Therefore, the slope of the approximate line can be easily adjusted to fall within a predetermined range.

[0143] The soft particles include, for example, hollow particles formed by foaming a foaming agent to have a hollow portion therein. The hollow particles are preferably hollow particles formed by foaming a microcapsule-type foaming agent. The microcapsule-type foaming agent is the same as the microcapsule-type foaming agent used in the first adhesive layer.

[0144] The soft particles may be any flexible non-metallic particles, such as rubber particles and resin particles, including melamine resin particles, acrylic resin particles, acrylic-styrene copolymer particles, polycarbonate particles, polyethylene particles, polystyrene particles, polyvinyl chloride particles, cross-linked urethane resin particles, and silicone resin particles.

[0145] The second adhesive layer is substantially free of a foaming agent. The term "the second adhesive layer is substantially free of a foaming agent" means that the content of the foaming agent in the second adhesive layer is 1% by mass or less. The content of the foaming agent in the second adhesive layer is preferably 0.5% by mass or less, more preferably 0% by mass. The foaming agent is the same as the foaming agent used in the first adhesive layer.

[0146] (3) Structure of the Second Adhesive Layer The thickness of the second adhesive layer is the same as that of the first adhesive layer. If the thickness of the second adhesive layer is too thick, the gap between the two components cannot be filled with the foamable adhesive sheet after foaming and curing, which may reduce the adhesive strength after foaming and curing.

[0147] The second adhesive layer may be a continuous layer or a discontinuous layer. The surface of the second adhesive layer may have an uneven shape such as an embossed shape.

[0148] The method for forming the second adhesive layer is the same as the method for forming the first adhesive layer.

[0149] 4. Substrate The substrate in the present disclosure is, for example, a member that supports the first adhesive layer and the second adhesive layer.

[0150] The substrate in the present disclosure preferably has insulating properties. The substrate is preferably in the form of a sheet. The substrate may have a single-layer structure or a multi-layer structure. The substrate may or may not have a porous structure inside.

[0151] Examples of the substrate include a resin substrate and a nonwoven fabric.

[0152] Examples of resins contained in the resin substrate include polyester resin, polycarbonate, polyarylate, polyurethane, polyamide resin, polyimide resin, polysulfone resin, polyether ketone resin, polyphenylene sulfide (PPS), modified polyphenylene oxide, etc. Examples of polyester resins include polyethylene terephthalate (PET), polybutylene terephthalate, polyethylene naphthalate (PEN), and aromatic polyester. Examples of polyamide resins include polyamide and polyether amide. Examples of polyimide resins include polyimide, polyether imide, and polyamide imide. Examples of polysulfonic acid resins include polysulfone and polyether sulfone. Examples of polyether ketone resins include polyether ketone and polyether ether ketone. Furthermore, liquid crystal polymers (LCPs) may also be used as the resin.

[0153] The glass transition temperature of the resin is, for example, 80° C. or higher, or may be 140° C. or higher, or may be 200° C. or higher.

[0154] Examples of nonwoven fabrics include nonwoven fabrics containing fibers such as cellulose fibers, polyester fibers, nylon fibers, aramid fibers, polyphenylene sulfide fibers, liquid crystal polymer fibers, glass fibers, metal fibers, and carbon fibers.

[0155] The substrate may be surface-treated to enhance adhesion to the first adhesive layer or the second adhesive layer.

[0156] The thickness of the substrate is not particularly limited and may be, for example, 2 μm or more, 5 μm or more, or 9 μm or more, and may be, for example, 200 μm or less, 100 μm or less, or 50 μm or less.

[0157] 5. First Intermediate Layer and Second Intermediate Layer The foamable adhesive sheet of the present disclosure may have a first intermediate layer between the substrate and the first adhesive layer. The foamable adhesive sheet of the present disclosure may also have a second intermediate layer between the substrate and the second adhesive layer. The presence of the first intermediate layer or second intermediate layer can improve the adhesion of the first adhesive layer or second adhesive layer to the substrate. Furthermore, the presence of the first intermediate layer or second intermediate layer can, for example, reduce stress at the bent portion when the foamable adhesive sheet is folded, or reduce stress at the cut portion when the foamable adhesive sheet is cut. As a result, lifting or peeling of the first adhesive layer or second adhesive layer from the substrate can be suppressed when the foamable adhesive sheet is bent or cut.

[0158] For example, in the foamable adhesive sheet 10 shown in Fig. 7, a first intermediate layer 4 is disposed between the substrate 2 and the first adhesive layer 1, and a second intermediate layer 5 is disposed between the substrate 2 and the second adhesive layer 3. Although the foamable adhesive sheet 10 in Fig. 7 has both the first intermediate layer 4 and the second intermediate layer 5, it may have only one of them.

[0159] The foamable adhesive sheet may have at least one of a first intermediate layer and a second intermediate layer; for example, it may have only the first intermediate layer arranged between the substrate and the first adhesive layer, or it may have only the second intermediate layer arranged between the substrate and the second adhesive layer, or it may have both the first intermediate layer arranged between the substrate and the first adhesive layer and the second intermediate layer arranged between the substrate and the second adhesive layer.

[0160] The materials contained in the first intermediate layer and the second intermediate layer are not particularly limited as long as they can increase the adhesion between the substrate and the first adhesive layer or the second adhesive layer and can relieve stress, and are appropriately selected depending on the materials of the substrate, the first adhesive layer, and the second adhesive layer, etc. Examples include polyester, polyvinyl chloride, polyvinyl acetate, polyurethane, polymers obtained by copolymerizing at least two or more of these, crosslinked products thereof, and mixtures thereof.

[0161] The crosslinked product is a crosslinked product obtained by crosslinking the above-mentioned resin with a curing agent. Examples of the curing agent include an isocyanate-based curing agent. Furthermore, for example, when the reactive group / NCO equivalent is 1, it is preferable to add the isocyanate-based curing agent in a ratio of 0.5 mass % to 20 mass % relative to the resin.

[0162] In particular, the first intermediate layer and the second intermediate layer preferably contain a crosslinked resin. Note that a crosslinked resin is one that does not melt even at high temperatures. This improves adhesive strength at high temperatures, i.e., heat resistance.

[0163] The thickness of the first intermediate layer and the second intermediate layer is not particularly limited, but may be, for example, 0.1 μm or more, 0.5 μm or more, or 1 μm or more. If the first intermediate layer or the second intermediate layer is too thin, the effect of suppressing peeling of the first adhesive layer or the second adhesive layer from the substrate when the foamable adhesive sheet is bent or cut may not be sufficiently obtained. On the other hand, the thickness of the first intermediate layer and the second intermediate layer may be, for example, 4 μm or less, or 3.5 μm or less. Since the first intermediate layer and the second intermediate layer themselves usually do not have high heat resistance, if the first intermediate layer or the second intermediate layer is too thick, heat resistance (adhesive strength at high temperatures) may be reduced.

[0164] The first intermediate layer and the second intermediate layer can be formed, for example, by applying a resin composition and removing the solvent. Examples of application methods include roll coating, reverse roll coating, transfer roll coating, gravure coating, gravure reverse coating, comma coating, rod coating, blade coating, bar coating, wire bar coating, die coating, lip coating, and dip coating.

[0165] 7. Foamable Adhesive Sheet The thickness of the foamable adhesive sheet according to the present disclosure is, for example, 10 μm or more, and may be 20 μm or more. On the other hand, the thickness of the foamable adhesive sheet is, for example, 1000 μm or less, and may be 200 μm or less.

[0166] The use of the foamable adhesive sheet of the present disclosure is not particularly limited. The foamable adhesive sheet of the present disclosure can be used, for example, when placing the foamable adhesive sheet between two components, foaming and curing the first adhesive layer of the foamable adhesive sheet, and curing the second adhesive layer to bond the two components. Specifically, the foamable adhesive sheet of the present disclosure is used to bond the stator core and coil in a stator that constitutes a motor.

[0167] The method for producing the foamable adhesive sheet of the present disclosure is not particularly limited, and may be appropriately selected depending on the layer structure of the foamable adhesive sheet.

[0168] B. Article Manufacturing Method The article manufacturing method according to the present disclosure includes a disposing step of disposing the foamable adhesive sheet described above between a first member and a second member, and a bonding step of foaming and curing the foamable adhesive sheet to bond the first member and the second member together.

[0169] 8(a) and 8(b) are process diagrams showing an example of a method for manufacturing an article according to the present disclosure. First, as shown in FIG. 8(a), a foamable adhesive sheet 10 is placed between a first member 20a and a second member 20b. Next, as shown in FIG. 8(b), the first adhesive layer of the foamable adhesive sheet 10 is foamed and cured by heating or the like, and the second adhesive layer is cured. The foamed and cured adhesive sheet 11 adheres (bonds) the first member 20a and the second member 20b to each other. This results in an article 100 in which the adhesive sheet 11 is placed between the first member 20a and the second member 20b.

[0170] The method for manufacturing the article according to the present disclosure will now be described.

[0171] 1. Foamable Adhesive Sheet The foamable adhesive sheet used in the method for producing an article according to the present disclosure is the same as the foamable adhesive sheet described above.

[0172] 2. Placement Step In the placement step of the present disclosure, the method for placing the adhesive sheet between the first member and the second member is not particularly limited. Examples include a method of inserting a foam adhesive sheet into the gap between the first member and the second member, a method of placing a foam adhesive sheet in a hole or groove in the first member and then inserting the second member into the gap after placing the foam adhesive sheet in the hole or groove in the first member, and a method of inserting the second member with the foam adhesive sheet placed in it into the hole or groove in the first member.

[0173] The material and shape of the first and second members are not particularly limited and may be appropriately selected depending on the intended use. Examples of the first and second members include a stator core and a coil in a stator that constitutes a motor.

[0174] 3. Bonding Step In the bonding step of the present disclosure, examples of methods for foaming and curing the first adhesive layer and the second adhesive layer of the foamable adhesive sheet include heating and light irradiation. Among these, it is preferable to foam and cure the first adhesive layer and cure the second adhesive layer by heating. Heating methods are also applicable even when the first and second members are not transparent, such as when the members are made of metal.

[0175] The heating conditions are appropriately set depending on the types of the first curable adhesive and foaming agent contained in the first adhesive layer, the type of the second curable adhesive contained in the second adhesive layer, the type of substrate, etc. The heating temperature is, for example, 130° C. or higher and 200° C. or lower. The heating time is, for example, 3 minutes or higher and 3 hours or lower.

[0176] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and any configuration that is substantially identical to the technical idea described in the claims of the present disclosure and that provides similar effects is included within the technical scope of the present disclosure.

[0177] [Materials] The components used in the adhesive composition are shown below.・Epoxy resin A: bisphenol A phenoxy type, solid at room temperature, epoxy equivalent: 7500 to 8500 g / eq, Mw 50,000, bifunctional ・Epoxy resin B: bisphenol A type, solid at room temperature, epoxy equivalent: 2400 to 3300 g / eq, softening temperature 144°C, Mw 3,800, bifunctional ・Epoxy resin C: bisphenol A novolac type, solid at room temperature, epoxy equivalent 200 to 220 g / eq, softening temperature 70°C, multifunctional ・Acrylic resin: PMMA-PBuA-PMMA (partially contains acrylamide groups), Tg -20°C, 120°C, Mw 150,000 ・Curing agent: α-(hydroxy (or dihydroxy) phenylmethyl)-ω-hydropoly[biphenyl-4,4'-diylmethylene (hydroxy (or dihydroxy) phenylenemethylene)] Curing catalyst: 2-phenyl-4,5-dihydroxymethylimidazole, average particle size: 3 μm, melting point: 230°C, reaction start temperature 145°C to 155°C, active region 155°C to 173°C) Foaming agent: thermally expandable microcapsules, average particle size 10 μm to 16 μm, expansion start temperature 123°C to 133°C, maximum expansion temperature 168°C to 178°C, core: hydrocarbon, shell: thermoplastic polymer Hollow particles: microballoons formed by expanding thermally expandable microcapsules, average particle size 15 μm to 25 μm Solvent: methyl ethyl ketone

[0178] [Examples 1 to 6, Comparative Example 1] A polyethylene naphthalate (PEN) film (thickness: 100 μm) was used as the substrate. A polyester polymer and a curing agent (polyisocyanate) were diluted with methyl ethyl ketone (MEK) to a solids content of 15% by mass to prepare a resin composition. The resin composition was applied to one side of the substrate using a bar coater and dried in an oven at 100°C for 1 minute to form a first intermediate layer. A second intermediate layer was then formed on the other side of the substrate in the same manner as the first intermediate layer.

[0179] Next, the adhesive composition shown in Table 1 below was applied to the surface of the first intermediate layer opposite the substrate using an applicator so that the thickness after application was 58 μm. This was then dried in an oven at 100°C for 3 minutes to form a first adhesive layer. Furthermore, the adhesive composition shown in Table 1 below was applied to the surface of the second intermediate layer opposite the substrate using an applicator so that the thickness after application was 48 μm. This was then dried in an oven at 100°C for 3 minutes to form a second adhesive layer. This resulted in a foamable adhesive sheet in which the first adhesive layer, first intermediate layer, substrate, second intermediate layer, and second adhesive layer were arranged in this order.

[0180] [Evaluation] (1) Shear adhesive strength test method (1-1) First adhesive layer after foaming and curing An adhesive composition shown in Table 1 below was applied to a 38 μm thick silicone-treated polyethylene terephthalate (PET) separator using an applicator so that the thickness after application was 58 μm. The composition was then dried in an oven at 100° C. for 3 minutes to form a single first adhesive layer.

[0181] The first adhesive layer after foaming and curing was subjected to the shear bond strength test method described above in the section "A. Foamable Adhesive Sheet 1. Physical Properties of Foamable Adhesive Sheet" to measure the shear bond strength. The slope of the approximate line in the stress-strain curve from 3% strain to 5% strain was also determined. In the shear bond strength test method, the spacer thickness was 180 μm. The foaming and curing conditions were 160°C and 8.5 minutes (3.5 minutes for temperature increase and 5 minutes for hold) using a heat press.

[0182] (1-2) Second adhesive layer after curing An adhesive composition shown in Table 1 below was applied to a 38 μm thick silicone-treated polyethylene terephthalate (PET) separator using an applicator so that the thickness after application was 48 μm. The composition was then dried in an oven at 100° C. for 3 minutes to form a single second adhesive layer.

[0183] The shear adhesive strength of the cured second adhesive layer was measured using the shear adhesive strength test method described above in "A. Foamable Adhesive Sheet 1. Physical Properties of the Foamable Adhesive Sheet." The slope of the approximate line in the stress-strain curve from 3% strain to 5% strain was also determined. In the shear adhesive strength test method, the spacer thickness was 35 μm. The curing conditions were 160°C and 8.5 minutes (3.5 minutes for temperature increase and 5 minutes for hold) using a heat press.

[0184] (1-3) Foamable adhesive sheet after foaming and curing The foamable adhesive sheet after foaming and curing was subjected to the shear bond strength test method as described above in the section "A. Foamable adhesive sheet 1. Physical properties of foamable adhesive sheet" to measure the shear bond strength. The fracture surface of the test piece was also visually observed. In the shear bond strength test method, the spacer thickness was 338 μm. The foaming and curing conditions were 160°C and 8.5 minutes (3.5 minutes for temperature increase, 5 minutes for holding) using a heat press.

[0185] (2) Adhesion A cross-cut test in accordance with JIS K5600-5-6:1999 was performed three times on the surface of the second adhesive layer of the foamable adhesive sheet after foaming and curing, and the number of peeled squares was counted. The cut interval was 1 mm. The tape used was Nitto Denko Corporation's adhesive tape No. 31B. The tape peeling conditions were a peeling speed of 3 m / s or more and 5 m / s or less, and a peeling angle of approximately 60°.

[0186]

[0187]

[0188] In Examples 1 to 6, the slope of the approximated line in the stress-strain curve for the cured second adhesive layer was within a predetermined range, and the fracture mode was cohesive failure of the first adhesive layer, so the adhesion of the cured second adhesive layer to the substrate was good. On the other hand, in Comparative Example 1, the slope of the approximated line in the stress-strain curve for the cured second adhesive layer was large, so the adhesion of the cured second adhesive layer to the substrate was poor.

[0189] The present disclosure provides the following [1] to [3]: [1] A foamable adhesive sheet having, in this order, a first adhesive layer, a substrate, and a second adhesive layer, wherein the first adhesive layer contains a first curable adhesive and a foaming agent, and the second adhesive layer contains a second curable adhesive but no foaming agent, wherein, when the foamable adhesive sheet after foaming and curing is subjected to a tensile shear adhesive strength test method, the failure mode is cohesive failure of the first adhesive layer after foaming and curing, and when the second adhesive layer after curing is subjected to a tensile shear adhesive strength test method, the slope of the approximation line in the section from 3% strain to 5% strain in the stress-strain curve obtained is 0.20 MPa or less. [2] The foamable adhesive sheet according to [1], wherein the difference between the slope of the approximate straight line in the section from 3% to 5% strain in a stress-strain curve obtained when the first adhesive layer after foaming and curing is subjected to a tensile shear bond strength test method and the slope of the approximate straight line in the section from 3% to 5% strain in a stress-strain curve obtained when the second adhesive layer after curing is subjected to a tensile shear bond strength test method is 0.20 MPa or less. [3] A method for manufacturing an article, comprising: a positioning step of positioning the foamable adhesive sheet according to [1] or [2] between a first member and a second member; and a bonding step of foaming and curing the foamable adhesive sheet, and bonding the first member and the second member.

[0190] REFERENCE SIGNS LIST 1... first adhesive layer 2... substrate 3... second adhesive layer 4... first intermediate layer 5... second intermediate layer 10... foamable adhesive sheet 11... adhesive sheet 20a... first member 20b... second member 100... article

Claims

1. A foamable adhesive sheet having a first adhesive layer, a substrate, and a second adhesive layer in that order, wherein the first adhesive layer contains a first curable adhesive and a foaming agent, and the second adhesive layer contains a second curable adhesive and no foaming agent, and when a tensile shear adhesive strength test method is performed on the foamable adhesive sheet after foaming and curing, the failure mode is cohesive failure of the first adhesive layer after foaming and curing, and when a tensile shear adhesive strength test method is performed on the second adhesive layer after curing, the slope of the approximation line in the section from 3% strain to 5% strain in a stress-strain curve obtained is 0.20 MPa or less.

2. A foamable adhesive sheet as described in claim 1, wherein the difference between the slope of the approximation line in the section from 3% strain to 5% strain in the stress-strain curve obtained when the tensile shear adhesive strength test method is performed on the first adhesive layer after foaming and curing, and the slope of the approximation line in the section from 3% strain to 5% strain in the stress-strain curve obtained when the tensile shear adhesive strength test method is performed on the second adhesive layer after curing, is 0.20 MPa or less.

3. A method for manufacturing an article, comprising: a step of placing the foamable adhesive sheet according to claim 1 or 2 between a first member and a second member; and a step of foaming and curing the foamable adhesive sheet to bond the first member and the second member.

Citation Information

Patent Citations

  • Heating expansion sheet

    JP2022178658A

  • Foamable adhesive sheet and method for manufacturing article

    JP2023052744A

  • Adhesive tape, article, motor, and method for producing article

    WO2015190235A1