Film for lid material

The laminate film structure with a polyethylene base and ethylene/α-olefin copolymer sealant layer addresses the adhesion and recyclability challenges of packaging materials, providing strong adhesion and recyclability for plastic containers.

WO2024237250A1PCT designated stage expired Publication Date: 2024-11-21TOSOH CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017781
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-04-26
Filing Date
2024-05-14
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Packaging materials composed of different types of resin films face challenges in recyclability and adhesion to plastic containers such as polyethylene terephthalate, polystyrene, polypropylene, and polyvinyl chloride, leading to insufficient adhesion and limited recycling options.

Method used

A laminate film structure with a polyethylene base material and an ethylene/α-olefin copolymer-based sealant layer, incorporating a tackifier and low-density polyethylene, which enhances adhesion and recyclability by optimizing molecular weight, density, and melt flow rate, ensuring excellent adhesive properties and recyclability.

Benefits of technology

The film achieves strong adhesion to various plastic containers while maintaining high recyclability, making it suitable for applications like lidding materials for polyethylene terephthalate, polystyrene, polypropylene, and polyvinyl chloride containers, and supports material recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

Provided is a film for a lid material, the film having high recyclability and excellent adhesiveness to a plastic container. The film for a lid material is a laminate comprising a base material and a sealant layer, wherein the base material is a stretched film composed of polyethylene, and the sealant layer is configured from a resin composition comprising 80-97 parts by weight of an ethylene / α-olefin copolymer (A) having a density of 880-910 kg / m3 and 3-20 parts by weight of a tackifier (B).
Need to check novelty before this filing date? Find Prior Art

Description

Lidding film

[0001] The present invention relates to a film for use as a covering material.

[0002] Traditionally, polypropylene and polystyrene have been used for packaging food, beverages, pharmaceuticals, industrial parts, etc.

[0003] Plastic containers such as polyethylene terephthalate and polyvinyl chloride containers, and paper containers mainly made of paper are used, and the lids are made of films that have stable adhesive properties to protect the contents and that have easy-peel properties that allow them to be opened with appropriate strength when peeled off.

[0004] Such a film for a lid material typically comprises a substrate and a sealant layer, and the substrate is typically a resin film such as a polyester film, a polyamide film, or a polypropylene film, which has excellent strength and heat resistance. On the other hand, the sealant layer is typically a resin composition comprising an ethylene-vinyl acetate copolymer, an ethylene-α-olefin copolymer, or the like, and a tackifier, and different types of resin films are used for the substrate and the sealant layer in typical packaging materials (see, for example, Patent Documents 1 to 4).

[0005] In recent years, social issues such as waste plastics have been attracting attention, and along with the increasing demand for building a recycling-oriented society, there is a demand for improving the recyclability of packaging materials. Packaging materials made up of a combination of different types of resin films as described above have the problem that they are difficult to recycle, such as by material recycling or chemical recycling. In response to this problem, packaging materials made up of the same type of resin material have been proposed (see, for example, Patent Documents 5 and 6).

[0006] However, the above-mentioned packaging materials are limited to applications such as standing pouches in which sealant layers of the same film are heat-sealed together, and have insufficient adhesiveness when used as lid material films for plastic containers made of polypropylene, polystyrene, polyethylene terephthalate, polyvinyl chloride, etc. Therefore, there has been a demand for lid material films that can be suitably used for these applications.

[0007] Japanese Patent Application Publication No. 2020-158763

[0008] Japanese Unexamined Patent Publication No. 11-228757 Japanese Unexamined Patent Application No. 10-147672 Japanese Unexamined Patent Application No. 11-269320 Unexamined Japanese Patent Application No. 2022-165191 International Publication No. 2021 / 054349

[0009] The present invention has been made to solve the above problems, and has high recyclability and

[0010] The object of the present invention is to provide a film for lid material that has excellent adhesiveness to plastic containers.

[0011] As a result of extensive research to solve the above problems, the present inventors have discovered a substrate and a system having specific properties.

[0012] The present inventors have found that a film for use as a covering material having a coating layer exhibits excellent recyclability and adhesiveness, and have completed the present invention.

[0013] That is, each aspect of the present invention is the following [1] to

[11] . [1] A laminate comprising a substrate and a sealant layer, wherein the substrate is a stretched film made of polyethylene, and the sealant layer has a density of 880 to 910 kg / m 3and 3 to 20 parts by weight of a tackifier (B) (the total of the ethylene / α-olefin copolymer (A) and the tackifier (B) is 100 parts by weight). [2] The lid material film according to [1] above, wherein the ethylene / α-olefin copolymer (A) contains an α-olefin having 3 to 20 carbon atoms, and has a melt mass flow rate of 0.1 to 25 g / 10 min measured at 190°C under a load of 2.16 kg in accordance with JIS K7210-1. [3] The lid material film according to [1] above or [2] above, wherein the tackifier (B) is an alicyclic saturated hydrocarbon resin having a softening temperature of 105 to 150°C measured by the ring and ball method and a hydrogenation rate of 80% or more to aromatic nuclei. [4] The polyethylene constituting the substrate has a weight average molecular weight (Mw) measured by gel permeation chromatography of 70,000 to 250,000, and the proportion of molecular weights of 10,000 or less is 8% by weight or less, and a density measured according to JIS K6922-1 of 945 to 980 kg / m 3[5] The covering material film according to any one of [1] to [3], wherein the resin composition constituting the sealant layer contains 3 to 20 parts by weight of a low-density polyethylene (C) that satisfies the following requirements (a) and (b) per 100 parts by weight of the ethylene-α-olefin copolymer (A) and the tackifier (B): (a) the melt mass flow rate measured in accordance with JIS K7210-1 at 190°C under a load of 2.16 kg is in the range of 0.3 to 5.0 g / 10 min; and (b) the swell ratio (SR) calculated by dividing the diameter (D) of a strand extruded at a temperature of 235°C and an extrusion rate of 3 g / min using a melt indexer used in JIS K7210-1 by the orifice diameter (D0) of the melt indexer is in the range of 1.7 to 3.0. [6] The film for lids according to any one of [1] to [5], which comprises an intermediate layer between the substrate and the sealant layer, the intermediate layer being polyethylene or an ethylene copolymer. [7] The film for lids according to [6], wherein the thickness (Y) of the sealant layer relative to the sum (X) of the thickness of the substrate and the thickness of the intermediate layer satisfies the relationship (X) ≧ (Y). [8] The film for lids according to any one of [1] to [7], wherein the content of polyethylene resin in the entire lids film is 90% by weight or more. [9] An easy-peel lid comprising the film for lids according to [1].

[10] A method for sealing a container, comprising adhering the lid according to [9] to the opening of a container made of at least one material selected from the group consisting of polyethylene terephthalate, polystyrene, polypropylene, polyvinyl chloride, and polylactic acid.

[11] A packaging container comprising a container having an opening and the lid material described in [9] above that seals the opening, wherein the container is made of at least one member selected from the group consisting of polyethylene terephthalate, polystyrene, polypropylene, polyvinyl chloride, and polylactic acid.

[0014] According to the present invention, in addition to recyclability, adhesion to various types of plastic containers is possible.

[0015] Therefore, it is possible to provide a film for a lid material having excellent adhesiveness.

[0016] The present invention will be described in detail below.

[0017] The covering film according to one embodiment of the present invention is a laminate comprising a substrate and a sealant layer.

[0018] The substrate is polyethylene that has been subjected to a stretching treatment. The stretching treatment can improve the strength and heat resistance of the substrate, and can satisfy the physical properties required for, for example, the outer layer of a packaging material. The stretching may be uniaxial or biaxial.

[0019] The polyethylene used for the substrate desirably has a weight average molecular weight (Mw) measured by gel permeation chromatography of 70,000 to 250,000, preferably 100,000 to 200,000, and more preferably 100,000 to 150,000. Mw of 70,000 or more is preferred because the strength of the resulting substrate is sufficient, while Mw of 250,000 or less is preferred because it provides excellent melt extrudability in material recycling and does not deteriorate the performance of the resulting recycled resin.

[0020] The polyethylene has a molecular weight of 10,000 or less as measured by gel permeation chromatography of 8% by weight or less, preferably 6% by weight or less, and more preferably 4% by weight or less. A ratio of 8% by weight or less is preferred because the stretched film has excellent heat resistance and the heat-sealed appearance of the laminated film is not impaired. This is presumably because the molecular chains are relaxed by molecules with low molecular weight during the stretching process, resulting in insufficient orientation of the polyethylene crystals.

[0021] The polyethylene used for the substrate has a density of 945 to 980 kg / m as measured according to JIS K6922-1 (1997). 3 It is preferable that the density is 945 kg / m 3 In the case of the above, the heat resistance of the polyethylene stretched film is excellent, and the density is preferably 980 kg / m 3 The following polyethylenes are easy to produce industrially:

[0022] Such polyethylene can be obtained by homopolymerizing ethylene or copolymerizing ethylene with a small amount of α-olefin (5 mol % or less). For the polymerization, a Ziegler catalyst consisting of a solid catalyst component containing magnesium and titanium and an organoaluminum compound, a metallocene catalyst consisting of an organic transition metal compound containing a cyclopentadienyl derivative and a compound and / or an organic metal compound that reacts with the organic transition metal compound to form an ionic complex, or a vanadium-based catalyst can be used. Metallocene catalysts and vanadium-based catalysts are preferred because they make it easy to control the proportion of molecular weights of 10,000 or less. The method for producing polyethylene is not particularly limited, but it can be produced by, for example, a slurry method, a solution method, a gas-phase method, or the like. The slurry method or solution method is preferred because it makes it easy to control the proportion of molecular weights of 10,000 or less.

[0023] Furthermore, the polyethylene may contain additives that are usually used in polyolefins, such as antioxidants, lubricants, neutralizing agents, antiblocking agents, surfactants, slip agents, etc., as required.

[0024] The sealant layer has a density of 880 to 910 kg / m 3 and 3 to 20 parts by weight of a tackifier (B) (the total of the ethylene / α-olefin copolymer (A) and the tackifier (B) is 100 parts by weight).

[0025] As the ethylene / α-olefin copolymer (A), any copolymer that falls within the category generally referred to as an ethylene / α-olefin copolymer can be used. While the α-olefin is not particularly limited, those having 3 to 20 carbon atoms are preferred, such as 1-butene, 1-pentene, 1-hexene, 1-octene, 1-heptene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-pentene, and octadecene. Among these α-olefins, 1-hexene, 1-octene, 1-heptene, and 4-methyl-1-pentene are preferred, with 1-hexene being particularly preferred due to its high and stable adhesive strength. These ethylene / α-olefin copolymers (A) can be suitably produced by copolymerizing ethylene and an α-olefin using a Ziegler catalyst, a chromium catalyst, or a metallocene catalyst. Examples of polymerization methods include solution polymerization, high-pressure polymerization, and gas-phase polymerization.

[0026] The ethylene / α-olefin copolymer (A) has excellent low-temperature adhesiveness, and therefore has a density measured in accordance with JIS K6922-1 of 880 to 910 kg / m 3 , preferably 900 to 910 kg / m 3 It is preferable that the density is in the range of 880 kg / m 3 If the density is less than 910 kg / m, the heat resistance of the resin composition will be poor and 3 If it exceeds this value, the adhesiveness of the resulting film for covering material will be poor.

[0027] The ethylene / α-olefin copolymer (A) preferably has a melt mass flow rate (hereinafter sometimes referred to as MFR) in the range of 0.1 to 25 g / 10 min, as measured in accordance with JIS K7210-1 at 190°C under a load of 2.16 kg. Ethylene / α-olefin polymers having a melt mass flow rate in this range are advantageous in that they have excellent formability when producing a film for a covering material.

[0028] Furthermore, since the ethylene / α-olefin copolymer has a small amount of low-molecular-weight components that particularly impair adhesiveness, it is preferable that the ratio (Mw / Mn) of the weight-average molecular weight (Mw) to the number-average molecular weight (Mn) measured by gel permeation chromatography (GPC) be 3 or less.

[0029] Any tackifier (B) can be used as long as it falls within the category of tackifier resins, such as aliphatic hydrocarbon resins, aromatic hydrocarbon resins, aliphatic-aromatic copolymer hydrocarbon resins, alicyclic hydrocarbon resins obtained by hydrogenating aromatic hydrocarbon resins, synthetic terpene hydrocarbon resins having a structure containing aliphatic, alicyclic, and aromatic groups, terpene hydrocarbon resins derived from α,β-pinene in turpentine oil, coumaroindene hydrocarbon resins derived from indene and styrenes in coal tar naphtha, low-molecular-weight styrene resins, and rosin hydrocarbon resins. Among these tackifiers, alicyclic hydrocarbon resins derived from hydrogenated aliphatic hydrocarbon resins and aromatic hydrocarbon resins are preferred because they have excellent dispersibility in the ethylene-α-olefin copolymer, which is the main component, and therefore provide a lid material film with excellent adhesiveness.

[0030] The tackifier (B) preferably has a softening temperature measured by the ring and ball method in the range of 105 to 150°C, more preferably 115 to 140°C. Furthermore, alicyclic hydrocarbons with a hydrogenation rate to aromatic nuclei of 80% or more, preferably 85% or more, are particularly preferred. A softening temperature of 105°C or higher results in a lid material film with excellent adhesiveness, while a softening temperature of 150°C or lower results in stable production without being limited by ambient temperature during production. Furthermore, a hydrogenation rate of 80% or higher results in a lid material film with excellent hygienic properties, making it suitable for use in food applications, etc.

[0031] Commercially available tackifiers can be used as the tackifier (B). Specific examples of alicyclic hydrocarbon resins include (trade names) Arkon P115, Arkon P125, Arkon P140, Arkon M115, and Arkon M135 (all manufactured by Arakawa Chemical Industries, Ltd.), Imave S110 and Imave P125 (all manufactured by Idemitsu Kosan Co., Ltd.), and T-REZ RC115 and T-REZ HA125 (all manufactured by JXTG Nippon Oil & Energy Corporation). Examples of rosin-based resins include Pine Crystal KE-311 (manufactured by Arakawa Chemical Industries, Ltd.). Examples of terpene-based resins include YS Resin PX1150 and YS Resin PX1150N (manufactured by Yasuhara Chemical Co., Ltd.).

[0032] The blending ratio of the ethylene-α-olefin copolymer (A) and the tackifier (B) constituting the sealant layer is as follows: The total of (A) and (B) is 100 parts by weight.

[0033] The blending ratio of the ethylene / α-olefin copolymer (A) is within the range of 80 to 97 parts by weight, preferably 90 to 97 parts by weight. If the blending ratio of (A) is less than 80 parts by weight, the resulting film for covering material will have poor formability, and if it exceeds 97 parts by weight, the resulting film will have poor adhesiveness, which is not preferred.

[0034] The blending ratio of the tackifier (B) is within the range of 3 to 20 parts by weight, and preferably 3 to 10 parts by weight. If the blending ratio of (B) is less than 3 parts by weight, the resulting covering material film will have poor adhesiveness, and if it exceeds 20 parts by weight, the blocking property during molding will be poor, which is not preferred.

[0035] The resin composition constituting the sealant layer may contain a low-density polyethylene (C) in order to further improve moldability.

[0036] The low-density polyethylene (C) is a low-density polyethylene obtained by polymerizing only ethylene using a known high-pressure polymerization method, and has a density of 910 to 940 kg / m as measured in accordance with JIS K6922-1. 3 It is preferable that the range is:

[0037] The low-density polyethylene (C) preferably has a melt mass flow rate, measured in accordance with JIS K7210-1 at 190°C under a load of 2.16 kg, in the range of 0.3 to 5.0 g / 10 min, more preferably 0.5 to 5.0 g / 10 min, and even more preferably 1.0 to 5.0 g / 10 min. A melt mass flow rate of 0.3 g / 10 min or more reduces the extrusion load during processing into a film for a covering material, and a melt mass flow rate of 5.0 g / 10 min or less is preferred because it significantly improves moldability.

[0038] Furthermore, the low-density polyethylene (C) preferably has a swell ratio (SR) in the range of 1.7 to 3.0, more preferably 1.7 to 2.5, and even more preferably 1.9 to 2.5. The inclusion of a low-density polyethylene having an SR in this range in the sealant layer is preferred because it improves molding processability. The SR can be measured by using a melt indexer according to JIS K7210-1, extruding a resin filled in the device through an orifice at a temperature of 235°C and an extrusion rate of 3 g / min, collecting a strand-like extrudate in a measuring cylinder containing isopropanol placed directly below the orifice, and dividing the diameter (D) of the extruded strand by the orifice diameter (D0) of the melt indexer.

[0039] The blending ratio of the low-density polyethylene (C) is preferably within the range of 3 to 20 parts by weight, more preferably 3 to 13 parts by weight, and even more preferably 3 to 10 parts by weight, relative to 100 parts by weight of the total resin composition containing the ethylene-α-olefin copolymer (A) and the tackifier (B). When the blending ratio of (C) is 3 parts by weight or more, the effect of improving the formability of the covering material film is excellent, and when it is 20 parts by weight or less, excellent adhesion is obtained, which is preferable.

[0040] The resin composition constituting the sealant layer may contain other thermoplastic resins or rubbers, as well as light stabilizers, ultraviolet absorbers, nucleating agents, lubricants, antioxidants, antiblocking agents, flow improvers, mold release agents, flame retardants, colorants, inorganic neutralizing agents, hydrochloric acid absorbers, fillers, conductive agents, and the like, within the scope of not impairing the effects of the present invention.

[0041] There are no particular restrictions on the method for preparing the resin composition constituting the sealant layer. For example, the ethylene-α-olefin copolymer (A), the tackifier (B), and materials to be added thereto are pre-blended simultaneously in a mixer such as a Henschel mixer or a tumbler, and then melt-kneaded in a single-screw or twin-screw extruder.

[0042] The above-mentioned lid material film comprises a substrate and a sealant layer. An intermediate layer can be provided between the substrate and the sealant layer to enhance adhesion between the two layers. The intermediate layer is a polyethylene or ethylene copolymer. The ethylene copolymer is not limited as long as it is a copolymer of ethylene and a monomer copolymerizable therewith, and examples thereof include ethylene-α-olefin copolymer, propylene-ethylene copolymer, ethylene-acrylic acid copolymer, ethylene-methacrylic acid copolymer, and ethylene-methyl acrylate copolymer. Modified versions of these copolymers are also acceptable. The intermediate layer may contain various additives, such as antioxidants, lubricants, antistatic agents, conductive agents, antiblocking agents, light stabilizers, and ultraviolet absorbers, as long as they do not impair the effects of the present invention.

[0043] The intermediate layer may be a single layer or a laminate, and may be a laminate selected from any polyethylene or ethylene copolymer, such as polyethylene / ethylene-α-olefin copolymer / polyethylene.

[0044] The thickness of the substrate is preferably 10 to 200 μm, more preferably 12 to 100 μm, and even more preferably 14 to 50 μm. Within such a range, a laminate film having sufficient strength as a substrate for a covering film can be obtained.

[0045] The thickness of the intermediate layer can be selected depending on the application as long as workability and other properties are not impaired, but is generally about 5 to 30 μm. The thickness of the sealant layer is preferably 3 to 50 μm, more preferably 5 to 40 μm, and even more preferably 5 to 25 μm. When the thickness is 5 μm or more, the resulting lid material film exhibits excellent adhesiveness, while when it is 25 μm or less, it exhibits sufficient adhesiveness and is also economical.

[0046] Furthermore, the sum of the thicknesses of the substrate and the intermediate layer (X) and the thickness of the sealant layer (Y) preferably satisfy the relationship (X) ≧ (Y). When the thicknesses satisfy the relationship (X) ≧ (Y), the substrate of the resulting lid material film can maintain sufficient strength, and the intermediate layer can sufficiently adhere the substrate and the sealant layer, thereby exhibiting good adhesive strength to various containers. Furthermore, since the proportion of non-polyethylene resin contained in the sealant layer is low, the resulting lid material film has excellent recyclability.

[0047] The polyethylene resin content in the entire covering film is preferably 90% by weight or more. Since such a film uses the same type of resin material, it can be classified as a mono-material material and has excellent recyclability. Here, the polyethylene resin refers to the polyethylene substrate, the polyethylene or ethylene copolymer intermediate layer, and the ethylene-α-olefin copolymer (A) and low-density polyethylene (C) sealant layer.

[0048] The above-mentioned lid material film can be suitably used as an easy-peel lid material for plastic containers made of resins containing polyethylene terephthalate, polystyrene, polypropylene, etc. as the main component, as well as various other resins as the main component.

[0049] Specific examples of materials for the plastic container include polyolefin resins, acrylic acid resins, polyamide resins, polyester resins, polycarbonate resins, polystyrene resins, styrene-acrylonitrile copolymers, and polyvinyl chloride resins.

[0050] Examples of polyolefin resins include low-density polyethylene, high-density polyethylene, ethylene-α-olefin copolymer, ethylene-vinyl acetate copolymer, polypropylene, etc. Examples of acrylic acid resins include polyacrylic acid, polymethyl acrylate, polyethyl acrylate, polybutyl acrylate, polyoctyl acrylate, polymethacrylic acid, polymethyl methacrylate, polyethyl methacrylate, polybutyl methacrylate, polyoctyl methacrylate, etc. Examples of polyamide resins include nylon 6, nylon 6,6, nylon 11, nylon 12, etc. Examples of polyester resins include polyethylene terephthalate, polybutylene terephthalate, polylactic acid (including poly-L-lactic acid, poly-D-lactic acid, copolymers of L-lactic acid and D-lactic acid, and stereocomplexes of poly-L-lactic acid and poly-D-lactic acid), polybutylene succinate, poly(butylene succinate / adipate), polyethylene succinate, poly(butylene succinate / terephthalate), poly(butylene adipate / terephthalate), poly(hydroxybutyrate / hydroxyhexanoate), polyglycolic acid, poly(3-hydroxybutyrate), and polycaprolactone.

[0051] Furthermore, a barrier layer can be provided between the substrate and the intermediate layer. Examples of gas barrier resins that can be used for the barrier layer include ethylene-vinyl alcohol copolymers, polyvinyl alcohol, polyamide resins, polyester resins, and polyurethane resins. Instead of a gas barrier resin, a vapor-deposited barrier layer can be provided, such as an aluminum vapor-deposited layer formed by vapor-depositing a metal such as aluminum. The presence of this barrier layer can improve the oxygen barrier property and water vapor barrier property.

[0052] In the present invention, an anchor coat layer of polyurethane or the like can be provided between the substrate and the sealant layer, or between the substrate and the intermediate layer, in order to enhance the adhesion between the two layers.

[0053] The method for producing the lid material is not particularly limited, but examples thereof include a method of laminating a resin composition for the sealant layer with a substrate, and a method of co-extruding a sealant adhesive with an intermediate layer.

[0054] Examples of lamination methods include: (1) an extrusion lamination method in which an anchor coating agent is applied to a substrate, and a sealant layer is melt-extruded; (2) an extrusion lamination method in which an anchor coating agent is applied to a substrate, and an intermediate layer is melt-extruded, and then a sealant layer is melt-extruded thereon; (3) an extrusion lamination method in which an intermediate layer having excellent adhesion to the substrate, such as an ethylene-methacrylic acid copolymer or an ethylene-methyl methacrylate copolymer, is melt-extruded onto the substrate, and then a sealant layer is melt-extruded thereon; (4) a co-extrusion lamination method in which an anchor coating agent is applied to a substrate, and then an intermediate layer and a sealant layer are melt-extruded simultaneously; and (5) a co-extrusion lamination method in which an anchor coating agent is applied to a substrate, and then an intermediate layer and a sealant layer are melt-extruded simultaneously. (6) a dry lamination method in which a film containing at least one sealant layer is formed in advance by inflation molding or cast molding, and then laminated to a substrate coated with an anchor coating agent; and (7) a sandwich extrusion lamination method in which an intermediate layer is melt-extruded using extrusion lamination to laminate between a substrate coated with an anchor coating agent and a film containing at least one sealant layer.

[0055] The lid material can be adhered to the opening of a plastic container to seal the opening. The main component of the plastic container may be a single component or a composition of multiple resins. The container may also be a multi-layer laminate of multiple materials. The lid material is particularly suitable for use with containers made of polyethylene terephthalate, polystyrene, polypropylene, polyvinyl chloride, or polylactic acid.

[0056] Furthermore, one aspect of the present invention is a packaging container comprising a container having an opening and the above-mentioned lid material that seals the opening, wherein the container is made of at least one member selected from the group consisting of polyethylene terephthalate, polystyrene, polypropylene, polyvinyl chloride, and polylactic acid.

[0057] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0058] The molecular weight is not specified. (Molecular Weight) The molecular weight was measured using a GPC apparatus (HLC-8121GPC / HT (trade name), manufactured by Tosoh Corporation) and a column (TSKgel GMHhr-H(20)HT (trade name), manufactured by Tosoh Corporation) with the column temperature set to 140°C and 1,2,4-trichlorobenzene as the eluent. The measurement sample was prepared at a concentration of 1.0 mg / ml, and 0.3 ml was injected for measurement. The molecular weight calibration curve was calibrated using a polystyrene sample with a known molecular weight. From the chromatogram obtained as a result of the measurement, the weight average molecular weight Mw and the proportion of components with a molecular weight of 10,000 or less were calculated. (Density) The measurement was performed in accordance with JIS K6922-1. (Swell Ratio SR) The SR of each material used was measured using a melt indexer specified in JIS K7210. The resin filled in the device was extruded through an orifice at a temperature of 235°C and an extrusion rate of 3 g / min, and a strand-like extrudate was collected in a measuring cylinder filled with isopropanol and placed directly below the orifice. The diameter (D) of the extruded strand was then divided by the orifice diameter (D0) of the melt indexer to determine the SR. (Adhesion strength) The sealant layer of the lid material obtained in the examples was superimposed on a 0.35 mm thick amorphous polyethylene terephthalate sheet (A-PET, manufactured by Toyobo Co., Ltd.), a 0.35 mm thick impact-resistant polystyrene sheet (HIPS, manufactured by DIC Corporation), and a 0.30 mm thick polypropylene sheet (PP, manufactured by OJK Corporation), and was then heat-pressed using a heat seal tester (manufactured by Tester Sangyo Co., Ltd., TP-701 model) at a temperature of 130 ° C, an air pressure of 0.2 MPa, and a time of 1 second. After cooling, the seal strength was measured at a peel angle of 180 ° and a peel speed of 300 mm / min. (Moldability) The moldability during lamination processing when producing the lid material film described in the examples was evaluated, and a ◎ was indicated for cases where molding was possible without problems, a ○ was indicated for cases where the molten film was somewhat unstable but molding was possible without problems, and an × was indicated for cases where molding was not possible due to film tearing. (Recyclability) The lid material obtained in each example was pulverized and melt-kneaded using a twin-screw extruder having a screw diameter of 25 mm (manufactured by Technovel, trade name ULTnano25TW) under conditions of a resin temperature of 160°C and a screw rotation speed of 300 rpm to obtain strands.The smoothness of the resulting strand was evaluated, and smoothness was considered to be excellent in recyclability. (Heat resistance) The sealant layer of the lid material obtained in the examples was superimposed on an A-PET cup (manufactured by Rispack Co., Ltd.) with a capacity of 210 ml and a diameter of 101 mm, and cut into a circle with a diameter of 101 mm. Next, using a cup sealer UF-500 (manufactured by Sunnypack Co., Ltd.), the lid material was heat-pressed at a temperature of 130°C, an air pressure of 0.8 MPa, and a time of 1 second, and then allowed to cool, and the appearance of the laminate was evaluated. If the thermal shrinkage of the lid material was significant and it peeled off from the cup, it was evaluated as ×, and if the thermal shrinkage was small and it did not peel off, it was evaluated as ◯.

[0059] [Example 1] [Preparation of organically modified clay] 300 ml of industrial alcohol (trade name Equinene F-3, manufactured by Japan Alcohol Sales Co., Ltd.) and 300 ml of distilled water were placed in a 1-liter flask, and 15.0 g of concentrated hydrochloric acid and dioleylmethylamine (C 18 H 35 ) 2 (CH 3 ) N, 63.7 g (120 mmol) of (trade name: Lipomin MO, manufactured by Lion Specialty Chemicals Co., Ltd.) was added, heated to 45 ° C, and 100 g of synthetic hectorite (trade name: Laponite RD, manufactured by BYK Corporation) was dispersed therein. The mixture was then heated to 60 ° C and stirred for 1 hour while maintaining that temperature. The slurry was filtered, washed twice with 600 ml of water at 60 ° C, and dried in a dryer at 85 ° C for 12 hours to obtain 130 g of organically modified clay. This organically modified clay was then pulverized in a jet mill to a median diameter of 15 μm.

[0060] [Preparation of polymerization catalyst] After replacing the air in a 300 mL flask equipped with a thermometer and a reflux condenser with nitrogen, 25.0 g of the organically modified clay obtained in [Preparation of organically modified clay] and 108 mL of hexane were added, followed by the addition of 0.392 g (1 mmol) of bis(indenyl)zirconium dichloride and 142 mL of 20% triisobutylaluminum, followed by stirring for 3 hours at 60° C. After cooling to room temperature, the supernatant was removed and washed twice with 220 mL of hexane, and then 220 mL of hexane was added to obtain a catalyst suspension (solid weight content: 12.0 wt %).

[0061] [Production of Polyethylene Powder] A 2-L autoclave was charged with 1.2 L of hexane, 1.0 mL of 20% triisobutylaluminum, and 200 mg (corresponding to 24 mg of solids) of the catalyst suspension obtained in [Preparation of Polymerization Catalyst]. The temperature was raised to 85°C, and then an ethylene / hydrogen mixed gas was continuously supplied so that the partial pressure became 0.90 MPa (hydrogen concentration in the ethylene / hydrogen mixed gas: 450 ppm). After 90 minutes, the pressure was released, and the slurry was filtered and dried to obtain a polyethylene powder. The obtained polyethylene powder had a weight-average molecular weight of 111,000, a proportion of components with a molecular weight of 10,000 or less of 3.4%, and a density of 950 kg / m 3 The obtained polyethylene powder was melt-kneaded using a twin-screw extruder (manufactured by Technovel, trade name ULTnano25TW) having a screw diameter of 25 mm under conditions of a resin temperature of 160°C and a screw rotation speed of 300 rpm, to obtain polyethylene pellets.

[0062] [Production of Stretched Polyethylene Film] Subsequently, the polyethylene pellets were formed into a film using an inflation molding machine equipped with an extruder having a screw diameter of 50 mm. The extrusion temperature was 220°C, the die lip clearance (L) was 3 mm, and the thickness of the resulting polyethylene film was 100 μm. The resulting polyethylene film was uniaxially stretched at 120°C to a stretching ratio of 4 using a tenter method stretching machine (manufactured by Toyo Seiki Seisaku-sho, Ltd., product name EX10-B) to obtain a stretched polyethylene film (I). The thickness of the resulting stretched polyethylene film (I) was 25 μm.

[0063] [Production of Resin Composition for Sealant Layer] An ethylene / α-olefin copolymer (A) having a density of 905 kg / m 390 parts by weight of an ethylene-1-hexene copolymer (A1) (manufactured by Tosoh Corporation, trade name Nipolon HM510R) with an MFR of 12 g / 10 min, and 10 parts by weight of an alicyclic hydrocarbon resin (B1) (manufactured by Arakawa Chemical Industries, Ltd., trade name Alcon P125; softening temperature 125°C, fully hydrogenated) as a tackifier (B) were pre-blended in a tumbler mixer, and then melt-kneaded at 160°C using a twin-screw extruder to obtain pellets of the resin composition. In consideration of thermal stability, the resin composition was added with 0.05 parts by weight of a phenolic antioxidant (manufactured by BASF, trade name Irganox 1010) and 0.2 parts by weight of a slip agent (manufactured by Lion Akzo, product name Armowax E) per 100 parts by weight of the sealant adhesive.

[0064] [Production of Lid Material] An anchor coating agent (a mixture of Takelac A3210 and Takenate A3072, manufactured by Mitsui Chemicals, Inc.) was applied to the surface of the polyethylene stretched film substrate, and then the intermediate layer and sealant layer were co-extrusion laminated using a co-extrusion laminator (manufactured by Sumiju Modern Industries, Inc., screw diameter 40 mm) at a processing temperature of 230°C in the order of substrate / intermediate layer / sealant layer to obtain a lid material. Low-density polyethylene (manufactured by Tosoh Corporation, product name Petrothene 203) was used as the intermediate layer, and the lid material had a structure of substrate 25 μm / intermediate layer 12 μm / sealant layer 20 μm. The evaluation results of the obtained lid material are shown in Table 1.

[0065] [Example 2] The resin composition for the sealant layer of Example 1 was used as an ethylene / α-olefin copolymer (A) having a density of 905 kg / m 3 A lid material was obtained in the same manner as in Example 1, except that the amount of the ethylene / 1-hexene copolymer (A2) having an MFR of 4.0 g / 10 min was 90 parts by weight, and the amount of the tackifier (B1) was 10 parts by weight. The evaluation results of the obtained lid material are shown in Table 1.

[0066] [Example 3] The resin composition for the sealant layer of Example 1 was used as an ethylene / α-olefin copolymer (A) having a density of 885 kg / m 3 A lid material was obtained in the same manner as in Example 1, except that the ethylene / 1-butene copolymer (A3) having an MFR of 3.5 g / 10 min was 90 parts by weight and the tackifier (B1) was 10 parts by weight. The evaluation results of the obtained lid material are shown in Table 1.

[0067] [Example 4] The resin composition for the sealant layer of Example 1 was used as an ethylene / α-olefin copolymer (A) having a density of 900 kg / m 3 A lid material was obtained in the same manner as in Example 1, except that the ethylene / 1-hexene copolymer (A4) having an MFR of 20 g / 10 min was 82 parts by weight and the tackifier (B1) was 18 parts by weight. The evaluation results of the obtained lid material are shown in Table 1.

[0068] [Example 5] A lid material was obtained in the same manner as in Example 1, except that 90 parts by weight of ethylene / α-olefin copolymer (A1) and 10 parts by weight of alicyclic hydrocarbon resin (B2) (manufactured by Arakawa Chemical Industries, Ltd., trade name Alcon P140; softening temperature 140°C, fully hydrogenated) were used as the tackifier (B) relative to the resin composition for the sealant layer of Example 1. The evaluation results of the obtained lid material are shown in Table 1.

[0069] [Example 6] The resin composition for the sealant layer of Example 1 was mixed with 90 parts by weight of an ethylene-α-olefin copolymer (A1), 10 parts by weight of a tackifier (B1), and a low-density polyethylene (C) having a density of 924 kg / m 3 A lid material was obtained in the same manner as in Example 1, except that 5 parts by weight of low-density polyethylene (C1) (manufactured by Tosoh Corporation, trade name Petrothene 205) having an MFR of 3.0 g / 10 min and an SR of 2.02 was used. The evaluation results of the obtained lid material are shown in Table 1.

[0070] [Example 7] The resin composition for the sealant layer of Example 1 was mixed with 90 parts by weight of ethylene / α-olefin copolymer (A1), 10 parts by weight of tackifier (B1), and low-density polyethylene (C) having a density of 922 kg / m 3 A lid material was obtained in the same manner as in Example 1, except that 14 parts by weight of low-density polyethylene (C2) (manufactured by Tosoh Corporation, trade name Petrothene 175R) having an MFR of 0.6 g / 10 min and an SR of 1.81 was used. The evaluation results of the obtained lid material are shown in Table 1.

[0071] [Example 8] The resin composition for the sealant layer of Example 1 was mixed with 90 parts by weight of ethylene / α-olefin copolymer (A1), 10 parts by weight of tackifier (B1), and low-density polyethylene (C) having a density of 924 kg / m 3A lid material was obtained in the same manner as in Example 1, except that 5 parts by weight of low-density polyethylene (C3) (manufactured by Tosoh Corporation, trade name Petrothene 183) having an MFR of 2.0 g / 10 min and an SR of 1.63 was used. The evaluation results of the obtained lid material are shown in Table 1.

[0072] [Example 9] A lid material was obtained in the same manner as in Example 1, except that 90 parts by weight of ethylene-α-olefin copolymer (A1), 10 parts by weight of tackifier (B1), and 2 parts by weight of low-density polyethylene (C1) were used in place of the resin composition for the sealant layer in Example 1. The evaluation results of the obtained lid material are shown in Table 1.

[0073] [Example 10] Instead of the polyethylene stretched film (I) of Example 1, a stretched polyethylene film (I) having a weight average molecular weight of 122,000, a proportion of components with a molecular weight of 10,000 or less of 10.2%, and a density of 954 kg / m 3 A lid material was obtained in the same manner as in Example 1, except that a 25 μm thick stretched polyethylene film (II) made from polyethylene pellets (manufactured by Tosoh Corporation, product name Nipolonhard 5700) was used. The evaluation results of the obtained lid material are shown in Table 1.

[0074] [Example 11] A lid material was obtained in the same manner as in Example 1, except that 90 parts by weight of ethylene / α-olefin copolymer (A1) and 10 parts by weight of alicyclic hydrocarbon resin (B3) (manufactured by Arakawa Chemical Industries, Ltd., trade name Alcon P100; softening temperature 100°C, fully hydrogenated) were used as the tackifier (B) relative to the resin composition for the sealant layer of Example 1. The evaluation results of the obtained lid material are shown in Table 1.

[0075] Example 12 A lid material was obtained in the same manner as in Example 1, except that 90 parts by weight of ethylene / α-olefin copolymer (A1) and 10 parts by weight of polymerized rosin ester resin (B4) (trade name Pencel D125, manufactured by Arakawa Chemical Industries, Ltd.; softening temperature 125°C) were used as the tackifier (B) relative to the resin composition for the sealant layer of Example 1. The evaluation results of the obtained lid material are shown in Table 1.

[0076] Example 13 A lid material was obtained in the same manner as in Example 4, except that a 15 μm thick oriented polyethylene film (IV) was used instead of the 25 μm thick oriented polyethylene film (I) of Example 4, the thickness of the intermediate layer made of low-density polyethylene (manufactured by Tosoh Corporation, product name Petrothene 203) was 2 μm, and the thickness of the sealant layer was 30 μm. The oriented polyethylene film (IV) was produced by uniaxially stretching a 60 μm thick polyethylene film produced in the same manner as the oriented polyethylene film (I) at 120° C. to a stretch ratio of 4. The evaluation results of the obtained lid material are shown in Table 1.

[0077]

[0078] Comparative Example 1 A lid material was obtained in the same manner as in Example 1, except that a 25 μm thick biaxially oriented polyester film (III) (manufactured by Toyobo Co., Ltd., product name E5100) was used instead of the polyethylene stretched film (I) in Example 1. The evaluation results of the obtained lid material are shown in Table 2. The obtained lid material had poor strand appearance during melt-kneading and was poor in recyclability. Furthermore, even when the resin temperature during melt-kneading was increased to 250° C., the strand appearance was similarly poor and the recyclability was poor.

[0079] Comparative Example 2 The resin composition for the sealant layer of Example 1 was used in combination with an ethylene / α-olefin copolymer (A) having a density of 920 kg / m 3 A lid material was obtained in the same manner as in Example 1, except that the ethylene / 1-hexene copolymer (A5) having an MFR of 2.0 g / 10 min was 90 parts by weight and the tackifier (B1) was 10 parts by weight. The evaluation results of the obtained lid material are shown in Table 2. The obtained lid material had poor adhesiveness.

[0080] Comparative Example 3 An attempt was made to produce a lid material in the same manner as in Example 1, except that 70 parts by weight of the ethylene-α-olefin copolymer (A1) and 30 parts by weight of the tackifier (B1) were used in place of the resin composition for the sealant layer in Example 1. However, film tearing of the molten film and blocking to the molding roll occurred during molding, making it difficult to produce the lid material.

[0081]

[0082] While the present invention has been described in detail and with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the invention.

[0083] The entire contents of the specifications, claims and abstracts of Japanese Patent Application No. 2023-081327 filed on May 17, 2023, and Japanese Patent Application No. 2024-072410 filed on April 26, 2024 are hereby cited and incorporated as the disclosure of the specification of the present invention.

Claims

1. A laminate comprising a substrate and a sealant layer, the substrate being a stretched film made of polyethylene, and the sealant layer having a density of 880 to 910 kg / m 3 The film for covering material is composed of a resin composition containing 80 to 97 parts by weight of an ethylene / α-olefin copolymer (A) and 3 to 20 parts by weight of a tackifier (B) (the total of the ethylene / α-olefin copolymer (A) and the tackifier (B) is 100 parts by weight).

2. The covering film according to claim 1, wherein the ethylene / α-olefin copolymer (A) has an α-olefin carbon number of 3 to 20, and has a melt mass flow rate, measured in accordance with JIS K7210-1 at 190°C under a load of 2.16 kg, in the range of 0.1 to 25 g / 10 min.

3. The covering material film according to claim 1, wherein the tackifier (B) is an alicyclic saturated hydrocarbon resin having a softening temperature of 105 to 150°C as measured by the ring and ball method and a hydrogenation rate of aromatic nuclei of 80% or more.

4. The polyethylene constituting the substrate has a weight average molecular weight (Mw) measured by gel permeation chromatography of 70,000 to 250,000, and the proportion of molecular weights of 10,000 or less is 8% by weight or less, and a density measured by JIS K6922-1 of 945 to 980 kg / m 3 The covering film according to claim 1 , 5. The film for covering material according to claim 1, wherein the resin composition constituting the sealant layer contains 3 to 20 parts by weight of a low-density polyethylene (C) that satisfies the following requirements (a) and (b) per 100 parts by weight of the total of the ethylene-α-olefin copolymer (A) and the tackifier (B): (a) the melt mass flow rate measured in accordance with JIS K7210-1 at 190°C and under a load of 2.16 kg is in the range of 0.3 to 5.0 g / 10 min; and (b) the swell ratio (SR) calculated by dividing the diameter (D) of a strand extruded at a temperature of 235°C and an extrusion rate of 3 g / min using a melt indexer used in JIS K7210-1 by the orifice diameter (D0) of the melt indexer is in the range of 1.7 to 3.

0.

6. The film for covering material according to claim 1, further comprising an intermediate layer between the substrate and the sealant layer, the intermediate layer being polyethylene or an ethylene copolymer.

7. The covering film according to claim 6, wherein the thickness (Y) of the sealant layer relative to the sum (X) of the thickness of the substrate and the thickness of the intermediate layer satisfies the relationship (X) ≧ (Y).

8. The covering film according to claim 1, wherein the content of polyethylene resin in the entire covering film is 90% by weight or more.

9. An easy-peel covering material comprising the covering film according to claim 1.

10. A method for sealing a container, comprising adhering the covering material according to claim 9 to the opening of a container made of at least one material selected from the group consisting of polyethylene terephthalate, polystyrene, polypropylene, polyvinyl chloride and polylactic acid.

11. A packaging container comprising a container having an opening and a lid material as described in claim 9 for sealing the opening, said container being made of at least one member selected from the group consisting of polyethylene terephthalate, polystyrene, polypropylene, polyvinyl chloride and polylactic acid.

Citation Information

Patent Citations

  • partial opening lid

    JP1994037169U

  • Adhesive composition and film comprising the same

    JP1999228757A

  • Laminate, production method thereof and packaging material formed of the laminate

    JP2018171834A