Curable composition and sealing material

The curable composition, featuring a polymer with hydrolyzable silyl groups, nitrogen-containing heterocyclic compounds, and metal oxides, addresses the issues of low mold resistance and short tack-free time in one-component sealants, offering improved mold resistance and flexibility in the cured product.

WO2024237252A1PCT designated stage expired Publication Date: 2024-11-21SEKISUI FULLER CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017795
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-15
Filing Date
2024-05-14
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

One-component moisture-curing sealant compositions have low mold resistance and short tack-free time, making them difficult to handle and cure insufficiently, especially in deep areas.

Method used

A curable composition containing a polymer with a hydrolyzable silyl group, a nitrogen-containing heterocyclic compound, and a metal oxide, which provides a longer tack-free time, easy handling, and excellent deep curability, resulting in a cured product with improved mold resistance and flexibility.

Benefits of technology

The curable composition achieves a sufficiently long tack-free time, easy handling, and deep curing, producing a cured product with enhanced mold resistance and flexibility, suitable for various applications including sealants and adhesives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

The present invention provides a curable composition which exhibits a sufficiently long tack-free time, which has excellent handleability, the inside of which can be sufficiently cured (deep-part curability), and which can produce a cured product having excellent anti-mold properties. A curable composition according to the present invention is characterized by comprising: a polymer that has a hydrolyzable silyl group; a nitrogen-containing heterocyclic compound; and a metal oxide. Thus, the curable composition exhibits a long tack-free time, has excellent deep-part curability, and can produce a cured product having excellent anti-mold properties.
Need to check novelty before this filing date? Find Prior Art

Description

Curable composition and sealant

[0001] The present invention relates to a curable composition and a sealant.

[0002] Modified silicone-based curable compositions containing polyoxyalkylene polymers having hydrolyzable silyl groups are safe in that they do not generate toxic substances during curing, and the cured products obtained by curing have excellent flexibility (elasticity), so they are widely used as sealants and adhesives.

[0003] Sealant is used in wet areas such as kitchens, bathrooms, toilets, and washrooms, where mold is likely to grow.

[0004] Therefore, Patent Document 1 discloses a one-component moisture-curing sealant composition containing an isocyanate group-containing urethane prepolymer (A), an antibacterial and antifungal agent (B), and a high-molecular-weight diluent resin (C), in which the antibacterial and antifungal agent (B) is a composite in which an antibacterial and antifungal compound is supported on a layered silicate.

[0005] JP 2011-111481 A

[0006] However, the one-component moisture-curing sealant composition disclosed in Patent Document 1 has poor mildew resistance and a short tack-free time, making it difficult to handle, and also has problems in that the interior of the one-component moisture-curing sealant composition is not sufficiently cured.

[0007] The present invention provides a curable composition that has a sufficiently long tack-free time, is excellent in handleability, can be cured sufficiently to the inside (deep curing), and can produce a cured product with excellent mildew resistance.

[0008] The curable composition of the present invention is characterized by containing a polymer having a hydrolyzable silyl group, a nitrogen-containing heterocyclic compound, and a metal oxide.

[0009] The curable composition of the present invention has a sufficiently long tack-free time, is easy to handle, can be cured sufficiently to the inside, and can impart excellent mold resistance to the cured product produced by curing.

[0010] The curable composition of the present invention is characterized by containing a polymer having a hydrolyzable silyl group, a nitrogen-containing heterocyclic compound, and a metal oxide.

[0011] [Polymer Having Hydrolyzable Silyl Group] The curable composition contains a polymer having a hydrolyzable silyl group. The polymer having a hydrolyzable silyl group crosslinks due to moisture (water) in the atmosphere or moisture (water) contained in a member such as a joint into which the curable composition is filled, forming a crosslinked structure and generating a cured product.

[0012] The polymer having a hydrolyzable silyl group is not particularly limited as long as it has a hydrolyzable silyl group and forms a crosslinked structure by moisture to harden, and examples thereof include polyoxyalkylene polymers having a hydrolyzable silyl group, acrylic polymers having a hydrolyzable silyl group, urethane polymers having a hydrolyzable silyl group, and polyolefin polymers having a hydrolyzable silyl group.The polymer having a hydrolyzable silyl group preferably contains a polyoxyalkylene polymer having a hydrolyzable silyl group, an acrylic polymer having a hydrolyzable silyl group, or a silicone polymer having a hydrolyzable silyl group, and more preferably contains a polyoxyalkylene polymer having a hydrolyzable silyl group.The polymer having a hydrolyzable silyl group may be used alone or in combination of two or more.

[0013] The content of the polyoxyalkylene polymer having a hydrolyzable silyl group in the polymer having a hydrolyzable silyl group is preferably 50% by mass or more, more preferably 60% by mass or more, more preferably 70% by mass or more, more preferably 80% by mass or more, more preferably 90% by mass or more, more preferably 95% by mass or more, more preferably 99% by mass or more, and more preferably 100% by mass.

[0014] The content of the urethane polymer having a hydrolyzable silyl group in the polymer having a hydrolyzable silyl group is preferably 50% by mass or more, more preferably 60% by mass or more, more preferably 70% by mass or more, more preferably 80% by mass or more, more preferably 90% by mass or more, more preferably 95% by mass or more, more preferably 99% by mass or more, and more preferably 100% by mass.

[0015] The content of the acrylic polymer having a hydrolyzable silyl group in the polymer having a hydrolyzable silyl group is preferably 50% by mass or more, more preferably 60% by mass or more, more preferably 70% by mass or more, more preferably 80% by mass or more, more preferably 90% by mass or more, more preferably 95% by mass or more, more preferably 99% by mass or more, and more preferably 100% by mass.

[0016] The polymer having a hydrolyzable silyl group preferably has a hydrolyzable silyl group in the molecule and at the molecular terminal. The hydrolyzable silyl group is more preferably bonded to only one of the two terminals of the main chain, or to both terminals. When the hydrolyzable silyl group is bonded to the terminal of the main chain, the cured product of the curable composition has excellent flexibility and adhesiveness. Due to the chain extension effect during curing of the curable composition, the curable composition has excellent deep curability. When the polymer having a hydrolyzable silyl group has multiple hydrolyzable silyl groups in the molecule, the hydrolyzable silyl groups may be the same or different. The main chain refers to the longest chain in the molecule, and the length of the chain is determined by the number of atoms directly constituting the chain; the greater the number of atoms, the longer the chain is considered to be.

[0017] The hydrolyzable silyl group refers to a group that undergoes a condensation reaction in the presence of moisture or a crosslinking agent, and if necessary, using a catalyst, such as a silicon-containing group or a silanol group having a hydrolyzable group bonded to a silicon atom. Note that a silanol group refers to a functional group in which a hydroxyl group (-OH) is bonded directly to a silicon atom [≡Si-OH, formula (1)]. In formula (1), *1 to *3 are bonds and represent single bonds.

[0018]

[0019] The hydrolyzable group of the hydrolyzable silyl group is not particularly limited, and examples thereof include a hydrogen atom, a halogen atom, an alkoxy group, an acyloxy group, a ketoximate group, an amino group, an amide group, an acid amide group, an aminooxy group, a mercapto group, and an alkenyloxy group.

[0020] Among these, the hydrolyzable silyl group is preferably an alkoxysilyl group, since it can impart excellent deep curability to the cured product of the curable composition while maintaining the flexibility of the cured product of the curable composition.

[0021] The alkoxysilyl group is —SiR 1 j (OR 2 ) 3-j Preferably, the compound has a structure represented by the formula: 1 represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or a hydrogen atom. 2 represents an alkyl group having 1 to 6 carbon atoms, and j represents an integer of 0 to 2.

[0022] Examples of the alkoxysilyl group include trialkoxysilyl groups such as trimethoxysilyl group, triethoxysilyl group, triisopropoxysilyl group, and triphenoxysilyl group; dialkoxysilyl groups such as propyldimethoxysilyl group, methyldimethoxysilyl group, and methyldiethoxysilyl group; and monoalkoxysilyl groups such as dimethylmethoxysilyl group and dimethylethoxysilyl group. Among these, dialkoxysilyl groups and trialkoxysilyl groups are preferred, dimethoxysilyl groups and trimethoxysilyl groups are preferred, and dimethoxysilyl groups are more preferred, as they can impart excellent deep curability to the curable composition.

[0023] [Polyoxyalkylene Polymer Having Hydrolyzable Silyl Group] In the polyoxyalkylene polymer having a hydrolyzable silyl group, the hydrolyzable silyl group is preferably an alkoxysilyl group, more preferably a dialkoxysilyl group, more preferably a dimethoxysilyl group, and more preferably a propyldimethoxysilyl group.

[0024] The polyoxyalkylene polymer having a hydrolyzable silyl group preferably has an average of 1 to 4 hydrolyzable silyl groups per molecule, more preferably 1.1 to 3.5 hydrolyzable silyl groups, more preferably 1.3 to 3.4 hydrolyzable silyl groups, even more preferably 2.0 to 3.3 hydrolyzable silyl groups, even more preferably 2.0 to 3.2 hydrolyzable silyl groups, and even more preferably 2.0 to 3.0 hydrolyzable silyl groups. When the number of hydrolyzable silyl groups in the polyoxyalkylene polymer having a hydrolyzable silyl group is within the above range, the deep curability of the curable composition is improved. The polyoxyalkylene polymer having a hydrolyzable silyl group preferably has a hydrolyzable silyl group at its molecular terminal, more preferably has a hydrolyzable silyl group at all of its molecular terminals. The polyoxyalkylene polymer having a hydrolyzable silyl group preferably has a hydrolyzable silyl group at at least one of both terminals of its main chain.

[0025] The average number of hydrolyzable silyl groups per molecule in the polyoxyalkylene polymer having hydrolyzable silyl groups is 1 It can be calculated based on the concentration of hydrolyzable silyl groups in the polyoxyalkylene polymer determined by H-NMR and the number average molecular weight of the polyoxyalkylene polymer determined by GPC.

[0026] The polyoxyalkylene polymer constituting the polyoxyalkylene polymer having a hydrolyzable silyl group has a main chain represented by the general formula: -(R-O) m - (wherein R represents an alkylene group having 1 to 14 carbon atoms, and m represents the number of repeating units and is a positive integer.) The main chain skeleton of the polyoxyalkylene polymer may be composed of only one type of repeating unit, or may be composed of two or more types of repeating units.

[0027] The polyoxyalkylene polymer having a hydrolyzable silyl group has the general formula: -(R-O)m It is preferable that the repeating unit has the general formula: -(R-O) m The repeating unit represented by - (wherein R represents an alkylene group having 1 to 14 carbon atoms, and m represents the number of repeating units and is a positive integer) may contain only one type of repeating unit, or may contain two or more types of repeating units.

[0028] The polyoxyalkylene polymer having a hydrolyzable silyl group preferably has a structure represented by the following formula (2): When the polyoxyalkylene polymer having a hydrolyzable silyl group has the structure represented by formula (2), the deep curing property and the recovery property described below are improved. 3 represents an alkylene group having 1 to 14 carbon atoms, and x, y, and z are each the number of repeating units and are positive integers. 4 represents an alkyl group having 1 to 20 carbon atoms which may have a substituent, or a hydrogen atom. 5 represents an alkyl group having 1 to 6 carbon atoms. k represents an integer of 0 to 2. 3 , R 4 and R 5 may be the same or different from each other. When there are multiple k's, they may be the same or different from each other.

[0029]

[0030] In formula (2), R 3 is preferably an alkylene group having 1 to 4 carbon atoms, more preferably an alkylene group having 1 to 3 carbon atoms, more preferably an alkylene group having 2 or 3 carbon atoms, and more preferably a propylene group [—CH(CH)—CH—]. 4 is preferably a hydrogen atom. 5 is preferably a methyl group or an ethyl group, more preferably a methyl group.

[0031] Curable compositions are used as sealants, adhesives, etc. Gaps between adherends or gaps in joints (hereinafter sometimes simply referred to as "gaps") expand due to changes in temperature, etc. Therefore, it is preferable that a cured product of the curable composition smoothly adapts to changes in the gaps.

[0032] When the gap expands and then shrinks to its original state, it is preferable that the cured product of the curable composition also shrinks to its original state in response to the shrinkage of the gap (resilience). The cured product of the curable composition expands in response to the expansion of the gap, thereby maintaining the gap in a closed state at all times. A cured product with excellent resilience shrinks in response to the shrinkage of the gap, thereby preventing slack within the gap and maintaining a state in which the gap is neatly filled. As the gap shrinks, the cured product of the curable composition is less likely to unexpectedly protrude from the gap or become wavy within the gap, allowing the cured product of the curable composition to maintain an excellent appearance and reduce the accumulation of dust and other particles on the surface of the cured product.

[0033] In the present invention, an alkylene group is a divalent atomic group formed by removing two hydrogen atoms bonded to two different carbon atoms in an aliphatic saturated hydrocarbon, and includes both straight-chain and branched atomic groups.

[0034] Examples of the alkylene group include a methylene group [-CH-], an ethylene group [-CH-CH-], a propylene group [-CH(CH)-CH-], a trimethylene group [-CH-CH-CH-], a butylene group, an amylene group [-(CH)-], and a hexylene group.

[0035] Examples of the main chain skeleton of the polyoxyalkylene polymer include polyethylene oxide, polypropylene oxide, polybutylene oxide, polytetramethylene oxide, polyethylene oxide-polypropylene oxide copolymer, and polypropylene oxide-polybutylene oxide copolymer. Among these, polypropylene oxide is preferred. When polypropylene oxide is used, the curable composition has excellent deep curing properties, and the cured product of the curable composition has excellent flexibility.

[0036] The number average molecular weight of the polyoxyalkylene polymer having a hydrolyzable silyl group is preferably 3,000 or more, more preferably 10,000 or more, more preferably 15,000 or more, more preferably 20,000 or more, more preferably 25,000 or more, more preferably 26,000 or more, more preferably 27,000 or more, more preferably 28,000 or more, and more preferably 29,000 or more. The number average molecular weight of the polyoxyalkylene polymer having a hydrolyzable silyl group is preferably 50,000 or less, more preferably 40,000 or less, more preferably 35,000 or less, more preferably 32,000 or less, and more preferably 30,000 or less. When the number average molecular weight of the polyoxyalkylene polymer is 3,000 or more, the curable composition has excellent deep curability, and the cured product of the curable composition has excellent flexibility. When the number average molecular weight of the polyoxyalkylene polymer is 50,000 or less, an increase in the viscosity of the curable composition is suppressed, and the coatability of the curable composition is improved.

[0037] The molecular weight distribution (Mw / Mn) of the hydrolyzable silyl group-containing polyoxyalkylene polymer is preferably 2.0 or less, more preferably 1.8 or less, and even more preferably 1.5 or less. When the hydrolyzable silyl group-containing polyoxyalkylene polymer has a molecular weight distribution (Mw / Mn) of 2.0 or less, when the curable composition is used as a sealant, the cured product of the curable composition has excellent maximum load elongation in normal adhesiveness.

[0038] In the present invention, the number-average molecular weight and weight-average molecular weight of the polyoxyalkylene polymer having a hydrolyzable silyl group are values ​​measured by gel permeation chromatography (GPC) and converted into polystyrene. Specifically, 6 to 7 mg of the polyoxyalkylene polymer having a hydrolyzable silyl group is sampled, the sampled polyoxyalkylene polymer having a hydrolyzable silyl group is placed in a test tube, and an o-DCB (ortho-dichlorobenzene) solution containing 0.05% by mass of BHT (dibutylhydroxytoluene) is added to the test tube to dilute the polyoxyalkylene polymer having a hydrolyzable silyl group to a concentration of 1 mg / mL, thereby preparing a diluted solution.

[0039] The diluted solution is shaken for 1 hour at 25 rpm at 145°C using a dissolution filter to dissolve the polyoxyalkylene polymer having a hydrolyzable silyl group in the o-DCB solution containing BHT, thereby obtaining a measurement sample. The number-average molecular weight and weight-average molecular weight of the polyoxyalkylene polymer having a hydrolyzable silyl group can be measured by GPC using this measurement sample.

[0040] The number average molecular weight and weight average molecular weight of a polyoxyalkylene polymer having a hydrolyzable silyl group can be measured, for example, using the following measuring device and measuring conditions: Measuring device: TOSOH Corporation, product name "HLC-8121GPC / HT" Measuring conditions: Column: TSKgelGMHHR-H(20)HT x 3, TSKguardcolumn-HHR(30)HT x 1 Mobile phase: o-DCB 1.0 mL / min Sample concentration: 1 mg / mL Detector: Bryce refractometer Standard: Polystyrene (TOSOH Corporation, molecular weight: 500 to 8420000) Elution conditions: 145°C SEC temperature: 145°C

[0041] Commercially available polyoxyalkylene polymers having a hydrolyzable silyl group can be used. For example, examples of polyoxyalkylene polymers having a hydrolyzable silyl group include those manufactured by Kaneka Corporation under the trade names "MS Polymer S-203," "MS Polymer S-303," "MS Polymer S-303H," "Silyl Polymer SAT-200," "Silyl Polymer SAT-350," and "Silyl Polymer SAT-400." Examples of polyoxyalkylene polymers having a hydrolyzable silyl group include those manufactured by AGC under the trade names "Excestar S6735D," "Excestar ESS-3620," "Excestar ESS-2420," "Excestar ESS2410," and "Excestar ESS3430."

[0042] A polyoxyalkylene polymer having a polypropylene oxide main chain and a (methoxymethyl)dimethoxysilyl group at the end of the polypropylene oxide is commercially available from Kaneka Corporation under the trade name "HS-2."

[0043] A polyoxyalkylene polymer having a polypropylene oxide main chain and an isopropyldimethoxymethylsilyl group at the end of the polypropylene oxide is commercially available from Kaneka Corporation under the trade name "SAX720."

[0044] [Acrylic polymer having hydrolyzable silyl group] The hydrolyzable silyl group of the acrylic polymer is preferably a trialkoxysilyl group, since the curable composition has excellent deep curability. Examples of the trialkoxysilyl group include a trimethoxysilyl group, a triethoxysilyl group, a triisopropoxysilyl group, and a triphenoxysilyl group, and the trimethoxysilyl group is preferred.

[0045] The acrylic polymer having hydrolyzable silyl groups preferably has an average of 1.0 to 4.0, more preferably 1.3 to 3.0, more preferably 2.0 to 3.0, and more preferably 2.0 to 2.5 hydrolyzable silyl groups per molecule. When the average number of hydrolyzable silyl groups per molecule of the acrylic polymer having hydrolyzable silyl groups is 1.0 or more, the curability of the curable composition is improved. When the average number of hydrolyzable silyl groups per molecule of the acrylic polymer having hydrolyzable silyl groups is 4.0 or less, the deep curability of the curable composition is improved.

[0046] The average number of hydrolyzable silyl groups per molecule in the acrylic polymer having hydrolyzable silyl groups is 1 The calculation can be based on the concentration of hydrolyzable silyl groups in the acrylic polymer having hydrolyzable silyl groups, determined by H-NMR, and the number average molecular weight of the acrylic polymer having hydrolyzable silyl groups, determined by GPC.

[0047] Examples of the main chain skeleton of the acrylic polymer having a hydrolyzable silyl group include acrylic polymers obtained by radical polymerization of (meth)acrylate monomers, where (meth)acrylate means methacrylate or acrylate.

[0048] Specific examples of the (meth)acrylate monomer that constitutes the main chain of the acrylic polymer having a hydrolyzable silyl group include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, and isomycin. Styryl (meth)acrylate, stearyl (meth)acrylate, isobornyl (meth)acrylate, benzyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, hexanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, epoxy(meth)acrylate, polyester(meth)acrylate, urethane(meth)acrylate, 2-hydroxyethyl(meth)acrylate, 3-hydroxypropyl(meth)acrylate, 2-hydroxypropyl(meth)acrylate p)acrylate, 4-hydroxybutyl(meth)acrylate, 2-hydroxybutyl(meth)acrylate, 5-hydroxypentyl(meth)acrylate, 6-hydroxyhexyl(meth)acrylate, 3-hydroxy-3-methylbutyl(meth)acrylate, 2-hydroxy-3-phenoxypropyl(meth)acrylate, 2-[acryloyloxy]ethyl-2-hydroxyethyl phthalate, and 2-[acryloyloxy]ethyl-2-hydroxypropyl phthalate.As the (meth)acrylate monomer, an alkyl(meth)acrylate in which the alkyl group has 1 to 6 carbon atoms is preferred, an alkyl(meth)acrylate in which the alkyl group has 1 to 5 carbon atoms is more preferred, and an alkyl acrylate in which the alkyl group has 1 to 5 carbon atoms is even more preferred. As the (meth)acrylate monomer, methyl(meth)acrylate and butyl(meth)acrylate are preferred, butyl(meth)acrylate is more preferred, and butyl acrylate is even more preferred. These (meth)acrylate monomers may be used alone or in combination of two or more.

[0049] In the acrylic polymer having a hydrolyzable silyl group, other monomers can also be copolymerized. Examples of such monomers include styrene derivatives such as styrene, indene, α-methylstyrene, p-methylstyrene, p-chlorostyrene, p-chloromethylstyrene, p-methoxystyrene, p-tert-butoxystyrene, and divinylbenzene; compounds having a vinyl ester group such as vinyl acetate, vinyl propionate, vinyl butyrate, vinyl caproate, vinyl benzoate, and vinyl cinnamate; maleic anhydride, N-vinylpyrrolidone, N-vinylmorpholine, (meth)acrylonitrile, (meth)acrylamide, N-cyclohexylmaleimide, N-phenylmaleimide, N-laurylmaleimide, N-benzylmaleimide, n-propyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether, tert-butyl vinyl ether, tert-amyl vinyl ether, cyclohexyl vinyl ether, 2-ethylhexyl vinyl ether, dodecyl vinyl ether, octadecyl vinyl ether, 2-chloroethyl vinyl ether, ethylene glycol butyl vinyl ether, and triethylene glycol butyl vinyl ether. Examples of vinyloxy group-containing compounds include glycol methyl vinyl ether, (4-vinyloxy)butyl benzoate, ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, tetraethylene glycol divinyl ether, butane-1,4-diol divinyl ether, hexane-1,6-diol divinyl ether, cyclohexane-1,4-dimethanol divinyl ether, di(4-vinyloxy)butyl isophthalate, di(4-vinyloxy)butyl glutarate, di(4-vinyloxy)butyl succinate, trimethylolpropane trivinyl ether, 2-hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, 6-hydroxyhexyl vinyl ether, cyclohexane-1,4-dimethanol monovinyl ether, diethylene glycol monovinyl ether, 3-aminopropyl vinyl ether, 2-(N,N-diethylamino)ethyl vinyl ether, urethane vinyl ether, and polyester vinyl ether. These monomers may be used alone or in combination of two or more.

[0050] Among these, the main chain skeleton of the acrylic polymer having a hydrolyzable silyl group is preferably a copolymer of butyl (meth)acrylate and methyl (meth)acrylate, more preferably a copolymer of butyl acrylate and methyl methacrylate, and more preferably a homopolymer of butyl acrylate. The acrylic polymer having a hydrolyzable silyl group, the main chain skeleton of which is the copolymer, can provide a curable composition capable of forming a cured product that maintains excellent antifungal properties for a long period of time after curing.

[0051] The polymerization method for the acrylic polymer having a hydrolyzable silyl group is not particularly limited, and known methods can be used. Examples of such polymerization methods include free radical polymerization, anionic polymerization, cationic polymerization, UV radical polymerization, living anionic polymerization, living cationic polymerization, and living radical polymerization.

[0052] The method for introducing a hydrolyzable silyl group into an acrylic polymer having a hydrolyzable silyl group is not particularly limited, and any known method can be used, such as a method of hydrosilylating an acrylic polymer having an unsaturated group introduced into the molecule by allowing a hydrosilane having a hydrolyzable silyl group to act on the polymer.

[0053] The number average molecular weight of the acrylic polymer having a hydrolyzable silyl group is at least 10,000, preferably at least 15,000, and more preferably at least 20,000. When the number average molecular weight of the acrylic polymer having a hydrolyzable silyl group is at least 10,000, the curable composition has excellent deep curability, and the cured product of the curable composition has excellent flexibility.

[0054] The number average molecular weight of the acrylic polymer having a hydrolyzable silyl group is not more than 50,000, more preferably not more than 40,000, and even more preferably not more than 30,000. When the number average molecular weight of the acrylic polymer having a hydrolyzable silyl group is not more than 50,000, an increase in viscosity of the curable composition is suppressed, and the coatability of the curable composition is improved.

[0055] In the present invention, the number-average molecular weight and weight-average molecular weight of the acrylic polymer having a hydrolyzable silyl group refer to values ​​measured by gel permeation chromatography (GPC) in terms of polystyrene. Measurement by GPC can be performed using, for example, a Tosoh Shodex KF800D GPC column and chloroform or the like as a solvent.

[0056] The number average molecular weight and weight average molecular weight of an acrylic polymer having a hydrolyzable silyl group can be measured, for example, using the following measuring device and under the following measuring conditions: Measuring device: TOSOH Corporation, product name "HLC-8121GPC / HT" Measuring conditions: Column: TSKgelGMHHR-H(20)HT x 3, TSKguardcolumn-HHR(30)HT x 1 Mobile phase: o-DCB 1.0 mL / min Sample concentration: 1 mg / mL Detector: Bryce refractometer Standard: Polystyrene (TOSOH Corporation, molecular weight: 500 to 8420000) Elution conditions: 145°C SEC temperature: 145°C

[0057] [Urethane polymer having hydrolyzable silyl groups] A urethane polymer refers to a polymer having a main chain formed by repeating urethane bonds (-NHCOO-). A urethane polymer having hydrolyzable silyl groups has a plurality of hydrolyzable silyl groups in the main chain of the urethane polymer. It is preferable that a urethane polymer having hydrolyzable silyl groups has hydrolyzable silyl groups at both ends of the main chain of the urethane polymer.

[0058] The urethane polymer having a hydrolyzable silyl group preferably has an average of 1.0 to 4.0, more preferably 1.3 to 3.0, more preferably 2.0 to 3.0, and more preferably 2.0 to 2.5 hydrolyzable silyl groups per molecule. When the average number of hydrolyzable silyl groups per molecule of the urethane polymer having a hydrolyzable silyl group is 1.0 or more, the curability of the curable composition is improved. When the average number of hydrolyzable silyl groups per molecule of the urethane polymer having a hydrolyzable silyl group is 4.0 or less, the deep curability of the curable composition is improved.

[0059] The average number of hydrolyzable silyl groups per molecule in the urethane polymer having hydrolyzable silyl groups is 1 The calculation can be based on the concentration of hydrolyzable silyl groups in the urethane polymer having a hydrolyzable silyl group determined by H-NMR and the number average molecular weight of the urethane polymer having a hydrolyzable silyl group determined by GPC.

[0060] The number average molecular weight of the urethane polymer having a hydrolyzable silyl group is at least 10,000, preferably at least 15,000, and more preferably at least 20,000. When the number average molecular weight of the urethane polymer having a hydrolyzable silyl group is at least 10,000, the curable composition has excellent deep curability, and the cured product of the curable composition has excellent flexibility.

[0061] The number average molecular weight of the urethane polymer having a hydrolyzable silyl group is not more than 50,000, more preferably not more than 40,000, more preferably not more than 35,000, and still more preferably not more than 30,000. When the number average molecular weight of the urethane polymer having a hydrolyzable silyl group is not more than 50,000, an increase in viscosity of the curable composition is suppressed, and the coatability of the curable composition is improved.

[0062] In the present invention, the number-average molecular weight and weight-average molecular weight of the urethane polymer having a hydrolyzable silyl group refer to values ​​measured by gel permeation chromatography (GPC) in terms of polystyrene. Measurement by GPC may use, for example, a Tosoh Shodex KF800D GPC column and chloroform or the like as a solvent.

[0063] The number average molecular weight and weight average molecular weight of a urethane polymer having a hydrolyzable silyl group can be measured, for example, using the following measuring device and measuring conditions: Measuring device: TOSOH Corporation, product name "HLC-8121GPC / HT" Measuring conditions: Column: TSKgelGMHHR-H(20)HT x 3, TSKguardcolumn-HHR(30)HT x 1 Mobile phase: o-DCB 1.0 mL / min Sample concentration: 1 mg / mL Detector: Bryce refractometer Standard substance: Polystyrene (TOSOH Corporation, molecular weight: 500 to 8420000) Elution conditions: 145°C SEC temperature: 145°C

[0064] [Nitrogen-containing heterocyclic compound] The curable composition contains a nitrogen-containing heterocyclic compound. By including the nitrogen-containing heterocyclic compound in the curable composition, a cured product of the curable composition has antifungal properties.

[0065] The nitrogen-containing heterocyclic compound may be any compound capable of imparting antifungal properties to the cured product of the curable composition. A nitrogen-containing heterocyclic compound is an organic compound having a cyclic structure, in which the elements constituting the ring are not only carbon atoms but also nitrogen atoms within the ring. The nitrogen-containing heterocyclic compound is preferably an aromatic compound. The nitrogen-containing heterocyclic compound preferably contains a six-membered ring having aromaticity. The nitrogen-containing heterocyclic compound is not particularly limited, and examples thereof include pyridine-based compounds, imidazole-based compounds, isothiazolin-based compounds, N-haloalkylthio-based compounds, phthalimide-based compounds, triazine-based compounds, and iodine-based compounds. Pyridine-based compounds and imidazole-based compounds are preferred. The nitrogen-containing heterocyclic compounds may be used alone or in combination of two or more.

[0066] The pyridine compound is not particularly limited, and examples thereof include 2,3,5,6-tetrachloro-4-(methylsulfonyl)pyridine, zinc pyrithione, sodium pyrithione, densyl (2,3,5,6-tetrachloro-4-(methylsulfonyl)pyridine), and bis(2-pyridithio-1-oxide)copper [copper pyrithione], with zinc pyrithione being preferred.

[0067] The imidazole compound is not particularly limited, and examples of the imidazole compound include methyl benzimidazol-2-ylcarbamate (abbreviated as "BCM", common name "carbendazim"), 2-(4-thiazolyl)benzimidazole, methyl 2-benzimidazolecarbamate, 1-[ortho-chloro-β-[(para-chlorobenzyl)oxy]phenethyl]-imidazole mononitrate, and the like, with methyl benzimidazol-2-ylcarbamate [carbendazim] being preferred.

[0068] The content of the nitrogen-containing heterocyclic compound in the curable composition is preferably 0.05 parts by mass or more, more preferably 0.06 parts by mass or more, more preferably 0.07 parts by mass or more, more preferably 0.08 parts by mass or more, more preferably 0.09 parts by mass or more, more preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and more preferably 1 part by mass or more, relative to 100 parts by mass of the polymer having a hydrolyzable silyl group. The content of the nitrogen-containing heterocyclic compound in the curable composition is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, more preferably 6 parts by mass or less, more preferably 4 parts by mass or less, more preferably 3.5 parts by mass or less, more preferably 3 parts by mass or less, more preferably 2.7 parts by mass or less, more preferably 2.5 parts by mass or less, more preferably 2.3 parts by mass or less, and more preferably 2 parts by mass or less, relative to 100 parts by mass of the polymer having a hydrolyzable silyl group. When the content of the nitrogen-containing heterocyclic compound is 0.05 parts by mass or more, the cured product of the curable composition has excellent antifungal properties. When the content of the nitrogen-containing heterocyclic compound is 10 parts by mass or less, the tack-free time of the curable composition is sufficient and the curable composition can be sufficiently cured to the inside (deep curing).

[0069] [Metal Oxide] The curable composition contains a metal oxide. When the curable composition contains a nitrogen-containing heterocyclic compound, the tack-free time tends to be too short or the deep curability of the curable composition tends to be reduced. Therefore, by using a nitrogen-containing heterocyclic compound and a metal oxide in combination, the curable composition can maintain an appropriate tack-free time of the curable composition and prevent the reduction in deep curability caused by the nitrogen-containing heterocyclic compound. Therefore, the curable composition has an appropriate tack-free time, is easy to handle, can be sufficiently cured to the inside, and can impart excellent mold resistance to the resulting cured product.

[0070] Although not clearly understood, the following mechanism is thought to be the case. Nitrogen-containing heterocyclic compounds tend to promote the reaction of hydrolyzable silyl groups in polymers having hydrolyzable silyl groups. On the other hand, metal oxides absorb moisture in the system, adjust the rate at which the absorbed moisture is released, and adjust the rate at which moisture is supplied to the hydrolyzable silyl groups. As a result, it is presumed that the reaction between the hydrolyzable silyl groups in the polymer occurs at an appropriate speed, and the tack-free time of the curable composition is controlled to an appropriate length. Furthermore, it is presumed that the curable composition can be sufficiently cured to the inside.

[0071] The metal oxide is not particularly limited, and examples thereof include alkaline earth metal oxides such as beryllium oxide, magnesium oxide, calcium oxide, strontium oxide, and barium oxide, zinc oxide, aluminum oxide, titanium oxide, indium oxide, tin oxide, indium tin oxide (ITO), fluorinated tin oxide (FTO), and indium zinc oxide (IZO). Of these, alkaline earth metal oxides and zinc oxide are preferred, magnesium oxide, calcium oxide, and zinc oxide are more preferred, magnesium oxide and zinc oxide are more preferred, and zinc oxide is still more preferred.

[0072] The content of the metal oxide in the curable composition is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, more preferably 0.5 parts by mass or more, more preferably 0.7 parts by mass or more, more preferably 0.8 parts by mass or more, more preferably 0.9 parts by mass or more, and more preferably 1 part by mass or more, relative to 100 parts by mass of the polymer having a hydrolyzable silyl group. The content of the metal oxide in the curable composition is preferably 50 parts by mass or less, more preferably 45 parts by mass or less, more preferably 40 parts by mass or less, more preferably 35 parts by mass or less, more preferably 30 parts by mass or less, more preferably 27 parts by mass or less, more preferably 25 parts by mass or less, more preferably 23 parts by mass or less, and more preferably 20 parts by mass or less, relative to 100 parts by mass of the polymer having a hydrolyzable silyl group. When the content of the metal oxide is 0.1 parts by mass or more, the curable composition can impart excellent antifungal properties to the cured product produced by curing. When the content of the metal oxide is 50 parts by mass or less, the curable composition has an appropriately long tack-free time, is excellent in handleability, and exhibits excellent deep curing properties. A cured product of the curable composition exhibits flexibility and recovery properties.

[0073] In the curable composition, the mass ratio of the nitrogen-containing heterocyclic compound content to the metal oxide content (nitrogen-containing heterocyclic compound content / metal oxide content) is preferably 0.001 or more, preferably 0.003 or more, more preferably 0.004 or more, more preferably 0.005 or more, more preferably 0.006 or more, more preferably 0.008 or more, more preferably 0.01 or more, more preferably 0.05 or more, more preferably 0.06 or more, more preferably 0.07 or more, more preferably 0.08 or more, more preferably 0.09 or more, and more preferably 0.095 or more. In the curable composition, the mass ratio of the nitrogen-containing heterocyclic compound content to the metal oxide content (nitrogen-containing heterocyclic compound content / metal oxide content) is preferably 0.6 or less, more preferably 0.55 or less, more preferably 0.5 or less, more preferably 0.47 or less, more preferably 0.45 or less, more preferably 0.43 or less, and more preferably 0.4 or less. When the mass ratio of the nitrogen-containing heterocyclic compound content to the metal oxide content (nitrogen-containing heterocyclic compound content / metal oxide content) is within the above range, the curable composition has an appropriately long tack-free time, is easy to handle, and exhibits excellent deep curing properties. A cured product of the curable composition exhibits excellent flexibility and recovery.

[0074] [Filler] The curable composition may contain a filler (excluding metal oxides). The filler is not particularly limited, and examples thereof include inorganic fillers such as calcium carbonate, magnesium carbonate, hydrous silicic acid, anhydrous silicic acid, calcium silicate, and carbon black. These fillers may be used alone or in combination of two or more. Among these, calcium carbonate is preferably used as the filler.

[0075] Precipitated calcium carbonate and ground calcium carbonate are preferred as calcium carbonate, and precipitated calcium carbonate is more preferred. Precipitated calcium carbonate includes light calcium carbonate and colloidal calcium carbonate.

[0076] As the calcium carbonate, either precipitated calcium carbonate or ground calcium carbonate may be used, or both may be used.

[0077] The content of the filler in the curable composition is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, more preferably 15 parts by mass or more, more preferably 20 parts by mass or more, more preferably 50 parts by mass or more, more preferably 70 parts by mass or more, more preferably 80 parts by mass or more, more preferably 100 parts by mass or more, more preferably 110 parts by mass or more, more preferably 120 parts by mass or more, more preferably 130 parts by mass or more, and more preferably 140 parts by mass or more, relative to 100 parts by mass of the polymer having a hydrolyzable silyl group. The content of the filler in the curable composition is preferably 500 parts by mass or less, more preferably 300 parts by mass or less, more preferably 200 parts by mass or less, more preferably 190 parts by mass or less, more preferably 180 parts by mass or less, more preferably 170 parts by mass or less, more preferably 165 parts by mass or less, more preferably 160 parts by mass or less, more preferably 155 parts by mass or less, more preferably 154 parts by mass or less, more preferably 153 parts by mass or less, relative to 100 parts by mass of the polymer having a hydrolyzable silyl group. When the content of the filler in the curable composition is 5 parts by mass or more, the film strength of the cured product of the curable composition is improved, the elongation properties are improved, and the restorability of the cured product is improved. When the content of the filler in the curable composition is 500 parts by mass or less, the flexibility and restorability of the cured product of the curable composition are improved.

[0078] In the curable composition, the mass ratio of the metal oxide content to the calcium carbonate content (metal oxide content / calcium carbonate content) is preferably 0.003 or more, preferably 0.004 or more, more preferably 0.005 or more, more preferably 0.006 or more, and more preferably 0.007 or more. In the curable composition, the mass ratio of the metal oxide content to the calcium carbonate content (metal oxide content / calcium carbonate content) is preferably 0.5 or less, more preferably 0.4 or less, more preferably 0.3 or less, more preferably 0.25 or less, and more preferably 0.2 or less. When the mass ratio of the metal oxide content to the calcium carbonate content (metal oxide content / calcium carbonate content) is within the above range, the curable composition has an appropriately long tack-free time, excellent handleability, and excellent deep curing properties. A cured product of the curable composition has excellent flexibility and recovery properties.

[0079] The average particle size of calcium carbonate is preferably 0.01 μm or more, more preferably 0.05 μm or more, more preferably 0.07 μm or more, more preferably 0.08 μm or more, more preferably 0.09 μm or more, and more preferably 0.1 μm or more. The average particle size of calcium carbonate is preferably 5 μm or less, more preferably 2.5 μm or less, more preferably 2 μm or less, and more preferably 1 μm or less. Calcium carbonate having such an average particle size exhibits an appropriate tack-free time, excellent handleability, and excellent deep curing properties. The cured product of the curable composition exhibits excellent flexibility, resilience, and mold resistance. The particle size of calcium carbonate is measured as the spherical volume equivalent diameter, and the average particle size of calcium carbonate is the particle size at which the cumulative distribution (cumulative curve) reaches 50% when the cumulative distribution of the volume-based particle size distribution measured using a laser scattering method is expressed as 100%. When multiple types of calcium carbonate are used, the average particle size of calcium carbonate refers to the average particle size of all calcium carbonates.

[0080] [Dehydrating Agent] The curable composition preferably further contains a dehydrating agent, which can prevent the curable composition from being cured by moisture contained in the air or the like during storage.

[0081] Examples of dehydrating agents include silane compounds such as vinyltrimethoxysilane, dimethyldimethoxysilane, tetraethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, tetramethoxysilane, phenyltrimethoxysilane, and diphenyldimethoxysilane; and ester compounds such as methyl orthoformate, ethyl orthoformate, methyl orthoacetate, and ethyl orthoacetate. These dehydrating agents may be used alone or in combination. Among them, vinyltrimethoxysilane is preferred.

[0082] The content of the dehydrating agent in the curable composition is preferably 0.5 to 20 parts by mass, more preferably 1 to 15 parts by mass, per 100 parts by mass of the polymer having a hydrolyzable silyl group. When the content of the dehydrating agent is 0.5 parts by mass or more, the effect of the dehydrating agent is sufficiently obtained. On the other hand, when the content of the dehydrating agent is 20 parts by mass or less, the curable composition has excellent curability.

[0083] [Silanol Condensation Catalyst] The curable composition preferably contains a silanol condensation catalyst, which is a catalyst for promoting a dehydration condensation reaction between silanol groups formed by hydrolysis of hydrolyzable silyl groups contained in a polymer having a hydrolyzable silyl group.

[0084] Examples of silanol condensation catalysts include organotin compounds such as 1,1,3,3-tetrabutyl-1,3-dilauryloxycarbonyl distannoxane, dibutyltin dilaurate, dibutyltin oxide, dibutyltin diacetate, dibutyltin phthalate, bis(dibutyltin laurate)oxide, dibutyltin bis(acetylacetonate), dibutyltin bis(monoester maleate), tin octoate, dibutyltin octoate, dioctyltin oxide, dibutyltin bis(triethoxysilicate), bis(dibutyltin bistriethoxysilicate)oxide, and dibutyltin oxybisethoxysilicate; and organotitanium compounds such as tetra-n-butoxytitanate and tetraisopropoxytitanate. These silanol condensation catalysts may be used alone or in combination of two or more.

[0085] The silanol condensation catalyst is preferably 1,1,3,3-tetrabutyl-1,3-dilauryloxycarbonyl-distannoxane, which makes it possible to easily adjust the curing rate of the curable composition.

[0086] The content of the silanol condensation catalyst in the curable composition is preferably 1 to 10 parts by mass, more preferably 1 to 5 parts by mass, per 100 parts by mass of the polymer having a hydrolyzable silyl group. When the content of the silanol condensation catalyst is 1 part by mass or more, the curing rate of the curable composition can be increased, thereby shortening the time required for curing the curable composition. On the other hand, when the content of the silanol condensation catalyst is 10 parts by mass or less, the curable composition has an appropriate curing rate, and the handleability of the curable composition can be improved.

[0087] [Other Additives] The curable composition may contain other additives such as a thixotropic agent, an antioxidant, an ultraviolet absorber, a pigment, a dye, an anti-settling agent, and a solvent. Among these, the thixotropic agent, the ultraviolet absorber, and the antioxidant are preferred.

[0088] [Thixotropy-imparting agent] The thixotropy-imparting agent may be any agent capable of imparting thixotropy to the curable composition. Preferred examples of the thixotropy-imparting agent include hydrogenated castor oil, fatty acid bisamide, and fumed silica.

[0089] The content of the thixotropy-imparting agent in the curable composition is preferably 0.1 to 200 parts by mass, and more preferably 1 to 150 parts by mass, per 100 parts by mass of the polymer having a hydrolyzable silyl group. When the content of the thixotropy-imparting agent is 0.1 part by mass or more, thixotropy can be effectively imparted to the curable composition. Furthermore, when the content of the thixotropy-imparting agent is 200 parts by mass or less, the curable composition has an appropriate viscosity, improving the handleability of the curable composition.

[0090] [UV Absorber] Examples of the UV absorber include benzotriazole-based UV absorbers and benzophenone-based UV absorbers, and benzotriazole-based UV absorbers are preferred. The content of the UV absorber in the curable composition is preferably 0.1 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, per 100 parts by mass of the polymer having a hydrolyzable silyl group.

[0091] [Antioxidant] Examples of the antioxidant include hindered phenol antioxidants, monophenol antioxidants, bisphenol antioxidants, and polyphenol antioxidants, and preferably hindered phenol antioxidants. The content of the antioxidant in the curable composition is preferably 0.1 to 20 parts by mass, more preferably 0.3 to 10 parts by mass, per 100 parts by mass of the polymer having a hydrolyzable silyl group.

[0092] [Light Stabilizer] The curable composition preferably contains a hindered amine-based light stabilizer. The hindered amine-based light stabilizer can provide a curable composition that can maintain excellent rubber elasticity for a longer period of time after curing.

[0093] Examples of the hindered amine light stabilizer include a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate and methyl 1,2,2,6,6-pentamethyl-4-piperidylsebacate, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, dibutylamine / 1,3,5-triazine / N,N'-bis(2,2,6,6-tetramethyl-4-piperidyl-1,6-hexamethylenediamine) and N-(2,2,6,6 poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidyl)imino}], and a polycondensate of dimethyl succinate and 4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol.

[0094] Preferred examples of the hindered amine light stabilizer include NOR-type hindered amine light stabilizers. The NOR-type hindered amine light stabilizer can provide a curable composition that is inhibited from decreasing in rubber elasticity over time after curing.

[0095] The NOR hindered amine light stabilizer has an NOR structure in which an alkyl group (R) is bonded to a nitrogen atom (N) contained in a piperidine ring skeleton via an oxygen atom (O). The number of carbon atoms in the alkyl group in the NOR structure is preferably 1 to 20, more preferably 1 to 18, and particularly preferably 18. Examples of the alkyl group include linear alkyl groups, branched alkyl groups, and cyclic alkyl groups (saturated alicyclic hydrocarbon groups).

[0096] Examples of linear alkyl groups include methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-octyl, n-nonyl, and n-decyl groups. Examples of branched alkyl groups include isopropyl, isobutyl, sec-butyl, and tert-butyl groups. Examples of cyclic alkyl groups (saturated alicyclic hydrocarbon groups) include cyclopentyl, cyclohexyl, and cyclooctyl groups. In addition, the hydrogen atoms constituting the alkyl group may be substituted with halogen atoms (e.g., fluorine, chlorine, and bromine atoms) or hydroxyl groups.

[0097] Examples of the NOR type hindered amine light stabilizer include a hindered amine light stabilizer represented by the following formula (4).

[0098]

[0099] When a NOR-type hindered amine light stabilizer is used, it is preferable to use the NOR-type hindered amine light stabilizer in combination with a benzotriazole-based ultraviolet absorber or a triazine-based ultraviolet absorber, thereby providing a curable composition in which the decrease in rubber elasticity over time after curing is more significantly suppressed.

[0100] The content of the hindered amine light stabilizer in the curable composition is preferably 0.01 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, based on 100 parts by mass of the polymer having a hydrolyzable silyl group.

[0101] [Aminosilane Coupling Agent] The curable composition preferably contains an aminosilane coupling agent. By using an aminosilane coupling agent, the rubber elasticity and adhesiveness of the cured product of the curable composition can be improved. The aminosilane coupling agent refers to a compound containing a silicon atom to which an alkoxy group is bonded and a functional group containing a nitrogen atom in one molecule.

[0102] Specific examples of aminosilane coupling agents include 3-aminopropyltrimethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N,N'-bis-[3-(trimethoxysilyl)propyl]ethylenediamine, N,N'-bis-[3-(triethoxysilyl)propyl]ethylenediamine, N,N'-bis-[3-(methyldimethoxysilyl)propyl]ethylenediamine, N,N'-bis-[3-(trimethoxysilyl)propyl]hexamethylenediamine, and N,N'-bis-[3-(triethoxysilyl)propyl]hexamethylenediamine. These aminosilane coupling agents may be used alone or in combination of two or more.

[0103] Among these, preferred examples of the aminosilane coupling agent include 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and N-(2-aminoethyl)-3-aminopropyltriethoxysilane, and more preferred example is N-(2-aminoethyl)-3-aminopropyltrimethoxysilane.

[0104] The content of the aminosilane coupling agent in the curable composition is preferably 1 to 10 parts by mass, more preferably 1 to 5 parts by mass, per 100 parts by mass of the polymer having a hydrolyzable silyl group. When the content of the aminosilane coupling agent is within the above range, the adhesiveness of the cured product of the curable composition can be improved.

[0105] [Curable Composition] The curable composition can be produced by uniformly mixing the polymer having a hydrolyzable silyl group, the nitrogen-containing heterocyclic compound, the metal oxide, and additives added as needed under a vacuum atmosphere using a general-purpose means.

[0106] The curable composition has a sufficiently long tack-free time, excellent handleability, and a short time until curing. The curable composition can be sufficiently cured to the inside, and can impart excellent mildew resistance, flexibility, and resilience to the cured product produced by curing. Therefore, the curable composition can be used in various applications such as sealants, coating materials, adhesives, and paints.

[0107] The cured product obtained by curing the curable composition with moisture has excellent mold resistance. However, mold is likely to grow in wet areas such as kitchens, bathrooms, toilets, and washrooms. By using the above-mentioned curable composition, the cured product can be used effectively, maintaining excellent mold resistance for a long period of time, even in wet areas.

[0108] A method for applying a curable composition to a gap to obtain a sealing structure includes filling the gap with the curable composition, curing the composition, and then curing the composition by moisture in the air or in the components that make up the gap. The resulting sealing structure comprises a structural member of an architectural structure and a cured product of the curable composition that has been filled into the gap formed between adjacent structural members. Examples of structural members of architectural structures include wall parts such as exterior walls, interior walls, and ceilings, as well as sinks, bathtubs, and system kitchens, with structural members that make up wet areas being preferred.

[0109] The cured product of the curable composition has excellent flexibility and recovery, and therefore, even if the gap expands, the cured product can smoothly follow the changes in the gap and maintain a stable state of closing the gap.

[0110] Specifically, when a cured product of the curable composition is subjected to an elongational stress that stretches the cured product and then the elongational stress is removed, the cured product smoothly returns to the state it was in before the stress was applied. Therefore, despite changes in the gap, the cured product can maintain a state in which the gap is stably closed. Because the cured product can change to match the state of the gap, it does not loosen or crack within the gap and exhibits an excellent appearance. The cured product is less likely to develop surface irregularities during the shape change due to the stress, which can reduce dust accumulation and maintain an excellent appearance.

[0111] The present invention will be described in more detail below using examples, but the present invention is not limited thereto. Specific numerical values ​​of the blending ratios (content ratios), physical property values, parameters, etc. used in the following description can be replaced with the upper limit values ​​(numeric values ​​defined as "equal to or less than") or lower limit values ​​(numeric values ​​defined as "equal to or greater than") of the corresponding blending ratios (content ratios), physical property values, parameters, etc. described in the "Description of the Invention."

[0112] The following raw materials were used in the production of the curable compositions of the Examples and Comparative Examples. [Polymer having a hydrolyzable silyl group] Polyoxypropylene polymer 1 having a hydrolyzable silyl group (formula (2), R 3 is a propylene group, x: 155, y: 155, z: 155, R 4 : hydrogen atom, R 5 : methyl group, k: 2, main chain is polyoxypropylene, hydrolyzable silyl group (bonded to each molecular end): dimethoxysilyl group, average number of dimethoxysilyl groups per molecule: 3.0, number average molecular weight: 30,000, molecular weight distribution (Mw / Mn): 1.1, AGC product name "Excestar S6735D"

[0113] - Polyoxypropylene polymer 2 having a hydrolyzable silyl group (main chain: polyoxypropylene, hydrolyzable silyl groups bonded to both ends of the main chain, hydrolyzable silyl group: dimethoxysilyl group, average number of dimethoxysilyl groups per molecule: 2.0, number average molecular weight: 26,000, molecular weight distribution (Mw / Mn): 1.1, manufactured by AGC, product name "Excestar S4530") - Urethane polymer having a hydrolyzable silyl group (urethane polymer having trimethoxysilyl groups at the end of the main chain skeleton or in the side chain, manufactured by WACKER, product name "STP E-35", number average molecular weight: 30,000, average number of trimethoxysilyl groups per molecule: 2.0) - Acrylic polymer having a hydrolyzable silyl group (acrylic polymer having trimethoxysilyl groups at the end of the main chain skeleton or in the side chain, main chain skeleton: homopolymer of butyl acrylate, manufactured by Soken Chemical & Engineering Co., Ltd. Product name: "NE-4003B", number average molecular weight: 40,000, average number of trimethoxysilyl groups per molecule: 2.0

[0114] [Nitrogen-containing heterocyclic compounds] Zinc pyrithione (pyridine-based compound) Methyl benzimidazol-2-ylcarbamate (carbendazim) (imidazole-based compound)

[0115] [Metal oxides] Zinc oxide Magnesium oxide

[0116] [Filler] Calcium carbonate 1 (precipitated calcium carbonate, manufactured by Maruo Calcium Co., Ltd. under the trade name "Kalfain 200M", average particle size: 0.1 μm) Calcium carbonate 2 (heavy calcium carbonate, manufactured by Nitto Funka Co., Ltd. under the trade name "NCC2310", average particle size: 1.0 μm)

[0117] [Silanol condensation catalyst] Silanol condensation catalyst (1,1,3,3-tetrabutyl-1,3-dilauryloxycarbonyl-distannoxane, manufactured by Nitto Kasei Co., Ltd., trade name "Neostan U-130")

[0118] [Dehydrating agent] Vinyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KBM-1003")

[0119] [Aminosilane Coupling Agent] Aminosilane coupling agent (N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, product name "KBM-603" manufactured by Shin-Etsu Chemical Co., Ltd.)

[0120] (Examples 1 to 21, Comparative Examples 1 to 5) The above-mentioned polymer having a hydrolyzable silyl group, nitrogen-containing heterocyclic compound, metal oxide, filler, silanol condensation catalyst, dehydrating agent, and aminosilane coupling agent were mixed in the amounts shown in Table 1 in a sealed mixer under reduced pressure until the mixture was uniform, thereby obtaining curable compositions.

[0121] The resulting curable compositions were measured for mildew resistance, tack-free time, deep curing, flexibility and recovery in the following manner. The results are shown in Table 1.

[0122] The average particle size of all the calcium carbonate particles constituting the hardenable composition is shown in Table 1.

[0123] [Mold Resistance] (Initial Mold Resistance) (a) Preparation of Test Pieces The obtained curable composition was molded into a disk having a thickness of 500 μm and a diameter of 3 cm, and the disk was air-dried to prepare a test piece.

[0124] (b) Preparation of agar medium An agar medium was prepared by mixing 1 part by weight of Nonsar LN-1 (manufactured by Nippon Oil & Fats Co., Ltd.), 1 part by weight of Nonsar TN-1 (manufactured by Nippon Oil & Fats Co., Ltd.), 1 part by weight of peptone (manufactured by DIFCO), 1.5 parts by weight of agar, and 100 parts by weight of water in a plastic petri dish. (c) Preparation of mixed spore suspensions A mixture of 1 part by weight each of Nonsar LN-1 and Nonsar TN-1 and 1,000 parts by weight of water was autoclaved and cooled, and then eight of these mixtures were prepared. One of the following bacteria was dispersed in each mixture: Alternaria, alternata, Cladosporium cladosporioides, Ulocladium atra, Exophiala, and jeanselmei. Equal amounts of the liquids obtained from each bacteria were mixed to prepare mixed spore suspensions.

[0125] (d) Test Method for Antifungal Properties (Initial Antifungal Properties) The test specimens prepared in (a) were placed on an agar medium, 1 milliliter of the mixed spore suspension was sprayed onto the specimens, and the specimens were then cultured in a thermostatic chamber (23°C, relative humidity 95-100%). On the 28th day, the state of mold growth was evaluated according to the following evaluation criteria, and the results are shown in Table 1. (Evaluation criteria) 0: No mold growth was observed with the naked eye or under a microscope. 1: No mold growth was observed with the naked eye, but was clearly visible under a microscope. 2: Mold growth was observed with the naked eye, and the growth area did not exceed 1 / 4 of the total planar area of ​​the test specimen. 3: Mold growth was observed with the naked eye, and the growth area was at least 1 / 4 but not more than 1 / 2 of the total planar area of ​​the test specimen. 4: Mold grew well, and the growth area was at least 1 / 2 of the total planar area of ​​the test specimen.

[0126] (Mold resistance after immersion in hot water) In the above (a) preparation of test specimens, the obtained curable composition was used to form a disk having a thickness of 500 μm and a diameter of 3 cm, and after air-drying this disk, it was immersed in hot water at 50° C. for 4 weeks to obtain a test specimen. The initial mold resistance was evaluated in the same manner as in the evaluation of the test specimens, except that this test specimen was used.

[0127] (Tack-free time) The curable composition was applied to a metal plate to a coating thickness of 2 mm in an atmosphere of 23°C and 50% relative humidity. Every 5 minutes after application, the surface of the applied curable composition was touched with a metal spatula, and the time until the applied curable composition no longer adhered to the spatula was measured as the tack-free time (minutes).

[0128] (Deep Curability) The curable composition was filled into a cylindrical metal container with a bottom (inner diameter: 50 mm, depth: 15 mm), the surface was smoothed with a spatula, and the container was allowed to stand for 3 days in an atmosphere of 25°C and a relative humidity of 50%.

[0129] Next, the thickness of the cured portion of the curable composition filled in the container was measured using a measuring device (manufactured by Mitutoyo Corporation, trade name "Decimatic Indicator").

[0130] (Flexibility) A test specimen was prepared by applying a curable composition to a metal plate in a thickness of 2 mm under an atmosphere of 23°C and 50% relative humidity, and curing the curable composition for 7 days. The rubber elasticity of the test specimen was measured in terms of Shore A using an A-type durometer at a measurement temperature of 23°C in accordance with JIS K6253. The smaller the rubber elasticity, the better the flexibility.

[0131] (Resilience) Using the curable composition, an I-type specimen was prepared in accordance with the standard JTC S-0001 of the NPO Housing Exterior Wall Technical Center. The obtained specimen was cured for 28 days at an ambient temperature of 23°C and a relative humidity of 50%. The dimension L0 (mm) of the specimen in the elongation direction of the specimen, described below, was measured at an ambient temperature of 23°C. Next, the specimen was left at rest in a 100% elongation state at an ambient temperature of 23°C for 24 hours, and then the elongation of the specimen was released. After the elongation of the specimen was released, it was left on a flat plate (float glass plate) at an ambient temperature of 23°C for 1 hour. The surface on the flat plate on which the specimen was placed was formed into a low-friction surface on which the specimen could slide and move with almost no resistance. The dimension L1 (mm) of the specimen in the elongation direction was measured at an ambient temperature of 23°C. The recovery rate was calculated based on the following formula: Recovery rate (%) = 100 × L1 / L0

[0132]

[0133] The curable composition of the present invention has a sufficiently long tack-free time, excellent handleability, and a short time until curing. The curable composition can be sufficiently cured to the inside, and the cured product produced by curing can be imparted with excellent mildew resistance, flexibility, and resilience. Therefore, the curable composition can be used in various applications such as sealants, coating materials, adhesives, and paints.

[0134] (Cross-reference to related applications) This application claims priority based on Japanese Patent Application No. 2023-80451, filed on May 15, 2023, the disclosure of which is incorporated herein by reference in its entirety.

Claims

1. A curable composition comprising a polymer having a hydrolyzable silyl group, a nitrogen-containing heterocyclic compound, and a metal oxide.

2. The curable composition according to claim 1, further comprising a silanol condensation catalyst.

3. The curable composition according to claim 1 or 2, characterized in that it contains 0.1 to 50 parts by mass of a metal oxide per 100 parts by mass of the polymer having a hydrolyzable silyl group.

4. A curable composition according to claim 1 or 2, characterized in that the metal oxide is zinc oxide.

5. The curable composition according to claim 1 or 2, characterized in that the polymer having a hydrolyzable silyl group includes a polyoxyalkylene polymer having a hydrolyzable silyl group.

6. The curable composition according to claim 1 or 2, characterized in that it contains 0.05 parts by mass or more of a nitrogen-containing heterocyclic compound per 100 parts by mass of the polymer having a hydrolyzable silyl group.

7. A curable composition according to claim 1 or 2, characterized in that the nitrogen-containing heterocyclic compound contains at least one nitrogen-containing heterocyclic compound selected from the group consisting of pyridine compounds and imidazole compounds.

8. A sealant comprising the curable composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Room temperature-curable polyorganosiloxane composition

    JP2013194063A

  • Antibacterial and antifungal flame-retardant aromatic polycarbonate resin composition and its molded product

    JP2014024886A

  • Curable composition and cured product thereof

    JP2014208787A

  • Curable composition for crawling pest control, sealing material, and crawling pest control method

    WO2018079780A1