Resin composition, resin solution, and method for producing crosslinked coating film
The resin composition, featuring a polycarbonate resin, activated methylene block polyisocyanate, and an amine catalyst, addresses the adhesion issues of polycarbonate films by forming a crosslinked film with enhanced substrate bonding, improving durability and impact resistance.
Patent Information
- Application Number
- PCT/JP2024/018107
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-17
- Filing Date
- 2024-05-16
- Publication Date
- 2024-11-21
AI Technical Summary
Polycarbonate resin films exhibit poor adhesion to substrates, leading to peeling issues, despite their excellent durability and impact resistance, which limits their application in mechanical and electrical products.
A resin composition comprising a polycarbonate resin, activated methylene block polyisocyanate, and an amine catalyst, specifically formulated to enhance adhesion by incorporating terminal structures and monomer-derived units, is used to create a crosslinked film with improved bonding to substrates.
The resin composition significantly enhances the adhesion of the crosslinked film to substrates, reducing the likelihood of peeling and providing superior durability and impact resistance, making it suitable for applications in mechanical and electrical products.
Smart Images

Figure JP2024018107_21112024_PF_FP_ABST
Abstract
Description
Resin composition, resin solution, and method for producing crosslinked coating
[0001] The present invention relates to a resin composition, a resin solution, and the like, and more particularly to a resin composition containing a polycarbonate resin and capable of forming a crosslinked coating film that has excellent adhesion to a predetermined substrate.
[0002] Polycarbonate resins have excellent transparency and moldability, as well as excellent mechanical properties such as impact resistance, and are therefore used in electrical appliances, automobiles, and other mechanical products. Among these, polycarbonate resin solutions are known for obtaining functional thin films and for coating articles (Patent Document 1).
[0003] Although coatings obtained from polycarbonate resin solutions have excellent durability such as impact resistance, they have poor adhesion, and this property has been utilized in the production of easily peelable nail polish (Patent Document 2). Therefore, there is room for improvement in the adhesion between these coating films and substrates.
[0004] As a resin composition obtained by blending a polycarbonate resin with another resin, for example, a blend resin composition of a polycarbonate resin and a polyphenylene ether resin is known (Patent Document 3), but even with such a blend resin composition, adhesion is not sufficiently improved. Therefore, there is still a need for the development of a polycarbonate resin composition or the like that can improve adhesion between a coating film and a substrate.
[0005] Japanese Patent Application Laid-Open No. 4-268365 Japanese Patent Application Laid-Open No. 2014-024789 Japanese Patent No. 6340811
[0006] From the viewpoint of the need for coating films with excellent adhesion to substrates, there is a demand for the development of new resin compositions.
[0007] The present invention includes, for example, the following aspects: [1] A resin composition comprising a polycarbonate resin, an active methylene-based blocked polyisocyanate, and an amine-based catalyst, wherein the polycarbonate resin comprises a terminal structure (A) represented by the following general formula (1) and a monomer-derived structural unit (B) represented by the following general formula (2). (In formula (1), R 1 represents an alkylene group having 1 to 20 carbon atoms or an alkenylene group having 2 to 20 carbon atoms, each of which may have a substituent; R 2 ~R 3 each independently represents hydrogen, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, or an aryl group having 6 to 12 carbon atoms, each of which may have a substituent; Z represents an ether bond (-O-), a carbonyl group (-C(O)-), or an ester bond (-C(O)O-), or represents a single bond; a is an integer of 1 to 3; Y represents an ether bond or an ester group; and * represents the bond to the polymer main chain. (In formula (2), R 4 ~R 7 are each independently hydrogen, fluorine, chlorine, bromine, iodine, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or an aralkyl group having 7 to 17 carbon atoms, each of which may have a substituent; X is represented by any of the following formulas (3): (In formula (3), R8 and R9 each independently represent hydrogen, fluorine, chlorine, bromine, iodine, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or an aryl group having 6 to 12 carbon atoms, each of which may have a substituent, or R8 and R9 combine to form a carbocyclic ring having 5 to 20 carbon atoms or a heterocyclic ring having 5 to 12 elements, each of which may have a substituent, and R 10 and R 11 each independently represents hydrogen, fluorine, chlorine, bromine, iodine, an alkyl group having 1 to 9 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms, each of which may have a substituent; R 12 are each independently an alkylene group having 1 to 9 carbon atoms which may have a substituent, c represents an integer of 0 to 20, and d represents an integer of 1 to 500. [2] In the general formula (1), Z is a single bond, and R 1 is an alkylene group having 1 to 2 carbon atoms, and R 2 and R 3[3] The resin composition according to the above [1] or [2], wherein the general formula (1) is represented by the following formula (1-1): (In the above formula (1-1), * represents the bonding portion.) [4] The resin composition according to any one of the above [1] to [3], wherein the monomer represented by the general formula (2) is at least one selected from the group consisting of the following formulas (4) to (10): [5] The resin composition according to any one of the above [1] to [4], wherein the polycarbonate resin further contains a structural unit (C) derived from a monomer represented by the following formula (11) derived from a branching agent: [6] The resin composition according to any one of [1] to [5] above, wherein the hydroxyl value (OH value) of the polycarbonate resin is 0.5 to 10 mgKOH / g. [7] The resin composition according to any one of [1] to [6] above, wherein the isocyanate (NCO) content in the active methylene-based blocked polyisocyanate is 4.0 to 12.0 mass%. [8] The resin composition according to any one of [1] to [7] above, wherein the NCO / OH ratio (mol / mol) calculated from the isocyanate content in the active methylene-based blocked polyisocyanate and the hydroxyl value of the polycarbonate resin using the following formula (I) is 0.5 to 1.5. [9] The resin composition according to any one of the above [1] to [8], wherein the amine catalyst is a non-basic amine catalyst.
[10] The resin composition according to any one of the above [1] to [9], wherein the amine catalyst has a triphenylamine structure.
[11] The resin composition according to any one of the above [1] to
[10] , wherein the amine catalyst is one or more selected from the group consisting of the following formulae (12) to (14):
[12] The resin composition according to any one of [1] to
[11] above, comprising 0.05 to 0.5 parts by mass of the active methylene-based blocked polyisocyanate and 1 to 20 parts by mass of the amine catalyst relative to 10 parts by mass of the polycarbonate resin.
[13] The resin composition according to any one of [1] to
[12] above, comprising 10 to 95% by mass of the polycarbonate resin, 0.5 to 5.0% by mass of the active methylene-based blocked polyisocyanate, and 5.0 to 89.5% by mass of the amine catalyst, based on the total mass of the resin composition.
[0008]
[14] A resin solution comprising the resin composition according to any one of [1] to
[13] above and one or more solvents selected from the group consisting of halogen-based solvents, ester-based solvents, ether-based solvents, carbonate ester-based solvents, and ketone-based solvents.
[15] A method for producing a crosslinked coating, comprising removing the solvent from the resin solution according to
[14] above and heating the resulting solution at 50 to 150°C.
[16] The method according to
[15] above, wherein the crosslinked coating is formed on a PVB (polybutyral resin) substrate or a PET (polyethylene terephthalate resin) substrate.
[0009] According to the present invention, a resin composition or the like is provided that can realize a coating film with high adhesion to a predetermined substrate. The resin coating obtained from the resin composition or the like of the present invention has the characteristics of having stronger adhesion to the predetermined substrate and being less likely to peel off than conventional resin coatings.
[0010] The present invention relates to a resin composition containing a specific polycarbonate resin, an active methylene-based blocked polyisocyanate, and an amine-based catalyst, a resin solution containing the resin composition, a coating obtained from the resin solution, a method for producing a crosslinked coating, etc. The subject matter of the present invention will be described below.
[0011] 1. Resin Composition 1-1. Components of the Resin Composition and Their Contents As described above, the resin composition of the present invention contains a polycarbonate resin, an active methylene-based blocked polyisocyanate, and an amine catalyst. The resin composition preferably contains these components as a mixture. The resin composition preferably contains 0.05 to 0.5 parts by mass of the active methylene-based blocked polyisocyanate and 1 to 20 parts by mass of the amine catalyst per 10 parts by mass of the polycarbonate resin. The resin composition more preferably contains 0.07 to 0.4 parts by mass of the active methylene-based blocked polyisocyanate per 10 parts by mass of the polycarbonate resin, even more preferably 0.10 to 0.35 parts by mass or 0.09 to 0.30 parts by mass of the active methylene-based blocked polyisocyanate, and particularly preferably 0.10 to 0.30 parts by mass of the active methylene-based blocked polyisocyanate. Furthermore, the resin composition more preferably contains 1.5 to 18 parts by mass of the amine catalyst, even more preferably 1.5 to 15 parts by mass or 2 to 16 parts by mass of the amine catalyst, and particularly preferably 2.5 to 12 parts by mass or 3 to 10 parts by mass of the amine catalyst, relative to 10 parts by mass of the polycarbonate resin.
[0012] The resin composition contains, for example, 10 to 95 mass% of a polycarbonate resin, 0.5 to 5.0 mass% of an active methylene-based blocked polyisocyanate, and 5.0 to 89.5 mass% of an amine-based catalyst, based on the total mass of the resin composition. The resin composition preferably contains, based on the total mass of the resin composition, 30 to 90 mass% of the polycarbonate resin, more preferably 40 to 80 mass% of the polycarbonate resin, and even more preferably 50 to 76 mass% of the polycarbonate resin. The resin composition contains, for example, 0.3 to 7.0 mass% or 0.4 to 6.0 mass% of the active methylene-based blocked polyisocyanate, based on the total mass of the resin composition. The resin composition preferably contains, based on the total mass of the resin composition, 0.5 to 4.0 mass% of the active methylene-based blocked polyisocyanate, more preferably 0.5 to 3.0 mass% of the active methylene-based blocked polyisocyanate, and even more preferably 0.5 to 2.5 mass% of the active methylene-based blocked polyisocyanate. The resin composition preferably contains, based on the total mass of the resin composition, 5.0 to 89.5 mass% of the amine catalyst, more preferably 10 to 70 mass% or 15 to 75 mass% of the amine catalyst, even more preferably 20 to 60 mass% or 20 to 65 mass% of the amine catalyst, and particularly preferably 22 to 55 mass% or 22 to 50 mass% of the amine catalyst.
[0013] In the resin composition, the total weight of the polycarbonate resin, active methylene-based blocked polyisocyanate, and amine catalyst is, for example, 50% by mass or more, based on the total mass of the resin composition. The total weight of the polycarbonate resin, active methylene-based blocked polyisocyanate, and amine catalyst in the resin composition is preferably 70% by mass or more or 80% by mass or more, more preferably 90% by mass or more or 95% by mass or more, and particularly preferably 97% by mass or more or 99% by mass or more, based on the total mass of the resin composition. Furthermore, the resin composition may essentially contain only the polycarbonate resin, active methylene-based blocked polyisocyanate, and amine catalyst.
[0014] 1-2. Polycarbonate Resin The polycarbonate resin contains the terminal structure (A) of general formula (1). In the general formula (1) showing the terminal structure (A), R 1 R is an alkylene group having 1 to 20 carbon atoms or an alkenylene group having 2 to 20 carbon atoms, both of which may have a substituent. 1 is preferably R 1 is an alkylene group having 1 to 12 carbon atoms, more preferably an alkylene group having 1 to 6 carbon atoms, still more preferably an alkylene group having 1 to 4 carbon atoms, and particularly preferably an alkylene group having 1 or 2 carbon atoms.
[0015] In general formula (1), R 2 and R 3 are each independently hydrogen, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxy group having 1 to 10 carbon atoms which may have a substituent, or an aryl group having 6 to 12 carbon atoms which may have a substituent. 2 and R 3 is preferably hydrogen, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or an aryl group having 6 to 10 carbon atoms, more preferably hydrogen, an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, or an aryl group having 6 to 8 carbon atoms, and particularly preferably hydrogen, an alkyl group having 1 or 2 carbon atoms, an alkoxy group having 1 or 2 carbon atoms, or an aryl group having 6 or 7 carbon atoms.
[0016] In general formula (1), Z represents an ether bond (-O-), a carbonyl group (-C(O)-), an ester bond (-C(O)O-), or a single bond, preferably a single bond. In general formula (1), a represents an integer of 1 to 3, preferably an integer of 1 or 2, and more preferably 1. In general formula (1), Y represents an ether bond or an ester group (ester bond: *-C(O)O-), preferably an ether bond. As mentioned above, * in general formula (1) represents the bond to the polymer main chain in the polycarbonate resin.
[0017] A preferred embodiment of the terminal structure (A) is R1 is an alkylene group having 1 or 2 carbon atoms, and R 2 and R 3 is hydrogen, Y is an ether bond (—O—), Z is a single bond, and a is 1. A specific example is a terminal structure represented by formula (1-1).
[0018] In the polycarbonate resin, the structural unit of the terminal structure (A) preferably accounts for 10% by mass or less or 8% by mass, more preferably 6% by mass or less or 4% by mass or less, and even more preferably 2% by mass or less, based on the total weight of the polycarbonate resin. Also, in the polycarbonate resin, the structural unit of the terminal structure (A) preferably accounts for 0.3% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more or 2% by mass or more, based on the total weight of the polycarbonate resin.
[0019] The polycarbonate resin contains a structural unit (B) derived from a monomer of general formula (2). R in formula (2) 4 ~R 7 are each independently hydrogen, fluorine, chlorine, bromine, iodine, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or an aralkyl group having 7 to 17 carbon atoms, each of which may have a substituent. 4 ~R 7 is preferably hydrogen, an alkyl group having 1 to 12 carbon atoms, an aryl group having 6 to 10 carbon atoms, an alkenyl group having 2 to 8 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms, more preferably hydrogen, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 8 carbon atoms, an alkenyl group having 2 to 4 carbon atoms, an alkoxy group having 1 or 2 carbon atoms, or an aralkyl group having 7 to 10 carbon atoms, still more preferably hydrogen, an alkyl group having 1 to 3 carbon atoms, an aryl group having 6 or 7 carbon atoms, an alkenyl group having 2 or 3 carbon atoms, an alkoxy group having 1 carbon atom, or an aralkyl group having 7 or 8 carbon atoms, and particularly preferably hydrogen, an alkyl group having 1 or 2 carbon atoms, or an aryl group having 6 or 7 carbon atoms.
[0020] X in formula (2) is represented by any one of the following formulas (3). R8 and R9 in formula (3) are each independently any of hydrogen, fluorine, chlorine, bromine, iodine, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, and an aryl group having 6 to 12 carbon atoms, each of which may have a substituent, or R8 and R9 may combine to form a carbocycle having 5 to 20 carbon atoms or a 5- to 12-membered heterocycle. R8 and R9 are preferably hydrogen, an alkyl group having 1 to 3 carbon atoms, or a group which combines with each other to form a carbocycle having 5 to 12 carbon atoms.
[0021] R in formula (3) 10 and R 11 are each independently any one of hydrogen, fluorine, chlorine, bromine, iodine, an alkyl group having 1 to 9 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, and an aryl group having 6 to 12 carbon atoms, each of which may have a substituent. 10 and R 11 is preferably hydrogen or an aryl group having 6 to 8 carbon atoms. 12 are each independently an alkylene group having 1 to 9 carbon atoms, preferably an alkylene group having 1 to 3 carbon atoms, and more preferably an alkylene group having 1 or 2 carbon atoms, which may have a substituent. In formula (3), c is an integer of 0 to 20, and d is an integer of 1 to 500. c is preferably an integer of 0 to 10, and more preferably an integer of 0 to 3. d is preferably an integer of 1 to 300, and more preferably an integer of 1 to 100.
[0022] The above-mentioned substituents are each independently selected from halogen, a hydroxyl group, a cyano group, an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 1 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, etc., and when an alkyl group, an alkenyl group, or an aryl group is contained as a substituent, the above-mentioned R 1 ~R 12 The number of carbon atoms in the formula is the total number of carbon atoms including the carbon atoms of the substituents.
[0023] Preferred forms of the structural unit (B) include those derived from any of the monomers of the above formulae (4) to (10), and examples of bisphenol compounds that can form the structural unit (B) include the following. For example, 4,4'-biphenyldiol, bis(4-hydroxyphenyl)methane (bisphenol F; BPF), bis(2-hydroxyphenyl)methane, 2,4'-dihydroxydiphenylmethane, bis(4-hydroxyphenyl)ether, bis(4-hydroxyphenyl)sulfone, 2,4'-dihydroxydiphenylsulfone, bis(2-hydroxyphenyl)sulfone, bis(4-hydroxy-3-methylphenyl)sulfone, bis(4-hydroxyphenyl)sulfoxide, bis(4-hydroxyphenyl)sulfide, bis(4-hydroxyphenyl)ketone, 1,1-bis(4-hydroxyphenyl)ethane (bisphenol E; BPE), 1,1-bis( 4-hydroxyphenyl)-1-phenylethane (bisphenol AP; BPAP), bis(4-hydroxyphenyl)diphenylmethane (bisphenol BP; BPBP), 2,2-bis(4-hydroxyphenyl)propane (bisphenol A; BPA), 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(4-hydroxy-3-methylphenyl)ethane, bis(4-hydroxy-3-methylphenyl)methane, 2,2-bis(4-hydroxy-3-t-butylphenyl)propane, 2,2-bis(4-hydroxyphenyl)butane (bisphenol B; BPB), 1,1-bis(4-hydroxyphenyl)cyclohexane (bisphenol Z;BPZ), 1,1-bis(4-hydroxy-3-methylphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)cycloundecane, 1,1-bis(4-hydroxyphenyl)cyclododecane (bisphenol CD), 2,2-bis(4-hydroxy-3-allylphenyl)propane, 3,3,5-trimethyl-1,1-bis(4-hydroxyphenyl)cyclohexane, 9,9-bis(4-hydroxy-3-ethylphenyl)fluorene , 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 9,9-bis(4-hydroxyphenyl)fluorene, α,ω-bis[3-(o-hydroxyphenyl)propyl]polydimethyldiphenyl random copolymer siloxane, α,ω-bis[3-(o-hydroxyphenyl)propyl]polydimethylsiloxane, 4,4'-[1,4-phenylenebis(1-methylethylidene)]bisphenol, 4,4'-[1,3-phenylenebis(1 -methylethylidene) bisphenol, 2,2-bis(4-hydroxy-3-isopropylphenyl)propane (bisphenol G), 1,1-bis(4-hydroxyphenyl)-2-ethylhexane (bisphenol IOTD), 1,1-bis(4-hydroxyphenyl)-2-methylpropane (bisphenol IBTD), 1,1-bis(4-hydroxyphenyl)-2-methylpentane (bisphenol MIBK), 5,5'-(1-methylethylidene)-bis[1,1'-(bisphenyl)-2-ol]propane (bisphenol PH), 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane (bisphenol TMC), 2,2-bis(4-hydroxyphenyl)-4-methylpentane, 1,1-bis(4-hydroxyphenyl)decane, 1,3-bis(4-hydroxyphenyl)-5,7-dimethyladamantane, and the like. These may be used alone or in combination of two or more types.
[0024] Preferred embodiments of the structural unit (B) include structural units of the following formulae (4A) to (10A) derived from any of the monomers of the above formulae (4) to (10).
[0025] The polycarbonate resin may contain a structural unit (C) derived from a branching agent. Specific examples of preferred branching agents include those having multiple aromatic rings and multiple phenolic hydroxyl groups. Examples of structural units that can be contained in the polycarbonate resin include those derived from a branching agent represented by the following formula (11):
[0026] In the polycarbonate resin, the content of the structural unit (C) derived from the branching agent is preferably 15% by mass or less or 10% by mass or less, more preferably 8% by mass or less or 5% by mass or less, even more preferably 3% by mass or less or 2% by mass or less, and particularly preferably 1% by mass or less or 0.5% by mass or less, based on the total weight of the polycarbonate resin. In addition, the polycarbonate resin does not have to contain the structural unit (C).
[0027] The resin composition may contain a polyester carbonate resin or a polyester resin in addition to a polycarbonate resin. The polyester carbonate resin and polyester resin that can be contained in the resin composition preferably contain a structural unit formed from a monomer that results in the above-mentioned structural unit (B). Furthermore, the polycarbonate resin may contain a polyester carbonate structural unit or a polyester structural unit. The polyester carbonate structural unit and the polyester structural unit are preferably structural units formed from a monomer that results in the above-mentioned structural unit (B).
[0028] In the resin composition, the content of each of the polyester carbonate resin and the polyester resin is preferably 15% by mass or less or 10% by mass or less, more preferably 8% by mass or less or 5% by mass or less, even more preferably 3% by mass or less or 2% by mass or less, and particularly preferably 1% by mass or less or 0.5% by mass or less, based on the total weight of the polyester carbonate resin and the polycarbonate resin. The resin composition does not need to contain the polyester carbonate resin or the polyester resin. Furthermore, in the polycarbonate resin, the total content of the polyester carbonate structural unit and the polyester structural unit is preferably 15% by mass or less or 10% by mass or less, more preferably 8% by mass or less or 5% by mass or less, even more preferably 3% by mass or less or 2% by mass or less, and particularly preferably 1% by mass or less or 0.5% by mass or less, based on the total weight of the polyester carbonate resin and the structural unit (B). Furthermore, the polycarbonate resin does not need to contain the polyester carbonate structural unit or the polyester structural unit.
[0029] 1-3. Active Methylene Blocked Polyisocyanate The resin composition contains an active methylene blocked polyisocyanate. The active methylene blocked polyisocyanate is produced by reacting an active methylene compound with a polyisocyanate compound using a known method. Examples of active methylene compounds include acetoacetate ester compounds, malonic acid diester compounds, and the like. Examples of acetoacetate ester compounds include methyl acetoacetate, ethyl acetoacetate, isopropyl acetoacetate, n-propyl acetoacetate, t-butyl acetoacetate, n-butyl acetoacetate, benzyl acetoacetate, and phenyl acetoacetate. These acetoacetate ester compounds may be used alone or in combination. Examples of malonic acid diester compounds include dimethyl malonate, diethyl malonate, diisopropyl malonate, di-n-propyl malonate, di-n-butyl malonate, ethyl n-butyl malonate, methyl n-butyl malonate, ethyl t-butyl malonate, methyl t-butyl malonate, diethyl methylmalonate, dibenzyl malonate, diphenyl malonate, benzyl methyl malonate, ethyl phenyl malonate, t-butylphenyl malonate, isopropylidene malonate, etc. These malonic acid diester compounds may be used alone or in combination.
[0030] The polyisocyanate compounds described above are derived from, for example, aliphatic, alicyclic, or aromatic diisocyanates. Aliphatic diisocyanates having 4 to 30 carbon atoms are preferred, while alicyclic and aromatic diisocyanates having 8 to 30 carbon atoms are preferred. Examples of diisocyanate compounds include tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate (HDI), 2,2,4 or 2,4,4-trimethyl-1,6-diisocyanatohexane, lysine diisocyanate, isophorone diisocyanate (IPDI), 1,3-bis(isocyanatomethyl)-cyclohexane, 4,4'-dicyclohexylmethane diisocyanate, tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, tolidine diisocyanate, and xylylene diisocyanate. These diisocyanates may be used alone or in combination.
[0031] For example, polyisocyanates derived from the above-mentioned diisocyanates include isocyanurate-type polyisocyanates, biuret-type polyisocyanates, urethane-type polyisocyanates, allophanate-type polyisocyanates, etc. The average number of functional groups of the polyisocyanate is preferably 2 to 15.
[0032] The reaction between the active methylene compound and the polyisocyanate compound can be carried out by known methods. For example, the reaction between the active methylene compound and the polyisocyanate compound can be carried out with or without a solvent. When a solvent is used, it is preferable to use a solvent that is inactive to isocyanate groups. A catalyst may be used. Examples of the catalyst include organometallic compounds such as organolead compounds such as lead octoate, organotin compounds such as dibutyltin diacetate, dibutyltin dilaurate, tetrabutyldiacetoxystannoxane, and tin octoate, organozinc compounds such as zinc octoate, metal alcoholates such as sodium methylate, and tertiary amines such as triethylenediamine. The reaction between the active methylene compound and the polyisocyanate compound is carried out, for example, at a temperature of −20 to 150° C., preferably 0 to 100° C.
[0033] As the active methylene-based blocked polyisocyanate, an existing product such as Bronate 1232E (manufactured by Daiei Sangyo Co., Ltd.) can also be used.
[0034] 1-4. Amine Catalyst The resin composition contains an amine catalyst, i.e., a catalyst having an amine compound. As the amine catalyst, it is preferable to use a non-basic amine catalyst with low basicity. The non-basic amine catalyst has, for example, an amine compound whose conjugate acid has a pKa value of, for example, 6.0 or less, preferably 4.0 or less, more preferably 2.0 or less, even more preferably 1.0 or less, and particularly preferably 0 or less. The amine catalyst compound preferably has a phenyl group, more preferably has two or three phenyl groups, and particularly preferably has a triphenylamine structure.
[0035] Specific examples of preferred amine catalyst compounds include those represented by formulas (12) to (14).
[0036] 1-5. Other Components The resin composition may contain components other than the polycarbonate resin, the active methylene-blocked polyisocyanate, and the amine-based catalyst. For example, additives such as antioxidants, rust inhibitors, dispersants, UV absorbers, defoamers, and leveling agents may be contained in the resin composition. In the resin composition, the total weight of secondary components excluding the polycarbonate resin, the active methylene-blocked polyisocyanate, and the amine-based catalyst is, for example, 15% by mass or less, based on the total mass of the resin composition. The total weight of the secondary components is, for example, 12% by mass or less or 10% by mass or less, more preferably 8% by mass or less or 6% by mass or less, and particularly preferably 4% by mass or less, 2% by mass or less, or 1% by mass or less.
[0037] 1-6. Properties of Components in Resin Composition The polycarbonate resin preferably has a hydroxyl value (OH value) of 0.5 to 10 mgKOH / g, as measured by the method described below. The hydroxyl value of the polycarbonate resin is more preferably 0.7 to 9 mgKOH / g, even more preferably 1 to 8 mgKOH / g, and particularly preferably 3 to 6 mgKOH / g. The hydroxyl value of the polycarbonate resin is, for example, 0.1 mgKOH / g or more, preferably 0.3 mgKOH / g or more or 0.5 mgKOH / g or more, more preferably 0.7 mgKOH / g or more or 1.0 mgKOH / g or more, and particularly preferably 1.5 mgKOH / g or more or 2.0 mgKOH / g or more.
[0038] In the active methylene-based blocked polyisocyanate, the isocyanate (NCO) content, i.e., the proportion of the weight of NCO groups based on the total weight of the molecules of the active methylene-based blocked polyisocyanate, is preferably 4.0 to 12.0 mass%, more preferably 6.0 to 11.5 mass%, and even more preferably 9.0 to 11.0 mass%.
[0039] The NCO / OH ratio (mol / mol) of the active methylene-based blocked polyisocyanate is preferably 0.5 to 1.5. The NCO / OH ratio (mol / mol) is calculated from the above-mentioned isocyanate content and the hydroxyl value of the polycarbonate resin using the following formula (I): The NCO / OH ratio (mol / mol) in the active methylene-based blocked polyisocyanate is more preferably 0.7 to 1.4, and even more preferably 0.8 to 1.3.
[0040] The resin solution of the present invention contains the resin composition described above and a solvent. In the resin solution, the resin composition and the solvent can be mixed in any ratio, but the concentration of the resin composition in the resin solution is, for example, 1.0 to 70 wt %, preferably 5.0 to 50 wt %, and more preferably 10 to 30 wt %.
[0041] The solvent for the resin solution is preferably one that has high solubility for the resin composition, and is selected from the group consisting of, for example, halogen-based solvents, ester-based solvents, ether-based solvents, carbonate-based solvents, and ketone-based solvents. These solvents may be used alone or in combination.
[0042] The viscosity of the resin solution can be set arbitrarily depending on the desired coating method, but is preferably within the range of 10 to 20,000 mPa / s. For airless spray, brush coating, and roller coating, it is 400 to 20,000 mPa / s, for air spray, it is 100 to 6,000 mPa·s, and for dip coating and can spray, it is 10 to 500 mPa·s.
[0043] Pigments, dyes, colored particles, and particles with optical coherence can be added to the resin solution to enhance the color effect. Examples of pigments and dyes include organic pigments such as azo pigments and phthalocyanine pigments. Specific examples include Red No. 104, Red No. 106, Red No. 201, Red No. 202, Red No. 204, Red No. 215, Red No. 220, Orange No. 203, Orange No. 204, Blue No. 1, Blue No. 404, Yellow No. 205, Yellow No. 401, and Yellow No. 405. Titanium mica, titanium oxide, iron oxide, tin oxide, zirconium oxide, chromium oxide, bismuth oxychloride, silica, chromium, titanium nitride, titanium, magnesium fluoride, gold, silver, and nickel can also be used to create white, pearlescent, metallic, and glitter colors. Optical coherence particles are particles that enhance the color effect by reflecting or scattering light, and examples include glass beads, tiny shells, and mica. These are preferably added in the range of 0.0001 to 10.0% by mass in the coating as desired.
[0044] If necessary, a rust inhibitor, an antioxidant, a dispersant, an ultraviolet absorber, an antifoaming agent, a leveling agent, etc. may be added to the resin solution.
[0045] The amount of the resin composition in the coating resin solution of the present invention depends on the intrinsic viscosity and solvent solubility, but is preferably 1 to 50 mass %, more preferably 4 to 30 mass %. When the concentration is within this range, a good balance between solvent solubility and coatability is achieved, improving workability and appearance.
[0046] 3. Method for Producing Resin Composition The polycarbonate resin used in the present invention can be produced by a conventional method. For example, the method is as follows. The polycarbonate resin used in the present invention can be produced, for example, by reacting a monohydric phenol that derives the terminal structure (A), a bisphenol that derives the structural unit (B), and a carbonate ester-forming compound. Known methods can be used, such as the direct reaction of a bisphenol with phosgene (phosgene method) or the transesterification of a bisphenol with a bisarylcarbonate (transesterification method).
[0047] In the phosgene method, for example, a bisphenol, a monohydric phenol that induces the terminal structure (A), and phosgene are reacted in the presence of a typical acid binder and a solvent. Examples of acid binders include pyridine and alkali metal hydroxides such as sodium hydroxide and potassium hydroxide, and examples of solvents include methylene chloride and chloroform. Furthermore, to promote the condensation polymerization reaction, it is preferable to use a catalyst such as a tertiary amine such as triethylamine or a quaternary ammonium salt such as benzyltriethylammonium chloride. The monohydric phenol that induces the terminal structure (A) functions as a polymerization modifier, but it is also possible to use other monohydric phenols such as phenol, p-t-butylphenol, p-cumylphenol, and long-chain alkyl-substituted phenols in combination in an amount of less than 50% by mass relative to the monohydric phenol that induces the terminal structure (A). If desired, small amounts of antioxidants such as sodium sulfite and hydrosulfite, or branching agents such as phloroglucin and isatin bisphenol, may be added. The reaction temperature is usually 0 to 150°C, preferably 5 to 40°C. The reaction time varies depending on the reaction temperature, but is usually 0.5 minutes to 10 hours, preferably 1 minute to 2 hours. During the reaction, it is desirable to maintain the pH of the reaction system at 10 or higher.
[0048] On the other hand, in the transesterification method, for example, bisphenol, a monohydric phenol that induces the terminal structure (A), and a bisaryl carbonate are mixed and reacted at high temperature under reduced pressure. Examples of bisaryl carbonates include bisaryl carbonates such as diphenyl carbonate, di-p-tolyl carbonate, phenyl-p-tolyl carbonate, di-p-chlorophenyl carbonate, and dinaphthyl carbonate. Two or more of these compounds can also be used in combination. The reaction is typically carried out at a temperature ranging from 150 to 350°C, preferably from 200 to 300°C, and the final pressure reduction is preferably 1 mmHg or less, allowing phenols derived from the bisaryl carbonate produced by the transesterification reaction to be distilled out of the system. The reaction time varies depending on the reaction temperature and the degree of vacuum, but is typically about 1 to 24 hours. The reaction is preferably carried out under an inert gas atmosphere such as nitrogen or argon. If desired, the reaction may be carried out in the presence of a small amount of a molecular weight modifier other than the monohydric phenol which induces the terminal structure (A), or by adding an antioxidant or a branching agent.
[0049] The polycarbonate resin used in the present invention preferably maintains a good balance of solvent solubility, coatability, adhesion, scratch resistance, impact resistance, etc., which are necessary for a film-forming resin for a coating resin solution. If the resin's intrinsic viscosity is too low, scratch resistance and impact strength will be insufficient, while if the intrinsic viscosity is too high, solvent solubility will decrease and the solution viscosity will increase, resulting in reduced coatability. The desirable intrinsic viscosity range is preferably 0.3 to 2.0 dl / g, and more preferably 0.35 to 1.5 dl / g.
[0050] In the present invention, the resin composition contains an active methylene-based blocked polyisocyanate compound as described above. The active methylene-based blocked polyisocyanate compound contained in the polycarbonate resin composition is preferably a compound having two or more isocyanate groups per molecule. By using a compound having two or more isocyanate groups per molecule as the active methylene-based blocked polyisocyanate compound, a crosslinked structure can be formed in the resin composition, allowing a crosslinked coating to be produced.
[0051] 4. Method for Producing Resin Solution The resin solution of the present invention is a solution in which a resin composition is dissolved in the above-mentioned solvent, and in this state, it becomes a coating film generally called a clear color. Furthermore, a desired dye or pigment can be dissolved or dispersed to make a colored coating film.
[0052] 5. Crosslinked Coating and Coating Production Method A crosslinked coating can be produced by removing the solvent from a resin solution and heating the resulting resin composition. The heating step causes crosslinking and polymerization of the resin composition to form a coating. The temperature in the heating step is preferably 50 to 150°C, more preferably 70 to 130°C, and even more preferably 80 to 120°C.
[0053] The crosslinked coating is preferably formed on, for example, a PVB (polybutyral resin) substrate or a PET (polyethylene terephthalate resin) substrate. The crosslinked coating formed on these substrates has particularly excellent adhesion to the substrate. In this way, the coating obtained by coating a resin solution and curing it by heating is less likely to be scratched or peeled off due to friction, impact, etc. during transportation or use than coatings made from conventional resin solutions.
[0054] The thickness of the crosslinked coating is preferably in the range of 5 to 200 μm, particularly 10 to 120 μm, and even more preferably 15 to 60 μm. A coating less than 5 μm thick is not strong enough and is prone to scratches reaching the substrate, while a coating that is too thick, exceeding 200 μm, is prone to peeling due to shrinkage, which is economically disadvantageous considering the use of the coating, which will ultimately be peeled and discarded.
[0055] The resin solution described above can be used as a binder resin solution to produce a printing ink. Such a printing ink can be used, for example, in decorative printing. Generally, printing inks for decorative printing are primarily composed of a solvent, a dye / pigment, and a binder resin. Examples of dyes / pigments used in the printing ink include, but are not limited to, anthraquinone-based and naphthoquinone-based dyes, inorganic pigments such as titanium oxide, car pump rack, calcium carbonate, and metal particles, and organic pigments such as azo pigments and phthalocyanine pigments. These dyes / pigments are present in the ink in a dissolved or dispersed state together with the binder resin. Printing inks using the resin solution of the present invention as a binder resin solution have excellent adhesion.
[0056] In addition to the binder resin and the dye / pigment, the printing ink may contain organic fine particles, inorganic fine particles, a release agent, an antioxidant, a plasticizer, a dispersant, an infrared absorber, an antistatic agent, an ultraviolet absorber, an antifoaming agent, a leveling agent, etc., as necessary.
[0057] The amount of binder resin in the printing ink depends on the intrinsic viscosity and solvent solubility, but is preferably 1 to 70% by mass, more preferably 5 to 50% by mass. When the binder resin concentration is within this range, a good balance between solvent solubility and ink application properties is achieved, improving workability.
[0058] 6. Substrate Film The substrate film is, for example, one coated with the above-mentioned printing ink. After decorative printing on the substrate film before coating with the printing ink, the solvent is removed by drying, and the dye / pigment is fixed to the binder resin while the film and the binder resin are adhered together, thereby obtaining a decoratively printed film, i.e., a substrate film coated with the above-mentioned printing ink. Conventional methods can be used to apply the printing ink to the substrate, and examples include, but are not limited to, screen printing, gravure printing, and flexographic printing.
[0059] 7. Film or Coating The polycarbonate resin composition of the present invention may be used to form a film, a coating, or the like. The film or coating contains the polycarbonate resin composition described above, and the coating may be in a form other than a crosslinked coating. In one embodiment, a film or coating is provided that contains the polycarbonate resin composition described above or a crosslinked composition obtained by crosslinking at least a portion of the polycarbonate resin composition described above.
[0060] In one embodiment of the present invention, the coating can be obtained by applying a resin solution or printing ink to a substrate, followed by heating or drying. In one embodiment of the present invention, the coating can be a single layer or a multi-layer laminate.
[0061] Synthesis Example 1 In 1,200 parts by mass of a 5 wt% aqueous sodium hydroxide solution, 57.3 parts by mass of 1,1-bis(4-hydroxyphenyl)cyclohexane (hereinafter abbreviated as "BPZ": manufactured by Honshu Chemical Industry Co., Ltd.), 42.7 parts by mass of bis(4-hydroxyphenyl)methane (hereinafter abbreviated as "BPF": manufactured by Sanko Co., Ltd.), and 0.5 parts by mass of hydrosulfite were dissolved. 450 parts by mass of methylene chloride was added to the mixture, and while stirring, the mixture was further maintained at 15°C. Then, 60 parts by mass of phosgene was blown in over 40 minutes. After the phosgene blowing was completed, 2.74 parts by mass of p-hydroxyphenethyl alcohol (hereinafter abbreviated as "PHEP": manufactured by Otsuka Chemical Co., Ltd.) was added as a molecular weight modifier (end terminator) and stirred vigorously to emulsify the reaction solution. After emulsification, 0.5 parts by mass of triethylamine was added, and the mixture was stirred at 20 to 25°C for about 1 hour to allow polymerization. After the polymerization was completed, the reaction solution was separated into an aqueous phase and an organic phase, the organic phase was neutralized with phosphoric acid, and repeatedly washed with water until the conductivity of the initial solution (aqueous phase) was 10 μS / cm or less. The obtained polymer solution was added dropwise to warm water maintained at 50°C, and the solvent was evaporated to obtain a white powdery precipitate. The obtained precipitate was filtered and dried at 105°C for 24 hours to obtain a polymer powder. The intrinsic viscosity of a solution of this polymer in dichloromethane at a concentration of 0.5 g / dl at 20°C was 0.65 dl / g. The obtained polymer was analyzed by infrared absorption spectroscopy, and the intrinsic viscosity was 1770 cm -1Absorption due to carbonyl groups at a position near 1240 cm -1 Absorption due to ether bonds was observed in the vicinity of 1000, and it was confirmed that the polymer was a polycarbonate resin having carbonate bonds (hereinafter abbreviated as "PC-1"). The hydroxyl value of the obtained polymer was 5 mgKOH / g.
[0062] Synthesis Example 2 Polymerization was carried out in the same manner as in Synthesis Example 1, except that the amount of PHEP was changed to 0.97 parts by mass, to obtain a polycarbonate resin (intrinsic viscosity: 1.14 dl / g, hydroxyl value: 1 mgKOH / g, hereinafter abbreviated as "PC-2").
[0063] Synthesis Example 3 Polymerization was carried out in the same manner as in Synthesis Example 1, except that 48.2 parts by mass of 2,2-bis(4-hydroxyphenyl)-4-methylpentane (hereinafter abbreviated as "MIBK": manufactured by Honshu Chemical Industry Co., Ltd.) was used instead of BPZ, 1,1-bis(4-hydroxyphenyl)-1-phenylethane (hereinafter abbreviated as "BPAP": manufactured by Honshu Chemical Industry Co., Ltd.) was used instead of BPF, and 1.64 parts by mass of PHEP was used, to obtain a polycarbonate resin (intrinsic viscosity: 0.60 dl / g, hydroxyl value: 3 mgKOH / g, hereinafter abbreviated as "PC-3").
[0064] Synthesis Example 4: 60 parts by mass of 2,2-bis(4-hydroxyphenyl)propane (hereinafter abbreviated as "BPA"; manufactured by Honshu Chemical Industry Co., Ltd.) was used instead of BPZ, and 2,2-bis(4-hydroxy-3-methylphenyl)propane (hereinafter abbreviated as "BPC"; manufactured by Honshu Chemical Industry Co., Ltd.) was used instead of BPF. 0.05 parts by mass of benzyltriethylammonium chloride (manufactured by Fujifilm Wako Pure Chemical Industries Co., Ltd.) was also added as a phase transfer catalyst. Polymerization was carried out in the same manner as in Synthesis Example 1, except that the amount of PHEP was changed to 4.52 parts by mass, to obtain a polycarbonate resin (intrinsic viscosity: 0.41 dl / g, hydroxyl value: 8 mgKOH / g; hereinafter abbreviated as "PC-4").
[0065] Synthesis Example 5 Polymerization was carried out in the same manner as in Synthesis Example 1, except that 22.2 parts by mass of BPA was used instead of BPZ, 77.8 parts by mass of 2,2-bis(4-hydroxyphenyl)hexafluoropropane (hereinafter abbreviated as "BPAF": manufactured by Central Glass Co., Ltd.) was used instead of BPF, and 0.91 parts by mass of PHEP was used, to obtain a polycarbonate resin (intrinsic viscosity: 0.55 dl / g, hydroxyl value: 2 mgKOH / g, hereinafter abbreviated as "PC-5").
[0066] Synthesis Example 6 Polymerization was carried out in the same manner as in Synthesis Example 1, except that the amounts of BPZ and BPF were changed to 56.9 parts by mass and 42.5 parts by mass, respectively, and 0.70 parts by mass of 1,1,1-tris(4-hydroxyphenyl)ethane (hereinafter abbreviated as "TPE"; manufactured by Honshu Chemical Industry Co., Ltd.) was further added, to obtain a polycarbonate resin (intrinsic viscosity: 0.62 dl / g, hydroxyl value: 5 mgKOH / g; hereinafter abbreviated as "PC-6").
[0067] Synthesis Example 7 Polymerization was carried out in the same manner as in Synthesis Example 1, except that 0.84 parts by mass of 4-t-butylphenol (hereinafter abbreviated as "PTBP": manufactured by Dainippon Ink and Chemicals, Inc.) was used instead of PHEP, to obtain a polycarbonate resin (intrinsic viscosity: 0.93 dL / g, hydroxyl value: 0 mgKOH / g, hereinafter abbreviated as "PC-7").
[0068] 1) Intrinsic Viscosity A 0.5% by mass / volume solution of polycarbonate resin in dichloromethane was measured at 20°C with a Huggins constant of 0.45 using an Ubbelohde viscometer. Specifically, the viscosity average molecular weight (Mv) was measured and the intrinsic viscosity [η] was calculated as follows: Measuring instrument: Ubbelohde capillary viscometer Solvent: dichloromethane Resin solution concentration: 0.5 grams / dl Measurement temperature: 25°C The viscosity average molecular weight (Mv) was measured under the above conditions, and the intrinsic viscosity [η] (dl / gram) was calculated using the following formula with a Huggins constant of 0.45.
[0069] 2) Hydroxyl value According to JIS K 0070, 2 g of polycarbonate resin was dissolved in 80 mL of chloroform, and 2-propanol was added. This solution was titrated with a 0.01 mol / L KOH alcohol solution using a potentiometric titrator, and the obtained inflection point was taken as the endpoint. A blank test was conducted in the same manner, and the acid value was calculated using the following formula. Acid value (mg KOH / g) = (V1 - V0) × N × 56.11 × f / S, where S is sample mass (g), V0 is the volume of titrant in the blank test (mL), V1 is the volume of titrant in the main test (mL), N is the concentration of the titrant (mol / L), and f is the titrant factor (1.003). Furthermore, according to JIS K 0070, 25 g / L of acetic anhydride-pyridine solution was added to 10 g of polycarbonate resin, and after attaching an air-cooled tube, the mixture was heated in a 105°C oil bath for 2.5 hours. After water cooling, 1 mL of purified water was added, and the mixture was further heated in the oil bath for 20 hours. After water cooling, 5 mL of ethanol was added while rinsing the air-cooled tube, and then 60 mL of pyridine was added. This solution was titrated with 0.5 mol / L potassium hydroxide alcohol solution using a potentiometric titrator, and the obtained inflection point was taken as the endpoint. A blank test was conducted in the same manner, and the hydroxyl value was calculated using the following formula: Hydroxyl value (mg KOH / g) = [(V1 - V0) x N x 56.11 x f / S] + acid value, where S is sample mass (g), V0 is the volume of titrant in the blank test (mL), V1 is the volume of titrant in the main test (mL), N is the concentration of titrant (mol / L), and f is the titrant factor (1.001).
[0070] 3) Number of Cross-Cut Peelings The following cross-cut test was performed on the cross-linked coatings formed on PVB substrates and PET substrates obtained in the examples. Cross-cut: Six incisions were made in the cross-linked coating using a cutter, and then six more incisions were made perpendicularly at a 90° angle. This allowed 25 test specimen slices to be prepared on the substrate. Cellophane tape cut to 75 mm was adhered to each test specimen slice, and the Cellophane tape (registered trademark) was peeled off at a 60° angle. The number of test specimen slices peeled off from the PVB substrate or PET substrate was counted. The sum of the measured numbers of peeled test specimen slices on the PVB substrate and the PET substrate was used as the overall evaluation. Therefore, it can be said that the smaller the overall evaluation value shown in Table 1 below for Examples and Comparative Examples, the better the adhesion of the coating to the substrate.
[0071] Example 1 10 parts by mass of the polycarbonate resin (PC-1) obtained in Synthesis Example 1, 0.3 parts by mass of Bronate 1232E (hereinafter abbreviated as "BI-1": active methylene-based blocked isocyanate: manufactured by Daiei Sangyo Co., Ltd.), and 5.8 parts by mass of triphenylamine (hereinafter abbreviated as "CT-1": manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were dissolved in 70 parts by mass of dichloromethane to obtain a resin solution containing a resin composition. The resin solution was applied to a PVB substrate using a cast coater so that the dry film thickness was 60 to 100 μm, and then air-dried for 24 hours. Thereafter, a crosslinking reaction was carried out at 100° C. for 1 hour while simultaneously drying, and a crosslinked coating was formed on the PVB substrate. The PVB substrate was prepared by dissolving 3.5 parts by mass of PVB resin (S-LEC BX-1, manufactured by Sekisui Chemical Co., Ltd.) in 31.5 parts by mass of tetrahydrofuran, applying the solution to a glass substrate to a dry film thickness of 80 μm, air-drying for 24 hours, and then further drying at 100°C for 1 hour. The resin solution was also applied to a PET substrate using a cast coater to a dry film thickness of 60 to 100 μm, followed by air-drying for 24 hours. Subsequently, a crosslinking reaction was carried out at 100°C for 1 hour while simultaneously drying, forming a crosslinked coating on the PET substrate. The physical properties of the resulting crosslinked coating are shown in Table 1.
[0072] (Examples 2 to 11, Comparative Examples 1 to 8) A resin solution containing a resin composition was obtained and a crosslinked coating was formed in the same manner as in Example 1, except that the resin, polyisocyanate, and amine catalyst shown in Table 1 were used. The physical properties of the obtained crosslinked coating are shown in Table 1.
[0073]
[0074] As described above, it has been demonstrated that the resin composition of the present invention can improve the adhesion between the coating film and the substrate, and is useful as a blend resin composition of a polycarbonate resin and another resin.
[0075] The resin composition of the present invention can be used as a coating resin solution for protecting articles, and is particularly suitable for coatings in fields where durability in everyday life is required, such as IC cards and security cards.
Claims
1. A resin composition comprising a polycarbonate resin, an active methylene-based blocked polyisocyanate, and an amine-based catalyst, wherein the polycarbonate resin comprises a terminal structure (A) represented by the following general formula (1) and a monomer-derived structural unit (B) represented by the following general formula (2). (In formula (1), R 1 represents an alkylene group having 1 to 20 carbon atoms or an alkenylene group having 2 to 20 carbon atoms, each of which may have a substituent; R 2 ~R 3 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, each of which may have a substituent, an alkoxy group having 1 to 10 carbon atoms, or an aryl group having 6 to 12 carbon atoms; Z represents an ether bond (-O-), a carbonyl group (-C(O)-), or an ester bond (-C(O)O-), or represents a single bond; a is an integer of 1 to 3; Y represents an ether bond or an ester group; and * represents a bond to the polymer main chain. (In formula (2), R 4 ~R 7 are each independently hydrogen, fluorine, chlorine, bromine, iodine, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or an aralkyl group having 7 to 17 carbon atoms, each of which may have a substituent; X is represented by any of the following formulas (3): (In formula (3), R 8 and R 9 each independently represents hydrogen, fluorine, chlorine, bromine, iodine, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or an aryl group having 6 to 12 carbon atoms, each of which may have a substituent; R 8 and R 9 represents a group which combines to form a carbocyclic ring having 5 to 20 carbon atoms or a heterocyclic ring having 5 to 12 elements, each of which may have a substituent; R 10 and R 11 each independently represents hydrogen, fluorine, chlorine, bromine, iodine, an alkyl group having 1 to 9 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms, each of which may have a substituent; R 12 are each independently an alkylene group having 1 to 9 carbon atoms which may have a substituent, c represents an integer of 0 to 20, and d represents an integer of 1 to 500.
2. In the general formula (1), Z is a single bond, and R 1 is an alkylene group having 1 to 2 carbon atoms, and R 2 and R 3 The resin composition according to claim 1 , wherein is hydrogen.
3. The resin composition according to claim 1, wherein the general formula (1) is represented by the following formula (1-1): (In the above formula (1-1), * represents the bond.) 4. The resin composition according to claim 1, wherein the monomer represented by the general formula (2) is at least one selected from the group consisting of the following formulas (4) to (10):
5. The resin composition according to claim 1, wherein the polycarbonate resin further contains a structural unit (C) derived from a monomer represented by the following formula (11) derived from a branching agent:
6. The resin composition according to claim 1, wherein the polycarbonate resin has a hydroxyl value (OH value) of 0.5 to 10 mgKOH / g.
7. The resin composition according to claim 1, wherein the active methylene blocked polyisocyanate has an isocyanate (NCO) content of 4.0 to 12.0 mass %.
8. The resin composition according to claim 1, wherein the NCO / OH ratio (mol / mol) calculated from the isocyanate content in the active methylene blocked polyisocyanate and the hydroxyl value of the polycarbonate resin according to the following formula (I) is 0.5 to 1.
5.
9. The resin composition according to claim 1, wherein the amine catalyst is a non-basic amine catalyst.
10. The resin composition according to claim 1, wherein the amine catalyst has a triphenylamine structure.
11. The resin composition according to claim 1, wherein the amine catalyst is at least one selected from the group consisting of the following formulas (12) to (14):
12. The resin composition according to claim 1, comprising 0.05 to 0.5 parts by mass of the active methylene-based blocked polyisocyanate and 1 to 20 parts by mass of the amine-based catalyst per 10 parts by mass of the polycarbonate resin.
13. The resin composition according to claim 1, comprising, based on the total mass of the resin composition, 10 to 95 mass % of the polycarbonate resin, 0.5 to 5.0 mass % of the active methylene-based blocked polyisocyanate, and 5.0 to 89.5 mass % of the amine-based catalyst.
14. A resin solution comprising the resin composition according to any one of claims 1 to 13 and at least one solvent selected from the group consisting of halogen-based solvents, ester-based solvents, ether-based solvents, carbonate-based solvents, and ketone-based solvents.
15. A method for producing a crosslinked coating, comprising removing the solvent from the resin solution according to claim 14 and heating the solution at 50 to 150°C.
16. The method of claim 15, wherein the crosslinked coating is formed on a PVB (polybutyral resin) substrate or a PET (polyethylene terephthalate resin) substrate.
Citation Information
Patent Citations
Polycarbonate resin solution for forming cast film
JP1992268365A
Manicure solution
JP2014024789A
Polycarbonate resin composition and heat-resistant printing ink using the same
JP6340811B2
Polycarbonate-polydiorganosiloxane copolymer and manufacturing method thereof
JP2014080496A
Block polyisocyanate composition, one-liquid type coating composition, coated film and coated article
JP2017052917A