Target for film deposition and method for producing functional layer
The use of a film-forming target with specific elemental compositions for phase change storage devices and OTS elements addresses the stability and capacity challenges, resulting in enhanced switching performance and capacity.
Patent Information
- Application Number
- PCT/JP2024/018186
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-07-21
- Filing Date
- 2024-05-16
- Publication Date
- 2024-11-21
AI Technical Summary
Current phase change storage devices and Ovonic threshold switch (OTS) elements face challenges in achieving stable resistance changes with applied voltage, which limits their capacity and switching performance.
A film-forming target composed of Ge, Te, and other elements like Si, Al, Ga, Sn, Bi, Cu, Ag, Zn, Y, In, Ca, and Mg, with specific atomic percentages, is used to manufacture a functional layer that exhibits stable switching characteristics, suitable for large-capacity storage devices and OTS elements.
The proposed method enables the production of functional layers with improved stability and switching performance, enhancing the capacity and efficiency of phase change storage devices and OTS elements.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Film formation target and method for manufacturing functional layer
[0001] The present invention relates to a film formation target and a method for manufacturing a functional layer.
[0002] Next-generation nonvolatile memory devices have been attracting attention as a replacement for NAND flash memory. For example, phase-change memory devices have been proposed as next-generation nonvolatile memory devices. Phase-change memory devices include a functional layer made of a phase-change material and record information by utilizing the difference in electrical resistance between the amorphous and crystalline states of the phase-change material.
[0003] Furthermore, cross-point memory devices have attracted attention as a next-generation nonvolatile memory device structure (Patent Documents 1 and 2). Cross-point memory devices include word lines, bit lines that are orthogonal to the word lines in a planar view, and memory elements and switch elements that are arranged at the intersections of the word lines and bit lines in a planar view. Ovonic threshold switch (OTS) elements have been proposed as switch elements. OTS elements include a functional layer made of a variable resistance material, and achieve a switching action by utilizing the change in resistance due to an applied voltage.
[0004] JP 2006-086526 A JP 2018-164085 A
[0005] Phase-change memory devices are required to have a stable amorphous state in order to achieve even larger capacities, and OTS elements are required to exhibit stable resistance changes with applied voltage in order to achieve stable switching action.
[0006] In view of the above, an object of the present invention is to provide a film formation target and a method for manufacturing a functional layer suitable for manufacturing a large-capacity memory device or an OTS element exhibiting a stable switching action.
[0007] Various aspects of a film formation target and a method for manufacturing a functional layer that solve the above problems will be described.
[0008] The film formation target of aspect 1 is characterized by containing, in atomic %, 0.1% to 50% of Ge, 40% to 90% of Te, and 1% to 59% of Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg, and substantially no Sb.
[0009] The film formation target of aspect 2 is characterized by being made of bulk chalcogenide glass containing, in atomic %, 0.1% to 50% of Ge, 40% to 90% of Te, and 1% to 59% of Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg, and substantially no Sb.
[0010] The film formation target of aspect 3 is characterized by containing, in atomic %, 0.1% to 50% of Ge, 40% to 90% of Te, and 1% to 59% of Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg, and substantially no Sb, and including a crystalline portion.
[0011] The film formation target of Aspect 4 is any one of Aspects 1 to 3, and preferably has a relative density of 90% or more.
[0012] The film formation target of Aspect 5 is any one of Aspects 1 to 4, and preferably has an oxygen content of 0.001 ppm or more and less than 1% in atomic percent.
[0013] The film formation target of Aspect 6 is any one of Aspects 1 to 5, and preferably has a difference Δ(Tm−Tx) between the crystalline melting point Tm and the crystallization temperature Tx of 500° C. or less.
[0014] The film formation target of Aspect 7 is preferably used in the production of a resistance change layer in any one of Aspects 1 to 6.
[0015] The film formation target of Aspect 8 is preferably a disk-shaped target having a diameter of 20 mm to 300 mm, a thickness of 1 mm to 100 mm, and a surface roughness of less than 500 μm in any one of Aspects 1 to 7.
[0016] The film formation target of Aspect 9 is preferably any one of Aspects 1 to 8, further comprising a substrate.
[0017] A tenth aspect of the method for manufacturing a functional layer is a method for manufacturing a functional layer using a film formation target, characterized in that the film formation target is made of bulk chalcogenide glass containing, in atomic %, 0.1% to 50% Ge, 40% to 90% Te, and 1% to 59% Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg, and containing substantially no Sb, and a functional layer is manufactured that contains, in atomic %, 0.1% to 50% Ge, 40% to 90% Te, and 1% to 59% Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg, and containing substantially no Sb.
[0018] In the method for producing a functional layer of Aspect 11, in Aspect 10, it is preferable that a second film formation target be further provided.
[0019] In the method for producing a functional layer of Aspect 12, in Aspect 10 or Aspect 11, the functional layer is preferably a resistance change layer.
[0020] In the method for producing a functional layer of Aspect 13, in Aspect 10 or Aspect 11, the functional layer is preferably a phase-change layer.
[0021] The method for manufacturing a functional layer according to aspect 14 is a method for manufacturing a functional layer using a plurality of film-forming targets, the film-forming targets including a film-forming target made of a Ga alloy or a Ga compound, and the functional layer being a resistance change layer or a phase change layer containing, in atomic %, 0.1% to 50% of Ge, 0.1% to 50% of Ga, and 40% to 90% of Te.
[0022] In the method for producing a functional layer of Aspect 15, in any one of Aspects 10 to 14, it is preferable that the functional layer does not substantially contain Sb.
[0023] According to the present invention, it is possible to provide a film formation target and a method for manufacturing a functional layer that are suitable for manufacturing a large-capacity storage device or an OTS element that exhibits a stable switching action.
[0024] FIG. 1 is a schematic cross-sectional view of a switching element according to one embodiment of the present invention. FIG. 2 is a schematic cross-sectional view of a memory element according to a first embodiment of the present invention. FIG. 3 is a schematic three-dimensional view of a memory element according to the first embodiment of the present invention. FIG. 4 is a schematic three-dimensional view of a memory element according to the first embodiment of the present invention. FIG. 5 is a schematic three-dimensional view of a modified memory element according to the first embodiment of the present invention. FIG. 6 is a schematic cross-sectional view of a memory element according to a second embodiment of the present invention. FIG. 7 is a schematic three-dimensional view of a memory element according to the second embodiment of the present invention. FIG. 8 is a schematic three-dimensional view of a modified memory element according to the second embodiment of the present invention.
[0025] Preferred embodiments will be described below, but the following embodiments are merely examples and the present invention is not limited to the following embodiments.
[0026] <Film formation target> The film formation target of the present invention is characterized by containing, in atomic percent, 0.1% to 50% Ge, 40% to 90% Te, and 1% to 59% Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg, and is substantially free of Sb. By using a film formation target having this configuration, it is possible to manufacture a functional layer suitable for large-capacity storage devices and OTS elements that exhibit stable switching action. The functional layer is preferably a resistance change layer or a phase change layer. In the following description, the OTS element may also be referred to as a switching element.
[0027] In a broad aspect, the film deposition target of the present invention preferably contains, in atomic percent, 0.1% to 50% Ge and 40% to 90% Te, and at least a portion thereof comprises a chalcogenide glass. In other words, the film deposition target of the present invention preferably includes a glass portion containing, in atomic percent, 0.1% to 50% Ge and 40% to 90% Te. For example, the film deposition target of the present invention preferably includes a glass portion containing, in atomic percent, 0.1% to 50% Ge, 40% to 90% Te, and 1% to 59% Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg, and substantially no Sb. Film deposition targets including a glass portion reduce variations in density and composition and tend to improve homogeneity. Furthermore, the target has a high relative density and is likely to have high mechanical strength.
[0028] In a broad aspect, the film deposition target of the present invention is preferably made of bulk chalcogenide glass. For example, the film deposition target of the present invention is preferably made of bulk chalcogenide glass containing, in atomic percent, 0.1% to 50% Ge, 40% to 90% Te, and 1% to 59% Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg, and substantially no Sb. Here, "bulk" refers to a thickness of 0.1 mm or more. A film deposition target made of bulk chalcogenide glass is likely to have improved homogeneity and mechanical strength. Furthermore, it is likely to form the textured shape described below on the surface of the film deposition target, which can improve product life.
[0029] In a broad aspect, the film deposition target of the present invention preferably contains at least a portion of crystallized chalcogenide glass. In other words, the film deposition target of the present invention preferably includes a glass portion containing, in atomic percent, 0.1% to 50% Ge and 40% to 90% Te, and a crystalline portion. For example, the film deposition target of the present invention preferably includes a glass portion containing, in atomic percent, 0.1% to 50% Ge, 40% to 90% Te, and 1% to 59% Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg, and substantially no Sb, and a crystalline portion. The crystallized chalcogenide glass preferably has a crystallized structure in which, for example, 10% or more of the chalcogenide glass (glass portion) is crystallized, and more preferably 50% or more of the chalcogenide glass is crystallized. Film deposition targets containing a crystalline portion are more likely to have increased mechanical strength. The crystalline portion is preferably a Ge-based crystal or a Te-based crystal.
[0030] In one broad aspect, the film deposition target of the present invention may be configured to be a sintered body or a compact containing a chalcogenide glass powder. For example, the film deposition target of the present invention preferably comprises a sintered body or a compact containing a chalcogenide glass powder containing, in atomic percent, 0.1% to 50% Ge, 40% to 90% Te, and 1% to 59% Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg, and substantially no Sb. A film deposition target that is a sintered body or a compact containing a chalcogenide glass powder is advantageous in reducing manufacturing costs and can be easily made larger in diameter.
[0031] In the above configuration, the film deposition target may contain a powder (other powder) other than chalcogenide glass powder. The other powder may include, for example, a metal powder. For example, the film deposition target of the present invention preferably comprises a sintered or compacted mixture containing a chalcogenide glass powder and a metal powder, the mixture containing, in atomic percent, 0.1% to 50% Ge, 40% to 90% Te, and 1% to 59% Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg, and substantially no Sb. The metal powder may be a metal powder consisting of a single component, or may be an alloy powder. For example, it may be Ge powder, Te powder, or Ge-Te alloy powder. The film deposition target may be a sintered mixture of a chalcogenide glass powder and a metal powder, or may be a compacted mixture of a chalcogenide glass powder and a metal powder.
[0032] In a broad aspect, the film deposition target of the present invention may be configured to not contain chalcogenide glass. In other words, the film deposition target of the present invention may be configured to not contain a glass portion. For example, the film deposition target of the present invention may be configured to be a sintered or compacted powder of metal powder and not contain a glass portion. For example, the film deposition target of the present invention preferably contains, in atomic %, 0.1% to 50% Ge, 40% to 90% Te, and 1% to 59% Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg, and is substantially free of Sb, and is configured to be a sintered or compacted powder of metal powder. The metal powder may be a metal powder consisting of a single component, or may be an alloy powder. For example, it may be Ge powder, Te powder, or Ge-Te alloy powder. Alternatively, the film deposition target may be a metal plate (single metal or alloy) processed into a desired shape.
[0033] The film formation target of the present invention preferably has a relative density of 90% or more, 91% or more, 92% or more, 95% or more, particularly 98% or more. A film formation target satisfying the above-mentioned configuration has a small amount of voids and is easy to form a uniform film. The upper limit of the relative density is not particularly limited, but may be, for example, 100% or less, 99.9% or less, particularly 99% or less. Here, the relative density means the value obtained by dividing the measured density measured by Archimedes' method by the theoretical density. The theoretical density can be calculated from the composition of the film formation target.
[0034] From the viewpoint of reducing manufacturing costs, the film formation target of the present invention preferably has an oxygen content, in atomic percent, of 0.001 ppm or more, 0.01 ppm or more, particularly 0.1 ppm or more. On the other hand, from the viewpoint of suppressing the generation of oxygen impurities, the oxygen content is preferably less than 1%, 0.8% or less, 0.5% or less, 0.3% or less, 1000 ppm or less, 500 ppm or less, 100 ppm or less, particularly 50 ppm or less. The oxygen content of the film formation target can be evaluated, for example, using an inert gas fusion-infrared absorption method or the like.
[0035] The film formation target of the present invention preferably has a difference Δ(Tm-Tx) between the crystalline melting point Tm and the crystallization temperature Tx of 500° C. or less, 400° C. or less, 300° C. or less, particularly 250° C. or less. The lower limit of Δ(Tm-Tx) is not particularly limited, but may be, for example, 30° C. or more, 50° C. or more, 60° C. or more, particularly 80° C. or more. A film formation target having a Δ(Tm-Tx) value within the above range is suitable for producing a phase change layer.
[0036] The film formation target of the present invention preferably has a crystalline melting point (Tm) of 600°C or less, 550°C or less, 500°C or less, 450°C or less, 430°C or less, 410°C or less, particularly 400°C or less. A functional layer formed using a film formation target having such a configuration can reduce the energy required for phase change. In addition, in order to achieve a desired value of Δ(Tm-Tx), the lower limit of the crystalline melting point (Tm) is preferably, for example, 250°C or more, 260°C or more, 280°C or more, 300°C or more, 320°C or more, 340°C or more, 360°C or more, particularly 370°C or more.
[0037] The film formation target of the present invention preferably has a crystallization temperature Tx of 160°C or higher, 170°C or higher, 175°C or higher, 180°C or higher, 185°C or higher, 190°C or higher, 195°C or higher, 200°C or higher, 205°C or higher, particularly 210°C or higher. A functional layer formed using a film formation target having such a configuration is likely to stabilize the amorphous state. The upper limit of the crystallization temperature Tx is not particularly limited, but may be, for example, 600°C or lower, 500°C or lower, particularly 450°C or lower. In addition, in order to achieve the desired value of Δ(Tm-Tx), the upper limit of the crystallization temperature Tx is preferably, for example, 400°C or lower, 350°C or lower, particularly 300°C or lower.
[0038] The crystalline melting point Tm and crystallization temperature Tx of the film formation target can be evaluated using differential thermal analysis (DTA) or differential scanning calorimetry (DSC). Alternatively, the temperature dependence of electrical resistance may be measured using a two-terminal method, and the temperature at which the electrical resistance drops sharply may be evaluated as the crystallization temperature Tx. Furthermore, the film formation target may be heat-treated at a predetermined temperature, and the point at which a crystallization peak appears in XRD may be evaluated as the crystallization temperature Tx. It is preferable that the crystallization temperature Tx evaluated by any of the above methods falls within the above-mentioned range.
[0039] The film formation target of the present invention can be suitably used for producing a resistance change layer, although it may also be used for producing a phase change layer.
[0040] The film deposition target of the present invention is preferably disk-shaped. For example, the film deposition target is preferably disk-shaped with a diameter of 20 mm to 300 mm, a thickness of 0.1 mm to 100 mm, and a surface roughness of less than 500 μm. The film deposition target is not limited to a disk shape, and may be, for example, a plate shape, a rectangular plate shape, or a cylinder shape. In this case, the diameter of the film deposition target may be read as the major axis.
[0041] The diameter of the film formation target can be appropriately designed depending on the size of the functional layer to be produced. For example, the diameter of the film formation target is preferably 20 mm or more, 30 mm or more, particularly 50 mm or more. The upper limit of the diameter of the film formation target is not particularly limited, but is preferably, for example, 300 mm or less, 280 mm or less, particularly 260 mm or less.
[0042] The thickness of the film formation target is preferably 0.1 mm or more, 0.5 mm or more, 1 mm or more, 2 mm or more, 4 mm or more, particularly preferably 5 mm or more, and is preferably 100 mm or less, 90 mm or less, 80 mm or less, particularly preferably 50 mm or less. If the thickness of the film formation target is too small, the mechanical strength is likely to decrease. If the thickness of the film formation target is too large, the manufacturing cost of the film formation target is likely to increase.
[0043] The surface roughness of the film formation target is preferably less than 500 μm, 400 μm or less, 300 μm or less, particularly 200 μm or less, and is preferably 10 μm or more, 20 μm or more, particularly 50 μm or more. If the surface roughness of the film formation target is too small, the manufacturing cost of the film formation target tends to increase. If the surface roughness of the film formation target is too large, particles are likely to be generated during film formation, making it difficult to obtain a homogeneous functional layer.
[0044] The film formation target of the present invention may have an uneven surface. For example, when magnetron sputtering is performed, the surface of the film formation target is locally eroded (erosion). As the erosion progresses, abnormal discharge and changes in sputtering rate occur, making it necessary to replace the film formation target, leading to increased film formation costs. Therefore, by forming an uneven shape on the film formation target in advance that matches the erosion area, the product life of the film formation target and the manufacturing efficiency of functional layers can be improved. Note that film formation targets that at least partially contain chalcogenide glass or film formation targets made of bulk chalcogenide glass are easily formed with an uneven surface by press molding.
[0045] From the viewpoint of increasing the mechanical strength of the film formation target, the film formation target of the present invention preferably further comprises a substrate. The material of the substrate is not particularly limited, but it is preferable to use any one of a metal material, a ceramic material, and quartz glass. As the metal material, copper, molybdenum, aluminum, etc. are preferably used. As the ceramic material, alumina, etc. are preferably used.
[0046] From the viewpoint of particularly suppressing damage to the film formation target, the thickness of the substrate is preferably 100 μm or more, 200 μm or more, 500 μm or more, 800 μm or more, particularly 1000 μm or more. The upper limit of the thickness of the substrate is not particularly limited, but may be, for example, 10 mm or less, 5 mm or less, particularly 2 mm or less.
[0047] The reasons for specifying the composition of the film formation target as described above and the content of each component will be explained below. In the following explanation, "%" means "atomic %" unless otherwise specified. In addition, in the present invention, "x + y + z + ..." means the total content of each component. Here, each component does not necessarily have to be contained as an essential component, and it is acceptable for there to be components that are not contained (content 0%). Furthermore, "x + y + z + ... A% to B%" includes, for example, cases such as "x = 0%, y + z + ... A% to B%" and "x = 0%, y = 0%, z + ... A% to B%".
[0048] Ge is a component that stabilizes the amorphous state of the film formation target and the functional layer. The Ge content is preferably 0.1% to 50%. More specifically, the Ge content is preferably 0.1% or more, 1% or more, 3% or more, 5% or more, 7% or more, 10% or more, 11% or more, 13% or more, and particularly 15% or more, and is preferably 50% or less, 40% or less, 30% or less, and particularly 20% or less. If the Ge content is too low, the amorphous state tends to become unstable. If the Ge content is too high, it becomes difficult to obtain OTS characteristics. Furthermore, the manufacturing cost tends to increase.
[0049] The OTS characteristic refers to the characteristic of changing resistance value when a voltage is applied. The details are as follows: A variable resistance material exhibits high resistance in its initial state (off state). When a voltage is applied to this state, it maintains the high resistance state until it exceeds a threshold voltage, at which point it suddenly switches to a low resistance state (on state). When the applied voltage is reduced from the on state, it returns to the off state. Therefore, a material with OTS characteristics can be used as a switch layer and a switch element. The larger the ON / OFF current ratio, the better the characteristics as a switch element. Here, the ON current value refers to the current value (ON current value) that flows when a voltage equal to or greater than the threshold voltage is applied. The OFF current value refers to the current value (OFF current value) that flows when a voltage equal to 1 / 2 the threshold voltage is applied. The ON / OFF current ratio refers to the value obtained by dividing the ON current value by the OFF current value.
[0050] Te is an essential component constituting the film formation target and the functional layer. The Te content is preferably 40% to 90%. More specifically, the Te content is preferably 40% or more, 42% or more, 47% or more, 50% or more, more than 50%, 51% or more, 53% or more, 55% or more, 60% or more, 61% or more, 65% or more, 67% or more, 70% or more, particularly 71% or more, and is preferably 90% or less, 89% or less, 85% or less, 82.5% or less, particularly 80% or less. If the Te content is too low, the amorphous state tends to become unstable. Furthermore, it becomes difficult to obtain OTS characteristics. If the Te content is too high, the amorphous state tends to become unstable. Furthermore, the OFF current value increases, making it difficult to obtain OTS characteristics.
[0051] The Ge+Te content (total amount of Ge and Te) is preferably 41% or more, 45% or more, 50% or more, 60% or more, 65% or more, 70% or more, 75% or more, particularly 80% or more, and is preferably 99% or less, 98% or less, 97% or less, particularly 95% or less. If the Ge+Te content is too low, the amorphous state tends to become unstable. Also, it becomes difficult to obtain OTS characteristics. If the Ge+Te content is too high, it becomes difficult to obtain OTS characteristics.
[0052] Si, Al, Ga, Sn, Bi, Cu, Ag, Zn, Y, In, Ca, and Mg are components that stabilize the amorphous state of the film formation target and functional layer. These components also tend to reduce the OFF current and increase the ON / OFF current ratio. Therefore, the content of Si + Al + Ga + Sn + Bi + Cu + Ag + Zn + Y + In + Ca + Mg (the total amount of Si, Al, Ga, Sn, Bi, Cu, Ag, Zn, Y, In, Ca, and Mg) is preferably 0% to 59%, and particularly preferably 1% to 59%. More specifically, the content of Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg is preferably 0% or more, 1% or more, particularly 2% or more, and is preferably 59% or less, 58% or less, 55% or less, 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 13% or less, 10% or less, particularly 9% or less. The above content can also be rephrased as containing one or more components selected from Si, Al, Ga, Sn, Bi, Cu, Ag, Zn, Y, In, Ca, or Mg. If the content of these components is too low, the above effects are difficult to achieve. If the content of these components is too high, the amorphous state tends to become unstable. Furthermore, it is difficult to achieve OTS characteristics. The content of each of the components Si, Al, Ga, Sn, Bi, Cu, Ag, Zn, Y, In, Ca, and Mg is preferably 0% or more, more than 0%, 0.1% or more, 0.5% or more, 1% or more, and particularly preferably 2% or more, and is preferably 59% or less, 58% or less, 55% or less, 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 13% or less, 10% or less, and particularly preferably 9% or less.
[0053] Among the above components, Ga and Ag are components that tend to reduce the OFF current, and therefore particularly contribute to improving the ON / OFF current ratio. These components also tend to particularly stabilize the amorphous state. The Ga+Ag content (total amount of Ga and Ag) is preferably 0% or more, more than 0%, 0.1% or more, 0.5% or more, 1% or more, 2% or more, 3% or more, and particularly 5% or more. It is also preferably 59% or less, 58% or less, 55% or less, 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 13% or less, 10% or less, and particularly 9% or less.
[0054] In particular, from the viewpoint of reducing the OFF current, Ga / (Ga+Ag) is preferably 0.1 or more, particularly 0.2 or more, and is preferably 1.2 or less, less than 1.2, particularly 1.1 or less. Here, Ga / (Ga+Ag) is the value obtained by dividing the Ga content by the combined amount of Ga and Ag.
[0055] Sb is a component that easily destabilizes the amorphous state at high temperatures. Therefore, it is preferable that Sb is not substantially contained. In this specification, "substantially not contained" means that Sb is not intentionally contained in the raw materials, and does not exclude contamination at the impurity level. Objectively, it refers to the content of each component being less than 0.1%. If it is desired to strictly suppress Sb contamination, it is preferable that the Sb content be less than 0.05%, less than 0.01%, less than 0.005%, less than 0.001%, and particularly less than 0.0005%.
[0056] Se is a component that easily stabilizes the amorphous state of the film formation target and functional layer. The Se content is preferably 58% or less, 55% or less, particularly 50% or less, and is preferably 0% or more, 1% or more, 5% or more, 10% or more, particularly 20% or more. If the Se content is too high, the amorphous state tends to become unstable. Se is also a toxic component. Therefore, from the viewpoint of reducing the burden on the environment, it is preferable that the Se content be 40% or less, 30% or less, 20% or less, 10% or less, particularly substantially absent.
[0057] As is a component that easily stabilizes the amorphous state of the film formation target and the functional layer. However, As is a toxic component. Therefore, from the viewpoint of reducing the burden on the environment, it is preferable that the As content be 30% or less, 25% or less, 20% or less, 10% or less, 5% or less, 3% or less, and particularly that As be substantially absent.
[0058] The film formation target of the present invention preferably contains substantially no Se and no As, which further facilitates reducing the burden on the environment.
[0059] S is a component that easily stabilizes the amorphous state of the film formation target and the functional layer. However, since S has a low vapor pressure and is easily vaporized, there is a possibility that the heat applied during film formation may contaminate the inside of the film formation apparatus. Therefore, it is preferable that the S content be 40% or less, 30% or less, 20% or less, 10% or less, or particularly that S is substantially absent.
[0060] B, C, N, F, Cl, Br, and I are components that tend to stabilize the amorphous state of the film formation target and functional layer. The content of B + C + N + F + Cl + Br + I (total amount of B, C, N, F, Cl, Br, and I) is preferably 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 12% or less, 10% or less, 8% or less, 6% or less, and particularly preferably 5% or less. If the content of B + C + N + F + Cl + Br + I is too high, the amorphous state tends to become unstable. Furthermore, weather resistance tends to decrease. The content of each of the components B, C, N, F, Cl, Br and I is preferably 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 12% or less, 10% or less, 8% or less, 6% or less, and particularly preferably 5% or less.
[0061] The film formation target of the present invention may contain P, Cr, Mn, Ti, or Fe. The content of P + Cr + Mn + Ti + Fe (the total amount of P, Cr, Mn, Ti, and Fe) is preferably 10% or less, 5% or less, 1% or less, less than 1%, or 0.1%, and particularly preferably substantially none. If the content of these components is too high, the amorphous state tends to become unstable. The content of each of P, Cr, Mn, Ti, and Fe is preferably 10% or less, 5% or less, 1% or less, less than 1%, or 0.1%, and particularly preferably substantially none. If it is desired to strictly suppress the inclusion of P, Cr, Mn, Ti, and Fe, the contents of P, Cr, Mn, Ti, and Fe are preferably less than 0.05%, less than 0.01%, less than 0.005%, or less than 0.001%, and particularly preferably less than 0.0005%, respectively.
[0062] It is preferable that the film formation target of the present invention is substantially free of Cd, Tl, and Pb. This can further reduce the burden on the environment. When it is necessary to strictly suppress the inclusion of Cd, Tl, and Pb, the contents of Cd, Tl, and Pb are preferably less than 0.05%, less than 0.01%, less than 0.005%, less than 0.001%, and particularly less than 0.0005%, respectively.
[0063] The components of the film formation target and the functional layer described below can be evaluated using energy dispersive X-ray spectroscopy (EDX), electron probe microanalyzer (EPMA), X-ray fluorescence analysis (XRF), Rutherford backscattering analysis (RBS), etc. EDX may be evaluated using a TEM-EDX or SEM-EDX attached to a transmission electron microscope (TEM) or a scanning electron microscope (SEM), etc.
[0064] <Method for Manufacturing Functional Layer> In one broad aspect, the method for manufacturing a functional layer of the present invention preferably comprises a deposition target made of bulk chalcogenide glass containing, in atomic percent, 0.1% to 50% Ge and 40% to 90% Te, and a functional layer containing, in atomic percent, 0.1% to 50% Ge and 40% to 90% Te is manufactured. The functional layer is preferably a resistance change layer or a phase change layer.
[0065] The thickness of the functional layer is preferably 1 to 300 nm. More specifically, the thickness of the functional layer is preferably 1 nm or more, 2 nm or more, 5 nm or more, 10 nm or more, 30 nm or more, particularly preferably more than 50 nm, and is preferably 300 nm or less, 200 nm or less, particularly preferably 100 nm or less. If the thickness is too small, the current value (OFF current) in the high resistance state tends to be high. If the thickness is too large, the threshold voltage tends to be high.
[0066] The film formation method is preferably physical vapor deposition because it allows for easy composition control and film thickness control. For example, sputtering, vacuum deposition, ion plating, etc. are preferably used, and sputtering is particularly preferred. In this case, the film formation target of the present invention can be used as a sputtering target. The film formation method is not limited to physical vapor deposition, and may be CVD (chemical vapor deposition), ALD (atomic layer deposition), etc.
[0067] For example, film formation by sputtering can be performed by setting the substrate temperature to 15°C to 400°C, the flow rate of an inert gas such as argon gas as a sputtering gas to 2 sccm to 1000 sccm, the flow rate of oxygen gas to 0 sccm to 400 sccm, and the applied power to 1 W to 1 kW.
[0068] In order to fine-tune the film formation conditions for each component, the method for manufacturing a functional layer of the present invention may use multiple film formation targets to manufacture the functional layer. For example, the method for manufacturing a functional layer of the present invention may include a second film formation target, or may use three or more film formation targets. More specifically, for example, multiple film formation targets made of bulk chalcogenide glass may be used. A film formation target made of bulk chalcogenide glass may also be used in combination with a metal target. Furthermore, a film formation target made of bulk chalcogenide glass may also be used in combination with an alloy target. However, the film formation target is not limited to a configuration made of bulk chalcogenide glass, and various film formation targets described above may be used in combination. Furthermore, multiple film formation targets having the same components may be used in combination. However, from the perspective of simplifying the film formation process, using a single film formation target is preferred.
[0069] The method for manufacturing a functional layer of the present invention may use a film formation target that does not contain chalcogenide glass. For example, in a method for manufacturing a functional layer using multiple film formation targets, the film formation targets preferably include a film formation target made of a Ga alloy or a Ga compound, and the functional layer is a resistance change layer or a phase change layer containing, in atomic percent, 0.1% to 50% Ge, 0.1% to 50% Ga, and 40% to 90% Te. In this embodiment, at least one film formation target is made of a Ga alloy or a Ga compound. Metallic Ga has a low melting point of approximately 30°C and melts easily, making it difficult to handle. Therefore, in this embodiment, by using a film formation target made of an alloy or compound of Ga rather than simple metallic Ga, its melting point is increased, making it easier to handle. Examples of Ga alloys that can be used include Ga-Te alloys, Ga-In alloys, Ga-Sn alloys, Ga-Ge alloys, and Ga-In-Sn alloys. The Ga alloy is not limited to the above alloys, and may contain components such as Si, Al, Bi, Cu, Ag, Zn, Y, Ca, Mg, etc. Furthermore, as the Ga compound, for example, Ga oxide, Ga hydroxide, Ga nitride, Ga intermetallic compound, etc. can be used.
[0070] For example, in the method for producing a functional layer of the present invention, a film formation target made of a Ga alloy or Ga compound, a Te metal target, and a Ge metal target can be used in combination. For example, when a Ga-Te alloy is used as the Ga alloy or Ga compound, a film formation target made of a Ga-Te alloy can be used in combination with a Ge metal target. For example, when a Ga-Ge alloy is used as the Ga alloy or Ga compound, a film formation target made of a Ga-Ge alloy can be used in combination with a Te metal target.
[0071] The functional layer preferably contains, in atomic percent, 0.1% to 50% Ge and 40% to 90% Te, and more preferably 0.1% to 50% Ge, 0.1% to 50% Ga, and 40% to 90% Te. The detailed contents of each component are as follows:
[0072] Ge is a component that stabilizes the amorphous state of the functional layer. The Ge content is preferably 0.1% to 50%. More specifically, the Ge content is preferably 0.1% or more, 1% or more, 3% or more, 5% or more, 7% or more, 10% or more, 11% or more, 13% or more, and particularly preferably 15% or more, and is preferably 50% or less, 40% or less, 30% or less, and particularly preferably 20% or less. If the Ge content is too low, the amorphous state tends to become unstable. If the Ge content is too high, it becomes difficult to obtain OTS characteristics. Furthermore, the manufacturing cost tends to increase.
[0073] Te is an essential component constituting the functional layer. The Te content is preferably 40% to 90%. More specifically, the Te content is preferably 40% or more, 42% or more, 47% or more, 50% or more, more than 50%, 51% or more, 53% or more, 55% or more, 60% or more, 61% or more, 65% or more, 67% or more, 70% or more, particularly 71% or more, and is preferably 90% or less, 89% or less, 85% or less, 82.5% or less, particularly 80% or less. If the Te content is too low, the amorphous state tends to become unstable. Furthermore, it becomes difficult to obtain OTS characteristics. If the Te content is too high, the amorphous state tends to become unstable. Furthermore, the OFF current value increases, making it difficult to obtain OTS characteristics.
[0074] The Ge+Te content (total amount of Ge and Te) is preferably 41% or more, 45% or more, 50% or more, 60% or more, 65% or more, 70% or more, 75% or more, particularly 80% or more, and is preferably 99% or less, 98% or less, 97% or less, particularly 95% or less. If the Ge+Te content is too low, the amorphous state tends to become unstable. Also, it becomes difficult to obtain OTS characteristics. If the Ge+Te content is too high, it becomes difficult to obtain OTS characteristics.
[0075] Si, Al, Ga, Sn, Bi, Cu, Ag, Zn, Y, In, Ca, and Mg are components that stabilize the amorphous state of the functional layer. These components also tend to reduce the OFF current and increase the ON / OFF current ratio. Therefore, the content of Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg (the total amount of Si, Al, Ga, Sn, Bi, Cu, Ag, Zn, Y, In, Ca, and Mg) is preferably 0% to 59%, and particularly preferably 1% to 59%. More specifically, the content of Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg is preferably 0% or more, 1% or more, particularly 2% or more, and is preferably 59% or less, 58% or less, 55% or less, 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 13% or less, 10% or less, particularly 9% or less. The above content can also be rephrased as containing one or more components selected from Si, Al, Ga, Sn, Bi, Cu, Ag, Zn, Y, In, Ca, or Mg. If the content of these components is too low, the above effects are difficult to achieve. If the content of these components is too high, the amorphous state tends to become unstable. Furthermore, OTS characteristics are difficult to achieve. The content of each of the components Si, Al, Ga, Sn, Bi, Cu, Ag, Zn, Y, In, Ca, and Mg is preferably 0% or more, more than 0%, 0.1% or more, 0.5% or more, 1% or more, and particularly preferably 2% or more, and is preferably 59% or less, 58% or less, 55% or less, 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 13% or less, 10% or less, and particularly preferably 9% or less.
[0076] Among the above components, Ga and Ag are components that tend to reduce the OFF current, and therefore particularly contribute to improving the ON / OFF current ratio. These components also tend to particularly stabilize the amorphous state. The Ga+Ag content (total amount of Ga and Ag) is preferably 0% or more, more than 0%, 0.1% or more, 0.5% or more, 1% or more, 2% or more, 3% or more, and particularly 5% or more. It is also preferably 59% or less, 58% or less, 55% or less, 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 13% or less, 10% or less, and particularly 9% or less.
[0077] In particular, from the viewpoint of reducing the OFF current, Ga / (Ga+Ag) is preferably 0.1 or more, particularly 0.2 or more, and is preferably 1.2 or less, less than 1.2, particularly 1.1 or less. Here, Ga / (Ga+Ag) is the value obtained by dividing the Ga content by the combined amount of Ga and Ag.
[0078] Sb is a component that easily destabilizes the amorphous state of the functional layer at high temperatures. Therefore, it is preferable that Sb is not substantially contained. If it is necessary to strictly suppress the inclusion of Sb, the Sb content is preferably less than 0.05%, less than 0.01%, less than 0.005%, less than 0.001%, and particularly less than 0.0005%.
[0079] Se is a component that easily stabilizes the amorphous state of the functional layer. The Se content is preferably 58% or less, 55% or less, particularly 50% or less, and is preferably 0% or more, 1% or more, 5% or more, 10% or more, particularly 20% or more. If the Se content is too high, the amorphous state tends to become unstable. Se is also a toxic component. Therefore, from the viewpoint of reducing the burden on the environment, it is preferable that the Se content be 40% or less, 30% or less, 20% or less, 10% or less, and particularly substantially none.
[0080] As is a component that easily stabilizes the amorphous state of the functional layer. However, As is a toxic component. Therefore, from the viewpoint of reducing the burden on the environment, it is preferable that the As content be 30% or less, 25% or less, 20% or less, 10% or less, 5% or less, 3% or less, and particularly that As is substantially absent.
[0081] It is preferable that the functional layer contains substantially no Se or As, which further facilitates reducing the burden on the environment.
[0082] S is a component that easily stabilizes the amorphous state of the functional layer. However, since S has a low vapor pressure and is easily vaporized, there is a possibility that the heat applied during film formation may contaminate the inside of the film formation apparatus. Therefore, it is preferable that the S content be 40% or less, 30% or less, 20% or less, 10% or less, or particularly that S is substantially absent.
[0083] B, C, N, F, Cl, Br, and I are components that tend to stabilize the amorphous state of the functional layer. The content of B+C+N+F+Cl+Br+I (total amount of B, C, N, F, Cl, Br, and I) is preferably 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 12% or less, 10% or less, 8% or less, 6% or less, and particularly preferably 5% or less. If the content of B+C+N+F+Cl+Br+I is too high, the amorphous state tends to become unstable. Furthermore, weather resistance tends to decrease. The content of each of the components B, C, N, F, Cl, Br and I is preferably 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 12% or less, 10% or less, 8% or less, 6% or less, and particularly preferably 5% or less.
[0084] The functional layer may contain P, Cr, Mn, Ti, or Fe. The content of P + Cr + Mn + Ti + Fe (the total amount of P, Cr, Mn, Ti, and Fe) is preferably 10% or less, 5% or less, 1% or less, less than 1%, or 0.1% or less, and particularly preferably substantially absent. If the content of these components is too high, the amorphous state tends to become unstable. It is preferable that the content of each of P, Cr, Mn, Ti, and Fe is 10% or less, 5% or less, 1% or less, less than 1%, or 0.1% or less, and particularly preferably substantially absent. If it is desired to strictly suppress the inclusion of P, Cr, Mn, Ti, and Fe, it is preferable that the content of P, Cr, Mn, Ti, and Fe is less than 0.05%, less than 0.01%, less than 0.005%, or less than 0.001%, and particularly preferably less than 0.0005%, respectively.
[0085] It is preferable that the functional layer is substantially free of Cd, Tl, and Pb. This can further reduce the burden on the environment. If it is necessary to strictly suppress the inclusion of Cd, Tl, and Pb, the contents of Cd, Tl, and Pb are preferably less than 0.05%, less than 0.01%, less than 0.005%, less than 0.001%, and particularly less than 0.0005%, respectively.
[0086] As described above, the film formation target of the present invention can be suitably used for manufacturing a functional layer. The functional layer can be suitably used as a resistance change layer or a phase change layer. Therefore, the film formation target of the present invention can be suitably used for manufacturing a memory element used in a resistance change type memory device or a phase change type memory device, or a switch element used in various memory devices.
[0087] <Switch Element> Fig. 1 is a schematic cross-sectional view of a switch element according to one embodiment of the present invention. The switch element 10 includes a first electrode 1, a second electrode 2, and a functional layer disposed on a main surface of the first electrode 1. In this embodiment, the functional layer is a switch layer 3. The second electrode 2 is disposed opposite the first electrode 1. The switch layer 3 is disposed between the first electrode 1 and the second electrode 2. In other words, the switch element 10 of this embodiment includes the switch layer 3 and the first electrode 1 disposed on the switch layer 3. In further words, the switch element 10 of this embodiment includes a second electrode 2 disposed opposite the first electrode 1, with the switch layer 3 sandwiched between them.
[0088] The switch element 10 can be used in a cross-point type memory device or a Bit-Cost Scalable (BiCS) type memory device, which will be described later. In the case of a BiCS type memory device, the first electrode 1 of the switch element 10 is preferably disposed on the outer circumferential surface of the switch layer 3, and the second electrode 2 is preferably disposed on the inner circumferential surface of the switch layer 3.
[0089] The first electrode 1 and the second electrode 2 can be made of an inorganic material. The inorganic material is preferably a metal material or a ceramic material. The metal material is preferably at least one selected from the group consisting of tungsten, titanium, copper, and platinum. The ceramic material is preferably tungsten nitride or titanium nitride.
[0090] The thickness of the first electrode 1 and the second electrode 2 can be designed as appropriate. For example, the thickness of the first electrode 1 and the second electrode 2 is preferably 200 nm or less, 100 nm or less, 80 nm or less, 60 nm or less, and particularly preferably 50 nm or less, respectively. The smaller the thickness of the first electrode 1 and the second electrode 2, the more advantageous it is for increasing the capacity of the memory device. There is no particular limit to the lower limit of the thickness of the first electrode 1 and the second electrode 2, but it is preferably 1 nm or more, and particularly preferably 2 nm or more, respectively.
[0091] The switch layer 3 is a resistance change layer and exhibits OTS characteristics. The switch layer 3 is disposed in contact with at least one electrode. In other words, the switch layer 3 is preferably disposed on the first electrode 1. In yet another expression, the first electrode 1 is preferably disposed on the switch layer 3.
[0092] The thickness of the switch layer 3 can be appropriately designed depending on the desired threshold voltage. The thickness of the switch layer 3 is preferably, for example, 300 nm or less, 200 nm or less, particularly 100 nm or less. If the thickness of the switch layer 3 is too large, the threshold voltage is likely to become too large. The lower limit of the thickness of the switch layer 3 is preferably, for example, 1 nm or more, 2 nm or more, 5 nm or more, 10 nm or more, 30 nm or more, particularly more than 50 nm.
[0093] The ON / OFF current ratio of the switch element 10 is 1×10 4 That's it, 1 x 10 5 Above, especially 1 x 10 6 By satisfying the above values, the switching element 10 has excellent OTS characteristics.
[0094] <Memory Element> Fig. 2 is a schematic cross-sectional view of a memory element according to a first embodiment of the present invention. The memory element 20 includes a first electrode 11, a second electrode 12, a memory layer 4, and an insulator 5. The memory layer 4 is a functional layer formed using the film formation target of the present invention. The first electrode 11 is formed on the upper surface of the memory layer 4. The second electrode 12 is formed on the lower surface of the memory layer 4 and is disposed in a position facing the first electrode 11. The periphery of the second electrode 12 is covered with the insulator 5. In this embodiment, the memory layer 4 is disposed between the first electrode 11 and the second electrode 12.
[0095] The first electrode 11 and the second electrode 12 can be made of an inorganic material. The inorganic material can be a metal material or a ceramic material. The metal material is preferably at least one selected from the group consisting of tungsten, titanium, copper, and platinum. The ceramic material is preferably tungsten nitride or titanium nitride.
[0096] The thickness of the first electrode 11 and the second electrode 12 can be designed as appropriate. For example, the thickness of the first electrode 11 and the second electrode 12 is preferably 200 nm or less, 100 nm or less, 80 nm or less, 60 nm or less, and particularly preferably 50 nm or less. The smaller the thickness of the first electrode 11 and the second electrode 12, the more advantageous it is for increasing the capacity of the memory device. There is no particular limit to the lower limit of the thickness of the first electrode 11 and the second electrode 12, but it is preferably 1 nm or more, and particularly preferably 2 nm or more.
[0097] The configuration of the memory layer 4 varies depending on the type of memory. For example, in the case of a phase-change memory, the memory layer 4 is a phase-change layer. The memory layer 4 changes phase between a crystalline state and an amorphous state by applying a high voltage, allowing information to be recorded. For example, applying a high voltage to the memory layer 4 in a crystalline state and then rapidly heating and cooling it causes it to change to an amorphous state (first phase change). Furthermore, applying a voltage lower than that used for the first phase change to the memory layer 4 in an amorphous state and then gently heating and cooling it causes it to change to a crystalline state (second phase change). Information can be recorded by associating 0 and 1 with the amorphous state (high resistance state) and the crystalline state (low resistance state), respectively.
[0098] The memory layer 4 is in a crystalline state. 2 Sb 2 Te 5 , GeTe 4 , GeTe, Te and Ga 2 Te 3 It is preferable that at least one crystal selected from the group consisting of GeTe 4 Crystals require less energy for phase transition from the crystalline state to the amorphous state, which reduces the power consumption of the memory element.
[0099] <Memory Device> (First Embodiment) A memory device according to this embodiment includes a switch element and a memory element. FIGS. 3 and 4 are schematic three-dimensional diagrams of a memory device according to a first embodiment of the present invention. FIG. 4 is an enlarged view of a portion of the schematic three-dimensional diagram of FIG. 3. As shown in FIGS. 3 and 4, the memory device 100 includes a switch element 10, a memory element 20, a word line 30, and a bit line 40. The bit line 40 is orthogonal to the word line 30 in a plan view. The switch element 10 and the memory element 20 are disposed at the intersection of the word line 30 and the bit line 40 in a plan view. In other words, the memory device 100 is a cross-point memory device.
[0100] FIG. 5 is a schematic three-dimensional diagram of a modified example of the memory device according to the first embodiment of the present invention. The memory device 200 includes a switch element 10, a memory element 20, a word line 30, and a bit line 40. The bit line 40 is disposed in a through hole formed in the word line 30. The memory element 20 and the switch element 10 are disposed on the outer periphery of the bit line 40. The switch element 10 has a first electrode 1 disposed on the outer periphery of the switch layer 3, and a second electrode 2 disposed on the inner periphery facing the first electrode with the switch layer 3 interposed therebetween. In other words, the memory device 200 of this embodiment is a BiCS-type memory device. As such, the memory device of the present invention is not limited to a cross-point-type memory device, and may be various other memory devices.
[0101] The memory element 20 can be any memory element such as a resistance change memory element, a magnetoresistive memory element, a phase change memory element, or a ferroelectric memory element. Preferred embodiments of each memory element will be described below.
[0102] The resistance change memory element includes a resistance change layer. More specifically, the resistance change memory element preferably includes a stacked body in which a resistance change layer is sandwiched between a first electrode and a second electrode. The resistance change layer is preferably made of a metal oxide material, a metal nitride material, or a chalcogenide material. The metal oxide material is, for example, NiO x , NbO x , TiO x , TaO x , HfO x , ZrO x , MoO x , W.O. x, Pr 1-x Ca x MnO 3 (PCMO). The metal nitride material is preferably at least one selected from, for example, SiN x , AlN x , ZrN x , NiN x , CuN x , CrN x Preferably, the chalcogenide material is at least one selected from the group consisting of Ge—Te, Sb—Te, Ge—Sb—Te, Si—Sb—Te, Ge—Ga—Te, In—Sb—Te, Ge—Se—As, and Ge—Se—As—Te. The resistance change layer may be made of carbon nanotubes.
[0103] The magnetoresistive memory element includes a stack (TMR element) in which an insulating layer is sandwiched between ferromagnetic layers. The insulating layer is made of an insulating material, such as MgO, CaO, SrO, or Al. 2 O 3 The insulating layer preferably comprises at least one material selected from the group consisting of CoFeB, FeB, NiFe, MnIr, Fe, CoPt, CoNi, Co, Ni, Pt, Ni, and Mn. The insulating layer preferably comprises at least one material selected from the group consisting of CoFeB, FeB, NiFe, MnIr, Fe, CoPt, CoNi, Co, Ni, Pt, Ni, and Mn.
[0104] The ferroelectric memory element includes a ferroelectric layer. More specifically, the ferroelectric memory element preferably includes a stacked body having a ferroelectric layer sandwiched between a first electrode and a second electrode. The ferroelectric layer is preferably made of a ferroelectric material containing hafnium oxide, and is preferably made of hafnium oxide doped with at least one element selected from Si, Zr, Ge, Gd, La, Y, and Yb. The ferroelectric layer may also be made of at least one material selected from lead zirconate titanate (PZT), strontium bismuthate tantalate (SBT), and bismuth ferrite (BFO).
[0105] The phase-change memory element includes a memory layer made of a phase-change material. More specifically, the phase-change memory element preferably includes a stacked body having a phase-change layer sandwiched between a first electrode and a second electrode. The phase-change layer is preferably made of a chalcogenide material. The chalcogenide material is preferably at least one selected from, for example, Ge—Te, Sb—Te, Ge—Sb—Te, Si—Sb—Te, Ge—Ga—Te, In—Sb—Te, Cu—Ge—Te, Cr—Ge—Te, Mn—Te, Ge—Se—As, and Ge—Se—As-Te.
[0106] In the memory element, the first electrode 1 and the second electrode 2 can be made of an inorganic material. The inorganic material is preferably a metal material or a ceramic material. The metal material is preferably at least one selected from the group consisting of tungsten, titanium, copper, and platinum. The ceramic material is preferably tungsten nitride or titanium nitride.
[0107] Second Embodiment The memory device is not limited to a configuration in which a switch layer and a memory element are separately provided. For example, the memory device of this embodiment includes only a switch element. In this case, the switch element functions as both a switch element and a memory element.
[0108] 6 is a schematic cross-sectional view of a memory element according to a second embodiment of the present invention. As shown in FIG. 6 , a switch element 21 includes a first electrode 1, a second electrode 2, and a functional layer disposed on a major surface of the first electrode 1. In this embodiment, the functional layer is a switch layer 3. The second electrode 2 is disposed opposite the first electrode 1. The switch layer 3 is disposed between the first electrode 1 and the second electrode 2. In other words, the switch element 10 of this embodiment includes the switch layer 3 and the first electrode 1 disposed on the switch layer 3. In further words, the switch element 10 of this embodiment includes the second electrode 2 disposed opposite the first electrode 1, with the switch layer 3 sandwiched between them. The switch element 21 functions as both a switch element and a memory element.
[0109] 7 is a schematic three-dimensional diagram of a memory device according to a second embodiment of the present invention. As shown in FIG. 7, the memory device 101 includes a switch element 21, a word line 30, and a bit line 40. The bit line 40 is orthogonal to the word line 30 in a plan view. The switch element 21 is disposed at the intersection of the word line 30 and the bit line 40 in a plan view. In other words, the memory device 101 of this embodiment is a so-called cross-point type memory device.
[0110] 8 is a schematic three-dimensional diagram of a modified example of a memory device according to the second embodiment of the present invention. As shown in FIG. 8, a memory device 201 includes a switch element 21, a word line 30, and a bit line 40. The bit line 40 is disposed in a through hole provided in the word line 30. The switch element 21 is disposed on the outer periphery of the bit line 40. In other words, the memory device 201 of this embodiment is a so-called BiCS type memory device. As such, the memory device in this embodiment is not limited to a cross-point type memory device, and various other memory devices may be used.
[0111] The present invention will be described below based on examples, but the present invention is not limited to these examples.
[0112] Tables 1 to 7 show Examples 1 to 51 of the present invention and Comparative Example 1.
[0113]
[0114]
[0115]
[0116]
[0117]
[0118]
[0119]
[0120] The samples were prepared as follows. First, a quartz glass ampoule was heated and evacuated. After that, raw materials were mixed to the compositions shown in Tables 1 to 7 and placed in the quartz glass ampoule. Next, the quartz glass ampoule was sealed with an oxygen burner. Next, the sealed quartz glass ampoule was placed in a melting furnace, heated to 650 to 1000°C at a rate of 10 to 40°C / hour, and then held for 6 to 12 hours. During this holding time, the quartz glass ampoule was turned upside down to stir the melt. Finally, the quartz glass ampoule was removed from the melting furnace and rapidly cooled to room temperature to obtain a bulk chalcogenide glass sample. The bulk chalcogenide glass sample was cut and polished to obtain a disk-shaped film formation target with a diameter of 50.8 mm and a thickness of 3 mm. Examples 12 to 15, 39, and 51 contained a crystalline phase. The precipitated crystals were Ge crystals, Te crystals, and GeTe crystals. 4 , GeTe, Ga 2 Te 3 etc.
[0121] The crystallization temperature Tx of the obtained sample was measured by DTA.
[0122] As shown in Tables 1 to 7, the film formation targets of Examples 1 to 51 had higher crystallization temperatures Tx than Comparative Example 1. Furthermore, when a 150 nm-thick thin film was fabricated using the film formation targets of Example 1 and Example 42, the composition of the thin film obtained using the film formation target of Example 1 was, in atomic percent, 17.7% Ge, 6.3% Ga, 3.8% Ag, and 72.2% Te. Furthermore, the composition of the thin film obtained using the film formation target of Example 42 was, in atomic percent, 22.2% Ge, 16.8% Ga, 2.7% Ag, and 58.3% Te. The film formation was performed by Ar sputtering under a reduced pressure atmosphere. The substrate temperature was 15°C to 400°C, the Ar gas flow rate was 2 sccm to 1000 sccm, the oxygen gas flow rate was 0 sccm to 400 sccm, and the applied power was 1 W to 1 kW. The components of the thin film were measured using EDX.
[0123] Next, switching elements were fabricated using the film formation targets of Examples 1, 2, 5, and 8 and Comparative Example 1. First, Si / SiO 2A W electrode with a thickness of 50 nm was formed on the substrate. Next, a 100 nm thick SiO 2 An insulating layer was then formed. Then, a focus ion beam device (JEOL, JIB-4600F) was used to form a SiO 2 Holes of 500 nm in diameter were formed in the insulating layer and the W electrode layer. Next, a 150 nm thick switch layer was formed in the formed holes. Finally, a 150 nm thick W electrode was formed on the switch layer to fabricate a switch element. The film formation was performed by Ar sputtering under a reduced pressure atmosphere. The substrate temperature was 15°C to 400°C, the Ar gas flow rate was 2 sccm to 1000 sccm, the oxygen gas flow rate was 0 sccm to 400 sccm, and the applied power was 1 W to 1 kW. When the film formation target of Example 1 was used, the composition of the resulting switch layer was, in atomic percent, 17.7% Ge, 6.3% Ga, 3.8% Ag, and 72.2% Te. The composition of the switch layer was measured using EDX.
[0124] The ON / OFF current ratio x was calculated as follows. First, a voltage of 0V to 5V was applied to the switch element, and the current value flowing through the switch element and the threshold voltage were measured. Next, the ON / OFF current ratio was calculated by dividing the ON current value by the OFF current value. The ON current value was the current value that flows when a voltage equal to or greater than the threshold voltage was applied. The OFF current value was the current value that flows when a voltage equal to 1 / 2 the threshold voltage was applied. The results are shown in Table 8.
[0125]
[0126] As shown in Table 8, in the switch elements manufactured using the film formation targets of Examples 1, 2, 5, and 8, the ON / OFF current ratio log 10 The value of x was 4.6 or more, and an excellent switching action was exhibited. On the other hand, the switching element of Comparative Example 1 did not exhibit a switching action.
[0127] The film formation target and the method for manufacturing a functional layer of the present invention can be suitably used for manufacturing a large-capacity memory device or an OTS element exhibiting stable switching action, and in particular, can be suitably used for manufacturing a functional layer such as a resistance change layer or a phase change layer.
[0128] 1, 11 First electrode 2, 12 Second electrode 3 Switch layer 4 Memory layer 5 Insulator 10, 21 Switch element 20 Memory element 30 Word line 40 Bit line 100, 200, 101, 201 Memory device
Claims
1. A film formation target containing, in atomic %, 0.1% to 50% Ge, 40% to 90% Te, and 1% to 59% Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg, and substantially no Sb.
2. A film formation target made of bulk chalcogenide glass containing, in atomic percent, 0.1% to 50% Ge, 40% to 90% Te, and 1% to 59% Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg, and substantially no Sb.
3. A film formation target containing, in atomic %, 0.1% to 50% Ge, 40% to 90% Te, and 1% to 59% Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg, substantially no Sb, and including a crystalline portion.
4. The film formation target according to any one of claims 1 to 3, having a relative density of 90% or more.
5. A film formation target according to any one of claims 1 to 3, having an oxygen content, in atomic percent, of 0.001 ppm or more and less than 1%.
6. The film formation target according to any one of claims 1 to 3, wherein the difference Δ(Tm-Tx) between the crystal melting point Tm and the crystallization temperature Tx is 500°C or less.
7. The film formation target according to any one of claims 1 to 3, which is used for producing a resistance change layer.
8. The film formation target according to any one of claims 1 to 3, which is in the form of a disk having a diameter of 20 mm to 300 mm, a thickness of 1 mm to 100 mm, and a surface roughness of less than 500 µm.
9. The film formation target according to any one of claims 1 to 3, further comprising a substrate.
10. A method for manufacturing a functional layer using a film formation target, wherein the film formation target is made of bulk chalcogenide glass containing, in atomic %, 0.1% to 50% Ge, 40% to 90% Te, and 1% to 59% Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg, and substantially no Sb, and a functional layer is produced which contains, in atomic %, 0.1% to 50% Ge, 40% to 90% Te, and 1% to 59% Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg, and substantially no Sb.
11. The method for producing a functional layer according to claim 10, further comprising a second film formation target.
12. The method for producing a functional layer according to claim 10 or 11, wherein the functional layer is a resistance change layer.
13. The method for producing a functional layer according to claim 10 or 11, wherein the functional layer is a phase change layer.
14. A method for manufacturing a functional layer using a plurality of film-forming targets, the film-forming targets including a film-forming target made of a Ga alloy or a Ga compound, and the functional layer being a resistance change layer or a phase change layer containing, in atomic %, 0.1% to 50% Ge, 0.1% to 50% Ga, and 40% to 90% Te.
15. The method for producing a functional layer according to claim 10 or 14, wherein the functional layer does not substantially contain Sb.
Citation Information
Patent Citations
Phase change material and phase change memory element
WO2011030916A1
Cu-te-alloy-based sintered body sputtering target
WO2013035695A1
Phase change material
WO2023008432A1
Variable resistance material, switch element material, switch layer, switch element, and storage device
WO2023145795A1