Fabric for wet tissue and manufacturing method thereof
A fabric made from biodegradable bleached kraft and bamboo pulp, enhanced with specific additives, achieves strong and antibacterial properties, overcoming manufacturing issues and environmental impact of conventional wet tissue fabrics.
Patent Information
- Application Number
- PCT/KR2024/002560
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-17
- Filing Date
- 2024-02-28
- Publication Date
- 2024-11-21
AI Technical Summary
Conventional wet tissue fabrics lack sufficient tensile strength, leading to tearing during manufacturing, and are non-biodegradable, causing environmental pollution upon disposal.
A fabric composed of biodegradable bleached kraft pulp and bamboo pulp, with the addition of a dispersant, temporary wet strength enhancer, degassing agent, and softener, manufactured using a process involving fibrillation and dehydration to achieve enhanced tensile strength and antibacterial properties.
The resulting fabric exhibits excellent tensile strength, reduced defect rates during manufacturing, and superior antibacterial performance, while being biodegradable, thus addressing environmental concerns.
Smart Images

Figure KR2024002560_21112024_PF_FP_ABST
Abstract
Description
Fabric for wet tissues and its manufacturing method
[0001] This application claims the benefit of priority to Korean Patent Application No. 2023-0063530, filed May 17, 2023, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a fabric for wet tissues and a method for manufacturing the same, and more particularly, to a fabric for wet tissues that is biodegradable and antibacterial and has excellent tensile strength, and a method for manufacturing the same.
[0003]
[0004] As living standards rise, concern for hygiene is growing. Driven by this growing concern, most restaurants now provide wet wipes to their customers.
[0005] Generally, fabric for wet tissues is manufactured using a dry manufacturing method and then impregnated with purified water and detergent.
[0006] They are classified into several types depending on their use, such as multi-use wet tissues for daily necessities and single-use wet tissues for food service.
[0007] However, most wet tissue fabrics used in the past are dry-laid nonwovens made from materials such as general pulp, rayon, PP, and PE. Therefore, when wet tissue fabrics are manufactured using only general pulp, they lack sufficient tensile strength, leading to tearing during the manufacturing process. Furthermore, when rayon, PP, or PE are used, the decomposition period upon disposal is long, which can cause serious environmental pollution.
[0008]
[0009] (Prior art literature)
[0010] (Patent Document 1) Korean Patent Publication No. 2014-0033888
[0011] (Patent Document 2) Korean Patent Publication No. 2017-0040524
[0012] (Patent Document 3) Korean Patent Publication No. 1990743
[0013] (Patent Document 4) Korean Patent Publication No. 1808097
[0014]
[0015] The present invention was developed to solve the above problems, and its purpose is to provide a biodegradable wet tissue fabric having antibacterial properties and a method for manufacturing the same.
[0016] In addition, the present invention aims to provide a wet tissue fabric having excellent tensile strength and a method for manufacturing the same.
[0017]
[0018] To solve such technical problems, the fabric for wet tissues according to the present invention is characterized by including biodegradable bleached kraft pulp and bamboo pulp.
[0019] In addition, the wet tissue fabric according to the present invention is characterized in that it further comprises at least one of a dispersant, a temporary wetting strength enhancer, a degassing agent, and a softener.
[0020] In addition, the wet tissue fabric according to the present invention is characterized in that it contains 90 to 110 parts by weight of the bleached kraft pulp, 5 to 15 parts by weight of bamboo pulp, 0.01 to 0.10 parts by weight of a dispersant, 4 to 15 parts by weight of a temporary wet strength enhancer, 0.01 to 0.25 parts by weight of a deaerator, and 0.5 to 3 parts by weight of a softener.
[0021] In addition, in the wet tissue fabric according to the present invention, the bleached kraft pulp has a diameter of 10 to 20 ㎛ and a length of 1 to 4 mm, the bamboo pulp has a diameter of 5 to 15 ㎛ and a length of 1 to 4 mm, the dispersant is a nonionic surfactant, the temporary wetting strength enhancer is an amine type, the deaerator is a higher alcohol type, and the softener is a quaternary ammonium type.
[0022] In addition, the wet tissue fabric according to the present invention is characterized in that it satisfies a longitudinal tensile strength of 25 N / cm or more, a transverse tensile strength of 15 N / cm or more, a longitudinal wet tensile strength of 7 N / cm or more, and a transverse wet tensile strength of 5 N / cm or more.
[0023] In addition, a method for manufacturing a wet tissue fabric according to the present invention comprises: a first step of preparing raw materials; a second step of preparing a raw material mixture by mixing the prepared raw materials; a third step of fibrillating the prepared raw material mixture; a fourth step of laminating the fibrillated raw material mixture on a mesh belt; and a fifth step of dehydrating the raw material mixture laminated on the mesh belt; wherein the raw materials include biodegradable bleached kraft pulp and bamboo pulp.
[0024] In addition, in the method for manufacturing a wet tissue fabric according to the present invention, the raw material is characterized in that it further includes at least one of a dispersant, a temporary wetting strength enhancer, a deaerator, and a softener.
[0025] In addition, in the method for manufacturing a wet tissue fabric according to the present invention, in the first step, it is characterized in that water is prepared in a ratio of 9,900 to 11,000 parts by weight, bleached kraft pulp is 90 to 110 parts by weight, bamboo pulp is 5 to 15 parts by weight, dispersant is 0.01 to 0.10 parts by weight, temporary wet strength enhancer is 4 to 15 parts by weight, deaerator is 0.01 to 0.25 parts by weight, and softener is 0.5 to 3 parts by weight.
[0026] In addition, in the method for manufacturing a wet tissue fabric according to the present invention, it is characterized in that fibrillation is performed by applying a pressure in the range of 130 to 160 N in the third step.
[0027] In addition, in the method for manufacturing a wet tissue fabric according to the present invention, the bleached kraft pulp has a diameter of 10 to 20 ㎛ and a length of 1 to 4 mm, the bamboo pulp has a diameter of 5 to 15 ㎛ and a length of 1 to 4 mm, the dispersant is a nonionic surfactant, the temporary wetting strength enhancer is an amine type, the deaerator is a higher alcohol type, and the softener is a quaternary ammonium type.
[0028]
[0029] According to the wet tissue fabric of the present invention having the above-described composition and the method for manufacturing the same, since it includes bleached kraft pulp and bamboo pulp, it has the advantage of being biodegradable and having excellent antibacterial performance.
[0030] In addition, the wet tissue fabric of the present invention and its manufacturing method have the advantage of being able to suppress the occurrence of fraying during the manufacturing process because of their excellent tensile strength, thereby significantly reducing the defect rate of the wet tissue fabric.
[0031]
[0032] Figure 1 is a flow chart for explaining a method for manufacturing a wet tissue fabric according to a preferred embodiment of the present invention.
[0033]
[0034] Hereinafter, the present invention will be described in more detail with reference to preferred embodiments and drawings of the present invention. However, this is intended to be a detailed description to an extent that a person having ordinary skill in the technical field to which the present invention pertains can easily practice the present invention, and does not mean that the technical idea and scope of the present invention are limited thereby.
[0035] Additionally, unless otherwise defined, all terms used herein, including technical or scientific terms, have the same meaning as commonly understood by those of ordinary skill in the art to which this invention pertains. Terms defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning within the context of the relevant technology, and shall not be interpreted in an idealized or overly formal sense unless explicitly defined herein.
[0036]
[0037] Hereinafter, the wet tissue fabric of the present invention and its manufacturing method will be described in detail.
[0038] First, the wet tissue fabric of the present invention comprises bleached kraft pulp and bamboo pulp, is biodegradable and flexible, and has excellent tensile strength. The wet tissue fabric with the aforementioned characteristics can be used as a single-use wet tissue fabric or a multi-use wet tissue fabric.
[0039] First, bleached kraft pulp is a skeleton material that maintains the wet tissue fabric in a non-woven form.
[0040] Here, the bleached kraft pulp is preferably 10 to 20 ㎛ in diameter and 1 to 4 mm in length. If it is outside the above range, there is a problem of reduced tensile strength and absorbency, so it is preferably within the above range.
[0041] Bamboo pulp is expected to have antibacterial properties. Quinone, a bioactive compound found in bamboo, has excellent antibacterial properties. Bamboo is the tallest plant in the family Bambooaceae, and is primarily distributed in Southeast Asia, including Korea and Japan. Worldwide, there are approximately 1,250 species in 47 genera.
[0042] Representative bamboo species include king bamboo, cotton bamboo, maengjong bamboo, and jori bamboo. Among them, maengjong bamboo contains quinone derivatives, which are antibacterial ingredients, and thus has a strong antibacterial effect.
[0043] Here, it is preferable that the bamboo pulp have a diameter of 5 to 15 ㎛ and a length of 1 to 4 mm. If it goes beyond the above range, there is a problem of reduced tensile strength and absorbency, so it is preferable that it be within the above range.
[0044] It is preferable that bleached kraft pulp and bamboo pulp be mixed in a weight ratio of 90 to 110:5 to 15, and more preferably in a weight ratio of 98 to 102:10 to 12.
[0045] If the content of bleached kraft pulp is less than the above range, not only will the tensile strength of the wet tissue fabric be lowered, but also the absorbency will be reduced, making it difficult to commercialize. Conversely, if the content of bleached kraft pulp is greater than the above range, the antibacterial property will be lowered, so it is preferable that bleached kraft pulp be mixed within the above range.
[0046] In addition, if the content of bamboo pulp is less than the above range, the antibacterial performance is lowered, and conversely, if it is greater than the above range, the tensile strength and absorbency are lowered, so it is preferable that bamboo pulp be mixed within the above range.
[0047] In addition, it is preferable that the wet tissue fabric of the present invention include at least one of a dispersant, a temporary wetting power enhancing agent, a deaerator, and a softener, more preferably a dispersant, a temporary wetting power enhancing agent, and a deaerator, and most preferably a dispersant, a temporary wetting power enhancing agent, a deaerator, and a softener.
[0048] The dispersant shortens the dissociation time of bleached kraft pulp and bamboo pulp and further suppresses their agglomeration, and may be, for example, a nonionic surfactant.
[0049] Temporary wettability enhancers are ingredients that temporarily increase strength when wet. Examples include amine-based temporary wettability enhancers. While standard wettability enhancers can be used, they offer reduced flushability, making them preferable.
[0050] During the process of mixing raw materials and manufacturing sheet-shaped wet tissue fabric, a large number of fine bubbles may be generated due to the mixing of atmospheric air or the reaction between raw materials. These bubbles may cause breakage, resulting in the inability to form sheet-shaped wet tissue fabric, or the destruction of the bubbles during the drying process may significantly reduce the strength of the wet tissue fabric. To address the above-mentioned problems, the present invention adds a deaerator, which may be, for example, a high-grade alcohol-based deaerator.
[0051] A softener is a substance that improves the flexibility of fabric for wet tissues, and can be, for example, a quaternary ammonium softener.
[0052] Meanwhile, when including all of bleached kraft pulp, bamboo pulp, dispersant, temporary wet strength enhancer, deaerator, and softener, it is preferable to include 90 to 110 parts by weight of bleached kraft pulp, 5 to 15 parts by weight of bamboo pulp, 0.01 to 0.10 parts by weight of dispersant, 4 to 15 parts by weight of temporary wet strength enhancer, 0.01 to 0.25 parts by weight of deaerator, and 0.5 to 3 parts by weight of softener, and it is more preferable to include 98 to 102 parts by weight of bleached kraft pulp, 10 to 12 parts by weight of bamboo pulp, 0.02 to 0.06 parts by weight of dispersant, 4 to 11 parts by weight of temporary wet strength enhancer, 0.01 to 0.15 parts by weight of deaerator, and 0.5 to 3 parts by weight of softener.
[0053] As a result, when the bleached kraft pulp, bamboo pulp, dispersant, temporary wet strength enhancer, and deaerator satisfy the above mixing range, the tensile strength (MD, longitudinal direction) required for wet tissue fabric can be satisfied as 25 N / cm or more, the tensile strength (CD, transverse direction) as 15 N / cm or more, the wet tensile strength (MD, longitudinal direction) as 7 N / cm or more, and the wet tensile strength (CD, transverse direction) as 5 N / cm or more.
[0054]
[0055] Next, a method for manufacturing a wet tissue fabric according to the present invention will be described. Figure 1 is a flowchart illustrating a method for manufacturing a wet tissue fabric according to a preferred embodiment of the present invention.
[0056] As illustrated in FIG. 1, the method for manufacturing a wet tissue fabric of the present invention comprises a first step of preparing raw materials, a second step of preparing a raw material mixture by mixing the prepared raw materials, a third step of fibrillating the prepared raw material mixture, a fourth step of laminating the fibrillated raw material mixture on a mesh belt, a fifth step of dehydrating the raw material mixture laminated on the mesh belt, and a sixth step of drying.
[0057] In the first step of preparing raw materials, the solvent, bleached kraft pulp and bamboo pulp, and dispersing agent, temporary wetting strength enhancer, deaerator, and softener are prepared, respectively, as needed.
[0058] Here, the solvent may be water to ensure that each raw material is evenly mixed.
[0059] The second step is to prepare a raw material mixture by mixing the prepared raw materials. This is a step in which bleached kraft pulp and bamboo pulp, and if necessary, a dispersant, a temporary wetting strength enhancer, a deaerator, and a softener are added to water as a solvent and stirred to prepare a raw material mixture in the form of a slurry.
[0060] Here, it is preferable to mix in a ratio of 9900 to 11,000 parts by weight of water, 90 to 110 parts by weight of bleached kraft pulp, 5 to 15 parts by weight of bamboo pulp, 0.01 to 0.10 parts by weight of dispersant, 4 to 15 parts by weight of temporary wet strength enhancer, 0.01 to 0.25 parts by weight of deaerator, and 1 to 3 parts by weight of softener, and it is more preferable to mix in a ratio of 9900 to 11,000 parts by weight of water, 98 to 102 parts by weight of bleached kraft pulp, 10 to 12 parts by weight of bamboo pulp, 0.02 to 0.06 parts by weight of dispersant, 4 to 11 parts by weight of temporary wet strength enhancer, 0.01 to 0.15 parts by weight of deaerator, and 0.5 to 3 parts by weight of softener.
[0061] Meanwhile, here, it is preferable to preheat the solvent water to 25 to 45°C. This is because if the water temperature is lower than the above range, dispersibility and dehydration properties are poor, and conversely, if it is higher than the above range, a strain is placed on the mesh, etc. during lamination. Therefore, it is preferable that the solvent water temperature be within the above range.
[0062] And, the raw material mixture made of the above mixing ratio is stirred at a speed of 900 to 1100 RPM for about 15 to 25 minutes to obtain a raw material mixture slurry.
[0063] Specific properties related to bleached kraft pulp, bamboo pulp, dispersant, temporary wetting strength enhancer, deaerator, and softener have been described in detail above, so redundant descriptions are omitted.
[0064] The third step, which involves fibrillating the prepared raw material mixture, involves fibrillating the bleached kraft pulp. Specifically, fibrillation can be achieved by passing the pulp through a refiner once at a pressure of 130 to 160 N.
[0065] By performing fibrillation in this manner, the strength of the fabric can be increased while reducing the amount of wet strength enhancer or temporary wet strength enhancer used.
[0066] In the fourth step, where the fibrillated raw material mixture is layered onto a mesh belt, the prepared slurry-state raw material mixture is layered onto the mesh belt. Specifically, the raw material mixture is supplied to a mesh belt moving at a speed of 25 to 45 m / min, and the supply volume is preferably 5,000 to 8,000 L / min.
[0067] The fifth step of dehydrating the raw material mixture laminated on the mesh belt is a step of dehydrating the raw material mixture laminated on the mesh belt to primarily remove water, which is a solvent.
[0068] At this time, dehydration is performed by applying a primary vacuum at the moment when the raw material mixture is laminated on the mesh belt, and then applying a secondary vacuum to perform the dehydration process.
[0069] In the first vacuum dehydration process, vacuum pressure is applied in four stages. In the first stage, vacuum pressure is applied in the range of 0 to 5 cmHg, in the second stage, vacuum pressure is applied in the range of 10 to 20 cmHg, in the third stage, vacuum pressure is applied in the range of 30 to 40 cmHg, and in the fourth stage, vacuum pressure is applied in the range of 50 to 65 cmHg. In this process, dehydration induces bonding between fibers, which is then formed into a porous nonwoven fabric.
[0070] In the secondary vacuum dehydration process, a vacuum pressure of approximately 18 to 22 cmHg is applied to remove residual moisture and at the same time make the bond between fibers more dense.
[0071] The final, sixth step of drying is a step to completely remove residual moisture, which is achieved by sequentially passing the product through a hot air dryer and a drum dryer. Specifically, the process is sequentially performed as follows: first drying in a hot air dryer operating at 100 to 170°C, more preferably 110 to 130°C, then second drying with hot air at 135 to 145°C, third drying with hot air at 100 to 110°C, and fourth passing through a drum dryer operating at 135 to 145°C.
[0072] Here, if drying is performed at high temperatures in the early stages of the drying process, drying will occur rapidly, resulting in shrinkage or fraying. Conversely, if the temperature is too low, the binder fibers will not fully bond, and the remaining moisture after winding will be high, which can negatively impact subsequent processes, such as fluffing or weakened bonding. Therefore, it is recommended to perform drying under four drying conditions, from the first to the fourth stages, as described above.
[0073] Afterwards, if necessary, an additional process of slitting with a slitting device and then storing may be performed.
[0074]
[0075] Hereinafter, the present invention will be described in more detail with reference to examples and experimental examples. However, the following examples and experimental examples are merely illustrative of the present invention, and the content of the present invention is not limited to the following examples and experimental examples.
[0076]
[0077] <Example>
[0078] Example 1
[0079] A raw material mixture was prepared by mixing 100 kg of bleached kraft pulp with an average diameter of 10 to 20 μm and an average length of 1 to 4 mm, 11 kg of bamboo pulp with an average diameter of 5 to 15 μm and an average length of 1 to 4 mm, 0.05 kg of nonionic surfactant, 10 kg of amine-based temporary wetting strength enhancer, 1 kg of softener, and 0.1 kg of high-grade alcohol-based deaerator in 10,000 L of water heated to 30°C, and stirring for approximately 20 minutes.
[0080] The prepared raw material mixture was fibrillated once through a refiner at a pressure of 140 to 145 N to achieve a freeness of 500 to 550 CSF. The prepared raw material mixture was then laminated onto an ultrafine mesh belt. The mesh belt conveying speed was 35 m / min, and the supplied raw material mixture was maintained at 6,500 L / min.
[0081] In addition, the first stage of natural dehydration was performed at a vacuum pressure of 0 cmHg at the moment when the raw material mixture was stacked on the mesh belt, followed by the first stage of dehydration at a vacuum pressure of 10 cmHg in the second stage, 30 cmHg in the third stage, and 50 cmHg in the fourth stage. After the first dehydration, the second dehydration was performed at a vacuum pressure of 20 cmHg.
[0082] Finally, the fabric was dried first in a hot air dryer operating at 110 to 130°C, dried secondarily at 135 to 145°C, dried thirdly at 100 to 110°C, and passed through a drum dryer operating at 135 to 145°C to remove residual moisture, thereby manufacturing a fabric for wet tissues.
[0083]
[0084] Example 2
[0085] A wet tissue fabric was manufactured under the same conditions as Example 1, except that the nonionic surfactant was changed to 0.025 kg.
[0086]
[0087] Example 3
[0088] A wet tissue fabric was manufactured under the same conditions as Example 1, except that the amount of the amine-based temporary wetting strength enhancer was changed to 5 kg.
[0089]
[0090] Example 4
[0091] A wet tissue fabric was manufactured under the same conditions as Example 1, except that the amount of high-grade alcohol-based deaerator was changed to 0.05 kg.
[0092]
[0093] <Comparative Example>
[0094] Comparative Example 1
[0095] A wet tissue fabric was manufactured under the same conditions as Example 1, except that the raw material mixture consisted of 10,000 L of water, 106 kg of bleached kraft pulp having an average diameter of 10 to 20 μm and an average length of 1 to 4 mm, 6 kg of bamboo pulp having an average diameter of 5 to 15 μm and an average length of 1 to 4 mm, 0.05 kg of nonionic surfactant, 10 kg of temporary wetting strength enhancer, 1 kg of softener, and 0.1 kg of high-grade alcohol-based deaerator.
[0096]
[0097] Comparative Example 2
[0098] A wet tissue fabric was manufactured under the same conditions as Example 1, except that the bleached kraft pulp was changed to 89 kg and the bamboo pulp was changed to 22 kg.
[0099]
[0100] Comparative Example 3
[0101] A wet tissue fabric was manufactured under the same conditions as Example 1, except that the bleached kraft pulp was changed to 78 kg and the bamboo pulp was changed to 33 kg.
[0102]
[0103] Comparative Example 4
[0104] A wet tissue fabric was manufactured under the same conditions as Example 1, except that the bleached kraft pulp was changed to 67 kg and the bamboo pulp was changed to 44 kg.
[0105]
[0106] Comparative Example 5
[0107] A wet tissue fabric was manufactured under the same conditions as Example 1, except that the bleached kraft pulp and bamboo pulp were changed to 56 kg and 56 kg, respectively.
[0108]
[0109] Water (L) Bleached Kraft Pulp (kg) Bamboo Pulp (kg) Dispersant (kg) Temporary Wetting Strength Enhancer (kg) Softener (Kg) Degassing Agent (kg) Example 110,000100110.051010.1 Example 210,000100110.0251010.1 Example 310,000100110.05510.1 Example 410,000100110.051010.05 Comparative Example 110,00010660.051010.1 Comparative Example 210,00089220.051010.1 Comparative Example 310,00078330.051010.1 Comparative Example Comparative example 510,00056560.051010.1
[0110] <Experimental Example>
[0111] The physical properties of the wet tissue fabrics manufactured in Examples 1 to 4 and Comparative Examples 1 to 5 were measured, and the results are shown in Table 2 below.
[0112] The basis weight was measured by collecting more than 10 100㎠ samples according to the TAPPI T 410 standard, measuring the weight of each, calculating the average value, and then correcting it (correction value x 100) to measure the basis weight.
[0113] The thickness of the nonwoven fabric was measured using a thickness measuring device according to the TAPPI T 411 standard, the tensile strength was measured according to the KS K 0743 standard, and the wet tensile strength was measured according to the ASTM D 828 standard.
[0114] Antibacterial tests were conducted using two strains of Staphylococcus aureus and Klebsiella pneumoniae according to KSK 0693-2001.
[0115] At this time, Staphylococcus aureus is preserved with the number ATCC 6538p, and Streptococcus pneumoniae is preserved with the number ATCC 4352. The inoculation concentration for both types is 1.0 * 10 5 It was dog / ml.
[0116]
[0117] Weight (g / ㎡) Thickness (mm) Tensile strength (MD, longitudinal) (N / cm) Tensile strength (CD, transverse) (N / cm) Wet tensile strength (MD, longitudinal) (N / cm) Wet tensile strength (CD, transverse) (N / cm) Antibacterial (%) Example 1 420.16 25.4 15.8 7.8 5.4 99.9 Example 2 430.15 25.115 27.15 199.9 Example 3 410.16 25.5 15.17 35.0 99.9 Example 4 420.15 25.115 97.15 499.9 Comparative example 1430.16 23.8 13.5 5.5 3.5 99.9 Comparative example 2430.1622.412.34.83.199.9Comparative Example 3410.1520.411.14.32.599.9Comparative Example 4420.1518.510.23.52.399.9Comparative Example 5410.1516.58.92.91.899.9
[0118] As summarized in Table 2, it can be seen that the wet tissue fabric manufactured by the manufacturing method of Examples 1 to 4 of the present invention has an excellent basis weight of 41 to 43 g / ㎡, a thickness of 0.15 to 0.16 mm, a tensile strength (MD, longitudinal direction) of 25.1 to 25.5 N / cm, a tensile strength (CD, transverse direction) of 15.1 to 15.9 N / cm, a wet tensile strength (MD, longitudinal direction) of 7.1 to 7.8 N / cm, a wet tensile strength (CD, transverse direction) of 5.0 to 5.4 N / cm, and an antibacterial power of 99.9%.
[0119] On the other hand, the wet tissue fabric manufactured by the manufacturing method of Comparative Examples 1 to 5, which had a lower content of bleached kraft pulp and a higher content of bamboo pulp compared to the examples, had a tensile strength (MD, longitudinal direction) of 16.5 to 23.8 N / cm and a tensile strength (CD, transverse direction) of only 8.9 to 13.5 N / cm.
[0120] In addition, the wet tensile strength (MD, longitudinal direction) was 2.9 to 5.5 N / cm, and the wet tensile strength (CD, transverse direction) was 1.8 to 3.5 N / cm, which were not suitable for use as products.
[0121]
[0122] The present invention has been described above, focusing on preferred embodiments thereof. Those skilled in the art will appreciate that the present invention can be implemented in modified forms without departing from its essential characteristics. Therefore, the disclosed embodiments should be considered illustrative rather than limiting. The scope of the present invention is set forth in the claims, not the foregoing description, and any equivalents thereof should be construed as encompassing the present invention.
Claims
1. A fabric for wet tissues characterized by containing biodegradable bleached kraft pulp and bamboo pulp.
2. In paragraph 1, A fabric for wet tissues characterized by further comprising at least one of a dispersant, a temporary wetting strength enhancer, a deaerator, and a softener.
3. In paragraph 2, A wet tissue fabric characterized by comprising 90 to 110 parts by weight of the above bleached kraft pulp, 5 to 15 parts by weight of bamboo pulp, 0.01 to 0.10 parts by weight of a dispersant, 4 to 15 parts by weight of a temporary wetting strength enhancer, 0.01 to 0.25 parts by weight of a deaerator, and 0.5 to 3 parts by weight of a softener.
4. In paragraph 3, The above bleached kraft pulp has a diameter of 10 to 20 μm and a length of 1 to 4 mm. The above bamboo pulp has a diameter of 5 to 15 μm and a length of 1 to 4 mm. The above dispersant is a nonionic surfactant, The above temporary wetting strength enhancer is an amine type, The above degassing agent is a high-grade alcohol type, A fabric for wet tissues, characterized in that the above softener is a quaternary ammonium type.
5. In paragraph 2, A fabric for wet tissue characterized by satisfying a longitudinal tensile strength of 25 N / cm or more, a transverse tensile strength of 15 N / cm or more, a longitudinal wet tensile strength of 7 N / cm or more, and a transverse wet tensile strength of 5 N / cm or more.
6. Step 1: Preparing raw materials; The second step is to prepare a raw material mixture by mixing the prepared raw materials; The third step is to fibrillate the prepared raw material mixture; Step 4: laminating the fibrillated raw material mixture onto a mesh belt; A fifth step of dehydrating the raw material mixture laminated on the mesh belt; including: A method for manufacturing a fabric for wet tissues, characterized in that the above raw materials include biodegradable bleached kraft pulp and bamboo pulp.
7. In paragraph 6, A method for manufacturing a fabric for wet tissues, characterized in that the above raw material further includes at least one of a dispersant, a temporary wetting strength enhancer, a deaerator, and a softener.
8. In paragraph 7, A method for manufacturing a wet tissue fabric, characterized in that in the first step, water is prepared in a ratio of 9,900 to 11,000 parts by weight, bleached kraft pulp in a ratio of 90 to 110 parts by weight, bamboo pulp in a ratio of 5 to 15 parts by weight, dispersant in a ratio of 0.01 to 0.10 parts by weight, temporary wet strength enhancer in a ratio of 4 to 15 parts by weight, deaerator in a ratio of 0.01 to 0.25 parts by weight, and softener in a ratio of 0.5 to 3 parts by weight.
9. In paragraph 8, A method for manufacturing a wet tissue fabric, characterized in that in the third step, fibrillation is performed by applying a pressure in the range of 130 to 160 N.
10. In paragraph 8, The above bleached kraft pulp has a diameter of 10 to 20 μm and a length of 1 to 4 mm. The above bamboo pulp has a diameter of 5 to 15 μm and a length of 1 to 4 mm. The above dispersant is a nonionic surfactant, The above temporary wetting strength enhancer is an amine type, The above degassing agent is a high-grade alcohol type, A method for manufacturing a fabric for wet tissues, characterized in that the above-mentioned softener is a quaternary ammonium type.
Citation Information
Patent Citations
Recycling Apparatus for Remnant of Wet Tissue Fabric
KR101808097B1
Fabric for wet tissue
KR1020140033888A
Fabrics for Wet Tissue and Method of Manufacturing The Same
KR102602509B1
Flexible crepe paper and its production
JP1995197400A
Method of manufacturing a eco-friendly wipes package using 100% TENCEL fabric
KR101990743B1