Catalyst for preparing c 2+ alcohol by means of co 2 hydrogenation, preparation method therefor and use thereof

By adjusting the ratio of Fe, Cu and other metals, an efficient CO2 hydrogenation catalyst was prepared, which solved the problems of low CO2 conversion and low selectivity of C2+ alcohols in the existing catalysts, and achieved high CO2 conversion and C2+ alcohols. Selectivity reduces CH4 selectivity and is suitable for industrial applications.

WO2024239536A1PCT designated stage expired Publication Date: 2024-11-28YANKUANG ENERGY R&D CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/127459
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-22
Filing Date
2023-10-30
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The existing CO2 hydrogenation catalysts for C2+ alcohols have problems such as low CO2 conversion, low C2+ alcohols and high CH4 selectivity, making it difficult to develop efficient catalysts.

Method used

By adjusting different proportions of metal active components, catalysts including Fe, Cu and M (such as Zn, Mn, Co, etc.) are prepared to achieve efficient synergistic catalytic effects between active components and improve CO2 conversion and C2+ alcohol selection. , reduce CH4 selectivity.

Benefits of technology

The CO2 conversion rate is ≥40%, C2+ alcohol selectivity is ≥20%, and CH4 selectivity is ≤10%, and the catalyst has high mechanical strength and stability, which is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023127459_28112024_PF_FP_ABST
    Figure CN2023127459_28112024_PF_FP_ABST
Patent Text Reader

Abstract

A catalyst for preparing C2+ alcohol by means of CO2 hydrogenation. Active components of the catalyst comprise Fe, Cu and M, M comprising one or more of Zn, Mn, Co, Cs, Ce, Ga, Al and Zr, and the molar ratio of Fe, Cu and M being Fe: Cu: M = 1: (1-4): (0.5-4). Further provided is a preparation method for the catalyst, involving a simple preparation process and cheap and readily-available raw materials. By adjusting the ratio of the different active components, a highly efficient synergistic effect among the components is achieved, thereby remarkably improving the CO2 conversion rate and C2+ alcohol selectivity. In addition, further provided is the use of the catalyst. During the process of catalyzing CO2 hydrogenation to prepare C2+ alcohol, a CO2 conversion rate≥35%, C2+ alcohol selectivity≥15% and CH4 selectivity≤15% can be achieved. The provided catalyst solves the problem of low content of high value-added C2+ alcohol in previous alcohol catalyst products prepared by means of CO2 hydrogenation.
Need to check novelty before this filing date? Find Prior Art

Description

A CO2 hydrogenation process 2+ Alcohol catalyst and its preparation method and application Technical Field

[0001] The present invention relates to the field of carbon dioxide conversion technology, and further relates to a method for producing carbon dioxide by hydrogenation of CO2. 2+ Alcohol catalyst, preparation method and application thereof. Background Art

[0002] The utilization of carbon dioxide has an important impact on the development of carbon cycle and circular economy, and its catalytic conversion has attracted worldwide attention. Among the many products of carbon dioxide conversion, methanol is the main product. 2+ There is less research on alcohol. 2+ Alcohol is not only non-toxic but also a more valuable product that can be easily converted into high value-added chemicals. 2+ Alcohol, need to develop high activity and high C 2+ Alcohol-selective catalysts. Currently, at relatively high carbon dioxide conversion levels, relatively high or absolutely dominant C 2+ Alcohol-selective catalysts remain very challenging.

[0003] Therefore, a high stability and efficient catalytic carbon dioxide hydrogenation to C 2+ Catalysts for the conversion of carbon dioxide to alcohols are crucial for their practical applications. Currently, the most mature catalysts used in CO2 hydrogenation to alcohols are typically derivatives of catalysts used in CO2 hydrogenation to methanol. The distribution of catalytic reaction products shows that CO2 hydrogenation primarily converts to methanol, with a small amount of methane also present as an organic product. Furthermore, because the catalysts also promote the reverse water-gas shift reaction, some CO2 is converted to CO.

[0004] Patent CN 111659432 A invented an iron-based catalyst for CO2 hydrogenation to ethanol, its preparation method and application. The active sites of the iron-based catalyst for CO2 hydrogenation to ethanol include Fe5C2, Fe2C and Fe3C. In the process of CO2 hydrogenation to ethanol, the catalyst has an ethanol selectivity of ≥20% and a CO selectivity of ≤10%. Thongthai Witoon et al. reported a new K-Co / In2O3 catalyst for CO2 hydrogenation to C 2+ The best C 2+ The space-time yield of alcohol was 169.6 g / kg cat -1 h -1The characterization results show that the KO-Co species generated by the catalyst can significantly reduce the amount of weak H2 adsorption and strengthen the interaction of adsorbed H. The reduced adsorption of weak H2 and the improved interaction of adsorbed H with the catalyst surface delay the hydrogenation ability and promote the insertion of CO into the adsorbed C before its hydrogenation to form hydrocarbons. x H y Species, resulting in a significant reduction in CH4 and higher hydrocarbons and a significant increase in the selectivity of higher alcohols.

[0005] But it is well known that compared with methanol, ethanol, propanol and other C 2+ Alcohols are more valuable chemicals. 2+ Compared with methanol, high carbon alcohols are also more superior gasoline additives. Therefore, it is necessary to develop high carbon 2+ CO2 hydrogenation to C with alcohol selectivity and high CO2 conversion 2+ New catalysts for the synthesis of alcohols.

[0006] Summary of the Invention

[0007] Regarding the existing technology of CO2 hydrogenation to C 2+ Alcohol catalysts have low CO2 conversion rates and C 2+ The present invention aims to provide a method for preparing C by hydrogenation of CO2. 2+ The catalyst provided by the present invention achieves efficient synergistic catalytic effect between active components by adjusting different proportions of metal active components. The catalyst prepared by the present invention is effective in CO2 hydrogenation to C 2+ In the alcohol process, CO2 conversion rate ≥ 40%, C 2+ Alcohol selectivity ≥ 20%, CH4 selectivity ≤ 10%.

[0008] In order to achieve the above object, the present invention provides a CO2 hydrogenation process for producing C 2+ A catalyst for alcohol, wherein the active components of the catalyst include Fe, Cu and M, wherein M includes one or more of Zn, Mn, Co, Cs, Ce, Ga, Al and Zr; and the molar ratio of Fe, Cu and M is Fe:Cu:M=1:(1-4):(0.5-4).

[0009] The present invention also provides a CO2 hydrogenation method for producing C 2+ The preparation method of the catalyst for alcohol comprises the following steps:

[0010] S1. According to the component ratio of the catalyst, a metal salt solution containing Fe, Cu and M is measured to prepare a mixed salt solution, and a precipitant is weighed to prepare a precipitant solution;

[0011] S2, adding the mixed salt solution and the precipitant solution into a container in parallel to perform a coprecipitation reaction to obtain a reaction mixture, and aging the reaction mixture;

[0012] S3. After aging, the reaction mixture is washed, dried, and calcined to obtain the catalyst.

[0013] Preferably, the step S3 further comprises testing the conductivity of the washed filtrate, washing the reaction mixture until the conductivity of the filtrate is 200 to 3000 μs / cm, and then performing the drying and roasting.

[0014] In some embodiments, the Fe-containing metal salt is ferric nitrate; the Cu-containing metal salt is copper nitrate; the M-containing metal salt is one or a mixture of zinc nitrate, manganese nitrate, cobalt nitrate, cesium nitrate, cerium nitrate, aluminum nitrate, and zirconium nitrate.

[0015] In some embodiments, the precipitant is one or a mixture of potassium carbonate, sodium carbonate, and ammonium carbonate.

[0016] In some embodiments, the reaction temperature of the coprecipitation reaction is 60-80°C; the pH value of the reaction mixture is 6.0-8.0; the aging temperature is 60-80°C, and the time is 0.5-4h; the drying temperature is 110°C, and the time is 12h; the calcination temperature is 450°C, and the time is 4h.

[0017] The present invention also provides a CO2 hydrogenation method for producing C 2+ The catalyst is first pre-reduced and the pre-reduced catalyst is used for CO2 hydrogenation to produce C 2+ alcohol.

[0018] In some embodiments, the pre-reduction conditions are: the reducing gas is H2, the space velocity of the reducing gas is 2000 mL / g / h, the reducing pressure is 0.5 MPa, the reducing temperature is 400°C, the reducing time is 2h, and the heating rate is 2°C / min.

[0019] In some embodiments, the catalyst is used for CO2 hydrogenation to C 2+ The reaction conditions of alcohol are: reaction atmosphere is H2 and CO2, reaction pressure is 2MPa~6MPa, and reaction temperature is 280℃~400℃.

[0020] In some embodiments, the ratio of H2 to CO2 in the reaction atmosphere is H2 / CO2=2, H2 / CO2=3 or H2 / CO2=4.

[0021] Compared with the prior art, the present invention can bring the following beneficial effects:

[0022] 1. The active components of the catalyst provided by the present invention include Fe and Cu. Fe has a strong Fischer-Tropsch reaction ability, and Cu has a good CO adsorption and insertion ability. The combination of the two makes the catalyst show a high CO2 hydrogenation to C 2+ The active components of this catalyst also include active metals such as Zn and Mn, which can further improve the CO adsorption and insertion capacity and hydrogenation performance. Taking Zn and Mn as an example, Mn combines with Fe to form Fe-Mn-O phase, further improving the CO adsorption capacity and promoting the particle dispersion of active metals Fe and Cu. Zn can improve the hydrogenation performance and increase active intermediates such as CH*, CH2*, and CH3*, thereby improving the selectivity of alcohols. By adjusting the ratio of each active component, efficient synergistic effect between the active components can be achieved, significantly improving the conversion rate of CO2 and C 2+ alcohol selectivity;

[0023] 2. The catalyst provided by the present invention has high mechanical strength, the active components are more dispersed, and can operate stably for a long period of time in the reactor;

[0024] 3. The catalyst provided by the present invention also has the characteristics of uniform composition, cheap and readily available raw materials, simple preparation method and short preparation cycle, and is easy to be produced on a large scale industrially. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] FIG1 is a CO2 hydrogenation to C method provided by the present invention. 2+ Scanning electron microscopy (SEM) images of the catalyst for the synthesis of alcohol. DETAILED DESCRIPTION

[0026] The following examples are only used to illustrate the technical solution of the present invention more clearly, and are not intended to limit the scope of protection of the present invention.

[0027] Example 1

[0028] The present invention provides a method for preparing C by hydrogenation of CO2 2+ The catalyst for alcohol production comprises active components of Fe, Cu and M, wherein M comprises one or more of Zn, Mn, Co, Cs, Ce, Ga, Al and Zr.

[0029] The molar ratio of Fe, Cu and M is Fe:Cu:M=1:1-4:0.5-4.

[0030] Example 2

[0031] Based on Example 1, the present invention provides a method for preparing the catalyst, and the specific steps are as follows:

[0032] S1. According to the composition ratio of the catalyst, the metal salt solution containing Fe, Cu and M is measured to prepare a mixed salt solution, and the precipitant is weighed to prepare a precipitant solution;

[0033] S2, adding the mixed salt solution and the precipitant solution into a container in parallel to perform a coprecipitation reaction to obtain a reaction mixture, and aging the reaction mixture;

[0034] S3. After aging, the reaction mixture is washed, dried, and calcined to obtain the catalyst.

[0035] In step S1, the metal salt containing Fe is ferric nitrate; the metal containing Cu is copper nitrate; and the metal salt containing M is one or a mixture of zinc nitrate, manganese nitrate, cobalt nitrate, cesium nitrate, lanthanum nitrate, cerium nitrate, aluminum nitrate, and zirconium nitrate.

[0036] The above metal salt solutions can be prepared into 1M metal salt solutions respectively, and the amount of metal salt solution containing Fe, Cu and M can be calculated according to the molar ratio of the active components of the catalyst. Then, the above metal salt solutions can be measured and evenly mixed to form a mixed salt solution.

[0037] The above-mentioned precipitant can be selected from one or a mixture of potassium carbonate, sodium carbonate and ammonium carbonate.

[0038] In step S2, the flow rates of the mixed salt solution and the precipitant solution are controlled by a peristaltic pump, and the mixed salt solution and the precipitant solution are added into a three-necked flask with a stirrer for a co-precipitation reaction to obtain a reaction mixture. The reaction temperature is 60 to 80° C., and the pH value of the reaction mixture is maintained at 6.0 to 8.0. After the mixed salt solution and the precipitant solution are added dropwise, the mixture is stirred at 60 to 80° C. for aging, and the aging time is 0.5 to 4 hours.

[0039] In step S3, after the aging is completed, the reaction mixture is naturally cooled to 20° C. and then filtered and washed with deionized water. The conductivity of the filtrate is detected by a conductivity meter. When the conductivity of the filtrate reaches 200-3000 μs / cm, the reaction mixture is placed in an oven at 110° C. for 12 hours and then calcined in a muffle furnace at 450° C. for 4 hours to obtain the catalyst.

[0040] Example 3

[0041] In this embodiment, the catalyst provided by the present invention is used to hydrogenate CO2 to produce C 2+ Application in alcohol reaction: First, the catalyst is pre-reduced under the following conditions: H2 as reducing gas, with a space velocity of 2000 mL / g / h, a reducing pressure of 0.5 MPa, a reducing temperature of 400°C, a reducing time of 2 hours, and a heating rate of 2°C / min.

[0042] The pre-reduced catalyst is then used for CO2 hydrogenation to C 2+ The alcohol reaction process and the catalytic reaction conditions are as follows: the reaction atmosphere is H2 and CO2, the ratio of H2 and CO2 is H2 / CO2=2, H2 / CO2=3 or H2 / CO2=4, the reaction pressure is 2MPa~6MPa, and the reaction temperature is 280℃~400℃.

[0043] The catalyst catalyzes CO2 hydrogenation to C 2+ The reactor of the alcohol process is a fixed bed reactor, a fluidized bed reactor or a slurry bed reactor, and its specific structure and form are not specifically limited in this embodiment.

[0044] In order to better understand and apply the above scheme and effectively demonstrate the corresponding benefits, the following is a CO2 hydrogenation method provided by the present invention in combination with specific examples. 2+ The catalyst for alcohol and its preparation method and application are further described.

[0045] Example 4

[0046] S1. First, copper nitrate, ferric nitrate, zinc nitrate, manganese nitrate and potassium carbonate (precipitant) were dissolved in deionized water to prepare a 1M solution. 150 ml of 1M copper nitrate solution, 75 ml of 1M ferric nitrate solution, 37.5 ml of 1M zinc nitrate solution and 135 ml of 1M manganese nitrate solution were measured and evenly mixed in a 500 ml beaker to prepare a mixed salt solution. 600 ml of 1M potassium carbonate solution was measured in a 500 ml beaker.

[0047] S2. The mixed salt solution and potassium carbonate solution were added dropwise to a three-necked flask with a stirrer to perform a coprecipitation reaction to obtain a reaction mixture. The reaction temperature was maintained at 80° C. The addition rate of the potassium carbonate solution was adjusted by a peristaltic pump to control the pH value to 8.0. After the addition was completed, the mixture was kept at 80° C. and stirred for 2 h for aging.

[0048] S3. After the aging reaction is completed, the reaction mixture is cooled to 20°C naturally and then filtered and washed with deionized water. The conductivity of the filtrate is measured by a conductivity meter to be 240 μs / cm. The mixture is then dried at 110°C for 12 hours and then calcined in a muffle furnace at 450°C for 4 hours to obtain KFe1Cu2Zn 0.5 Mn 1.8 catalyst.

[0049] KFe1Cu2Zn 0.5 Mn 1.8 Catalyst activity test:

[0050] The catalyst was pre-reduced under the following conditions: reducing gas H2, reducing pressure of 0.5 MPa, space velocity of reducing gas of 2000 mL / g / h, reduction at a reducing temperature of 400°C for 2 h, and a heating rate of 2°C / min.

[0051] After reduction, the catalytic performance of the catalyst was evaluated. The catalytic conditions were: the ratio of H2 and CO2 in the reaction atmosphere was H2 / CO2 = 3.0, the space velocity was 3000 mL / g / h, the reaction temperature was 300°C, and the reaction pressure was 3.0 MPa. The catalyst was tested for activity for 50 hours. The catalytic performance results are shown in Table 1.

[0052] Example 5

[0053] Refer to Example 4, except that the amount of 1M manganese nitrate solution in Example 4 was changed to 45ml, and other preparation conditions were the same as Example 4 to obtain KFe1Cu2Zn 0.5 Mn 0.6 catalyst.

[0054] The activity test conditions were the same as those in Example 4. The catalyst was tested for 50 hours. The catalytic performance results are shown in Table 1.

[0055] Example 6

[0056] Refer to Example 4, except that 37.5 ml of 1 M cobalt nitrate solution was added when preparing the mixed salt solution. Other preparation conditions were the same as those in Example 4 to obtain KCo 0.5 Fe1Cu2Zn 0.5 Mn 1.8 catalyst.

[0057] The activity test conditions were the same as those in Example 4. The catalyst was subjected to activity testing for 50 hours. The catalytic performance results are shown in Table 1.

[0058] Example 7

[0059] Refer to Example 4, except that 37.5 ml of 1 M zirconium nitrate solution was added when preparing the mixed salt solution. Other preparation conditions were the same as those in Example 4 to obtain KZr 0.5 Fe1Cu2Zn 0.5 Mn 1.8 catalyst.

[0060] The activity test conditions were the same as those in Example 4. The catalyst was subjected to activity testing for 50 hours. The catalytic performance results are shown in Table 1.

[0061] Example 8

[0062] Refer to Example 4, except that the pH of the reaction mixture was adjusted to 7.0, and other preparation conditions were the same as in Example 4 to obtain KFe1Cu2Zn 0.5 Mn 1.8 catalyst.

[0063] The activity test conditions were the same as those in Example 4. The catalyst was subjected to activity testing for 50 hours. The catalytic performance results are shown in Table 1.

[0064] Example 9

[0065] Refer to Example 4, except that the conductivity of the water filtrate of the reaction mixture was controlled at 1300 μs / cm, and the other preparation conditions were the same as those in Example 4 to obtain KFe1Cu2Zn 0.5 Mn 1.8 catalyst.

[0066] The activity test conditions were the same as those in Example 4. The catalyst was subjected to activity testing for 50 hours. The catalytic performance results are shown in Table 1.

[0067] Comparative Example 1

[0068] Refer to Example 4, except that 1M manganese nitrate solution is not added when preparing the mixed salt solution. Other preparation conditions are the same as those in Example 4 to obtain KFe1Cu2Zn 0.5 catalyst.

[0069] The activity test conditions were the same as those in Example 4. The catalyst was subjected to activity testing for 50 hours. The catalytic performance results are shown in Table 1.

[0070] Comparative Example 2

[0071] Refer to Example 4, except that 1M zinc nitrate solution is not added when preparing the mixed salt solution. Other preparation conditions are the same as those in Example 4 to obtain KFe1Cu2Mn 1.8 catalyst.

[0072] The activity test conditions were the same as those in Example 4. The catalyst was subjected to activity testing for 50 hours. The catalytic performance results are shown in Table 1.

[0073] Table 1 Catalytic performance results of different catalysts in Examples 4 to 9 and Comparative Examples 1 to 2

[0074] As shown in Table 1, the difference between the catalyst obtained in Example 4 and Comparative Example 1 is that the active component Mn is added during the catalyst preparation process. From the catalytic performance results of the two, it can be seen that the CO2 conversion rate and C 2+ The alcohol selectivity is higher than that of comparative example 1, CO, CH4, C 2-4 The selectivity of alcohols and hydrocarbons such as alkanes and methanol is lower than that of Comparative Example 1.

[0075] The difference between the catalyst obtained in Example 4 and Comparative Example 2 is that the active component Zn is added during the catalyst preparation process. From the catalytic performance results of the two, it can be seen that the CO2 conversion rate and C 2+ The alcohol selectivity is higher than that of comparative example 2, CO, CH4, C 5+ The selectivity of alcohols and hydrocarbons such as hydrocarbons and methanol is lower than that of Comparative Example 1.

[0076] Combined with Examples 4-9, the catalysts provided in the above examples all achieved a CO2 conversion rate of ≥35%, C 2+ The catalytic effect of alcohol selectivity ≥15% and CH4 selectivity ≤15% shows good CO2 hydrogenation to C 2+ The application potential of alcohol.

[0077] Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enables any technician in the field to practice the present invention, including the manufacture and use of any device or system, and the implementation of any combined method.

[0078] It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention, and these improvements and modifications should also be considered as the scope of protection of the present invention.

Claims

1. A CO2 hydrogenation process to produce C 2+ A catalyst for alcohols, characterized in that The active components of the catalyst include Fe, Cu and M, wherein M includes one or more of Zn, Mn, Co, Cs, Ce, Ga, Al and Zr; The molar ratio of Fe, Cu and M is Fe:Cu:M=1:(1-4):(0.5-4).

2. A CO2 hydrogenation process as claimed in claim 1 2+ A method for preparing a catalyst for alcohol, characterized in that: The steps include: S1. According to the composition ratio of the catalyst, a metal salt solution containing Fe, Cu and M is weighed to prepare a mixed salt solution, and a precipitant is weighed to prepare a precipitant solution; S2, adding the mixed salt solution and the precipitant solution into a container in parallel to perform a coprecipitation reaction to obtain a reaction mixture, and aging the reaction mixture; S3. The reaction mixture after aging is washed, dried and calcined to obtain the catalyst.

3. The preparation method according to claim 2, characterized in that: The step S3 also includes conducting conductivity testing on the washed filtrate, washing the reaction mixture until the conductivity of the filtrate is 200-3000 μs / cm, and then performing the drying and roasting.

4. The preparation method according to claim 2, characterized in that: The Fe-containing metal salt is ferric nitrate; The Cu-containing metal salt is copper nitrate; The metal salt containing M is one or a mixture of zinc nitrate, manganese nitrate, cobalt nitrate, cesium nitrate, cerium nitrate, aluminum nitrate, and zirconium nitrate.

5. The preparation method according to claim 2, characterized in that: The precipitant is one or a mixture of potassium carbonate, sodium carbonate and ammonium carbonate.

6. The preparation method according to claim 2, characterized in that: The reaction temperature of the coprecipitation reaction is 60-80°C; The pH value of the reaction mixture is 6.0 to 8.0; The aging temperature is 60-80°C and the aging time is 0.5-4h; The drying temperature is 110°C and the drying time is 12h; The calcination temperature is 450° C. and the calcination time is 4 hours.

7. A CO2 hydrogenation process to produce C 2+ The use of a catalyst for alcohols, characterized in that The catalyst according to claim 1 is pre-reduced, and the pre-reduced catalyst is used to catalyze CO2 hydrogenation to produce C 2+ alcohol.

8. The use according to claim 7, characterized in that: The pre-reduction conditions are: the reducing gas is H2, the space velocity of the reducing gas is 2000mL / g / h, the reducing pressure is 0.5MPa, the reducing temperature is 400°C, the reducing time is 2h, and the heating rate is 2°C / min.

9. The use according to claim 7, characterized in that: The catalyst is used for CO2 hydrogenation to produce C 2+ The reaction conditions of alcohol are: reaction atmosphere is H2 and CO2, reaction pressure is 2MPa~6MPa, reaction temperature is 280℃~400℃.

10. The use according to claim 9, characterized in that: The ratio of H2 to CO2 in the reaction atmosphere is H2 / CO2=2, H2 / CO2=3 or H2 / CO2=4.

Citation Information

Patent Citations

  • Catalyst for synthesizing methanol through carbon dioxide hydrogenation as well as preparation method and application thereof

    CN103263926A

  • Catalyst for directly synthesizing ethanol from syngas and preparation method and application thereof

    CN110280261A

  • Catalyst for preparing low-carbon alcohol by CO2 hydrogenation, and preparation method and application thereof

    CN111659402A

  • Catalyst for synthesizing methanol through carbon dioxide hydrogenation, preparation method and application

    CN112755996A

  • Catalyst for CO hydrogenation synthesis of mixed alcohol, and preparation method thereof