Catalyst and process
The process of forming an aqueous mixture of metal iridium oxide with an acid produces chloride-free iridium oxide catalysts with high catalytic activity, addressing the challenges of chloride contamination and scalability in existing iridium oxide production for oxygen evolution reactions, enhancing efficiency and reducing iridium usage in water electrolysis and fuel cells.
Patent Information
- Application Number
- PCT/GB2024/051332
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2024-05-23
- Publication Date
- 2024-11-28
AI Technical Summary
Current methods for producing iridium oxide catalysts for oxygen evolution reactions often result in chloride-containing materials that are hygroscopic, corrosive, and difficult to scale up, with high iridium demand and limited efficiency, especially in water electrolysis and fuel cells.
A process involving the formation of an aqueous mixture of metal iridium oxide with an acid, such as barium iridium oxide and nitric acid, under mild conditions to produce iridium oxide materials substantially free of chloride, with high catalytic activity for oxygen evolution reactions.
The process yields iridium oxide materials with high surface area and catalytic activity, suitable for water electrolysis and fuel cells, reducing chloride content and operational challenges, and enabling efficient large-scale production with lower iridium loadings.
Smart Images

Figure GB2024051332_28112024_PF_FP_ABST
Abstract
Description
[0001] CATALYST AND PROCESS
[0002] Field of the Invention
[0003] The present invention relates to iridium oxide materials which are suitable for use as oxygen evolution reaction (OER) catalysts, for example in a water electrolyser, and to improved processes for their manufacture.
[0004] Background of the Invention
[0005] The electrolysis of water to produce hydrogen and oxygen can be carried out in both alkaline and acidic electrolyte systems and practical devices using both types of electrolyte systems exist as commercial products. Those electrolysers that employ a solid proton-conducting polymer membrane, or proton exchange membrane (PEM), are known as proton exchange membrane water electrolysers (PEMWEs). Those electrolysers that utilise a solid anion- conducting polymer membrane, or anion exchange membrane (AEM), are known as anion exchange membrane water electrolysers (AEMWEs).
[0006] Ion-conducting membranes, such as PEMs and AEMs, are also used in fuel cells. In a proton exchange membrane fuel cell (PEMFC), the membrane is proton conducting and protons, produced at the anode are transported across the membrane to the cathode, where they combine with oxygen to form water.
[0007] Catalyst-coated membranes (CCMs) may be employed within electrochemical devices, such as electrolysers and fuel cells. Such CCMs comprise an ion-conducting membrane, such as a PEM or an AEM, and an anode catalyst layer and / or a cathode catalyst layer applied to a face of the membrane, the anode catalyst layer and cathode catalyst layer being applied to opposite faces of the membrane.
[0008] During PEM water electrolyser operation the oxygen evolution reaction (OER) takes place at the anode and the hydrogen evolution reaction (HER) takes place at the cathode, approximated by the following equations:
[0009] H2O O2+ 4H++ 4e- (OER)
[0010] 4H++ 4e- 2H2(HER)
[0011] The cathode catalyst used in both PEM water electrolysers and PEM fuel cells is generally a platinum catalyst, usually platinum on carbon. Iridium and iridium oxide (IrOx) materials are well known for their properties as excellent OER catalysts and are preferred materials for the oxygen evolution reaction on the anode side of an electrolyser.
[0012] Iridium oxide (lrOx) materials are typically produced from chloride-containing precursors, such as iridium chloride or hydrogen hexachloroiridate (H2I rCh), through reaction with a base such as an alkali metal hydroxide. Such methods provide iridium oxide (IrOx) materials which inevitably contains some chloride ions. The presence of chloride is detrimental as it increases the hygroscopicity of the iridium oxide (IrOx) material, can facilitate migration of iridium and other components through catalyst coated membrane structures, is corrosive towards metal parts and can be oxidised to chlorine gas during electrochemical operation.
[0013] It is also known to produce iridium oxide (I rOx) materials using an Adam’s fusion method. In such reactions, an iridium precursor, such as F^IrCle is heated under oxidising conditions, for example in the presence of NaNCh. Producing IrOx using an Adam’s fusion method on a large scale can be challenging due to management of reagent decomposition.
[0014] Due to the rising global demand for hydrogen and the scarcity of iridium, there is a need to develop catalysts with improved performance and / or equivalent performance using lower loadings of metal. There is also a need to develop more efficient processes for the production of iridium oxide (IrOx) materials, in particular routes which avoid the presence of chloride-containing reagents, and which can be safely operated on a large scale.
[0015] Summary of the Invention
[0016] The present inventors have surprisingly found that iridium oxide (IrOx) materials may be efficiently produced from metal iridium oxide materials containing certain Group 2 elements. This method allows for the formation of iridium oxide materials under relatively mild conditions, which are substantially free of chloride, and which show high OER catalytic activity.
[0017] Therefore, in a first aspect of the invention there is provided a process for manufacturing iridium oxide (IrOx), the process comprising the steps of:
[0018] (i) forming an aqueous mixture comprising a metal iridium oxide and an acid, the metal being selected from Ba, Ca, Mg, and Sr;
[0019] (ii) isolating iridium oxide from the mixture;
[0020] (iii) optionally heat treating the isolated iridium oxide.
[0021] It may be particularly preferred that the metal iridium oxide is barium iridium oxide.
[0022] It has also been found that certain barium-containing iridium oxide (IrOx) materials, which may be formed by the process as described herein, have a high catalytic activity for the oxygen evolution reaction.
[0023] Therefore, in a second aspect of the invention there is provided an iridium oxide (IrOx) material obtained or obtainable by a process according to the first aspect. In a third aspect of the invention, there is provided an iridium oxide (IrOx) material with a total content of Ba in the range of and including 0.01 to 5 wt% based on the total weight of the material, preferably with a total content of Ba in the range of and including 0.01 to 1.0 wt% based on the total weight of the material. Preferably the iridium oxide (IrOx) material has a BET surface area greater than 20 m2 / g. Preferably, the iridium oxide (IrOx) material is substantially free of chloride.
[0024] Such materials have particular utility in water electrolysis and fuel cell applications, for example as part of a COM for a water electrolyser or for a fuel cell.
[0025] Therefore, in a fourth aspect of the invention there is provided a catalyst-coated membrane comprising an iridium oxide (IrOx) material according to the second or to the third aspect.
[0026] In a fifth aspect of the invention there is provided a fuel cell or a water electrolyser, such as a PEM fuel cell or a PEM water electrolyser, comprising a COM according to the fourth aspect.
[0027] Brief description of the Figures
[0028] Figure 1 shows the results of XRD analysis of the material formed in Example 1.
[0029] Figure 2 shows the results of XRD analysis of the material formed in Example 2.
[0030] Figure 3 shows the results of electrochemical activity testing.
[0031] Figure 4 shows the results of further electrochemical activity testing.
[0032] Detailed Description
[0033] Preferred and / or optional features of the invention will now be set out. Any aspect of the invention may be combined with any other aspect of the invention unless the context demands otherwise. Any of the preferred and / or optional features of any aspect may be combined, either singly or in combination, with any aspect of the invention unless the context demands otherwise.
[0034] A process for manufacturing iridium oxide (IrOx) materials is provided. The term “iridium oxide (IrOx) material” as used herein refers to a material which may be entirely I rO2, or may be a mixture of oxidic iridium species, such as I rO2, I^Os and iridium. Iridium oxyhydroxides are iridium compounds having both oxo (lr=O) and hydroxo (Ir-OH) functionalities and may have a composition which can be represented, for example, by the following formula: lrOx(OH)ywherein 1 < x < 2 and 0 < y < 2, and 3 < 2x+y < 4, and may be included in the mixture of oxidic iridium species present in the iridium oxide (IrOx) material.
[0035] It may be preferred that the iridium oxide material is substantially in the form of lrO2,for example at least 95 wt% of the iridium is in the form of I rO2, such as at least 97 wt% of the iridium is in the form of I rO2, or at least 98 wt% of the iridium is in the form of lrO2. Preferably, the iridium oxide (IrOx) materials are substantially free of chloride. By substantially free it is meant herein that the catalyst materials have a chloride content less than 20 ppm, such as less than 15 ppm, or less than 10 ppm. The chloride content may be determined using ion chromatography.
[0036] The process comprises the step of forming an aqueous mixture comprising a metal iridium oxide and an acid. The metal iridium oxide is selected from barium iridium oxide, calcium iridium oxide, magnesium iridium oxide and strontium iridium oxide. Preferably, the metal iridium oxide is selected from barium iridium oxide, calcium iridium oxide, and strontium iridium oxide. Barium iridium oxide is particularly preferred. It has been found that certain barium salts have a particularly suitable solubility profile enabling facile extraction of barium from the barium iridium oxide material.
[0037] Metal iridium oxides may be advantageously prepared though the treatment of iridium in a powder form (iridium sponge) with excess metal peroxide. Therefore, it may be preferred that the process comprises an initial step of treating iridium sponge with a metal peroxide to form the metal iridium oxide. Typically, the treatment is at an elevated temperature, for example at a temperature in the range of about 700 °C to about 900 °C. Without being bound by theory, the use of high temperature during the formation of the mixed oxide may help to provide iridium oxide materials via the process described herein with high stability. For example, barium iridium oxide (BalrOx) may be produced by sintering a mixture of excess barium peroxide and iridium sponge at a temperature of sintering in excess of 700°C and below 900 °C, preferably from about 750 °C to about 815 °C for a period between one and five hours as described in GB2413323A (Johnson Matthey Public Limited Company).
[0038] Typically, the aqueous mixture of metal iridium oxide and an acid is formed by (a) forming a mixture of metal iridium oxide and water; and (b) adding the acid to the aqueous mixture. Other methods of formation of the aqueous mixture are also contemplated, for example the addition of the metal iridium oxide to an aqueous acid solution.
[0039] It may be preferred that the acid is an inorganic acid. In order to avoid chloride contamination in the product it is preferred that pH adjustment is carried out using an acid that does not contain chloride ions, for example it is preferred that acid is not HCI. It may be further preferred that the acid is selected from one or more of nitric acid, acetic acid, and phosphoric acid. Such acids have a particularly suitable balance of properties including high solubility of the barium salt of the acid at ambient or slightly elevated temperatures. Nitric acid may be particularly preferred as processes to treat effluents containing nitric acid are well established. The acid is typically provided as an aqueous solution. The Group 2 metal may suitably be recovered from the effluent, using known chemical precipitation techniques or using, for example, ion-exchange resins.
[0040] It is preferred that the aqueous mixture formed in step (i) has a pH less than 3. It may be preferred that the pH of the aqueous mixture is less than 2.5, or less than 2.0. Whilst precipitation can still be achieved when the pH is above 3, it has been found that providing an aqueous mixture with a pH value less than around 3 can lead to significantly lower noniridium metal content in the isolated iridium oxide material. It may be particularly preferred that the pH of the aqueous mixture is around 1.5.
[0041] Suitably, step (i) comprises adjusting the pH of the aqueous mixture with the acid to a value less than 3. It may be preferred that step (i) comprises adjusting the pH of the aqueous mixture with the acid to a value less than 2.5, less than 2.0, less than 1.5, or around 1.5 (such as a pH of 1.5 ± 0.2).
[0042] Typically, step (i) comprises: (a) forming a mixture of metal iridium oxide and water; and (b) adding the acid to the mixture until the pH of the mixture is less than 3. It may be preferred that step (i) comprises (b) adding the acid to the mixture until the pH of the mixture is less than 2.5, less than 2.0, or until the pH of the mixture is around 1.5 (such as a pH of 1.5 ± 0.2).
[0043] After formation, the aqueous mixture is typically mixed prior to isolation step (ii), for example by stirring or agitation. Suitably, mixture is mixed for a period in the range of and including 0.5 hours to 8 hours, preferably in the range of and including 2 to 6 hours.
[0044] Preferably, after formation of the aqueous mixture, the aqueous mixture is heated to an elevated temperature prior to isolation step (ii), such as heated to a temperature in the range of and including 40 and 95 °C, preferably in the range of and including 60 to 90 °C, or 70 to 90 °C, such as around 80 °C. The aqueous mixture is typically mixed whilst it is heated, for example by stirring or agitation.
[0045] It may be preferred that after formation of the aqueous mixture, the aqueous mixture is heated to an elevated temperature prior to isolation step (ii), such as a temperature in the range of and including 40 and 95 °C, such as in the range of and including 60 to 90 °C, for a period of 0.5 to 8 hours, preferably for a period of 2 to 6 hours.
[0046] It is preferred that the pH of the aqueous mixture is maintained at a value less than 3, less than 2.5, less than 2.0, or around 1.5 (such as a pH of 1.5 ± 0.2) during the mixing and I or heating process. This may require the further addition of acid.
[0047] It may be preferred that step (i) of the process comprises the steps of (a) forming a mixture of the metal iridium oxide and water; (b) adding an acid to the mixture until the pH is less than 3, such as less than 2.5, less than 2.0 or around 1.5 (such as a pH of 1.5 ± 0.2); and (c) mixing the aqueous mixture, for example for a period in the range of and including 0.5 hours to 8 hours, preferably in the range of and including 2 to 6 hours. It may be preferred that step (c) is carried out at an elevated temperature, such as a temperature in the range of and including 40 and 95 °C, such as in the range of and including 60 to 90 °C. It may be further preferred that during step (c) the pH of the aqueous mixture is maintained at a value less than 3, less than 2.5, less than 2.0, or around 1.5 during the mixing and I or heating process.
[0048] The process comprises step (ii) isolating iridium oxide (IrOx) from the mixture. The IrOx material may be isolated by techniques known to the skilled person, such as by filtration and I or by evaporation of volatile components. The isolated IrOx material may be washed after isolation, for example using deionised water. Typically the isolated IrOx material is dried, for example by heating to a temperature above 100 °C, for example in a drying furnace.
[0049] The isolated IrOx material may be utilised directly as a catalyst for oxygen evolution or may be heat treated. Heat treatment may be used to increase the crystallinity of the material.
[0050] The optional heat treatment step (iii) may be carried out at a temperature of at least 300 °C, at least 400 °C, or at least 450 °C. The heat treatment step may be carried out at a temperature of 800 °C or less, 700 °C or less, or 600 °C or less. It may be preferred that the heat treatment step comprises heating to a temperature in the range of and including 300 to 800 °C. It may be further preferred that the heat treatment step comprises heating to a temperature in the range of and including 400 to 600 °C.
[0051] The material to be heated may be at a temperature of 300 °C, at least 400 °C, or at least 450 °C for a period of at least 30 minutes, at least 1 hour, or at least 2 hours. The period may be less than 6 hours, or less than 4 hours. Preferably, the heat treatment step comprises heating to a temperature in the range of and including 300 to 800 °C for a period of from 30 mins to 6 hours.
[0052] Iridium oxide (IrOx) materials are provided herein with a Ba content in the range of and including 0.01 to 5 wt% based on the total weight of the material. The amount of Ba may be determined by Inductively Coupled Plasma - Mass spectroscopy (ICP-MS). It may be preferred that the Ba content is in the range of and including 0.01 to 4 wt%, 0.01 to 3 wt%, 0.01 to 2.5 wt%, 0.01 to 2.0 wt%, or preferably 0.01 to 1.0 wt%. It may be preferred that the Ba content is in the range of and including 0.02 to 1.8 wt%, 0.03 to 1.6 wt%, 0.04 to 1.4 wt%, 0.05 to 1.2 wt%, 0.05 to 1.0 wt%, 0.1 to 0.9 wt%, 0.2 to 0.9 wt%, or 0.2 to 0.8 wt%.
[0053] The process as described herein advantageously provides materials with a high surface area. It is preferred that the BET surface area is at least 20 m2 / g. A surface area of at least 20 m2 / g is considered beneficial, enabling a high catalytic activity for a certain mass of catalytic material. The BET surface area may be calculated from the nitrogen adsorption isotherm. An instrument such as a Micrometrics TriStar 3000 may be used.
[0054] It may be preferred that the BET surface area is at least 25 m2 / g, at least 30 m2 / g, at least 35 m2 / g or at least 40 m2 / g. The BET surface area may be less than 100 m2 / g. It may be preferred that the BET surface area is in the range of and including 25 m2 / g and 100 m2 / g, such as between 30 m2 / g and 90 m2 / g.
[0055] It may be preferred that the materials are substantially amorphous. By substantially amorphous it is meant herein that no crystalline peaks associated with I rC>2 are observable in the x-ray diffraction (XRD) pattern of the material. It is considered that amorphous materials may offer higher catalytic activity. It may be preferred that the materials are substantially amorphous by XRD and have a BET surface in the range of and including 30 m2 / g and 90 m2 / g.
[0056] Alternatively, it may be preferred that the materials are crystalline. It is considered that crystalline materials may offer greater stability. It may be further preferred that the material has a rutile structure. This may be determined by XRD analysis.
[0057] Preferably, the iridium oxide (IrOx) materials are substantially free of chloride. By substantially free it is meant herein that the catalyst materials have a chloride content less than 20 ppm, such as less than 15 ppm, or less than 10 ppm. The chloride content may be determined using ion chromatography.
[0058] The iridium oxide material may be used as an oxygen evolution reaction catalyst in a water electrolyser, especially in the anode of a water electrolyser, such as a PEMWE.
[0059] The iridium oxide material may also be used in a fuel cell, such as a PEMFC, especially in a fuel cell anode for the purposes of cell reversal tolerance.
[0060] The iridium oxide material may be formulated as an ink, typically by dissolving or dispersing the iridium oxide in a mixture of an ion-conducting polymer and water, or a mixture of an ionconducting polymer, water and an organic solvent, such as ethanol or propan-1 -ol. Suitable ion-conducting polymers are known to those skilled in the art and include fluorinated ionconducting polymers, such as perfluorinated sulfonic-acid (PFSA) ionomers, partially- fluorinated sulfonated or phosphonated polymers, non-fluorinated hydrocarbon sulfonated or phosphonated polymers, or mixtures thereof.
[0061] The inks may be used to form a catalyst layer. Such layers suitably comprise the catalyst material and an ion-conducting polymer (suitable ion-conducting polymers including those set out hereinbefore in relation to inks). The catalyst layers may also comprise additional components, such as additional catalysts, radical scavengers, etc., as will be known to those skilled in the art.
[0062] The catalyst layer may form a component of a catalyst coated membrane (CCM) which comprises a membrane with the catalyst layer on a first face thereof and, optionally, a second catalyst layer on a second face thereof. Suitably, the membrane is a proton exchange membrane (PEM) or an anion exchange membrane (AEM). The membrane in the CCM may include additional components (e.g. recombination catalysts, radical scavengers, reinforcements, multiple layers) as will be known to those skilled in the art.
[0063] Typically, the CCM is for use in a water electrolyser, such as a PEM water electrolyser. In such cases the CCM typically comprises: (i) an ion-conducting membrane with a first face and a second face; (ii) an anode layer on the first face of the membrane, the anode layer comprising the iridium oxide material as described herein and an ion-conducting polymer; and (iii) a cathode catalyst layer on the second face of the membrane, the cathode catalyst layer comprising a hydrogen evolution reaction (HER) catalyst, such as a HER catalyst comprising platinum (for example platinum on carbon).
[0064] The CCM may also be suitable for use in a fuel cell, such as a PEM fuel cell. In such cases the CCM typically comprises: (i) an ion-conducting membrane with a first face and a second face; (ii) an anode layer on the first face of the membrane the anode layer comprising the iridium oxide material as described herein, a hydrogen oxidation reaction (HOR) catalyst, such as a hydrogen oxidation reaction (HOR) catalyst comprising platinum (for example platinum on carbon), and an ion-conducting polymer; and (iii) a cathode catalyst layer on the second face of the membrane, the cathode catalyst layer comprising an oxygen reduction reaction (ORR) catalyst, such as an ORR catalyst comprising platinum (for example platinum on carbon).
[0065] The present invention will now be described with reference to the following examples, which are provided to assist with understanding the present invention and are not intended to limit its scope.
[0066] Examples
[0067] Example 1 - Formation of an iridium oxide catalyst using nitric acid
[0068] BalrOx (10g) was mixed with deionised water (50mL) and stirred at ambient temperature for fifteen minutes. Nitric acid was added dropwise until the pH was around 1.5 (approximately 6.5 mL of nitric acid). The mixture was heated to 80 °C and stirred for 4 hours whilst maintaining the pH at around 1.5 through the further addition of nitric acid as required. The mixture was then filtered on a membrane filter and the iridium oxide was washed with deionised water until the conductivity of the filtrate was less than 10 microsiemens per cm. The iridium oxide material was dried in a furnace at 105 °C for 1 hour.
[0069] The BET surface area of the dried iridium oxide catalyst was measured as 66 m2 / g using the nitrogen adsorption isotherm measured using a TriStar 3000 instrument.
[0070] The barium content of the dried iridium oxide catalyst was measured as 0.79 wt% by ICP-MS.
[0071] XRD analysis of the dried iridium oxide catalyst indicates a substantially amorphous material (shown in Figure 1).
[0072] Example 2 - Heat treatment of a precipitated iridium oxide catalyst
[0073] The iridium oxide material formed in Example 1 was heat-treated using a static furnace in air by heating at a 5 °C / min rate to 500 °C and then holding at a temperature of 500 °C for a period of 1 hour before cooling.
[0074] The BET surface area of the dried iridium oxide catalyst was measured as 30 m2 / g.
[0075] XRD analysis (Figure 2) of the heat-treated iridium oxide catalyst indicates rutile iridium oxide as the major phase (>99%) with additional peaks indicating the presence of iridium and BalrCh.
[0076] Example 3 - Variation in the pH of the aqueous mixture.
[0077] Example 1 was repeated with a variation in the pH of the aqueous mixture. The formed iridium oxide materials were isolated and analysed for barium content. The results are shown in T able 1 . The results indicate that adjusting to a pH of the aqueous mixture to less than 3 provides a material with a barium content < 5 wt%, and a pH less than 2 provides < 1 wt% Ba.
[0078] Table 1 - The results of varying the pH of the aqueous mixture.
[0079] Example 4 - Formation of an iridium oxide catalyst using acetic acid
[0080] BalrOx (10g) was mixed with deionised water (100mL) and stirred at ambient temperature for thirty minutes. Acetic acid (10mL) was added, and the mixture stirred at room temperature for 1 hour. The mixture was dried on a rotary evaporator and then subsequently heat treated. The heat treatment was carried out either by (i) heating to 500 °C for one hour; or (ii) heating to 400 °C for one hour. The material heated at 400 °C was subsequently washed with a mixture of deionised water: acetic acid (ratio 10:1) and then dried in a furnace at 105 °C for at least an hour.
[0081] The BET surface area of the iridium oxide catalyst formed by heat treatment at 400 °C was measured as 70 m2 / g.
[0082] XRD analysis of the formed material showed an amorphous structure.
[0083] Assessment of PER catalytic activity
[0084] The iridium oxide catalyst formed in Example 1 (two batches) and reference samples of commercially available iridium oxides ((i) high activity sample: “benchmark IrOx”; (ii) a crystalline lrO2 example analogous to prior art materials: “Crystalline Benchmark”) were tested for PER catalytic activity using a potentiostat measuring an electrode with a 0.2 mg / cm-2catalyst loading (prepared using a catalyst ink made with an acidic Nation binder, spray coated onto carbon) as part of a glass three electrode electrochemical cell. The electrochemical activity was measured using an initial activity test (cyclic voltammetry (CV): 300, 300, 100, 50 and 10 mV s’1; linear sweep voltammetry (LSV): 1-1.55 V; electrochemical impedance spectroscopy (EIS): 1.45 V), a degradation cycling test (0.6-1.35V x 1000 cycles (4h 10 min), and a final activity test (CV: 300, 100, 50 and 10 mV s’1; LSV: 1-1.55 V; EIS: 1.45 V).
[0085] The results of testing vs the high activity “benchmark IrPx” sample are shown in Figure 3 which indicate that high PER activity has been achieved (at least equivalent to the high activity benchmark) using the process as set out herein and avoiding the use of chlorides in the synthesis route.
[0086] The results of testing vs the Crystalline Benchmark are shown in Figure 4, which indicate a significantly higher PER activity of the material of Example 1 than is provided by the comparative material.
Claims
Claims1. A process for manufacturing iridium oxide (IrOx), the process comprising the steps of:(i) forming an aqueous mixture comprising a metal iridium oxide and an acid, the metal being selected from Ba, Ca, Mg, and Sr;(ii) isolating iridium oxide from the mixture;(iii) optionally heat treating the isolated iridium oxide.
2. A process according to claim 1 , wherein the acid is selected from one or more of nitric acid, acetic acid, or phosphoric acid.
3. A process according to claim 1 or claim 2, wherein the aqueous mixture formed in step (i) has a pH less than 3.
4. A process according to any one of the preceding claims, wherein step (i) comprises adjusting the pH of the aqueous mixture with the acid to obtain a pH of less than 3.
5. A process according to any one of the preceding claims, wherein step (i) comprises (a) forming a mixture of the metal iridium oxide and water; and (b) adding the acid to the mixture until the pH of the mixture is less than 3.
6. A process according to any one of the preceding claims, wherein the aqueous mixture is heated to a temperature in the range of and including 40 and 95 °C, preferably in the range of and including 60 to 90 °C, prior to isolation of iridium oxide in step (ii).
7. A process according to claim 6, wherein the aqueous mixture is heated for a period in range of and including 0.5 to 8 hours, preferably for a period in the range of and including 2 to 6 hours.
8. A process according to any one of the preceding claims wherein the iridium oxide is isolated by filtration.
9. A process according to any one of the preceding claims, wherein the heat treatment comprises heating to a temperature greater than 300 °C, such as in the range of and including 300 to 800 °C.
10. A process according to any one of the preceding claims, wherein the metal iridium oxide is barium iridium oxide.
11. A process according to any one of the preceding claims, wherein the metal iridium oxide is formed by metal peroxide treatment of iridium sponge.
12. An iridium oxide (IrOx) material obtained or obtainable by a process according to any one of claims 1 to 11.
13. An iridium oxide (IrOx) material according to claim 12, with a total content of Ba in the range of and including 0.01 to 5 wt% based on the total weight of the material.
14. An iridium oxide material according to claim 13 with a BET surface area greater than 20 m2 / g.
15. An iridium oxide material according to claim 13 or 14, wherein the material is substantially amorphous.
16. An iridium oxide material according to any one of claims 13 to 15, with a total content of Ba in the range of and including 0.01 to 1.0 wt% based on the total weight of the material.
17. An iridium oxide material according to any one of claims 13 to 16 which is substantially free of chloride.
18. A catalyst-coated membrane comprising an iridium oxide material according to any one of claims 12 to 17.
19. A fuel cell or a water electrolyser comprising a catalyst-coated membrane according to claim 18.
Citation Information
Patent Citations
Superfine IrOx nano-cluster composite material as well as preparation method and application thereof
CN114369845A
Process for preparing nano iridium dioxide through strong dispersion
CN115465904A
Improvements to processes for the preparation of iridium acetate
GB2413323A
Iridium-containing oxide, method for producing same and catalyst containing iridium-containing oxide
WO2022138309A1
Catalyst and method for producing same
WO2023048101A1