An extraction process of metals from jarosite
The process of roasting jarosite at 600-900°C and subsequent froth flotation with optimized reagents effectively recovers zinc, lead, and silver from jarosite residues, addressing inefficiencies in existing methods by achieving high recovery rates and reducing environmental impact.
Patent Information
- Application Number
- PCT/IN2024/050488
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-22
- Filing Date
- 2024-05-06
- Publication Date
- 2024-11-28
AI Technical Summary
Current methods for extracting zinc, lead, and silver from jarosite residues are inefficient, particularly in reducing chemical solvent use, CO2 emissions, and achieving high-grade recoveries, with existing processes often requiring high temperatures and generating significant slag losses.
A process involving roasting jarosite at 600-900°C followed by froth flotation with optimized reagents and conditions to obtain high-grade concentrates of zinc, lead, and silver, while minimizing solvent use and emissions.
Achieves high recovery rates of 40-100% for lead, zinc, and silver concentrates with reduced chemical solvent consumption and lower carbon footprint, providing a sustainable and cost-effective alternative to conventional methods.
Smart Images

Figure IN2024050488_28112024_PF_FP_ABST
Abstract
Description
AN EXTRACTION PROCESS OF METALS FROM JAROSITEFIELD OF THE INVENTION:
[0001] The present disclosure relates to a field of metallurgy. Particularly, the present disclosure relates to a process of extracting metals from jarosite which is a residue generated during above extraction from ores. Specifically, the present disclosure relates to the process of extracting zinc, lead, and silver through the combined process of roasting and froth flotation. The present disclosure also relates to the concentrates of zinc, silver, and lead thereofBACKGROUND OF THE INVENTION:
[0002] The process of zinc extraction from different ores that are rich in sulphides, oxides, and silicates involve various techniques such as concentration of ore through flotation, concentrate roasting to convert sulphides into oxides, leaching of the roasted products and electro- winning process. It has been observed that a lot of impurities present in the ores are removed at various stages of the aforementioned processes for extraction of zinc from ores.
[0003] One of the detrimental impurities, is iron that is removed during the step of leaching. This impure iron is obtained in the form of Jarosite, when the residue obtained upon carrying out of leaching process using a weak acid is further extracted with an acid and subsequently treated with sodium sulphate. Jarosite being a stable compound contains a lot of valuable metals such as Zinc, Lead and Silver and thus the recovery of these metals from jarosite is of paramount importance in the metallurgical industry.
[0004] Various researchers have worked on the decomposition of jarosite. In CN114774676A, a method for enriching metals and a material for refining metals is disclosed. The said method includes the steps of providing an additive and a reducing agent, mixing the raw material, the reducing agent and the additive, and pelletizing; preheating the pellets at 300-750 °C for 20-300 minutes; then roasting for 20-200 minutes at 600-850 °C; the calcined product is cooled in a liquid, in a reducing gas or an inert gas or under burial of a solid, grinding the cooled roasted balls; and after grinding, entering a flotation process, and performing flotation to obtain concentrate enriched in target metal.
[0005] In US 2144932A, a method of treating silver-rich argento-jarosite ore containing more than 5 wt% Ag is disclosed. It comprises subjecting the argento-jarosite to a lowtemperature roasting under non-reducing conditions not over 525 X3. and recovering the silver by flotation and solution methods. However, the low temperature process is not effective for concentrating by flotation from roasting of sodium jarosite (contain only small amount of Ag < 0.5%), which is generated in zinc production. Thus, the long standing problem for metal recovery from residue of zinc production process by simple extension to zinc residue is not effective.
[0006] In CN110983061, a method for the cooperative recycling treatment of lead-zinc smelting slag and iron-vitriol slag is disclosed. According to the method, lead-zinc smelting slag, ferrous sulfate slag and a carbonaceous reducing agent are evenly mixed and pressed into balls, the balls are roasted, roasting melt is subjected to slow cooling and crystallizing, and roasting products including metal iron and lead-zinc sulfide are obtained; and the roasting products are subjected to flotation to recover lead-zinc sulfide concentrates, and flotation tailings are subjected to magnetic separation to recover iron ore concentrates.
[0007] Further, Wang et al (F. Wang et. al, Chemical Engineering Journal Advances, 2020, https: / / doi.org / ! 0.1016 / j.ceja.2020.100023) disclosed mixing of jarosite with coal, lime and water and heating it in nitrogen atmosphere to volatilize Zn. R. Serbia et al (D. Radovanovic et. al, Physicochem. Probl. Miner. Process., 2018, DOI: 10.5277 / ppmpl 842) discloses a similar mixture but heated in Waelz furnace at 1200X3 to volatilize Zn. K.K. Sahu (IJSTRE, 2016, 1(4), 36-46 ) discloses mixing of sulfuric acid with jarosite and roasted in muffle furnace and then leaching in water or brine for Pb and Zn recovery. Han et al (Journal of Hazardous Materials, 2014, https: / / doi.Org / 10.1016 / j.jhazmat.2014.05.091 discloses heating jarosite with coal in muffle and performed flotation to get a Pb recovery of 44% and Ag recovery of 82%. Shao-Hua Ju (Trans. Nonferrous Met. Soc. China 23(2013), DOI: 10.1016 / S1003 -6326(13)62581 -9) discloses direct roasting of jarosite alone and reported decomposition at 300-850 °C for 1 hr and examined leachability of the products in NH4CI. Steinlechter ( doi:l 0.3390 / met8050335, https: / / doi.org / ! 0.1016 / j.clet.202L 100214) discloses carrying out of simulation to predict thermal decomposition of jarosite during roasting.
[0008] Zhang et. al and W. Linsong et. al (TMS and ASM International 2019, https: / / doi.org / 10.1007 / sl l663-019-01517 & Hydrometallurgy, 2020, https: / / doi.Org / 10.1016 / j.hydromet.2020.105493) discloses that heating jarosite with carbonat different temperatures has yielded in different recoveries of zinc and lead. Such direct reduction (with carbon / coke / coal / CO) roasting or smelting processes requires high temperature, consume a large amount of fuel and reducing agent such as coal or coke, and in case of process-waste feeds with low feed-grades, these are often able to achieve limited metal recovery due significant losses with slag generated during these recovery processes. Alternative processes involve leaching of the small amounts of metals directly from the low-grade wastes or their roasted products, thus requiring large amounts of harmful solvents. Our process aims as concentrating the roasted product by flotation prior to leaching etc., thus dramatically reducing the use of solvents.
[0009] Although researchers have worked on the recovery of zinc and lead from jarosite, but there not much focus has been placed on the recovery of silver from the jarosite generated as waste in zinc production processes. Therefore, there is a need to develop a process for the recovery of zinc, silver and lead from jarosite.OBJECT(S) OF THE INVENTION:
[0010] The principal objective of the present invention is to provide a process for extraction of zinc, silver and lead from jarosite, an important residue obtained after processing of metallic ores for Zn production.
[0011] Yet another objective of the present invention is to provide for a process for extraction of silver, zinc, and lead from jarosite with reduced chemical solvents, reduced CO or CO2 emissions and less carbon footprint.
[0012] Yet another objective of the present invention is to provide for a process for extraction of silver from jarosite, which has a higher grade and recovery.
[0013] Yet another objective of the present invention is to provide for a process for extraction of zinc, silver and lead from jarosite is environment friendly and sustainable.
[0014] These and other objects and advantages of the present subject matter would be apparent to a person skilled in the art after consideration of the following detailed description taken into consideration with accompanying drawings in which preferred embodiments of the present subject matter are illustrated.SUMMARY OF THE INVENTION
[0015] The present disclosure relates to a method of extracting silver, lead and zinc concentrates from jarosite comprising the steps of: i) roasting jarosite at a temperature in the range of 600 °C - 900 °C to obtain roasted jarosite; and ii) subjecting roasted jarosite to froth flotation with reagents to obtain the solid concentrates of silver and lead.
[0016] These and other aspects of the disclosed subject matter, as well as additional novel features, will be apparent from the description provided herein. The intent of this summary is not to be a comprehensive description of the claimed subject matter, but rather to provide a short overview of some of the subject matter's functionality. Other composite, methods, features and advantages here provided will become apparent to one with skill in the art upon examination of the following figures and detailed description. It is intended that all such additional systems, methods, features and advantages that are included within this description, be within the scope of any claims.BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The disclosure may be more fully understood by reading the following detailed description of the embodiment, with reference made to the accompanying drawings as follows:
[0018] Figure 1 (Fig. 1) illustrates variation of Vol% of Jarosite during roasting as a function of (a) Time at 750°C and (b) Temperature for 4 hrs each; Mineralogic software showing jarosite (c) preheated and (d) post heated;
[0019] Figure 2 (Fig. 2) illustrates Grade vs Recovery performance of (a) flotation from roasted jarosite and (b) flotation from the concentrate of (a);
[0020] Figure 3 (Fig. 3) illustrates performance of flotation from roasted and washed jarosite (a) Grade vs recovery of lead (b) Grade vs recovery of silver;
[0021] Figure 4 (Fig. 4) illustrates Scanning Electron Microscopy / Energy-Dispersive X- Ray Spectroscopy (SEM / EDS) to show elemental mapping of Ag in concentrate.
[0022] The figures depict embodiments of the present subject matter for the purposes of illustration only. A person skilled in the art will easily recognize from the following description that alternative embodiments of the structures and methods illustrated herein may be employed without departing from the principles of the disclosure described herein.DETAILED DESCRIPTION OF THE INVENTION
[0023] The detailed description of various exemplary embodiments of the disclosure is described herein. It should be noted that the embodiments are described herein in such details as to clearly communicate the disclosure. However, the amount of details provided herein are not intended to limit the anticipated variations of embodiments; on the contrary, the intention is to cover all modifications, equivalents, variations, optimizations, and alternatives falling within the scope of the present disclosure as defined by the appended claims.
[0024] It is also to be understood that various arrangements may be devised that, although not explicitly described or shown herein, embody the principles of the present disclosure. Moreover, all statements herein reciting principles, aspects, and embodiments of the present disclosure, as well as specific examples, are intended to encompass equivalents thereof.
[0025] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of example embodiments. As used herein, the singular forms “a",” “an” and “the” are intended to include the plural forms as well, unless the context clearly indicates otherwise. It will be further understood that the terms “comprises,” “comprising,” “includes” and / or “including,” when used herein, specify the presence of stated features, integers, steps, operations, elements and / or components, but do not preclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or groups thereof.
[0026] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which example embodiments belong. It will be further understood that terms, e.g., those defined in commonly used dictionaries, should be interpreted as having a meaning that is consistent with their meaning in the context of the relevant art and will not be interpreted in an idealized or overly formal sense unless expressly so defined herein.
[0027] The present disclosure discloses a process for extraction of zinc, silver and lead from jarosite, an important residue obtained after processing of metallic ores. The present process comprises of roasting of jarosite followed by flotation of the roasted jarosite to recover the metals like lead, zinc and silver.
[0028] In an embodiment of the present disclosure, the first step of roasting is carried out in an air atmosphere at varying temperatures ranging from 400°C - 1100°C, preferably 600°C - 900°C to obtain roasted jarosite. The roasting step is carried out for a time period in the range of 0.5 hours - 12 hours in a furnace. The “air” in the context of the present application refers to atmospheric air.
[0029] In an embodiment of the present disclosure, the composition of input or feed raw material may be varied using various additives including lime, sulfur, coke, or similar materials in order to optimize decomposition of jarosite for rendering it even more suitable for the subsequent step of flotation of the present process of extraction.
[0030] In an embodiment of the present disclosure, the roasting step is followed by the washing of the roasted jarosite, wherein the washing step includes washing with excess water to extract the soluble zinc sulfate produced during the roasting step. The term “excess water” means simply washing the roasted jarosite with water 5 to 10 times, each time at a ratio of water Jarosite (1: 1 to 10: 1). In yet another embodiment of the present disclosure, the methods like counter-current leaching may be employed to reduce water consumption during commercial implementation of the process.
[0031] In an embodiment of the present disclosure, zinc is recovered by extraction from the roasted jarosite in water by simply washing 10 times with water, each time at a ratio of water: jarosite of 1: 1 followed by filtration.
[0032] In an embodiment of the present disclosure, the extraction of zinc may be carried out by any combination of the extraction processes such as solvent extraction, stripping, and electrowinning. Further, the extraction of zinc may be carried out by other processes that are known to the person skilled in the art.
[0033] In an embodiment of the present disclosure, the lead-silver concentrates are treated in lead furnaces such as Ausmelt or ISF to recover lead bullion.
[0034] In an embodiment of the present disclosure, during the flotation process, various associated technical parameters of the flotation process step such as promoters (Lead-Agpromoter (di thiophosphate, Aero 3418A): 50-1000 gpt), collectors (Lead-Ag collector : Xanthate (< 200 gpt)), iron depressant (Fe depressant (NaCN): 10-100 gpt), zinc depressant (Zn Depressant (ZnSO4) < 1000 gpt), Conditioner or Sulfidzing agent (18% strength of Na2S) : 1000-10000 gpt, zinc promoters and Frother MIBC 50-200 gpt including their concentrations are selected by optimization tests for specific roasted jarosite where (gpt or g / tonne, is based on tonne of the feed to flotation)
[0035] In an embodiment of the present disclosure, the froth flotation process further includes the addition of sulphurizing materials and pH to attain the recovery of highest amount of silver, zinc and lead from jarosite through the present process of extraction.
[0036] In an embodiment of the present disclosure, the froth flotation process includes the step of addition of frothers, promoters, collectors, depressant for better recovery of lead and silver concentrate.
[0037] In yet another embodiment of the present disclosure, the frothers are selected from the group consisting of: pine oil or methyl isobutyl carbinol (MIBC). Examples of frothers are not limited to given frothers but also include all the known frothers that may be used in the froth flotation process.
[0038] In an embodiment of the present disclosure, the collectors are selected from the group consisting of: potassium amyl xanthate (PAX), sodium isopropyl xanthate (SiPX), Octadecyl amine, sodium ethyl xanthate, sodium isobutyl xanthate, or potassium ethyl xanthate. Examples of the collectors are not limited to given collectors but also include all the known collectors that may be used in the froth flotation process.
[0039] In an embodiment of the present disclosure, the promoters are selected from the group consisting of: dithiophosphate (DTP), monothiophosphate, or thionocarbamate, dithiophosphinate. Examples of the promoters are not limited to given promoters but also include all the known promoters that may be used in the froth flotation process.
[0040] In an embodiment of the present disclosure, the depressants are selected from the group consisting of: sodium cyanide (NaCN) or Na-metabisulfite. Examples of the depressants are not limited to given collectors but also include all the known depressants that may be used in the froth flotation process.
[0041] In another embodiment of the present disclosure, the froth flotation process may also include addition of conditioners or stabilizers. The conditioners or stabilizers are selectedfrom the group consisting of conditioner or sulphide based compounds like elemental sulfur, sodium sulphide, and similar components having same characteristics.
[0042] In an embodiment of the present disclosure, the step of flotation is carried out at pH in the range of 1 to 7, preferably 3 to 5.
[0043] The present disclosure also relates to lead, zinc, and silver concentrates. The recovery of lead, zinc, and silver concentrates is present in the range of 40-100% respectively.
[0044] Although embodiments for the present subject matter have been described in language specific to structural features, it is to be understood that the present subject matter is not necessarily limited to the specific features described. Rather, the specific features and methods are disclosed as embodiments for the present subject matter. Numerous modifications and adaptations of the system / component of the present invention will be apparent to those skilled in the art, and thus it is intended by the appended claims to cover all such modifications and adaptations, which fall within the scope of the present subject matter.
[0045] The invention is further illustrated by the following example, which is provided to be exemplary of the invention and does not limit the scope of the invention. While the present invention has been described in terms of its specific embodiments, certain modifications and equivalents will be apparent to those skilled in the art and are intended to be included within the scope of the present invention.ADVANTAGES OF THE PRESENT INVENTION
[0046] The recovery amount of lead, zinc, and silver concentrates obtained is high in the range of 40-100% respectively.
[0047] The process for recovery of zinc, lead and silver from jarosite provides a green alternative to the conventional method.
[0048] The process to recover zinc, lead and silver from jarosite is cost-effective.EXAMPLES:Example 1:
[0049] The jarosite produced as a by product of leaching contains about 4% zinc along with 4.3% lead and 280 ppm silver as measured by digestion followed by Atomic Absorption Spectroscopy (AAS) (table 1). Keeping in mind the need to reduce the CO emissions, the jarosite was roasted in open air at varying temperature ranging from 400 °C - 1100 °C for different time 0.5 hr - 4 hrs in a box furnace. All the different roasted products obtained are characterized under FESEM produced by Carl Zeiss (Sigma 300) with the Bruker EDS (XFlash 6160) for understanding the morphology and the phase identification using the mineralogy software made by Zeiss (Mineralogic).
[0050] The roasted jarosite had been subjected to flotation testing in 1.25 litre capacity Outokumpu flotation cell. The density of mixture of water and roasted jarosite was kept at around 1.3 gm / cc and the tests were performed at room temperature under standard atmospheric condition. Various types of reagents (frothers, collectors, promoters, depressants and conditioners) were added in different combination and concentrations to get the maximum recovery and grade of precious elements of the slag like zinc, lead and silver. Also pH was varied in different scenarios to obtain the highest grade and recovery. Post flotation the concentrates were dried at a temp of 100- 150 °C over a time span of 12- 16 hrs.Results and discussion:
[0051] The typical composition of jarosite of the present disclosure is shown in table 1 as following:Table 1: Composition of jarosite* ppm; ** weight percentage
[0052] The roasted jarosite was subjected to minerology study in Field Emission Scanning Electron Microscope (Sigma 300) using Mineralogic software. The volume fraction of the jarosite as a function of time and temperature is shown in Figure 1 (a) and (b) respectively:
[0053] It was observed that the vol% of jarosite significantly decreased on roasting it around 750 °C for about 4 hrs with a yield of around ~70 %. In the process some amount of Zinc is lost in the form of oxides. The 750 °C -4 hr roasted jarosite (composition shown in table 2) has been used for further study on recovery of metals by dissolution and floatation.
[0054] The composition of this silver concentrate are as below: Table 2: Composition of silver-rich concentrate after froth collection time of 1 minute:* ppm; ** weight percentage
[0055] The roasted jarosite was subjected to flotation studies for extraction of silver from the same. The effect of various parameters of flotation was evaluated and the silver recovery of 80% was observed with a grade cone, of 1800 ppm as shown in figure 2(a). The re floatation of the rougher concentrate (having grade ~ 4000 ppm Ag) resulted in a further enriched concentrate having 14000 ppm Ag with 76% Ag recovery as shown in figure 2(b).
[0056] However, the above condition was unfavourable for recovery of lead and zinc by flotation. The zinc present in the roasted jarosite is in the form of zinc sulphate as confirmed by XRD and it was easily recovered by dissolving the soluble components of the roasted jarosite in water by simply washing 2 times with water, each time at a ratio of water: jarosite of 1 : 1 followed by filtration. This increased the residue pH from ~ 1.0 to ~7.0 and recovered ~ 75 % zinc in the final wash water with Zn concentration of 3- 4 gpl. Zinc metal is recovered from this solution by known processes of solvent extraction, stripping in water and electrowinning.
[0057] Further flotation tests were performed with roasted and washed jarosite (zinc got recovered by washing) as shown in figure 3(a) and (b). Flotation of washed roasted jarosite with Aero 3148A gave promising results in terms of lead grade and recovery: highestcumulative Pb grade achieved ~ 16 wt% with a cumlative Pb recovery of ~ 56%. Along with the lead, silver also got floated and we could achieve a cumulative silver recovery of ~ 62%.SEM / EDS analysis was also done in the Ag rich concentrate to identify the type of compounds floated and it was observed to mainly in oxide and sulphide forms as shown in figure 4 and table 3 below.Table 3: Energy-Dispersive X-Ray Spectroscopy (EDS) analysis of Ag particles:SPECIFIC EMBODIMENTS OF THE PRESENT INVENTION
[0058] The present disclosure relates to a method of extracting silver, lead and zinc concentrates from jarosite comprising the steps of: roasting jarosite at a temperature in the range of 600 °C - 900 °C to obtain roasted jarosite; and subjecting roasted jarosite to froth flotation with reagents to obtain the aqueous solution of zinc and solid concentrates of silver and lead.
[0059] Such method is disclosed, wherein washing the roasted jarosite of step i) with water to extract the soluble zinc sulfate produced during roasting.
[0060] Such method is disclosed, wherein zinc is extracted from the aqueous solution of zinc sulfate.
[0061] Such method is disclosed, wherein carrying out the roasting at a time period in the range of 0.5 - 12 hours in a furnace under air.
[0062] Such method is disclosed, wherein the reagents are selected from the group consisting of frothers, collectors, promoters, depressants, or combinations thereof.
[0063] Such method is disclosed, wherein the frothers are selected from the group consisting of: pine oil or methyl isobutyl carbinol (MIBC) and wherein the collectors are selected from the group consisting of: potassium amyl xanthate (PAX), sodium isopropyl xanthate (SiPX), Octadecyl amine, sodium ethyl xanthate, sodium isobutyl xanthate, or potassium ethyl xanthate.
[0064] Such method is disclosed, wherein the promoters are selected from the group consisting of: dithiophosphate (DTP), monothiophosphate, or thionocarbamate, dithiophosphinate, and wherein the depressants are selected from the group consisting of: sodium cyanide (NaCN) or Na-metabisulfite.
[0065] Such method is disclosed, wherein the promoters are selected from the group consisting of: dithiophosphate (DTP), monothiophosphate, or thionocarbamate, dithiophosphinate, and wherein the depressants are selected from the group consisting of: sodium cyanide (NaCN) or Na-metabisulfite.
[0066] Such method is disclosed, wherein the step of flotation is carried out at pH in the range of 3 to 5.
[0067] Such method is disclosed, wherein the lead, zinc, and silver concentrates obtained from the method as claimed in any of claims 1 to 8, wherein an amount of lead, zinc, and silver concentrates is in the range of 40-100% respectively.
Claims
WE CLAIM1. A method of extracting silver, lead and zinc concentrates from jarosite comprising the steps of: i) roasting jarosite at a temperature in the range of 600 °C - 900 °C to obtain roasted jarosite; and ii) subjecting roasted jarosite to froth flotation with reagents to obtain the aqueous solution of zinc and solid concentrates of silver and lead.
2. The method as claimed in claim 1, wherein washing the roasted jarosite of step i) with water to extract the soluble zinc sulfate produced during roasting.
3. The method as claimed in claim 1, wherein zinc is extracted from the aqueous solution of zinc sulfate.
4. The method as claimed in claim 1 , wherein carrying out the roasting at a time period in the range of 0.5 - 12 hours in a furnace under air.
5. The method as claimed in claim 1, wherein the reagents are selected from the group consisting of frothers, collectors, promoters, depressants, or combinations thereof.
6. The method as claimed in claimed in claim 5, wherein the frothers are selected from the group consisting of: pine oil or methyl isobutyl carbinol (MIBC) and wherein the collectors are selected from the group consisting of: potassium amyl xanthate (PAX), sodium isopropyl xanthate (SiPX), Octadecyl amine, sodium ethyl xanthate, sodium isobutyl xanthate, or potassium ethyl xanthate.
7. The method as claimed in claim 5, wherein the promoters are selected from the group consisting of: dithiophosphate (DTP), mono thiophosphate, or thionocarbamate, dithiophosphinate, and wherein the depressants are selected from the group consisting of: sodium cyanide (NaCN) or Na-metabisulfite.
8. The method as claimed in claim 1, wherein the step of flotation is carried out at pH in the range of 3 to 5.Lead, zinc, and silver concentrates obtained from the method as claimed in any of claims 1 to 8, wherein an amount of lead, zinc, and silver concentrates is in the range of 40-100% respectively.