Connection structure manufacturing method, and connection structure

The method of using film-like solder connection materials with controlled thickness and spacing addresses the issue of short circuits in surface-mounted components by ensuring uniform solder placement and thickness, thereby improving continuity reliability.

WO2024241858A1PCT designated stage expired Publication Date: 2024-11-28DEXERIALS CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016883
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-03-27
Filing Date
2024-05-02
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing methods for mounting surface-mounted components on rigid or flexible boards using solder particles often result in short circuits due to inefficient arrangement of solder particles between terminal rows, leading to reliability issues with continuity.

Method used

A method involving the use of film-like solder connection materials with rectangular portions corresponding to terminal rows, where the solder connection films are arranged and bonded without mechanical load, ensuring the relative standard deviation of solder thickness is less than 25%, and the distance between film portions is controlled to prevent solder particle movement and agglomeration.

Benefits of technology

This approach enables efficient placement of solder particles onto electrodes, enhancing conduction reliability and preventing short circuits by maintaining uniform solder thickness and preventing solder particle movement between terminal rows.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016883_28112024_PF_FP_ABST
    Figure JP2024016883_28112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are: a connection structure manufacturing method that allows solder particles to be efficiently arranged on an electrode and enables obtaining high conduction reliability; and a connection structure. The method includes: a disposition step for disposing a surface mounting component provided with a plurality of terminal rows, on a wiring substrate via a film-like solder connection material having rectangular parts corresponding to the respective terminal rows; and a joining step for joining the surface mounting component to the wiring substrate. The relative standard deviation of the solder thicknesses between terminals of the surface mounting component and terminals of the wiring substrate after the joining step is less than 25%.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing a connection structure, and connection structure

[0001] This technology relates to a method for manufacturing a connection structure that connects, for example, surface-mounted components using solder particles, and the connection structure. This application claims priority based on Japanese Patent Application No. 2023-084414 filed in Japan on May 23, 2023, and Japanese Patent Application No. 2024-050937 filed in Japan on March 27, 2024, both of which are incorporated herein by reference.

[0002] Mounting of surface mount devices (SMD) onto rigid or flexible substrates is generally performed by printing or temporarily attaching solder paste or film to the substrate, placing the surface mount components on top of it, and then performing a reflow process (see, for example, Patent Documents 1 to 3).

[0003] In the techniques described in Patent Documents 1 to 3, when a surface-mounted component having multiple terminal rows is mounted, some of the solder particles tend to be disposed between the terminal rows, making it difficult to efficiently dispose the solder particles on the electrodes (lines). This can cause short circuits (bridges) between adjacent terminals, making it difficult to achieve high electrical reliability.

[0004] JP 2017-041442 A JP 2016-219808 A International Publication No. 2008 / 023452

[0005] The present technology solves the above-mentioned problems, and provides a method for manufacturing a connection structure that allows solder particles to be efficiently moved onto an electrode and high conductivity reliability to be obtained, and a connection structure.

[0006] As a result of extensive research, the present inventors have found that the following method for manufacturing a connection structure and the connection structure can achieve the above-mentioned object, and have completed the present technology.

[0007] [1] A method for manufacturing a connection structure, comprising: an arrangement step of arranging a surface mount component having a plurality of terminal rows on a wiring board via a film-like solder connecting material having a rectangular portion corresponding to each of the terminal rows, and a joining step of joining the surface mount component to the wiring board. [2] A method for manufacturing a connection structure as described in [1], in which the relative standard deviation of the solder thickness between the terminals of the surface mount component and the terminals of the wiring board after the joining step is less than 25%. [3] A method for manufacturing a connection structure as described in [1] or [2], in which the surface mount component has a first terminal row and a second terminal row arranged in parallel, and in the arrangement step, a first film-like solder connecting material corresponding to the first terminal row and a second film-like solder connecting material corresponding to the second terminal row are arranged, and the distance between the rectangular portion of the first film-like solder connecting material and the rectangular portion of the second film-like solder connecting material is 0 mm or more. [4] The method for manufacturing a connection structure according to [3], wherein the surface mount component comprises a first terminal row and a second terminal row arranged in parallel, and wherein, in the arranging step, the width W of the rectangular portion of the first film-like solder connection material and the width W of the rectangular portion of the second film-like solder connection material satisfy the following formula (1): W≦(2L+S) / 2 (1) In the formula (1), L is the length of the terminals in the first terminal row and the second terminal row, and S is the distance between the first terminal row and the second terminal row. [5] The method for manufacturing a connection structure according to [1] or [2], wherein, in the joining step, the surface mount component is joined to the wiring board without load using a reflow oven. [6] The method for manufacturing a connection structure according to [1] or [2], wherein the pitch of the terminal rows of the surface mount component and the wiring board is 0.1 mm to 0.4 mm. [7] The method for manufacturing a connection structure according to [1] or [2], wherein the content of solder particles in the film-like solder connection material is 10% by volume to 60% by volume relative to a terminal row pitch of 0.1 mm to 0.4 mm of the surface mount component and the wiring board.[8] The method for manufacturing a connection structure according to [1] or [2], wherein the surface mount component comprises a first terminal row and a second terminal row arranged in parallel, and in the arranging step, a first film-like solder connection material corresponding to the first terminal row and a second film-like solder connection material corresponding to the second terminal row are arranged, and the amount of protrusion of the rectangular portion of the first film-like solder connection material from the first terminal row in the width direction is 50% or less of the terminal length of the first terminal row, and the amount of protrusion of the rectangular portion of the second film-like solder connection material from the second terminal row in the width direction is 50% or less of the terminal length of the second terminal row. [9] The method for manufacturing a connection structure according to [1] or [2], wherein the surface mount component comprises first and second terminal rows arranged in parallel, and third and fourth terminal rows arranged in parallel and perpendicular to the first and second terminal rows, and wherein the amount of protrusion in the width direction of a rectangular portion corresponding to the first, second, third, or fourth terminal row from the terminal row is 50% or less of the length of the terminal of the corresponding first, second, third, or fourth terminal row.

[10] A connection structure comprising a surface mount component having a plurality of terminal rows, a wiring board, and a cured film of a film-like solder connecting material provided for each of the terminal rows, bonding the surface mount component to the wiring board, and having a rectangular portion corresponding to each of the terminal rows.

[11] The connection structure according to

[10] , wherein the relative standard deviation of the solder thickness between the terminals of the surface mount component and the terminals of the wiring board is less than 25%.

[12] The connection structure according to

[10] or

[11] , wherein the pitch of the terminal rows of the surface mount component and the wiring board is 0.1 mm to 0.4 mm.

[13] The connection structure according to

[10] or

[11] , wherein the surface mount component comprises a first terminal row and a second terminal row arranged in parallel, and the amount of protrusion of the rectangular portions of the first film-like solder connection material from the first terminal row in the width direction is 50% or less of the terminal length of the first terminal row, and the amount of protrusion of the rectangular portions of the second film-like solder connection material from the second terminal row in the width direction is 50% or less of the terminal length of the second terminal row.

[14] The connection structure according to

[10] or

[11] , wherein the surface mount component comprises a first terminal row and a second terminal row arranged in parallel, and a third terminal row and a fourth terminal row arranged in parallel and perpendicular to the first terminal row and the second terminal row, and the amount of protrusion in the width direction of the rectangular portion corresponding to the first terminal row, the second terminal row, the third terminal row or the fourth terminal row from the terminal row is 50% or less of the terminal length of the corresponding first terminal row, the second terminal row, the third terminal row or the fourth terminal row.

[0008] According to this technique, solder particles can be efficiently moved onto the electrodes, and high conductivity reliability can be obtained.

[0009] FIG. 1 is a plan view schematically showing a state in which a solder connection film is provided on each of parallel first and second terminal rows of a wiring board. FIG. 2 is a cross-sectional view schematically showing a state in which a solder connection film is provided on the first terminal row of a wiring board. FIG. 3 is a cross-sectional view schematically showing a state in which the first terminal row of the wiring board and the first terminal row of a surface-mounted component are aligned. FIG. 4 is a cross-sectional view schematically showing a state in which the wiring board and the surface-mounted component are heated in a reflow furnace. FIG. 5 is a plan view schematically showing an example of a wiring board. FIG. 6(A) is a plan view schematically showing an example of a metal mask as an example, and FIG. 6(B) is a plan view schematically showing an example of a solder paste film printed using the metal mask shown in FIG. 6(A). FIG. 7(A) is a plan view schematically showing an example of a metal mask as a comparative example, and FIG. 7(B) is a plan view schematically showing an example of a solder paste film printed using the metal mask shown in FIG. 7(A). FIG. 8(A) is a plan view schematically showing an example of a metal mask as a comparative example, and FIG. 8(B) is a plan view schematically showing an example of a solder paste film printed using the metal mask shown in FIG. 8(A). FIG. 9 is a cross-sectional view showing an example of a short-side direction of a plug and a receptacle in a vertical mating type connector. FIG. 10 is a cross-sectional view schematically showing a long-side direction of a connection structure in which a connector plug and a wiring board are connected. FIG. 11 is a cross-sectional view schematically showing a short-side direction of a connection structure in which a connector plug and a wiring board are connected. FIG. 12(A) is a photograph showing a state in which a solder connection film is temporarily attached to a printed wiring board for Example 1, FIG. 12(B) is a photograph showing a state in which a connector is mounted on a printed wiring board for Example 1, and FIG. 12(C) is an X-ray photograph showing the connection structure after reflow for Example 1. Fig. 13(A) is a photograph showing a state in which a solder connection film is temporarily attached to a printed wiring board for Comparative Example 1, Fig. 13(B) is a photograph showing a state in which a connector is mounted on a printed circuit board for Comparative Example 1, and Fig. 13(C) is an X-ray photograph showing the connection structure after reflow for Comparative Example 1. Fig. 14 is a photograph showing a sample after reflow for Example 13. Fig. 15 is a photograph showing a sample after reflow for Comparative Example 6.Fig. 16 is an X-ray photograph showing a sample after reflow for Example 15. Fig. 17 is an X-ray photograph showing a sample after reflow for Comparative Example 8. Fig. 18(A1) is a photograph showing a state in which an anisotropic conductive film of a predetermined shape is temporarily attached to a wiring board for a plug connector as Comparative Example 9, Fig. 18(A2) is a plan view schematically showing the shape of the anisotropic conductive film, Fig. 18(B) is a photograph showing a state in which a plug connector is reflow-mounted on a wiring board for a plug connector, and Fig. 18(C) is an X-ray photograph showing the plug connector structure after mounting. Fig. 19(A1) is a photograph showing a state in which an anisotropic conductive film of a predetermined shape is temporarily attached to a wiring board for a plug connector as Example 16, Fig. 19(A2) is a plan view schematically showing the shape of the anisotropic conductive film, Fig. 19(B) is a photograph showing a state in which a plug connector is reflow-mounted on the wiring board for a plug connector, and Fig. 19(C) is an X-ray photograph showing the plug connector structure after mounting. Fig. 20(A1) is a photograph showing a state in which an anisotropic conductive film of a predetermined shape is temporarily attached to a wiring board for a plug connector as Example 17, Fig. 20(A2) is a plan view schematically showing the shape of the anisotropic conductive film, Fig. 20(B) is a photograph showing a state in which a plug connector is reflow-mounted on the wiring board for a plug connector, and Fig. 20(C) is an X-ray photograph showing the plug connector structure after mounting. Fig. 21(A1) is a photograph showing a state in which an anisotropic conductive film of a predetermined shape is temporarily attached to a wiring board for a plug connector as Example 18, Fig. 21(A2) is a plan view schematically showing the shape of the anisotropic conductive film, Fig. 21(B) is a photograph showing a state in which a plug connector is reflow-mounted on the wiring board for a plug connector, and Fig. 21(C) is an X-ray photograph showing the plug connector structure after mounting. Fig. 22(A1) is a photograph showing a state in which an anisotropic conductive film of a predetermined shape is temporarily attached to a wiring board for a receptacle connector as Comparative Example 10, Fig. 22(A2) is a plan view schematically showing the shape of the anisotropic conductive film, Fig. 22(B) is a photograph showing a state in which a receptacle connector is reflow-mounted on the wiring board for a receptacle connector, and Fig. 22(C) is an X-ray photograph showing the receptacle connector structure after mounting.Fig. 23(A1) is a photograph showing a state in which an anisotropic conductive film of a predetermined shape has been temporarily attached to a wiring board for a receptacle connector as Example 19, Fig. 23(A2) is a plan view schematically showing the shape of the anisotropic conductive film, Fig. 23(B) is a photograph showing a state in which a receptacle connector has been reflow-mounted on the wiring board for a receptacle connector, and Fig. 23(C) is an X-ray photograph showing the receptacle connector structure after mounting. Fig. 24(A1) is a photograph showing a state in which an anisotropic conductive film of a predetermined shape has been temporarily attached to a wiring board for a receptacle connector as Example 20, Fig. 24(A2) is a plan view schematically showing the shape of the anisotropic conductive film, Fig. 24(B) is a photograph showing a state in which a receptacle connector has been reflow-mounted on the wiring board for a receptacle connector, and Fig. 24(C) is an X-ray photograph showing the receptacle connector structure after mounting.

[0010] Hereinafter, embodiments of the present technology will be described in detail with reference to the drawings in the following order: 1. Connection structure manufacturing method and connection structure 2. Solder connection film 3. First example 4. Second example 5. Third example 6. Fourth example

[0011] 1. Method for Manufacturing Connection Structure and Connection Structure The method for manufacturing a connection structure according to the present embodiment includes an arrangement step of arranging a surface-mounted component having a plurality of terminal rows on a wiring board via a film-like solder connection material having a rectangular portion whose longitudinal direction is the row direction of the terminal rows, and a joining step of joining the surface-mounted component to the wiring board. Here, when the surface-mounted component has a first terminal row and a second terminal row arranged in parallel, it is preferable that the amount of protrusion of the solder connection film of the first terminal row or the second terminal row arranged between the first terminal row and the second terminal row is 50% or less of the terminal length in a direction perpendicular to the row direction of the first terminal row or the second terminal row. Furthermore, when a surface mount component includes first and second terminal rows arranged in parallel and third and fourth terminal rows arranged in parallel and perpendicular to the first and second terminal rows, the amount of protrusion of the solder connection film of the first, second, third, or fourth terminal row arranged between the first and second terminal rows is preferably 50% or less of the terminal length in the direction perpendicular to the row direction of the first, second, third, or fourth terminal row, thereby preventing solder particles from remaining between the first and second terminal rows without agglomerating.

[0012] The connection structure according to the present embodiment includes a surface-mounted component having a plurality of terminal rows, a wiring board, and a cured film of a film-like solder connection material provided for each terminal row, the film-like solder connection material having a rectangular portion with its longitudinal direction aligned with the row direction of the terminal row for each terminal row. Here, when the surface-mounted component has a first terminal row and a second terminal row arranged in parallel, it is preferable that the amount of protrusion of the cured film of the solder connection film of the first terminal row or the second terminal row arranged between the first terminal row and the second terminal row is 50% or less of the terminal length in a direction perpendicular to the row direction of the first terminal row or the second terminal row. Furthermore, when a surface mount component includes first and second terminal rows arranged in parallel, and third and fourth terminal rows arranged in parallel and perpendicular to the first and second terminal rows, the amount of protrusion of the cured film of the solder connection film of the first, second, third, or fourth terminal row arranged between the first and second terminal rows is preferably 50% or less of the terminal length in a direction perpendicular to the row direction of the first, second, third, or fourth terminal row. This prevents solder particles from remaining unaggregated inside the first to fourth terminal rows.

[0013] In this embodiment, a film-like solder connection material having a rectangular portion with its longitudinal direction aligned with the direction of the terminal row is provided for each terminal row, thereby limiting the movement of solder particles between terminal rows due to the self-alignment effect during the joining process. This allows the solder particles within a predetermined rectangular portion to aggregate for a predetermined terminal row, thereby achieving high electrical connection reliability. As will be described later, the film-like solder connection material may be a solder connection film or a solder paste film on which solder paste is printed.

[0014] Furthermore, the film-like solder connection material may be continuous in portions other than the rectangular portions corresponding to the terminal rows. For example, when connecting a connector having a first terminal row and a second terminal row arranged in parallel, a film-like solder connection material may be used in which both ends of the parallel rectangular portions in the longitudinal direction are connected by continuous portions. With such a film-like solder connection material, the continuous portions at both ends can further improve the adhesive strength.

[0015] Here, a connection structure refers to two materials or members electrically connected together. Bonding refers to joining two materials or members together. A terminal row refers to terminals (electrodes) lined up in a predetermined direction at a predetermined interval (pitch). The predetermined direction in which the terminals are lined up is called the row direction of the terminal row, and the direction perpendicular to the row direction is called the width direction of the terminal row.

[0016] The surface mount component is not particularly limited as long as it has multiple terminal rows, and examples include a component having a first terminal row and a second terminal row arranged in parallel, a component having a first terminal row and a second terminal row arranged in parallel, and a component having a third terminal row and a fourth terminal row arranged in parallel and perpendicular to the first terminal row and the second terminal row.

[0017] Specific examples of surface-mounted components include connectors, IC (Integrated Circuit) and LSI (Large Scale Integration) packages, LEDs (Light Emitting Diodes), and switches. For example, connectors include SMT (Surface Mount) type connectors, which include a first terminal row in which multiple pins (lead frames) extending outward from one side of the short side are arranged in the longitudinal direction, and a second terminal row in which multiple pins (lead frames) extending outward from the other side of the short side are arranged in the longitudinal direction. Furthermore, examples of IC packages include surface-mounted lead-type packages, such as SOP (Small Outline Package) and SOJ (Small Outline J-leaded) which include terminal rows on two opposing sides of a rectangle, and QFP (Quad Flat Package) and QFN (Quad Flat No-leaded package) which include terminal rows on four sides of a rectangle.

[0018] The wiring board is not particularly limited as long as it has wiring, and may be broadly defined as a so-called printed wiring board (PWB) provided with electrodes on which surface-mounted components can be mounted, and may be either a rigid board or a flexible board (FPC: Flexible Printed Circuits). Examples of substrates based on the type of base material include glass substrates, ceramic substrates, and plastic substrates.

[0019] The upper limit of the pitch of the terminal rows of the surface mount components and the wiring board is preferably 2 mm or less, more preferably 1 mm or less, and even more preferably 0.5 mm or less, and the lower limit of the pitch of the terminal rows is preferably 0.06 mm or more, more preferably 0.08 mm or more, and even more preferably 0.1 mm or more.

[0020] The average thickness (height) of the solder between the terminals of the connection structure depends on the electrode area of ​​the wiring board and the surface-mounted component, the solder particle content of the film-like solder connection material, etc., but the lower limit of the thickness is preferably 5 μm or more, more preferably 20 μm or more, and even more preferably 40 μm or more. The upper limit of the thickness is preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 80 μm or less. This makes it possible to withstand the stress caused by the difference in linear expansion between the surface-mounted component and the wiring board due to thermal shock, and achieve high conductivity reliability.

[0021] Furthermore, the relative standard deviation (coefficient of variation, RSD) of the thickness (height) of the solder between the terminals after reflow is preferably less than 25%, more preferably 20% or less, and even more preferably 15% or less. A small rate of variation in the thickness (height) of the solder between the terminals makes it possible to obtain high conductivity reliability. Furthermore, the standard deviation (σ) of the thickness (height) of the solder between the terminals of the connection structure depends on the average thickness (height) of the solder between the terminals, etc., but for example, when the average thickness (height) of the solder between the terminals is 5 μm or more and 200 μm, it is preferably 20 μm or less, more preferably 12 μm or less, and even more preferably 10 μm or less. A small rate of variation in the thickness of the solder between the terminals makes it possible to obtain high conductivity reliability.

[0022] Hereinafter, with reference to Figures 1 to 4, we will explain the process (A) of providing a solder connection film on multiple terminal rows of a wiring board, the process (B) of fixing surface-mounted components on the solder connection film, and the process (C) of joining the multiple terminal rows of the wiring board and the multiple terminal rows of the surface-mounted components using a reflow furnace.

[0023] [Step (A)] Fig. 1 is a plan view showing a state in which a solder connection film is provided on each of parallel first and second terminal rows of a wiring board, and Fig. 2 is a cross-sectional view showing a state in which a solder connection film is provided on the first terminal row of a wiring board. As shown in Figs. 1 and 2, in step (A), a rectangular first solder connection film 21 and a rectangular second solder connection film 22 containing solder particles 20 and having a longitudinal direction aligned with the row direction of the terminal rows are provided on each of the first terminal row 11 and the second terminal row 12 of a wiring board 10.

[0024] Process (A) may be a temporary bonding process in which the first solder connection film 21 and the second solder connection film 22 are respectively attached to the first terminal row 11 and the second terminal row 12 of the wiring board 10 at low temperature and low pressure, or may be a lamination process in which the first solder connection film 21 and the second solder connection film 22 are respectively laminated onto the first terminal row 11 and the second terminal row 12 of the wiring board 10.

[0025] The width W of the first and second solder connection films 21, 22 is preferably 50% to 150% of the length L of the terminals 11a, 12a, and more preferably 75% to 125% of the length L. This allows the solder particles to aggregate on the terminals of the terminal row, thereby reducing the variation in the solder height on the terminals of the terminal row.

[0026] Furthermore, the first and second solder connection films 21, 22 are preferably provided aligned with the outer widthwise edges of the first terminal row 11 and the second terminal row 12. Furthermore, the widthwise protrusion amount (WL) of the rectangular portion of the first or second solder connection film disposed between the first and second terminal rows 11, 12 is preferably 50% or less, and more preferably 25% or less, of the length L of the terminals 11a, 12a. This makes it possible to prevent solder particles 20 from remaining between the first terminal row 11 and the second terminal row 12 without agglomerating.

[0027] Furthermore, it is preferable that the width W of the first and second solder connection films 21, 22 satisfy the following formula (1): W≦(2L+S) / 2 (1) In the formula (1), L is the length of the terminals 11a, 12a, and S is the distance between the first terminal row 11 and the second terminal row 12. It is sufficient that there is a boundary between the first solder connection film 21 and the second solder connection film 22, and the distance (gap) S F may be zero.

[0028] The distance S between the first terminal row 11 and the second terminal row 12 is preferably 10 mm or less, more preferably 1 mm or less, and even more preferably 0.5 mm or less. Even if the distance S between the first terminal row 11 and the second terminal row 12 is short, it is preferable that there is a boundary between the first solder connection film 21 and the second solder connection film 22, and the distance (gap) S F is preferably 0 mm or more, preferably 0.1 mm or more, and more preferably 0.2 mm or more. The presence of a boundary between the first solder connection film 21 and the second solder connection film 22 can restrict the movement of solder particles and reduce variations in the solder height on the terminals of the terminal row.

[0029] 3 is a cross-sectional view showing a state in which the first terminal row of the wiring board 10 and the first terminal row of the surface mount component 30 are aligned. As shown in FIG. 3, in step (B), the first and second terminal rows 11 and 12 of the wiring board 10 are aligned with the first and second terminal rows 31 and 32 of the surface mount component 30, and the surface mount component 30 is fixed onto the first solder connection film 21.

[0030] In step (B), for example, a tool is used to align the first and second terminal rows 11, 12 with the first and second terminal rows 31, 32 of the surface mount component 30. The tool preferably has a suction mechanism for suctioning the surface mount component. In step (B), temporary pressure bonding may be performed by pressing the surface mount component 30 from the side using the tool.

[0031] [Step (C)] Figure 4 is a cross-sectional view schematically illustrating the state in which the wiring board and surface-mounted components are heated in a reflow furnace. As shown in Figure 4, in step (C), the first and second terminal rows 11, 12 of the wiring board 10 and the first and second terminal rows 31, 32 of the surface-mounted components 30 are joined with solder 41 using a reflow furnace set at a temperature above the melting point of the solder particles 20. The wiring board 10 and the surface-mounted components 30 are also bonded with the binder 40 of the solder connection film. Here, the first and second solder connection films 21, 22 containing solder particles 20 are provided on the first and second terminal rows 11, 12 of the wiring board 10, respectively. This limits the movement of solder particles between the terminal rows due to the self-alignment effect during reflow. This allows only the solder particles 20 in the first and second solder connection films 21, 22 to aggregate relative to the first and second terminal rows 11, 12, respectively.

[0032] Examples of reflow furnaces include atmospheric pressure reflow, vacuum reflow, atmospheric pressure ovens, and autoclaves (pressure ovens). Among these, it is preferable to use vacuum reflow and autoclaves, which can eliminate air bubbles contained in the joints. A reflow furnace can heat and bond the components without applying mechanical pressure and without load, thereby suppressing damage to the wiring board 10 and the surface-mounted components 30. Here, "without load" refers to a state in which no mechanical pressure is applied.

[0033] The lower limit of the peak temperature (maximum temperature reached) in the reflow furnace should be equal to or higher than the temperature at which the solder particles melt and the temperature at which the solder connection film begins to harden, and is preferably 150°C or higher, more preferably 180°C or higher, and even more preferably 200°C or higher. The upper limit of the peak temperature in the reflow furnace is 300°C or lower, more preferably 290°C or lower, and even more preferably 280°C or lower. This results in solder bonding between the first terminal row 11 of the wiring board 10 and the first terminal row 31 of the surface-mounted component 30. Furthermore, when a thermosetting binder is used for the solder connection film, the thermosetting binder bonds the portions of the terminals other than the solder joints. Here, solder bonding refers to connecting the terminals (electrodes) of opposing electronic components by melting solder.

[0034] The average thickness (height) T of the solder 41 between the terminals after reflow depends on the electrode area of ​​the wiring board and surface-mounted component, the solder particle content of the solder connection film, etc., but the lower limit of the thickness is preferably 5 μm or more, more preferably 20 μm or more, and even more preferably 40 μm or more. The upper limit of the thickness T is preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 80 μm or less. This makes it possible to withstand the stress caused by the difference in linear expansion between the surface-mounted component and the wiring board due to thermal shock, and achieve high conductivity reliability.

[0035] Furthermore, the relative standard deviation (coefficient of variation, RSD) of the thickness (height) of the solder between the terminals after reflow is preferably less than 25%, more preferably 20% or less, and even more preferably 15% or less. A small rate of variation in the thickness (height) of the solder between the terminals makes it possible to obtain high conductivity reliability. Furthermore, the standard deviation (σ) of the thickness (height) of the solder between the terminals of the connection structure depends on the average thickness (height) of the solder between the terminals, etc., but for example, when the average thickness (height) of the solder between the terminals is 5 μm or more and 200 μm, it is preferably 20 μm or less, more preferably 12 μm or less, and even more preferably 10 μm or less. A small rate of variation in the thickness of the solder 41 between the terminals makes it possible to obtain high conductivity reliability.

[0036] According to the above-described method for manufacturing a connection structure, by providing a solder connection film for each terminal row, it is possible to limit the movement of solder particles between terminal rows due to the self-alignment effect during heating, and therefore it is possible to aggregate only the solder particles in a predetermined solder connection film for a predetermined terminal row, thereby achieving high electrical reliability.

[0037] In the above-described method for manufacturing a connection structure, in step (C), a reflow furnace is used to join multiple terminal rows of the wiring board and multiple terminal rows of the surface-mounted component, but this is not limited to this, and for example, joining may be performed using a heating and pressurizing tool within a range that does not prevent the solder particles from agglomerating onto the terminals.

[0038] The solder connection film may be shaped according to the electrode pattern of the wiring board. For example, the solder connection film may have a substantially rectangular first shaped portion corresponding to a predetermined terminal row, a second shaped portion connected to one end of the first shaped portion and corresponding to an electrode at one end of the predetermined terminal row, and a third shaped portion connected to the other end of the first shaped portion and corresponding to an electrode at the other end of the predetermined terminal row, and may have a shape in which the first shaped portion to the third shaped portion are combined. Furthermore, for example, the solder connection film may have a substantially rectangular first shaped portion corresponding to the first terminal row, a substantially rectangular second shaped portion corresponding to the second terminal row, a third shaped portion connecting one end of the first shaped portion to one end of the second shaped portion and corresponding to a pair of electrodes at one end of the first terminal row and the second terminal row, and a fourth shaped portion connecting the other end of the first shaped portion to the other end of the second shaped portion and corresponding to a pair of electrodes at the other end of the first terminal row and the second terminal row, and may have a shape in which the first shaped portion to the fourth shaped portion are combined.

[0039] As described above, the distance (gap) between the shaped portions corresponding to adjacent terminal rows is preferably 0 mm or more, preferably 0.1 mm or more, and more preferably 0.2 mm or more. The presence of a boundary between the shaped portions corresponding to adjacent terminal rows can limit the movement of solder particles and reduce the variation in solder height on the terminals of the terminal row. A solder connection film of this shape can be obtained by punching, slitting, or the like.

[0040] [Modification] In the above-described method for manufacturing a connection structure, a solder connection film is provided on the terminal row in step (A), but this is not limited to this, and for example, a solder paste film may be provided on the terminal row by printing solder paste using a metal mask (stencil). Examples of solder paste include those obtained by removing polymer components from the binder formulation of the solder connection film described below to reduce viscosity.

[0041] Printing of solder paste using a metal mask will be described below with reference to FIGS. 5 to 8 . FIG. 5 is a plan view schematically illustrating an example of a wiring board. As shown in FIG. 5 , wiring board 50 includes a first terminal row 51 in which a plurality of terminals 51 a, 51 b, 51 c, and 51 d are arranged at predetermined intervals, and a second terminal row 52 in which a plurality of terminals 52 a, 52 b, 52 c, and 52 d are arranged at predetermined intervals. The row directions of first terminal row 51 and second terminal row 52 are parallel to each other, and the distance between first terminal row 51 and second terminal row 52 is preferably 10 mm or less, more preferably 1 mm or less, and even more preferably 0.5 mm or less, as described above.

[0042] Fig. 6(A) is a plan view schematically showing an example of a metal mask according to an embodiment, and Fig. 6(B) is a plan view schematically showing an example of a solder paste film printed using the metal mask shown in Fig. 6(A). The metal mask 53 shown in Fig. 6(A) has a first opening 54 corresponding to the first terminal row 51 and a second opening 55 corresponding to the second terminal row 52.

[0043] The solder paste printing method involves aligning and setting the wiring board 50 under the metal mask 53, then moving the squeegee downward from above the metal mask 53 while pressing it down, applying the solder paste to predetermined locations through the openings in the metal mask 53, and then releasing the set wiring board 50. This allows a solder paste film with the same shape as the openings in the metal mask 53 to be transferred to the wiring board 50.

[0044] 6(B), in the wiring board 50, a first solder paste film 56 having the same shape as the first opening 54 is provided on the first terminal row 51, and a second solder paste film 57 having the same shape as the second opening 55 is provided on the second terminal row 52, ​​with a gap provided between the first solder paste film 56 and the second solder paste film 57. This makes it possible to limit the movement of solder particles between the terminal rows due to the self-alignment effect during heating, and therefore makes it possible to aggregate only the solder particles in a predetermined solder connection film for a predetermined terminal row, thereby achieving high conductivity reliability.

[0045] Similarly to the solder connection film described below, the thickness of the solder paste film printed on the wiring board 50 has a lower limit of preferably 0.6 or more, more preferably 0.8 or more, and even more preferably 0.9 or more, relative to the average particle size of the solder particles. The upper limit of the thickness is preferably 3.0 or less, more preferably 2.0 or less, and even more preferably 1.5 or less, relative to the average particle size of the solder particles. If the ratio of the average particle size of the solder particles to the thickness of the solder paste film is large, printing using a metal mask may become more difficult.

[0046] Here, the thickness of the solder paste film refers to the thickness of the binder resin layer only, and does not include the particle diameter. The thickness of the film-like solder paste can be measured using a known micrometer or digital thickness gauge (e.g., MDE-25M, minimum display 0.0001 mm, manufactured by Mitutoyo Corporation) that can measure thicknesses of 1 μm or less, preferably 0.1 μm or less. The film thickness can be determined by measuring at 10 or more locations and averaging the measured thickness.

[0047] Fig. 7(A) is a plan view schematically showing an example of a metal mask as a comparative example, and Fig. 7(B) is a plan view schematically showing an example of a solder paste film printed using the metal mask shown in Fig. 7(A). The metal mask 58 shown in Fig. 7(A) has openings 59 corresponding to both the first terminal row 51 and the second terminal row 52.

[0048] 7B , when a solder paste film having the same shape as the openings of metal mask 58 is transferred to wiring board 50, solder paste film 60 having the same shape as openings 59 is provided on first terminal row 51 and second terminal row 52 on wiring board 50. In this case, solder particles move between terminal rows during heating, resulting in uneven distribution of the solder particles, which increases the degree of variation in the thickness (height) of the solder between the upper and lower terminals and makes it difficult to obtain high conductivity reliability.

[0049] Fig. 8(A) is a plan view schematically showing an example of a metal mask as a comparative example, and Fig. 8(B) is a plan view schematically showing an example of a solder paste film printed using the metal mask shown in Fig. 8(A). Metal mask 61 shown in Fig. 8(A) has openings 62a, 62b, 62c, and 62d corresponding to the terminals of first terminal row 51, and openings 63a, 63b, 63c, and 63d corresponding to the terminals of second terminal row 52, ​​respectively.

[0050] 8(B), when a solder paste film having the same shape as the openings of the metal mask 61 is transferred to the wiring board 50, solder paste films 64a, 64b, 64c, 64d, 65a, 65b, 65c, and 65d having the same shapes as the openings 62a, 62b, 62c, 62d, 63a, 63b, 63c, and 63d are provided on the wiring board 50 over the terminals 51a, 51b, 51c, and 51d of the first terminal row 51 and the terminals 52a, 52b, 52c, and 52d of the second terminal row 52. In this case, if the openings of the metal mask become smaller due to finer patterning, the solder paste will remain in the openings, and a situation will occur in which the solder paste is not transferred to the wiring board 50, as in the case of the terminal 52b shown in FIG.

[0051] [Connector Mounting Body] The following describes in detail a connector mounting body using a vertical mating type connector as a specific example of a surface-mounted component. The connector is mainly a resin molded product having a mating portion, and may be, for example, a resin molded product with multiple electrodes protruding in the longitudinal direction (a so-called centipede-type connector) or one without protruding electrodes (a flip-chip-type connector).

[0052] Figure 9 is a cross-sectional view showing an example of a plug and receptacle in a vertical mating connector in the short direction. The connector shown in Figure 9 is composed of a receptacle 70 to which receptacle terminals 71A and 71B are fixed with insulating resin, and a plug 80 to which plug terminals 81A and 81B are fixed with insulating resin. Furthermore, receptacle terminals 71A and 71B are formed at a predetermined pitch along the length of receptacle 70, and plug terminals 81A and 81B are formed at a predetermined pitch along the length of plug 80.

[0053] Fig. 10 is a cross-sectional view schematically showing the longitudinal direction of a connection structure in which a connector plug and a wiring board are connected, and Fig. 11 is a cross-sectional view schematically showing the transverse direction of a connection structure in which a connector plug and a wiring board are connected. That is, the longitudinal cross section shown in Fig. 10 is a Y cross section perpendicular to the transverse cross section shown in Fig. 11, and the transverse cross section shown in Fig. 11 is an X cross section perpendicular to the longitudinal cross section shown in Fig. 10.

[0054] As shown in Figures 10 and 11, the connector assembly includes a plug 80 having plug terminals 81A as a first terminal row and plug terminals 81B as a second terminal row, a wiring board 90 having board terminals 91A and 91B corresponding to the plug terminals 81A and 81B, and an adhesive layer 100 that joins the plug terminals 81A and 81B and the board terminals 91A and 91B with solder 101.

[0055] The plug 80 includes plug terminals 81A, 81B, connection pins 82A, 82B formed by bending conductive metal continuous with the plug terminals 81A, 81B, and insulating resin 83 that fixes the plug terminals 81A, 81B and the connection pins 82A, 82B.

[0056] The insulating resin 83 is made of, for example, polyamide or LCP (Liquid Crystal Polymer), and fixes the plug terminals 81A, 81B and the connection pins 82A, 82B by, for example, resin molding. Leads are formed at the ends of the plug terminals 81A, 81B, respectively, and the plug terminals 81A, 81B form a surface-mounted lead array.

[0057] The upper limit of the minimum distance between adjacent terminals (space distance) of plug terminals 81A, 81B and board terminals 91A, 91B is preferably 0.8 mm or less, more preferably 0.3 mm or less, and even more preferably 0.2 mm or less. The lower limit of the minimum distance between adjacent terminals of plug terminals 81A, 81B and board terminals 91A, 91B is preferably 50 μm or more, more preferably 60 μm or more, and even more preferably 70 μm or more. The surfaces of plug terminals 81A, 81B are preferably gold-plated.

[0058] The wiring board 90 has board terminals 91A and 91B on a base material that correspond to the plug terminals 81A and 81B. The wiring board 90 may be any board that can be broadly defined as a so-called printed wiring board (PWB), and may be either a rigid board or a flexible board (FPC: Flexible Printed Circuits). Examples of substrate types include glass boards, ceramic boards, and plastic boards. Furthermore, the surfaces of the board terminals 91A and 91B are preferably gold-plated.

[0059] The adhesive layer 100 includes solder 101 that joins the plug terminals 81A, 81B and the board terminals 91A, 91B, and a cured binder 102. The adhesive layer 80 is formed by curing a solder connection film (described later), joining the plug terminals 81A, 81B and the board terminals 91A, 91B with the solder 81, and by curing the binder of the solder connection film between the plug 80 and the wiring board 90.

[0060] 2. Solder Connection Film The solder connection film according to this embodiment contains a binder, solder particles, and a flux compound. The film shape of the solder connection film not only makes it possible to uniformize the amount of solder particles, but also makes it easy to handle, thereby improving work efficiency.

[0061] The lower limit of the thickness of the solder connection film is preferably 0.6 or more, more preferably 0.8 or more, and even more preferably 0.9 or more, relative to the average particle size of the solder particles. The upper limit of the thickness of the solder connection film is preferably 3.0 or less, more preferably 2.0 or less, and even more preferably 1.5 or less, relative to the average particle size of the solder particles. If the ratio of the average particle size of the solder particles to the thickness of the solder connection film is large, the handling of the solder connection film may become more difficult. Here, the thickness of the solder connection film refers to the thickness of the binder resin layer only, and does not include the particle size.

[0062] The thickness of the solder connection film can be measured using a known micrometer or digital thickness gauge (e.g., Mitutoyo Corporation: MDE-25M, minimum display 0.0001 mm) that can measure to 1 μm or less, preferably 0.1 μm or less. The film thickness can be determined by measuring at 10 or more locations and averaging. However, when the film thickness is thinner than the particle diameter, a contact-type thickness measuring device is not suitable, so it is preferable to use a laser displacement meter (e.g., Keyence Corporation, spectral interference displacement type SI-T series, etc.).

[0063] The binder of the solder connection film may be either thermosetting or thermoplastic, but is preferably thermosetting, which can be melted and hardened by temperature control in a reflow process. The following describes thermosetting binders (insulating binders).

[0064] [Thermosetting Binder] The thermosetting binder preferably has a heat generation peak temperature higher than the melting point of the solder particles, and a minimum melt viscosity temperature lower than the melting point of the solder particles. This allows the thermosetting binder to be melted by heating, the solder particles to aggregate on the terminals, and then the thermosetting binder can be cured. Here, the heat generation peak temperature and the minimum melt viscosity temperature can be measured using, for example, a rotational rheometer (manufactured by Thermo Fisher Scientific) under the following conditions: a measurement pressure of 1 N, a temperature range of 30 to 200°C, a heating rate of 10°C / min, a measurement frequency of 1 Hz, and a measurement plate diameter of 8 mm.

[0065] Examples of thermosetting binders include a thermal radical polymerization resin composition containing a (meth)acrylate compound and a thermal radical polymerization initiator, a thermal cationic polymerization resin composition containing an epoxy compound and a thermal cationic polymerization initiator, and a thermal anionic polymerization resin composition containing an epoxy compound and a thermal anionic polymerization initiator. Also, known pressure-sensitive adhesive compositions may be used. The term "(meth)acrylic monomer" refers to both acrylic monomers and methacrylic monomers.

[0066] In the following, a specific example will be described, taking as an example a thermally polymerizable resin composition containing a solid epoxy resin, a liquid epoxy resin, and an epoxy resin curing agent.

[0067] The solid epoxy resin is not particularly limited as long as it is solid at room temperature and has one or more epoxy groups in its molecule. Examples include bisphenol A epoxy resin and biphenyl epoxy resin. Among these, it is preferable to use a crystalline bisphenol A epoxy resin with a low melt viscosity. A specific example of a commercially available crystalline bisphenol A epoxy resin is Mitsubishi Chemical Corporation's "YL6810" (crystalline BPA epoxy resin), which has a viscosity of 40 to 55 P measured by the Gardner-Holdt method. The solid epoxy resin may also be a phenoxy resin synthesized from bisphenols and epichlorohydrin. An example of a phenoxy resin is "YP-50" manufactured by Nippon Steel Chemical & Material Co., Ltd. This allows the film shape to be maintained. Note that room temperature refers to the range of 20°C ± 15°C (5°C to 35°C) as specified in JIS Z 8703.

[0068] The liquid epoxy resin is not particularly limited as long as it is liquid at room temperature, and may be, for example, a bisphenol A epoxy resin, a bisphenol F epoxy resin, hydrogenated bisphenol A glycidyl ether, or a urethane-modified epoxy resin. An example of a bisphenol F epoxy resin is "YL983U" manufactured by Mitsubishi Chemical Corporation, and an example of a hydrogenated bisphenol A glycidyl ether is "YX8000" manufactured by Mitsubishi Chemical Corporation.

[0069] The amount of liquid epoxy resin blended is preferably 160 parts by mass or less, more preferably 140 parts by mass or less, and even more preferably 120 parts by mass or less, per 100 parts by mass of solid epoxy resin. If the amount of liquid epoxy resin blended is too large, it becomes difficult to maintain the film shape. Furthermore, if the amount of liquid epoxy resin blended is too large, the cured physical properties after thermal curing generally become high elasticity due to a high crosslink density, and therefore the stress relaxation ability decreases.

[0070] The epoxy resin curing agent is not particularly limited as long as it is a heat curing agent that initiates curing by heat, and examples thereof include anionic curing agents such as amines and imidazoles, and cationic curing agents such as sulfonium salts. The curing agent may also be microencapsulated to provide resistance to the solvent used in forming the film. Examples of anionic curing agents include imidazole-based epoxy resin curing agents such as "2P4MHZ-PW" manufactured by Shikoku Chemicals Corporation.

[0071] [Solder Particles] The solder particles can be appropriately selected from, for example, Sn—Pb-based, Pb—Sn—Sb-based, Sn—Sb-based, Sn—Pb—Bi-based, Bi—Sn-based, Sn—Cu-based, Sn—Pb—Cu-based, Sn—In-based, Sn—Ag-based, Sn—Pb—Ag-based, Pb—Ag-based, etc. as specified in JIS Z 3282-1999, depending on the electrode material, connection conditions, etc. Among these, the solder particles are preferably one or more selected from the group consisting of Sn—Bi—Cu alloy, Sn—Bi—Ag alloy, Sn—Bi alloy, Sn—Pb—Bi alloy, and Sn—In alloy. Specific examples of solder particles include Sn59.9Bi40Cu0.1, Sn30Bi0.5Cu, Sn30Bi, Sn40Bi, Sn50Bi, Sn58Bi, Sn40Bi0.1Cu, Sn43Pb14Bi, Sn20In, etc. This makes it possible to obtain excellent connection reliability.

[0072] The lower limit of the melting point of the solder particles is preferably 110°C or higher, more preferably 120°C or higher, and even more preferably 130°C or higher. The upper limit of the melting point of the solder particles may be 250°C or lower, preferably 200°C or lower, more preferably 180°C or lower, and even more preferably 160°C or lower. Furthermore, a flux compound may be directly bonded to the surface of the solder particles for the purpose of activating the surface. Activating the surface can promote metal bonding with the electrode portion.

[0073] The average particle size of the solder particles is preferably 0.5 times or less, more preferably 0.3 times or less, and even more preferably 0.2 times or less, the minimum inter-terminal distance (space distance) between the terminal row of the surface-mounted component and the terminal row of the wiring board. Due to this relationship between the space distance and the average particle size of the solder particles, the terminal row of the surface-mounted component and the terminal row of the wiring board can be joined using a reflow furnace. If the average particle size of the solder particles is greater than 0.5 times the minimum inter-terminal distance between the terminal row of the surface-mounted component and the terminal row of the wiring board, the possibility of a short circuit occurring increases.

[0074] The lower limit of the average particle size of the solder particles is preferably 0.5 μm or more, more preferably 3 μm or more, and even more preferably 5 μm or more, and the upper limit of the average particle size of the solder particles may be 50 μm or less, and is 30 μm or less, preferably 25 μm or less, and even more preferably 20 μm or less. This allows for a good solder joint state and high reliability to be obtained.

[0075] The average particle size is the average value of the major axis diameter of particles measured, for example, at N = 20 or more, preferably N = 50 or more, and more preferably N = 200 or more, in observation images using a metallurgical microscope, optical microscope, or electron microscope such as a scanning electron microscope (SEM). In the case of spherical particles, it is the average value of the particle diameter. Also, the observed image may be measured using known image analysis software (such as "WinROOF" from Mitani Shoji Co., Ltd. or "Azo-kun (registered trademark)" from Asahi Kasei Engineering Co., Ltd.), or may be measured (N = 1000 or more) using an image-type particle size distribution analyzer (e.g., FPIA-3000 (Malvern Instruments)). The average particle size determined from the observed image or image-type particle size distribution analyzer can be the average value of the maximum length of the particles. When preparing a solder connection film, manufacturer values ​​such as the particle size (D50) at which the cumulative frequency in the particle size distribution determined by a simple laser diffraction / scattering method reaches 50%, or the arithmetic mean diameter (preferably on a volume basis) may be used.

[0076] The solder particles are preferably dispersed in a binder, and may be arranged randomly or with a certain regularity. The solder particles may also be in the form of aggregates in which a plurality of solder particles are aggregated.

[0077] The content of solder particles in the solder connection film can be determined appropriately based on the pitch of the terminal rows of the surface-mounted components and the wiring board. For example, for a terminal row pitch of 0.1 mm to 0.4 mm for the surface-mounted components and the wiring board, it is preferably 10 to 60% by volume. For example, it is preferably 20 to 58% by volume when the pitch is 0.4 mm, 20 to 58% by volume when the pitch is 0.35 mm, 20 to 48% by volume when the pitch is 0.2 mm, 15 to 48% by volume when the pitch is 0.15 mm, and 10 to 38% by volume when the pitch is 0.1 mm. If the solder particle content is too low, excellent conductivity, heat dissipation, and adhesion cannot be obtained, while if the content is too high, anisotropy is easily impaired, making it difficult to obtain excellent conductivity reliability.

[0078] [Flux Compound] The flux compound removes foreign matter and oxide film from the electrode surface, prevents oxidation of the electrode surface, and reduces the surface tension of the molten solder. Examples of the flux compound include carboxylic acids such as levulinic acid, maleic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, and sebacic acid. Among these, glutaric acid is preferably used because it is excellent at removing oxide film.

[0079] [Other Additives] In addition to the binder, solder particles, and flux compound described above, various additives conventionally used as adhesives can be blended into the solder connection film as long as they do not impair the effects of the present technology. The particle size of the additive is preferably smaller than the average particle size of the solder particles, but is not particularly limited as long as it does not inhibit inter-electrode bonding.

[0080] The solder connection film can be obtained, for example, by mixing an insulating binder, solder particles, and a flux compound in a solvent, applying the mixture to a release-treated film to a predetermined thickness using a bar coater, and then drying to volatilize the solvent. Alternatively, the mixture may be applied to a release-treated film using a bar coater and then pressurized to a predetermined thickness. To improve the dispersibility of the solder particles, it is preferable to apply a high shear force while the film contains the solvent. For example, a known batch-type planetary stirring device can be used. The residual solvent content of the solder connection film is preferably 2% or less, more preferably 1% or less.

[0081] The solder connection film according to the present embodiment appropriately suppresses the removal of oxide film by the flux compound, making it easier for the solder to remain in an appropriate range, thereby making it possible to maintain the remaining solder area in an appropriate range. Furthermore, by maintaining the remaining solder area in an appropriate range, moisture resistance and mechanical strength are improved, and a decrease in joint strength and an increase in resistance value can be suppressed.

[0082] 3. First Example In the first example, an anisotropic conductive film containing solder particles was produced as a form of solder connection film. Then, a connector was mounted on a substrate having a first terminal row and a second terminal row using the anisotropic conductive film, and the connection structure after reflow was evaluated for bridge formation, conduction resistance, solder residue, and solder height.

[0083] [Preparation of Anisotropic Conductive Film] A binder was prepared by blending 45 parts by mass of phenoxy resin (YP-50, Nippon Steel Chemical & Material Co., Ltd.), 10 parts by mass of hydrogenated bisphenol A glycidyl ether (YX8000, Mitsubishi Chemical Corporation), 45 parts by mass of crystalline bisphenol A epoxy resin (YL6810, Mitsubishi Chemical Corporation), 10 parts by mass of imidazole-based epoxy resin curing agent (2P4MHZ-PW (2-phenyl-4-methyl-5-hydroxymethylimidazole), Shikoku Chemical Industry Co., Ltd.), and 8 parts by mass of glutaric acid (1,3-propanedicarboxylic acid, Tokyo Chemical Industry Co., Ltd.). A predetermined amount of solder particles (Sn59.9Bi40Cu0.1) with an average particle size of 20 μm was blended with 118 parts by mass of the binder to prepare an anisotropic conductive film of a predetermined thickness.

[0084] [Fabrication of Connection Structure] A printed wiring board (having a first terminal row and a second terminal row, with a distance of 0.8 mm between the first terminal row and the second terminal row, the first terminal row and the second terminal row having a 0.35 mm pitch (line / space = 0.18 / 0.17 mm, terminal length 0.8 mm), a glass epoxy substrate thickness of 1.5 mm, a copper pattern thickness of 18 μm, and a surface OSP treatment) was prepared as a substrate.

[0085] The connectors used were a plug connector (Hirose BM23FR0.6-20DP, 10 pins on one side (20 pins on both sides), 0.35 mm lead, line / space = 0.12 / 0.23 mm, Au-plated terminal surface) and a receptacle connector (Hirose BM23FR0.6-20DS, 10 pins on one side (20 pins on both sides), 0.35 mm lead, line / space = 0.12 / 0.23 mm, Au-plated terminal surface).

[0086] An anisotropic conductive film was cut to a predetermined size and temporarily pressure-bonded to the terminals of the substrate at 45°C, 1 MPa, and 1 second, temporarily attaching the anisotropic conductive film to the terminals of the substrate. Next, connectors (plug connector and receptacle connector) were placed on the anisotropic conductive film, and reflow was performed under the following reflow conditions to produce a connection structure. Reflow conditions: 150°C to 260°C - 100 seconds, peak top set at 260°C

[0087] [Evaluation of Bridge Occurrence] After reflow, the connection structure was measured for its insulation resistance when a voltage of 20 V was applied between adjacent terminals using a digital multimeter. 6 Ω or less was counted as the occurrence of solder bridging.

[0088] [Evaluation of Conduction Resistance] The connection structure after reflow was measured for its conduction resistance value when DC 10 mA was applied using a four-terminal method with a digital multimeter, and the connection structure was evaluated based on the maximum resistance value. The evaluation criteria for A to C were as follows: A: Maximum resistance value is 50 mΩ or less B: Maximum resistance value is more than 50 mΩ but not more than 90 mΩ C: Maximum resistance value is more than 90 mΩ

[0089] [Evaluation of Solder Remainings] After reflow, the connection structure was X-rayed using an X-ray imaging device to determine whether or not there was solder remaining outside the terminals.

[0090] [Evaluation of Solder Height] For the connection structure after reflow, the cross section between the terminal of the first electronic component and the pin of the second component was observed with an electron microscope, the solder height (thickness) was measured, and the average value, standard deviation σ, and relative standard deviation (RSD) were calculated.

[0091] Example 1 118 parts by mass of binder and 460 parts by mass of solder particles were mixed to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 0.8 mm.

[0092] Fig. 12(A) is a photograph showing the state in which an anisotropic conductive film is temporarily attached to a printed wiring board for Example 1, Fig. 12(B) is a photograph showing the state in which a connector is mounted on a printed circuit board for Example 1, and Fig. 12(C) is an X-ray photograph showing the connection structure after reflow for Example 1. Anisotropic conductive films with a width of 0.8 mm were temporarily attached to each of the first terminal row and the second terminal row, and a gap of 0.8 mm wide was provided between the first terminal row and the second terminal row, and the connector was mounted.

[0093] As shown in Table 1, the connection structure of Example 1 did not experience any bridges, the conduction resistance was evaluated as A, and there was no residual solder as shown in the X-ray photograph of Fig. 12(C). The average solder height was 51 µm, the standard deviation was 6 µm, and the relative standard deviation was 12%.

[0094] Example 2 A connection structure was produced in the same manner as in Example 1, except that 690 parts by mass of solder particles were blended with 118 parts by mass of binder to produce an anisotropic conductive film with a thickness of 40 μm. As shown in Table 1, the connection structure of Example 2 did not exhibit any bridge formation, was rated A for conduction resistance, and had no residual solder. The average solder height was 60 μm, the standard deviation was 7 μm, and the relative standard deviation was 12%.

[0095] Example 3 A connection structure was produced in the same manner as in Example 1, except that 1,040 parts by mass of solder particles were blended with 118 parts by mass of binder to produce an anisotropic conductive film having a thickness of 40 μm. As shown in Table 1, the connection structure of Example 3 showed no bridge formation, an evaluation of conduction resistance of A, and no residual solder. The average solder height was 71 μm, the standard deviation was 8 μm, and the relative standard deviation was 11%.

[0096] Comparative Example 1 118 parts by mass of binder and 300 parts by mass of solder particles were mixed to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 2.4 mm.

[0097] Fig. 13(A) is a photograph showing the state in which an anisotropic conductive film is temporarily attached to a printed wiring board for Comparative Example 1, Fig. 13(B) is a photograph showing the state in which a connector is mounted on a printed circuit board for Comparative Example 1, and Fig. 13(C) is an X-ray photograph showing the connection structure after reflow for Comparative Example 1. An anisotropic conductive film with a width of 2.4 mm was temporarily attached to the entire surface including the first terminal row and the second terminal row, and the connector was mounted.

[0098] As shown in Table 1, the connection structure of Comparative Example 1 did not experience any bridges, was rated B for conduction resistance, and had residual solder as shown in the X-ray photograph of Fig. 13(C). The average solder height was 48 µm, the standard deviation was 17 µm, and the relative standard deviation was 35%.

[0099] Comparative Example 2 A connection structure was produced in the same manner as in Comparative Example 1, except that 460 parts by mass of solder particles were blended with 118 parts by mass of binder to produce an anisotropic conductive film with a thickness of 40 μm. As shown in Table 1, the connection structure of Comparative Example 2 had bridges (3ch), was rated C for conduction resistance, and had residual solder. The average solder height was 74 μm, the standard deviation was 21 μm, and the relative standard deviation was 28%.

[0100] Comparative Example 3 A connection structure was produced in the same manner as in Comparative Example 1, except that 460 parts by mass of solder particles were blended with 118 parts by mass of binder to produce an anisotropic conductive film having a thickness of 30 μm. As shown in Table 1, the connection structure of Comparative Example 3 showed no bridge formation, was rated B for conduction resistance, and had residual solder. The average solder height was 59 μm, the standard deviation was 23 μm, and the relative standard deviation was 39%.

[0101] Comparative Example 4 A connection structure was produced in the same manner as in Comparative Example 1, except that 690 parts by mass of solder particles were blended with 118 parts by mass of binder to produce an anisotropic conductive film with a thickness of 40 μm. As shown in Table 1, the connection structure of Comparative Example 4 had bridges (2ch), was rated C for conduction resistance, and had residual solder. The average solder height was 87 μm, the standard deviation was 25 μm, and the relative standard deviation was 29%.

[0102]

[0103] In Comparative Examples 1 to 4, an anisotropic conductive film was temporarily attached to the entire surface including the first and second terminal rows, which resulted in residual solder between the first and second terminal rows and high standard deviations and relative standard deviations of the solder height. This is thought to be because solder particles moved between the first and second terminal rows, making the solder particles less efficiently aggregated on the terminals.

[0104] On the other hand, in Examples 1 to 3, anisotropic conductive films were temporarily attached to the first and second terminal rows, respectively, so no solder remained between the first and second terminal rows, and the standard deviation and relative standard deviation of the solder height were low. This is thought to be because the solder particles did not move between the first and second terminal rows, and the solder particles efficiently aggregated on the terminals.

[0105] 4. Second Example In the second example, an anisotropic conductive film was temporarily attached to a substrate having a first terminal row and a second terminal row, and reflow was performed, and the occurrence of bridging and solder height were evaluated.

[0106] A printed wiring board (having a first terminal row and a second terminal row, with a distance of 0.8 mm between the first terminal row and the second terminal row, the first terminal row and the second terminal row having a 0.35 mm pitch (line / space = 0.18 / 0.17 mm, terminal length 0.8 mm), a glass epoxy substrate thickness of 1.5 mm, a copper pattern thickness of 18 μm, and a surface OSP treatment) was prepared as the substrate.

[0107] The anisotropic conductive film was cut to a predetermined size and temporarily pressed onto the terminals of the substrate at 45°C, 1 MPa, and 1 second. The anisotropic conductive film was then temporarily attached to the terminals of the substrate, and reflow was performed under the following reflow conditions to produce a sample. Reflow conditions: 150°C to 260°C for 100 seconds, peak top set at 260°C.

[0108] [Evaluation of Bridge Occurrence] After reflow, the insulation resistance of the sample was measured when a voltage of 20 V was applied between adjacent terminals using a digital multimeter. 6 A resistance of Ω or less was counted as the occurrence of solder bridging, and the case where no bridging occurred was evaluated as "OK", and the case where bridging occurred was evaluated as "NG".

[0109] [Evaluation of Solder Height] The solder height (thickness) on the wiring of the sample after reflow was measured using a 3D measuring laser microscope (Olympus Corporation, LEXT OLS5000), and the average value, standard deviation σ, and relative standard deviation (RSD) were calculated.

[0110] [Preparation of Anisotropic Conductive Film] A binder was prepared by blending 45 parts by mass of phenoxy resin (YP-50, Nippon Steel Chemical & Material Co., Ltd.), 10 parts by mass of hydrogenated bisphenol A glycidyl ether (YX8000, Mitsubishi Chemical Corporation), 45 parts by mass of crystalline bisphenol A epoxy resin (YL6810, Mitsubishi Chemical Corporation), 10 parts by mass of imidazole-based epoxy resin curing agent (2P4MHZ-PW (2-phenyl-4-methyl-5-hydroxymethylimidazole), Shikoku Chemical Industry Co., Ltd.), and 8 parts by mass of glutaric acid (1,3-propanedicarboxylic acid, Tokyo Chemical Industry Co., Ltd.). A predetermined amount of solder particles (Sn59.9Bi40Cu0.1) with an average particle size of 20 μm was blended with 118 parts by mass of the binder to prepare an anisotropic conductive film of a predetermined thickness.

[0111] Example 4: 118 parts by weight of binder and 460 parts by weight of solder particles were mixed to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 1.2 mm. Anisotropic conductive films each having a width of 1.2 mm were temporarily attached to the first and second terminal rows, respectively, and a gap of 0 mm was provided between the first and second terminal rows. As shown in Table 2, the sample of Example 4 was evaluated as having a good bridge formation rate, with an average solder height of 58.8 μm, a standard deviation of 8.4 μm, and a relative standard deviation of 14%.

[0112] Example 5: 118 parts by weight of binder and 460 parts by weight of solder particles were mixed to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 1.0 mm. Anisotropic conductive films each having a width of 1.0 mm were temporarily attached to the first and second terminal rows, respectively, and a gap of 0.4 mm was provided between the first and second terminal rows. As shown in Table 2, the sample of Example 5 was evaluated for bridge formation as OK, with an average solder height of 56.8 μm, a standard deviation of 5.8 μm, and a relative standard deviation of 10%.

[0113] Example 6: 118 parts by weight of binder and 460 parts by weight of solder particles were mixed to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 0.8 mm. Anisotropic conductive films each having a width of 0.8 mm were temporarily attached to the first and second terminal rows, respectively, and a gap of 0.8 mm was provided between the first and second terminal rows. As shown in Table 2, the sample of Example 6 was evaluated for bridge formation as OK, with an average solder height of 44.3 μm, a standard deviation of 5.3 μm, and a relative standard deviation of 14%.

[0114] Example 7: 118 parts by weight of binder and 460 parts by weight of solder particles were mixed to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 0.6 mm. Anisotropic conductive films each having a width of 0.6 mm were temporarily attached to the first and second terminal rows, respectively, and a gap of 1.2 mm was provided between the first and second terminal rows. As shown in Table 2, the sample of Example 7 was evaluated as having a good bridge formation rate, with an average solder height of 42.8 μm, a standard deviation of 3.8 μm, and a relative standard deviation of 9%.

[0115] Example 8: 118 parts by weight of binder and 460 parts by weight of solder particles were mixed to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 0.4 mm. Anisotropic conductive films each having a width of 0.4 mm were temporarily attached to the first and second terminal rows, respectively, and a gap of 1.6 mm was provided between the first and second terminal rows. As shown in Table 2, the sample of Example 8 was evaluated for bridge formation as OK, with an average solder height of 42.2 μm, a standard deviation of 8.5 μm, and a relative standard deviation of 20%.

[0116] Comparative Example 5: 118 parts by weight of binder was mixed with 460 parts by weight of solder particles to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 2.4 mm. An anisotropic conductive film having a width of 2.4 mm was temporarily attached to the entire surface including the first terminal row and the second terminal row. As shown in Table 2, the sample of Comparative Example 5 was evaluated as NG for bridge formation, and the average solder height was 57.0 μm, the standard deviation was 14.0 μm, and the relative standard deviation was 25%.

[0117]

[0118] In Comparative Example 5, an anisotropic conductive film was temporarily attached to the entire surface including the first and second terminal rows, which resulted in bridging and a high standard deviation and relative standard deviation of the solder height. This is thought to be because solder particles moved between the first and second terminal rows, making the solder particles less efficiently aggregated on the terminals.

[0119] On the other hand, in Examples 4 to 8, anisotropic conductive films were temporarily attached to the first and second terminal rows, respectively, so bridges did not occur and the standard deviation and relative standard deviation of the solder height were low. Furthermore, in Examples 5 to 7, the protrusion amount of the rectangular portions in the width direction of the first and second anisotropic conductive films, respectively, between the first and second terminal rows, was 25% or less, which further reduced the standard deviation and relative standard deviation of the solder height. This is thought to be due to efficient aggregation of solder particles onto the terminals.

[0120] Example 9: 118 parts by weight of binder and 690 parts by weight of solder particles were mixed to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 1.2 mm. Anisotropic conductive films each having a width of 1.2 mm were temporarily attached to the first and second terminal rows, respectively, and a gap of 0 mm was provided between the first and second terminal rows. As shown in Table 3, the sample of Example 9 was evaluated for bridge formation as OK, with an average solder height of 67.5 μm, a standard deviation of 9.7 μm, and a relative standard deviation of 14%.

[0121] Example 10: 118 parts by weight of binder and 690 parts by weight of solder particles were mixed to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 1.0 mm. Anisotropic conductive films each having a width of 1.0 mm were temporarily attached to the first and second terminal rows, respectively, and a gap of 0.4 mm was provided between the first and second terminal rows. As shown in Table 3, the sample of Example 10 was evaluated as having a good bridge formation rate, with an average solder height of 66.0 μm, a standard deviation of 7.9 μm, and a relative standard deviation of 12%.

[0122] Example 11: 118 parts by weight of binder and 690 parts by weight of solder particles were mixed to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 0.8 mm. Anisotropic conductive films each having a width of 0.8 mm were temporarily attached to the first and second terminal rows, respectively, and a gap of 0.8 mm was provided between the first and second terminal rows. As shown in Table 3, the sample of Example 11 was evaluated for bridge formation as OK, with an average solder height of 50.5 μm, a standard deviation of 6.4 μm, and a relative standard deviation of 13%.

[0123] Example 12: 118 parts by weight of binder and 690 parts by weight of solder particles were mixed to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 0.6 mm. Anisotropic conductive films each having a width of 0.6 mm were temporarily attached to the first and second terminal rows, respectively, and a gap of 1.2 mm was provided between the first and second terminal rows. As shown in Table 3, the sample of Example 12 was evaluated for bridge formation as OK, with an average solder height of 48.4 μm, a standard deviation of 4.7 μm, and a relative standard deviation of 10%.

[0124] Example 13: 118 parts by weight of binder and 690 parts by weight of solder particles were blended to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 0.4 mm. Anisotropic conductive films each having a width of 0.4 mm were temporarily attached to the first and second terminal rows, respectively, and a gap of 1.6 mm was provided between the first and second terminal rows. As shown in Table 3, the sample of Example 13 was evaluated for bridge formation as OK, with an average solder height of 49.0 μm, a standard deviation of 8.1 μm, and a relative standard deviation of 17%.

[0125] Figure 14 is a photograph showing a sample after reflow for Example 13. From the photograph in Figure 14, it can be seen that there is no residual solder in the gap and a solder joint without bridging has been formed. It can also be seen that a solder joint has been formed in a part of the terminal to which the anisotropic conductive film is attached.

[0126] Comparative Example 6: 118 parts by weight of binder and 690 parts by weight of solder particles were mixed to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 2.4 mm. An anisotropic conductive film having a width of 2.4 mm was temporarily attached to the entire surface including the first terminal row and the second terminal row. As shown in Table 3, the sample of Comparative Example 6 was evaluated as NG for bridge formation, and the average solder height was 88.2 μm, the standard deviation was 28.5 μm, and the relative standard deviation was 32%.

[0127] Fig. 15 is a photograph showing a sample after reflow for Comparative Example 6. From the photograph shown in Fig. 15, it can be seen that solder joints with bridges have been formed. It can also be seen that solder joints have been formed on all of the terminals to which the anisotropic conductive film was attached.

[0128]

[0129] In Comparative Example 6, an anisotropic conductive film was temporarily attached to the entire surface including the first and second terminal rows, which resulted in bridging and a high standard deviation and relative standard deviation of the solder height. This is thought to be because solder particles moved between the first and second terminal rows, making the solder particles less efficiently aggregated on the terminals.

[0130] On the other hand, in Examples 9 to 13, anisotropic conductive films were temporarily attached to the first and second terminal rows, respectively, so bridges did not occur and the standard deviation and relative standard deviation of the solder height were low. Furthermore, in Examples 10 to 21, the protrusion amount of the rectangular portions in the width direction of the first and second anisotropic conductive films, respectively, between the first and second terminal rows, was 25% or less, which further reduced the standard deviation and relative standard deviation of the solder height. This is thought to be due to efficient aggregation of solder particles onto the terminals.

[0131] 5. Third Example In the third example, an anisotropic conductive film was temporarily attached to a substrate having first to fourth terminal rows, and reflow was performed, and the occurrence of bridging and solder height were evaluated.

[0132] A printed wiring board (first to fourth terminal rows are arranged in a rectangular shape and wired on the outside, with no terminals inside the rectangle, first to fourth terminal rows each having a 0.2 mm pitch (line / space = 0.1 / 0.1 mm, terminal length 0.6 mm), 40 pins (8 mm), glass epoxy substrate thickness 1.5 mm, copper pattern thickness 18 μm, surface OSP treatment) was prepared as the substrate.

[0133] The anisotropic conductive film was cut to a predetermined size and temporarily pressed onto the terminals of the substrate at 45°C, 1 MPa, and 1 second. The anisotropic conductive film was then temporarily attached to the terminals of the substrate, and reflow was performed under the following reflow conditions to produce a sample. Reflow conditions: 150°C to 260°C for 100 seconds, peak top set at 260°C.

[0134] [Evaluation of Bridge Occurrence] After reflow, the insulation resistance of the sample was measured when a voltage of 20 V was applied between adjacent terminals using a digital multimeter. 6 A resistance of Ω or less was counted as the occurrence of solder bridging, and the case where no bridging occurred was evaluated as "OK", and the case where bridging occurred was evaluated as "NG".

[0135] [Evaluation of Solder Height] The solder height (thickness) on the wiring of the sample after reflow was measured using a 3D measuring laser microscope (Olympus Corporation, LEXT OLS5000), and the average value, standard deviation σ, and relative standard deviation (RSD) were calculated.

[0136] [Preparation of Anisotropic Conductive Film] A binder was prepared by blending 45 parts by mass of phenoxy resin (YP-50, Nippon Steel Chemical & Material Co., Ltd.), 10 parts by mass of hydrogenated bisphenol A glycidyl ether (YX8000, Mitsubishi Chemical Corporation), 45 parts by mass of crystalline bisphenol A epoxy resin (YL6810, Mitsubishi Chemical Corporation), 10 parts by mass of imidazole-based epoxy resin curing agent (2P4MHZ-PW (2-phenyl-4-methyl-5-hydroxymethylimidazole), Shikoku Chemical Industry Co., Ltd.), and 8 parts by mass of glutaric acid (1,3-propanedicarboxylic acid, Tokyo Chemical Industry Co., Ltd.). A predetermined amount of solder particles (Sn59.9Bi40Cu0.1) with an average particle size of 20 μm was blended with 118 parts by mass of the binder to prepare an anisotropic conductive film of a predetermined thickness.

[0137] Example 14: 204 parts by mass of solder particles were blended with 118 parts by mass of binder to produce an anisotropic conductive film with a thickness of 40 μm, which was then cut to a width of 0.6 mm and a length of 8 mm. Anisotropic conductive films with a width of 0.6 mm were temporarily attached to the first to fourth terminal rows, respectively. As shown in Table 4, the sample of Example 14 was evaluated as having a good bridge formation rate, with an average solder height of 24.5 μm, a standard deviation of 4.0 μm, and a relative standard deviation of 17%.

[0138] Comparative Example 7: 204 parts by mass of solder particles were blended with 118 parts by mass of binder to produce an anisotropic conductive film with a thickness of 40 μm, which was then cut to a width of 9.2 mm and a length of 9.2 mm. A 9.2 mm x 9.2 mm anisotropic conductive film was temporarily attached to the entire surface, including the first to fourth terminal rows. As shown in Table 4, the sample of Comparative Example 7 was evaluated as NG for bridge formation, and the average solder height was 17.7 μm, the standard deviation was 6.0 μm, and the relative standard deviation was 34%.

[0139] Example 15: 225 parts by mass of solder particles were mixed with 118 parts by mass of binder to produce an anisotropic conductive film with a thickness of 40 μm, which was then cut to a width of 0.6 mm and a length of 8 mm. Anisotropic conductive films with a width of 0.6 mm were temporarily attached to the first to fourth terminal rows, respectively. As shown in Table 4, the sample of Example 15 was evaluated as having a good bridge formation rate, with an average solder height of 26.3 μm, a standard deviation of 4.4 μm, and a relative standard deviation of 17%.

[0140] Fig. 16 is an X-ray photograph showing the sample after reflow for Example 15. From the photograph shown in Fig. 16, it can be seen that there is no residual solder in the void portion and a solder joint without bridging has been formed.

[0141] Comparative Example 8: 225 parts by mass of solder particles were mixed with 118 parts by mass of binder to prepare an anisotropic conductive film with a thickness of 40 μm, which was then cut to a width of 9.2 mm and a length of 9.2 mm. A 9.2 mm x 9.2 mm anisotropic conductive film was temporarily attached to the entire surface, including the first to fourth terminal rows. As shown in Table 4, the sample of Comparative Example 8 was evaluated as NG for bridge formation, and the average solder height was 28.1 μm, the standard deviation was 16.1 μm, and the relative standard deviation was 57%.

[0142] Fig. 17 is an X-ray photograph showing the sample after reflow for Comparative Example 8. From the photograph shown in Fig. 17, it can be seen that there is residual solder in the void portion and that a solder joint with bridge formation has been formed.

[0143]

[0144] In Comparative Examples 7 and 8, an anisotropic conductive film was temporarily attached to the entire surface including the first to fourth terminal rows, which resulted in bridging and high standard deviations and relative standard deviations of the solder height. This is thought to be because solder particles moved between the first and second terminal rows, making the agglomeration of the solder particles to the terminals inefficient.

[0145] On the other hand, in Examples 14 and 15, anisotropic conductive films were temporarily attached to the first to fourth terminal rows, respectively, so no bridging occurred and the standard deviation and relative standard deviation of the solder height were low.

[0146] 6. Fourth Example In the fourth example, a connection structure was produced using an anisotropic conductive film of a predetermined shape, and solder residue, where solder particles existed outside the terminal portion, was observed and evaluated using X-ray photography.

[0147] [Preparation of Anisotropic Conductive Film] A binder was prepared by blending 45 parts by mass of phenoxy resin (YP-50, Nippon Steel Chemical & Material Co., Ltd.), 10 parts by mass of hydrogenated bisphenol A glycidyl ether (YX8000, Mitsubishi Chemical Corporation), 45 parts by mass of crystalline bisphenol A epoxy resin (YL6810, Mitsubishi Chemical Corporation), 10 parts by mass of an imidazole-based epoxy resin curing agent (2P4MHZ-PW (2-phenyl-4-methyl-5-hydroxymethylimidazole), Shikoku Chemical Industry Co., Ltd.), and 8 parts by mass of glutaric acid (1,3-propanedicarboxylic acid, Tokyo Chemical Industry Co., Ltd.). 300 parts by mass of solder particles (Sn59.9Bi40Cu0.1) having an average particle size of 20 μm was mixed with 118 parts by mass of binder (28 Vol %) to prepare an anisotropic conductive film having a thickness of 30 μm.

[0148] [Fabrication of Connection Structure] (Plug Connector Structure) A wiring board for a plug connector (having a first terminal row and a second terminal row formed in parallel, with a pair of electrodes formed at both ends of the first and second terminal rows at a distance smaller than the distance between the first and second terminal rows, the distance between the first and second terminal rows being 0.8 mm, the first and second terminal rows having a 0.35 mm pitch (line / space = 0.18 / 0.17 mm, terminal length 0.8 mm), a glass epoxy substrate thickness of 1.5 mm, a copper pattern thickness of 18 μm, and a surface OSP treatment) was prepared as a substrate.

[0149] As the connector, a plug connector (terminal row 10 pins on one side (20 pins on both sides), 0.35 mm P, line / space = 0.12 / 0.23 mm, 2 pins + 1 pin on both ends on one side, terminal surface Au plated) was prepared.

[0150] (Receptacle Connector Structure) A wiring board for a receptacle connector (first and second terminal rows formed in parallel, with electrodes formed at both ends of the first and second terminal rows spanning the space between the first and second terminal rows, the spacing between the first and second terminal rows being 0.8 mm, the first and second terminal rows having a 0.35 mm pitch (line / space = 0.18 / 0.17 mm, terminal length 0.8 mm), a glass epoxy substrate thickness of 1.5 mm, a copper pattern thickness of 18 μm, and a surface OSP treatment) was prepared as the substrate.

[0151] As the connector, a receptacle connector (10 pins on one side (20 pins on both sides), 0.35 mm P, line / space = 0.12 / 0.23 mm, 2 pins on both ends of one side + 1 pin, terminal surface Au plated) was prepared.

[0152] An anisotropic conductive film was cut to a predetermined shape and temporarily attached to the terminals of the substrate by temporary pressure bonding at 45°C, 1 MPa, and 1 second. Subsequently, a connector (plug connector or receptacle connector) was placed on the anisotropic conductive film of the predetermined shape, and reflow was performed under the following reflow conditions to produce a connection structure.

[0153] Reflow conditions: 150°C to 250°C for 100 seconds, peak top set at 250°C, temperature rise rate 3.0°C / second

[0154] Figure 18(A1) is a photograph showing the state in which an anisotropic conductive film of a predetermined shape has been temporarily attached to a wiring board for a plug connector as Comparative Example 9, Figure 18(A2) is a plan view schematically showing the shape of the anisotropic conductive film, Figure 18(B) is a photograph showing the state in which a plug connector has been reflow-mounted on a wiring board for a plug connector, and Figure 18(C) is an X-ray photograph showing the plug connector structure after mounting.

[0155] 18(A1) to 18(C), in Comparative Example 9, a rectangular anisotropic conductive film was temporarily attached to the entire surface including the first terminal row, the second terminal row, and the pair of electrodes at both ends, and then the plug connector was mounted. As shown in Fig. 18(A1) and Fig. 18(A2), an anisotropic conductive film with no gap between the first terminal row and the second terminal row was used. As a result, in the X-ray photograph shown in Fig. 18(C), residual solder was observed between the first terminal row and the second terminal row, and also, a solder joint with a bridge larger than the terminal width was observed.

[0156] Figure 19 (A1) is a photograph showing the state in which an anisotropic conductive film of a predetermined shape has been temporarily attached to a wiring board for a plug connector as Example 16, Figure 19 (A2) is a plan view schematically showing the shape of the anisotropic conductive film, Figure 19 (B) is a photograph showing the state in which a plug connector has been reflow-mounted on a wiring board for a plug connector, and Figure 19 (C) is an X-ray photograph showing the plug connector structure after mounting.

[0157] As shown in Figures 19(A1) to 19(C), in Example 16, an anisotropic conductive film having a substantially rectangular first shape portion 161 corresponding to the first terminal row, a substantially rectangular second shape portion 162 corresponding to the second terminal row, a third shape portion 163 connecting one end of the first shape portion with one end of the second shape portion 162 and bonding one longitudinal end of the plug connector, and a fourth shape portion 164 connecting the other end of the first shape portion with the other end of the second shape portion and bonding the other longitudinal end of the plug connector was temporarily attached, and the plug connector was mounted.

[0158] As shown in Figures 19(A1) and 19(A2), when an anisotropic conductive film having a gap between the first terminal row and the second terminal row was used, the amount of solder residue was dramatically improved compared to Comparative Example 9, and almost no solder residue was observed in the X-ray photograph shown in Figure 19(C).

[0159] Figure 20 (A1) is a photograph showing the state in which an anisotropic conductive film of a predetermined shape has been temporarily attached to a wiring board for a plug connector as Example 17, Figure 20 (A2) is a plan view schematically showing the shape of the anisotropic conductive film, Figure 20 (B) is a photograph showing the state in which a plug connector has been reflow-mounted on a wiring board for a plug connector, and Figure 20 (C) is an X-ray photograph showing the plug connector structure after mounting.

[0160] As shown in Figures 20(A1) to 20(C), in Example 17, a first anisotropic conductive film was temporarily attached, the first anisotropic conductive film having a substantially rectangular first shape portion 171 corresponding to the first terminal row, a second shape portion 172 that is continuous with one longitudinal end of the first shape portion 171 and to which one longitudinal end of the plug connector is bonded, and a third shape portion 173 that is continuous with the other longitudinal end of the first shape portion 171 and to which the other longitudinal end of the plug connector is bonded. Also, a second anisotropic conductive film was temporarily attached, the second anisotropic conductive film having a substantially rectangular fourth shape portion 174 corresponding to the second terminal row, a fifth shape portion 175 that is continuous with one longitudinal end of the fourth shape portion 174 and to which one longitudinal end of the plug connector is bonded, and a sixth shape portion 176 that is continuous with the other longitudinal end of the fourth shape portion 174 and to which the other longitudinal end of the plug connector is bonded, and the plug connector was mounted. When the first anisotropic conductive film and the second anisotropic conductive film are temporarily attached, the distances between the first shape portion 171 to the third shape portion 173 and the distances between the fourth shape portion 174 to the sixth shape portion 176 are approximately the same.

[0161] As shown in Figures 20(A1) and 20(A2), a first anisotropic conductive film and a second anisotropic conductive film were used that were shaped to bond both longitudinal ends of the plug connector, and a gap was provided between the first anisotropic conductive film and the second anisotropic conductive film.As a result, almost no residual solder was observed in the X-ray photograph shown in Figure 20(C), and in particular, the residual solder at both longitudinal ends of the plug connector was improved.

[0162] Figure 21 (A1) is a photograph showing the state in which an anisotropic conductive film of a predetermined shape has been temporarily attached to a wiring board for a plug connector as Example 18, Figure 21 (A2) is a plan view schematically showing the shape of the anisotropic conductive film, Figure 21 (B) is a photograph showing the state in which a plug connector has been reflow-mounted on a wiring board for a plug connector, and Figure 21 (C) is an X-ray photograph showing the plug connector structure after mounting.

[0163] As shown in Figures 21(A1) to 21(C), in Example 18, a first anisotropic conductive film was temporarily attached, the first anisotropic conductive film having a substantially rectangular first shape portion 181 corresponding to the first terminal row, a second shape portion 182 that is continuous with one longitudinal end of the first shape portion 181 and to which one longitudinal end of the plug connector is bonded, and a third shape portion 183 that is continuous with the other longitudinal end of the first shape portion 181 and to which the other longitudinal end of the plug connector is bonded. Also, a second anisotropic conductive film was temporarily attached, the second anisotropic conductive film having a substantially rectangular fourth shape portion 184 corresponding to the second terminal row, a fifth shape portion 185 that is continuous with one longitudinal end of the fourth shape portion 184 and to which one longitudinal end of the plug connector is bonded, and a sixth shape portion 186 that is continuous with the other end of the fourth shape portion 184 and to which the other longitudinal end of the plug connector is bonded, and the plug connector was mounted. When the first anisotropic conductive film and the second anisotropic conductive film are temporarily attached, the distance between the first shape portion 181 and the fourth shape portion 184 is greater than the distance between the second shape portion 182 and the fifth shape portion 185 and the distance between the third shape portion 183 and the sixth shape portion 186.

[0164] As shown in Figures 21 (A1) and 21 (A2), a first anisotropic conductive film and a second anisotropic conductive film shaped to bond both longitudinal ends of the plug connector were used, and the gap distance between the first shape portion 181 and the fourth shape portion 184 was made larger than in Example 17.As a result, almost no residual solder was observed in the X-ray photograph shown in Figure 21 (C), and in particular, the residual solder in the first terminal row and the second terminal row was improved.

[0165] Figure 22 (A1) is a photograph showing a state in which an anisotropic conductive film of a predetermined shape has been temporarily attached to a wiring board for a receptacle connector as comparison example 10, Figure 22 (A2) is a plan view schematically showing the shape of the anisotropic conductive film, Figure 22 (B) is a photograph showing the state in which a receptacle connector has been reflow-mounted on a wiring board for a receptacle connector, and Figure 22 (C) is an X-ray photograph showing the receptacle connector structure after mounting.

[0166] As shown in Figures 22(A1) to 22(C), in Comparative Example 10, a rectangular anisotropic conductive film was temporarily attached to the entire surface of the receptacle connector, including both longitudinal ends, and the receptacle connector was then mounted. As shown in Figures 22(A1) and 22(A2), an anisotropic conductive film with no gap between the first and second terminal rows was used. As a result, in the X-ray photograph shown in Figure 22(C), residual solder was observed between the first and second terminal rows, and also, solder joints with bridges larger than the terminal width were observed.

[0167] Figure 23 (A1) is a photograph showing the state in which an anisotropic conductive film of a predetermined shape has been temporarily attached to a wiring board for a receptacle connector as Example 19, Figure 23 (A2) is a plan view schematically showing the shape of the anisotropic conductive film, Figure 23 (B) is a photograph showing the state in which a receptacle connector has been reflow-mounted on a wiring board for a receptacle connector, and Figure 23 (C) is an X-ray photograph showing the receptacle connector structure after mounting.

[0168] As shown in Figures 23(A1) to 23(C), in Example 19, an anisotropic conductive film having a rectangular gap having a width greater than the distance between the first terminal row and the second terminal row and the length of the terminal row portion of the receptacle connector was temporarily attached to the center of a rectangle including both longitudinal ends of the receptacle connector, and the receptacle connector was then mounted.

[0169] As shown in Figures 23(A1) and 23(A2), when an anisotropic conductive film having a gap between the first terminal row and the second terminal row was used, the amount of solder residue was dramatically improved compared to Comparative Example 10, and almost no solder residue was observed in the X-ray photograph shown in Figure 23(C).

[0170] Figure 24 (A1) is a photograph showing the state in which an anisotropic conductive film of a predetermined shape has been temporarily attached to a wiring board for a receptacle connector as Example 20, Figure 24 (A2) is a plan view schematically showing the shape of the anisotropic conductive film, Figure 24 (B) is a photograph showing the state in which a receptacle connector has been reflow-mounted on a wiring board for a receptacle connector, and Figure 24 (C) is an X-ray photograph showing the receptacle connector structure after mounting.

[0171] As shown in FIGS. 24(A1) to 24(C), in Example 20, a first anisotropic conductive filter is provided having a substantially rectangular first shaped portion 201 corresponding to a first terminal row, a second shaped portion 202 that is continuous with one longitudinal end of the first shaped portion 201 and to which one longitudinal end of the receptacle connector is bonded, and a third shaped portion 203 that is continuous with the other longitudinal end of the first shaped portion 201 and to which the other longitudinal end of the receptacle connector is bonded. a second anisotropic conductive film having a substantially rectangular fourth shaped portion 204 corresponding to the second terminal row, a fifth shaped portion 205 continuous with one longitudinal end of the fourth shaped portion 204 and to which one longitudinal end of the receptacle connector is bonded, and a sixth shaped portion 206 continuous with the other longitudinal end of the fourth shaped portion 204 and to which the other longitudinal end of the receptacle connector is bonded, and the receptacle connector is mounted. In a state in which the first anisotropic conductive film and the second anisotropic conductive film are temporarily bonded, the distance between the first shaped portion 201 and the fourth shaped portion 204 is greater than the distance between the second shaped portion 202 and the fifth shaped portion 205 and the distance between the third shaped portion 203 and the sixth shaped portion 206.

[0172] As shown in Figures 24(A1) and 24(A2), a first anisotropic conductive film and a second anisotropic conductive film were used that were shaped to bond both longitudinal ends of the receptacle connector, and a gap was provided between the first anisotropic conductive film and the second anisotropic conductive film.As a result, almost no residual solder was observed in the X-ray photograph shown in Figure 24(C), and in particular, the residual solder at both longitudinal ends of the receptacle connector was improved.

[0173] 10 wiring board, 11 first terminal row, 11a terminal, 12 second terminal row, 12a terminal, 20 solder particle, 21 first solder connection film, 22 second solder connection film, 30 surface mounted component, 31 first terminal row, 32 second terminal row, 40 binder, 41 solder, 50 wiring board, 51 first terminal row, 51a to 51d terminal, 52 second terminal row, 52a to 52d terminal, 53 metal mask, 54 first opening, 55 second opening, 556 first solder paste film, 57 second solder paste film, 58 metal mask, 59 opening, 60 solder paste film, 61 metal mask, 62a to 62d opening, 63a to 63d opening, 64a to 64d Solder paste film, 65a to 65d: solder paste film 70: receptacle, 71A, 71B: receptacle terminal, 80: plug, 81A, 81B: plug terminal, 82A, 82B: connection pin, 83: insulating resin, 90: wiring board, 91A, 91B: board terminal, 100: adhesive layer, 101: solder, 102: binder hardened product

Claims

1. A method for manufacturing a connection structure, comprising: an arrangement step of arranging a surface mount component having a plurality of terminal rows on a wiring board via a film-like solder connection material having rectangular portions corresponding to each of the terminal rows; and a joining step of joining the surface mount component to the wiring board.

2. The method for manufacturing a connection structure according to claim 1, wherein the relative standard deviation of the solder thickness between the terminal of the surface mount component and the terminal of the wiring board after the joining step is less than 25%.

3. A method for manufacturing a connection structure as claimed in claim 1 or 2, wherein the surface mount component comprises a first terminal row and a second terminal row arranged in parallel, and in the arranging step, a first film-like solder connecting material corresponding to the first terminal row and a second film-like solder connecting material corresponding to the second terminal row are arranged, and the distance between the rectangular portion of the first film-like solder connecting material and the rectangular portion of the second film-like solder connecting material is set to 0 mm or more.

4. The method for manufacturing a connection structure according to claim 3, wherein the surface mount component comprises a first terminal row and a second terminal row arranged in parallel, and in the arranging step, the width W of the rectangular portion of the first film-like solder connection material and the width W of the rectangular portion of the second film-like solder connection material satisfy the following formula (1): W≦(2L+S) / 2 (1) In the above formula (1), L is the length of the terminals in the first terminal row and the second terminal row, and S is the distance between the first terminal row and the second terminal row.

5. The method of manufacturing a connection structure according to claim 1 or 2, wherein in the joining step, the surface mount component is joined to the wiring board without load using a reflow furnace.

6. The method for manufacturing a connection structure according to claim 1 or 2, wherein the pitch of the terminal rows of the surface mount components and the wiring board is 0.1 mm to 0.4 mm.

7. A method for manufacturing a connection structure according to claim 1 or 2, wherein the content of solder particles in the film-like solder connection material is 10 volume % to 60 volume % for a terminal row pitch of 0.1 mm to 0.4 mm on the surface mount components and wiring board.

8. A method for manufacturing a connection structure as claimed in claim 1 or 2, wherein the surface mount component comprises a first terminal row and a second terminal row arranged in parallel, and in the arranging step, a first film-like solder connecting material corresponding to the first terminal row and a second film-like solder connecting material corresponding to the second terminal row are arranged, and the amount of protrusion in the width direction of the rectangular portion of the first solder connecting material relative to the first terminal row is 50% or less of the terminal length of the first terminal row, and the amount of protrusion in the width direction of the rectangular portion of the second solder connecting material relative to the second terminal row is 50% or less of the terminal length of the second terminal row.

9. A method for manufacturing a connection structure as claimed in claim 1 or 2, wherein the surface mount component comprises a first terminal row and a second terminal row arranged in parallel, and a third terminal row and a fourth terminal row arranged in parallel and perpendicular to the first terminal row and the second terminal row, and the amount of protrusion in the width direction of the rectangular portion corresponding to the first terminal row, the second terminal row, the third terminal row or the fourth terminal row from the terminal row is 50% or less of the terminal length of the corresponding first terminal row, the second terminal row, the third terminal row or the fourth terminal row.

10. A connection structure comprising: a surface mount component having a plurality of terminal rows; a wiring board; and a cured film of a film-like solder connecting material provided for each of the terminal rows, joining the surface mount component and the wiring board, and having a rectangular portion corresponding to each of the terminal rows.

11. The connection structure according to claim 10, wherein the relative standard deviation of the solder thickness between the terminal of the surface mount component and the terminal of the wiring board is less than 25%.

12. The connection structure according to claim 10 or 11, wherein the pitch of the terminal rows of the surface mount component and the wiring board is 0.1 mm to 0.4 mm.

13. A connection structure as claimed in claim 10 or 11, wherein the surface mount component comprises a first terminal row and a second terminal row arranged in parallel, the amount of protrusion in the width direction of the rectangular portion of the first film-like solder connection material from the first terminal row is 50% or less of the terminal length of the first terminal row, and the amount of protrusion in the width direction of the rectangular portion of the second film-like solder connection material from the second terminal row is 50% or less of the terminal length of the second terminal row.

14. A connection structure as claimed in claim 10 or 11, wherein the surface mount component comprises a first terminal row and a second terminal row arranged in parallel, and a third terminal row and a fourth terminal row arranged in parallel and perpendicular to the first terminal row and the second terminal row, and the amount of protrusion in the width direction of the rectangular portion corresponding to the first terminal row, the second terminal row, the third terminal row or the fourth terminal row from the terminal row is 50% or less of the terminal length of the corresponding first terminal row, the second terminal row, the third terminal row or the fourth terminal row.

Citation Information

Patent Citations

  • Method for producing connecting structure, connecting structure, film structure, and method for producing film structure

    JP2020198422A

  • Manufacturing method of connection body and connection body

    JP2021125692A

  • Method of producing connecting film

    JP2023050162A