Target assembly and method for manufacturing target assembly
By using a metal thin film layer of Ti, V, Cr, Nb, Pd, Ir, or Pt between the target and insert material in a diffusion-bonded assembly, the bonding strength is improved, addressing the issue of intermetallic compound layer formation and ensuring stability during high-power sputtering.
Patent Information
- Application Number
- PCT/JP2024/018568
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-22
- Filing Date
- 2024-05-20
- Publication Date
- 2024-11-28
AI Technical Summary
The formation of a brittle intermetallic compound layer between aluminum or aluminum alloy insert materials and copper alloy backing plates in sputtering targets leads to decreased bonding strength, particularly due to differences in thermal expansion coefficients and varying bonding temperatures, which affects the stability and performance of tungsten or molybdenum targets during high-power sputtering.
A target assembly is created by diffusion bonding a tungsten or molybdenum target with a copper or copper alloy backing plate using an aluminum or aluminum alloy insert material, with a metal thin film layer of Ti, V, Cr, Nb, Pd, Ir, or Pt interposed between the target, insert material, and backing plate to prevent intermetallic compound formation, ensuring sufficient bonding strength through a thickness of 0.1 μm to 3.0 μm.
This approach enhances the bonding strength between the target and insert material, maintaining stability during high-power sputtering and reducing the coefficient of variation in shear strength, ensuring reliable bonding and preventing intermetallic compound layer formation, thus improving the overall performance of the target assembly.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure 00000017_0000
Abstract
Description
Target assembly and method for manufacturing the target assembly
[0001] The present invention relates to a target assembly and a method for manufacturing the target assembly.
[0002] Diffusion bonding is known to be an effective method for joining a sputtering target and a backing plate that can withstand high-power sputtering. In recent years, as wafer diameters have increased, sputtering targets themselves have also become larger, and deformation and peeling after diffusion bonding have become a major problem, especially when there is a large difference in the thermal expansion coefficients of the target material and the backing plate material.
[0003] Meanwhile, in recent years, in the field of semiconductor device manufacturing, tungsten, which has heat resistance and low resistance characteristics, has been widely used as a wiring material or electrode material. However, it has been found that when using a target such as tungsten, deformation after diffusion bonding becomes a major problem.
[0004] Therefore, a tantalum or tungsten target-copper alloy backing plate assembly has been proposed, in which a tantalum or tungsten target and a copper alloy backing plate are diffusion bonded via an insert material of aluminum or aluminum alloy plate having a thickness of 0.8 mm or more, and a diffusion bonded interface is provided between the respective materials (see Patent Document 1).
[0005] Patent No. 3905301
[0006] However, although the technology of Patent Document 1 is considered effective as a countermeasure against warpage, it has been confirmed that an intermetallic compound layer is formed between the aluminum or aluminum alloy insert material and the copper alloy backing plate, and that this intermetallic compound layer is very brittle, and the thicker the intermetallic compound layer, the lower the bonding strength. This poses the problem of requiring bonding at low temperatures. On the other hand, there is a problem that the bonding strength between tungsten and the insert material is insufficient and there is a large variation in bonding strength, which poses the problem of requiring high-temperature bonding.
[0007] In view of the above circumstances, an object of the present invention is to provide a target assembly and a method for manufacturing the target assembly that can suppress the formation of an intermetallic compound layer between an aluminum or aluminum alloy plate insert material and a copper alloy backing plate, thereby preventing a decrease in bonding strength, and can improve the bonding strength between the target and the insert material to a sufficient level.
[0008] To achieve the above object, a first aspect of the present invention is a target assembly in which an insert material of aluminum or aluminum alloy plate is sandwiched between a target made of tungsten or molybdenum and a backing plate made of copper or a copper alloy and diffusion-bonded, wherein the target and the insert material and the backing plate and the insert material are diffusion-bonded via metal thin film layers each having a thickness of more than 0.1 μm and not more than 3.0 μm and made of Ti, V, Cr, Nb, Pd, Ir, Pt or an alloy containing at least one of these metals. A second aspect of the present invention is a target assembly in which the average shear strength across the plane between the target and the insert material and the average shear strength across the plane between the insert material and the backing plate are each 4 [kg / mm 2
[0013] A third aspect of the present invention is directed to the target assembly of the first or second aspect, wherein a coefficient of variation, which is the ratio of the average shear strength across the plane to the standard deviation σ of the shear strength across the plane, is 0.15 or less. A fourth aspect of the present invention is directed to a method for manufacturing a target assembly in which a target made of tungsten or molybdenum is sandwiched between a copper or copper alloy backing plate and an aluminum or aluminum alloy plate insert material and diffusion bonded therebetween, comprising: providing a metal thin film layer having a thickness of more than 0.1 μm and not more than 3.0 μm, the metal thin film layer being made of Ti, V, Cr, Nb, Pd, Ir, Pt, or an alloy containing at least one of these metals, at least one between the target and the insert material and at least one between the backing plate and the insert material; and then performing diffusion bonding to form the target assembly. A fifth aspect of the present invention resides in a method for manufacturing the target assembly of the fourth aspect, in which a metal thin film layer having a thickness of more than 0.1 μm and not more than 3.0 μm and made of Ti, V, Cr, Nb, Pd, Ir, Pt or an alloy containing at least one of these metals is provided between the target and the insert material and between the backing plate and the insert material, and then diffusion bonding is performed.
[0009] In the present invention, a metal thin film layer made of Ti, V, Cr, Nb, Pd, Ir, Pt or an alloy containing at least one of these metals and having a thickness of more than 0.1 μm and not more than 3.0 μm is provided between the target and the insert material, and between the backing plate and the insert material, respectively, for diffusion bonding. This makes it possible to provide a target assembly and a method for manufacturing a target assembly that suppresses the formation of an intermetallic compound layer between the aluminum or aluminum alloy plate insert material and the copper alloy backing plate, thereby preventing a decrease in bonding strength and improving the bonding strength between the target and the insert material to a sufficient level.
[0010] Binary phase diagrams of Al-Ti, Cu-Ti, and Ti-W. Binary phase diagrams of Al-V, Cu-V, and V-W. Binary phase diagrams of Al-Cr, Cr-Cu, and Cr-W. Binary phase diagrams of Al-Fe, Cu-Fe, and Fe-W. Binary phase diagrams of Al-Co, Co-Cu, and Co-W. Binary phase diagrams of Al-Ni, Cu-Ni, and Ni-W. Binary phase diagrams of Al-Nb, Cu-Nb, and Nb-W. Binary phase diagrams of Al-Pd, Cu-Pd, and Pd-W. Binary phase diagrams of Al-Ir, Cu-Ir, and Ir-W. Binary phase diagrams of Al-Pt, Cu-Pt, and Pt-W. Graph showing shear strength for Examples 1-7 and Comparative Examples 1-8. 1 is a graph showing the shear strength of Examples 11-17 and Comparative Examples 11-18. It is a cross-sectional SEM observation image of the interface between the insert material and the backing plate of Example 3. It is a cross-sectional SEM observation image of the interface between the insert material and the backing plate of Comparative Example 2. It is a cross-sectional SEM observation image of the interface between the insert material and the backing plate of Comparative Example 5. It is a cross-sectional SEM observation image of the interface between the target and the insert material of Comparative Example 7.
[0011] The target used in the present invention is a target made of tungsten or molybdenum, and preferably has a purity of 5N (99.999% by mass) or higher, contains impurities of carbon and oxygen in amounts of 30 ppm by mass or less, has a relative density of 99% or higher, and has an average crystal grain size of 150 μm or less.
[0012] The backing plate used in the present invention is made of copper or a copper alloy. The material of this copper alloy backing plate is not particularly limited, but it is preferable to use a copper alloy such as a copper-chromium alloy or a copper-zinc alloy, which has a lower thermal expansion coefficient than aluminum alloys, is hard and less prone to deformation, and has good thermal conductivity. The thickness of the backing plate is approximately 30 mm.
[0013] The target assembly of the present invention is formed by diffusion bonding the target and backing plate described above with an insert material interposed therebetween. The insert material interposed between the target and backing plate is an aluminum or aluminum alloy plate having a thickness of 0.8 mm or more, preferably 4 to 5 mm. The reason why the insert material must be 0.8 mm or thick is that it softens sufficiently at the temperature during diffusion bonding, and microscopically, the surface oxide film breaks down, revealing a new active surface, facilitating atomic diffusion. It also alleviates stress caused by the difference in thermal expansion between the sputtering target and backing plate when cooled to room temperature after diffusion bonding. From this perspective, the insert material is preferably as thick as possible. However, due to sputtering equipment limitations, the total thickness of the backing plate and insert material is regulated, so increasing the insert material thickness necessitates a thinner backing plate. However, a thinner backing plate reduces cooling efficiency, which is problematic in high-power sputtering, so a certain thickness of the backing plate must be maintained. Taking these factors into consideration, it is preferable to use an insert material with a thickness of 4 to 5 mm. In this case, the thickness of the backing plate is about 30 mm. As the aluminum alloy plate, for example, A1050 or A6061 can be used.
[0014] In the present invention, a metal thin film layer made of Ti, V, Cr, Nb, Pd, Ir, Pt, or an alloy containing at least one of these metals is provided between the target and the insert material, and between the insert material and the backing plate, and diffusion-bonded. Therefore, a metal thin film layer exists between the target and the insert material, and between the insert material and the backing plate.
[0015] Here, Ti, V, Cr, Fe, Co, Ni, Nb, Pd, Ir, and Pt are metals that can form solid solutions with the elements Al, Cu, and W, and are therefore preferred as the metal thin film layer to be interposed between these elements. Whether or not solid solutions are formed between metals containing these metals becomes clear, for example, from the data shown in Figures 1 to 10. Figures 1 to 10 are binary phase diagrams of Al, Cu, and W with each metal, and it can be seen that Ti, V, Cr, Fe, Co, Ni, Nb, Pd, Ir, and Pt form solid solutions with Al, Cu, and W.
[0016] Therefore, these metal thin film layers improve the adhesion between the target and the insert material, and between the insert material and the backing plate, thereby increasing the bonding strength. Furthermore, the metal thin film layer between the aluminum or aluminum alloy insert material and the copper or copper alloy backing plate can prevent the formation of an intermetallic compound layer between the aluminum alloy and the copper alloy during diffusion bonding, thereby preventing a decrease in the bonding strength between them.
[0017] Among the metals Ti, V, Cr, Fe, Co, Ni, Nb, Pd, Ir, and Pt, Fe, Co, and Ni are magnetic materials and therefore are not preferred as they may affect sputtering. V is not particularly preferred as its oxide is toxic, and Pd, Ir, and Pt are noble metals or metals equivalent to noble metals, so it is best to avoid them, but there is no problem in terms of functionality.
[0018] The metal thin film layer preferably has a thickness of more than 0.1 μm and not more than 3.0 μm. It is preferable that the thickness is more than 0.1 μm, preferably 0.2 μm or more and not more than 3.0 μm. If the thickness is 0.1 μm or less, intermetallic compounds or similar substances may be partially formed, reducing the bonding strength, and if the thickness is more than 3.0 μm, there is a risk that an intermetallic compound layer may be formed between the metal thin film layer and the backing plate or target, reducing the bonding strength.
[0019] Such a metal thin film layer may be formed as a coating layer on at least one of the bonding surfaces between the target and the insert material and at least one of the bonding surfaces between the insert material and the backing plate. The method for forming the coating layer is not particularly limited, and physical vapor deposition methods such as sputtering, ion plating, and vacuum deposition, or wet plating can be used. The coating layer may consist of one layer or two or more layers. When forming the coating layer, it is preferable to perform a pretreatment such as washing with ethanol on the bonding surfaces.
[0020] The metal thin film layer between the target and the insert material and the metal thin film layer between the insert material and the backing plate may be the same or different. In order to prevent the formation of an intermetallic compound layer between the aluminum alloy of the insert material and the copper alloy of the backing plate by diffusion bonding and to prevent a decrease in the bonding strength between them, it is sufficient to provide a metal thin film layer only between the insert material and the backing plate.
[0021] The bond strength between the target and the insert material of the diffusion-bonded target assembly, and the bond strength between the insert material and the backing plate, each have an average shear strength of 4 kg / mm 2 ] or more is preferable. This is because this provides sufficient bonding strength to withstand high-power sputtering. Also, it is preferable that the coefficient of variation, which is the ratio of the average shear strength to the standard deviation σ of shear strength across the surface, is 0.15 or less. This is because the value obtained by subtracting 3σ from the average shear strength is 2.2 [kg / mm 2 ] or more, and it is believed that reliability of the bonding strength is guaranteed.
[0022] As described above, the method for manufacturing the target assembly of the present invention simply requires forming a coating layer on at least one of the bonding surfaces between the target and the insert material and on at least one of the bonding surfaces between the insert material and the backing plate before diffusion bonding; otherwise, the manufacturing process can be the same as that for manufacturing a target assembly using conventional diffusion bonding.
[0023] Since the bonding conditions under which an intermetallic compound layer is likely to be formed by diffusion bonding vary, a metal thin film layer may be provided only on bonding surfaces under which an intermetallic compound layer is likely to be formed depending on the bonding conditions.
[0024] The conditions for the diffusion bonding may be conventionally known conditions and are not particularly limited. For example, the conditions may be hot isostatic pressing (HIP) at a temperature of 400 to 500°C for 2 to 4 hours with a pressure of 4 to 10 kg / mm 2 ] can be performed under the conditions.
[0025] The present invention will be described below with reference to examples and comparative examples. (Examples 1-7) A tungsten (W: 99.999%) target material (a 460 mm diameter disc-shaped plate) and a copper-zinc backing plate material of the same dimensions were cleaned with ethanol. A 5 mm thick pure aluminum (A-1050) plate was used as an insert material and similarly cleaned with ethanol. After cleaning, the insert material was cleaned by bombardment in an Ar atmosphere (cleaning conditions: Ar atmosphere: 0.7 Pa, input power: 2 kW, time: 30 minutes), and a continuous metal thin film layer was formed. An intermetallic thin film layer was formed on the bonding surface by physical vapor deposition (physical vapor deposition conditions: Ar atmosphere: 0.4 Pa, input power: 3 kW, deposition rate: 0.1 μm / min) using a thin film composed of the metal listed in Table 1. Next, this assembly was canned into a container (vacuum level 1 Pa or less) and diffusion bonded by hot isostatic pressing (HIP). The diffusion bonding was carried out at the temperature, time and pressure shown in Table 1.
[0026] Comparative Examples 1 and 2 Target assemblies were manufactured in the same manner as in the Examples, except that diffusion bonding was performed without providing a thin metal film between the target and the insert material and between the backing plate and the insert material. The results are shown in Table 1 and FIG. 14.
[0027] Comparative Examples 3 and 4 Target assemblies were manufactured in the same manner as in the Examples, except that the diffusion bonding temperature was set outside the range of conventionally known conditions.
[0028] Comparative Examples 5 to 8 Target assemblies were manufactured in the same manner as in Examples, except that the thickness of the metal thin film layer was outside the range of the present invention. The results are shown in Table 1 and FIGS.
[0029] Examples 11 to 17 were carried out in the same manner as in Examples 1 to 7, except that a molybdenum target was used instead of a tungsten target, as shown in Table 2. The results are shown in Table 2.
[0030] Comparative Examples 11 and 12 As shown in Table 2, target assemblies were produced in the same manner as in Comparative Examples 1 and 2, except that a molybdenum target was used.
[0031] Comparative Examples 13 and 14 As shown in Table 2, target assemblies were produced in the same manner as in Comparative Examples 3 and 4, except that a molybdenum target was used.
[0032] Comparative Examples 15-18 As shown in Table 2, target assemblies were produced in the same manner as in Comparative Examples 5-8, except that molybdenum targets were used.
[0033] (Method for Testing Average Shear Strength) The average shear strength across the plane between the target and the insert material, and the average shear strength across the plane between the insert material and the backing plate were examined by the following method.
[0034] (Shear test method) The shear strength at room temperature of test pieces cut from various positions (0 mm from the center of the 460 mm diameter target and 230 mm from the outer periphery) of the diffusion-bonded material was examined. (Test conditions: Shimadzu AUTOGRAPH AG-50kNG, speed 5 mm / min) In addition, the standard deviation σ of shear strength and the coefficient of variation, which is the ratio of the standard deviation σ to the standard deviation σ of shear strength across the surface, were calculated. These results are shown in Tables 1 and 2 and in Figures 11 and 12.
[0035] (Whether or not compounds were formed at the diffusion-bonded interface) The presence or absence of compounds formed at the diffusion-bonded interface was confirmed by observing the cross section with a scanning electron microscope (SEM) (observation conditions: Hitachi High-Tech TM4000Plus, acceleration voltage 15 kV). The results are shown in Figs. 13 to 16.
[0036] (Results) In Examples 1-7, a thin metal layer of Ti, Cr, or Nb was provided between the target and the insert material, and between the backing plate and the insert material, respectively, and diffusion bonding was performed under specified conditions. This suppressed the formation of an intermetallic compound layer between the aluminum or aluminum alloy insert material and the copper alloy backing plate, preventing a decrease in bond strength and achieving a target assembly with a sufficiently improved bond strength between the target and the insert material. When compared at the same bonding temperature, Ti and Cr had similar bond strengths, while Nb had lower bond strengths than Ti and Cr. This is thought to be due to Nb's higher melting point and smaller diffusion coefficient in Al and W than Ti and Cr. Furthermore, when Al deforms due to thermal expansion during diffusion bonding, Ti is a soft metal and is easily deformed, while Cr has a low Young's modulus and is a hard metal, which may cause cracks. Therefore, Ti is more suitable than Cr in this respect. On the other hand, in Comparative Examples 1 and 2, diffusion bonding was performed without providing a metal thin film layer between the target and the insert material and between the backing plate and the insert material. Therefore, in Comparative Example 1, where diffusion bonding was performed at a low temperature to prevent compound formation, delamination occurred between the target and the insert material. In Comparative Example 2, where diffusion bonding was performed at a high temperature, compound formation occurred between the insert material and the backing plate, resulting in delamination. In Comparative Example 3, even though a metal thin film layer was provided, the diffusion bonding temperature was low, so little diffusion occurred and delamination occurred. In Comparative Example 4, the diffusion bonding temperature was too high, resulting in a thick compound layer and delamination. In Comparative Example 5, the metal thin film layer was too thin, resulting in significant variation in bonding strength. On the other hand, in Comparative Examples 6-8, where the metal thin film layer was too thick, the compound layer became thick, resulting in insufficient strength and resulting in delamination. As shown in the cross-sectional SEM image of the interface between the insert material and the backing plate in Example 3 in Figure 13, no intermetallic compound layer was observed at the bonding interface between the insert material and the backing plate in Example 3. On the other hand, in the cross-sectional SEM image of the interface between the insert material and the backing plate of Comparative Example 2 in FIG. 14, an intermetallic compound layer was observed.In the cross-sectional SEM image of the interface between the insert material and the backing plate of Comparative Example 5 in Fig. 15, the metal thin film layer was too thin, and partial formation of an intermetallic compound was observed. In the cross-sectional SEM image of the interface between the target and the insert material of Comparative Example 7 in Fig. 16, the metal thin film layer was too thick, and an intermetallic compound layer was observed.
[0037]
[0038]
Claims
1. A target assembly in which an insert material of aluminum or aluminum alloy plate is sandwiched between a target made of tungsten or molybdenum and a backing plate made of copper or copper alloy and diffusion-bonded, wherein a thin metal layer made of Ti, V, Cr, Nb, Pd, Ir, Pt or an alloy containing at least one of these metals and having a thickness of more than 0.1 μm and not more than 3.0 μm is diffusion-bonded between the target and the insert material, and between the backing plate and the insert material, respectively.
2. The average shear strength across the surface between the target and the insert material, and the average shear strength across the surface between the insert material and the backing plate are each 4 [kg / mm 2 2. The target assembly of claim 1, wherein the axial length of the target is equal to or greater than 100 mm.
3. A target assembly as described in claim 1 or claim 2, wherein a coefficient of variation which is the ratio of the average shear strength across the plane between the target and the insert material to the standard deviation σ of the shear strength across the plane, and a coefficient of variation which is the ratio of the average shear strength across the plane between the insert material and the backing plate to the standard deviation σ of the shear strength across the plane, are each 0.15 or less.
4. A method for manufacturing a target assembly in which an insert material of aluminum or aluminum alloy plate is sandwiched between a target made of tungsten or molybdenum and a backing plate made of copper or copper alloy and diffusion-bonded, comprising providing a thin metal layer having a thickness of more than 0.1 μm and not more than 3.0 μm and made of Ti, V, Cr, Nb, Pd, Ir, Pt or an alloy containing at least one of these metals, at least one between the target and the insert material and the backing plate and the insert material, and then diffusion-bonding the layers to form a target assembly.
5. A method for manufacturing a target assembly according to claim 4, further comprising providing a thin metal layer having a thickness of more than 0.1 μm and not more than 3.0 μm, the thin metal layer being made of Ti, V, Cr, Nb, Pd, Ir, Pt or an alloy containing at least one of these metals, between the target and the insert material and between the backing plate and the insert material, and then performing diffusion bonding.
6. The metal thin film layer provided at least one between the target and the insert material and between the backing plate and the insert material has an average shear strength across the surface between the target and the insert material and an average shear strength across the surface between the insert material and the backing plate of 4 [kg / mm 2 6. The method for manufacturing a target assembly according to claim 4, wherein the metal thin film layer has a thickness of at least 100 nm.
Citation Information
Patent Citations
Insert material for joining ti-al series intermetallic compound and ti base alloy and joining method therefor and joined body
JP1999077365A
Assembly composed of tantalum or tungsten target and packing plate made from copper alloy, and manufacturing method therefor
JP2002129316A
Ceramic sputtering target assembly and a method for producing the same
US20100288631A1
Backing plate, target assembly, and sputtering target
WO2012066764A1
Cited By
Diffusion bonded tungsten containing target to titanium or titanium alloy backing plate
US12644174B2
Diffusion bonded tungsten containing target to titanium or titanium alloy backing plate
US20250122608A1