Waste lithium battery pyrogenic slag lithium extraction method applied to integration of entire industrial chain of lithium batteries

By using heat treatment technology of using chloride calciner and cation exchanger in waste lithium battery fire slag, the silicate structure is activated and lithium ions are transformed from insoluble to soluble, which solves the slow leaching process rate and low lithium recovery rate. Problem, an efficient and environmentally friendly lithium battery fire slag recycling process has been achieved.

WO2024243839A1PCT designated stage expired Publication Date: 2024-12-05GUANGDONG BRUNP RECYCLING TECH CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/097346
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

In the prior art, when dealing with waste lithium battery fire slag, the leaching process rate is slow and the lithium recovery rate is low, and the frequent use of strong acids and strong alkalis leads to environmental protection problems.

Method used

The mixed inorganic salt formed by chloride is heat treated as a calcining agent and a cation exchanger to activate the silicate structure, transforming lithium ions from insoluble to soluble, and efficient recovery is achieved through microwave heating and water leach extraction.

Benefits of technology

It realizes efficient recycling of lithium ions, with an extraction rate of more than 90%, a simple process, reduces acid and alkali consumption, reduces environmentally friendly treatment costs, and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023097346_05122024_PF_FP_ABST
    Figure CN2023097346_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure relates to the technical field of lithium battery recovery, and relates to a waste lithium battery pyrogenic slag lithium extraction method applied to the integration of the entire industrial chain of lithium batteries. Pyrogenic slag is mixed with a roasting agent which is a mixed inorganic salt and a cation exchanger for heat treatment; silicate structures in the pyrogenic slag can be activated under the action of high temperature; when silicates are mixed with a molten salt formed by the roasting agent, under the driving of a chemical position gradient, ions would diffuse and large-radius cations can exchange with small-radius cations in lattices; a cation exchanger is added for catalysis, and under the condition, lithium ions are converted from an insoluble silicate phase into a soluble lithium salt phase, so that lithium is recycled by leaching. The method has a high conversion rate, a simple process, and is easy for industrial production; the process does not require the use of strong acids or strong alkalis, so that the consumption of acids and alkalis is reduced; in addition, no acidic and alkaline waste gas would be generated in the process, thereby reducing the cost of environmental protection treatment. The method is a green and environmentally friendly recovery process.
Need to check novelty before this filing date? Find Prior Art

Description

Lithium extraction method for waste lithium battery pyrometallurgical slag applied to the full chain integration of lithium batteries Technical Field

[0001] The present disclosure belongs to the field of lithium battery recycling technology, and specifically relates to a method for extracting lithium from waste lithium battery pyrometallurgical slag applied to the full-chain integration of lithium batteries. Background Art

[0002] Because fossil fuels are non-renewable energy sources and their combustion contributes to global warming, humanity is spurring the development of new renewable energy sources. However, most of these new energy sources are difficult to store and unstable, requiring a transition to energy storage media. Lithium batteries are currently the most widely used energy storage medium. Their widespread use consumes significant amounts of lithium resources and generates a significant amount of waste.

[0003] The currently developed pyrometallurgical process for directly processing spent lithium batteries has garnered widespread attention. This process eliminates the need for extensive pretreatment and consumes relatively low amounts of chemical reagents. In this process, spent lithium batteries undergo ultra-high-temperature treatment to form an alloy phase and a lithium-containing slag. Currently, only the alloy phase is recovered, while the lithium-containing slag remains as waste. Research has shown that the lithium content of the lithium-containing slag is similar to that of lithium ore, suggesting that extracting lithium from the slag has potential economic value.

[0004] Currently, the treatment of spent lithium battery pyrometallurgical slag often involves roasting and leaching with acids and alkalis (sulfuric acid, hydrochloric acid, or sodium hydroxide). However, this process forms silicate and aluminum hydroxide gels, slowing the leaching process. Increasing the roasting temperature can address the slow leaching rate, but the lithium recovery rate decreases significantly.

[0005] Therefore, developing an environmentally friendly and efficient method for recycling waste lithium battery pyrometallurgical slag is a technical problem that urgently needs to be solved.

[0006] In view of this, the present disclosure is proposed.

[0007] Summary of the Invention

[0008] The purpose of the present disclosure includes providing a method for extracting lithium from waste lithium battery pyrometallurgical slag that is applied to the entire lithium battery chain integration, aiming to provide an environmentally friendly and efficient method for recycling pyrometallurgical slag.

[0009] In order to achieve the above-mentioned purpose of the present disclosure, the following technical solutions can be adopted:

[0010] The solution provided by the present disclosure includes providing a method for extracting lithium from waste lithium battery slag using pyrometallurgical process, which is applied to the integrated lithium battery chain. The method comprises: heat-treating a mixture of pyrometallurgical process slag, a roasting agent, and a cation exchanger, and then leaching the heat-treated material;

[0011] The calcining agent is a mixed inorganic salt formed by two or more chlorides, the melting point of the calcining agent is 190°C-230°C, the decomposition temperature of the calcining agent is greater than 700°C, and the treatment temperature of the heat treatment is greater than the melting point of the calcining agent and less than the decomposition temperature of the calcining agent.

[0012] In some embodiments of the present disclosure, the calcining agent includes sodium chloride, potassium chloride, and zinc chloride.

[0013] In some embodiments of the present disclosure, the calcining agent includes, by mass percentage, 1%-70% sodium chloride, 1%-70% potassium chloride, and 1%-75% zinc chloride.

[0014] In some embodiments of the present disclosure, the calcining agent includes, by mass percentage, 7%-11% sodium chloride, 15%-32% potassium chloride, and 61%-75% zinc chloride.

[0015] In some embodiments of the present disclosure, the molar ratio of anions in the calcining agent to lithium ions in the pyrometallurgical slag is (1-10):1.

[0016] In some embodiments of the present disclosure, the molar ratio of anions in the calcining agent to lithium ions in the pyrometallurgical slag is (7-8):1.

[0017] In some embodiments of the present disclosure, the cation exchanger is selected from at least one of a polymer of 2-acrylic acid and divinylbenzene, ethanesulfonic acid, and a styrene-based cation exchange resin.

[0018] In some embodiments of the present disclosure, the styrene-based cation exchange resin includes cation exchange resin IR120 and cation exchange resin IR200.

[0019] In some embodiments of the present disclosure, the mass ratio of the cation exchanger to the mixed powder of pyrometallurgical slag and calcining agent is 1:5-10.

[0020] In some embodiments of the present disclosure, the mass ratio of the cation exchanger to the pyrometallurgical slag is 1:7-8.

[0021] In some embodiments of the present disclosure, the heat treatment is microwave heating.

[0022] In some embodiments of the present disclosure, the heating temperature of the microwave heating treatment is 210° C.-230° C., and the treatment time is 15 min-30 min.

[0023] In some embodiments of the present disclosure, grinding and screening are performed after the heat treatment is completed, and the screened material obtained by screening is subjected to water leaching for lithium, followed by solid-liquid separation.

[0024] In some embodiments of the present disclosure, during the process of water leaching for lithium extraction, the liquid-to-solid mass ratio of the water leaching is controlled to be 5-50:1.

[0025] In some embodiments of the present disclosure, water leaching of lithium is carried out at 25°C-80°C.

[0026] In some embodiments of the present disclosure, the leaching time for water leaching of lithium is 15 min to 60 min.

[0027] In some embodiments of the present disclosure, the process of water leaching lithium is assisted by stirring, and the stirring rate is controlled to be 150 r / min-400 r / min.

[0028] In some embodiments of the present disclosure, the particle size of the undersize is less than 200 mesh.

[0029] In some embodiments of the present disclosure, after the water leaching of lithium is completed, the leachate is allowed to stand or cool to room temperature, and then vacuum filtered to separate the filtrate and filter residue in the leachate.

[0030] In some embodiments of the present disclosure, the preparation process of the mixture includes: first crushing the pyrometallurgical slag to obtain slag powder, mixing and grinding the slag powder with a roasting agent, and then mixing it with a cation exchanger.

[0031] Using two or more chlorides to form a mixed inorganic salt as a calcining agent, the pyrometallurgical slag is mixed with the calcining agent and a cation exchanger for heat treatment. The high temperature can activate the silicate structure in the pyrometallurgical slag. When the silicate is mixed with the molten salt formed by the calcining agent, the ions diffuse under the drive of the chemical potential gradient, and the large-radius cations can exchange the small-radius cations from the lattice. The addition of a cation exchanger catalyzes the separation or enrichment of substances through the adsorption and desorption of the cation exchanger to promote ion exchange. Under these conditions, lithium ions are transformed from an insoluble silicate phase to a soluble lithium salt phase, thereby facilitating further lithium recovery through leaching. This method has a high lithium ion conversion rate, a simple process, and is easy to industrialize. The process does not require the use of strong acids or bases, reducing acid and base consumption, and does not produce acid and base waste gas during the process, reducing environmental treatment costs. It is a green and environmentally friendly recovery process. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work.

[0033] FIG1 is a first process flow chart of the present disclosure;

[0034] FIG2 is a second process flow chart of the present disclosure. DETAILED DESCRIPTION

[0035] The embodiments of the present disclosure will be described in detail below with reference to the examples. However, those skilled in the art will appreciate that the following examples are intended only to illustrate the present disclosure and should not be construed as limiting the scope of the present disclosure. Where specific conditions are not specified in the examples, the experiments were performed under conventional conditions or the conditions recommended by the manufacturer. Where the manufacturer of the reagents or instruments is not specified, all are commercially available conventional products.

[0036] The endpoints of the ranges and any values ​​disclosed in this disclosure are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoints of each range, the endpoints of each range and individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be considered to be specifically disclosed herein.

[0037] Pyrometallurgical slag refers to the lithium-containing slag obtained after direct pyrometallurgical processing of waste lithium batteries. Elements such as Si, Al and O in the slag will form a stable, insoluble silicate structure with Li. How to convert the lithium in the silicate into leachable lithium salts is the key technology for lithium extraction from slag.

[0038] As shown in Figure 1, an embodiment of the present disclosure provides a method for extracting lithium from pyrometallurgical slag of waste lithium batteries that is applied to the integrated lithium battery chain, including: heat-treating a mixture of pyrometallurgical slag, a calcining agent, and a cation exchanger, and then leaching the heat-treated material; wherein the calcining agent is a mixed inorganic salt formed by two or more chlorides, the melting point of the calcining agent is 190°C-230°C, and the decomposition temperature of the calcining agent is greater than 700°C; the treatment temperature of the heat treatment is greater than the melting point of the calcining agent and less than the decomposition temperature of the calcining agent.

[0039] It should be noted that the calcining agent is a mixed inorganic salt, which produces a molten salt under high temperature conditions. This ionic melt, like an aqueous solution, is also a solvent—specifically, a non-aqueous high-temperature flux. High temperatures activate the silicate structure in the pyrometallurgical slag. When the silicates and molten salts mix, driven by the chemical potential gradient, ions diffuse, and cations with larger radii can exchange smaller cations from the lattice. Furthermore, when the radii of the cations in the molten salts are similar to those in the silicates, isomorphism—the ability of the two ions to exchange with each other—is readily observed. The key characteristic of molten salts formed by melting salts is that they dissociate into ions upon melting. The positive and negative ions interact via Coulomb forces, making them useful as reaction media at high temperatures, enabling ion exchange between the solid slag and the ionic melt. The cation exchanger can separate and enrich cations in the molten salt. Since the cation exchanger is also infusible, ions can freely diffuse into the cation exchanger, enter the microscopic pores of the cation exchanger, and react with the internal exchange groups, allowing the lithium ions in the silicate after the molten salt to exchange with the cations in the roasting agent. Therefore, by adding the cation exchanger as a catalyst, the adsorption and desorption of the cation exchanger can separate or enrich the substances and promote ion exchange. Lithium ions can be transformed from the insoluble silicate phase to the soluble lithium salt phase, facilitating lithium recovery through leaching.

[0040] Specifically, the calcining agent can be a variety of mixed inorganic salts with a melting point of 190°C, 195°C, 200°C, 205°C, 210°C, 215°C, 220°C, 225°C, 230°C, etc., which is slightly lower than the heat treatment temperature; the decomposition temperature is greater than 700°C, such as about 800°C.

[0041] Referring to FIG. 2 , the lithium extraction method provided in the embodiment of the present disclosure may specifically include the following steps:

[0042] S1. Mixing

[0043] The pyrometallurgical slag, the calcining agent and the cation exchanger are mixed to obtain a mixture for later use.

[0044] In some embodiments, the calcining agent includes sodium chloride (NaCl), potassium chloride (KCl) and zinc chloride (ZnCl2). A mixed inorganic salt formed by the three inorganic salts is used as the calcining agent. It is a ternary mixed inorganic salt with a low melting point and a high decomposition temperature, which is beneficial to further improve the efficiency of ion exchange.

[0045] In some embodiments, the calcining agent comprises, by mass percentage, 1%-70% sodium chloride, 1%-70% potassium chloride, and 1%-75% zinc chloride. Preferably, by mass percentage, the calcining agent comprises 7%-11% sodium chloride, 15%-32% potassium chloride, and 61%-75% zinc chloride. Optimizing the amounts of the various components in the calcining agent can help improve the recovery rate of lithium ions.

[0046] Specifically, the mass percentage of sodium chloride in the roasting agent can be 1%, 5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, etc.; the mass percentage of potassium chloride can be 1%, 5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, etc.; the mass percentage of zinc chloride can be 1%, 5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, etc.; the total amount of sodium chloride (NaCl), potassium chloride (KCl) and zinc chloride (ZnCl2) is 100%.

[0047] In some embodiments, the molar ratio of the anions in the roasting agent to the lithium ions in the pyro slag is (1-10):1, preferably (7-8):1. The amount of the roasting agent is optimized to improve the recovery rate of lithium. Specifically, the molar ratio of the anions in the roasting agent to the lithium ions in the pyro slag can be 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, etc.

[0048] In some embodiments, the cation exchanger is selected from at least one of a polymer of 2-acrylic acid and divinylbenzene, ethanesulfonic acid, and a styrene-based cation exchange resin. The styrene-based cation exchange resin includes cation exchange resin IR120 and cation exchange resin IR200, any one or more of which may be used. All of the above cation exchangers are commercially available, and optimizing the cation exchangers can further improve the recovery rate of lithium.

[0049] In some embodiments, the mass ratio of the cation exchanger to the mixed powder of slag and calcining agent is 1:5-10, preferably 1:7-8. By optimizing the amount of the cation exchanger, the lithium ions can be converted from the insoluble silicate phase to the soluble lithium salt phase, thereby improving the recovery rate of lithium.

[0050] Specifically, the mass ratio of the mixed powder of the cation exchanger, slag and roasting agent can be 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, etc.

[0051] In some embodiments, the mixture is prepared by crushing pyrometallurgical slag to obtain slag powder, mixing and grinding the slag powder with a roasting agent, and then mixing with a cation exchanger. The mixing steps are controlled to improve the uniformity of the mixture.

[0052] Specifically, the crushing method is not limited, and a blade crusher can be used to crush large pieces of slag. The mixed grinding can be performed using a general grinder, and the grinding is performed until no granular feeling appears, and the size is approximately 80-150 mesh.

[0053] S2. Heat treatment

[0054] In some embodiments, the heat treatment may be performed by microwave heating, but is not limited thereto.

[0055] It should be noted that through microwave treatment, the molecules rotate back and forth, collide and rub with the surrounding molecules, the total energy of the molecules increases, the material temperature rises sharply, and the reaction of lithium ions with anions in the molten salt is further accelerated to form soluble salts, and the lithium ions are transformed from the insoluble silicate phase to the soluble lithium salt phase, so that the lithium is extracted and recycled by water leaching. This method effectively solves the problem of recycling the unreduced lithium contained in the slag and avoids the waste of resources.

[0056] In some embodiments, the microwave heating treatment is performed at a temperature of 210° C. to 230° C., and for a time of 15 to 30 minutes. The microwave heating treatment can be performed using a conventional microwave oven, and the heating temperature can be 210° C., 215° C., 220° C., 225° C., 230° C., etc., and the treatment time can be 15 minutes, 20 minutes, 25 minutes, 30 minutes, etc.

[0057] S3, grinding and screening

[0058] After the heat treatment is completed, the material is cooled and ground twice and screened, and enters the leaching process with a finer particle size to improve the leaching effect.

[0059] Specifically, secondary grinding can be performed using a conventional grinding machine, and screening can be performed using a circular vibrating screen with a mesh size of 200. The undersize fraction with a particle size of less than 200 mesh is used for water leaching of lithium. The oversize fraction can be ground again and sieved. Once the particle size meets the requirements, it can also be used in the subsequent leaching process.

[0060] S4. Leaching

[0061] The leaching method is not limited and can be a water leaching method for lithium. In actual operation, the screened undersize is subjected to water leaching for lithium extraction, followed by solid-liquid separation.

[0062] In some embodiments, during the water leaching of lithium, the liquid-to-solid mass ratio of the water leaching is controlled to be 5-50:1, the water leaching temperature is controlled to be 25°C-80°C, and the leaching time is controlled to be 15 minutes-60 minutes. By further optimizing the parameters of the water leaching of lithium, the lithium extraction rate can be increased.

[0063] Specifically, the liquid-to-solid mass ratio can be 5:1, 10:1, 20:1, 30:1, 40:1, 50:1, etc.; the water immersion temperature can be 25°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, etc., and the immersion time can be 15min, 20min, 30min, 40min, 50min, 60min, etc.

[0064] In some embodiments, the lithium extraction process is assisted by stirring, and the stirring rate is controlled to be 150 r / min-400 r / min. Stirring can accelerate the lithium extraction process and help improve the lithium extraction rate. Specifically, the stirring rate can be 150 r / min, 200 r / min, 250 r / min, 300 r / min, 350 r / min, 400 r / min, etc.

[0065] In some embodiments, after the completion of lithium leaching in water, the leachate is allowed to stand or cool to room temperature, and then vacuum filtered to separate the filtrate and filter residue in the leachate.

[0066] The features and performance of the present disclosure are further described in detail below with reference to the embodiments.

[0067] It should be noted that the treatment objects of the following embodiments and comparative examples are all: slag after pyrometallurgical treatment of waste lithium batteries, and the composition of the slag is shown in Table 1.

[0068] Table 1 Slag content before treatment

[0069] Example 1

[0070] This embodiment provides a method for extracting lithium from waste lithium battery pyrometallurgical slag applied to the full-chain integration of lithium batteries, comprising the following steps:

[0071] (1) Mixing

[0072] Under the protection of nitrogen and carbon dioxide, 60g of slag from the pyrometallurgical treatment of waste lithium batteries was crushed to obtain slag powder.

[0073] The slag powder and the calcining agent (by mass percentage, 8.1% NaCl-31.3% KCl-60.6% ZnCl2) were mixed according to the formula (calcining agent anion / Li +) in a molar ratio of 1:1, the mixture is ground into about 100 mesh, and then ethanesulfonic acid is added in a mass ratio of the total amount of the cation exchanger, the slag powder and the roasting agent of 1:5 to obtain a mixture.

[0074] (2) Heat treatment

[0075] The mixture obtained in step (1) was treated by microwave at 230°C for 20 min.

[0076] (3) Grinding and screening

[0077] After the microwave treatment, the mixed powder was cooled to room temperature and then subjected to secondary grinding for 10 min. The secondary ground powder was sieved through a 200-mesh circular vibrating sieve to obtain undersize powder.

[0078] (4) Extraction

[0079] The powder under the sieve was mixed with water at a liquid-to-solid mass ratio of 10:1, stirred at 150 r / min at 25°C for 15 minutes, and the leachate was allowed to stand and naturally cool to room temperature before being filtered and separated to obtain the leachate and filter residue.

[0080] Test: The following formulas are used to calculate the lithium mass in the slag and the lithium extraction rate.

[0081] Calculation formula: m0=c2*V2,η=c1*V1 / m0*100%;

[0082] Wherein, c2 is the concentration of lithium ions in the prepared solution measured by slag dissolution, mg / L;

[0083] V2 is the volume of the prepared solution, L;

[0084] η is the extraction rate of lithium, %;

[0085] c1 is the measured concentration of lithium ions in the prepared filtrate, mg / L;

[0086] V1 is the volume of the prepared filtrate, L;

[0087] m0 is the mass of lithium in the slag taken before roasting.

[0088] After testing, the lithium extraction rate was calculated to be 91.03%.

[0089] Example 2

[0090] This embodiment provides a method for extracting lithium from waste lithium battery pyrometallurgical slag applied to the full-chain integration of lithium batteries, comprising the following steps:

[0091] (1) Mixing

[0092] Under the protection of nitrogen and carbon dioxide, 100g of slag from the pyrometallurgical treatment of waste lithium batteries was crushed to obtain slag powder.

[0093] The slag powder and the calcining agent (by mass percentage, 10.0% NaCl-15.1% KCl-74.9% ZnCl2) were mixed according to the ratio (calcining agent anion / Li + ) in a molar ratio of 2:1, the mixture is ground into about 100 mesh, and then a macroporous strongly acidic styrene cation exchange resin is added in a mass ratio of the cation exchanger to the total amount of the slag powder and the roasting agent of 1:10 to obtain a mixture.

[0094] (2) Heat treatment

[0095] The mixture obtained in step (1) was treated by microwave at 220°C for 20 min.

[0096] (3) Grinding and screening

[0097] After the microwave treatment, the mixed powder was cooled to room temperature and then subjected to secondary grinding for 10 min. The secondary ground powder was sieved through a 200-mesh circular vibrating sieve to obtain undersize powder.

[0098] (4) Extraction

[0099] The powder under the sieve was mixed with water at a liquid-to-solid mass ratio of 30:1, stirred at 150 r / min at 60°C for 30 minutes, and the leachate was allowed to stand and naturally cool to room temperature before being filtered and separated to obtain a filtrate and a filter residue.

[0100] The lithium extraction rate was calculated to be 92.04%.

[0101] Example 3

[0102] This embodiment provides a method for extracting lithium from waste lithium battery pyrometallurgical slag applied to the full-chain integration of lithium batteries, comprising the following steps:

[0103] (1) Mixing

[0104] Under the protection of nitrogen and carbon dioxide, 100g of slag from the pyrometallurgical treatment of waste lithium batteries was crushed to obtain slag powder;

[0105] The slag powder and the calcining agent (by mass percentage, 7.5% NaCl-23.9% KCl-68.6% ZnCl2) were mixed according to the formula (calcining agent anion / Li + ) in a molar ratio of 5:1, the mixture is ground into about 100 mesh, and then a strongly acidic styrene cation exchange resin is added in a mass ratio of the cation exchanger to the total amount of the slag powder and the roasting agent of 1:15 to obtain a mixture.

[0106] (2) Heat treatment

[0107] The mixture obtained in step (1) was treated by microwave at 210°C for 20 min.

[0108] (3) Grinding and screening

[0109] After the microwave treatment, the mixed powder was cooled to room temperature and then subjected to secondary grinding for 10 min. The secondary ground powder was sieved through a 200-mesh circular vibrating sieve to obtain undersize powder.

[0110] (4) Extraction

[0111] The powder under the sieve was mixed with water at a liquid-to-solid mass ratio of 15:1, stirred at 150 r / min at 30°C for 30 minutes, and the leachate was allowed to stand and naturally cool to room temperature before being filtered and separated to obtain a filtrate and a filter residue.

[0112] The lithium extraction rate was calculated to be 93.1%.

[0113] Example 4

[0114] This embodiment provides a method for extracting lithium from waste lithium battery pyrometallurgical slag applied to the full-chain integration of lithium batteries, comprising the following steps:

[0115] (1) Mixing

[0116] Under the protection of nitrogen and carbon dioxide, 1 kg of slag from the pyrometallurgical treatment of waste lithium batteries was crushed to obtain slag powder;

[0117] The slag powder and the calcining agent (by mass percentage, 8.1% NaCl-31.3% KCl-60.6% ZnCl2) were mixed according to the formula (calcining agent anion / Li + ) in a molar ratio of 9:1, the mixture was mixed and ground to about 100 mesh, and then cation exchange resin IR200 was added at a mass ratio of cation exchanger to the total amount of slag powder and roasting agent of 1:15 to obtain a mixture.

[0118] (2) Heat treatment

[0119] The mixture obtained in step (1) was treated by microwave at 230°C for 20 min.

[0120] (3) Grinding and screening

[0121] After the microwave treatment, the mixed powder was cooled to room temperature and then subjected to secondary grinding for 10 min. The secondary ground powder was sieved through a 200-mesh circular vibrating sieve to obtain undersize powder.

[0122] (4) Extraction

[0123] The powder under the sieve was mixed with water at a liquid-to-solid mass ratio of 10:1, stirred at 150 r / min at 50°C for 30 minutes, and the leachate was allowed to stand and naturally cool to room temperature before being filtered and separated to obtain a filtrate and a filter residue.

[0124] The lithium extraction rate was calculated to be 93.87%.

[0125] Example 5

[0126] This embodiment provides a method for extracting lithium from waste lithium battery pyrometallurgical slag applied to the full-chain integration of lithium batteries, comprising the following steps:

[0127] (1) Mixing

[0128] Under the protection of nitrogen and carbon dioxide, 1 kg of slag from the pyrometallurgical treatment of waste lithium batteries was crushed to obtain slag powder;

[0129] The slag powder and the calcining agent (by mass percentage, 7.5% NaCl-23.9% KCl-68.6% ZnCl2) were mixed according to the formula (calcining agent anion / Li + ) in a molar ratio of 6:1, the mixture was mixed and ground to about 100 mesh, and then cation exchange resin IR200 was added in a mass ratio of cation exchanger to the total amount of slag powder and roasting agent of 1:15 to obtain a mixture.

[0130] (2) Heat treatment

[0131] The mixture obtained in step (1) was treated by microwave at 210°C for 20 min.

[0132] (3) Grinding and screening

[0133] After the microwave treatment, the mixed powder was cooled to room temperature and then subjected to secondary grinding for 10 min. The secondary ground powder was sieved through a 200-mesh circular vibrating sieve to obtain undersize powder.

[0134] (4) Extraction

[0135] The powder under the sieve was mixed with water at a liquid-to-solid mass ratio of 10:1, stirred at 150 r / min at 60°C for 30 minutes, and the leachate was allowed to stand and naturally cool to room temperature before being filtered and separated to obtain a filtrate and a filter residue.

[0136] The lithium extraction rate was calculated to be 93.58%.

[0137] Example 6

[0138] The only difference from Example 1 is that the cation exchanger is replaced by cation exchange resin IR120.

[0139] The lithium extraction rate was calculated to be 94.75%.

[0140] Example 7

[0141] The only difference from Example 1 is that the amount of the cation exchanger is controlled so that the mass ratio of the cation exchanger to the total amount of the slag powder and the roasting agent is 1:5.

[0142] The lithium extraction rate was calculated to be 93.68%.

[0143] Example 8

[0144] The only difference from Example 1 is that the calcining agent is replaced by 10.0% NaCl-15.1% KCl-74.9% ZnCl2 (by mass percentage).

[0145] The lithium extraction rate was calculated to be 90.1%.

[0146] Example 9

[0147] The only difference from Example 1 is that the calcining agent is replaced by 7.5% NaCl-23.9% KCl-68.6% ZnCl2 (by mass percentage).

[0148] The lithium extraction rate was calculated to be 90.7%.

[0149] Example 10

[0150] The only difference from Example 1 is that the amount of the calcining agent used is such that the molar ratio of (calcining agent anion / Li+) is 5:1.

[0151] The lithium extraction rate was calculated to be 94.3%.

[0152] Example 11

[0153] The only difference from Example 1 is that the amount of the calcining agent used is such that the molar ratio of (calcining agent anion / Li+) is 7:1.

[0154] The lithium extraction rate was calculated to be 94.62%.

[0155] Example 12

[0156] The only difference from Example 1 is that the cation exchanger is replaced by cation exchange resin IR200.

[0157] The lithium extraction rate was calculated to be 93.42%.

[0158] Example 13

[0159] The only difference from Example 1 is that the cation exchanger is replaced by a macroporous strongly acidic styrene-based cation exchange resin.

[0160] The lithium extraction rate was calculated to be 94.5%.

[0161] Example 14

[0162] The only difference from Example 1 is that the amount of the cation exchanger is controlled so that the mass ratio of the cation exchanger to the total amount of the slag powder and the roasting agent is 1:7.

[0163] The lithium extraction rate was calculated to be 93.56%.

[0164] Example 15

[0165] The only difference from Example 1 is that the amount of the cation exchanger is controlled so that the mass ratio of the cation exchanger to the total amount of the slag powder and the roasting agent is 1:8.

[0166] The lithium extraction rate was calculated to be 93.51%.

[0167] Example 16

[0168] The only difference from Example 1 is that the heat treatment temperature is 300°C.

[0169] The lithium extraction rate was calculated to be 88.6%. At higher temperatures, the resin exchange capacity decreased, and the lithium extraction effect decreased.

[0170] Example 17

[0171] The only difference from Example 1 is that the heat treatment temperature is 400°C.

[0172] The lithium extraction rate was calculated to be 64.8%.

[0173] Comparative Example 1

[0174] The only difference from Example 1 is that no calcining agent is introduced in step (1).

[0175] The lithium extraction rate was calculated to be 5.53%.

[0176] Comparative Example 2

[0177] The only difference from Example 1 is that no cation exchanger is introduced in step (1).

[0178] The lithium extraction rate was calculated to be 74.3%.

[0179] In summary, the method of the present invention activates the silicate structure under the catalysis of a cation exchanger and the action of microwaves, so that the lithium ions in the silicate after molten salt can quickly exchange with the cations in the roasting agent. The exchanged lithium ions can react with the anions in the molten salt to form soluble salts, thereby extracting and recycling the lithium through water leaching, with a lithium extraction rate of over 90%. By efficiently recycling and reusing the slag after pyrometallurgical treatment of waste lithium batteries, the pollution problem of the slag after pyrometallurgical treatment of waste lithium batteries can be solved, and the lithium resources in the slag after pyrometallurgical treatment of waste lithium batteries can be recovered to provide raw materials for lithium battery manufacturing, thus realizing the resource reuse of the slag after pyrometallurgical treatment of waste lithium-ion batteries.

[0180] The preferred embodiments of the present disclosure are described in detail above, but the present disclosure is not limited thereto. Within the technical concept of the present disclosure, various simple variations of the technical solution of the present disclosure may be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as disclosed by the present disclosure and fall within the scope of protection of the present disclosure. Industrial Applicability

[0181] The present invention discloses a method of heat-treating pyrometallurgical slag by mixing it with a calcining agent and a cation exchanger containing mixed inorganic salts. Under the action of high temperature, the calcining agent and the cation exchanger are used to transform lithium ions from an insoluble silicate phase into a soluble lithium salt phase, thereby recovering lithium through leaching. This method can efficiently transform lithium ions from an insoluble silicate phase into a soluble lithium salt, has a high conversion rate, is simple in process, and has excellent industrial applicability. In addition, no strong acid or alkali is required during the extraction process, which reduces acid and alkali consumption, and no acid and alkali waste gas is generated during the process, reducing environmental treatment costs. It is a green and environmentally friendly recovery process.

Claims

1. A method for extracting lithium from waste lithium battery pyrometallurgical slag applied to the full chain of lithium batteries, characterized in that: include: heat-treating a mixture of pyrometallurgical slag, a roasting agent and a cation exchanger, and then leaching the heat-treated material; The calcining agent is a mixed inorganic salt formed by two or more chlorides, the melting point of the calcining agent is 190°C-230°C, the decomposition temperature of the calcining agent is greater than 700°C, and the treatment temperature of the heat treatment is greater than the melting point of the calcining agent and less than the decomposition temperature of the calcining agent.

2. The lithium extraction method according to claim 1, characterized in that: The calcining agent includes sodium chloride, potassium chloride and zinc chloride.

3. The lithium extraction method according to claim 2, characterized in that: Calculated by mass percentage, the calcining agent comprises 1%-70% of sodium chloride, 1%-70% of potassium chloride and 1%-75% of zinc chloride.

4. The lithium extraction method according to claim 2 or 3, characterized in that: Calculated by mass percentage, the calcining agent comprises 7%-11% of sodium chloride, 15%-32% of potassium chloride and 61%-75% of zinc chloride.

5. The lithium extraction method according to any one of claims 2 to 4, characterized in that: The molar ratio of the anions in the calcining agent to the lithium ions in the pyrometallurgical slag is (1-10):

1.

6. The lithium extraction method according to claim 5, characterized in that: The molar ratio of the anions in the calcining agent to the lithium ions in the pyrometallurgical slag is (7-8):

1.

7. The lithium extraction method according to any one of claims 1 to 6, characterized in that: The cation exchanger is selected from at least one of a polymer of 2-acrylic acid and divinylbenzene, ethanesulfonic acid and a styrene-based cation exchange resin.

8. The lithium extraction method according to claim 7, characterized in that: The styrene-based cation exchange resins include cation exchange resin IR120 and cation exchange resin IR200.

9. The lithium extraction method according to claim 7 or 8, characterized in that: The mass ratio of the cation exchanger to the mixed powder of pyrometallurgical slag and roasting agent is 1:5-10.

10. The lithium extraction method according to claim 9, characterized in that: The mass ratio of the cation exchanger to the pyrometallurgical slag is 1:7-8.

11. The lithium extraction method according to any one of claims 1 to 10, characterized in that: The heat treatment is microwave heating.

12. The lithium extraction method according to claim 11, characterized in that: The heating temperature of the microwave heating treatment is 210° C.-230° C., and the treatment time is 15 min-30 min.

13. The lithium extraction method according to any one of claims 1 to 12, characterized in that: After the heat treatment is completed, the product is ground and sieved, and the screened product is subjected to water leaching for lithium extraction, followed by solid-liquid separation.

14. The lithium extraction method according to claim 13, characterized in that: During the water leaching process for lithium extraction, the liquid-to-solid mass ratio of the water leaching is controlled to be 5-50:

1.

15. The lithium extraction method according to claim 13 or 14, characterized in that: The water leaching of lithium is carried out at 25°C-80°C.

16. The lithium extraction method according to any one of claims 13 to 15, characterized in that: The leaching time of the water leaching lithium is 15min-60min.

17. The lithium extraction method according to any one of claims 13 to 16, characterized in that: The water leaching process of lithium is assisted by stirring, and the stirring rate is controlled to be 150r / min-400r / min.

18. The lithium extraction method according to any one of claims 13 to 17, characterized in that: The particle size of the undersize is less than 200 meshes.

19. The lithium extraction method according to any one of claims 13 to 18, characterized in that: After the water leaching of lithium is completed, the leaching solution is allowed to stand or cool to room temperature, and then vacuum filtered to separate the filtrate and the filter residue in the leaching solution.

20. The lithium extraction method according to any one of claims 1 to 19, characterized in that: The preparation process of the mixture includes: firstly crushing the pyrometallurgical slag to obtain slag powder, mixing and grinding the slag powder with the roasting agent, and then mixing it with the cation exchanger.

Citation Information

Patent Citations

  • A process of extracting lithium from lithium ore through calcination with a chloridizing agent and an inorganic base and dissolving out with an organic solvent

    CN105907943A

  • Method for preferentially extracting lithium from waste lithium ion battery and synergistically recovering manganese

    CN112079369A

  • Thermally-driven ion-exchange process for lithium recovery

    CN1157800A

  • High-valued recovery method of waste lithium iron phosphate / sodium iron phosphate battery positive electrode material

    CN115893345A

  • Method for recovering lithium from lithium-containing solution

    JP2019099901A