Method and hub mold for machining hub by means of cold extrusion
Through the cold extrusion processing method, the problems of bubbles, low density and rough surface in the hub manufacturing are solved, efficient and environmentally friendly hub production are achieved, the density and structural strength of the hub are improved, materials and processing steps are saved, and the High quality and safety of the product.
Patent Information
- Application Number
- PCT/CN2023/107373
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-01
- Filing Date
- 2023-07-14
- Publication Date
- 2024-12-05
AI Technical Summary
In the existing hub manufacturing process, there are problems such as bubbles, low density, rough surface, poor mechanical properties, and insufficient environmental protection and safety, especially defects caused by casting methods and high-temperature environment and material waste in forging methods.
Using the cold extrusion processing method, the forged metal material is formed from the first mold into a deep cylindrical rough blank through three steps, and then the serial shape is formed from the second mold, and finally the rim is formed in the third mold to ensure that the rim diameter is larger than the rim Diameter to avoid defects and processed at room temperature.
It improves the density and structural strength of the wheel hub, surface finish, saves raw materials and processing equipment, avoids defects such as cracks and pores, and improves production efficiency and overall product performance.
Smart Images

Figure CN2023107373_05122024_PF_FP_ABST
Abstract
Description
Method for cold extrusion processing wheel hub and wheel hub mold Technical Field
[0001] The invention relates to the technical field of cold extrusion, in particular to a method for cold extrusion processing a wheel hub and a wheel hub die. Background Art
[0002] At present, there are many ways to manufacture wheels, but the mainstream manufacturing processes are casting, forging and spinning.
[0003] The casting method uses gravity or low pressure to pour the alloy solution into the mold. After forming, it is completed through mechanical processing and surface coating. The advantages are low cost and high production efficiency, but the disadvantages are that it cannot eliminate the defects caused by casting, it is easy to produce bubbles, low density, rough surface, poor comprehensive mechanical properties, and is not environmentally friendly.
[0004] Forging is a process that uses a forging machine to apply pressure to a metal blank, causing it to plastically deform to a specific shape and size, and then spin the rim. Conventional forging production is performed while the metal is hot. While this method offers good product reliability, it also carries high production temperatures, high risks, low raw material utilization, significant material loss, multiple steps, and high subsequent processing costs.
[0005] The existing wheel hub generally has a rim smaller than the spokes, which may cause defects such as foreign matter easily being mixed in the intersection area, weak bonding, folding, cracks, etc.
[0006] Summary of the Invention
[0007] The present invention aims to solve the technical problems of easy generation of bubbles, low density, rough surface, poor comprehensive mechanical properties and environmental pollution in the existing wheel hub casting process. It provides a method for cold extrusion processing of wheel hubs with low pollution and low risk in forging production environment, high utilization rate of product raw materials, low material loss and low subsequent processing cost, and makes the wheel rim larger than the spoke to avoid problems such as breakage, wrinkling, peeling and entrapment of foreign objects in the wheel rim during the step of making the spoke shape.
[0008] For the purpose of the present invention, the following technical solutions are adopted:
[0009] A method for cold extrusion processing a wheel hub, comprising the following steps:
[0010] S1. Deep cylindrical blank forming: A round forgeable metal material is placed in a first die. The first die uses a cold extrusion process to extrude the round forgeable metal material into a U-shaped deep cylindrical blank with a downward opening. The upper portion of the deep cylindrical blank serves as the wheel spoke, and the lower portion of the deep cylindrical blank serves as the wheel rim. The wheel rim diameter of the deep cylindrical blank is larger than the wheel rim diameter of the deep cylindrical blank. Finally, the deep cylindrical blank is removed from the first die.
[0011] S2. Secondary rough blank forming: The deep cylindrical rough blank is placed in the second die, and the second die is used to extrude the deep cylindrical rough blank into a secondary rough blank with the desired spoke shape by a cold extrusion process; spoke notches are formed on both the upper and lower sides of the spoke center of the secondary rough blank; and extrusion steps are formed on the outer wall of the wheel rim of the secondary rough blank; the extruded secondary rough blank is removed from the second die;
[0012] S3. Hub forming: The sub-rough blank is turned 180 degrees and placed in the third die. The third die first preliminarily shapes the rim of the sub-rough blank through a cold extrusion process, making the rim flared; then the top of the rim is cold extruded and bent outward to finally obtain a finished hub in the shape of a rim.
[0013] Compared to existing technologies, this method extrudes forged metal material through a first die to produce a deep cylindrical rough blank with a protruding rim shape. This is then cold-extruded through a second die to create the spoke shape, and then through a third die to create the rim shape. This method uses dies throughout the entire cold extrusion process to produce the finished wheel hub, resulting in extremely high material utilization and a high product qualification rate. Furthermore, production is performed at room temperature, making it safe and environmentally friendly. The resulting wheels exhibit excellent consistency and high overall mechanical properties.
[0014] 1. Compared with the casting method, the wheel hub produced by the cold extrusion processing method provided by the present application has a higher density and a significantly improved structural strength; the surface of the wheel hub produced by the casting method is usually rough and needs to be processed again, while the wheel hub produced by the cold extrusion processing method of the present application has a better surface finish, the surface finish can usually reach above 0.4, does not require further processing, has a higher structural strength, and is of better quality.
[0015] 2. Since the forging method cannot directly forge the spoke shape, it will cause a large amount of raw materials to be wasted. The method of cold extrusion processing hub provided in the present application can greatly save raw materials for producing hubs. In addition, the method of cold extrusion processing hub provided in the present application can also eliminate the step of using processing equipment to mill the spoke shape of the hub blank, which can save equipment costs and labor costs. The hub produced by the method of cold extrusion processing hub provided in the present application will not destroy the streamline of the raw materials, can obtain better structural strength and mechanical properties, and will not have defects such as cracks, pores, folds or non-metallic inclusions.
[0016] 3. In the present application, a forgeable metal material is extruded through a first die to obtain a deep cylindrical blank including a protruding rim shape. The deep cylindrical blank with a protruding rim shape can facilitate the production of the spoke shape and can avoid breakage, wrinkling, peeling and inclusion of foreign matter at the rim position during the step of producing the spoke shape. The wheel hub produced by the cold extrusion wheel hub processing method of the present application has smoother streamlines, high structural strength, good integrity and better comprehensive mechanical properties.
[0017] 4. The product of this application has few production processes. The wheel hub completed by three-step extrusion only needs a small amount of fine processing to complete the process, which can effectively improve production efficiency and save manpower and material resources.
[0018] Preferably, the ratio of the rim diameter of the deep cylindrical blank to the rim diameter of the deep cylindrical blank is between 1.09 and 1.15. Properly setting the rim diameter to the rim diameter can effectively reduce the possibility of unreasonable rim streamlines in step two, improve the overall strength of the finished product, and have great practical value.
[0019] A cold extrusion wheel hub mold includes the first mold, the second mold and the third mold in the above-mentioned cold extrusion wheel hub method; the first mold includes a first upper mold, a first lower mold, a first ejector pin and a first cavity support seat; the first cavity support seat is hollow and the hollow portion of the first cavity support seat forms the first wheel hub cavity; the first upper mold and the first lower mold cooperate with each other and simultaneously cold extrude toward the middle to obtain a deep cylindrical blank including a protruding rim shape, so that the rim diameter of the deep cylindrical blank is larger than the rim diameter of the deep cylindrical blank, and the deep cylindrical blank is ejected from the first mold by the first ejector pin. By making the rim diameter of the deep cylindrical blank larger than the rim diameter of the deep cylindrical blank, it is possible to avoid the occurrence of rim breakage, wrinkles, peeling and inclusion of foreign matter in the step of making the spoke shape, so that the produced wheel hub has smoother streamlines, higher structural strength, better integrity and better comprehensive mechanical properties.
[0020] Preferably, the inner circumferential wall of the first cavity support seat is provided with a circumferentially formed annular bevel that slopes from top to bottom and from outside to inside. The formed annular bevel facilitates better shaping of the spokes and further facilitates achieving a larger rim diameter than the rim diameter of the deep cylindrical rough blank. This prevents breakage, wrinkling, peeling, and inclusion of debris at the rim during the spoke shaping process, resulting in a smoother streamlined hub, higher structural strength, better integrity, and better overall mechanical properties.
[0021] Preferably, a first annular recess is circumferentially provided on the outer peripheral wall of the first lower die; a first rim cavity is formed between the annular recess and the first hub cavity; the first upper die and the first lower die are simultaneously driven to extrude and form a deep cylindrical cavity containing the shape of the rim in the combined state; the first ejector pin is lifted and connected to the first lower die; during ejection, the first ejector pin passes through the first lower die from bottom to top and is pushed onto the deep cylindrical blank. The deep cylindrical blank is formed by cold extrusion in cooperation with the first upper die and the first lower die, and the deep cylindrical blank is conveniently ejected by the first ejector pin, thereby facilitating the transfer of the deep cylindrical blank to the next process.
[0022] Preferably, the second mold includes a second upper mold, a second lower mold, a second push rod and a second cavity support seat; the second cavity support seat is hollow and the hollow part of the second cavity support seat forms a second hub cavity; the second upper mold and the second lower mold cooperate with each other to cold extrude to obtain a rough blank with the required spoke shape.
[0023] Preferably, the inner circumferential wall of the second cavity support seat is provided with an annular step surface from top to bottom and from outside to inside. The annular step surface facilitates better squeezing of the spokes at the step, thereby facilitating better shaping of the spokes, improving strength and aesthetics.
[0024] Preferably, the bottom surface of the second upper die is provided with a convex strip corresponding to the shape of the wheel spoke; the top surface of the second lower die is provided with a strip-shaped concave surface matching the convex strip; a second annular recess is circumferentially provided on the outer peripheral wall of the second lower die; a second rim cavity is formed between the second annular recess and the second hub cavity; a protruding push rod is provided on the top of the second ejector pin; the second upper die, the second lower die, and the second ejector pin are combined to press the deep cylindrical blank into a secondary blank with the shape of the wheel spoke. The downward pressure of the second upper die facilitates the cold extrusion of the wheel spoke.
[0025] Preferably, the third mold includes a third upper mold I, a third upper mold II, a third lower mold, at least two sliders arranged on the side and a third push rod. The secondary rough blank is placed on the third lower mold and fixed using the sliders arranged on the side. The third upper mold II is sleeved on the third upper mold I. The rim is first preliminarily shaped by pressing down by the third upper mold I, and then the top end of the rim is cold-extruded by pressing down by the third upper mold II to finally obtain a finished wheel hub in the shape of a rim. The third push rod is lifted and connected to the middle part of the third lower mold. When ejecting, the third push rod passes through the third lower mold from bottom to top and pushes onto the finished wheel hub to take out the finished wheel hub.
[0026] Preferably, the top surface of the third lower mold is provided with a support surface corresponding to the shape of the wheel spoke; the lower part of each slider is provided with a slider step surface matching the shape of the annular step surface; the upper part of the slider is provided with a rim step surface extending from top to bottom and from outside to inside, the top of the rim step surface forms a rim end forming recess, and the rim step surface matches the rim; the outer peripheral wall of the third upper mold I is provided with a rim matching surface extending from top to bottom and from outside to inside; the bottom surface of the third upper mold I is provided with a spoke cavity surface identical to the top surface of the second lower mold; The third upper mold II is sleeved outside the third upper mold I and is located above the third upper mold II. A ring-shaped rim end forming recess is circumferentially provided at the bottom of the third upper mold II. The third upper mold II is pressed downward so that the rim end forming recess is pressed onto the rim end forming recess. The rim end is extruded and shaped by the rim end forming recess and the rim end forming recess cooperating with the rim end forming recess. The third mold also includes a third ejector pin, which is connected to the middle part of the third lower mold by lifting. During ejection, the third ejector pin passes through the third lower mold from bottom to top and is pushed onto the finished wheel hub. By inverting the rough blank onto the third mold and through the extrusion fit between the third upper mold I and the third lower mold, the rim is better shaped and expanded outward, thereby improving the connection strength and the use effect.
[0027] To sum up, the advantages of the method of the present application are that the hub has higher density, significantly improved structural strength, better surface finish of the hub, surface finish can usually reach above 0.4, no further processing is required, structural strength is also higher, and quality is better; the production of the hub can greatly save raw materials, and can also save the step of using processing equipment to mill the hub blank into the spoke shape, which can save equipment costs and labor costs. The hub will not destroy the streamline of the raw material, can obtain better structural strength and mechanical properties, and will not have defects such as cracks, pores, folds or non-metallic inclusions; the hub streamlines more smoothly, has high structural strength, good integrity, and better comprehensive mechanical properties; there are fewer production processes, and the hub completed by three-step extrusion only requires a small amount of fine processing to complete the process, which can effectively improve production efficiency and save manpower and material resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] FIG1 is a flow chart of a method for cold extrusion processing a hub according to the present invention.
[0029] FIG2 is a schematic diagram of step 1 in the method for cold extrusion processing a wheel hub of the present invention.
[0030] FIG3 is a planar structural diagram of a deep cylindrical blank (the rim is larger than the wheel rim) of the present invention.
[0031] FIG4 is a three-dimensional structural diagram of a deep cylindrical blank (the rim is larger than the wheel rim) of the present invention.
[0032] FIG5 is a schematic diagram of step 2 in the method for cold extrusion processing a wheel hub according to the present invention.
[0033] FIG6 is a schematic diagram of step three in the method for cold extrusion processing a wheel hub of the present invention.
[0034] FIG7 is an exploded view of step three in the method for cold extrusion processing of a wheel hub according to the present invention.
[0035] FIG8 is a schematic structural diagram of a finished wheel hub according to the present invention.
[0036] FIG9 is a structural cross-sectional view of an existing deep cylindrical blank (the wheel rim is smaller than the wheel rim).
[0037] FIG. 10 is a diagram showing the principle of streamline formation during the spoke forming process obtained by conventional extrusion.
[0038] Wherein: 1. Deep cylindrical rough blank; 101. Wheel rim; 102. Spoke; 103. Rim; 110. First upper die; 120. First lower die; 130. First ejector pin; 140. First cavity support seat; 150. Forming annular slope; 170. First annular recess; 180. First rim cavity; 2. Second rough blank; 210. Second upper die; 2101. Protruding strip; 220. Second lower die; 2201. Strip concave surface; 2202. Second annular recess; 2203. Second rim cavity; 230. Second ejector pin; 2301. Ejector pin protrusion; 240. Second cavity support seat; 250, annular step surface; 3, finished wheel hub; 310, third upper mold I; 3101, rim mating surface; 320, third lower mold; 3201, support surface; 330, slider; 3301, slider step surface; 3302, rim step surface; 340, third push rod; 350, third upper mold II; 3501, rim end forming concave surface; 3502, rim end forming notch. DETAILED DESCRIPTION
[0039] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0040] It should be noted that although the system diagrams illustrate functional module divisions and the flowcharts illustrate logical sequences, in certain circumstances, the steps shown or described may be performed in a sequence that differs from the module divisions in the system or the sequence in the flowcharts. The terms "first," "second," and so on, in the specification, claims, and drawings, are used to distinguish similar items and are not necessarily used to describe a specific sequence or precedence.
[0041] As shown in FIG9 and FIG10 , the existing wheel hub has a rim 101 that is smaller than the spokes 102 , which may result in defects such as foreign matter being easily mixed in the intersection area, weak bonding, folding, and cracks.
[0042] The present invention provides a method for cold extrusion processing of a wheel hub, which can improve the yield rate of the product and is produced under normal temperature environment, and the safety is significantly improved compared with high temperature environment.
[0043] As shown in Figures 1 to 8, the method for cold extrusion processing of a wheel hub includes the following steps:
[0044] S1. Deep cylindrical blank forming: take a forgeable metal material and put it into the first mold. Take a round cake-shaped forgeable metal material and put it into the first mold. The first mold uses a cold extrusion process to extrude the round cake-shaped forgeable metal material into a U-shaped deep cylindrical blank 1 with an opening downward. The upper part of the deep cylindrical blank 1 is the spoke 102, and the lower part of the deep cylindrical blank is the rim 102; and the diameter of the rim 101 of the deep cylindrical blank 1 is larger than the diameter of the rim 103 of the deep cylindrical blank 1. Finally, the deep cylindrical blank 1 is taken out from the first mold. The first mold includes a first upper mold 110, a first lower mold 120, a first ejector pin 130, and a first cavity support seat 140; the first cavity support seat 140 is hollow, and the hollow portion of the first cavity support seat 140 forms a first hub cavity; the first upper mold 110 and the first lower mold 120 cooperate with each other and simultaneously cold extrude toward the middle to obtain a deep cylindrical rough blank 1 including a protruding wheel rim 101, so that the diameter of the wheel rim 101 of the deep cylindrical rough blank 1 is larger than the diameter of the wheel rim 103 of the deep cylindrical rough blank 1, and the deep cylindrical rough blank 1 is ejected from the first mold by the first ejector pin 130;
[0045] S2, forming the secondary rough blank: put the deep cylindrical rough blank 1 into the second mold, put the deep cylindrical rough blank 1 into the second mold, and the second mold extrude the deep cylindrical rough blank 1 into the desired spoke shape through the cold extrusion process; the spokes 102 of the secondary rough blank 2 are extruded on both the upper and lower sides of the center to form spoke notches; and the outer wall of the rim 101 of the secondary rough blank 2 is formed into an extrusion step; the extruded secondary rough blank 2 is taken out from the second mold. The second mold includes a second upper mold 210, a second lower mold 220, a second ejector pin 230 and a second cavity support seat 240; the second cavity support seat 240 is hollow and the hollow part of the second cavity support seat 240 forms a second hub cavity; the secondary rough blank 2 in the desired spoke 102 shape is obtained by cold extrusion with the cooperation of the second upper mold 210 and the second lower mold 220;
[0046] S3, wheel hub forming: Flip the secondary blank 2 180 degrees and place it in the third die. Flip the secondary blank 2 180 degrees and place it in the third die. The third die will initially shape the rim 103 of the secondary blank 2 by cold extrusion, making the rim 103 flared. Then, the top of the rim 103 will be cold extruded and bent outward to form a finished wheel hub in the shape of the rim 103. The third die includes: a third upper die I 310, a third lower die 320, and at least two sliders 330 provided on the side. The secondary blank 2 is placed on the third lower die 320 and fixed by the sliders 330 provided on the side. The third upper die II 350 is sleeved on the third upper die I 310. The rim 103 is initially shaped by pressing downwards by the third upper die I 310. Then, the end of the rim 103 is cold extruded by pressing downwards by the third upper die II 350, to finally form a finished wheel hub 3 in the shape of the rim 103.
[0047] As shown in Figures 9 and 10 , in the prior art, the diameter of the rim 101 of the deep cylindrical blank 1 extruded is equal to or smaller than the diameter of the rim 103. This approach can easily cause the outer ring of the second die to press against the inner ring of the hub top when the second die is extruding the hub, causing the spokes 102 to be squeezed toward the rim 101, resulting in a thinner rim 101 and, in turn, causing the metal material at the rim 101 to be squeezed and folded. In the prior art, the streamlines of the extruded spokes 102 intersect, disrupting the overall streamlines of the product. Defects such as inclusions, weak bonding, folds, and cracks are likely to occur at the intersection, resulting in low structural strength and poor durability. Conversely, in the case of a deep cylindrical blank 1 with a rim 101 diameter greater than the rim 103 diameter, even if the spokes 102 are squeezed toward the rim 101, this does not affect the intersection of the spokes 102 and rim 101, nor does it affect the overall structural strength.
[0048] The specific implementation steps of cold extrusion processing wheel hub are as follows:
[0049] As shown in Figures 2 to 4, in the first step, a forgeable metal material of corresponding mass is selected according to the size and shape of the wheel hub, and the forgeable metal material is placed vertically in the first mold. The first mold is composed of a first upper mold 110 and a first lower mold 120. The first lower mold 120 and the first upper mold 110 are extruded toward the middle at the same time, and when combined, a deep cylindrical cavity containing the shape of the rim 101 is formed. During the extrusion of the conventional first lower mold 120 and the first upper mold 110, only the first upper mold 110 is pressed down, while the first lower mold 120 is fixed. This results in a higher tonnage requirement for the first upper mold 110. However, by performing the simultaneous extrusion action from top to bottom, the tonnage requirement for the first upper mold 110 is lower. At the same time, the first lower mold 120 and the first upper mold 110 extrude the wheel hub, achieving a better shaping effect. The forgeable metal material is extruded using the first lower die 120 and the first upper die 110 to obtain a deep cylindrical blank 1 including the shape of a rim 101. The diameter of the rim 101 of the deep cylindrical blank 1 is larger than the diameter of the rim 103. Processing a blank with a larger rim 101 is beneficial to the subsequent step of processing the shape of the spokes 102. The larger diameter of the rim 101 can reduce the possibility of streamline intersection, weak bonding, folding and cracking at the edge, and can improve the mechanical strength of the product.
[0050] As shown in Figure 2, in the first mold of the wheel hub mold, a forming annular inclined surface 150 is circumferentially provided on the inner circumferential wall of the first cavity support seat 140, which is inclined from top to bottom and from outside to inside. The forming annular inclined surface 150 facilitates better shaping of the spokes 102 and further facilitates ensuring that the diameter of the rim 101 of the deep cylindrical blank 1 is larger than the diameter of the rim 103 of the deep cylindrical blank 1. This prevents the rim 101 from breaking, wrinkling, peeling, and inclusion of foreign matter during the step of shaping the spokes 102, resulting in a smoother streamlined wheel hub with higher structural strength, better integrity, and better overall mechanical properties.
[0051] As shown in Figure 2, a first annular recess 170 is circumferentially provided on the outer peripheral wall of the first lower die 120; a first rim cavity 180 is formed between the first annular recess 170 and the first hub cavity; the first upper die 110 and the first lower die 120, when combined, form a deep cylindrical cavity in the shape of the wheel rim 101. The first ejector pin 130 is connected to the first lower die 120 by a lifting mechanism. During ejection, the first ejector pin 130 passes through the first lower die 120 from bottom to top and pushes onto the deep cylindrical blank 1. The deep cylindrical blank 1 is formed by cold extrusion through the cooperation of the first upper die 110 and the first lower die 120, and the deep cylindrical blank 1 is easily ejected by the first ejector pin 130, thereby facilitating the transfer of the deep cylindrical blank 1 to the next process.
[0052] In the first step, the forgeable metal material is extruded through the first die to obtain a deep cylindrical rough blank 1 including the shape of a protruding rim 101. The deep cylindrical rough blank 1 with the shape of a protruding rim 101 can facilitate the production of the shape of the spokes 102, and can avoid the occurrence of breakage, wrinkles, peeling and entrapment of foreign matter at the position of the rim 101 during the step of producing the shape of the spokes 102. The method of cold extrusion processing of the hub in this application produces a hub with smoother streamlines, high structural strength, good integrity and better comprehensive mechanical properties.
[0053] As shown in Figure 5, in the second step, the deep cylindrical blank 1 is placed in the second lower mold 220 of the second mold. The bottom of the second upper mold 210 of the second mold is provided with a convex strip 2101 corresponding to the shape of the spoke 102. The shape of the mold can be flexibly changed according to the shape of the spoke 102. The second upper mold 210 and the second lower mold 220 are used to extrude a sub-blank 2 including the shape of the spoke 102. The one-time formed sub-blank 2 has smoother streamlines and higher structural strength, and will not have defects such as the intersection of material streamlines.
[0054] In the second mold of the wheel hub mold, an annular step surface 250 is circumferentially provided on the inner circumference of the second cavity support seat 240. The annular step surface 250 facilitates better squeezing of the spokes 102 at the step, thereby facilitating better shaping of the spokes 102, improving strength and aesthetics. The bottom surface of the second upper mold 210 is provided with a convex strip 2101 corresponding to the shape of the spoke 102; the top surface of the second lower mold 220 is provided with a strip-shaped concave surface 2201 matching the convex strip 2101; a second annular recess 2202 is circumferentially provided on the outer peripheral wall of the second lower mold 220; a second rim cavity 2203 is formed between the second annular recess 2202 and the second hub cavity; a protruding pusher head 2301 is provided on the top of the second ejector pin 230 of the second lower mold 220; the second upper mold 210, the second lower mold 220, and the second ejector pin 230 are combined to press the deep cylindrical blank 1 into a secondary blank 2 in the shape of the spoke 102. The downward pressure of the second upper mold 210 facilitates the cold extrusion of the spoke 102.
[0055] As shown in Figures 6 and 7, in the third step, since the shape of the wheel hub has been basically completed in the stage of the secondary rough blank 2, in the third stage of the process, only the shape of the rim 103 needs to be machined. The secondary rough blank 2 is fixed to the third lower die 320 and fixed using a slider 330 provided on the side. The third upper die II 350 is sleeved on the third upper die I 310. The rim 103 is first initially shaped by pressing downward with the third upper die I 310, and then the end of the rim 103 is cold-extruded by pressing downward with the third upper die II 350, ultimately obtaining the finished wheel hub 3 in the shape of the rim 103. Furthermore, after obtaining the finished wheel hub 3 in the shape of the rim 103, the wheel hub still needs to undergo a small amount of finishing processing such as deburring, drilling bolt holes, and surface coating.
[0056] In the processing of forged wheels, the forming method is usually through spinning and then turning. In the processing of cast wheels, the top of the rim is prone to fracture due to insufficient density and low strength. However, through the double extrusion method of the present application, the lower part of the rim 103 is initially shaped as a whole by the third upper die I 310, and the top of the rim 103 is extruded and formed by the third upper die II 350. The pressure values of the two times can be different, which facilitates better shaping of the top of the rim 103 while also ensuring the integrity and precision requirements of the rim 103.
[0057] As shown in Figures 6 to 8, in the third mold of the hub mold, the top surface of the third lower mold 320 is provided with a support surface 3201 corresponding to the shape of the spoke 102; the lower part of each slider 330 is provided with a slider step surface 3301 matching the shape of the annular step surface 250; the upper part of the slider 330 is provided with a rim step surface 3302 extending from top to bottom and from outside to inside, and the top of the rim step surface 3302 forms a rim end forming concave surface 3501, and the rim step surface 3302 cooperates with the rim 103; the outer peripheral wall of the third upper mold I310 is circumferentially provided with a rim mating surface 3101 extending from top to bottom and from outside to inside; the bottom surface of the third upper mold I310 is provided with a spoke cavity surface identical to the top surface of the second lower mold 220. The third upper mold II 350 is sleeved outside the third upper mold I 310 and located above it. A ring-shaped rim end-forming concave surface 3501 is circumferentially arranged at the bottom of the third upper mold II 350. The third upper mold II 350 is pressed downward, pressing the rim end-forming concave surface 3501 against the rim end-forming recess 3502. The rim end-forming concave surface 3501 cooperates with the rim end-forming recess 3502 to squeeze and shape the end of the rim 103. By placing the semi-rough blank 2 upside down on the third mold and through the extrusion fit between the third upper mold I 310 and the third lower mold 320, the rim 103 is better shaped and expanded outward, thereby improving the connection strength and performance. The third mold further includes a third ejector pin 340, which is connected to the middle portion of the third lower mold 320 and is movable upward. During ejection, the third ejector pin 340 passes through the third lower mold 320 from bottom to top and is pushed onto the finished wheel hub 3. The lifting of the third ejector pin 340 facilitates ejection of the finished wheel hub 3.
[0058] The wrought metal material commonly used is 6061 aluminum alloy or 6082 aluminum alloy. Aluminum alloy is a common material for wheels and offers advantages such as high structural strength. Aluminum alloy has a low density, resulting in lightweight wheels with high structural strength, which contributes to lightweight vehicle production. Other alloy materials, such as wrought alloys that meet the wheel requirements, can also be used.
[0059] As shown in Figures 6 and 7, there can be two sliders 330, each having a semicircular cross-section. By combining the two sliders 330 and cooperating with the third lower die 320, the semi-rough blank 2 can be well fixed. By extruding the two sliders 330 and the third upper die I 310, a finished wheel hub 3 in the shape of the rim 103 can be obtained. The number of sliders 330 can also be three or more. By cooperating with the three sliders 330, the semi-rough blank 2 is fixed to the third lower die 320. Since the sliders 330 and the third upper die I 310 both have the shape of the rim 103, the semi-rough blank 2 is cold-extruded through the third upper die I 310 to obtain a finished wheel hub 3 in the shape of the rim 103. The provision of three sliders 330 can shorten the formation of the sliders 330 and improve production efficiency.
[0060] The ratio of the diameter of the rim 101 of the deep cylindrical blank 1 to the diameter of the rim 103 is between 1.09 and 1.15. The ratio of the diameter of the rim 101 of the deep cylindrical blank 1 to the diameter of the rim 103 can be 1.09 or 1.15. By reasonably setting the size of the diameter of the rim 101 and the diameter of the rim 103, the possibility of unreasonable streamlines of the rim 101 in process two can be effectively reduced, and the overall strength of the finished product can be improved, which has great practical value.
[0061] The cold extrusion method for wheel hubs provided in this embodiment requires only three cold extrusion operations at room temperature on a wrought alloy material to produce the finished wheel hub 3. Compared to conventional casting and forging-spinning processes, the cold extrusion method for wheel hubs provided in this embodiment can significantly improve wheel hub production efficiency, provide safe and environmentally friendly production at room temperature, significantly save raw materials, reduce process steps, lower costs, and improve quality, achieving technological innovation in wheel hub production and possessing high economic value.
[0062] The present invention also provides an electronic device, comprising: a memory, a processor, and a computer program stored on the memory and executable on the processor, wherein the processor implements the method for cold extrusion processing of a wheel hub as described above when executing the computer program. The processor and the memory may be connected via a bus or other means. The memory, as a non-transitory computer-readable storage medium, may be used to store non-transitory software programs and non-transitory computer executable programs. In addition, the memory may include a high-speed random access memory, and may also include a non-transitory memory, such as at least one disk storage device, a flash memory device, or other non-transitory solid-state storage device. In some embodiments, the memory may optionally include a memory remotely located relative to the processor, and these remote memories may be connected to the processor via a network. Examples of the above-mentioned network include, but are not limited to, the Internet, an intranet, a local area network, a mobile communication network, and combinations thereof.
[0063] To sum up, the advantages of this application are that the hub has higher density, significantly improved structural strength, better surface finish of the hub, surface finish can usually reach above 0.4, no need for reprocessing, higher structural strength and better quality; the production of the hub can greatly save raw materials, and can also save the step of using processing equipment to mill the hub blank into the spoke shape, which can save equipment costs and labor costs. The hub will not destroy the streamline of the raw material, can obtain better structural strength and mechanical properties, and will not have defects such as cracks, pores, folds or non-metallic inclusions; the hub streamlines more smoothly, has high structural strength, good integrity, and better comprehensive mechanical properties; there are fewer production processes, and the hub completed by three-step extrusion only requires a small amount of fine processing to complete the process, which can effectively improve production efficiency and save manpower and material resources.
[0064] The above is a specific description of the preferred implementation of the present invention, but the present invention is not limited to the above-mentioned implementation mode. Those skilled in the art can make various equivalent modifications or substitutions without violating the spirit of the present invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of the present invention, such as using the method or equipment provided in this application for warm extrusion or hot forging.
[0065] The specific embodiments of the present invention described above do not limit the scope of protection of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the scope of protection of the claims of the present invention.
Claims
1. A method for cold extrusion processing of a wheel hub, characterized in that: The following steps are involved: S1. Deep cylindrical blank forming: a round forgeable metal material is put into a first die, and the first die extrudes the round forgeable metal material into a U-shaped deep cylindrical blank (1) with an opening facing downward by a cold extrusion process, wherein the upper part of the deep cylindrical blank (1) is a wheel spoke (102), and the lower part of the deep cylindrical blank (1) is a wheel rim (103); and the diameter of the wheel rim (101) of the deep cylindrical blank (1) is larger than the diameter of the wheel rim (103) of the deep cylindrical blank (1), and finally the deep cylindrical blank (1) is taken out from the first die; S2, forming a secondary rough blank: placing the deep cylindrical rough blank (1) into a second mold, and using the second mold to extrude the deep cylindrical rough blank (1) through a cold extrusion process to obtain a secondary rough blank (2) in the shape of a desired spoke (102); extruding spoke notches on both the upper and lower sides of the center of the spoke (102) of the secondary rough blank (2); and forming an extrusion step on the outer wall of the rim (101) of the secondary rough blank (2); and taking out the extruded secondary rough blank (2) from the second mold; S3, wheel hub molding: the secondary rough blank (2) is turned 180 degrees and placed in a third mold. The third mold first preliminarily shapes the rim (103) of the secondary rough blank (2) by a cold extrusion process, so that the rim (103) is in a flared shape; then the top of the rim (103) is cold extruded and bent outward to finally obtain a finished wheel hub (3) in the shape of the rim (103).
2. The method for cold extrusion processing of a wheel hub according to claim 1, characterized in that: The ratio of the diameter of the rim (101) of the deep cylindrical blank (1) to the diameter of the rim (103) of the deep cylindrical blank (1) is between 1.09 and 1.
15.
3. A cold extrusion wheel hub die, characterized in that: The method comprises a first die, a second die and a third die in the method for cold extrusion processing of a wheel hub as described in any one of claims 1-2; the first die comprises a first upper die (110), a first lower die (120), a first push rod (130) and a first cavity support seat (140); the first cavity support seat (140) is hollow and the hollow part of the first cavity support seat (140) forms a first wheel hub cavity; a deep cylindrical blank (1) including a protruding rim shape is obtained by cold extruding the first upper die (110) and the first lower die (120) in cooperation with each other and simultaneously in the middle, so that the diameter of the rim (101) of the deep cylindrical blank (1) is larger than the diameter of the spoke (102) of the deep cylindrical blank (1), and the deep cylindrical blank (1) is ejected from the first die by the first push rod (130).
4. The cold extrusion wheel hub die according to claim 3, characterized in that: The inner peripheral wall of the first cavity support seat (140) is circumferentially provided with a molding annular inclined surface (150) which is inclined from top to bottom and from outside to inside.
5. The cold extrusion wheel hub die according to claim 3, characterized in that: A first annular recess (170) is circumferentially provided on the outer peripheral wall of the first lower die (120); a first rim cavity (180) is formed between the annular recess (170) and the first hub cavity; the first upper die (110) and the first lower die (120) are simultaneously driven to extrude to form a deep cylindrical cavity containing a rim shape inside the merged state; the first ejector pin (130) is connected to the first lower die (120) in a lifting manner; when ejecting, the first ejector pin (130) passes through the first lower die (120) from bottom to top and is ejected onto the deep cylindrical rough blank (1).
6. The cold extrusion wheel hub die according to claim 3, characterized in that: The second mold comprises a second upper mold (210), a second lower mold (220), a second ejector pin (230) and a second cavity support seat (240); the second cavity support seat (240) is hollow and the hollow portion of the second cavity support seat (240) forms a second hub cavity; the second upper mold (210) and the second lower mold (220) cooperate with each other to cold extrude to obtain a sub-rough blank (2) in the shape of a desired wheel spoke (102).
7. The cold extrusion wheel hub die according to claim 6, characterized in that: An annular step surface (250) is circumferentially arranged on the inner circumferential wall of the second cavity support seat (240) from top to bottom and from outside to inside.
8. The cold extrusion wheel hub die according to claim 6, characterized in that: The bottom surface of the second upper mold (210) is provided with a convex strip (2101) corresponding to the shape of the spoke (102); the top surface of the second lower mold (220) is provided with a strip-shaped concave surface (2201) matching the convex strip (2101); a second annular recess (2202) is circumferentially provided on the outer peripheral wall of the second lower mold (220); a second rim cavity (2203) is formed between the second annular recess (2202) and the second hub cavity; a push rod boss (2301) is provided on the top of the second push rod (230); the second upper mold (210), the second lower mold (220) and the second push rod (230) are combined to press the deep cylindrical rough blank (1) into a sub-rough blank (2) containing the shape of the spoke (102).
9. The cold extrusion wheel hub die according to claim 3, characterized in that: The third mold comprises a third upper mold I (310), a third upper mold II (350), a third lower mold (320), at least two sliders (330) arranged on the side, and a third ejector (340). The secondary rough blank (2) is placed on the third lower mold (320), and the sliders (330) arranged on the side are used to fix the secondary rough blank (2). The third upper mold II (350) is sleeved on the third upper mold I (310); first, the third upper mold I (31 0) is pressed down to preliminarily shape the rim (103), and then the top of the rim (103) is pressed down by the third upper mold II (350) to cold extrude and shape, and finally a finished wheel hub (3) in the shape of the rim (103) is obtained; the third push rod (340) is lifted and connected to the middle part of the third lower mold (320); when ejecting, the third push rod (340) passes through the third lower mold (320) from bottom to top and pushes onto the finished wheel hub (3), and the finished wheel hub (3) is taken out.
10. The cold extrusion wheel hub die according to claim 9, characterized in that: The top surface of the third lower mold (320) is provided with a support surface (3201) corresponding to the shape of the spoke (102); the lower part of each slider (330) is provided with a slider step surface (3301) matching the shape of the annular step surface (250); the upper part of the slider (330) is provided with a rim step surface (3302) extending from top to bottom and from outside to inside, the top of the rim step surface (3302) forms a rim end forming recess (3502), and the rim step surface (3302) matches the rim (103); the outer peripheral wall of the third upper mold I (310) is provided with a rim matching surface (3101) extending from top to bottom and from outside to inside; the bottom surface of the third upper mold I (310) is provided with the same The spoke cavity surface; the third upper mold II (350) is sleeved outside the third upper mold I (310) and is located at the upper part of the third upper mold II (350); the bottom of the third upper mold II (350) is circumferentially provided with an annular rim end forming concave surface (3501); the third upper mold II (350) is pressed downward to press the rim end forming concave surface (3501) onto the rim end forming recess (3502); and the rim end forming recess (3502) cooperates with the rim end forming concave surface (3501) to squeeze and shape the rim (103) end; the third ejector rod (340) is lifted and connected to the middle part of the third lower mold (320); when ejecting, the third ejector rod (340) passes through the third lower mold (320) from bottom to top and is ejected onto the finished wheel hub (3).
Citation Information
Patent Citations
Multiway shaping method of magnesium alloy wheel and mold
CN101474642A
Magnesium alloy wheel forging forming method
CN105014321A
Forged aluminum-alloy wheel rim extrusion molding method
CN108555048A
Forming die and method for wide special-shaped hub
CN115780723A
A labor-saving automobile hub forming method and device
CN1864915A
Cited By
Method for cold extrusion machining of hub and hub mold
CN116618463A
Method of cold extrusion of a wheel hub and wheel hub die
CN116618463B
Hub lip thickening forming device
CN119456762A