Graft polymer, preparation method, binder, positive electrode sheet, secondary battery, and electric apparatus
By using grafted polymers that graft non-fluorine branched polymers on fluorine-containing main chain polymers in secondary batteries, the problems of high cost and poor performance of traditional binders are solved, and high flexibility and fast The liquid absorption rate and low resistance effect improve the battery's circulation capacity retention rate and safety performance.
Patent Information
- Application Number
- PCT/CN2023/123803
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-01
- Filing Date
- 2023-10-10
- Publication Date
- 2024-12-05
AI Technical Summary
The adhesives in existing secondary batteries have high production costs and insufficient production capacity, which are harmful to the environment, and gels are prone to appear during the preparation process, resulting in poor flexibility of the electrode sheet, low adhesion force, low liquid absorption rate and high resistance. It is difficult to meet the market's requirements for battery cost and performance.
Using a graft polymer, by grafting non-fluorine branched polymer on the fluorine-containing main chain polymer, the α crystal form is transformed into a β crystal form, and the β crystal form content of the graft polymer is increased, and the β crystal form content of the graft polymer is combined with the content of the The advantages of fluorine and non-fluorine binders are prepared with high flexibility, excellent liquid absorption rate and low DC impedance.
It improves the flexibility and liquid absorption rate of the pole sheet, reduces the DC impedance growth rate of the battery, improves the circulation capacity retention rate, and improves the dynamic performance and safety performance of the battery.
Smart Images

Figure CN2023123803_05122024_PF_FP_ABST
Abstract
Description
Graft polymer, preparation method, binder, positive electrode sheet, secondary battery and electrical device
[0001] Cross-references
[0002] This application refers to Chinese Patent Application No. 202310638796.2 filed on June 1, 2023, entitled “Grafted polymer, preparation method, binder, positive electrode sheet, secondary battery and electrical device,” which is incorporated into this application in its entirety by reference. Technical Field
[0003] The present application relates to the technical field of secondary batteries, and in particular to a graft polymer, a preparation method, a binder, a positive electrode sheet, a secondary battery, and an electrical device. Background Art
[0004] In recent years, secondary batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields.
[0005] Binders are common materials in secondary batteries, widely used in battery electrodes, separators, and packaging. However, traditional binders have high production costs, insufficient production capacity, and significant environmental hazards. They also tend to gel during the preparation process, resulting in poor slurry stability and high processing costs. The resulting electrodes, produced with these binders, exhibit poor flexibility, low adhesion, slow liquid absorption, high resistance, and low yield rates. Furthermore, the batteries exhibit high DC impedance growth, poor cycle capacity retention, and unstable performance, making them difficult to meet market requirements for battery cost and performance. Therefore, existing binders still need improvement.
[0006] Summary of the Invention
[0007] The present application is made in view of the above-mentioned problems, and its purpose is to provide a grafted polymer that can improve the flexibility of the electrode, increase the liquid absorption rate of the electrode, reduce the DC impedance growth rate of the battery, and improve the cycle capacity retention rate of the battery.
[0008] The first aspect of the present application provides a graft polymer, comprising a main chain polymer and a branched polymer, wherein the main chain polymer comprises a structural unit shown in formula I, and the branched polymer comprises a structural unit shown in formula II.
[0009] The wavy line in Formula I represents the junction position of the main chain polymer and the branched polymer, and R1 and R2 each independently contain hydrogen, fluorine, C containing at least one fluorine atom, 1-3 One or more of the alkyl groups, R3, R4, and R5 each independently contain hydrogen, substituted or unsubstituted C 1-5One or more of the alkyl groups, R6 contains hydrogen, substituted or unsubstituted C 1-5 Alkyl, ester, carboxyl, amide, cyano, hydroxyl, substituted or unsubstituted C 6-30 One or more aromatic groups.
[0010] Grafting non-fluorinated side-chain polymers onto a fluorinated main-chain polymer causes the polymer to undergo a transition from an α- to a β-crystalline phase, increasing the β-crystalline content of the grafted polymer and improving its ferroelectric and piezoelectric properties. Simultaneously, the non-fluorinated side-chain polymers are grafted onto the fluorinated main-chain polymer, leveraging the respective advantages of the fluorinated and non-fluorinated binders and achieving a complementary effect. This grafted polymer binder can improve the flexibility of the electrode, increase the electrode's liquid absorption rate, reduce the battery's DC impedance growth rate, and improve the battery's cycle capacity retention rate.
[0011] In any embodiment, the content of the β crystal form in the graft polymer is 32% to 74%, based on the total content of the α crystal form and the β crystal form in the graft polymer.
[0012] By controlling the content of the β-crystal in the grafted polymer within an appropriate range, the film resistance of the electrode can be reduced.
[0013] In any embodiment, the main chain polymer further comprises a structural unit represented by formula III,
[0014] wherein R7, R8, and R9 independently contain hydrogen, fluorine, or a C 1-3 One or more of alkyl groups.
[0015] In any embodiment, R6 comprises an ester group, a carboxyl group, an amide group, a cyano group, a hydroxyl group, a substituted or unsubstituted C 6-12 One or more aromatic groups.
[0016] The grafted polymer contains ester groups, carboxyl groups, amide groups, cyano groups, hydroxyl groups, substituted or unsubstituted C 6-12 The aromatic functional group can increase the viscosity of the slurry, improve the cohesion and flexibility of the electrode, increase the liquid absorption rate of the electrode, and reduce the DC impedance growth rate of the battery.
[0017] In any embodiment, the mass content of the branched polymer is 1%-30%, optionally 5%-25%, based on the total mass of the grafted polymer.
[0018] The mass content of the branched polymer is within an appropriate range, the electrode has excellent adhesion, cohesion and flexibility, the electrode has low membrane resistance, the electrode has an excellent liquid absorption rate, and the battery has a low DC impedance growth rate and a high cycle capacity retention rate.
[0019] In any embodiment, the weight average molecular weight of the grafted polymer is 600,000 to 2,000,000, and can be optionally 800,000 to 2,000,000.
[0020] The weight average molecular weight of the grafted polymer is within a suitable range, the electrode has excellent adhesion, cohesion and flexibility, the electrode has low membrane resistance, the electrode has excellent liquid absorption rate, and the battery has a low DC impedance growth rate and a high cycle capacity retention rate.
[0021] In any embodiment, the structural unit shown in Formula I comprises
[0022] At least one of .
[0023] In any embodiment, the structural unit shown in formula II comprises At least one of .
[0024] In any embodiment, the structural unit shown in formula III comprises
[0025] At least one of .
[0026] In any embodiment, the graft polymer includes one or more of polyvinylidene fluoride-trifluoroethylene-g-polyacrylic acid, polyvinylidene fluoride-trifluoroethylene-g-polypropylene, polyvinylidene fluoride-trifluoroethylene-g-polystyrene, polyvinylidene fluoride-trifluoroethylene-g-polyvinyl alcohol, polyvinylidene fluoride-trifluoroethylene-g-polyacrylamide, polyvinylidene fluoride-trifluoroethylene-g-polyacrylonitrile, polyvinylidene fluoride-trifluoroethylene-g-polymethyl methacrylate, polyvinylidene fluoride-trifluoroethylene-g-polyacrylic acid-acrylamide-ethyl acrylate, polyvinylidene fluoride-trifluoroethylene-g-polyacrylonitrile-ethyl acrylate, polyvinylidene fluoride-trifluoroethylene-g-polypropylene-methyl methacrylate, polyvinylidene fluoride-trifluoroethylene-g-polyacrylic acid-methyl methacrylate, polyvinylidene fluoride-trifluoroethylene-g-polyacrylic acid-methyl methacrylate, polyvinylidene fluoride-trifluoroethylene-g-polyvinyl alcohol-styrene, and polyvinylidene fluoride-trifluoroethylene-g-polyacrylic acid-acrylamide-methyl methacrylate.
[0027] The second aspect of the present application provides a method for preparing a grafted polymer, comprising the following steps:
[0028] Under polymerizable conditions, a first reactant comprising at least one structural unit represented by formula V is subjected to a graft reaction with a second reactant comprising at least one monomer represented by formula VI to prepare the graft polymer.
[0029] wherein R1 and R2 each independently contain hydrogen, fluorine, C containing at least one fluorine atom 1- 3 alkyl, R3, R4, R5 each independently contain hydrogen, substituted or unsubstituted C 1-5 One or more of the alkyl groups, R6 contains hydrogen, substituted or unsubstituted C 1-5 Alkyl, ester, carboxyl, amide, cyano, substituted or unsubstituted C 6-30 One or more aromatic groups.
[0030] Grafting non-fluorinated segments onto fluorinated segments causes the polymer to undergo a transition from an α- to a β-crystalline form, increasing the β-crystalline content in the grafted polymer and improving its ferroelectric properties. Simultaneously, grafting non-fluorinated segments onto fluorinated segments maximizes the weight-average molecular weight of the fluorinated and non-fluorinated blocks, leveraging the respective strengths of the fluorinated and non-fluorinated binders to achieve a complementary effect. This grafted polymer binder can improve the flexibility of the electrode, increase the electrode's liquid absorption rate, reduce the battery's DC impedance growth rate, and improve the battery's cycle capacity retention rate.
[0031] In any embodiment, the first reactant further comprises at least one structural unit represented by formula III,
[0032] wherein R7, R8, and R9 independently contain hydrogen, fluorine, or a C 1-3 One or more of alkyl groups.
[0033] In any embodiment, based on the total mass of the first reactant and the second reactant, the mass percentage of the second reactant is 1%-30%, and optionally 5%-25%.
[0034] In any embodiment, the preparation method of the first reactant comprises a hydrogenation reaction and an elimination reaction,
[0035] Hydrogenation reaction: hydrogenating the intermediate polymer comprising the structural unit represented by formula VII to obtain a hydrogenated intermediate polymer comprising the structural unit represented by formula VIII.
[0036] Elimination reaction: subjecting the hydrogenated intermediate polymer to an elimination reaction to prepare a first reactant;
[0037] wherein R1 and R2 each independently contain hydrogen, fluorine, C containing at least one fluorine atom 1- 3 alkyl group or more.
[0038] Through hydrogenation and elimination reactions, the first reactant containing a double bond was successfully prepared.
[0039] In any embodiment, the hydrogenation reaction specifically comprises the following steps:
[0040] The intermediate polymer and the first catalyst are subjected to a hydrogenation reaction in a first solvent to obtain a hydrogenated intermediate polymer.
[0041] In any embodiment, the elimination reaction specifically comprises the following steps:
[0042] The hydrogenated intermediate polymer, the second catalyst and the ligand are subjected to an elimination reaction in a second solvent to obtain a first reactant.
[0043] In any embodiment, the preparation method of the intermediate polymer specifically comprises the following steps:
[0044] Under polymerizable conditions, the monomer represented by formula IX and the monomer represented by formula X are polymerized to form an intermediate polymer,
[0045] wherein R1 and R2 each independently contain hydrogen, fluorine, C containing at least one fluorine atom 1- 3 alkyl group or more.
[0046] In any embodiment, based on the total mass of the monomer represented by formula IX and the monomer represented by formula X, the mass percentage of the monomer represented by formula X is 1% to 30%.
[0047] The third aspect of the present application provides a binder, which includes the graft polymer of the first aspect or the graft polymer prepared by the preparation method of the second aspect.
[0048] The binder can improve the flexibility of the pole piece, increase the liquid absorption rate of the pole piece, reduce the DC impedance growth rate of the battery, and improve the cycle capacity retention rate of the battery.
[0049] A fourth aspect of the present application provides an application of a grafted polymer in a secondary battery.
[0050] The fifth aspect of the present application provides a positive electrode plate, comprising a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector, wherein the positive electrode film layer comprises a positive electrode active material, a conductive agent and a binder, and the binder comprises the grafted polymer of the first aspect or the grafted polymer prepared by the preparation method of the second aspect.
[0051] The positive electrode sheet has excellent flexibility, adhesion, cohesion and low membrane resistance.
[0052] In any embodiment, based on the mass of the positive electrode active material, the mass percentage of the binder is 0.4%-2%, and optionally 0.8%-1.6%.
[0053] When the mass percentage of the binder is within an appropriate range, the electrode has excellent adhesion, cohesion and flexibility, the electrode has low diaphragm resistance, the electrode has an excellent liquid absorption rate, and the battery has a low DC impedance growth rate and a high cycle capacity retention rate.
[0054] In any embodiment, the bonding force per unit length between the positive electrode film layer and the positive electrode current collector is not less than 7.5 N / m, and can be optionally not less than 9 N / m.
[0055] The positive electrode film layer of the electrode sheet has high bonding strength with the positive electrode current collector. During use, the positive electrode film layer is not easy to fall off from the positive electrode current collector, which helps to improve the cycle performance of the battery.
[0056] In any embodiment, the cohesive force of the positive electrode sheet is not less than 65 N / m, and can be optionally not less than 100 N / m.
[0057] The electrode has high cohesion, and the positive electrode film layer is not easy to fall off during use, which helps to improve the cycle performance of the battery.
[0058] In any embodiment, the density of the electrolyte is 1.1-1.3 g / cm 3 The electrolyte absorption rate of the positive electrode plate is greater than 0.32 μg / s, and can be optionally greater than 0.35 μg / s.
[0059] The electrode has a high liquid absorption rate, which can improve the electrolyte infiltration efficiency of the electrode, improve the ion transmission path, reduce the interface resistance, and improve the battery dynamics performance.
[0060] A sixth aspect of the present application provides a secondary battery comprising an electrode assembly and an electrolyte, wherein the electrode assembly comprises a separator, a negative electrode plate and the positive electrode plate of the fifth aspect.
[0061] In any embodiment, the secondary battery includes at least one of a lithium ion battery, a sodium ion battery, a magnesium ion battery, and a potassium ion battery.
[0062] A seventh aspect of the present application provides an electrical device comprising the secondary battery of the sixth aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0063] FIG1 is a schematic diagram of a secondary battery according to an embodiment of the present application;
[0064] FIG2 is an exploded view of the secondary battery according to one embodiment of the present application shown in FIG1 ;
[0065] FIG3 is a schematic diagram of a battery module according to an embodiment of the present application;
[0066] FIG4 is a schematic diagram of a battery pack according to an embodiment of the present application;
[0067] FIG5 is an exploded view of the battery pack according to an embodiment of the present application shown in FIG4 ;
[0068] FIG6 is a schematic diagram of an electric device using a secondary battery as a power source according to an embodiment of the present application.
[0069] Description of reference numerals:
[0070] 1 battery pack; 2 upper box; 3 lower box; 4 battery module; 5 secondary battery; 51 shell; 52 electrode assembly; 53 cover plate. DETAILED DESCRIPTION
[0071] Below, the embodiments of the grafted polymer, preparation method, binder, positive electrode sheet, secondary battery and electrical device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0072] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0073] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0074] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0075] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0076] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0077] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0078] In the existing technology, polyvinylidene fluoride (PVDF) is often used as an electrode binder. However, PVDF has many problems during use, such as being sensitive to water content during the production process; in the battery recycling process, a large amount of HF will be generated to pollute the environment, and it cannot be recycled on a large scale due to restrictions on environmental protection policies; polyvinylidene fluoride is a polycrystalline semi-crystalline polymer, and the most common crystal forms are α, β and γ. Among them, the β crystal form and the γ crystal form are polar phases with ferroelectricity, while the PVDF commonly used in the existing technology is the α crystal form, which does not have ferroelectricity, which is not conducive to the transmission of electrons in the electrode, thereby resulting in high resistance of the electrode and poor electron transmission performance, which is not conducive to the performance of high-capacity positive electrode active materials.
[0079] [Graft polymer]
[0080] Based on this, the present application proposes a graft polymer, including a main chain polymer and a branched polymer, wherein the main chain polymer includes a structural unit shown in formula I, and the branched polymer includes a structural unit shown in formula II.
[0081] The wavy line in Formula I represents the junction position of the main chain polymer and the branched polymer, and R1 and R2 each independently contain hydrogen, fluorine, C containing at least one fluorine atom, 1-3 One or more of the alkyl groups, R3, R4, and R5 each independently contain hydrogen, substituted or unsubstituted C 1-5 One or more of the alkyl groups, R6 contains hydrogen, substituted or unsubstituted C 1-5 Alkyl, ester, carboxyl, amide, cyano, hydroxyl, substituted or unsubstituted C 6-30 One or more aromatic groups.
[0082] As used herein, the term "graft polymer" refers to a copolymer in which branched polymers are attached to certain atoms of a main-chain polymer. The main-chain polymer and the branched polymers may be homopolymers or copolymers. The main-chain polymer and the branched polymers each comprise different structural units. In some embodiments, the main-chain polymer is a segment formed by polymerization of a fluorinated monomer, and the branched polymers are segments formed by polymerization of a non-fluorinated monomer.
[0083] As used herein, the term "polymer" includes, on the one hand, a collection of chemically homogeneous macromolecules prepared by polymerization, but differing in degree of polymerization, molar mass, and chain length. The term also includes derivatives of such collections of macromolecules formed by polymerization, i.e., compounds that can be obtained by reaction, for example, addition or substitution, of functional groups in the aforementioned macromolecules and that can be chemically homogeneous or chemically heterogeneous.
[0084] In this article, the term “C 1-3 "Alkyl" refers to a straight or branched hydrocarbon chain radical consisting solely of carbon and hydrogen atoms, with no unsaturation present, having from one to three carbon atoms, and attached to the remainder of the molecule by a single bond. 1-3 Examples of alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, and 1-methylethyl (isopropyl).
[0085] In this context, the term "C 1-3 "Alkyl" refers to an alkyl group containing 1-3 carbon atoms in which at least one H atom is replaced by a F atom. In some embodiments, a C 1‐3 Alkyl groups include -CF3 groups and -C2F6 groups.
[0086] In this article, the term “C 1-5 "Alkyl" can refer to the term "C 1-3 This is understood from the definition of "alkyl".
[0087] As used herein, the term "substituted" refers to a compound or chemical moiety in which at least one hydrogen atom is replaced by another chemical moiety, wherein the substituents are each independently selected from the group consisting of hydroxyl, thiol, amino, cyano, nitro, aldehyde, halogen, alkenyl, alkynyl, aryl, heteroaryl, C 1-6 Alkyl, C 1-6 Alkoxy.
[0088] As used herein, the term "ester group" refers to a -COO- group.
[0089] As used herein, the term "carboxyl" refers to a -COOH group.
[0090] As used herein, the term "amido" refers to a -CO-NH2 group.
[0091] As used herein, the term "cyano" refers to a -CN group.
[0092] As used herein, the term "hydroxyl" refers to an -OH group.
[0093] In this article, the term “C 6-30 "Aryl" refers to an aromatic ring system in which at least one ring is aromatic, including but not limited to phenyl, biphenyl, indanyl, 1-naphthyl, 2-naphthyl, and tetrahydronaphthyl.
[0094] In this article, the substituted C 6-30 The aromatic group includes, but is not limited to, aralkyl, aralkyloxy, aryloxyalkyl, and symmetrical or unsymmetrical aryl groups linked via a carbonyl or ether group.
[0095] In this article, the term “C 6-12 "Aryl" can refer to the term "C 6-30 This is understood from the definition of "aromatic group".
[0096] In some embodiments, the structural unit shown in Formula I comprises
[0097] At least one of .
[0098] In some embodiments, the structural unit shown in Formula I comprises
[0099] In some embodiments, the structural unit shown in Formula II comprises
[0100] At least one of .
[0101] In some embodiments, the graft polymer includes one or more of polyvinylidene fluoride-trifluoroethylene-g-polyacrylic acid, polyvinylidene fluoride-trifluoroethylene-g-polypropylene, polyvinylidene fluoride-trifluoroethylene-g-polystyrene, polyvinylidene fluoride-trifluoroethylene-g-polyvinyl alcohol, polyvinylidene fluoride-trifluoroethylene-g-polyacrylamide, polyvinylidene fluoride-trifluoroethylene-g-polyacrylonitrile, polyvinylidene fluoride-trifluoroethylene-g-polymethyl methacrylate, polyvinylidene fluoride-trifluoroethylene-g-polyacrylic acid-acrylamide-ethyl acrylate, polyvinylidene fluoride-trifluoroethylene-g-polyacrylonitrile-ethyl acrylate, polyvinylidene fluoride-trifluoroethylene-g-polypropylene-methyl methacrylate, polyvinylidene fluoride-trifluoroethylene-g-polyacrylic acid-methyl methacrylate, polyvinylidene fluoride-trifluoroethylene-g-polyacrylic acid-methyl methacrylate, polyvinylidene fluoride-trifluoroethylene-g-polyvinyl alcohol-styrene, and polyvinylidene fluoride-trifluoroethylene-g-polyacrylic acid-acrylamide-methyl methacrylate.
[0102] In some embodiments, the grafted polymer acts as an electrode binder.
[0103] As used herein, the term "binder" refers to a chemical compound, polymer, or mixture that forms a colloidal solution or colloidal dispersion in a dispersion medium.
[0104] In some embodiments, the binder's dispersion medium is an aqueous solvent, such as water. That is, the binder is dissolved in the aqueous solvent. In some embodiments, the binder's dispersion medium is an oily solvent. Examples of oily solvents include, but are not limited to, dimethylacetamide, N,N-dimethylformamide, N-methylpyrrolidone, acetone, dimethyl carbonate, ethyl cellulose, and polycarbonate. That is, the binder is dissolved in the oily solvent.
[0105] In some embodiments, a binder is used to hold the electrode material and / or conductive agent in place and adhere them to the conductive metal component to form an electrode.
[0106] In some embodiments, the binder serves as a positive electrode binder, and is used to bind the positive electrode active material and / or the conductive agent to form an electrode.
[0107] In some embodiments, the binder serves as a negative electrode binder, and is used to bind the negative electrode active material and / or the conductive agent to form an electrode.
[0108] In this article, the term "α-form" refers to a crystal structure in which the molecular chains are arranged antiparallel in space, in a TGTG' conformation, with a net dipole moment of 0 and no apparent polarity. The α-form belongs to the monoclinic system, with unit cell parameters: a = 0.496 nm, b = 0.964 nm, and c = 0.462 nm.
[0109] In this article, the term "β-form" refers to a crystalline form in which the molecular chains are in a planar zigzag TTTT all-trans configuration. The β-form is an orthorhombic crystal with unit cell parameters of a = 0.858 nm, b = 0.491 nm, and c = 0.256 nm. The β-form exhibits high polarity and excellent piezoelectric and ferroelectric properties.
[0110] The fluorine contained in the main-chain polymer forms hydrogen bonds with the hydroxyl and / or carboxyl groups on the surface of the active material and the current collector, giving the electrode excellent adhesion and cohesion. Grafting a branched polymer onto the main-chain polymer causes the polymer to transform from an α-crystalline form to a β-crystalline form, increasing the β-crystalline content of the grafted polymer, improving the ferroelectric and piezoelectric properties of the grafted polymer, increasing the electrode's liquid absorption rate, improving the electrode's ability to wet the electrolyte, facilitating the formation of a conductive network, and improving the battery's kinetic performance. At the same time, the branched polymer increases the longitudinal complexity of the polymer, facilitating the formation of physical crosslinks between the grafted polymers, effectively dispersing the positive electrode active material and conductive agent, and constructing a three-dimensional conductive network. While increasing the electrode's cohesion, it also improves the insertion and extraction of ions and the transfer of electrons during battery charge and discharge, improving the electrode's ionic and electronic conductivity, reducing the battery's DC impedance growth rate, and improving battery cycle performance.
[0111] In addition, the branched polymer can reduce the crystallinity of the main chain polymer, increase the mobility of the chain segments, and improve the flexibility of the electrode. At the same time, the branched polymer can weaken the intermolecular forces of the main chain polymer, increase the flexibility of the electrode, reduce the risk of brittle fracture of high-load and high-voltage dense electrode, and improve the safety performance of the battery.
[0112] In summary, grafting a non-fluorinated side-chain polymer onto a fluorinated main-chain polymer fully leverages the respective advantages of the fluorinated binder and the non-fluorinated binder, achieving a complementary effect. This grafted polymer binder can improve the flexibility of the electrode, increase the electrode's liquid absorption rate, reduce the battery's DC impedance growth rate, and improve the battery's cycle capacity retention rate.
[0113] In some embodiments, the content of the β crystal form in the graft polymer is 32% to 74%, based on the total content of the α crystal form and the β crystal form in the graft polymer.
[0114] In this application, the content of β-crystal has a meaning known in the art and can be measured using instruments and methods known in the art. As an example, the content of β-crystal can be measured using FTIR. Specifically, the FTIR test instrument is a Nieolet 5700 infrared spectrometer, with 32 infrared scans and a spectrum wave number range of 700-4000 cm -1 , resolution is 4cm -1 From the obtained spectrum, the wave number 765cm, which is the characteristic absorption of α crystal form, was determined. -1The absorption intensity and the wave number 840 cm-1, which is the characteristic absorption of β crystal form -1 The absorption intensity of each peak corresponding to the above wavenumber is obtained by connecting the starting and ending points of the formation with a straight line. The intersection of this straight line and the peak wavenumber is set as A, the point where the spectrum intersects the peak wavenumber is set as B, and the point where the transmittance at the peak wavenumber is 0% is set as C. The lengths between AC and BC are calculated, and Log(AC / BC) is used as the absorption intensity at each wavenumber.
[0115] The content of β crystal is as described above, and the wave number 765cm corresponding to α crystal and β crystal is obtained. -1 and wave number 840cm -1 The absorption intensity is calculated by substituting it into the following formula:
[0116] β-crystal content = 840 cm -1 Absorption intensity / (765cm -1 Absorption intensity +840cm - 1 absorption intensity)×100%.
[0117] In some embodiments, based on the total content of α-crystalline form and β-crystalline form in the grafted polymer, the content of β-crystalline form in the grafted polymer can be selected as any one of 32%-40%, 32%-50%, 32%-60%, 32%-70%, 32%-74%, 40%-50%, 40%-60%, 40%-70%, 40%-74%, 50%-60%, 50%-70%, 50%-74%, 60%-70%, and 60%-74%.
[0118] By controlling the content of the β-crystal form of the grafted polymer within a suitable range, the piezoelectric and ferroelectric properties of the grafted polymer can be improved, the diaphragm resistance of the electrode can be reduced, and the dynamic performance of the battery can be improved.
[0119] In some embodiments, the main chain polymer further comprises a structural unit represented by formula III,
[0120] wherein R7, R8, and R9 independently contain hydrogen, fluorine, or a C 1-3 One or more of alkyl groups.
[0121] In some embodiments, the structural unit shown in Formula III comprises
[0122] At least one of .
[0123] In some embodiments, the backbone polymer further comprises
[0124] At least one of .
[0125] In some embodiments, R6 comprises an ester group, a carboxyl group, an amide group, a cyano group, a hydroxyl group, a substituted or unsubstituted C 6-12 One or more aromatic groups.
[0126] In some embodiments, the structural unit shown in Formula II comprises
[0127] One or more of .
[0128] The grafted polymer contains ester groups, carboxyl groups, amide groups, cyano groups, hydroxyl groups, substituted or unsubstituted C 6-12 The aromatic functional group can increase the viscosity of the slurry, improve the cohesion and flexibility of the electrode, increase the liquid absorption rate of the electrode, and reduce the DC impedance growth rate of the battery.
[0129] In some embodiments, R6 comprises an ester group.
[0130] In some embodiments, the structural unit shown in Formula II comprises
[0131] One or both of .
[0132] The ester groups contained in the branched polymers help weaken the excessively strong dipole moment between the main-chain polymers, reducing the brittleness of the electrode caused by the obstruction of free movement of polymer segments due to the strong polarity of the C-H bonds in the main-chain polymers, thereby improving the safety performance of the battery. At the same time, the ester groups can form hydrogen bonds with the hydroxyl and / or carboxyl groups on the surface of the active material and / or the current collector, thereby improving the adhesion and cohesion of the electrode. In addition, the ester groups have good affinity with the electrolyte, increasing the liquid absorption rate of the electrode and helping to enhance the contact between the electrolyte and the active material, thereby improving ionic conductivity and reducing the DC impedance growth rate of the battery.
[0133] In some embodiments, R6 comprises a substituted or unsubstituted C 6-12 Aromatic group.
[0134] In some embodiments, the structural unit shown in Formula II comprises
[0135] The aromatic groups contained in the branched polymer help to improve the mechanical strength of the electrode to cope with the volume changes of the positive electrode active material during charging and discharging, so that the electrode maintains structural integrity during charging and discharging, and improves the battery cycle performance.
[0136] In some embodiments, R6 comprises a carboxyl group.
[0137] In some embodiments, the structural unit shown in Formula II comprises
[0138] The carboxyl groups contained in the branched polymer can form strong hydrogen bonds and dipole-dipole interactions with the active material and / or hydroxyl groups on the surface, improving the adhesion and cohesion of the electrode, improving the dispersion of the binder in the slurry, and reducing the membrane resistance. In addition, the carboxyl groups have a good affinity for the electrolyte, increasing the liquid absorption rate of the electrode and helping to enhance the contact between the electrolyte and the active material, thereby improving ionic conductivity and reducing the DC impedance growth rate of the battery.
[0139] In some embodiments, R6 comprises an amide group.
[0140] In some embodiments, the structural unit shown in Formula II comprises
[0141] The amide groups contained in the branched polymers easily form hydrogen bonds with the hydroxyl groups of the active material and / or current collector, which can improve the adhesion and cohesion of the electrode. At the same time, the amide groups help to weaken the excessively strong dipole moment between the main chain polymers, reduce the brittleness of the electrode caused by the obstruction of the free movement of the polymer segments due to the strong polarity CF bonds in the main chain polymer, and improve the safety performance of the battery. In addition, the amide groups can improve the liquid absorption capacity of the electrode, improve the wettability of the electrode in the electrolyte, facilitate the rapid formation of ion transmission channels on the electrode, help reduce the membrane resistance of the electrode, and improve the cycle performance of the battery.
[0142] In some embodiments, R6 comprises cyano.
[0143] In some embodiments, the structural unit shown in Formula II comprises
[0144] The branched polymer contains a strong polar group, cyano, which can form strong hydrogen bonds and dipole-dipole interactions with the hydroxyl groups on the surface of the active material and / or the current collector, helping to further improve the adhesion and cohesion of the electrode and reduce the membrane resistance of the electrode. In addition, the strong polar group cyano can enhance the stability of the molecular structure, increase the glass transition temperature of the grafted polymer, improve the rigidity and thermal stability of the grafted polymer, help improve the oxidation stability of the electrode, and enhance the cycle performance of the battery. In addition, the cyano group gives the branched polymer a certain coating property for the active material. The cyano group can complex with the transition metal ions on the surface of the active material, hindering the dissolution of the transition metal ions, thereby reducing the deposition of transition metal ions on the negative electrode surface, helping to improve the cycle performance of the battery.
[0145] In some embodiments, the mass content of the branched polymer is 1%-30%, optionally 5%-25%, based on the total mass of the grafted polymer.
[0146] In some embodiments, the weight content of the branched polymer is 1%-30% based on the total weight of the grafted polymer. In some embodiments, the weight content of the branched polymer can be 1%, 5%, 10%, 15%, 20%, 25%, 30%, or a value within a range formed by any two of the above values, based on the total weight of the grafted polymer.
[0147] When the mass content of the branched polymer is within an appropriate range, the branched polymer can play its role, improve the adhesion and cohesion of the electrode, improve the flexibility of the electrode, reduce the membrane resistance, increase the liquid absorption rate of the electrode, reduce the DC impedance growth rate of the battery, and improve the cycle performance of the battery. At the same time, it can also reduce the possibility of excessive swelling of the electrode due to excessive liquid absorption rate of the electrode caused by excessive mass content of the branched polymer, and reduce the impact of excessive swelling of the electrode on the DC impedance growth rate and cycle performance of the battery.
[0148] The mass content of the branched polymer is within an appropriate range, the electrode has excellent adhesion, cohesion and flexibility, the electrode has low membrane resistance, the electrode has an excellent liquid absorption rate, and the battery has a low DC impedance growth rate and a high cycle capacity retention rate.
[0149] In some embodiments, the weight content of the branched polymer is 5% to 25% based on the total weight of the grafted polymer. In some embodiments, the weight content of the branched polymer can be 5%, 10%, 15%, 20%, 25%, or a value within a range formed by any two of the above values, based on the total weight of the grafted polymer.
[0150] When the mass content of the branched polymer is within an appropriate range, the bonding force of the electrode can be improved, the DC impedance growth rate of the battery can be reduced, and the cycle capacity retention rate of the battery can be improved.
[0151] In some embodiments, the weight average molecular weight of the grafted polymer is 600,000 to 2,000,000, and can be optionally 800,000 to 2,000,000.
[0152] As used herein, the term "weight average molecular weight" refers to the sum of the weight fractions of molecules of different molecular weights in a polymer multiplied by their corresponding molecular weights.
[0153] The weight-average molecular weight of the grafted polymer can be measured using methods and equipment known in the art. For example, a Waters 2695Isocratic HPLC gel chromatograph (differential refractive index detector 2141) is used. A polystyrene solution sample with a mass fraction of 3.0% is used as a reference, and a matching chromatographic column is selected (oily: Styragel HT5 DMF7.8×300mm+Styragel HT4). A 3.0% polymer glue is prepared with purified N-methylpyrrolidone (NMP) solvent, and the prepared solution is allowed to stand for one day for use. During the test, tetrahydrofuran is first drawn into a syringe and rinsed, and repeated several times. Then 5 ml of the experimental solution is drawn, the air in the syringe is expelled, and the needle tip is wiped dry. Finally, the sample solution is slowly injected into the injection port. The data is obtained after the reading stabilizes.
[0154] In some embodiments, the weight average molecular weight of the grafted polymer is 600,000 to 2,000,000. In some embodiments, the weight average molecular weight of the grafted polymer is 600,000, 800,000, 1,000,000, 1,200,000, 1,400,000, 1,600,000, 1,800,000, 2,000,000, or a value in a range formed by any two of the foregoing values.
[0155] If the weight-average molecular weight of the grafted polymer is too large, the binder will be difficult to dissolve and will easily agglomerate with the conductive agent, increasing the internal resistance of the diaphragm. In addition, the viscosity of the slurry will increase, reducing the dispersibility of the substances in the slurry, affecting the uniformity of subsequent coating, making it easy for the battery to undergo local lithium deposition during long-term cycles, thereby deteriorating the cycle performance of the battery. If the weight-average molecular weight of the grafted polymer is too small, the viscosity of the slurry will be too small, the slurry will easily gel, making it difficult to form a three-dimensional network bonding structure, and it will not be able to play an effective bonding role. The electrode will easily fall off during the long-term cycle of the battery, deteriorating the cycle performance of the battery. In addition, the electrode's liquid absorption capacity and wettability in the electrolyte will decrease, resulting in an increase in the internal resistance of the electrode diaphragm.
[0156] The weight average molecular weight of the grafted polymer is within a suitable range, the electrode has excellent adhesion, cohesion and flexibility, the electrode has low membrane resistance, the electrode has excellent liquid absorption rate, and the battery has a low DC impedance growth rate and a high cycle capacity retention rate.
[0157] In some embodiments, the weight average molecular weight of the grafted polymer is 800,000 to 2,000,000. In some embodiments, the weight average molecular weight of the grafted polymer is 800,000, 1,000,000, 1,200,000, 1,400,000, 1,600,000, 1,800,000, 2,000,000, or a value in a range formed by any two of the foregoing values.
[0158] Controlling the weight-average molecular weight of the grafted polymer within an appropriate range can improve the stability of the slurry, improve the slurry's anti-gel properties, reduce the diaphragm resistance of the electrode, improve the adhesion and cohesion of the electrode, and reduce the DC impedance growth rate of the battery.
[0159] In some embodiments, a method for preparing a grafted polymer is provided, comprising the steps of:
[0160] Under polymerizable conditions, a first reactant comprising at least one structural unit represented by formula V is subjected to a graft reaction with a second reactant comprising at least one monomer represented by formula VI to prepare the graft polymer.
[0161] wherein R1 and R2 each independently contain hydrogen, fluorine, C containing at least one fluorine atom 1- 3 alkyl, R3, R4, R5 each independently contain hydrogen, substituted or unsubstituted C 1-5 One or more of the alkyl groups, R6 contains hydrogen, substituted or unsubstituted C 1-5 Alkyl, ester, carboxyl, amide, cyano, substituted or unsubstituted C 6-30 One or more aromatic groups.
[0162] The above-mentioned grafting reaction can be used to graft non-fluorinated side-chain polymers onto a fluorinated main-chain polymer, causing the polymer to undergo a transition from an α- to a β-crystalline form, increasing the β-crystalline content in the grafted polymer and improving the grafted polymer's ferroelectric and piezoelectric properties. Simultaneously grafting the non-fluorinated side-chain polymer onto the fluorinated main-chain polymer fully leverages the advantages of both the fluorinated and non-fluorinated binders, achieving a complementary effect. This grafted polymer binder can improve the flexibility of the electrode, increase its liquid absorption rate, reduce the battery's DC impedance growth rate, and improve the battery's cycle capacity retention rate.
[0163] In addition, compared to the grafting reaction using the halogen atoms on the main chain as the initiation site and utilizing atom transfer radical polymerization, the present application uses a first reactant containing a double bond and a second reactant containing a monomer for a grafting reaction. The initiation efficiency of the grafting reaction is high, and the grafted polymer has an excellent grafting rate, which can improve the adhesion, cohesion and flexibility of the electrode, reduce the membrane resistance of the electrode, increase the liquid absorption rate of the electrode, reduce the DC internal resistance growth rate of the battery, and improve the cycle capacity retention rate of the battery.
[0164] In some embodiments, the grafting reaction is a free radical polymerization reaction.
[0165] In this context, "free radical polymerization" refers to a chemical reaction in which monomers, under the influence of external factors, form free radical active centers in the monomers, which then undergo chain polymerization with other monomers to form polymers. The characteristic of this reaction is that free radical active centers must be generated at the beginning of the reaction.
[0166] In some embodiments, the reaction temperature of the grafting reaction is 70°C-90°C.
[0167] In some embodiments, the grafting reaction time is 18 hours to 36 hours.
[0168] In some embodiments, the first reactant further comprises at least one structural unit represented by formula III,
[0169] wherein R7, R8, and R9 independently contain hydrogen, fluorine, or a C 1-3 One or more of alkyl groups.
[0170] In some embodiments, based on the total mass of the first reactant and the second reactant, the mass percentage of the second reactant is 1%-30%, optionally 5%-25%.
[0171] By controlling the mass percentage of the second reactant within a suitable range, and then controlling the mass content of the branched polymer within a suitable range, the grafted polymer has excellent structural properties, can improve the flexibility of the electrode, increase the liquid absorption rate of the electrode, reduce the DC impedance growth rate of the battery, and improve the cycle capacity retention rate of the battery.
[0172] In some embodiments, the preparation method of the first reactant includes a hydrogenation reaction and an elimination reaction,
[0173] Hydrogenation reaction: hydrogenating the intermediate polymer comprising the structural unit represented by formula VII to obtain a hydrogenated intermediate polymer comprising the structural unit represented by formula VIII.
[0174] Elimination reaction: subjecting the hydrogenated intermediate polymer to an elimination reaction to prepare a first reactant;
[0175] wherein R1 and R2 each independently contain hydrogen, fluorine, C containing at least one fluorine atom 1- 3 alkyl group or more.
[0176] Through hydrogenation and elimination reactions, a first reactant containing a double bond was successfully prepared, which is conducive to the grafting reaction and generates a grafted polymer with excellent structural properties.
[0177] In some embodiments, the hydrogenation reaction specifically comprises the following steps:
[0178] The intermediate polymer and the first catalyst are subjected to a hydrogenation reaction in a first solvent to obtain a hydrogenated intermediate polymer.
[0179] In some embodiments, the first catalyst comprises tributyltin hydride.
[0180] In some embodiments, the first solvent comprises tetrahydrofuran.
[0181] In some embodiments, the elimination reaction specifically comprises the following steps:
[0182] The hydrogenated intermediate polymer, the second catalyst and the ligand are subjected to an elimination reaction in a second solvent to obtain a first reactant.
[0183] In some embodiments, the second catalyst comprises copper.
[0184] In some embodiments, the ligand includes one or both of 2,2'-bipyridine and 4,4'-bipyridine.
[0185] In some embodiments, the second solvent comprises dimethyl sulfoxide.
[0186] In some embodiments, the method for preparing the intermediate polymer specifically comprises the following steps:
[0187] Under polymerizable conditions, the monomer represented by formula IX and the monomer represented by formula X are polymerized to form an intermediate polymer,
[0188] wherein R1 and R2 each independently contain hydrogen, fluorine, C containing at least one fluorine atom 1- 3 alkyl group or more.
[0189] In some embodiments, based on the total mass of the monomer represented by formula IX and the monomer represented by formula X, the mass percentage of the monomer represented by formula X is 1%-30%.
[0190] Controlling the mass percentage of the monomer represented by formula X within a suitable range is beneficial for preparing an intermediate polymer with a suitable structure, which is beneficial for subsequent hydrogenation and elimination reactions. Controlling the first reactant to contain a suitable number of double bonds can control the grafted polymer to have a suitable grafting rate, and the grafted polymer has excellent structural properties.
[0191] In some embodiments, a binder is provided, comprising the graft polymer in some embodiments or the graft polymer prepared by the preparation method in some embodiments.
[0192] The binder can improve the flexibility of the pole piece, increase the liquid absorption rate of the pole piece, reduce the DC impedance growth rate of the battery, and improve the cycle capacity retention rate of the battery.
[0193] In some embodiments, a use of a graft polymer in a secondary battery is provided.
[0194] [Positive electrode]
[0195] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector. The positive electrode film layer includes a positive electrode active material, a conductive agent and a binder. The binder is a graft polymer in some embodiments or a graft polymer prepared by the preparation method in some embodiments.
[0196] The positive electrode sheet has excellent flexibility, adhesion, cohesion and low membrane resistance.
[0197] In some embodiments, based on the mass of the positive electrode active material, the mass percentage of the binder is 0.4%-2%, and optionally 0.8%-1.6%.
[0198] In some embodiments, the mass percentage of the binder is 0.4%-2% based on the mass of the positive electrode active material. In some embodiments, the mass percentage of the binder is 0.4%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.6%, 1.8%, 2%, or a value in the range of any two of the above points based on the mass of the positive electrode active material.
[0199] When the binder content is too low, the binder will not be able to exert sufficient bonding effect. On the one hand, the binder cannot fully disperse the conductive agent and active material, resulting in an increase in the diaphragm resistance of the electrode. Conversely, when the binder content is too high, the viscosity of the slurry is too high, resulting in an excessively thick binder coating on the surface of the active material, which affects the transmission of electrons and ions during the battery cycle and increases the internal resistance of the diaphragm.
[0200] When the mass percentage of the binder is within an appropriate range, the electrode has excellent adhesion, cohesion and flexibility, the electrode has low diaphragm resistance, the electrode has an excellent liquid absorption rate, and the battery has a low DC impedance growth rate and a high cycle capacity retention rate.
[0201] In some embodiments, the mass percentage of the binder is 0.8%-1.6% based on the mass of the positive electrode active material. In some embodiments, the mass percentage of the binder is 0.8%, 1.0%, 1.2%, 1.4%, 1.6%, or a value in the range of any two of the above points based on the mass of the positive electrode active material.
[0202] The mass percentage of the binder is within an appropriate range, and the slurry has an appropriate viscosity, which is beneficial to the subsequent electrode coating and coating drying process, reduces the membrane resistance of the battery, and improves the dynamic performance of the battery.
[0203] In any embodiment, the bonding force per unit length between the positive electrode film layer and the positive electrode current collector is not less than 7.5 N / m, and can be optionally not less than 9 N / m.
[0204] In some embodiments, the bonding force per unit length between the positive electrode film layer and the positive electrode current collector may be 7.5 N / m, 8 N / m, 8.5 N / m, 9 N / m, 10 N / m, 11 N / m, 12 N / m, 13 N / m, 14 N / m, 14.5 N / m, 15 N / m, 15.5 N / m, 16 N / m, 16.5 N / m, 17 N / m, 17.5 N / m, 18 N / m, 18.5 N / m, 19 N / m, 19.5 N / m, 20 N / m, 20.5 N / m, 21 N / m, 21.5 N / m, 23 N / m, 24 N / m, 25 N / m, or a value in the range formed by any two of the above points.
[0205] The adhesion strength per unit length between the positive electrode film layer and the positive electrode current collector can be tested using any method known in the art. For example, referring to the national standard GBT 2790-1995 "Test method for 180° peel strength of adhesives," the adhesion strength test process for the examples and comparative examples of this application is as follows:
[0206] Use a blade to cut a 30mm wide and 100-160mm long electrode sample. Apply a 20mm wide and 90-150mm long double-sided tape to the steel plate. Attach the previously cut electrode sample to the double-sided tape with the test surface facing down. Then use a roller to roll the sample three times in the same direction.
[0207] Insert a paper tape with a width equal to that of the electrode sample and a length of 250 mm under the electrode current collector and fix it with wrinkle glue.
[0208] Turn on the Sansi tensile testing machine (sensitivity 1N), the indicator light will illuminate, adjust the limit block to the appropriate position, and secure the end of the steel plate specimen without the electrode with the lower clamp. Fold the paper tape upward and secure it with the upper clamp. Use the "up" and "down" buttons on the manual controller included with the tensile testing machine to adjust the position of the upper clamp, then perform the test and read the value. The force at the electrode when the force is balanced is divided by the width of the tape as the bonding force per unit length of the electrode, which represents the bonding strength between the positive electrode film layer and the current collector.
[0209] The positive electrode film layer of the electrode sheet has high bonding strength with the positive electrode current collector. During use, the positive electrode film layer is not easy to fall off from the positive electrode current collector, which helps to improve the cycle performance of the battery.
[0210] In some embodiments, the cohesive force of the positive electrode sheet is not less than 65 N / m, and can be optionally not less than 100 N / m.
[0211] In some embodiments, the cohesive force of the positive electrode sheet may be selected as 65 N / m, 70 N / m, 80 N / m, 90 N / m, 100 N / m, 110 N / m, 120 N / m, 130 N / m, 140 N / m, 145 N / m, 150 N / m, 155 N / m, 160 N / m, 165 N / m, 170 N / m, 175 N / m, 180 N / m, 185 N / m, 190 N / m, 195 N / m, 200 N / m, 205 N / m, 210 N / m, or a value in the range formed by any two of the above points.
[0212] The cohesion of the positive electrode sheet can be tested by any means known in the art. For example, the positive electrode sheet is cut into a sample to be tested with a length of 100 mm and a width of 10 mm. A stainless steel plate with a width of 25 mm is taken and the sample to be tested is attached to the stainless steel plate with a 3M double-sided tape (width 11 mm), wherein the current collector is bonded to the double-sided tape. A 2000g roller is used to roll back and forth on the surface of the sample three times (300 mm / min). Then, a tape with a width of 10 mm and a thickness of 50 μm (model NITTO.NO5000NS) is attached to the surface of the positive electrode film layer and a 2000g roller is used to roll back and forth on its surface three times (300 mm / min). Bend the tape 180 degrees and manually peel 25mm off the tape and the positive electrode film. The sample was then mounted on an Instron 336 tensile testing machine, aligning the peeling surface with the tester's force line (i.e., performing a 180° peel). After pre-pulling for 10mm at a peeling speed of 100mm / min, the tensile testing machine was reset, and the sample was peeled continuously at 300mm / min to obtain a cohesion curve. The average value of the plateau was taken as the peeling force F0, and the cohesion F1 of the tested electrode was calculated using the following formula: F1 = F0 / width of the sample to be tested, with F1 measured in N / m.
[0213] The electrode has high cohesion, and during use, the active material particles maintain good adhesion, which helps to improve the cycle performance of the battery.
[0214] In some embodiments, the density of the electrolyte is 1.1-1.3 g / cm 3 The electrolyte absorption rate of the positive electrode plate is greater than 0.32 μg / s, and can be optionally greater than 0.35 μg / s.
[0215] In some embodiments, the liquid absorption rate of the positive electrode sheet to the electrolyte is 0.33 μg / s, 0.34 μg / s, 0.35 μg / s, 0.36 μg / s, 0.37 μg / s, 0.38 μg / s, 0.39 μg / s, 0.40 μg / s, 0.41 μg / s, 0.42 μg / s, 0.43 μg / s, 0.44 μg / s, 0.45 μg / s, 0.46 μg / s, 0.47 μg / s, 0.48 μg / s, 0.49 μg / s, 0.50 μg / s, 0.51 μg / s, 0.52 μg / s, or a value in the range of any two of the above points, and the density of the electrolyte is 1.1-1.3 g / cm 3 .
[0216] The liquid absorption rate of the electrode can reflect the ability of the electrode to be wetted in the electrolyte. The test can be performed by any means known in the art. As an example, the cold-pressed positive electrode is cut into a test sample of 5cm×5cm size; first, the sample is dried at 80°C for 4h, and after the thickness of the electrode is tested, it is fixed on the sample table, and then a capillary with d=200μm is selected, and the end face is polished with 5000 mesh sandpaper until it is flat, and the state between the capillary and the electrode is observed under a microscope; the electrolyte is absorbed with a capillary, and the electrolyte height h=3mm is controlled. The capillary is lowered to contact the electrode, and a stopwatch is used at the same time. When the liquid level has dropped, the timer is stopped, the liquid absorption time t is read, and the data is recorded; the average liquid absorption rate v of the electrode is calculated using the formula, v=π×(d / 2)2×h×ρ / t. In this test, the density ρ of the selected electrolyte is 1.1-1.3g / cm 3 As an example, the electrolyte can be prepared by dissolving lithium hexafluorophosphate in a mixed solvent of ethylene carbonate and ethyl methyl carbonate, wherein the mass content of the lithium hexafluorophosphate solution is 12.5%, and the volume ratio of ethylene carbonate to ethyl methyl carbonate in the solution is 3:7.
[0217] The electrode has a high liquid absorption rate, which can improve the electrolyte infiltration efficiency of the electrode, improve the ion transmission path, reduce the interface resistance, and improve the battery dynamics performance.
[0218] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.
[0219] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0220] In some embodiments, the positive electrode active material may adopt the positive electrode active material for batteries that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 ), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 ), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.
[0221] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0222] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0223] [Negative electrode]
[0224] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.
[0225] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0226] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0227] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0228] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0229] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0230] In some embodiments, the negative electrode film layer may optionally further include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0231] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0232] [Electrolytes]
[0233] The electrolyte conducts ions between the positive and negative electrodes. This application does not specify the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.
[0234] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte salt and a solvent.
[0235] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bisfluorosulfonyl imide, lithium bistrifluoromethanesulfonyl imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium bisoxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0236] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0237] In some embodiments, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.
[0238] [Isolation film]
[0239] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.
[0240] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0241] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.
[0242] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0243] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0244] [Secondary battery]
[0245] The present application does not particularly limit the shape of the secondary battery; it can be cylindrical, square, or any other shape. For example, FIG1 shows a secondary battery 5 having a square structure as an example. The secondary battery can also be a sodium ion battery, a magnesium ion battery, or a potassium ion battery.
[0246] In some embodiments, referring to Figure 2, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.
[0247] [Battery Module]
[0248] In some embodiments, secondary batteries can be assembled into a battery module. The number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.
[0249] Figure 3 shows an example battery module 4. Referring to Figure 3 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured together using fasteners.
[0250] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.
[0251] [Battery Pack]
[0252] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.
[0253] Figures 4 and 5 illustrate an example battery pack 1. Referring to Figures 4 and 5 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be placed over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0254] [Electrical devices]
[0255] In one embodiment of the present application, an electric device is provided, comprising at least one of a secondary battery according to any embodiment, a battery module according to any embodiment, or a battery pack according to any embodiment.
[0256] The electrical device includes at least one of the secondary battery, battery module, or battery pack provided in this application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.
[0257] As the electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.
[0258] Figure 6 shows an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery, a battery pack or battery module can be used.
[0259] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.
[0260] Example
[0261] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.
[0262] 1. Preparation method
[0263] Example 1
[0264] 1) Preparation of grafted polymer
[0265] Preparation of the intermediate polymer: 4 kg of deionized water and 2 g of methyl cellulose ether were added to a 10 L autoclave. The mixture was evacuated and the O2 was replaced with N2 three times. 5 g of tert-butyl peroxypivalate and 2 g of sodium bicarbonate were added. 0.8 kg of vinylidene fluoride and 0.2 kg of chlorotrifluoroethylene were added to the mixture until the pressure reached 5 MPa. Mixing and stirring were continued for 30 minutes. The temperature was raised to 38°C and the reaction was continued for 5 hours. 42 g of cyclohexane was added to continue the reaction. The reaction was terminated when the pressure in the autoclave dropped to 2 MPa. The reaction system was centrifuged, the solid phase was collected, washed, and dried to obtain polyvinylidene fluoride-chlorotrifluoroethylene, wherein the mass content of chlorotrifluoroethylene was 20%, based on the total mass of vinylidene fluoride and chlorotrifluoroethylene.
[0266] Hydrogenation Reaction: Add 10 g of the poly(vinylidene fluoride)-chlorotrifluoroethylene (PVDF) intermediate polymer and 0.44 g of azobisisobutyronitrile to a 500 mL three-necked flask. Purge the flask three times with nitrogen, then inject purified tetrahydrofuran (200 mL) and stir thoroughly to obtain a mixed solution. Add tributyltin hydride (7.3 mL, 26.8 mmol) to the mixed solution using a sampler and further mix thoroughly. The mixture reacts at 60°C for 24 h, then quenches with methanol. The reaction mixture is precipitated in a mixture of water and methanol (1:1, volume ratio) to obtain a precipitate, which is then washed with n-hexane to obtain a crude product. The crude product is dissolved in acetone and precipitated three times in a mixture of water and methanol (1:1, volume ratio). The mixture is dried under reduced pressure at room temperature to obtain the hydrogenated intermediate polymer of poly(vinylidene fluoride)-chlorotrifluoroethylene (PVDF).
[0267] Elimination Reaction: In a 250 mL two-necked flask purged with nitrogen, completely dissolve 1 g of the hydrogenated intermediate polymer in 100 mL of dimethyl sulfoxide. Add 0.19 g of copper powder and 0.92 g of 2,2'-bipyridine to the reaction. Under a nitrogen atmosphere, maintain the reaction temperature at 80°C for 24 hours. Precipitate the resulting product in a 3% calcium chloride aqueous solution to remove the hydrogen fluoride byproduct. Dissolve the resulting precipitate in acetone and then precipitate it three times in methanol. Dry under reduced pressure at room temperature to obtain the first reactant, polyvinylidene fluoride-trifluoroethylene, which has double bonds.
[0268] Grafting reaction: In a 50 ml double-necked flask purged with N2, 0.2 g of the first reactant was added and completely dissolved in 12.5 ml of N-methylpyrrolidone (NMP) at room temperature. Then acrylic acid, acrylamide and ethyl acrylate (monomer molar ratio 1:1:1) were added, wherein the total mass of acrylic acid, acrylamide and ethyl acrylate was 17.4 mg. The reaction was carried out in an N2 atmosphere, the reaction temperature was 80 ° C, and the reaction time was 24 h. The resulting mixture was precipitated in a mixture of water and methanol (water to methanol volume ratio 1:1), and then the resulting product was dissolved in acetone, and then precipitated in methanol three times and dried under reduced pressure at room temperature. Soaked in chloroform three times to remove small molecular polymers, and finally a grafted polymer polyvinylidene fluoride-trifluoroethylene-g-polyacrylic acid-acrylamide-ethyl acrylate was obtained. The main chain polymer of the grafted polymer contains the three structural units shown below, and the side chain polymer is polyacrylic acid-acrylamide-ethyl acrylate.
[0269] 2) Preparation of positive electrode sheet
[0270] LiNi 0.8 Co 0.1 Mn 0.1 , conductive agent carbon black, the binder of Example 1, and N-methylpyrrolidone (NMP) are stirred and mixed in a weight ratio of 96.7:2:1.2:21 to obtain a positive electrode slurry; the positive electrode slurry is then evenly coated on the positive electrode collector, and then dried, cold pressed, and cut to obtain a positive electrode sheet.
[0271] 3) Preparation of negative electrode sheet
[0272] The active material artificial graphite, the conductive agent carbon black, the binder styrene-butadiene rubber (SBR), and the thickener sodium hydroxymethyl cellulose (CMC-Na) are dissolved in the solvent deionized water in a weight ratio of 96.2:0.8:0.8:1.2, and mixed evenly to prepare a negative electrode slurry; the negative electrode slurry is evenly coated on the negative electrode collector copper foil once or multiple times, and the negative electrode sheet is obtained after drying, cold pressing, and slitting.
[0273] 4) Isolation film
[0274] Polypropylene film is used as the isolation film.
[0275] 5) Preparation of electrolyte
[0276] In an argon atmosphere glove box (H2O<0.1ppm, O2<0.1ppm), the organic solvent ethylene carbonate (EC) / ethyl methyl carbonate (EMC) was mixed uniformly in a volume ratio of 3 / 7, 12.5% LiPF6 lithium salt was added and dissolved in the organic solvent, and stirred uniformly to obtain the electrolyte of Example 1.
[0277] 6) Preparation of batteries
[0278] The positive electrode sheet, separator, and negative electrode sheet of Example 1 are stacked in order, with the separator placed between the positive and negative electrode sheets to serve as an isolation. The cells are then wound to obtain battery cells, the tabs are welded to the battery cells, and the battery cells are placed in an aluminum shell. The electrolyte is then injected and sealed. After standing, cold pressing, formation, shaping, capacity testing, and other processes, a lithium-ion secondary battery is obtained.
[0279] Example 2-26
[0280] The battery preparation method of Example 2-26 is similar to that of Example 1, but the components, component contents, weight-average molecular weight, and mass percentage of the binder based on the positive electrode active material in the grafted polymer are adjusted. The specific adjustment parameters are shown in Table 1 below, wherein Examples 2-5 adjust the mass of trifluorochloroethylene added during the preparation of the intermediate polymer to adjust the mass percentage of trifluorochloroethylene; Examples 6-12 adjust the total mass of acrylic acid, acrylamide, and ethyl acrylate added to the grafting reaction to adjust the mass content of the branched polymer; Examples 13-16 adjust the reaction time and reaction temperature of the intermediate polymer of polyvinylidene fluoride-trifluorochloroethylene to adjust the weight-average molecular weight of the grafted polymer, specifically:
[0281] The reaction time of Example 13 was 2 h and the reaction temperature was 38° C.
[0282] The reaction time of Example 14 was 3.5 h and the reaction temperature was 38° C.
[0283] The reaction time of Example 15 was 6 h and the reaction temperature was 38°C;
[0284] The reaction time of Example 16 was 8 h and the reaction temperature was 37° C.
[0285] Examples 17-20 adjusted the mass fraction of the binder;
[0286] Examples 21-26 adjusted the types of monomers added in the grafting reaction. See Table 1 for specific parameters.
[0287] Comparative Example 1
[0288] The battery of Comparative Example 1 was prepared in a similar manner to that of Example 1, except that the binder was polyvinylidene fluoride, the specific parameters of which are shown in Table 1, and which was purchased from Solvay Group.
[0289] Comparative Example 2
[0290] The battery of Comparative Example 2 was prepared in a similar manner to that of Example 1, except that the binder was polyvinylidene fluoride-trifluoroethylene, with specific parameters shown in Table 1, purchased from Solvay Group.
[0291] Comparative Example 3
[0292] The preparation method of the battery of Comparative Example 3 is similar to that of the battery of Example 1, but there is a difference in the preparation method of the grafted polymer. The specific preparation method is:
[0293] In a 50 ml two-necked flask purged with N2, 10 g of the intermediate polymer of polyvinylidene fluoride-chlorotrifluoroethylene was dissolved in N-methylpyrrolidone, and then 0.87 g of acrylic acid, acrylamide and ethyl acrylate (monomer molar ratio of 1:1:1), 0.19 g of CuCl, 0.19 g of CuCl2 and 0.92 g of 2,2-bipyridine were added to react at a temperature of 140°C and a reaction time of 24 h. The product was washed with water and dried to obtain a grafted polymer.
[0294] Comparative Example 4
[0295] The battery of Comparative Example 4 is prepared in a similar manner to that of Example 1, except that the binder is polyacrylic acid-acrylamide-ethyl acrylate, wherein the preparation method of polyacrylic acid-acrylamide-ethyl acrylate is:
[0296] Azobisisobutyronitrile (AIBN) at 1% monomer weight was dissolved in 300 ml of anhydrous acetonitrile, and the solution was then introduced into a high-pressure reactor and purged with N2 for 30 minutes. Subsequently, acrylic acid monomer, acrylamide monomer, and ethyl acrylate monomer were weighed and transferred to the reactor at a molar ratio of 1:1:1 at room temperature. The temperature inside the reactor was raised to 85°C, and the reaction mixture was stirred at 500 rpm for another 8 hours. The reactor was cooled to room temperature with water and decompressed to remove unreacted monomer. The solvent was removed in vacuo, and the resulting solid was washed several times with chloroform to remove initiator residues. Finally, the polymer was vacuum-dried at 45°C to obtain polyacrylic acid-acrylamide-ethyl acrylate.
[0297] Comparative Example 5
[0298] The battery of Comparative Example 5 was prepared in a similar manner to that of Example 1, except that the polyvinylidene fluoride-trifluoroethylene in Comparative Example 2 and the polyacrylic acid-acrylamide-ethyl acrylate in Comparative Example 4 were physically mixed to obtain a binder, wherein the mass fraction of the polyacrylic acid-acrylamide-ethyl acrylate was 8%, based on the total mass of the binder.
[0299] Comparative Example 6
[0300] The preparation method of the battery of Comparative Example 6 is similar to that of the battery of Example 1, but the binder is polyvinylidene fluoride-trifluoroethylene-acrylic acid-acrylamide-ethyl acrylate. The specific preparation method is:
[0301] Azobisisobutyronitrile (AIBN) at 1% monomer weight was dissolved in 300 mL of anhydrous acetonitrile. The solution was then introduced into a high-pressure reactor and purged with N2 for 30 minutes. Vinylidene fluoride and trifluoroethylene were then added at a mass ratio of 80:20 at room temperature. The reactor temperature was raised to 85°C, and the reaction mixture was stirred at 500 rpm for an additional 3 hours. Acrylic acid, acrylamide, and ethyl acrylate were weighed and transferred to the reactor at a molar ratio of 1:1:1. The total mass fraction of acrylic acid, acrylamide, and ethyl acrylate was 8%, based on the total mass of vinylidene fluoride, trifluoroethylene, acrylic acid, acrylamide, and ethyl acrylate. The mixture was stirred at 500 rpm for an additional 7 hours. The reactor was cooled to room temperature with water and depressurized to remove unreacted monomer. The solvent was removed under vacuum, and the resulting solid was washed multiple times with chloroform to remove initiator residues. Finally, the polymer was vacuum-dried at 45°C to yield polyvinylidene fluoride-trifluoroethylene-acrylic acid-acrylamide-ethyl acrylate.
[0302] 2. Performance Testing
[0303] 1. Polymer detection
[0304] 1) Weight average molecular weight (W g / mol) test method
[0305] A Waters 2695 Isocratic HPLC gel chromatography instrument (differential refractive index detector 2141) was used. A 3.0% polystyrene solution sample was used as a reference, and a matching chromatographic column was selected (oil-based: Styragel HT5 DMF 7.8×300mm + Styragel HT4). A 3.0% polymer gel was prepared using purified N-methylpyrrolidone (NMP) solvent. The prepared solution was allowed to stand for one day before use. During testing, tetrahydrofuran was first drawn into the syringe and rinsed several times. Then, 5 ml of the experimental solution was drawn, the air in the syringe was expelled, and the needle tip was wiped dry. Finally, the sample solution was slowly injected into the injection port. Data was acquired after the reading stabilized.
[0306] 2) β-crystal content
[0307] The β-crystal content was tested by FTIR. Specifically, the FTIR test instrument was a Nieolet 5700 infrared spectrometer, with 32 infrared scans and a spectrum wave number range of 700-4000 cm -1 , resolution is 4cm -1 From the obtained spectrum, the wave number 765cm, which is the characteristic absorption of α crystal form, was determined. -1 The absorption intensity and the wave number 840 cm-1, which is the characteristic absorption of β crystal form -1 The absorption intensity of each peak corresponding to the above wavenumber is obtained by connecting the starting and ending points of the formation with a straight line. The intersection of this straight line and the peak wavenumber is set as A, the point where the spectrum intersects the peak wavenumber is set as B, and the point where the transmittance at the peak wavenumber is 0% is set as C. The lengths between AC and BC are calculated, and Log(AC / BC) is used as the absorption intensity at each wavenumber.
[0308] The content of β crystal is as described above, and the wave number 765cm corresponding to α crystal and β crystal is obtained. -1 and wave number 840cm -1 The absorption intensity is calculated by substituting it into the following formula:
[0309] β-crystal content = 840 cm -1 Absorption intensity / (765cm -1 Absorption intensity +840cm - 1 absorption intensity)×100%.
[0310] 2. Slurry performance test
[0311] 1) Slurry viscosity test
[0312] After the slurry is shipped, take 500 ml of the slurry and place it in a beaker. Use a rotational viscometer, select the rotor, set the speed to 12 rpm, and set the rotation time to 5 minutes. After the value stabilizes, read and record the viscosity value.
[0313] 2) Slurry stability test
[0314] After re-stirring the slurry for 30 minutes, take a certain amount of slurry and pour it into the sample bottle of the stability instrument. After putting it into the sample bottle, close the test tower cover. Open the test tower cover, and a scanning curve will begin to appear on the test interface, and the sample stability test will begin. The test will continue for more than 48 hours to complete the test.
[0315] 3. Pole performance test
[0316] 1) Diaphragm resistance test
[0317] Cut small 3mm x 3mm discs from the left, center, and right sides of the electrode. Turn on the indicator light on the Yuanneng Technology electrode resistance meter, place the probe in the appropriate position on the membrane resistance meter, click the "Start" button, and wait for the reading to stabilize before reading. Test two positions on each disc. Calculate the average of the six measurements to obtain the membrane resistance of the electrode.
[0318] 2) Adhesion test
[0319] With reference to the national standard GBT 2790-1995 "Test method for 180° peel strength of adhesives", the adhesion test process of the examples and comparative examples of the present application is as follows:
[0320] Use a blade to cut a 30mm wide and 100-160mm long electrode sample. Apply a 20mm wide and 90-150mm long double-sided tape to the steel plate. Attach the previously cut electrode sample to the double-sided tape with the test surface facing down. Then use a roller to roll the sample three times in the same direction.
[0321] Insert a paper tape with a width equal to that of the electrode sample and a length of 250 mm under the electrode current collector and fix it with wrinkle glue.
[0322] Turn on the Sansi tensile testing machine (sensitivity 1N), the indicator light will illuminate, adjust the limit block to the appropriate position, and secure the end of the steel plate specimen without the electrode with the lower clamp. Fold the paper tape upward and secure it with the upper clamp. Use the "up" and "down" buttons on the manual controller included with the tensile testing machine to adjust the position of the upper clamp, then perform the test and read the value. The force at the electrode when the force is balanced is divided by the width of the tape as the bonding force per unit length of the electrode, which represents the bonding strength between the positive electrode film layer and the current collector.
[0323] 3) Cohesion test
[0324] Cut the positive electrode sheet into a 100mm long and 10mm wide sample. Take a 25mm wide stainless steel plate and affix the sample to the plate with 3M double-sided tape (11mm wide), with the current collector bonded to the double-sided tape. Roll the sample back and forth three times with a 2000g roller (300mm / min). Then, apply a 10mm wide, 50μm thick tape (NITTO.NO5000NS) to the surface of the positive electrode film and roll it back and forth three times with a 2000g roller (300mm / min). Bend the tape 180 degrees and manually peel 25mm off the tape and the positive electrode film. The sample was then mounted on an Instron 336 tensile testing machine, aligning the peeling surface with the tester's force line (i.e., performing a 180° peel). After pre-pulling for 10mm at a peeling speed of 100mm / min, the tensile testing machine was reset, and the sample was peeled continuously at 300mm / min to obtain a cohesion curve. The average value of the plateau was taken as the peeling force F0, and the cohesion F1 of the tested electrode was calculated using the following formula: F1 = F0 / width of the sample to be tested, with F1 measured in N / m.
[0325] 4) Flexibility testing
[0326] The cold-pressed positive electrode sheet is cut into test specimens of 20mm×100mm size; after folding it in the forward direction, flatten it with a 2kg roller, and unfold it to check whether there is light transmittance through the gap. If there is no light transmittance, fold it in the reverse direction, flatten it with a 2kg roller, and check again against the light. Repeat this process until light transmittance appears in the gap, and record the number of folding times; repeat the test three times, and take the average value as the reference data for the flexibility of the electrode sheet.
[0327] 5) Liquid absorption rate
[0328] Cut the cold-pressed positive electrode into test samples of 5cm×5cm size; first, dry the sample at 80℃ for 4h, test the thickness of the electrode, and then fix it on the sample table. Then select a capillary with d=200μm and polish the end face with 5000-grit sandpaper until it is flat. Use a microscope to observe the state between the capillary and the electrode; use the capillary to absorb the electrolyte, control the electrolyte height h=3mm, lower the capillary to contact the electrode, and use a stopwatch to time it. When the liquid level drops, stop the timer, read the liquid absorption time t, and record the data; use the formula to calculate the average liquid absorption rate v of the electrode, v=π×(d / 2)2×h×ρ / t. The electrolyte density is 1.194g / cm 3 .
[0329] 4. Battery performance test
[0330] 1) Battery cycle capacity retention rate (500ds) test
[0331] The battery capacity retention rate test process is as follows: at 25°C, the prepared battery is charged to 4.3V at a constant current of 1 / 3C, then charged to a current of 0.05C at a constant voltage of 4.3V, left for 5 minutes, and then discharged to 2.8V at 1 / 3C. The obtained capacity is recorded as the initial capacity C0. Repeat the above steps for the same battery mentioned above, and at the same time record the discharge capacity Cn of the battery after the nth cycle. The battery capacity retention rate after each cycle is Pn = Cn / C0 × 100%. The 500 point values P1, P2...P500 are used as the vertical coordinates, and the corresponding number of cycles is used as the horizontal coordinates to obtain a curve graph of the battery capacity retention rate and the number of cycles. During this test process, the first cycle corresponds to n = 1, the second cycle corresponds to n = 2, ... the 500th cycle corresponds to n = 500. The battery capacity retention rate data corresponding to the embodiment or comparative example in Table 2 are the data measured after 500 cycles under the above test conditions, that is, the value of P500. The test process of the comparative example and other embodiments is the same as above.
[0332] 2) Battery DC impedance growth rate (100cls) test
[0333] The battery DC impedance test process is as follows: At 25°C, charge the battery at a constant current of 1 / 3C to 4.3V, then charge it at a constant voltage of 4.3V to a current of 0.05C. After 5 minutes, record the voltage V1. Then discharge it at 1 / 3C for 30 seconds, record the voltage V2, and then calculate the internal resistance DCR1 of the battery after the first cycle as (V2-V1) / 1 / 3C. Repeat the above steps for the same battery and simultaneously record the internal resistance DCRn of the battery after the nth cycle (n=1, 2, 3...100). The 100 points DCR1, DCR2, DCR3...DCR100 are plotted as the vertical axis and the corresponding number of cycles as the horizontal axis to obtain a curve of the battery discharge DCR and the number of cycles.
[0334] During this test, the first cycle corresponds to n=1, the second cycle corresponds to n=2, and so on and so forth. The battery internal resistance increase ratio for Example 1 in Table 1 = (DCRn - DCR1) / DCR1 × 100%. The testing procedures for Comparative Example 1 and the other examples are the same as above. The data in Table 2 were measured after 100 cycles under the above test conditions.
[0335] 3. Analysis of test results of various embodiments and comparative examples
[0336] The graft polymer, binder, positive electrode slurry, positive electrode sheet and secondary battery of each embodiment and comparative example were prepared according to the above method, and various parameters were measured. The results are shown in Tables 1 and 2 below.
[0337] Table 1 Preparation parameters and characterization parameters of Examples and Comparative Examples
[0338] Table 2 Preparation parameters and performance characteristics of examples and comparative examples
[0339] From the above table, it can be seen that the graft polymers in Examples 1-26 include main chain polymers and branched polymers. The main chain polymers include The structural unit of the branched polymer includes One or more structural units.
[0340] From the comparison of Examples 1-16, 21-26 with Comparative Example 1, it can be seen that compared with the traditional polyvinylidene fluoride binder, the grafted polymer of the present application can increase the content of β crystal form, improve the flexibility of the electrode, increase the liquid absorption rate of the electrode, reduce the DC impedance growth rate of the battery, and improve the cycle capacity retention rate of the battery.
[0341] From the comparison of Examples 1, 6-12, 21-26 with Comparative Example 2, it can be seen that compared with polyvinylidene fluoride-trifluoroethylene that does not contain branched polymers, the grafted polymer of the present application can increase the content of β crystal form, improve the adhesion, cohesion and flexibility of the electrode, increase the liquid absorption rate of the electrode, reduce the DC impedance growth rate of the battery, and improve the cycle capacity retention rate of the battery.
[0342] From the comparison between Example 1 and Comparative Example 3, it can be seen that the graft polymer in Comparative Example 3 includes a main chain polymer and a branched polymer. The main chain polymer includes Branched polymers include Compared with comparative example 3, the grafted polymer of the present application can increase the content of β crystal form, improve the adhesion, cohesion and flexibility of the electrode, reduce the diaphragm resistance of the electrode, increase the liquid absorption rate of the electrode, reduce the DC impedance growth rate of the battery, and improve the cycle capacity retention rate of the battery.
[0343] From the comparison of Examples 1-12 and Comparative Example 4, it can be seen that compared with polyacrylic acid-acrylamide-ethyl acrylate, the graft polymer of the present application can improve the cohesion and flexibility of the electrode, increase the liquid absorption rate of the electrode, and reduce the DC impedance growth rate of the battery.
[0344] From the comparison between Example 1 and Comparative Example 5, it can be seen that compared with the blend of polyacrylic acid-acrylamide-ethyl acrylate and polyvinylidene fluoride-trifluoroethylene, the grafted polymer of the present application can increase the content of β crystal form, can increase the cohesion and flexibility of the electrode, increase the liquid absorption rate of the electrode, reduce the DC internal resistance growth rate of the battery, and improve the cycle capacity retention rate of the battery.
[0345] From the comparison between Example 1 and Comparative Example 6, it can be seen that compared with polyvinylidene fluoride-trifluoroethylene-acrylic acid-acrylamide-ethyl acrylate, the grafted polymer of the present application can increase the content of β crystal form, can improve the cohesion, adhesion and flexibility of the electrode, increase the liquid absorption rate of the electrode, reduce the DC impedance growth rate of the battery, and improve the cycle capacity retention rate of the battery.
[0346] From the comparison between Examples 1, 3-12 and Example 2, it can be seen that based on the total content of α-crystal and β-crystal in the grafted polymer, the content of β-crystal in the grafted polymer is 32%-74%, which can reduce the film resistance of the electrode.
[0347] From the comparison of Examples 1, 21-24, 26 and Example 25, it can be seen that compared with the branched polymer containing The structural unit of the branched polymer contains It can increase the content of β crystal, increase the viscosity of slurry, increase the cohesion and flexibility of the pole piece, increase the liquid absorption rate of the pole piece, and reduce the DC impedance growth rate of the battery.
[0348] As can be seen from Examples 1, 6-12, when the mass content of the branched polymer is 1%-30% based on the total mass of the grafted polymer, the electrode has excellent adhesion, cohesion, and flexibility, the electrode has low membrane resistance, the electrode has excellent liquid absorption rate, and the battery has a low DC impedance growth rate and a high cycle capacity retention rate. As can be seen from the comparison of Examples 1, 8-10 with Examples 6-7, 11-12, when the mass content of the branched polymer is 5%-25% based on the total mass of the grafted polymer, the adhesion of the electrode can be improved, the DC impedance growth rate of the battery can be reduced, and the cycle capacity retention rate of the battery can be improved.
[0349] As can be seen from Examples 1, 13-16, the weight-average molecular weight of the grafted polymer is 600,000-2,000,000, the electrode has excellent adhesion, cohesion, and flexibility, the electrode has low sheet resistance, the electrode has excellent liquid absorption rate, and the battery has a low DC impedance growth rate and a high cycle capacity retention rate. As can be seen from the comparison of Examples 1, 14-15, and 16 with Example 13, the weight-average molecular weight of the grafted polymer is 800,000-2,000,000, which can improve the stability of the slurry, improve the anti-gel properties of the slurry, reduce the sheet resistance of the electrode, improve the adhesion and cohesion of the electrode, and reduce the DC impedance growth rate of the battery.
[0350] As can be seen from Examples 1 and 17-20, the grafted polymer binder has a mass percentage of 0.4%-2% based on the mass of the positive electrode active material, resulting in excellent bonding, cohesion, and flexibility of the electrode sheet, low sheet resistance, and excellent liquid absorption rate. The battery has a low DC impedance growth rate and high cycle capacity retention. Comparing Examples 1, 18-19 with Examples 17 and 20, it can be seen that the grafted polymer binder has a mass percentage of 0.8%-1.6% based on the mass of the positive electrode active material, the slurry has an appropriate viscosity, reducing the sheet resistance of the battery.
[0351] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A graft polymer, It is characterized in that It comprises a main chain polymer and a branched chain polymer, wherein the main chain polymer comprises a structural unit shown in formula I, and the branched chain polymer comprises a structural unit shown in formula II, Wherein, the wavy line in Formula I represents the junction position between the main chain polymer and the branched polymer, R 1 , R 2 Each independently contains hydrogen, fluorine, C containing at least one fluorine atom 1- 3 One or more of the alkyl groups, R 3 , R 4 , R 5 Each independently contains hydrogen, substituted or unsubstituted C 1-5 One or more of the alkyl groups, R 6 Contains hydrogen, substituted or unsubstituted C 1-5 Alkyl, ester, carboxyl, amide, cyano, hydroxyl, substituted or unsubstituted C 6-30 One or more aromatic groups.
2. The graft polymer according to claim 1, It is characterized in that The content of the β crystal form in the graft polymer is 32% to 74%, based on the total content of the α crystal form and the β crystal form in the graft polymer.
3. The graft polymer according to claim 1 or 2, It is characterized in that The main chain polymer also includes a structural unit shown in formula III, Among them, R 7 , R 8 , R 9 Each independently contains hydrogen, fluorine, C containing at least one fluorine atom 1-3 One or more of the alkyl groups.
4. The graft polymer according to any one of claims 1 to 3, It is characterized in that The R 6 Containing ester, carboxyl, amide, cyano, hydroxyl, substituted or unsubstituted C 6-12 One or more aromatic groups.
5. The graft polymer according to any one of claims 1 to 4, It is characterized in that The mass content of the branched polymer is 1%-30% based on the total mass of the grafted polymer.
6. The graft polymer according to any one of claims 1 to 4, It is characterized in that Based on the total mass of the grafted polymer, the mass content of the branched polymer is 5%-25%.
7. The graft polymer according to any one of claims 1 to 6, It is characterized in that The weight average molecular weight of the grafted polymer is 600,000-2,000,000.
8. The graft polymer according to any one of claims 1 to 6, It is characterized in that The weight average molecular weight of the grafted polymer is 800,000-2,000,000.
9. The graft polymer according to any one of claims 1 to 8, It is characterized in that The structural unit shown in Formula I comprises At least one of .
10. The graft polymer according to any one of claims 1 to 9, It is characterized in that The structural unit shown in formula II includes At least one of .
11. The graft polymer according to any one of claims 3 to 10, It is characterized in that The structural unit shown in formula III includes At least one of .
12. The graft polymer according to any one of claims 1 to 11, It is characterized in that The graft polymer includes one or more of polyvinylidene fluoride-trifluoroethylene-g-polyacrylic acid, polyvinylidene fluoride-trifluoroethylene-g-polypropylene, polyvinylidene fluoride-trifluoroethylene-g-polystyrene, polyvinylidene fluoride-trifluoroethylene-g-polyvinyl alcohol, polyvinylidene fluoride-trifluoroethylene-g-polyacrylamide, polyvinylidene fluoride-trifluoroethylene-g-polyacrylonitrile, polyvinylidene fluoride-trifluoroethylene-g-polymethyl methacrylate, polyvinylidene fluoride-trifluoroethylene-g-polyacrylic acid-acrylamide-ethyl acrylate, polyvinylidene fluoride-trifluoroethylene-g-polyacrylonitrile-ethyl acrylate, polyvinylidene fluoride-trifluoroethylene-g-polypropylene-methyl methacrylate, polyvinylidene fluoride-trifluoroethylene-g-polyacrylic acid-methyl methacrylate, polyvinylidene fluoride-trifluoroethylene-g-polyacrylic acid-methyl methacrylate, polyvinylidene fluoride-trifluoroethylene-g-polyvinyl alcohol-styrene, and polyvinylidene fluoride-trifluoroethylene-g-polyacrylic acid-acrylamide-methyl methacrylate.
13. A method for preparing a grafted polymer, It is characterized in that The following steps are involved: Under polymerizable conditions, a first reactant including at least one structural unit represented by formula V is subjected to a grafting reaction with a second reactant including at least one monomer represented by formula VI to prepare the graft polymer, Among them, R 1 , R 2 Each independently contains hydrogen, fluorine, C containing at least one fluorine atom 1- 3 One or more of the alkyl groups, R 3 , R 4 , R 5 Each independently contains hydrogen, substituted or unsubstituted C 1-5 One or more of the alkyl groups, R 6 Contains hydrogen, substituted or unsubstituted C 1-5 Alkyl, ester, carboxyl, amide, cyano, substituted or unsubstituted C 6-30 One or more aromatic groups.
14. The preparation method according to claim 13, It is characterized in that The first reactant further comprises at least one structural unit represented by formula III, Among them, R 7 , R 8 , R 9 Each independently contains hydrogen, fluorine, C containing at least one fluorine atom 1-3 One or more of the alkyl groups.
15. The preparation method according to claim 13 or 14, It is characterized in that Based on the total mass of the first reactant and the second reactant, the mass percentage of the second reactant is 1%-30%.
16. The preparation method according to any one of claims 13 to 15, It is characterized in that The preparation method of the first reactant comprises a hydrogenation reaction and an elimination reaction, Hydrogenation reaction: hydrogenating the intermediate polymer containing the structural unit shown in formula VII to obtain a hydrogenated intermediate polymer containing the structural unit shown in formula VIII, Elimination reaction: subjecting the hydrogenated intermediate polymer to an elimination reaction to prepare the first reactant; Among them, R 1 , R 2 Each independently contains hydrogen, fluorine, C containing at least one fluorine atom 1- 3 One or more of the alkyl groups.
17. The preparation method according to claim 16, It is characterized in that The hydrogenation reaction specifically comprises the following steps: The intermediate polymer and the first catalyst are subjected to the hydrogenation reaction in a first solvent to obtain the hydrogenated intermediate polymer.
18. The preparation method according to claim 16 or 17, It is characterized in that The elimination reaction specifically comprises the following steps: The hydrogenated intermediate polymer, the second catalyst, and the ligand are subjected to the elimination reaction in a second solvent to obtain the first reactant.
19. The preparation method according to any one of claims 16 to 18, It is characterized in that The preparation method of the intermediate polymer specifically comprises the following steps: Under polymerizable conditions, the monomer represented by formula IX and the monomer represented by formula X are polymerized to form the intermediate polymer, Among them, R 1 , R 2 Each independently contains hydrogen, fluorine, C containing at least one fluorine atom 1- 3 One or more of the alkyl groups.
20. The preparation method according to claim 19, It is characterized in that Based on the total mass of the monomer represented by formula IX and the monomer represented by formula X, the mass percentage of the monomer represented by formula X is 1%-30%.
21. A binder, It is characterized in that The binder comprises the graft polymer according to any one of claims 1 to 12 or the graft polymer prepared by the preparation method according to any one of claims 13 to 20.
22. Use of the graft polymer according to any one of claims 1 to 12 in a secondary battery.
23. A positive electrode sheet, comprising a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode film layer comprises a positive electrode active material, a conductive agent and a binder, It is characterized in that The binder comprises the graft polymer according to any one of claims 1 to 12 or the graft polymer prepared by the preparation method according to any one of claims 13 to 20.
24. The positive electrode sheet according to claim 23, It is characterized in that Based on the mass of the positive electrode active material, the mass percentage of the binder is 0.4%-2%.
25. The positive electrode sheet according to claim 23, It is characterized in that Based on the mass of the positive electrode active material, the mass percentage of the binder is 0.8%-1.6%. 26 . The positive electrode sheet according to claim 23 , wherein the bonding force per unit length between the positive electrode film layer and the positive electrode current collector is not less than 7.5 N / m.
27. The positive electrode sheet according to any one of claims 23 to 26, It is characterized in that The bonding force per unit length between the positive electrode film layer and the positive electrode current collector is not less than 9 N / m.
28. The positive electrode sheet according to any one of claims 23 to 27, It is characterized in that The cohesive force of the positive electrode plate is not less than 65 N / m.
29. The positive electrode sheet according to any one of claims 23 to 27, It is characterized in that The cohesive force of the positive electrode sheet is not less than 100 N / m.
30. The positive electrode sheet according to any one of claims 23 to 29, It is characterized in that The electrolyte absorption rate of the positive electrode plate is greater than 0.32 μg / s, and the density of the electrolyte is 1.1-1.3 g / cm 3 .
31. The positive electrode sheet according to any one of claims 23 to 29, It is characterized in that The electrolyte absorption rate of the positive electrode plate is greater than 0.35 μg / s, and the density of the electrolyte is 1.1-1.3 g / cm 3 .
32. A secondary battery, It is characterized in that It comprises an electrode assembly and an electrolyte, wherein the electrode assembly comprises a separator, a negative electrode sheet and a positive electrode sheet as claimed in any one of claims 23 to 31.
33. An electrical device, It is characterized in that Includes the secondary battery as claimed in claim 32.
Citation Information
Patent Citations
Copolymer for polymer electrolyte, gel polymer electrolyte comprising same, and lithium secondary battery
CN113906065A
Graft polymer, preparation method, binder, positive pole piece, secondary battery and electric device
CN116355147A
Production of fluorine-containing graft copolymer
JP1994087935A
Graft copolymer, binder composition for secondary battery, separator for secondary battery, secondary battery and manufacturing method of graft copolymer
JP2017115102A
apparatus and system for charging battery of transportation means using electronic power
KR102183183B1
Cited By
High-energy-density self-repairing long-circulation positive pole piece, preparation method, application and lithium ion battery