Composition and use thereof
By grinding the semiconductor substrate using a modified oxide particle-modified composition, the problems of slow silicon nitride removal rate and high defect value are solved, and efficient silicon nitride removal and low defect surface treatment are achieved.
Patent Information
- Application Number
- PCT/CN2024/095344
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-30
- Filing Date
- 2024-05-24
- Publication Date
- 2024-12-05
AI Technical Summary
In the process of electronic product manufacturing, the removal rate of silicon nitride is slow and the defect value on the substrate surface after grinding is high. Traditional silicon sols and commercially modified silica abrasives have insufficient mechanical effects and high defects.
Provided is a composition including modified oxide particles, pH adjusting agents and solvents that are modified by negatively charged modified groups of specific structures for grinding of semiconductor substrates, enhancing electrostatic attraction and chemical corrosion. Increase the removal rate of silicon nitride and reduce the defect value.
The removal rate and flattening effect of silicon nitride are significantly improved, and the residual particles on the surface of the semiconductor substrate after grinding are reduced, and a lower defect value and a higher removal selection ratio are obtained.
Smart Images

Figure CN2024095344_05122024_PF_FP_ABST
Abstract
Description
Composition and application thereof
[0001] This application claims priority to the Chinese patent application filed with the State Intellectual Property Office of China on May 30, 2023, with application number 202310623934.X and application name “Compositions and Their Applications”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The embodiments of the present application relate to the technical field of electronic product manufacturing, and in particular to a composition and its application. Background Art
[0003] The manufacturing process of electronic products usually involves surface treatment processes that involve grinding materials such as metals, silicon, silicon oxide, polysilicon, and silicon nitride. This process requires controlling the removal rate of each material based on the structure of the product. Among them, silicon nitride (SiN) has a high hardness. When it is ground using traditional silica sol, the mechanical interaction between the silica sol and the grinding layer is weak, resulting in a slow SiN removal rate. While the use of currently commercially available sulfonic acid-modified silica improves the SiN removal rate compared to traditional silica sol, the defect value on the substrate surface after grinding is high. In order to better meet process requirements, it is necessary to provide a new abrasive to increase the SiN removal rate and obtain a lower defect value.
[0004] Summary of the Invention
[0005] In view of this, an embodiment of the present application provides a composition comprising oxide particles modified by special structural groups. The composition can be used for grinding various semiconductor substrates, especially for grinding silicon nitride, to increase the removal rate of silicon nitride and obtain a lower defect value.
[0006] Specifically, a first aspect of an embodiment of the present application provides a composition comprising modified particles, a pH adjuster, and a solvent, wherein the modified particles comprise oxide particles and a modifying group represented by formula (1) bound to the oxide particles;
[0007] In formula (1), X is selected from phosphorus, arsenic, antimony, and bismuth; R1 is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkoxy, substituted or unsubstituted aryl, and substituted or unsubstituted aryloxy; R2 is selected from H, NH4, Li, Na, K, substituted or unsubstituted alkyl, and substituted or unsubstituted aryl; R3 is selected from substituted or unsubstituted alkylene, substituted or unsubstituted alkyleneoxy, substituted or unsubstituted arylene, and substituted or unsubstituted aryleneoxy;
[0008] The oxide particles include any one of silicon dioxide particles, aluminum oxide particles, zinc oxide particles, titanium dioxide particles, zirconium dioxide particles, and cerium oxide particles.
[0009] The composition of the embodiment of the present application can be used to perform surface smoothing treatment on semiconductor substrates in the process of preparing electronic products, that is, the composition of the embodiment of the present application is a liquid smoothing composition, which uses modified oxide particles as abrasives, wherein the modified oxide particles are modified by the negatively charged modified groups of the structure shown in formula (1) to obtain oxide particles. The modified oxide particles can generate a strong electrostatic attraction between their negative charge and the surface of the semiconductor substrate to be processed, thereby facilitating the mechanical grinding effect; at the same time, the negatively charged modified groups of the structure shown in formula (1) can act as nucleophiles to attack the positively charged semiconductor substrate material, thereby facilitating the hydrolysis of the semiconductor substrate material and the breaking of the chemical bonds; the above two aspects can greatly improve the removal rate of the semiconductor substrate material. The composition can be used to perform surface smoothing treatment on various semiconductor substrates in the process of preparing electronic products, in particular, it can be used for grinding semiconductor substrates with positive charges on the surface, improving the removal rate of semiconductor substrate materials with positive charges on the surface, for example, it can be used for grinding silicon nitride, improving the removal rate of silicon nitride. In addition, since the negatively charged modified group of the structure shown in formula (1) of the present application has a low degree of ionization, it can reduce the residual particles on the surface of the semiconductor substrate after grinding, making it easier to clean, obtain a lower defect value, and improve the flattening effect.
[0010] In an embodiment of the present application, the content of X atoms in the modified particles, as measured by X-ray photoelectron spectroscopy, is greater than or equal to 0.01 atomic % (atomic percentage) and less than or equal to 30 atomic %. That is, the atomic percentage of X atoms in the modified particles characterized by X-ray photoelectron spectroscopy is between 0.01% and 30%. The X atoms are derived from the modifying groups, and an appropriate amount of X atoms indicates that an appropriate amount of modifying groups is bound to the surface of the oxide particles. By controlling the atomic percentage of X atoms on the surface of the modified particles within an appropriate range, the embodiments of the present application can achieve a better modification effect and increase the removal rate of the semiconductor substrate material from the composition.
[0011] In embodiments of the present application, the carbon atom content of the modified particles, as measured by X-ray photoelectron spectroscopy, is greater than or equal to 2 atomic % and less than or equal to 45 atomic %. That is, the atomic percentage of carbon atoms in the modified particles, as characterized by X-ray photoelectron spectroscopy, is between 2% and 45%. Carbon atoms originate from the modifying groups, and an appropriate carbon atom content can reflect the modification amount of the modifying groups. By controlling the atomic percentage of carbon atoms on the surface of the modified particles within an appropriate range, embodiments of the present application can achieve a better modification effect and increase the removal rate of the semiconductor substrate material from the composition.
[0012] In an embodiment of the present application, the oxide particles are silica particles, and the ratio of the number of X atoms to silanol groups on the modified particles is greater than or equal to 0.4% and less than or equal to 48%. The ratio of the number of X atoms to silanol groups on the surface of the modified particles can reflect the relationship between the number of modified groups and the number of remaining silanol groups on the surface of the silica particles after modification. In the embodiments of the present application, by controlling the ratio of the number of X atoms to silanol groups on the surface of the modified particles within a suitable range, a good modification effect can be achieved, thereby improving the removal rate and / or selectivity of the composition for semiconductor substrate materials with positively charged surfaces.
[0013] The ratio of the number of X atoms to the number of silanol groups on the surface of the modified particles can be obtained by the following characterization and calculation:
[0014] The X element content of the modified particles is determined using inductively coupled plasma emission spectroscopy (ICP). The number of X atoms per unit weight of the modified particles is then converted to the number of silanol groups. The number of silanol groups per unit weight of the modified particles can then be determined using commonly available titration methods (such as acid-base titration and potentiometric titration). The ratio of the number of X atoms per unit weight of the modified particles to the number of silanol groups per unit weight of the modified particles is obtained by dividing the number of X atoms per unit weight of the modified particles by the number of silanol groups per unit weight of the modified particles.
[0015] In embodiments of the present application, the modifying groups are chemically bonded to the oxide particles. Chemical bonding of the modifying groups to the oxide particle surfaces allows the modifying groups with specific properties to be stably present on the oxide particle surfaces, thereby providing a uniform and stable planarization effect when the modified particles are used to treat the surface of a semiconductor substrate. The chemical bonding may be covalent bonding.
[0016] In an embodiment of the present application, the average particle size of the modified particles measured by dynamic light scattering (DLS) is 5nm-500nm (i.e., greater than or equal to 5nm and less than or equal to 500nm). The average particle size measured by the dynamic light scattering method can be understood as the average particle size of secondary particles formed by the aggregation or association of primary particles. In one embodiment of the present application, the modified particles are modified silica particles, and the modified particles are modified colloidal silica. The modified particles have a smaller particle size, which is beneficial to reducing the generation of scratches on the surface of the semiconductor substrate (such as a semiconductor substrate) during the grinding process and improving the grinding quality. In some embodiments of the present application, the average particle size of the modified particles is 10nm-300nm. In some embodiments of the present application, the average particle size of the modified particles is 20nm-200nm. In some embodiments of the present application, the average particle size of the modified particles is 25nm-100nm. The modified particles have a suitable particle size, which can better balance the smoothing rate and surface scratch problems.
[0017] In the embodiment of the present application, the weight proportion of the modified particles in the composition is 0.1% to 50%. The modified particles, as abrasives, have a direct impact on the planarization effect. The appropriate amount of modified particles in the composition is conducive to generating sufficient chemical corrosion and mechanical friction to achieve efficient removal of the semiconductor substrate, while maintaining suitable fluidity of the composition and high uniformity of the modified particles in the composition.
[0018] In the embodiment of the present application, the pH of the composition is less than 12. The pH of the composition of the present application can be adjusted by a pH adjuster, and the pH of the composition can be controlled at a suitable value, which is beneficial to improving the removal rate of the semiconductor substrate.
[0019] In some embodiments of the present application, the pH of the composition is 1-6. Since the composition of the present application uses oxide particles modified with a modifying group having a structure represented by formula (1) as an abrasive, and since most semiconductor substrate surfaces are positively charged in practical applications, and since using a negatively charged planarization composition can better promote the improvement of the removal rate of positively charged semiconductor substrates, controlling the pH of the composition to 1-6 is beneficial to improving the removal rate of positively charged semiconductor substrates.
[0020] In an embodiment of the present application, the average degree of association of the modified particles is 1-10 (i.e., greater than or equal to 1 and less than or equal to 10). The average degree of association is the average particle size (nm) of the modified particles divided by the average primary particle size (nm) of the modified particles. The value of the average primary particle size can be calculated based on the specific surface area of the modified particles measured by the BET method, and the average particle size is determined by dynamic light scattering. In the embodiments of the present application, the average degree of association of the modified particles is controlled to be 1-10, which can better avoid the influence of the modified particles on the flattening effect due to dispersibility issues.
[0021] In embodiments of the present application, the composition has a potential in the range of -55 to -5°C. The potential herein refers to the overall potential of the composition, which can be measured using a zeta potential meter using electrophoretic light scattering. Controlling the overall potential of the composition within this range can better minimize the impact of potential factors on the planarization effect.
[0022] In an embodiment of the present application, the substituted or unsubstituted alkyl group is a substituted or unsubstituted C1-C6 alkyl group, the substituted or unsubstituted alkoxy group is a substituted or unsubstituted C1-C6 alkoxy group; the substituted or unsubstituted alkylene group is a substituted or unsubstituted C1-C6 alkylene group, and the substituted or unsubstituted alkyleneoxy group is a substituted or unsubstituted C1-C6 alkyleneoxy group. Controlling the carbon chain length of the substituted or unsubstituted alkyl, substituted or unsubstituted alkoxy, substituted or unsubstituted alkylene, and substituted or unsubstituted alkyleneoxy group in the modifying group within a suitable range is beneficial for controlling the hydrophilic and hydrophobic properties of the modifying group, so that the modified particles can better grind the semiconductor substrate; on the other hand, it is beneficial for the modifying group to better modify the silica particles and avoid the adverse effects caused by excessive steric hindrance of the modifying group.
[0023] In an embodiment of the present application, the pH regulator includes an acid, or a composition formed by an acid and a base or a base salt, and the acid includes an organic acid and / or an inorganic acid. The pH regulator has the function of regulating the pH of the composition. In some embodiments, the pH regulator may include only one or more organic acids; in some embodiments, the pH regulator may include only one or more inorganic acids; in some embodiments, the pH regulator may include both one or more organic acids and one or more inorganic acids. In some embodiments, the pH regulator may also use one or more of the above-mentioned acids in combination with one or more bases or base salts. In the combination of acid and base or base salt, the effect of simultaneously regulating pH and conductivity can be achieved.
[0024] Wherein, organic acid can be various monocarboxylic acids, dicarboxylic acids, tricarboxylic acids, such as but not limited to formic acid, acetic acid, propionic acid, butyric acid, 2-methylbutyric acid, 2-ethylbutyric acid, 3,3-dimethylbutyric acid, valeric acid, 4-methylvaleric acid, n-hexanoic acid, 2-methylhexanoic acid, 2-ethylhexanoic acid, n-heptanoic acid, n-octanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, phthalic acid, malic acid, tartaric acid, citric acid, maleic acid, lactic acid, diglycolic acid. Inorganic acid such as but not limited to hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid and phosphoric acid. Alkali can be amines such as quaternary ammonium hydroxide, aliphatic amine, aromatic amine, alkali metal hydroxide, alkaline earth metal hydroxide and ammonia etc. Alkali salt can use ammonium salt, alkali metal salt etc. of the aforementioned acid.
[0025] It is understood that in order to increase the removal rate of the composition from the semiconductor substrate, the pH adjuster can be an acid selected to be beneficial to increasing the removal rate of the semiconductor substrate, or a combination of an acid and a base or a base salt.
[0026] In the embodiment of the present application, the solvent may include water or an organic solvent. Water and organic solvents serve as dispersion media for the modified particles and other components of the composition. The organic solvent may be any organic solvent that is conducive to the dispersion of the modified particles and other components of the composition.
[0027] In the embodiments of the present application, in order to improve certain aspects of the performance of the composition and better meet the surface planarization treatment of semiconductor substrates in various scenarios, the composition may also include other additives, which may be but are not limited to one or more of catalysts, oxidants, surfactants, preservatives, passivators, and reducing agents.
[0028] In the embodiment of the present application, the mass content of the solvent in the composition is greater than or equal to 50% and less than 100%. A composition with a larger mass content of solvent can have better fluidity, help maintain good dispersion of particles in the composition, and also control the polishing effect of the composition on the semiconductor substrate.
[0029] In the embodiment of the present application, the viscosity of the composition at 25° C. is 1 centipoise to 80 centipoise (cP). The composition having a suitable room temperature viscosity is conducive to its rapid and uniform spreading during the planarization process, which is conducive to sufficient fluidity of the particles in the composition, improves the grinding efficiency, and obtains a better grinding effect.
[0030] In the embodiment of the present application, the removal rate of silicon nitride by the composition is greater than The composition of the embodiment of the present application can achieve high-speed removal of silicon nitride by adding modified particles with a specific structure and utilizing the strong chemical action and mechanical grinding action of the modified particles on silicon nitride, thereby improving the grinding efficiency.
[0031] In embodiments of the present application, the composition has a removal selectivity of greater than 1.5 for silicon nitride and silicon oxide. The composition of the present application has a high removal selectivity for silicon nitride and silicon oxide, and can preferentially remove silicon nitride when performing surface planarization treatment on a semiconductor substrate having both silicon nitride and silicon oxide on its surface.
[0032] The second aspect of the present invention provides an application of the composition described in the first aspect in surface treatment of a semiconductor substrate. The surface treatment is specifically surface flattening treatment, and the composition is used as a polishing liquid.
[0033] In the embodiment of the present application, the application may specifically be to use the composition to perform surface planarization treatment on a semiconductor substrate with a positively charged surface. The use of the composition of the embodiment of the present application can increase the removal rate of the semiconductor substrate material with a positively charged surface.
[0034] In the embodiment of the present application, the application is to use the composition to perform surface treatment on a semiconductor containing nitrogen-silicon bonds on the surface. For example, it can be used for grinding silicon nitride to increase the removal rate of silicon nitride. On the one hand, the modified particles in the embodiment composition of the present application can utilize their negative charge to generate a strong electrostatic attraction between the surface of the semiconductor substrate to be processed with a positive charge, thereby facilitating the mechanical grinding effect; at the same time, the negatively charged modified group can be used as a nucleophilic agent to attack the positively charged semiconductor substrate material, thereby facilitating the hydrolysis of the semiconductor substrate material and the breaking of the chemical bonds; the above two aspects can greatly increase the removal rate of the semiconductor substrate material.
[0035] A third aspect of the present invention provides a surface treatment method, wherein the composition described in the first aspect contacts and polishes the surface of a semiconductor substrate to be treated. This surface treatment method utilizes the composition as a polishing liquid to polish the surface of the semiconductor substrate to be treated. Due to the use of the composition of the present invention, this surface treatment method can improve treatment efficiency and effectiveness.
[0036] The present application also provides a modified particle dispersion for surface treatment of a semiconductor substrate, wherein the modified particle dispersion comprises modified particles and a solvent, wherein the modified particles comprise oxide particles and a modifying group represented by formula (1) bound to the oxide particles;
[0037] In formula (1), X is selected from phosphorus, arsenic, antimony, and bismuth; R1 is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkoxy, substituted or unsubstituted aryl, and substituted or unsubstituted aryloxy; R2 is selected from H, NH4, Li, Na, K, substituted or unsubstituted alkyl, and substituted or unsubstituted aryl; R3 is selected from substituted or unsubstituted alkylene, substituted or unsubstituted alkyleneoxy, substituted or unsubstituted arylene, and substituted or unsubstituted aryleneoxy;
[0038] The oxide particles include any one of silicon dioxide particles, aluminum oxide particles, zinc oxide particles, titanium dioxide particles, zirconium dioxide particles, and cerium oxide particles.
[0039] The modified particle dispersion of the embodiment of the present application can be used as an abrasive raw material to prepare a planarizing composition for surface planarizing treatment of semiconductor substrates. The modified particles in the modified particle dispersion are modified with negatively charged modified groups of a special structure, which can be used for grinding semiconductor substrates with positively charged surfaces, thereby increasing the removal rate of semiconductor substrate materials with positively charged surfaces, and can also enable the semiconductor substrate to obtain a lower defect value after surface planarization treatment.
[0040] The embodiment of the present application further provides a semiconductor substrate, which is obtained by subjecting the semiconductor substrate to surface planarization treatment using the composition described in the first aspect of the embodiment of the present application.
[0041] In an embodiment of the present application, the semiconductor substrate includes silicon nitride and / or silicon oxide.
[0042] An embodiment of the present application further provides a semiconductor device, comprising the semiconductor substrate described above in the embodiment of the present application, and a functional layer disposed on the semiconductor substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] FIG1 is a schematic diagram of the process operation of chemical-mechanical polishing in the application scenario of this application;
[0044] FIG2 is a schematic structural diagram of a modified particle 10 according to an embodiment of the present application;
[0045] FIG3 is a schematic structural diagram of a semiconductor device 100 according to an embodiment of the present application. DETAILED DESCRIPTION
[0046] The embodiments of the present application will be described below with reference to the accompanying drawings.
[0047] The application scenario involved in this application is chemical-mechanical polishing. Chemical-mechanical polishing refers to the process in which, under the conditions of a certain pressure and the presence of abrasive liquid, abrasive liquid containing abrasives produces a chemical corrosion effect on the grinding layer, and at the same time, the abrasives grind the grinding layer through mechanical action, and the grinding layer gradually becomes flat. As shown in Figure 1, during the chemical-mechanical polishing process, the semiconductor substrate 103 is fixed at the bottom of the grinding head 104, and the rotating grinding head 104 is pressed on the rotating grinding pad 102 located on the grinding table 101 with a certain pressure, while the grinding liquid 105 flows between the surface of the semiconductor substrate 103 and the grinding pad 102, and is evenly distributed into a layer of liquid film under the transmission and centrifugal action of the grinding pad 102. Through the dual chemical and mechanical effects of the liquid, the surface of the semiconductor substrate is smoothed and made highly flat.
[0048] In the manufacturing process of electronic products, it is usually involved in a surface treatment process for grinding materials such as metals, silicon, silicon oxide, polysilicon, and silicon nitride. This process needs to control the removal rate of each material according to the structure of the product. Among them, silicon nitride (SiN) has a high hardness. When it is ground using traditional silica sol, the mechanical action between the silica sol and the grinding layer is weak, which makes the removal rate of SiN slow. When using currently commercial sulfonic acid-modified silica, although the removal rate of SiN is improved compared to traditional silica sol, the defect value of the substrate surface after grinding is higher. In order to better meet the process requirements, the embodiment of the present application provides a composition, which can be used as a grinding liquid for grinding various semiconductor substrates, especially for grinding silicon nitride, to improve the removal rate of silicon nitride and obtain a lower defect value.
[0049] Specifically, an embodiment of the present application provides a composition comprising modified particles, a pH regulator, and a solvent, wherein, as shown in FIG2 , the modified particles 10 comprise oxide particles 11 and a modifying group 12 represented by formula (1) bound to the oxide particles 11;
[0050] In formula (1), X is selected from phosphorus, arsenic, antimony, and bismuth; R1 is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkoxy, substituted or unsubstituted aryl, and substituted or unsubstituted aryloxy; R2 is selected from H, NH4, Li, Na, K, substituted or unsubstituted alkyl, and substituted or unsubstituted aryl; R3 is selected from substituted or unsubstituted alkylene, substituted or unsubstituted alkyleneoxy, substituted or unsubstituted arylene, and substituted or unsubstituted aryleneoxy;
[0051] The oxide particles 11 include any one of silica particles, alumina particles, zinc oxide particles, titania particles, zirconium dioxide particles, and ceria particles.
[0052] The composition of the embodiment of the present application can be used to perform surface smoothing treatment on semiconductor substrates in the process of preparing electronic products, that is, the composition of the embodiment of the present application is a liquid smoothing composition, which uses modified oxide particles as abrasives, wherein the modified oxide particles are modified by the negatively charged modified groups of the structure shown in formula (1) to obtain oxide particles. The modified oxide particles can generate a strong electrostatic attraction between their negative charge and the surface of the semiconductor substrate to be processed, thereby facilitating the mechanical grinding effect; at the same time, the negatively charged modified groups of the structure shown in formula (1) can act as nucleophiles to attack the positively charged semiconductor substrate material, thereby facilitating the hydrolysis of the semiconductor substrate material and the breaking of the chemical bonds; the above two aspects can greatly improve the removal rate of the semiconductor substrate material. The composition can be used to perform surface smoothing treatment on various semiconductor substrates in the process of preparing electronic products, in particular, it can be used for grinding semiconductor substrates with positive charges on the surface, improving the removal rate of semiconductor substrate materials with positive charges on the surface, for example, it can be used for grinding silicon nitride, improving the removal rate of silicon nitride. In addition, since the negatively charged modified group of the structure shown in formula (1) of the present application has a low degree of ionization, it can reduce the residual particles on the surface of the semiconductor substrate after grinding, making it easier to clean, obtain a lower defect value, and improve the flattening effect.
[0053] In the embodiment of the present application, the content of X atoms in the modified particles measured by X-ray photoelectron spectroscopy is greater than or equal to 0.01 atomic % and less than or equal to 30 atomic %. That is, the atomic percentage of X atoms in the modified particles characterized by the X-ray photoelectron spectrometer is 0.01%-30%. The X atoms are derived from the modifying groups. The appropriate amount of X atoms indicates that an appropriate amount of modifying groups is bound to the surface of the oxide particles. The embodiment of the present application controls the atomic percentage of X atoms on the surface of the modified particles within a suitable range to obtain a better modification effect. It is also possible to regulate the hydrophilicity / hydrophobicity of the modified particles, thereby regulating the effective contact area of the composition with the semiconductor substrate material and regulating the removal rate of the composition with respect to the semiconductor substrate material. For example, the content of X atoms in the modified particles measured by X-ray photoelectron spectroscopy is 0.05 atomic %, 0.1 atomic %, 0.5 atomic %, 1 atomic %, 2 atomic %, 5 atomic %, 10 atomic %, 15 atomic %, 20 atomic %, 25 atomic %, 30 atomic %.
[0054] In the embodiment of the present application, the carbon atom content of the modified particles measured by X-ray photoelectron spectroscopy is greater than or equal to 2 atomic % and less than or equal to 45 atomic %. That is, the atomic percentage of carbon atoms of the modified particles characterized by the X-ray photoelectron spectrometer is 2%-45%. Carbon atoms come from the modifying group, and the appropriate carbon atom content can reflect the modification amount of the modifying group. In the embodiment of the present application, by controlling the atomic percentage of carbon atoms on the surface of the modified particles within a suitable range, a better modification effect can be obtained, and the hydrophilicity / hydrophobicity of the modified particles can also be regulated, thereby regulating the effective contact area of the composition to the semiconductor substrate material and improving the removal rate of the composition to the semiconductor substrate material. For example, the carbon atom content of the modified particles measured by X-ray photoelectron spectroscopy is 2 atomic %, 5 atomic %, 10 atomic %, 15 atomic %, 20 atomic %, 25 atomic %, 30 atomic %, 35 atomic %, 40 atomic %, 45 atomic %.
[0055] In some embodiments of the present application, the oxide particles are silica particles, and the ratio of the number of X atoms on the surface of the modified particles to the number of silanol groups (Si-OH) is greater than or equal to 0.4% and less than or equal to 48%. The ratio of the number of X atoms on the surface of the modified particles to the number of silanol groups can reflect the relationship between the number of modified groups on the surface of the silica particles after modification and the number of remaining silanol groups. In the embodiments of the present application, by controlling the ratio of the number of X atoms on the surface of the modified particles to the number of silanol groups within a suitable range, a better modification effect can be obtained, thereby improving the removal rate and / or selectivity of the composition for semiconductor substrate materials with positive surface charge. For example, the ratio of the number of X atoms on the surface of the modified particles to the number of silanol groups can be 0.5%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 46%, 47%, or 48%.
[0056] The ratio of the number of X atoms to the number of silanol groups on the surface of the modified particles can be obtained by the following characterization and calculation:
[0057] The X element content of the modified particles is determined using inductively coupled plasma emission spectroscopy (ICP). The number of X atoms per unit weight of the modified particles is then converted to the number of silanol groups. The number of silanol groups per unit weight of the modified particles can then be determined using commonly available titration methods (such as acid-base titration and potentiometric titration). The ratio of the number of X atoms per unit weight of the modified particles to the number of silanol groups per unit weight of the modified particles is obtained by dividing the number of X atoms per unit weight of the modified particles by the number of silanol groups per unit weight of the modified particles.
[0058] In the embodiment of the present application, the modified group 12 is chemically bonded to the surface of the oxide particle 11, which allows the modified group with specific properties to be stably present on the surface of the oxide particle, thereby allowing the modified particle to have a uniform and stable flattening effect when treating the surface of the semiconductor substrate, and to obtain a better flattening effect. The chemical bonding can be a covalent bonding. For example, the modified group can form a covalent bond with the silanol group on the surface of the silica particle through the R3 group.
[0059] In embodiments of the present application, the average particle size of the modified particles, measured using a dynamic light scattering (DLS) instrument, is 5 nm to 500 nm (i.e., greater than or equal to 5 nm and less than or equal to 500 nm). The average particle size measured by the dynamic light scattering method can be understood as the average particle size of secondary particles formed by the aggregation or association of primary particles. The average particle size of the modified particles is less than or equal to 500 nm. In embodiments of the present application, the modified particles are modified silica particles, specifically modified colloidal silica. The modified particles have a smaller particle size, which helps reduce the occurrence of scratches on the surface of the semiconductor substrate during the grinding process and improve the grinding quality. In some embodiments of the present application, the average particle size of the modified particles is 10 nm to 300 nm. In some embodiments, the average particle size of the modified particles is 20 nm to 200 nm. In some embodiments, the average particle size of the modified particles is 25 nm to 100 nm. The modified particles have an appropriate particle size, which can better balance the smoothing rate and surface scratch issues. Illustratively, the average particle size of the modified particles can be 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 120 nm, 150 nm, 200 nm, 250 nm, 300 nm, 400 nm, or 500 nm.
[0060] In the embodiment of the present application, in the composition, the weight proportion of the modified particles is 0.1%-50%. The modified particles, as abrasives, have a direct impact on the smoothing effect. The appropriate amount of modified particles in the composition is conducive to producing sufficient chemical corrosion and mechanical friction to jointly achieve efficient removal of semiconductor substrate materials, while enabling the composition to maintain suitable fluidity and maintaining high uniformity of the modified particles in the composition. Exemplarily, the weight proportion of the modified particles in the composition is 0.1%, 0.5%, 1%, 3%, 5%, 8%, 10%, 20%, 25%, 30%, 35%, 40%, 45%, and 50%. The composition is centrifuged to remove the supernatant, and the solid content is obtained after the remaining precipitate is dried to obtain the solid content, and the weight proportion of the modified particles can be obtained.
[0061] In an embodiment of the present application, the pH of the composition is less than 12. The composition of the present application can be adjusted in pH by a pH adjuster to control the pH of the composition at a suitable value, which is beneficial to improving the removal rate of the semiconductor substrate material. In the present application, the pH of the composition can be, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12.
[0062] In some embodiments of the present application, the pH of the composition is 1-6. Since the composition of the present application uses oxide particles modified with a modifying group having a structure represented by formula (1) as an abrasive, and in actual applications, many semiconductor substrate surfaces are positively charged, and considering that the use of a negatively charged planarization composition can better promote the improvement of the removal rate of positively charged semiconductor substrates, controlling the pH of the composition to 1-6 is beneficial to improving the removal rate of positively charged semiconductor substrates.
[0063] In the embodiment of the present application, the average degree of association of the modified particles is 1-10 (i.e., greater than or equal to 1 and less than or equal to 10). The average degree of association is the average particle size (nm) of the modified particles / the average primary particle size (nm) of the modified particles. The value of the average primary particle size can be calculated based on the specific surface area of the modified particles measured by the BET method, and the average particle size is measured by a dynamic light scattering method. In the embodiment of the present application, the average degree of association of the modified particles is controlled at 1-10, which can better avoid the influence of the modified particles on the smoothing effect due to dispersibility problems. Exemplarily, the average degree of association of the modified particles can be 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10.
[0064] In the embodiment of the present application, the potential of the composition is in the range of -55 to -5. Here, the potential refers to the overall potential of the composition, and the potential value of the composition can be obtained by measuring the potential value of the composition using a zeta potential meter according to an electrophoretic light scattering method. By controlling the overall potential of the composition within the above range, the influence of the potential factor on the planarization effect can be better avoided. For example, the potential of the composition can be -55, -50, -40, -35, -30, -25, -20, -15, -10, or -5.
[0065] In the embodiment of the present application, in the modifying group of the structure shown in formula (1), the substituted or unsubstituted alkyl group is a substituted or unsubstituted C1-C6 alkyl group, the substituted or unsubstituted alkoxy group is a substituted or unsubstituted C1-C6 alkoxy group; the substituted or unsubstituted alkylene group is a substituted or unsubstituted C1-C6 alkylene group, and the substituted or unsubstituted alkyleneoxy group is a substituted or unsubstituted C1-C6 alkyleneoxy group. Controlling the carbon chain length of the substituted or unsubstituted alkyl group, substituted or unsubstituted alkoxy group, substituted or unsubstituted alkylene group, and substituted or unsubstituted alkyleneoxy group in the modifying group within a suitable range is beneficial for controlling the hydrophilic and hydrophobic properties of the modifying group on the one hand, so that the modified particles can better grind the semiconductor substrate; on the other hand, it is beneficial for the modifying group to better modify the silica particles and avoid the adverse effects caused by the excessive volume steric hindrance of the modifying group. For example, substituted or unsubstituted C1-C6 alkyl can be substituted or unsubstituted methyl (-CH3), substituted or unsubstituted ethyl (-CH2CH3), substituted or unsubstituted propyl group, substituted or unsubstituted butyl, substituted or unsubstituted pentyl, substituted or unsubstituted hexyl.Substituted or unsubstituted C1-C6 alkoxy can be substituted or unsubstituted methoxy (-OCH3), substituted or unsubstituted ethoxy (-OCH2CH3), substituted or unsubstituted propoxy, substituted or unsubstituted butoxy, substituted or unsubstituted pentyloxy, substituted or unsubstituted hexyloxy.Substituted or unsubstituted C1-C6 alkylene can be substituted or unsubstituted methylene (-CH2-), substituted or unsubstituted ethylidene (-CH2CH2-), substituted or unsubstituted propylene, substituted or unsubstituted butylidene, substituted or unsubstituted pentylene, substituted or unsubstituted hexylene. The substituted or unsubstituted C1-C6 alkyleneoxy group may be a substituted or unsubstituted methyleneoxy group (-OCH2-), a substituted or unsubstituted ethyleneoxy group (-OCH2CH2-), a substituted or unsubstituted propyleneoxy group, a substituted or unsubstituted butyleneoxy group, a substituted or unsubstituted pentyleneoxy group, or a substituted or unsubstituted hexyleneoxy group. The substituted or unsubstituted alkyl group, the substituted or unsubstituted alkoxy group, the substituted or unsubstituted alkylene group, or the substituted or unsubstituted alkyleneoxy group may have a straight chain structure or a linear structure. The substituents in the substituted alkyl group, the substituted alkoxy group, the substituted alkylene group, and the substituted alkyleneoxy group may be halogen atoms, alkyl groups, aryl groups, amino groups, alkali metal elements, or the like.
[0066] In the embodiments of the present application, the pH adjuster is an acid, or a composition of an acid and a base or base salt, wherein the acid includes an organic acid and / or an inorganic acid. In some embodiments, the pH adjuster may include only one or more organic acids; in some embodiments, the pH adjuster may include only one or more inorganic acids; in some embodiments, the pH adjuster may include both one or more organic acids and one or more inorganic acids. In some embodiments, the pH adjuster may also include one or more of the above-mentioned acids in combination with one or more bases or base salts. In this combination of acid and base or base salt, the effect of simultaneously adjusting pH and conductivity can be achieved.
[0067] Among them, the organic acid can be various monocarboxylic acids, dicarboxylic acids, and tricarboxylic acids, and specific examples include but are not limited to formic acid, acetic acid, propionic acid, butyric acid, 2-methylbutyric acid, 2-ethylbutyric acid, 3,3-dimethylbutyric acid, valeric acid, 4-methylvaleric acid, n-hexanoic acid, 2-methylhexanoic acid, 2-ethylhexanoic acid, n-heptanoic acid, n-octanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, phthalic acid, malic acid, tartaric acid, citric acid, maleic acid, lactic acid, and diglycolic acid. Specific examples of the inorganic acid include but are not limited to hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid, and phosphoric acid.
[0068] It is understood that in order to increase the removal rate of the composition on the semiconductor substrate, the pH adjuster can be an acid selected to be conducive to increasing the removal rate of the semiconductor substrate, or a combination of an acid and a base or a base salt. The acid can be an acid containing a carboxylate, a phosphonate, or a phosphate.
[0069] The modified particles of the embodiments of the present application can adapt to a variety of composition systems with organic acids and inorganic acids as pH adjusters, and can effectively improve the removal rate of semiconductor substrate materials such as silicon nitride in different pH adjuster systems.
[0070] In the embodiments of the present application, the solvent may include water or an organic solvent. Water and the organic solvent serve as a dispersion medium for the modified particles and other components of the composition. The organic solvent may be any organic solvent that facilitates the dispersion of the modified particles and other components of the composition, such as ethanol, methanol, isopropanol, n-butanol, acetone, butanone, dimethyl carbonate, and the like.
[0071] In the embodiment of the present application, in order to improve certain aspects of the performance of the composition and better meet the surface smoothing treatment of semiconductor substrates under various scenarios, the composition may also include other additives, which may be, but are not limited to, one or more of catalysts, oxidants, surfactants, preservatives, passivators, and reducing agents. For example, the oxidant may be one or more of hydrogen peroxide, ammonium persulfate, periodic acid, hypochlorous acid, etc., which are used to promote oxidation of the surface of the grinding object and regulate its removal rate. The preservative may be an isothiazolinone-based preservative, parabens, and phenoxyethanol, etc. These preservatives may be used alone or in combination. Adding a preservative is used to extend the service life of the composition and to inhibit deterioration. The surfactant may be a water-soluble polymer such as cellulose, polyvinyl pyrrolidone, polyethyleneimine, polyacrylic acid, polyvinyl alcohol, etc. The surfactant serves to improve the stability of the particles, or to regulate the interaction between the particles and the grinding object so as to regulate the removal rate.
[0072] The composition of the present invention can be prepared by adding a solvent to the modified colloidal silica, then adding a pH adjuster, and mixing thoroughly under stirring to obtain the composition. The pH of the composition can be stabilized to a desired value by controlling the amount of the pH adjuster added.
[0073] The present application does not particularly limit the method for modifying the surface of oxide particles with the modifying group shown in formula (1). For example, the modified particles can be obtained by heating and stirring the raw oxide particles with one or more modifiers containing the modifying group of formula (1) or more under solvent conditions, or by cooling and stirring the reaction, so that the modifying group of formula (1) is bound to the surface of the oxide particles, thereby obtaining oxide particles modified with the structural modifying group of formula (1). The modified particles can also be obtained by first reacting the modifying group of formula (1) with a protective group to the surface of the oxide particles, and then adding a reagent for removing the protective group to remove the protective group after the reaction is completed, thereby finally obtaining oxide particles modified with the structural modifying group of formula (1). The solvent can be an aqueous medium or an organic medium. The aqueous medium can be water or a combination medium of water and one or more water-soluble solvents such as methanol, ethanol, isopropanol, acetone, butanone, etc. The organic medium can be a combination medium of one or more conventional organic solvents such as methanol, ethanol, isopropanol, acetone, butanone, toluene, xylene, ethyl acetate, dimethyl carbonate, etc.
[0074] In an embodiment of the present application, the mass content of the solvent in the composition is greater than or equal to 50% and less than 100%. A composition having a larger amount of solvent can have better fluidity and can also control the polishing effect of the composition on the semiconductor substrate. Exemplarily, the mass content of the solvent in the composition can be 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, or 95%.
[0075] In an embodiment of the present application, the viscosity of the composition at 25°C is 1 centipoise to 80 centipoise (cP). The composition having a suitable room temperature viscosity facilitates faster and more uniform spreading during the planarization process, improves polishing efficiency, and achieves better polishing results. Exemplarily, the viscosity of the composition at 25°C is 1 centipoise, 5 centipoise, 10 centipoise, 25 centipoise, 30 centipoise, 40 centipoise, 50 centipoise, 60 centipoise, 65 centipoise, or 80 centipoise (cP).
[0076] In the embodiment of the present application, the removal rate of the composition for silicon nitride is greater than The compositions of the present invention are modified particles with a specific structure as abrasives. The modified particles can remove silicon nitride at a high speed by using their strong chemical and mechanical grinding effects on silicon nitride, thereby improving the grinding efficiency. In some embodiments, the removal rate of silicon nitride by the composition is greater than In some embodiments, the composition has a silicon nitride removal rate greater than In some embodiments, the composition has a silicon nitride removal rate greater than In some embodiments, the composition has a silicon nitride removal rate greater than In some embodiments, the composition has a silicon nitride removal rate greater than In some embodiments, the composition has a silicon nitride removal rate greater than
[0077] In an embodiment of the present application, the composition has a removal selectivity of silicon nitride and silicon oxide greater than 1.5. The composition of the embodiment of the present application has a higher removal selectivity of silicon nitride and silicon oxide, and can preferably remove silicon nitride preferentially when a semiconductor substrate having both silicon nitride and silicon oxide on its surface is subjected to surface planarization treatment. In some embodiments, the composition has a removal selectivity of silicon nitride and silicon oxide greater than 2. In some embodiments, the composition has a removal selectivity of silicon nitride and silicon oxide greater than 3. In some embodiments, the composition has a removal selectivity of silicon nitride and silicon oxide greater than 5. In some embodiments, the composition has a removal selectivity of silicon nitride and silicon oxide greater than 10. In some embodiments, the composition has a removal selectivity of silicon nitride and silicon oxide greater than 15.
[0078] In the embodiment of the present application, after surface treatment of a semiconductor substrate using the composition of the embodiment of the present application, under the same conditions, a relatively lower defect value can be obtained than that of a planarization composition using commercial sulfonic acid group-modified silica as an abrasive.
[0079] The embodiments of the present application also provide the application of the above-mentioned composition in surface treatment of semiconductor substrates. The surface treatment is specifically a surface flattening treatment, and the composition is used as a grinding liquid. The application of the present application can specifically be to use the composition to perform surface flattening treatment on a semiconductor substrate with a positive surface charge, and the composition of the embodiments of the present application can increase the removal rate of the semiconductor substrate material with a positive surface charge. And because the negatively charged modified group of the structure shown in formula (1) of the present application has a relatively high pKa value compared with the common organic acid sulfonic acid group or the strong acidic group nitrate and sulfate, it can be understood that under the same low pH conditions, the group shown in structural formula (1) has a relatively low degree of dissociation, which can reduce the residual particles on the surface of the semiconductor substrate after grinding, make it easier to clean, obtain a lower defect value, and improve the flattening effect.
[0080] The semiconductor substrate in the embodiment of the present application may be a substrate to be planarized produced at various process nodes during the manufacturing process of an electronic product, for example, may be a chip with various structures.
[0081] In the embodiment of the present application, the above application is to use the composition to perform surface treatment on semiconductors containing nitrogen-silicon bonds on the surface. For example, it can be used for grinding silicon nitride to increase the removal rate of silicon nitride. On the one hand, the modified particles in the embodiment of the present application composition can utilize their negative charge to generate a strong electrostatic attraction between the surface of the semiconductor substrate to be treated with a positive charge, thereby facilitating the mechanical grinding effect; at the same time, the negatively charged modified group can be used as a nucleophilic agent to attack the positively charged semiconductor substrate material, thereby facilitating the hydrolysis of the semiconductor substrate material and the breaking of the chemical bonds; the above two effects can greatly increase the removal rate of the semiconductor substrate material.
[0082] Accordingly, an embodiment of the present application further provides a semiconductor substrate, which is obtained by surface smoothing the semiconductor substrate using the composition of the embodiment of the present application. In the embodiment of the present application, the semiconductor substrate can be a substrate to be smoothed produced at each process node in the production process of an electronic product, and a substrate obtained by surface smoothing the semiconductor substrate using the composition of the embodiment of the present application. For example, the semiconductor substrate can be a chip with various structures. The shape, size, material composition, etc. of the semiconductor substrate are designed according to actual needs. For example, the semiconductor substrate can include silicon nitride and / or silicon oxide.
[0083] Referring to FIG3 , an embodiment of the present application further provides a semiconductor device 100 . The semiconductor device 100 includes the semiconductor substrate 111 described above in the embodiment of the present application, and a functional layer 112 disposed on the semiconductor substrate 111 . The functional layer 112 may be a film layer or component designed to meet the functional requirements of the semiconductor device 100 , such as an electrode layer, a wiring layer, or a conductor layer. It should be noted that FIG3 is merely a schematic diagram of the cross-sectional structure of the semiconductor device 100 , and its specific structural design is not limited thereto.
[0084] The present invention also provides a surface treatment method, wherein the composition described above is contacted with and polishes the surface of a semiconductor substrate to be treated. This surface treatment method is a surface planarization method, wherein the composition is used as a polishing liquid to polish the surface of the semiconductor substrate to be treated. The use of the composition described in the present invention improves the efficiency and effectiveness of the planarization treatment.
[0085] Taking a semiconductor substrate to be processed as an example, a semiconductor substrate containing silicon nitride on its surface, specifically, the process of the surface treatment method of an embodiment of the present application includes, as shown in Figure 1, placing a polishing pad 102 flat on a polishing table 101, hanging a semiconductor substrate to be processed 103 upside down on a polishing head 104, and bringing the side surface containing silicon nitride to be polished into contact with the polishing head 104. Then, a certain pressure is applied to the polishing pad 102 rotating on the polishing table 101. The polishing head 104 is caused to begin rotating with the semiconductor substrate 103, and the polishing table 101 also rotates at a certain speed. Simultaneously, a polishing liquid 105, i.e., the above-mentioned composition, is added to the polishing pad 102 at a certain rate and spreads out due to centrifugal force. The silicon nitride is removed from the semiconductor substrate 103 through the dual effects of chemical and mechanical treatment. After the above process is completed, a post-cleaning process is performed to remove the abrasive and organic matter remaining on the surface of the semiconductor substrate.
[0086] The present application also provides a modified particle dispersion for surface treatment of a semiconductor substrate. The modified particle dispersion comprises modified particles and a solvent. The modified particles comprise oxide particles and a modifying group represented by formula (1) bound to the oxide particles.
[0087] In formula (1), X is selected from phosphorus, arsenic, antimony, and bismuth; R1 is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkoxy, substituted or unsubstituted aryl, and substituted or unsubstituted aryloxy; R2 is selected from H, NH4, Li, Na, K, substituted or unsubstituted alkyl, and substituted or unsubstituted aryl; R3 is selected from substituted or unsubstituted alkylene, substituted or unsubstituted alkyleneoxy, substituted or unsubstituted arylene, and substituted or unsubstituted aryleneoxy;
[0088] The oxide particles include any one of silicon dioxide particles, aluminum oxide particles, zinc oxide particles, titanium dioxide particles, zirconium dioxide particles, and cerium oxide particles.
[0089] In the embodiments of the present application, the specific features of the modified particles are as described above and will not be repeated here. In the embodiments of the present application, the solvent may be water or the aforementioned organic solvent.
[0090] The modified particle dispersion of the embodiment of the present application can be used as an abrasive to prepare a planarizing composition for surface planarizing treatment of semiconductor substrates. The modified particles in the modified particle dispersion are modified with negatively charged modified groups of a special structure and can be used for grinding semiconductor substrates with positively charged surfaces, thereby increasing the removal rate of semiconductor substrate materials with positively charged surfaces and enabling the semiconductor substrate to obtain a lower defect value after surface planarization treatment.
[0091] The embodiments of the present application are further described below with reference to a number of embodiments.
[0092] Example 1
[0093] An appropriate amount of water is added to the modified colloidal silica, followed by phosphoric acid as a pH regulator, and the mixture is thoroughly mixed under stirring to obtain a composition, wherein the weight content of the modified particles in the composition is 0.5%, wherein the amount of phosphoric acid added is controlled so that the pH of the composition is stabilized at 2. The modified colloidal silica comprises silica particles and a modifying group represented by formula (1) bound to the silica particles; wherein X is phosphorus; R1 is an ethoxy group, R2 is H, and R3 is -CH2-CH2-; and the ratio of the number of phosphorus atoms to the number of silanol groups in the modified colloidal silica is 10%. The average particle size of the modified colloidal silica is 70 nm as measured by dynamic light scattering. The carbon atom content of the modified colloidal silica is 10.5 atomic % as measured by X-ray photoelectron spectroscopy.
[0094] Example 2
[0095] The only difference from Example 1 is that in formula (1), X is phosphorus; R1 is methyl, R2 is H, and R3 is -CH2-; the carbon atom content of the modified colloidal silica measured by X-ray photoelectron spectroscopy is 6.1 atomic %.
[0096] Example 3
[0097] The only difference from Example 1 is that in formula (1), X is phosphorus; R1 is methyl, R2 is NH4, and R3 is -CH2-CH2-CH2-; the carbon atom content of the modified colloidal silica measured by X-ray photoelectron spectroscopy is 8.9 atomic %.
[0098] Example 4
[0099] The only difference from Example 1 is that in formula (1), X is phosphorus; R1 is methyl, R2 is Na, and R3 is -CH2-; the carbon atom content of the modified colloidal silica measured by X-ray photoelectron spectroscopy is 7.6 atomic %.
[0100] Example 5
[0101] The only difference from Example 1 is that in formula (1), X is phosphorus; R1 is a methyl group, R2 is K, and R3 is -CH2-CH2-CH2-; and the carbon atom content of the modified colloidal silica measured by X-ray photoelectron spectroscopy is 13.0 atomic %.
[0102] Example 6
[0103] The only difference from Example 1 is that in formula (1), X is phosphorus; R1 is a methyl group, R2 is a methyl group, and R3 is -CH2-CH2-CH2-; and the carbon atom content of the modified colloidal silica measured by X-ray photoelectron spectroscopy is 11.2 atomic %.
[0104] Comparative Example 1.1
[0105] The only difference from Example 1 is that unmodified colloidal silica is used as the abrasive.
[0106] Comparative Example 2.1
[0107] The only difference from Example 1 is that commercial sulfonic acid group-modified colloidal silica is used as the abrasive.
[0108] The compositions of Examples 1 to 6, Comparative Example 1.1 and Comparative Example 2.1 were subjected to the following grinding test:
[0109] Grinding conditions: using a desktop grinder, 1psi pressure, 63rpm platen speed, 57rpm carrier speed, the composition feed flow rate is 200mL / min, the composition is used to polish silicon nitride (SiN) substrates and silicon oxide (TEOS) substrates separately, and the composition is measured as the removal rate of different semiconductor substrates, RR (` / min) is the removal rate. The film thickness of the semiconductor substrate before and after grinding is measured using a film thickness measuring device, and the difference in film thickness before and after is divided by the grinding time to obtain the RR value. The selection ratio is the ratio of SiN RR to TEOS RR. The CANNA-600 wafer surface defect detection equipment of China Science and Technology Feice Testing Co., Ltd. is used to measure the number of defects (pieces) above 0.1μm on the grinding object, which is recorded as the defect value.
[0110] The grinding test results of the compositions of Examples 1 to 6, Comparative Example 1.1 and Comparative Example 2.1 are shown in Table 1:
[0111] Table 1
[0112] From the results in Table 1, it can be seen that compared with the composition of Comparative Example 1 using unmodified silica as an abrasive and the composition of Comparative Example 2 using commercial sulfonic acid group-modified silica as an abrasive, Examples 1 to 6 of the present application using colloidal silica modified with the modifying group shown in formula (1) as an abrasive composition, a higher SiN removal rate, a higher SiN / TEOS selectivity ratio, and lower SiN defect and TEOS defect values.
[0113] Example 7
[0114] The only difference from Example 2 is that the ratio of phosphorus atoms to silanol groups in the modified colloidal silica is 0.5%. The P atom content of the modified colloidal silica measured by X-ray photoelectron spectroscopy is 0.21 atomic %.
[0115] Example 8
[0116] The only difference from Example 2 is that the ratio of phosphorus atoms to silanol groups in the modified colloidal silica is 4.7%, and the P atom content of the modified colloidal silica measured by X-ray photoelectron spectroscopy is 2.4 atomic %.
[0117] Example 9
[0118] The only difference from Example 2 is that the ratio of phosphorus atoms to silanol groups in the modified colloidal silica is 22%. The P atom content of the modified colloidal silica measured by X-ray photoelectron spectroscopy is 8.1 atomic %.
[0119] Example 10
[0120] The only difference from Example 2 is that the ratio of phosphorus atoms to silanol groups in the modified colloidal silica is 46%, and the P atom content of the modified colloidal silica measured by X-ray photoelectron spectroscopy is 23.5 atomic %.
[0121] Example 11
[0122] The only difference from Example 2 is that the ratio of phosphorus atoms to silanol groups in the modified colloidal silica is 0.3%. The P atom content of the modified colloidal silica measured by X-ray photoelectron spectroscopy is 0.13 atomic %.
[0123] The compositions of Examples 7 to 11 were subjected to grinding tests. The test results are shown in Table 2:
[0124] Table 2
[0125] According to the results in Table 2, compared with Example 2 and Examples 7-11, it can be seen that when the content of the modifying groups on the surface of the colloidal silica in the planarization composition is maintained within a certain range, it is beneficial to promote the improvement of the SiN RR or SiN / TEOS selectivity. When the modification amount of the silica surface modifying groups in the planarization composition exceeds the appropriate ratio, it is not conducive to further increasing the SiN RR or SiN / TEOS selectivity.
[0126] Example 12
[0127] The only difference from Example 2 is that the pH of the composition was adjusted to 3.
[0128] Example 13
[0129] The only difference from Example 2 is that the pH of the composition was adjusted to 4.
[0130] Example 14
[0131] The only difference from Example 2 is that the pH of the composition was adjusted to 5.
[0132] Example 15
[0133] The only difference from Example 2 is that the pH of the composition was adjusted to 6.
[0134] Comparative Example 1.2
[0135] The only difference from Example 12 is that unmodified colloidal silica is used as the abrasive with an average particle size of 70 nm.
[0136] Comparative Example 1.3
[0137] The only difference from Example 13 is that unmodified colloidal silica is used as the abrasive with an average particle size of 70 nm.
[0138] Comparative Example 1.4
[0139] The only difference from Example 14 is that unmodified colloidal silica is used as the abrasive with an average particle size of 70 nm.
[0140] Comparative Example 1.5
[0141] The only difference from Example 15 is that unmodified colloidal silica is used as the abrasive with an average particle size of 70 nm.
[0142] Comparative Example 2.2
[0143] The only difference from Example 12 is that commercial sulfonic acid-modified colloidal silica is used as the abrasive, and the average particle size is 70 nm.
[0144] Comparative Example 2.3
[0145] The only difference from Example 13 is that commercial sulfonic acid-modified colloidal silica is used as the abrasive, and the average particle size is 70 nm.
[0146] Comparative Example 2.4
[0147] The only difference from Example 14 is that commercial sulfonic acid-modified colloidal silica is used as the abrasive, and the average particle size is 70 nm.
[0148] Comparative Example 2.5
[0149] The only difference from Example 15 is that commercial sulfonic acid-modified colloidal silica is used as the abrasive, and the average particle size is 70 nm.
[0150] The compositions of Examples 12 to 15, Comparative Examples 1.1 to 1.5, and Comparative Examples 2.1 to 2.5 were subjected to grinding tests, and the test results are shown in Table 3. The potential of the compositions was measured using a zeta potential meter according to the electrophoretic light scattering method.
[0151] Table 3
[0152] As can be seen from the results in Table 3, within the pH range of 2-6, compared to the planarization compositions of Comparative Examples 1.1 to 1.5, and Comparative Examples 2.1 to 2.5, the planarization compositions prepared using modified particles modified with specific modifying groups provided in Example 2 of the present application, and Examples 12 to 15, exhibited higher SiN removal rates and higher SiN / TEOS selectivities under different pH conditions. Among them, compared to Example 2, and Examples 12 to 15, it can be seen that when the pH is 2, the composition has a higher SiN RR, and as the pH increases, the SiN RR decreases, indicating that the pH value of the composition has a greater effect on the SiN removal rate. In addition, as can be seen from Example 2, and Examples 12 to 15, compared to the composition of Example 15 at a pH of 6, the compositions of Example 2, and Examples 12 to 14 have a higher SiN / TEOS selectivity.
[0153] Compared with the planarization compositions using unmodified colloidal silica in Comparative Examples 1.1 to 1.5, the planarization compositions of Example 2, and Examples 12 to 15 of the present application exhibit higher SiN removal rates and higher SiN / TEOS selectivities. This is because the colloidal SiO2 surface in the planarization compositions of the present application examples is modified with negatively charged specific modifying groups, which can effectively improve the SiN RR.
[0154] Compared with the planarization compositions of Comparative Examples 2.1 to 2.5 using commercial sulfonic acid group-modified colloidal silica, the planarization compositions of Example 2, and Examples 12 to 15 of the present application exhibit higher SiN removal rates and higher SiN / TEOS selectivities, which strongly demonstrates that the planarization compositions of colloidal silica modified with specific groups provided in the present application are highly competitive in promoting SiN RR and are more conducive to promoting SiN removal by polishing.
[0155] Example 16
[0156] The only difference from Example 2 is that citric acid is used as a pH adjuster to adjust the pH of the composition to 2.
[0157] Example 17
[0158] The only difference from Example 2 is that nitric acid is used as a pH adjuster to adjust the pH of the composition to 2.
[0159] Comparative Example 1.6
[0160] The only difference from Comparative Example 1.1 is that citric acid is used as a pH adjuster to adjust the pH of the composition to 2.
[0161] Comparative Example 1.7
[0162] The only difference from Comparative Example 1.1 is that nitric acid is used as a pH adjuster to adjust the pH of the composition to 2.
[0163] Comparative Example 2.6
[0164] The only difference from Comparative Example 2.1 is that citric acid is used as a pH adjuster to adjust the pH of the composition to 2.
[0165] Comparative Example 2.7
[0166] The only difference from Comparative Example 2.1 is that nitric acid is used as a pH adjuster to adjust the pH of the composition to 2.
[0167] The compositions of Examples 16 and 17 and Comparative Examples 2.6 and 2.7 were subjected to the aforementioned grinding test. The test results are listed in Table 4.
[0168] Table 4
[0169] As can be seen from the results in Table 4, when different organic acids or inorganic acids are used as pH adjusters, the planarization compositions prepared using modified particles modified with specific modifying groups provided in Examples 2, 16, and 17 of the present application exhibit higher SiN removal rates and higher SiN / Ox selectivities than the planarization compositions containing unmodified silica in Comparative Examples 1.1, 1.6, and 1.7, and the planarization compositions containing commercial sulfonic acid-modified silica in Comparative Examples 2.1, 2.6, and 2.7. This indicates that the planarization compositions prepared using modified particles modified with specific modifying groups provided in the present application are beneficial for significantly promoting the improvement of SiN RR when different types of inorganic acids and organic acids are used as pH adjusters.
[0170] Example 18
[0171] The only difference from Example 12 is that the weight content of the modified particles in the composition is 4%.
[0172] Comparative Example 2.8
[0173] The only difference from Example 2 is that the weight content of the commercial sulfonic acid-modified silica particles in the composition is 4%.
[0174] The parameter characteristics and grinding test results of the compositions of Example 2, Example 12, Example 18, Comparative Example 2.1, Comparative Example 2.2, and Comparative Example 2.8 are listed in Table 5.
[0175] Table 5
[0176] As shown in Table 5, a comparison of Examples 12 and 18 reveals that increasing the abrasive content in the composition significantly increases the SiN RR. Compared to the planarization compositions containing commercial sulfonic acid group-modified silica in Comparative Examples 2.1, 2.2, and 2.8, the planarization compositions provided herein exhibit higher SiN removal rates and SiN / Ox selectivities at both low and high abrasive concentrations. This demonstrates that the planarization compositions provided herein, containing silica modified with specific structural modifying groups, are capable of effectively removing SiN over a wide range of abrasive concentrations.
[0177] In addition, as can be seen from the results in Table 5, the planarization composition of the present application exhibits lower SiN defect (defect) and Ox defect (defect) values than the planarization composition containing commercial sulfonic acid-modified silica. Specifically, there are fewer surface particles remaining in the polishing layer after polishing, and it is easier to clean. This is mainly due to the low degree of ionization of the modified groups on the modified silica in the examples of the present application, which makes the planarization composition of the examples of the present application exhibit lower surface residue and easier cleaning properties.
[0178] The planarization compositions of Examples 1-18 of the present application have low viscosity and high water content. The viscosity of the compositions at 25° C. is in the range of 1 centipoise to 10 centipoise, and the water content is in the range of 80% to 99.3%. The viscosity of the compositions can be measured using a viscometer.
[0179] It should be understood that the first, second and various numerical numbers involved in this document are only distinguished for the convenience of description and are not intended to limit the scope of this application.
[0180] In this application, "and / or" describes the relationship between related objects, indicating that three possible relationships exist. For example, "A and / or B" can mean: A exists alone, A and B exist simultaneously, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the related objects are in an "or" relationship.
[0181] In this application, "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.
[0182] In this application, “-” represents a range value, including the endpoint values at both ends. For example, the average particle size of the modified particles is 5nm-500nm, which means that the average particle size of the modified particles is between 5nm and 500nm, and includes the endpoint values 5nm and 500nm.
[0183] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution. Some or all of the steps can be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
Claims
1. A composition, characterized in that The composition comprises modified particles, a pH adjuster and a solvent, wherein the modified particles comprise oxide particles and a modifying group represented by formula (1) bonded to the oxide particles; In formula (1), X is selected from phosphorus, arsenic, antimony, and bismuth; R1 is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkoxy, substituted or unsubstituted aryl, and substituted or unsubstituted aryloxy; R2 is selected from H, NH4, Li, Na, K, substituted or unsubstituted alkyl, and substituted or unsubstituted aryl; R3 is selected from substituted or unsubstituted alkylene, substituted or unsubstituted alkyleneoxy, substituted or unsubstituted arylene, and substituted or unsubstituted aryleneoxy; The oxide particles include any one of silicon dioxide particles, aluminum oxide particles, zinc oxide particles, titanium dioxide particles, zirconium dioxide particles, and cerium oxide particles.
2. The composition according to claim 1, characterized in that The content of X atoms in the modified particles measured by X-ray photoelectron spectroscopy is greater than or equal to 0.01 atomic % and less than or equal to 30 atomic %.
3. The composition according to claim 1 or 2, characterized in that The carbon atom content of the modified particles measured by X-ray photoelectron spectroscopy is greater than or equal to 2 atomic % and less than or equal to 45 atomic %.
4. The composition according to any one of claims 1 to 3, characterized in that The oxide particles are silicon dioxide particles, and the ratio of the number of X atoms to the number of silanol groups in the modified particles is greater than or equal to 0.4% and less than or equal to 48%.
5. The composition according to any one of claims 1 to 4, characterized in that The modifying group is bonded to the oxide particle by chemical bonding.
6. The composition according to any one of claims 1 to 5, characterized in that The average particle size of the modified particles measured by dynamic light scattering method is 5nm-500nm.
7. The composition according to any one of claims 1 to 6, characterized in that In the composition, the weight proportion of the modified particles is 0.1%-50%.
8. The composition according to any one of claims 1 to 7, characterized in that The pH of the composition is less than 12.
9. The composition according to claim 8, characterized in that The pH of the composition is 1-6.
10. The composition according to any one of claims 1 to 9, characterized in that The average association degree of the modified particles is 1-10.
11. The composition according to any one of claims 1 to 10, characterized in that The potential of the composition is in the range of -55 to -5.
12. The composition according to any one of claims 1 to 11, characterized in that The substituted or unsubstituted alkyl group is a substituted or unsubstituted C1-C6 alkyl group, the substituted or unsubstituted alkoxy group is a substituted or unsubstituted C1-C6 alkoxy group; the substituted or unsubstituted alkylene group is a substituted or unsubstituted C1-C6 alkylene group, and the substituted or unsubstituted alkyleneoxy group is a substituted or unsubstituted C1-C6 alkyleneoxy group.
13. The composition according to any one of claims 1 to 12, characterized in that The pH adjuster includes an acid, or a combination of an acid and a base or a base salt, and the acid includes an organic acid and / or an inorganic acid.
14. The composition according to any one of claims 1 to 13, characterized in that The solvent includes water or an organic solvent.
15. The composition according to any one of claims 1 to 14, characterized in that The composition further comprises one or more of a catalyst, an oxidant, a surfactant, a preservative, a passivator, and a reducing agent.
16. The composition according to any one of claims 1 to 15, characterized in that The mass content of the solvent in the composition is greater than or equal to 50% and less than 100%.
17. The composition according to any one of claims 1 to 16, characterized in that The viscosity of the composition at 25° C. is 1 centipoise to 80 centipoise.
18. The composition according to any one of claims 1 to 17, characterized in that The removal rate of silicon nitride by the composition is greater than 19. The composition according to any one of claims 1 to 18, characterized in that The removal selectivity of the composition to silicon nitride and silicon oxide is greater than 1.
5.
20. Use of the composition according to any one of claims 1 to 19 in surface treatment of a semiconductor substrate.
21. The use according to claim 20, characterized in that The composition is used to treat the surface of a semiconductor substrate with positive surface charge.
22. The use according to claim 21, characterized in that The composition is used to perform surface treatment on a semiconductor substrate containing nitrogen-silicon bonds on the surface.
23. A surface treatment method, characterized in that: The composition according to any one of claims 1 to 19 is brought into contact with and polished on the surface of a semiconductor substrate to be processed.
24. A modified particle dispersion for surface treatment of a semiconductor substrate, characterized in that: The modified particle dispersion comprises modified particles and a solvent, wherein the modified particles comprise oxide particles and a modified group represented by formula (1) bonded to the oxide particles; In formula (1), X is selected from phosphorus, arsenic, antimony, and bismuth; R1 is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkoxy, substituted or unsubstituted aryl, and substituted or unsubstituted aryloxy; R2 is selected from H, NH4, Li, Na, K, substituted or unsubstituted alkyl, and substituted or unsubstituted aryl; R3 is selected from substituted or unsubstituted alkylene, substituted or unsubstituted alkyleneoxy, substituted or unsubstituted arylene, and substituted or unsubstituted aryleneoxy; The oxide particles include any one of silicon dioxide particles, aluminum oxide particles, zinc oxide particles, titanium dioxide particles, zirconium dioxide particles, and cerium oxide particles.
25. A semiconductor substrate, characterized in that: The semiconductor substrate is obtained by subjecting the surface of the semiconductor substrate to a planarization treatment using the composition described in any one of claims 1 to 19.
26. The semiconductor substrate according to claim 25, wherein: The semiconductor substrate includes silicon nitride and / or oxide.
27. A semiconductor device, characterized in that: It comprises the semiconductor substrate as described in any one of claims 25-26, and a functional layer arranged on the semiconductor substrate.
Citation Information
Patent Citations
Slurry Compositions for Polishing a Metal Layer and Methods for Fabricating Semiconductor Devices Using the Same
CN109021833A
CMP slurry composition for metal film, and polishing method
CN109415598A
Compositions and methods for chemical mechanical planarization of tungsten and titanium
CN1676563A
Polishing liquid composition for sapphire plate
JP2017190363A
Abrasives composition, substrate and process for producing the same, and magnetic recording medium and process for producing the same
US5868604A