Ultrahigh-heat-conducting cubic boron nitride-based heat-conducting gasket and preparation method therefor
Through the combination of specific modifiers and powders, the dispersion performance of cubic boron nitride is optimized, which solves the problems of insufficient thermal conductivity and poor dispersion performance in thermally conductive materials, and achieves high thermal conductivity and good mechanical properties.
Patent Information
- Application Number
- PCT/CN2024/096840
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-02
- Filing Date
- 2024-05-31
- Publication Date
- 2024-12-05
AI Technical Summary
The prior art is difficult to effectively improve the thermal conductivity of cubic boron nitride while ensuring compression and resilience. The high chemical inertia leads to poor dispersion performance in the resin, resulting in failure to meet the high thermal conductivity.
By using specific proportions of octyltrimethoxysilane and hexamethyldisilazane as modifiers, combining spherical alumina, single crystal alumina, zinc oxide and other metal oxide powders and aluminum nitride powders, the cubic is optimized. The dispersion properties of boron nitride and the combination of vinyl silicone oil and crosslinking agent improve thermal conductivity while controlling hardness and flexibility.
The thermal conductivity is achieved above 18W/(m·K), the hardness is controlled at about shore 00 20, the compression rate is maintained at 15%, and the high-temperature aging performance is improved.
Smart Images

Figure CN2024096840_05122024_PF_FP_ABST
Abstract
Description
A super-high thermal conductivity cubic boron nitride-based thermal pad and its preparation method Technical Field
[0001] The present invention relates to the technical field of thermal conductive materials, in particular to the field of IPC C08K3, and more specifically to an ultra-high thermal conductivity cubic boron nitride-based thermal conductive gasket and a preparation method thereof. Background Art
[0002] With the advancement of industrial production and science and technology, thermally conductive silicone sheets, as a high-performance thermal interface material, are used to fill gaps between heat-generating components and heat sinks or metal bases. They create a good thermal path while also providing insulation, shock absorption, and sealing. They are a popular material in electronic products and equipment. However, with the continuous upgrading of electronic products, power consumption and heat generation are increasing, leading to increasingly demanding thermal conductivity requirements for thermally conductive silicone sheets. Cubic boron nitride (c-BN) is a synthetic superhard material with an atomic structure similar to that of carbon atoms in diamond, resulting in its high density. Cubic boron nitride has a crystal structure similar to that of diamond, with similar lattice constants. This gives it excellent thermal conductivity, at 79.54 W / m·K, far exceeding that of ceramic materials. However, due to its high chemical inertness and high chemical stability to acids and bases in neutral and reducing gases, c-BN is difficult to dissolve in resins, making it difficult to prepare high-performance thermal interface materials. Therefore, finding a method to better add cubic boron nitride crystals into thermal pads to improve their thermal conductivity while ensuring compressibility and resilience is an urgent problem to be solved.
[0003] CN 112457673A discloses a highly thermally conductive, insulating silicone gasket. The thermally conductive filler comprises at least one of nano-aluminum nitride, cubic boron nitride, and nano-silicon carbide, along with spherical alumina modified with dodecamethyltrimethoxysilane. This invention, through filler modification and compounding, achieves excellent properties such as high thermal conductivity, high insulation, and chemical stability. However, the gasket's thermal conductivity does not exceed 15 W / (m·K), and its flexibility is poor (Shore 00 is above 40).
[0004] CN 113322037B discloses a thermally shock-resistant, highly thermally conductive epoxy potting compound and its preparation method. The addition of soft boron nitride as a second phase absorbs energy when the material is subjected to external forces, inducing the formation of microcracks and hindering crack propagation, leading to crack arrest and improved material toughness. The layered micronized boron nitride layers overlap to form heat-conducting channels for phonon transmission, effectively improving the thermal conductivity of the epoxy potting compound while meeting the potting compound's heat dissipation requirements. CN 109880297 A discloses a thermally conductive, insulating epoxy resin composite material and its preparation method. A hexagonal boron nitride / gold nanoparticle composite and modified cubic boron nitride micropowder are used as thermally conductive fillers. However, due to compatibility issues with epoxy resin, the boron nitride addition percentage is too low, and the thermal conductivity does not exceed 2 W / (m·K).
[0005] Summary of the Invention
[0006] The first aspect of the present invention provides an ultra-high thermal conductivity cubic boron nitride-based thermal conductive gasket. The raw materials for preparing the gasket include, by weight: 35-150 parts of cubic boron nitride powder, 30-105 parts of metal oxide powder, 15-40 parts of metal nitride powder, 0.2-0.6 parts of modifier, 2-8 parts of vinyl silicone oil, 0.1-0.8 parts of cross-linking agent, 0.1-0.9 parts of inhibitor, and 0.2-1 parts of catalyst.
[0007] The particle size of the cubic boron nitride powder is 5-180 μm.
[0008] Preferably, the cubic boron nitride powder includes two types with particle sizes of 5-50 μm and 80-180 μm.
[0009] Preferably, the weight ratio of the cubic boron nitride with a particle size of 5-50 μm to that of 80-180 μm is 1:(2-5).
[0010] Further preferably, the weight ratio of the cubic boron nitride with a particle size of 5-50 μm to that of 80-180 μm is 1:2.5.
[0011] Further preferably, the cubic boron nitride has a particle size of 5-10 μm and is purchased from Yingkou Liaobin Fine Chemical Co., Ltd., model: BN-C.
[0012] The cubic boron nitride has a particle size of 37-45 μm, model: CBN-810, and is purchased from Funaike Superhard Materials Co., Ltd.
[0013] The cubic boron nitride has a particle size of 125-150 μm, model: CBN-850, and is purchased from Funaike Superhard Materials Co., Ltd.
[0014] The applicant's research has found that the modifier includes octyltrimethoxysilane and hexamethyldisilazane, and the weight ratio of octyltrimethoxysilane to hexamethyldisilazane is 1:(0.2-2). While achieving good flexibility, it also improves the thermal conductivity of the gasket. Cubic boron nitride is chemically inert and has high chemical stability in the system of the present invention, but its dispersion performance with resins and various fillers is poor. In the process of exploring the influence of different substances in the components on the dispersion performance of cubic boron nitride, the applicant accidentally discovered that octyltrimethoxysilane and hexamethyldisilazane compounded in a specific ratio effectively improved the thermal conductivity of the gasket. This may be because the presence of several active surfaces in cubic boron nitride makes hexamethyldisilazane easier to disperse with cubic boron nitride, while octyltrimethoxysilane has better wettability with metal oxide powders and metal nitride powders in the system. The two specific modifiers act as a bridge between different molecular structures, increasing the addition amount of cubic boron nitride while improving the wettability with silicone resin.
[0015] The modifier includes octyltrimethoxysilane and hexamethyldisilazane, and the weight ratio of the octyltrimethoxysilane to the hexamethyldisilazane is 1:(0.2-2).
[0016] Preferably, the modifier includes octyltrimethoxysilane and hexamethyldisilazane, and the weight ratio of octyltrimethoxysilane to hexamethyldisilazane is 1:0.8.
[0017] The metal oxide powder includes at least two of spherical aluminum oxide, single crystal aluminum oxide, magnesium oxide, and zinc oxide.
[0018] Preferably, the metal oxide powder includes spherical alumina, single crystal alumina and zinc oxide, and the weight ratio of the spherical alumina, single crystal alumina and zinc oxide is 1:(0.5-2):(0.2-0.5).
[0019] Further preferably, the metal oxide powder includes spherical alumina, single crystal alumina, and zinc oxide, and the weight ratio of the spherical alumina, single crystal alumina, and zinc oxide is 1:1:0.5.
[0020] Preferably, the spherical alumina particle size is 1-70 μm.
[0021] Further preferably, the spherical alumina has a particle size of 10 μm and is purchased from Shijiazhuang Jinghuang Technology Co., Ltd.
[0022] Preferably, the particle size of the single crystal alumina is 0.3-5 μm.
[0023] Further preferably, the single crystal alumina has a particle size of 1 μm and is purchased from Dongguan Dongchao New Material Technology Co., Ltd.
[0024] Preferably, the particle size of the zinc oxide is 0.5-3 μm.
[0025] Further preferably, the zinc oxide has a particle size of 1 μm and is purchased from Shanghai Pantian Powder Materials Co., Ltd., model: PT-ZnO.
[0026] Preferably, the metal nitride powder includes aluminum nitride, and the aluminum nitride has a particle size of 2-150 μm.
[0027] Preferably, the aluminum nitride particle size is 50-120 μm.
[0028] Further preferably, the aluminum nitride has a particle size of 70 μm and is purchased from Shanghai Xiangtian Nanomaterials Co., Ltd., model: XT-ALN-10.
[0029] The weight ratio of the cubic boron nitride powder, the metal oxide powder and the metal nitride powder is (1.5-6):(1.7-3.5):1.
[0030] Preferably, the weight ratio of the cubic boron nitride powder, the metal oxide powder, and the metal nitride powder is (50-100): (3-6).
[0031] Preferably, the weight ratio of the cubic boron nitride powder to the vinyl silicone oil is 20:1.
[0032] The vinyl content in the vinyl silicone oil is 0.08-2.6%.
[0033] Preferably, the vinyl silicone oil includes single-ended vinyl silicone oil, the vinyl content in the vinyl silicone oil is 0.18%, and it is purchased from Guangdong Chensi New Material Technology Co., Ltd., model: CX-352M.
[0034] The cross-linking agent includes at least one of terminal hydrogen-containing silicone oil, side hydrogen-containing silicone oil, and terminal-side hydrogen-containing silicone oil.
[0035] Preferably, the cross-linking agent includes end-side hydrogen-containing silicone oil, purchased from Guangdong Chensi New Material Technology Co., Ltd., model: CX350T.
[0036] The catalyst includes a platinum catalyst.
[0037] The platinum catalyst was purchased from Beiteli Polymer Materials Co., Ltd., model: CSAT-F1.
[0038] The inhibitor includes at least one of methylbutynol, acetylene cyclohexanol, and polyvinyl compounds.
[0039] Preferably, the inhibitor comprises acetylene cyclohexanol (CAS: 78-27-3).
[0040] A second aspect of the present invention provides a method for preparing an ultra-high thermal conductivity cubic boron nitride-based thermally conductive gasket, comprising the following steps:
[0041] S1, mixing cubic boron nitride powder and a portion of a modifier to obtain a mixture 1;
[0042] S2, uniformly mixing the metal oxide powder, the metal nitride powder, and the remaining modifier to obtain a mixture 2;
[0043] S3, adding vinyl silicone oil and mixture 2 into a container and stirring uniformly to obtain mixture 3;
[0044] S4, adding mixture 1 to mixture 3, stirring evenly, then adding a crosslinking agent, an inhibitor, and a catalyst, stirring evenly, to obtain mixture 4;
[0045] S5, kneading the mixture 4 into a ball, and placing it in a vacuum box for vacuum treatment 2-4 times, unloading, rolling, and baking to obtain the product.
[0046] Preferably, the method for preparing the ultra-high thermal conductivity cubic boron nitride-based thermally conductive gasket comprises the following steps:
[0047] S1, mixing cubic boron nitride powder and a portion of the modifier (stirring at 10-200 rpm for 0.5-90 min) to obtain a mixture 1;
[0048] S2, mixing the metal oxide powder, the metal nitride powder, and the remaining modifier (stirring at 150-500 rpm for 0.5-30 min), and baking in an oven at 50-170° C. for 0.5-24 h to obtain a mixture 2;
[0049] S3, adding vinyl silicone oil and mixture 2 into a container, stirring evenly (stirring at 20-50 rpm for 5-30 minutes) to obtain mixture 3;
[0050] S4, adding mixture 1 to mixture 3, raising the temperature to 120-140° C., stirring uniformly (stirring at 30-50 rpm for 1-10 minutes), cooling to room temperature, then adding a crosslinker, inhibitor, and catalyst, stirring uniformly (stirring at 5-20 rpm for 10-120 minutes), and turning on vacuum during stirring to obtain mixture 4;
[0051] S5, knead the mixture 4 into a ball, and put it into a vacuum box for vacuum treatment three times, discharge it, roll it (the thickness can be controlled at 0.3-5mm), and bake it (120℃, baking for 15-90min). Beneficial effects:
[0052] 1. The cubic boron nitride powder has two particle sizes of 5-50 μm and 80-180 μm. The weight ratio of the cubic boron nitride with particle sizes of 5-50 μm and 80-180 μm is 1:2.5, which can effectively improve the wettability of cubic boron nitride with vinyl silicone oil, thereby improving the thermal conductivity of the gasket.
[0053] 2. The metal oxide powder includes spherical alumina, single crystal alumina and zinc oxide. The weight ratio of the spherical alumina, single crystal alumina and zinc oxide is 1:(0.5-2):(0.2-0.5), which can balance the thermal conductivity and flexibility of the gasket.
[0054] 3. The weight ratio of the cubic boron nitride powder to the vinyl silicone oil is (50-100): (3-6), which can improve the high-temperature aging performance of the gasket.
[0055] 4. The modifier includes octyltrimethoxysilane and hexamethyldisilazane, and the weight ratio of octyltrimethoxysilane to hexamethyldisilazane is 1: (0.2-2), which can improve the dispersion performance of various fillers in the system, while controlling the hardness of shore 00 to about 20 and the thermal conductivity to above 18W (m·K), and
[0056] Its compression rate can also be maintained at 15%. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] Figure 1 is a graph showing the change in thermal conductivity of the gasket of Example 1 after aging. The curves from top to bottom are high temperature test (125°C), high temperature and high humidity test (85°C & 85% rh), and temperature cycle aging test (-40°C ~ 85°C).
[0058] Figure 2 is a graph showing the hardness change of the gasket in Example 1 after aging. The curves from top to bottom are high temperature test (125°C), high temperature and high humidity test (85°C & 85% rh), and temperature cycle aging test (-40°C ~ 85°C). DETAILED DESCRIPTION
[0059] Example 1
[0060] Disclosed is an ultra-high thermal conductivity cubic boron nitride-based thermally conductive gasket. The raw materials for preparing the gasket are, by weight, 80 parts of cubic boron nitride powder, 65 parts of metal oxide powder, 25 parts of metal nitride powder, 0.43 parts of a modifier, 4 parts of vinyl silicone oil, 0.2 parts of a cross-linking agent, 0.1 parts of an inhibitor, and 0.5 parts of a catalyst.
[0061] The cubic boron nitride powder has two particle sizes: 5-50 μm and 80-180 μm.
[0062] The weight ratio of the cubic boron nitride with a particle size of 5-50 μm to that of 80-180 μm is 1:2.5.
[0063] The cubic boron nitride with a particle size of 5-50 μm is of two types: particle size 5-10 μm and particle size 37-45 μm, with a weight ratio of 1:1. The cubic boron nitride with a particle size of 5-10 μm is purchased from Yingkou Liaobin Fine Chemical Co., Ltd., model: BN-C; the cubic boron nitride with a particle size of 37-45 μm, model: CBN-810, is purchased from Funike Superhard Materials Co., Ltd.
[0064] The metal oxide powders are spherical alumina, single crystal alumina and zinc oxide, and the weight ratio of the spherical alumina, single crystal alumina and zinc oxide is 1:1:0.5.
[0065] The spherical alumina has a particle size of 10 μm and is purchased from Shijiazhuang Jinghuang Technology Co., Ltd.
[0066] The single crystal alumina has a particle size of 1 μm and is purchased from Dongguan Dongchao New Material Technology Co., Ltd.
[0067] The zinc oxide has a particle size of 1 μm and is purchased from Shanghai Pantian Powder Material Co., Ltd., model: PT-ZnO.
[0068] The metal nitride powder is aluminum nitride with a particle size of 70 μm, purchased from Shanghai Xiangtian Nanomaterial Co., Ltd., model: XT-ALN-10.
[0069] The vinyl silicone oil is a single-ended vinyl silicone oil with a vinyl content of 0.18%. It is purchased from Guangdong Chensi New Material Technology Co., Ltd., model: CX-352M.
[0070] The cross-linking agent is end-side hydrogen-containing silicone oil, purchased from Guangdong Chensi New Material Technology Co., Ltd., model: CX350T.
[0071] The modifiers are octyltrimethoxysilane and hexamethyldisilazane, and the weight ratio of octyltrimethoxysilane to hexamethyldisilazane is 1:0.8.
[0072] The catalyst is a platinum catalyst purchased from Beiteli Polymer Materials Co., Ltd., model: CSAT-F1.
[0073] The inhibitor is acetylene cyclohexanol (CAS: 78-27-3).
[0074] A method for preparing an ultra-high thermal conductivity cubic boron nitride-based thermally conductive gasket comprises the following steps:
[0075] S1, mixing cubic boron nitride powder and 0.2 parts of modifier (stirring at 50 rpm for 10 min) to obtain mixture 1;
[0076] S2, mixing metal oxide powder, metal nitride powder, and 0.23 parts of modifier (stirring at 200 rpm for 10 min), and baking in an oven at 150° C. for 2 h to obtain mixture 2;
[0077] S3, vinyl silicone oil and mixture 2 are added to a container and stirred evenly (20 rpm for 5 min) to obtain mixture 3;
[0078] S4, adding mixture 1 to mixture 3, heating to 130°C, stirring evenly (stirring at 20 rpm for 5 minutes), cooling to 25°C, adding a crosslinker, inhibitor, and catalyst, stirring evenly (stirring at 10 rpm for 20 minutes), and turning on vacuum (-0.1 MPa) during stirring to obtain mixture 4;
[0079] S5, knead the mixture 4 into a ball, and put it into a vacuum box for vacuuming (-0.1 MPa, 60 min) for 3 times, discharge the material, roll it (thickness 1 mm), and bake it (120° C., baking for 90 min).
[0080] Example 2
[0081] The specific implementation is the same as Example 1; the difference is that in Example 2: 65 parts of cubic boron nitride powder, 52 parts of metal oxide powder, 21 parts of metal nitride powder, and 0.33 parts of modifier.
[0082] Comparative Example 1
[0083] The specific implementation is the same as that of Example 1; the difference is that in Comparative Example 1: the preparation raw materials do not include a modifier.
[0084] A method for preparing an ultra-high thermal conductivity cubic boron nitride-based thermally conductive gasket comprises the following steps:
[0085] S1, heating vinyl silicone oil, metal oxide powder, metal nitride powder, and cubic boron nitride powder to 130°C, stirring uniformly (stirring at 20 rpm for 60 min), cooling to 25°C, then adding a crosslinker, inhibitor, and catalyst, stirring uniformly (stirring at 10 rpm for 30 min), and applying vacuum (-0.1 MPa) during stirring to obtain mixture 1;
[0086] S2, knead the mixture 1 into a ball, and put it into a vacuum box for vacuuming (-0.1MPa, 60min) repeatedly for 3 times, discharge the material, roll it (the thickness can be controlled at 1mm), and bake it (120℃, baking for 90min).
[0087] Comparative Example 2
[0088] The specific implementation is the same as in Example 1; except that, in Comparative Example 2:
[0089] A method for preparing an ultra-high thermal conductivity cubic boron nitride-based thermally conductive gasket comprises the following steps:
[0090] S1, vinyl silicone oil, metal oxide powder, metal nitride powder, cubic boron nitride powder, and modifier were stirred uniformly (stirring at 20 rpm for 60 min), and then a crosslinker, inhibitor, and catalyst were added and stirred uniformly (stirring at 10 rpm for 30 min). During the stirring, vacuum was applied (-0.1 MPa) to obtain a mixture 1;
[0091] S2, knead the mixture 1 into a ball, and put it into a vacuum box for vacuuming (-0.1MPa, 60min) repeatedly for 3 times, discharge the material, roll it (the thickness can be controlled at 1mm), and bake it (120℃, baking for 90min).
[0092] Comparative Example 3
[0093] The specific implementation is the same as Example 1; the difference is that in Comparative Example 3: the modifier is vinyltrimethoxysilane and octyltrimethoxysilane, and the weight ratio of vinyltrimethoxysilane to octyltrimethoxysilane is 0.8:1.
[0094] Comparative Example 4
[0095] The specific implementation is the same as Example 1; the difference is that in Comparative Example 4: the weight ratio of octyltrimethoxysilane to hexamethyldisilazane is 2:1.
[0096] Performance testing methods
[0097] The performance tests were carried out in the embodiments and comparative examples.
[0098] Thermal conductivity: measured according to ASTM D 5470-17 using a Taiwan Ruiling LW-9389 interface material thermal resistance and thermal conductivity measuring device (at 25°C). The test data are listed in Table 1.
[0099] Hardness: measured using a shore 00 durometer (at 25° C.) according to ASTM D2240. The gasket obtained in Comparative Example 3 was not formed, and the test result is indicated by “-”. The test data are listed in Table 1.
[0100] Aging performance test: Example 1 was tested using GFG-400-15 according to standard GB / T2423, as shown in Figures 1 and 2. The tests included: temperature cycle aging test (-40°C to 85°C), high temperature and high humidity test (85°C & 85% rh), and high temperature test (125°C). The test time was 1000 h. The test data are listed in Table 2.
[0101] Performance test data
[0102] Table 1
[0103] Table 2
Claims
1. An ultra-high thermal conductivity cubic boron nitride-based thermally conductive pad, characterized in that: By weight, the raw materials for preparing the gasket include: 35-150 parts of cubic boron nitride powder, 30-105 parts of metal oxide powder, 15-40 parts of metal nitride powder, 0.2-0.6 parts of modifier, 2-8 parts of vinyl silicone oil, 0.1-0.8 parts of crosslinking agent, 0.1-0.9 parts of inhibitor, and 0.2-1 parts of catalyst.
2. The ultra-high thermal conductivity cubic boron nitride-based thermally conductive gasket according to claim 1, characterized in that: The particle size of the cubic boron nitride powder is 5-180 μm.
3. The ultra-high thermal conductivity cubic boron nitride-based thermally conductive gasket according to claim 2, characterized in that: The cubic boron nitride powder includes two types with particle sizes of 5-50 μm and 80-180 μm.
4. The ultra-high thermal conductivity cubic boron nitride-based thermally conductive gasket according to claim 3, characterized in that: The weight ratio of the cubic boron nitride with a particle size of 5-50 μm and 80-180 μm is 1:(2-5).
5. The ultra-high thermal conductivity cubic boron nitride-based thermally conductive gasket according to claim 1, characterized in that: The modifier includes octyltrimethoxysilane and hexamethyldisilazane, and the weight ratio of the octyltrimethoxysilane to the hexamethyldisilazane is 1:(0.2-2).
6. The ultra-high thermal conductivity cubic boron nitride-based thermally conductive gasket according to claim 1 or 5, characterized in that: The metal oxide powder includes at least two of spherical aluminum oxide, single crystal aluminum oxide, magnesium oxide, and zinc oxide.
7. The ultra-high thermal conductivity cubic boron nitride-based thermally conductive gasket according to claim 1, characterized in that: The weight ratio of the cubic boron nitride powder, the metal oxide powder and the metal nitride powder is (1.5-6):(1.7-3.5):
1.
8. The ultra-high thermal conductivity cubic boron nitride-based thermally conductive gasket according to claim 7, characterized in that: The weight ratio of the cubic boron nitride powder to the vinyl silicone oil is (50-100):(3-6).
9. The ultra-high thermal conductivity cubic boron nitride-based thermally conductive gasket according to claim 1, characterized in that: The cross-linking agent includes at least one of terminal hydrogen-containing silicone oil, side hydrogen-containing silicone oil, and terminal-side hydrogen-containing silicone oil.
10. A method for preparing the ultra-high thermal conductivity cubic boron nitride-based thermally conductive gasket according to claim 1, characterized in that: The following steps are involved: S1, mixing cubic boron nitride powder and a part of a modifier uniformly to obtain a mixture 1; S2, mixing metal oxide powder, metal nitride powder and remaining modifier to obtain mixture 2; S3, adding vinyl silicone oil and mixture 2 into a container, stirring evenly, to obtain mixture 3; S4, add mixture 1 to mixture 3, stir evenly, then add crosslinking agent, inhibitor and catalyst, and stirring to obtain a mixture 4; S5, kneading the mixture 4 into a ball shape, and putting it into a vacuum box for vacuum treatment 2-4 times, unloading, calendering, and baking to obtain.
Citation Information
Patent Citations
High-thermal-conductivity insulating silica gel gasket and preparation method thereof
CN112457673A
Ultrahigh-heat-conductivity cubic boron nitride-based heat-conducting gasket and preparation method thereof
CN117089207A
Heat conductive silicone composition
JP1999049958A
Silicone resin composition
JP2016034991A
Thermal interface material and method for making the same
US20220025241A1
Cited By