Hybrid wood veneer composite modified with bacterial cellulose and woven aramid fibres and its manufacturing process
The hybrid wood veneer composite, formed by modifying wood veneer with bacterial cellulose and aramid fibers, addresses the inefficiency of current composite armor systems by enhancing energy absorption, offering a promising alternative for bulletproof vests with improved ballistic and trauma protection.
Patent Information
- Application Number
- PCT/ID2023/000005
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2023-12-01
- Publication Date
- 2024-12-05
AI Technical Summary
Current composite armor systems, such as Multi-layered Armour Systems, are inefficient in stopping high-impact energy ammunition like 7.62 mm caliber projectiles, necessitating the development of alternative materials that can enhance ballistic and trauma energy absorption.
A hybrid composite is created by modifying wood veneer with bacterial cellulose and woven aramid fibers, using a process involving delignification, soaking in bacterial cellulose solution, pressing with epoxy adhesive, and layering with aramid fibers, to produce a material with improved energy absorption properties.
The hybrid wood veneer composite demonstrates superior ballistic and trauma energy absorption capabilities compared to non-hybrid composites, making it a potential alternative for bulletproof vests.
Smart Images

Figure ID2023000005_05122024_PF_FP_ABST
Abstract
Description
[0001] Description
[0002] HYBRID WOOD VENEER COMPOSITE MODIFIED WITH BACTERIAL CELLULOSE
[0003] AND WOVEN ARAMID FIBRES AND ITS MANUFACTURING PROCESS
[0004] Technical Field of the Invention
[0005] This invention relates to a hybrid composite and its manufacturing process, specifically, a hybrid composite made from wood veneer modified with bacterial cellulose and woven aramid fibres to produce a composite that can be used as bulletproof material .
[0006] Background of the Invention
[0007] In recent years, the growing number of armed conflicts has increased the demand for an efficient personal armour protection system. For high-impact energy ammunition, such as the 7. 62 mm calibre, a shield made of a single material is inefficient enough to stop the proj ectile or prevent lethal trauma to the wearer .
[0008] Therefore, lightweight, and efficient shields have been developed as Multi-layered Armour Systems (MAS) or Composite Armour . This system can be used for various ballistic protection applications, including bulletproof vests . Composite armour provides security by layering lightweight and efficient materials in multiple layers .
[0009] It is typically three layers : a ceramic layer on the front, a fibre composite on the second, and a metal material for the back layer .
[0010] There is extensive research on the second layer of MAS . Patent
[0011] US6253655 "Lightweight AArrmmoouurr wwiitthh aa DDuurraabbllee Spall Cover", describes the use of flexible foam sheets on the second layer of composite armour . In the US6253655 patent method the foam sheets are formed into a hexagonal shape . Meanwhile, in this proposed patent, the material used is a combination of wood veneer, aramid fibres, and wood veneer that is formed into a box .
[0012] Patent PID201904109, "The Composition of Bulletproof Sheets
[0013] Made from Non-Woven Oil Palm Empty Fruit Bunch Fibres, ” introduced a manufacturing method for a composite armour layer using a mixture of epoxy and Oil Palm Empty Fruit Bunch (OPEFB) fibres . In
[0014] PID201904109, the OPEFB fibres serve as a filler and reinforcement material for the epoxy thermoset polymer . Meanwhile, in this proposed invention, the cellulose bacteria function as a filler and reinforcement material for the polymer in the wood veneer .
[0015] Patent S00202112055, "Hemp Fibre Reinforced and Tungsten
[0016] Carbide Ceramic Coated Polymer Composite for Bulletproof Panels, " describes the manufacturing method of bulletproof panels by combining ceramic tungsten carbide with hemp fibre . In patent
[0017] S00202112055, hemp fibre is used as the second layer . Meanwhile, in this proposed invention, the second layer combines wood veneer and aramid fibres to improve the panel' s strength in stopping bullets .
[0018] Based on our search of existing patents, this invention has not been done before and can potentially be an alternative material for composite armour in bulletproof vests .
[0019] Summary of the Invention
[0020] This invention aims to provide products and describe the manufacturing process of a hybrid wood veneer composite modified with bacterial cellulose and woven aramid fibres . The product materials in this invention consist of (a) wood veneers, (b) bacterial cellulose and (c) aramid woven fibres . The hybrid wood veneer composite manufacturing process begins with preparing wood veneers, delignification, adding bacterial cellulose to the veneer, drying, solidifying the material using a hot press machine, and making a hybrid composite product by placing woven aramid fibres between the modified wood veneers and adding epoxy as an adhesive .
[0021] The hybrid composites in this invention have better ballistic energy and trauma energy-absorbing properties compared to non- hybrid composites as the constituent material of bulletproof vests .
[0022] Brief Description of the Figures
[0023] This invention can be illustrated with a figure, as presented below: Figure 1 is a flow diagram of this invention’ s manufacturing process of a hybrid wood veneer composite modified with bacterial cellulose and aramid woven fibres .
[0024] Description of the Invention
[0025] This invention aims to provide a product and describe the manufacturing process of a hybrid wood veneer composite modified with bacterial cellulose and aramid woven fibres . The materials in this invention consist of (a) wood veneers, (b) bacterial cellulose, and (c) aramid woven fibres . The manufacturing process of hybrid wood veneer composites modified with bacterial cellulose and aramid woven fibres in this invention is composed of the following stages :
[0026] 1 . Preparation of raw materials
[0027] The wood veneers are cut into 150 mm lengths that are 150 mm wide and 2.3 mm thick, using a cutting machine . After that, the wood veneers are boiled at 50°C-100°C in a solution of 0.5-1 Molar NaOH for 60-90 minutes . Next, the wood veneers are lifted and placed into a container . Then, 0.5-1 litre of boiled coconut water and bacterial cellulose from an Acetobacter xylinum culture is poured into the container containing the veneer in a ratio of 1 : 2 to 1 :
[0028] 3. Next, the container is closed with sterile paper and stored at a temperature of 30°C-35 ° C for 3-7 days .
[0029] 2. Manufacturing Process of the Hybrid Composite
[0030] The soaked veneers are lifted, cleaned, and drained to a water content of 20-40% . Next, the veneer is pressed with a hot press machine at a temperature of 120°C-150°C with a pressure of 8-10
[0031] MPa for 10-20 minutes . The wood veneer is then removed from the hot press machine . Epoxy adhesives are then applied to the pressed wood veneers, and the veneers are placed on the bottom of a mould with a length of 150 mm and a width of 150 mm. Afterwards, woven aramid fibres are applied with epoxy adhesive and placed on the wood veneer . Next, the pressed wood veneers applied with epoxy are placed on top of the woven aramid fibres . Then, the combined wood veneer and aramid fibres are pressed with cold press machines for
[0032] 12-24 hours . Finally, the hybrid composite product is left at room temperature for seven days before it is ready for use .
[0033] 3 . Hybrid composite testing
[0034] Ballistic tests were conducted at threat Level III using NATO standard 7. 62 mm calibre bullets with STEYR SSG 08 weapons per NIJ procedure 0101.06.
[0035] Furthermore, the embodiment of this invention will be shown through an example . However, this example does not limit the embodiments of the invention.
[0036] <Embodiment of the Invention)
[0037] Based on the study' s results (Table 1 ) , hybrid wood veneer composites modified with bacterial cellulose and aramid woven fibres can absorb ballistic energy and trauma energy.
[0038] Tabel 1. Hybrid composite ballistic test .
Claims
Claims1 . A hybrid composite manufacturing process that consists of the following stages : a) preparing and choosing teak wood veneer; b) boiling the wood veneer at a temperature of 50°C - 100°C in a solution of 0.5-1 Molar NaOH for 60-90 minutes; c) lifting and draining the boiled wood veneer into a container; d) soaking wood veneer in boiled coconut water and bacterial cellulose from an acetobacter xylinum culture with a ratio of 1 : 2 to 1 : 3; e) closing the container using sterile paper and storing at a temperature of 30-35°C for 3-7 days; f) lifting, cleaning, and draining the veneer to obtain wood veneers with a 20% 60% water content; g) pressing the wood veneer with a hot press machine at a temperature of 120°C-150°C with a pressure of 8-10 MPa for10-20 minutes; h) removing and evenly applying epoxy adhesive to the wood veneers, placing the veneers on the bottom of a mould with a length of 150 mm and a width of 150 mm; i) placing the aramid woven fibres in between the wood veneers that were applied with epoxy adhesive; j ) pressing the wood veneer and aramid fibre stack with a cold press machine for 12 - 24 hours; k) conditioning the hybrid composite product by leaving it at room temperature for 7 days before it is ready for use; l) finally, the hybrid composites are produced.
2. A hybrid composite that has the following characteristics : lightweight, rigid, and has a BFS Test value that meets level III testing criteria per the NIJ 0101.06 standard.
Citation Information
Patent Citations
Bulletproof wood plate
CN106364072A
Method for producing electric heating composite material based on high frequency non-adhesive consolidation technique