Silicone composition for release sheet and release sheet
The silicone composition for release sheets, featuring specific organopolysiloxanes and organohydrogensiloxanes, addresses the challenge of poor adhesion and durability by forming a cured film with excellent substrate adhesion and low peeling force, maintaining performance under harsh conditions without compromising release properties.
Patent Information
- Application Number
- PCT/JP2023/019985
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-29
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional silicone compositions for release sheets exhibit poor adhesion to plastic films and lack durability under harsh environmental conditions such as high temperature and high humidity, while attempting to improve adhesion often compromises release properties.
A silicone composition comprising specific organopolysiloxanes with alkenyl groups, glycidyl groups, and organohydrogensiloxanes, which form a cured film with excellent adhesion to substrates and low peeling force, maintaining adhesion over time even in severe conditions without affecting release properties.
The composition achieves both strong adhesion to substrates and low peeling force, maintaining performance under high temperature and high humidity conditions without impairing release properties, addressing the limitations of existing compositions.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Silicone composition for release sheets and release sheets
[0001] The present invention relates to a silicone composition for release sheets, and to a release sheet obtained using said composition.
[0002] Conventionally, release properties for adhesive materials have been imparted by forming a cured coating of a silicone composition on the surface of a sheet-like substrate such as paper or plastic film.
[0003] A well-known method for forming a cured coating of a silicone composition on the surface of a substrate is to use a platinum-based compound as a catalyst to carry out an addition reaction between an alkenyl group-containing organopolysiloxane and an organohydrogenpolysiloxane to form a release coating on the surface of the substrate. Although this type of silicone composition adheres well to paper substrates, it has long been pointed out that it has poor adhesion to plastic films such as polyester films and polypropylene films, and that it requires pretreatment of the substrate.
[0004] As a method for improving adhesion to the substrate, RSiO 3/2 A composition of a base polymer having a branched structure containing alkenyl units has been reported, but this method is not practical because it requires the use of a large amount of branched organopolysiloxane containing alkenyl groups, which increases the production cost.
[0005] Patent Document 1 reports the addition of an organopolysiloxane having an epoxy group as a method for improving adhesion to a substrate by using a small amount of an additive. However, this method only describes substrate adhesion under high temperature and high humidity conditions, and does not evaluate adhesion immediately after curing or after storage at room temperature. Furthermore, there is no description of the effect of adding an organopolysiloxane having an epoxy group on release properties.
[0006] In Patent Document 2, adhesion to a substrate is improved by adding a reaction product of a liquid polyorganosiloxane containing alkenyl groups and silanol groups with a hydrolyzable silane containing epoxide groups. However, this method also does not consider the effect of the addition on release properties.
[0007] In Patent Document 3, an alkenyl-containing low-molecular-weight siloxane is added, and the coating is cured by heating after irradiating with ultraviolet light, thereby improving substrate adhesion without affecting release properties. However, this method requires a heating dryer and a UV irradiation device.
[0008] Recently, release sheet performance has been required to have not only a lower release force than conventional products, but also high durability that can maintain good substrate adhesion even under harsh environments such as high temperatures and high humidity during the release sheet molding process. However, existing release sheet compositions tend to have poorer substrate adhesion as the release force decreases, and there are hardly any compositions that can satisfy the requirement for long-term adhesion under even harsher environments. This is thought to be because many of the materials that are effective in achieving low release, such as those used as various migration components, act to reduce adhesion to the substrate, and it is actually difficult to achieve both low release and excellent substrate adhesion.
[0009] In order to solve the above problems, we previously proposed in Patent Document 4 that a silicone composition using a combination of an epoxy group-containing siloxane with a specific structure and an organohydrogensiloxane can achieve both easy release and excellent adhesion to substrates. However, depending on the application, further improvements may be required.
[0010] Japanese Patent Application Publication No. 2011-132532 Japanese Patent Application Publication No. 2010-500462 Japanese Patent Application Publication No. 2011-252142 International Publication No. 2021 / 192100
[0011] The present invention has been made in view of the above circumstances, and has as its object the provision of a silicone composition for release sheets that is capable of forming a cured coating (release coating) that has excellent adhesion to substrates and imparts a small release force by not increasing the release force, and that maintains the adhesion of the coating to the substrate for long periods of time, even in harsh environments such as high temperatures and high humidity.
[0012] A further object of the present invention is to provide a release sheet obtained from the composition of the present invention.
[0013] The present invention has been made to solve the above-mentioned problems, and provides an addition-curable silicone composition for release sheets, comprising: (A) 100 parts by mass of an organopolysiloxane having at least two alkenyl groups per molecule, the alkenyl group content being 0.001 to 0.2 mol / 100g, and having a 30% by mass toluene dilution viscosity at 25°C of 0.001 to 70 Pa·s; (B) a component including the following compounds (B1), (B2), and (B3): (B1) 0.1 to 8 parts by mass of an organopolysiloxane containing per molecule 10 mol% or more siloxane units having a glycidyl group and / or glycidoxy group bonded to a silicon atom via a carbon atom, containing 0.002 to 0.02 mol / 100g of silanol groups, and containing 0.5 to 2.5 mol / 100g of alkoxy groups, and having an average degree of polymerization of 3 to 50; (B2) an organohydrogensiloxane having at least three silicon-bonded hydrogen atoms per molecule, an average degree of polymerization of 10 to 200, and 5 to 20 mol % of the substituents being aryl groups: 0.05 to 2.0 parts by mass; (B3) an organopolysiloxane having an alkenyl group content of 0.3 mol / 100 g or more and a viscosity at 25°C of 0.01 to 1 Pa s: 0.05 to 3.0 parts by mass; (C) an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms per molecule, other than the (B2) compound: the number of moles of silicon-bonded hydrogen atoms in component (C) corresponds to 0.5 to 15 times the number of moles of alkenyl groups in the composition; (D) a platinum group metal catalyst: a catalytic amount; (E) an organic solvent: 0 to 20,000 parts by mass; The present invention provides an addition-curable silicone composition for release sheets, which comprises:
[0014] The silicone composition for release sheets of the present invention contains the above-mentioned components (A), (B), (C), and (D) in predetermined amounts, and is therefore capable of forming a cured coating (release coating) that exhibits excellent adhesion to substrates, particularly plastic film substrates such as polyester films. Furthermore, the cured coating obtained from the silicone composition for release sheets of the present invention is capable of exhibiting a low release force, and despite exhibiting such a low release force, it is able to maintain good substrate adhesion for long periods of time, even when placed under harsh conditions of high temperature and high humidity, as well as under conditions at room temperature.
[0015] The silicone composition for release sheets of the present invention is characterized in that the compound (B3) is R 9 (3-g1) R 8 g1 SiO 1 / 2 Siloxane units (M R8R9 Units), R 9 SiO 3 / 2 Siloxane units (T R9 units) (wherein R 8 are independently an alkenyl group, and R 9 are independently unsubstituted or halogen atom- or cyano group-substituted monovalent hydrocarbon groups that do not contain aliphatic unsaturated bonds, and g1 is a number from 0 to 3. R8R9 Unit / T R9 The molar ratio of the units is 2 / 8 to 8 / 2, and the molecular end is M R8R9 It is preferable that the organopolysiloxane is an organopolysiloxane in which the unit is a silanol group or an alkoxy group, some of which form the terminals.
[0016] By including such a compound (B3), better adhesion can be obtained.
[0017] The compound (B1) is preferably an organopolysiloxane that is a partial hydrolysis condensate of an organoalkoxysilane represented by the following general formula (1-1) and at least one of organoalkoxysilanes represented by the following general formulas (1-2), (1-3), and (1-4), or a mixture thereof. (In the formula, R1 may be the same or different and is an unsubstituted or substituted hydrocarbon group having 1 to 10 carbon atoms and no aliphatic unsaturated bond, which may contain an oxygen atom, or a hydrogen atom; R12 is an unsubstituted or substituted hydrocarbon group having 1 to 20 carbon atoms; and n is an integer from 3 to 10.)
[0018] The inclusion of such a (B1) compound can improve the strength of the cured product and achieve a greater adhesion-improving effect. The (B3) compound, which has a higher alkenyl group content and lower viscosity than the (A) component, has less restriction on molecular movement in the composition and is excellent in reactivity with SiH groups, improving curability and reducing the number of remaining SiH groups, thereby achieving an easy release effect. Furthermore, it is presumed that the crosslinking density increases as the crosslinking reaction progresses, thereby improving substrate adhesion immediately after curing.
[0019] The compound (B1) is preferably a partial hydrolysis condensate of an organoalkoxysilane mixture containing organoalkoxysilanes represented by the general formulas (1-1) and (1-4) as essential components and organoalkoxysilanes represented by the general formulas (1-2) and (1-3) as optional components, and is preferably an organopolysiloxane having a linear, branched or cyclic siloxane structure, or a mixture thereof.
[0020] By including such a compound (B1), the strength of the cured product can be further improved, and a higher adhesion improving effect can be exhibited.
[0021] The silicone composition for release sheets according to claim 1, wherein the compound (B2) is an organohydrogensiloxane represented by the following general formula (2-1) or (2-2), or a mixture thereof: (R12) 3 SiO-{(R12)HSiO} m {(R12) 2 SiO} n -Si(R12) 3 ...(2-1) (R12) 2 HSiO-{(R12)HSiO} m {(R12) 2 SiO} n -SiH(R12)2 (2-2) (wherein R12 may be the same or different and are unsubstituted or substituted hydrocarbon groups having 1 to 20 carbon atoms, 5 to 20 mol % of the total number of substituents, which is the sum of H groups directly bonded to Si and R12, are aryl groups, and m+n is an integer of 2 to 198)
[0022] By incorporating such a (B2) compound in combination with a (B1) compound, the strength of the cured product can be improved and a more effective adhesion improvement effect can be achieved. Since it is difficult to obtain a sufficient adhesion improvement effect when the (B2) compound is used alone, it is presumed that this is because the (B1) and (B3) compounds increase the strength of the adhesion-improving layer formed at the interface between the silicone cured coating and the substrate, and strengthen the bond between the adhesion-improving layer and the substrate and the silicone cured coating.
[0023] In the silicone composition for release sheets of the present invention, the (B2) compound and the (B3) compound are preferably blended in such a manner that the number of moles of hydrogen atoms bonded to silicon atoms in the (B2) compound divided by the number of moles of alkenyl groups in the (B3) compound is 1.6 or more parts by mass.
[0024] Such a blending ratio can achieve a higher adhesion improving effect.
[0025] The present invention also provides a release sheet obtained by applying the silicone composition for release sheets of the present invention to a paper substrate or a film substrate and curing the composition.
[0026] The release sheet of the present invention is obtained by applying the silicone composition for release sheets of the present invention to a substrate and curing it. Therefore, the cured film obtained by curing is able to exhibit a small release force and good adhesion to the substrate, and this good adhesion to the substrate can be maintained for long periods of time even when placed under harsh conditions of high temperature and high humidity, as well as at room temperature.
[0027] The silicone composition for release sheets of the present invention not only produces a non-tacky cured coating that has excellent adhesion to the substrate, but also produces good release properties with little change in the non-tackiness of the cured coating before and after adhesion improvement. Conventional adhesion improvement techniques inevitably affect release properties, but a release sheet formed with a cured coating of the silicone composition for release sheets of the present invention can improve adhesion to the substrate with almost no effect on release properties. Furthermore, the cured coating produced by the silicone composition for release sheets of the present invention can maintain good adhesion to the substrate for long periods of time, even when placed under harsh conditions of high temperature and high humidity.
[0028] The present invention will be described in detail below, but the present invention is not limited thereto. In the present invention, the term "release sheet" should be understood in a broad sense, and may be, for example, a release paper containing a paper substrate, or a release film containing a film made of plastic or the like. The composition for release sheets should also be understood in a broad sense, and may be, for example, a silicone composition for release paper, or a silicone composition for release films.
[0029] The present inventors have conducted extensive research to achieve the above object, and as a result, have found that a composition containing: 100 parts by mass of component (A), which is an organopolysiloxane having at least two alkenyl groups per molecule, with an alkenyl group content of 0.001 to 0.2 mol / 100 g, and having a 30% by mass toluene dilution viscosity at 25°C of 0.001 to 70 Pa s; 0.1 to 8 parts by mass of compound (B1), which is an organopolysiloxane containing 10 mol% or more siloxane units having glycidyl groups and / or glycidoxy groups bonded to silicon atoms via carbon atoms per molecule, 0.002 to 0.02 mol / 100 g of silanol groups, and 0.5 to 2.5 mol / 100 g of alkoxy groups, and having an average degree of polymerization of 3 to 50; and 0.1 to 8 parts by mass of compound (B2), which is an organopolysiloxane containing at least two alkenyl groups per molecule, with an alkenyl group content of 0.001 to 0.2 mol / 100 g, and having a 30% by mass toluene dilution viscosity at 25°C of 0.001 to 70 Pa s. a component (B) comprising: 0.05 to 2.0 parts by mass of a (B2) compound which is an organohydrogensiloxane having at least three hydrogen atoms, an average degree of polymerization of 10 to 200, and in which 5 to 20 mol % of the substituents are aryl groups; and 0.05 to 3.0 parts by mass of a (B3) compound which is an organopolysiloxane having an alkenyl group content of 0.3 mol / 100 g or more and a viscosity at 25°C of 0.01 to 1 Pa s; The inventors have found that a cured coating having excellent adhesion to a substrate can be obtained by using a composition containing: component (C), which is an organohydrogenpolysiloxane different from compound (B2) and which has at least two hydrogen atoms bonded to silicon atoms per molecule; an amount in which the number of moles of hydrogen atoms bonded to silicon atoms in component (C) corresponds to 0.5 to 15 times the number of moles of alkenyl groups in the composition; (D) a platinum group metal catalyst: a catalytic amount; and (E) an organic solvent: 0 to 20,000 parts by mass.
[0030] Furthermore, while conventional adhesion improvement techniques have failed to provide sufficient substrate adhesion with compositions having a low release force, the present inventors have found that the composition of the present invention can simultaneously achieve both a low release force and excellent substrate adhesion, and that this excellent substrate adhesion can be maintained for a long period of time, leading to the present invention.
[0031] In the aforementioned Patent Document 4, we have previously achieved a similar effect using a composition that combines an epoxy group-containing siloxane and an organohydrogensiloxane, but in the present invention we have discovered a composition that further enhances this effect, leading to the present application.
[0032] [Silicone Composition for Release Sheets] The addition-curable silicone composition for release sheets of the present invention comprises: (A) 100 parts by mass of an organopolysiloxane having at least two alkenyl groups per molecule, the alkenyl group content being 0.001 to 0.2 mol / 100 g, and having a 30% by mass toluene dilution viscosity at 25°C of 0.001 to 70 Pa s; (B) a component containing the following compounds (B1), (B2), and (B3): (B1) 0.1 to 8 parts by mass of an organopolysiloxane containing per molecule 10 mol % or more siloxane units having a glycidyl group and / or glycidoxy group bonded to a silicon atom via a carbon atom, containing 0.002 to 0.02 mol / 100 g of silanol groups, and 0.5 to 2.5 mol / 100 g of alkoxy groups, and having an average degree of polymerization of 3 to 50; (B2) 0.05 to 2.0 parts by mass of an organohydrogensiloxane having at least three silicon-bonded hydrogen atoms per molecule, an average degree of polymerization of 10 to 200, and in which 5 to 20 mol % of the substituents are aryl groups; (B3) 0.05 to 3.0 parts by mass of an organopolysiloxane having an alkenyl group content of 0.3 mol / 100 g or more and a viscosity at 25°C of 0.01 to 1 Pa s; (C) an organohydrogenpolysiloxane other than the compound (B2) having at least two silicon-bonded hydrogen atoms per molecule, in an amount such that the number of moles of silicon-bonded hydrogen atoms in component (C) is 0.5 to 15 times the number of moles of alkenyl groups in the composition; (D) a platinum group metal catalyst: a catalytic amount; (E) 0 to 20,000 parts by mass of an organic solvent.
[0033] In the silicone composition for release sheets of the present invention, the organic solvent (E) is an optional component, since its blending amount may be 0 parts by mass per 100 parts by mass of component (A). Furthermore, the silicone composition for release sheets of the present invention can also contain other optional components in addition to components (A), (B), (C), and (D). Specific examples of such optional components are described below.
[0034] Each component of the silicone composition for release sheets of the present invention will now be described in turn.
[0035] [Component (A): Organopolysiloxane Having Alkenyl Groups] The component (A) used in the present invention is an organopolysiloxane having at least two alkenyl groups per molecule, an alkenyl group content of 0.001 to 0.2 mol / 100 g, and a viscosity at 25°C when diluted with 30% by mass of toluene of 0.001 to 70 Pa s, and is preferably represented by the following general formula (5):
[0036]
[0037] In the above formula (5), R 5 are the same or different, and are unsubstituted or substituted monovalent hydrocarbon groups having 1 to 20 carbon atoms and no aliphatic unsaturated bonds, or alkenyl groups having 2 to 12 carbon atoms which may contain an oxygen atom; R 5 At least two of the groups are alkenyl groups.
[0038] Specific examples of the monovalent hydrocarbon group having 1 to 20 carbon atoms and no aliphatic unsaturated bonds include alkyl groups preferably having 1 to 6 carbon atoms, such as methyl, ethyl, propyl, and butyl; cycloalkyl groups preferably having 5 to 8 carbon atoms, such as cyclohexyl; aryl groups preferably having 6 to 10 carbon atoms, such as phenyl and tolyl; aralkyl groups preferably having 7 to 10 carbon atoms, such as benzyl; and monovalent hydrocarbon groups having 1 to 10 carbon atoms selected from hydroxypropyl, cyanoethyl, 3-chloropropyl, and 3,3,3-trifluoropropyl groups in which some or all of the hydrogen atoms bonded to the carbon atoms of these groups have been substituted with hydroxy groups, cyano groups, halogen atoms, or the like. However, from the viewpoint of releasability in particular, the monovalent hydrocarbon group having 1 to 20 carbon atoms and no aliphatic unsaturated bonds is preferably an alkyl group or an aryl group, and more preferably a methyl group, ethyl group, propyl group, or phenyl group.
[0039] The alkenyl group having 2 to 12 carbon atoms which may contain an oxygen atom is —(CH 2 ) x -CH=CH 2 (x is 0 or a positive number from 1 to 10), and specific examples thereof include vinyl, propenyl, butenyl, hexenyl, octenyl, and decenyl groups. The methylene chain may contain an ether bond, for example, -(CH 2 ) 2 -O-CH 2 -CH=CH 2 , -(CH 2 ) 3 -O-CH 2 -CH=CH 2 Among these, a vinyl group is preferred.
[0040] The organopolysiloxane of component (A) contains two or more alkenyl groups per molecule. That is, the organopolysiloxane of component (A) contains at least two alkenyl groups per molecule. Fewer than two alkenyl groups are likely to leave uncrosslinked molecules after curing, undesirably reducing curability. The organopolysiloxane of component (A) may contain, for example, up to 2,000 alkenyl groups per molecule. Furthermore, the alkenyl group content per 100 g of organopolysiloxane of component (A) is 0.001 to 0.2 mol, more preferably 0.002 to 0.15 mol. A content of less than 0.001 mol may result in reduced curability, while a content of more than 0.2 mol may result in heavy release.
[0041] The viscosity of component (A) at 25°C when diluted with 30% by mass of toluene is 0.001 to 70 Pa·s, preferably 0.005 to 60 Pa·s when diluted with 30% by mass of toluene, and more preferably 0.01 to 50 Pa·s when diluted with 30% by mass of toluene. If the viscosity is less than 0.001 Pa·s, the composition will not have sufficient coatability, and if it exceeds 70 Pa·s, workability will decrease. The viscosity can be measured using a rotational viscometer (the same applies hereinafter).
[0042] In the above formula (5), h, i, j, and k are selected from positive numbers that satisfy the above viscosity range, and in particular, h is a positive number of 2 or more, preferably 2 to 300; i is a positive number of 30 or more, preferably 50 to 19,998, and more preferably 100 to 14,700; j is a number of 0 or more, preferably 0 to 100; k is a number of 0 or more, preferably 0 to 100; and 32≦h+i+j+k≦20,000, and preferably 100≦h+i+j+k≦15,000.
[0043] Specific examples of component (A) include, but are not limited to, the following: In the following formula, Me, Vi, and Ph represent a methyl group, a vinyl group, and a phenyl group, respectively.
[0044]
[0045]
[0046] [Component (B)] The component (B) used in the present invention is an adhesion improving component, and is a component containing the following compounds (B1), (B2) and (B3).
[0047] Compound (B1) Compound (B1) is a compound that has the effect of improving adhesion when incorporated into the composition of the present invention, and is an organopolysiloxane that contains, per molecule, 10 mol % or more siloxane units having a glycidyl group and / or glycidoxy group bonded to a silicon atom via a carbon atom, 0.002 to 0.02 mol / 100 g of silanol groups, and 0.5 to 2.5 mol / 100 g of alkoxy groups, and has an average degree of polymerization of 3 to 50. Compound (B1) is used in an amount of 0.1 to 8 parts by mass per 100 parts by mass of component (A).
[0048] The (B1) compound is highly effective in maintaining the substrate adhesion of the cured coating (release coating) obtained using the composition of the present invention even under heated and humidified conditions (high-temperature, high-humidity environments), and is a component that is added in the hope of improving adhesion, particularly under severe usage conditions. The average degree of polymerization is the weight-average degree of polymerization in terms of polystyrene, determined by gel permeation chromatography (GPC).
[0049] The organopolysiloxane of compound (B1) is an organopolysiloxane containing 10 mol% or more of siloxane units having glycidyl groups and / or glycidoxy groups bonded to silicon atoms via carbon atoms per molecule, and if the content of these siloxane units is less than 10 mol%, the adhesive effect to the substrate cannot be obtained. The upper limit of the content of these siloxane units is not particularly limited, but can be, for example, 100 mol%.
[0050] The organopolysiloxane (B1) compound contains 0.002 to 0.02 mol / 100 g of silanol groups. If the silanol group content is less than 0.002 mol / 100 g, sufficient adhesion to the substrate cannot be achieved. On the other hand, if the silanol group content exceeds 0.02 mol / 100 g, there is a risk of adversely affecting release properties. The silanol group content is preferably 0.003 to 0.02 mol / 100 g.
[0051] The organopolysiloxane (B1) compound contains 0.5 to 2.5 mol / 100g of alkoxy groups. If the alkoxy group content is less than 0.5 mol / 100g, sufficient adhesion to the substrate cannot be achieved. On the other hand, if the alkoxy group content exceeds 2.5 mol / 100g, there is a risk of adversely affecting release properties. The alkoxy group content is preferably 0.6 to 2.0 mol / 100g.
[0052] The organopolysiloxane that is compound (B1) has an average degree of polymerization of 3 to 50, and preferably 3 to 20. If the average degree of polymerization is less than 3, the adhesion to the substrate is insufficient, whereas if the average degree of polymerization exceeds 50, the adhesion to the substrate decreases or workability decreases.
[0053] The organopolysiloxane of compound (B1) may be linear, branched, or cyclic, or may be a mixture thereof, but is preferably a partial hydrolysis condensate of an organoalkoxysilane. Among the organoalkoxysilanes used as raw materials, the alkoxysilane having a glycidyl group and / or a glycidoxy group bonded to a silicon atom via a carbon atom is preferably a unit trifunctional organoalkoxysilane, and more preferably an organoalkoxysilane represented by the following general formula (1-1): (In the formula, R1 may be the same or different and represents an unsubstituted or substituted hydrocarbon group having 1 to 10 carbon atoms and no aliphatic unsaturated bond, which may contain an oxygen atom, or a hydrogen atom; and n is an integer from 3 to 10.)
[0054] Specific examples of organoalkoxysilanes include the following:
[0055] As the other organoalkoxysilane to be co-hydrolyzed and condensed with the above alkoxysilane, at least one of the organoalkoxysilanes represented by the following general formulas (1-2), (1-3), and (1-4) is preferably used, and more preferably trifunctional and tetrafunctional alkoxysilanes represented by the following general formulas (1-3) and (1-4) are used. By including such a branched structure or three-dimensional crosslinked structure in the molecule or by imparting the ability to form it during the process of forming the cured product, the strength of the cured product is improved. Furthermore, by appropriately reducing the solubility and dispersibility of the (B1) compound in a silicone cured coating layer that is mainly composed of a linear structure and has excellent mold releasability, the (B1) compound is more likely to collect near the interface between the substrate and the silicone cured coating, which is thought to provide a greater adhesion-improving effect.
[0056] (R12) 2 -Si(OR1) 2 ...(1-2) R12-Si (OR1) 3 ...(1-3) Si (OR1) 4 ....(1-4) (In the formula, R1 may be the same or different and is an unsubstituted or substituted hydrocarbon group having 1 to 10 carbon atoms and no aliphatic unsaturated bond, which may contain an oxygen atom, or a hydrogen atom, and R12 is an unsubstituted or substituted hydrocarbon group having 1 to 20 carbon atoms.)
[0057] Specific examples of organoalkoxysilanes that undergo co-hydrolytic condensation with alkoxysilanes having a glycidyl group and / or glycidoxy group bonded to a silicon atom via a carbon atom (for example, organoalkoxysilanes of general formula (1-1)) include the following:
[0058] In the above formula (1-1), the hydrogen atoms on the monovalent organic group having a glycidoxy group may be replaced by a substituent. In terms of safety and economy, the substituent is preferably one other than an epoxycyclohexyl group. Examples of epoxycyclohexyl groups include a 3,4-epoxycyclohexylmethyl group, a 2-(3,4-epoxycyclohexyl)ethyl group, and a 3-(3,4-epoxycyclohexyl)propyl group.
[0059] Furthermore, R1 is a hydrogen atom or an unsubstituted or substituted hydrocarbon group having 1 to 10 carbon atoms and no aliphatic unsaturated bonds, which may contain an oxygen atom. Specific examples of the hydrocarbon group represented by R1 include alkyl groups such as methyl, ethyl, propyl, and butyl; cycloalkyl groups such as cyclohexyl; aryl groups such as phenyl and tolyl; aralkyl groups such as benzyl and phenethyl; and groups in which some or all of the hydrogen atoms bonded to carbon atoms of these groups have been substituted with hydroxy groups, such as a hydroxypropyl group. Of these groups, R1 is preferably a hydrogen atom or an alkyl group, and more preferably an alkyl group having 1 to 5 carbon atoms.
[0060] The following siloxane units formed by the partial hydrolysis and condensation reaction of organoalkoxysilanes represented by the above general formulas (1-1) to (1-4) are respectively represented by T E , D, T, Q, (B1) compound D a T E b T c Q d This can be expressed as the average equation: Here, a+b+c+d is 3 to 50, b / (a+b+c+d) is 0.1 to 1, a, c, and d are each independently 0 to 35, and the molecular terminals that do not form siloxane bonds with other siloxane units are alkoxy groups or silanol groups.
[0061] The compound (B1) preferably does not have an alkenyl group in the molecule. By including such a compound (B1), the adhesion effect to the substrate can be improved.
[0062] The amount of compound (B1) added is in the range of 0.1 to 8 parts by mass, preferably 0.1 to 7 parts by mass, per 100 parts by mass of the organopolysiloxane of component (A). Less than 0.1 part by mass fails to improve adhesion to the substrate, whereas more than 8 parts by mass affects release properties and reduces the strength of the cured coating. More than 8 parts by mass may make it difficult to maintain excellent adhesion to the substrate over long periods of time, even under harsh environments.
[0063] Specific examples of the compound (B1) include the following:
[0064] More preferred examples include: Examples include:
[0065] Preferably, the (B1) compound is a partial hydrolysis condensate of an organoalkoxysilane mixture containing organoalkoxysilanes represented by the above general formulas (1-1) and (1-4) as essential components and organoalkoxysilanes represented by the above general formulas (1-2) and (1-3) as optional components, and is an organopolysiloxane having a linear, branched, or cyclic siloxane structure, or a mixture thereof. By including such a (B1) compound, the strength of the cured product can be further improved and a greater adhesion-improving effect can be achieved.
[0066] (B2) Compound The (B2) compound is an organohydrogensiloxane having at least three hydrogen atoms bonded to silicon atoms per molecule, an average degree of polymerization of 10 to 200, and 5 to 20 mol % of the substituents being aryl groups. When used in combination with the (B1) and (B3) compounds, its adhesion-improving effect is further enhanced. If the number of hydrogen atoms bonded to silicon atoms in the (B2) compound per molecule is less than three, the adhesion-improving effect cannot be obtained. There is no upper limit, but it is preferably in the range of 0.5 to 1.5 mol / 100g, more preferably 0.7 to 1.3 mol / 100g. If it exceeds 1.5 mol / 100g, the release properties of the cured coating decrease.
[0067] Although the adhesion-improving effect can be obtained even when compound (B2) is used alone, it is presumed that when compound (B1) and compound (B3) are used in combination, compounds (B1) and (B3) increase the strength of the adhesion-improving layer formed at the interface between the silicone cured coating and the substrate, thereby strengthening the bond between the adhesion-improving layer and the substrate and the silicone cured coating.
[0068] Its average degree of polymerization is 10 to 200; if it is less than 10, the adhesion-improving effect is low, and if it exceeds 200, stability decreases, which is undesirable. The average degree of polymerization of the (B2) compound is more preferably 20 to 150. 5 to 20 mol % of its substituents are aryl groups; if it is less than 5 mol %, the adhesion-improving effect is insufficient, and if it exceeds 20 mol %, compatibility with other components decreases, which is undesirable. It is more preferable that this is 8 to 18 mol % of the substituents on the organohydrogensiloxane.
[0069] A preferred structure of the compound (B2) is one in which the main chain is mainly composed of siloxane units H(R12)SiO 2/2 Here, R12 may be the same or different and is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 20 carbon atoms.
[0070] More preferred are organohydrogensiloxanes represented by the following general formula (2-1) or (2-2), or mixtures thereof: (R12) 3 SiO-{(R12)HSiO}m{(R12) 2 SiO}n-Si (R12) 3 ...(2-1) (R12) 2 HSiO-{(R12)HSiO}m{(R12) 2 SiO}n-SiH (R12) 2 (2-2) (wherein R12 may be the same or different and are unsubstituted or substituted hydrocarbon groups having 1 to 20 carbon atoms, 5 to 20 mol % of the total number of substituents, which is the sum of H groups directly bonded to Si and R12, are aryl groups, and m+n is an integer of 2 to 198)
[0071] The amount of compound (B2) blended is 0.05 to 2.0 parts by mass, more preferably 0.06 to 1.5 parts by mass, per 100 parts by mass of (A). Less than 0.05 parts by mass results in little improvement in adhesion, while more than 2.0 parts by mass may result in heavier release and other adverse effects on release properties. It is preferable that the amount of compound (B2) be such that the number of moles of hydrogen atoms bonded to silicon atoms in compound (B2) is 1.6 or more, more preferably 1.6 to 15, and even more preferably 1.7 to 10, relative to the number of moles of alkenyl groups in compound (B3).
[0072] Specific examples of the (B2) compound include the following:
[0073] (Me) 3 SiO-[H(Me)SiO]a'[(Me) 2 SiO]b'[(Ph) 2 SiO]c'-Si(Me) 3 Here, a' is 15 to 97, b' is 0 to 13, and c' is 1 to 6
[0074] H (Me) 2 SiO-[H(Me)SiO]a'[(Me) 2 SiO]b'[(Ph) 2 SiO]c'-Si(Me) 2 H where a' is 11 to 97, b' is 0 to 15, and c' is 1 to 7 [(Me) 3 SiO 1/2 ]a'[H(Me)SiO 2/2 ]b′[(Me) 2 SiO 2/2 ]c′[(Ph) 2 SiO]d'[MeSiO 3/2 ]e' where a'+b'+c'+d'+e'=10 to 100, c' is 13 or less, d' is 1 to 6, and the molecular end is (Me) 3 SiO 1/2 It is blocked by [H(Me) 2 SiO 1/2 ]a'[H(Me)SiO 2/2 ]b′[(Me) 2 SiO 2/2 ]c′[(Ph) 2 SiO]d'[MeSiO 3/2 ]e' where a'+b'+c'+d'+e'=10 to 100, c' is 15 or less, d' is 1 to 7, and the molecular end is (Me) 3 SiO 1/2 is blocked off by
[0075] More preferred compounds include those having the following average structural formula: [(Me) 3 SiO 1/2 ] 2 [H(Me)SiO 2/2 ] 108 [(Ph) 2 SiO]10 [(Me) 3 SiO 1/2 ] 2 [H(Me)SiO 2/2 ] 88 [(Ph) 2 SiO] 10 [(Me) 3 SiO 1/2 ] 2 [H(Me)SiO 2/2 ] 56 [(Ph) 2 SiO] 12
[0076] Compound (B3) Compound (B3) is an organopolysiloxane having an alkenyl group content of 0.3 mol / 100 g or more and a viscosity of 0.01 to 1 Pa·s at 25°C. Compound (B3) is used in an amount of 0.05 to 3.0 parts by mass per 100 parts by mass of component (A). Preferably, compound (B3) is an organopolysiloxane having a monofunctional siloxane unit of the following formula and R 9 (3-g1) R 8 g1 SiO 1/2 (Hereafter M R8R9 The trifunctional siloxane unit of the following formula is an essential unit, R 9 SiO 3/2 (Hereafter T R9 (Written as unit) M R8R9 Unit / T R9 An organopolysiloxane in which the molar ratio of units is 2 / 8 to 8 / 2, and the molecular terminal is M R8R9 It is desirable that the units are bonded together, but some of them may form terminal groups as silanol groups or alkoxy groups. 8 are independently alkenyl groups, among which vinyl groups are industrially preferred. 9 are independently unsubstituted or halogen atom- or cyano-substituted monovalent hydrocarbon groups that contain no aliphatic unsaturated bonds, among which methyl and phenyl groups are industrially preferred. g1 is a number from 0 to 3, preferably 1 or 2.
[0077] (B3) Compound is the above M R8R9 Unit / T R9The molar ratio of the units is 2 / 8 to 8 / 2, preferably 3 / 7 to 7 / 3. A molar ratio of 2 / 8 or more is expected to improve adhesion, while a molar ratio of 8 / 2 or less is preferred because it facilitates industrial production. Compound (B3) also contains a bifunctional R 9 (2-g2) R 8 g2 SiO 2/2 Siloxane units (wherein g2 is 0, 1 or 2. D R8R9 unit), tetrafunctional SiO 4 / 2 Although it may contain siloxane units (Q units), when stronger adhesion is required, particularly in a release film, M R8R9 Place / T R9 Siloxanes with a molar ratio of units of 2 / 8 to 8 / 2 are preferred. R8R9 If it contains M or Q units, R8R9 Units and T R9 It is preferable to use a small amount relative to any one unit.
[0078] The amount of alkenyl groups in the organopolysiloxane of compound (B3) is preferably 0.3 to 2.5 mol / 100 g, more preferably 0.35 to 2.0 mol / 100 g, and even more preferably 0.4 to 1.5 mol / 100 g, expressed as the alkenyl group content per 100 g of organopolysiloxane. If this content is too low, the effect of improving adhesion may be reduced. A content below the above upper limit is preferred because a good pot life can be achieved. The organopolysiloxane of compound (B3) preferably has a viscosity at 25°C of 0.01 to 1 Pa s, particularly preferably 0.015 to 0.5 Pa s, more preferably 0.02 to 0.2 Pa s, and even more preferably 0.025 to 0.1 Pa s, and preferably has a degree of polymerization within this viscosity range. If the viscosity is less than 0.01 Pa·s, the effect of improving adhesion may be small, and if it exceeds 1 Pa·s, the solubility or dispersibility in the composition may decrease.
[0079] Specific examples of the compound (B3) include the following:
[0080] The amount of the (B3) compound is 0.05 to 3.0 parts by mass, preferably 0.1 to 2.5 parts by mass, per 100 parts by mass of component (A). Less than 0.05 parts by mass may result in a reduced effect in improving adhesion to the substrate, while more than 3.0 parts by mass may result in a reduced releasability of the cured coating. The (B3) compound is preferably incorporated so that the ratio of the number of moles of SiH groups in the (B2) compound to the number of moles of alkenyl groups in the (B3) compound (SiH groups / alkenyl groups) is 1.6 or more, more preferably 1.6 to 15, and even more preferably 1.7 to 10, in order to achieve both improved adhesion and the releasability of the cured coating.
[0081] [(C): Organohydrogenpolysiloxane] The silicone composition for a release sheet of the present invention further contains (C) an organohydrogenpolysiloxane that has at least two hydrogen atoms bonded to silicon atoms in each molecule and is different from the compound (B2).
[0082] The organohydrogenpolysiloxane of component (C) has at least two hydrogen atoms bonded to silicon atoms (hereinafter also referred to as "SiH groups") per molecule, and a cured coating is formed by addition reaction of these SiH groups with alkenyl groups in component (A) and compound (B3).
[0083] The organohydrogenpolysiloxane of component (C) is not particularly limited as long as it has at least two hydrogen atoms bonded to silicon atoms per molecule and is different from compound (B2). Specific differences from compound (B2) include, for example, the amount of aryl groups in the substituents being less than 5 mol %.
[0084] Examples of the component (C) include those represented by the following average composition formula (7).
[0085] R 7 s H t SiO (4-s-t)/2 (7) In the above formula (7), R 7are the same or different, and are unsubstituted or substituted monovalent hydrocarbon groups free from aliphatic unsaturated bonds, and specific examples include alkyl groups preferably having 1 to 6 carbon atoms, such as methyl, ethyl, propyl, and butyl groups; cycloalkyl groups preferably having 5 to 8 carbon atoms, such as cyclohexyl groups; aryl groups preferably having 6 to 10 carbon atoms, such as phenyl and tolyl groups; aralkyl groups preferably having 7 to 10 carbon atoms, such as benzyl groups; and hydroxypropyl groups, cyanoethyl groups, 3-chloropropyl groups, and 3,3,3-trifluoropropyl groups in which some or all of the hydrogen atoms bonded to carbon atoms of these groups have been substituted with hydroxy groups, cyano groups, halogen atoms, or the like. Of these, alkyl groups and aryl groups are preferred, and methyl groups are more preferred from the viewpoint of improving the addition reaction rate.
[0086] s is a positive number of 0.5 to 2, preferably 0.6 to 1.5; t is a positive number of 0.1 to 2, preferably 0.2 to 1.5; and s+t is 3.0 or less, particularly preferably 0.5 to 2.7.
[0087] Examples of organohydrogenpolysiloxanes represented by the above formula (7) include R 7 HSiO 2/2 Unit (R 7 is the same as above, the same below), HSiO 3/2 Units and R 7 2 HSiO 1/2 and optionally R 7 2 SiO 2/2 Unit, R 7 SiO 3/2 Units and R 7 3 SiO 1/2 Examples include polymers or copolymers further comprising at least one unit of R 7 HSiO 2/2 Unit or R 7 2 HSiO 1/2 It is preferable that the total number of the SiO units is at least 2, preferably 10 to 100, in one molecule. 4/2 The units may be contained in any amount.
[0088] The SiH group content in the organopolysiloxane of component (C) is preferably 0.1 to 1.7 mol / 100 g, and more preferably 0.2 to 1.6 mol / 100 g.
[0089] The organohydrogenpolysiloxane may be linear, branched, or cyclic, or may be a mixture thereof.
[0090] The viscosity of component (C) at 25°C is preferably 0.001 to 10 Pa s, and particularly preferably 0.005 to 5 Pa s. When the viscosity of component (C) is 0.001 to 10 Pa s, both appropriate curability and workability can be achieved.
[0091] Specific examples of component (C) include, but are not limited to, the following: In the following formula, Me and Ph represent a methyl group and a phenyl group, respectively.
[0092]
[0093] The amount of component (C) blended is such that the number of moles of hydrogen atoms bonded to silicon atoms is 0.5 to 15 times the number of moles of alkenyl groups in the composition, and preferably 1 to 10. By having the number of moles of hydrogen atoms bonded to silicon atoms in the composition be 0.5 to 15 times the number of moles of alkenyl groups, it is possible to further enhance curability and adhesion to the substrate while maintaining light releasability.
[0094] As explained above, compound (B2) contains Si—H groups and therefore contains silicon-bonded hydrogen atoms. Therefore, the silicon-bonded hydrogen atoms in the composition include hydrogen atoms bonded to silicon atoms in component (C) and compound (B2). The number of moles of silicon-bonded hydrogen atoms in the composition of the present invention is preferably 0.5 to 15 times the total number of moles of alkenyl groups in component (A) and compound (B3). That is, the total number of moles of silicon-bonded hydrogen atoms in component (C) and compound (B2) is preferably 0.5 to 15 times, and more preferably 1 to 13 times, the total number of moles of alkenyl groups in component (A) and compound (B3).
[0095] Furthermore, in this case, the blending amount of component (C) is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 15 parts by mass, and even more preferably 0.5 to 10 parts by mass, per 100 parts by mass of component (A), in terms of obtaining an appropriate crosslink density.
[0096] [(D): Platinum Group Metal Catalyst] The platinum group metal catalyst of component (D) is a catalyst for promoting the addition reaction between component (A) and compound (B3) and compound (B2) and component (C). Any catalyst known to those skilled in the art for promoting the so-called hydrosilylation reaction can be used. Examples of such platinum group metal catalysts include platinum-based, palladium-based, rhodium-based, and ruthenium-based catalysts, with platinum-based catalysts being particularly preferred. Examples of platinum catalysts include chloroplatinic acid, alcoholic or aldehyde solutions of chloroplatinic acid, complexes of chloroplatinic acid with various olefins or vinylsiloxanes, and platinum complexes with various olefins or vinylsiloxanes. The amount of component (D) used is a catalytic amount. To obtain a good cured coating, it is preferable to use a platinum group metal catalyst in an amount of 10 to 1,000 ppm, particularly 20 to 500 ppm, calculated as the mass of platinum group metal relative to the mass of component (A).
[0097] [(E): Organic Solvent for Dilution] The silicone composition of the present invention can optionally contain an organic solvent for dilution. Specifically, the organic solvent of component (E) is used in an amount of 0 to 20,000 parts by mass per 100 parts by mass of component (A).
[0098] The silicone composition of the present invention may also be a solvent-free composition obtained by blending the above components (A), (B), (C), and (D) with predetermined amounts of optional components. Diluting with an organic solvent provides practical advantages such as improved coating workability and improved coating film condition, including the thickness and surface finish of the coating film.
[0099] Usable organic solvents include aromatic hydrocarbon compounds such as toluene and xylene, aliphatic hydrocarbon compounds such as hexane, heptane and isoparaffin, ketone compounds such as acetone, methyl ethyl ketone and methyl isobutyl ketone, ester compounds such as ethyl acetate and butyl acetate, and ether compounds such as diisopropyl ether and 1,4-dioxane, but any compound that can dissolve silicone will do. It is also possible to use the solvent by dispersing and diluting it in water at any ratio.
[0100] When component (E) is blended, the blending amount is preferably 100 to 20,000 parts by mass, and particularly preferably 200 to 10,000 parts by mass, per 100 parts by mass of component (A). By blending component (E) in an amount of 100 to 20,000 parts by mass, the above-mentioned benefits of dilution can be fully obtained.
[0101] [(F) Release Force Controlling Component] The composition of the present invention can further contain a release force controlling component (F). The component (F) can be the following component (F1) and / or the following component (F2), and the blending amount can be 0.1 to 20 parts by mass per 100 parts by mass of component (A). By including the component (F) in this amount, it is possible to appropriately control the release force while maintaining adhesion to the substrate.
[0102] (F1): Release Force Control Component Containing Acrylic-Silicone Graft Copolymer Component (F1) is a release force control component containing an acrylic-silicone graft copolymer, and by incorporating this component, it is possible to obtain a very small release force and to provide an excellent cured coating (release coating) that exhibits a high residual adhesion rate on the released PSA sheet.
[0103] The acrylic-silicone graft copolymer used in the present invention is a copolymer having a weight average molecular weight of 1,000 to 100,000, obtained by radical polymerization of an organopolysiloxane compound (a) having an acrylic group and / or a methacrylic group (hereinafter also referred to as a (meth)acrylic group) with a radically polymerizable monomer (b) having one radically polymerizable group per molecule.
[0104] The weight-average molecular weight of the copolymer, as measured by gel permeation chromatography (hereinafter abbreviated as "GPC") using toluene as the developing solvent, is 1,000 to 100,000, preferably 1,500 to 50,000, and more preferably 2,000 to 30,000, in terms of polystyrene. A weight-average molecular weight of 1,000 to 100,000 allows for both a high residual adhesion rate and excellent dispersibility in the silicone composition.
[0105] [Component (a): Organopolysiloxane Compound Having a (Meth)acrylic Group] The organopolysiloxane compound (a) used in the present invention is not particularly limited as long as it has a (meth)acrylic group, but from the standpoints of ease of copolymerization with the radically polymerizable monomer (b) having one radically polymerizable group per molecule, ease of synthesis of the organopolysiloxane compound itself, and the effect of the release force controlling component, it is preferable that the organopolysiloxane compound (a) be a radically polymerizable silicone macromonomer represented by the following general formula (3):
[0106] In the above general formula (3), R 2 is a hydrogen atom or a methyl group, and X is a group (divalent functional group) selected from an oxygen atom, an NH group, and a sulfur atom.
[0107] Y is a divalent hydrocarbon group having 1 to 12 carbon atoms, preferably 1 to 10 carbon atoms, which may contain an oxygen atom therebetween, and specifically includes alkylene groups such as methylene, ethylene, propylene (trimethylene, methylethylene), butylene (tetramethylene, methylpropylene), hexamethylene, and octamethylene, arylene groups such as phenylene, combinations of two or more of these groups (e.g., alkylene-arylene groups), -CH 2 CH 2 -O-CH 2 CH 2 -, -CH 2 CH 2 -O-CH 2 CH 2 -O-CH 2 CH 2 -, -CH(CH 3 ) CH 2 -O-CH(CH 3 ) CH 2 -, -CH 2 CH 2 CH 2 CH 2 -O-CH 2 CH 2 CH 2 CH 2 -, etc. Y is preferably an ethylene group, a propylene group, or a butylene group. f is an integer of 0 to 1,000, preferably 0 to 500, and more preferably 0 to 200.
[0108] R 3 may be the same or different and are an unsubstituted or substituted monovalent hydrocarbon group having 1 to 20 carbon atoms, preferably 1 to 18 carbon atoms, a hydrogen atom, a hydroxyl group, an alkoxy group having 1 to 10 carbon atoms, preferably 1 to 8 carbon atoms, or a substituent represented by the following general formula (4): (In the formula, R 4 may be the same or different and are an unsubstituted or substituted monovalent hydrocarbon group having 1 to 20 carbon atoms, preferably 1 to 18 carbon atoms, a hydrogen atom, a hydroxyl group, or an alkoxy group having 1 to 10 carbon atoms, preferably 1 to 8 carbon atoms; and g is an integer from 0 to 300.
[0109] Here, R 3 , R 4Specific examples of the unsubstituted or substituted monovalent hydrocarbon group having 1 to 20 carbon atoms include alkyl groups such as methyl, ethyl, propyl, and butyl groups, cycloalkyl groups such as cyclohexyl groups, aryl groups such as phenyl and tolyl groups, aralkyl groups such as benzyl and phenethyl groups, and hydroxypropyl groups, cyanoethyl groups, 3-chloropropyl groups, and 3,3,3-trifluoropropyl groups in which some or all of the hydrogen atoms bonded to the carbon atoms of these groups have been substituted with hydroxy groups, cyano groups, halogen atoms, or the like. Specific examples of the alkoxy group having 1 to 10 carbon atoms include methoxy groups, ethoxy groups, propoxy groups, and butoxy groups. R 3 is preferably an alkyl group or an aryl group, more preferably an alkyl group having 1 to 5 carbon atoms. 4 is preferably an alkyl group or an aryl group, more preferably an alkyl group having 1 to 5 carbon atoms. g is an integer of 0 to 300, preferably 0 to 100, more preferably 0 to 50.
[0110] Specific examples of component (a) include, but are not limited to, the following: In the following formula, Me, OMe, and Ph represent a methyl group, a methoxy group, and a phenyl group, respectively.
[0111]
[0112]
[0113]
[0114] [Component (b): Radically Polymerizable Monomer] The radically polymerizable monomer (b) used in the present invention may be a single type or a mixture of two or more types, and is not particularly limited as long as it is a compound having one radically polymerizable group in one molecule.
[0115] Examples of component (b) include compounds having one radically polymerizable group per molecule, such as acrylic, methacrylic, styryl, cinnamic acid ester, vinyl, and allyl. Specific examples include (meth)acrylic acid ester compounds such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, trifluoropropyl (meth)acrylate, perfluorobutylethyl (meth)acrylate, and perfluorooctylethyl (meth)acrylate; epoxy group-containing radically polymerizable monomers such as glycidyl (meth)acrylate, β-methylglycidyl (meth)acrylate, and 3,4-epoxycyclohexylmethyl (meth)acrylate; 2-hydroxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, and 2-hydroxyethyl (meth)acrylate; Examples include hydroxyl group-containing radical polymerizable monomers such as dipropyl (meth)acrylate and 2-hydroxybutyl (meth)acrylate; radical polymerizable silane compounds such as γ-methacryloxypropyl trimethoxysilane, γ-methacryloxypropyl methyl dimethoxysilane, γ-methacryloxypropyl dimethyl methoxysilane, γ-methacryloxypropyl triethoxysilane, γ-methacryloxypropyl methyl diethoxysilane, γ-methacryloxypropyl tributoxysilane, γ-methacryloxypropyl triisopropenoxysilane, γ-acryloxypropyl trimethoxysilane, acryloxymethyl trimethoxysilane, γ-acryloxypropyl triethoxysilane, γ-acryloxypropyl methyl diethoxysilane, styryl trimethoxysilane, styryl triethoxysilane, and α-methylstyryl trimethoxysilane; polyoxyalkylene group-containing radical polymerizable monomers; and glycerol (meth)acrylate.
[0116] Considering the light release effect and high residual adhesion rate effect obtained by the (F) release force controlling component, it is preferable that the composition contains an alkyl(meth)acrylate having 1 to 30 carbon atoms, and more preferably methyl(meth)acrylate.
[0117] [Component (a) / Component (b) Ratio] The polymerization mass ratio [(a) / (b)] of the (meth)acrylic group-containing organopolysiloxane compound (a) to the radically polymerizable monomer (b) having one radically polymerizable group per molecule is preferably within the range of 30 / 70 to 99 / 1, more preferably 40 / 60 to 97 / 3, and even more preferably 50 / 50 to 95 / 5. When the polymerization mass ratio [(a) / (b)] is within the range of 30 / 70 to 99 / 1, sufficient compatibility with the silicone composition can be exhibited while maintaining a light release effect, thereby preventing separation of the release force controlling component (F).
[0118] [Method for Synthesizing Acrylic-Silicone Graft Copolymer] Copolymerization of a monomer raw material containing an organopolysiloxane compound (a) having a (meth)acrylic group and a radically polymerizable monomer (b) having one radically polymerizable group per molecule is carried out in the presence of a common radical polymerization initiator such as a peroxide such as benzoyl peroxide, dicumyl peroxide, lauroyl peroxide, or tert-butyl 2-ethylperoxyhexanoate, or an azo compound such as 2,2'-azobis(2-methylbutyronitrile), and any of solution polymerization, emulsion polymerization, suspension polymerization, and bulk polymerization can be used.
[0119] In the present invention, of these polymerization methods, solution polymerization is particularly preferred because it allows for easy adjustment of the molecular weight of the resulting acrylic-silicone graft copolymer to an optimum range. Solvents that can be used in this case include, but are not limited to, aromatic hydrocarbons such as benzene, toluene, and xylene; ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; esters such as ethyl acetate, n-butyl acetate, and isobutyl acetate; and alcohols such as ethanol, isopropanol, n-butanol, and isobutanol, either alone or in combination.
[0120] The polymerization temperature is preferably in the range of 50 to 180°C, and particularly preferably in the range of 60 to 120°C. Under these temperature conditions, the polymerization reaction can be completed in about 1 to 10 hours. There are no particular restrictions on the method for extracting the copolymer from the copolymer solution, but examples include a method of evaporating the solvent, and a method of adding a poor solvent such as water or methanol to the copolymer solution to precipitate the copolymer, followed by drying.
[0121] When component (F) is blended, the blending amount is preferably 0.1 to 20 parts by mass, and more preferably 0.1 to 15 parts by mass, per 100 parts by mass of component (A). When component (F) is blended in the above-mentioned preferred amount, both excellent light release effect and excellent curability can be achieved.
[0122] (F2): Linear Phenylmethylpolysiloxane The component (F2) is a phenylmethylpolysiloxane with a linear structure, and may have no functional groups or may have alkoxy groups and / or silanol groups at the terminals.
[0123] Component (F2) is preferably an organopolysiloxane having a viscosity of 0.01 to 70 Pa s when diluted with 30% by mass of toluene at 25° C. By including component (F2) having a viscosity within this range, both an excellent release force control effect and excellent productivity can be achieved.
[0124] [Other Optional Components] The silicone composition of the present invention can be obtained by blending the above-mentioned component (A), (B1) compound, (B2) compound, (B3) compound, component (C), and component (D) in predetermined amounts, but can also contain the above-mentioned optional components (E) and (F) in the preferred amounts, and can also add other components in any amounts as needed. Components known as those normally used in silicone-based release agent compositions can be added in the usual blending amounts.
[0125] Other optional components that can be used include, for example, various known pot life extenders, such as organic nitrogen compounds, organic phosphorus compounds, acetylenic compounds, oxime compounds, and organic chloro compounds. Examples include acetylenic alcohols such as 3-methyl-1-butyn-3-ol, 3,5-dimethyl-1-hexyn-3-ol, 3-methyl-1-penten-3-ol, and phenylbutynol, acetylenic compounds such as 3-methyl-3-1-penten-1-yne and 3,5-dimethyl-1-hexyn-3-yne, reaction products of these acetylenic compounds with alkoxysilanes, siloxanes, or hydrogensilanes, vinylsiloxanes such as tetramethylvinylsiloxane cyclics, organic nitrogen compounds such as benzotriazole, and other organic phosphorus compounds, oxime compounds, and organic chromium compounds.
[0126] When these compounds are blended, the blending amount may be any amount that provides a good pot life, and generally, the blending amount is preferably 0.01 to 10 parts by mass, and more preferably 0.05 to 5 parts by mass, per 100 parts by mass of component (A).
[0127] When the composition of the present invention is made into an emulsion composition, a surfactant and a high-molecular-weight emulsifier can be blended therein. A suitable blending amount is in the range of 0.1 to 10 parts by mass per 100 parts by mass of component (A).
[0128] Furthermore, if necessary, other optional components such as known antioxidants, pigments, stabilizers, antistatic agents, defoamers, adhesion improvers other than component (B), thickeners, and inorganic fillers such as silica may be blended.
[0129] In terms of pot life, the silicone composition for release sheets is preferably prepared by mixing the above-mentioned component (A), compound (B1), compound (B2), compound (B3), component (C), and any optional components uniformly in advance, and then adding component (D) immediately before use.
[0130] Another preparation method is to uniformly mix component (A), component (C), and any optional components in advance, and then add component (B) (compound (B1), compound (B2), and compound (B3)), which are adhesion improving components, and component (D) just before use. This method is advantageous for optimizing the release properties of the cured product.
[0131] Furthermore, a method of separately adding the (B1), (B2), and (B3) compounds is also preferably used. Since the (B1), (B2), and (B3) compounds exhibit their adhesion-improving effects under different conditions, it is desirable to adjust the amounts of the (B1), (B2), and (B3) compounds added to be optimal depending on the use conditions of the composition, from the standpoints of adhesion, release properties, and cost. When used as an additive as described above, the (B1), (B2), and / or (B3) compounds can also be used as an additive composition in which they are mixed with other components.
[0132] [Release Sheet (Coated Product)] The release sheet of the present invention is obtained by applying the silicone composition for release sheets of the present invention to a paper substrate or a film substrate and curing the composition.
[0133] The release sheet of the present invention can comprise, for example, a sheet-like substrate such as a paper substrate or a film substrate, and a cured product (cured coating) of the silicone composition for release sheets of the present invention formed on the substrate.
[0134] The silicone composition for release sheets of the present invention described above can be applied as is, or after further diluting with the dilution solvent or water within the ranges described above, to one or both sides of a sheet-like substrate such as paper or film using a coating method such as coating with a comma coater, lip coater, roll coater, die coater, knife coater, blade coater, rod coater, kiss coater, gravure coater, or wire bar coater, or by screen coating, dip coating, or cast coating. 2 After application, a cured coating can be formed on the substrate by heating at 50 to 200° C. for 1 to 120 seconds. When forming cured coatings (release layers) on both sides of the substrate, it is preferable to perform the cured coating formation operation on each side of the substrate at a time.
[0135] Examples of the substrate include polyethylene-laminated paper, glassine paper, fine paper, kraft paper, various coated papers such as clay-coated paper, synthetic paper such as Yupo, polyethylene film, polypropylene films such as CPP and OPP, polyester films such as polyethylene terephthalate film (PET film), polyamide film, polyimide film, polylactic acid film, polyphenol film, polycarbonate film, etc. In order to improve the adhesion between these substrates and the cured coating (release layer), the substrate surface may be corona-treated, etched, or plasma-treated.
[0136] The present invention will be specifically explained below with reference to Synthesis Examples, Examples, and Comparative Examples, but the present invention is not limited to the following Examples. In the following Examples, parts refer to parts by mass. Viscosity was measured using a TVB-10M rotational viscometer manufactured by Toki Sangyo Co., Ltd.
[0137] Preparation of Silicone Composition and Release Film (Release Sheet) <Raw Materials Used> Component (A) (A-1) (CH 3 ) 2 (CH 2 =CH)SiO 1/2 0.2 mol% of dimethylvinylsiloxane units represented by (CH 3 ) 2 SiO 2/2 Viscosity at 25°C of 100 Pa·s Viscosity when diluted with 30% by mass of toluene of 0.10 Pa·s Alkenyl group content = 0.003 mol / 100g
[0138] (A-2) (CH 3 ) 2 (CH 2 =CH)SiO 1/2 0.03 mol % of dimethylvinylsiloxane units represented by (CH 3 ) (CH 2 =CH)SiO 2/2 0.12 mol % of methylvinylsiloxane units represented by (C 6 H 5 )2 SiO 2/2 1.5 mol % of diphenylsiloxane units represented by (CH 3 ) 2 SiO 2/2 An organopolysiloxane having an average of 10 alkenyl groups per molecule, and composed of 98.35 mol% of dimethylsiloxane units represented by the formula: Viscosity at 25°C in 30% by mass toluene solution is 10 Pa·s Alkenyl group content = 0.002 mol / 100g
[0139] Component (B) Compound (B1-1) Epoxy group-containing siloxane oligomer obtained by partial hydrolysis and condensation of 166.7 parts by mass (0.7 mol) of tetraethoxysilane, 47.3 parts by mass (0.2 mol) of 3-glycidoxypropyltrimethoxysilane, 17.8 parts by mass (0.1 mol) of methyltriethoxysilane, and 15 parts by mass (0.83 mol) of water in the presence of hydrochloric acid at 80°C for 5 hours. Viscosity at 25°C: 0.02 Pa·s Average degree of polymerization: 5 20 mol% of siloxane units having an epoxy group bonded to a silicon atom via a carbon atom Silanol group content: 0.015 mol / 100g, silanol amount measured by the Grignard method in which the amount of methane generated is quantified using methylmagnesium iodide Alkoxy group content: 1.4 mol / 100g
[0140] (B1-2) Compound: An epoxy group-containing siloxane oligomer obtained by partial hydrolysis and condensation of 118.2 parts by mass (0.5 mol) of 3-glycidoxypropyltrimethoxysilane, 68.1 parts by mass (0.5 mol) of methyltrimethoxysilane, and 15 parts by mass (0.83 mol) of water in the presence of hydrochloric acid at 70°C for 5 hours. Viscosity at 25°C: 0.05 Pa s Average degree of polymerization: 50 mol% of siloxane units having an epoxy group bonded to a silicon atom via a carbon atom Silanol group content: 0.012 mol / 100 g Alkoxy group content: 0.9 mol / 100 g
[0141] (b1-3) Compound: An epoxy group-containing siloxane oligomer obtained by partial hydrolysis and condensation of 236.3 parts by mass (1 mole) of 3-glycidoxypropyltrimethoxysilane and 9 parts by mass (0.5 mole) of water in the presence of hydrochloric acid at 70°C for 5 hours. Viscosity at 25°C: 0.005 Pa s Average degree of polymerization: 2 100 mol% siloxane units having an epoxy group bonded to a silicon atom via a carbon atom Silanol group content: 0.015 moles / 100 g Alkoxy group content: 0.9 moles / 100 g
[0142] (b1-4) Compound: An organopolysiloxane represented by the following formula, which has 2-(3,4-epoxycyclohexyl)ethyl groups but contains substantially no silanol groups or alkoxy groups. (w1=42, w2=33, Ep 1 represents a 2-(3,4-epoxycyclohexyl)ethyl group, and Me represents a methyl group. Average degree of polymerization: 77. 43 mol% of siloxane units have an epoxy group bonded to a silicon atom via a carbon atom. Silanol group content: 0 mol / 100 g. Alkoxy group content: 0 mol / 100 g.
[0143] (b1-5) Compound: An organopolysiloxane represented by the following formula, which contains 2-(3,4-epoxycyclohexyl)ethyl groups but contains substantially no silanol groups or alkoxy groups: (w=20, Ep 1 represents a 2-(3,4-epoxycyclohexyl)ethyl group, and Me represents a methyl group. Average degree of polymerization: 22. Siloxane units having an epoxy group bonded to a silicon atom via a carbon atom: 9 mol%. Silanol group content: 0 mol / 100 g. Alkoxy group content: 0 mol / 100 g.
[0144] (B2-1) Compound (CH 3 ) 3 SiO 1/2 1.67 mol % of trimethylsiloxane units represented by (CH 3 ) HSiO 2/2 90.00 mol% of methylhydrogensiloxane units represented by (C 6 H 5 ) 2 SiO 2/2and 8.33 mol% of diphenylsiloxane units represented by the formula: Viscosity at 25°C: 0.15 Pa·s Average number of SiH groups per molecule: 108 Si—H group content: 1.25 mol / 100 g Phenyl group content: 8 mol% Average degree of polymerization: 120
[0145] (B2-2) Compound (CH 3 ) 3 SiO 1/2 2.86 mol % of trimethylsiloxane units represented by (CH 3 ) HSiO 2/2 80.00 mol% of methylhydrogensiloxane units represented by (C 6 H 5 ) 2 SiO 2/2 and 17.14 mol% of diphenylsiloxane units represented by the formula: Viscosity at 25°C: 0.1 Pa·s Average number of SiH groups per molecule: 56 Si—H group content: 0.95 mol / 100 g Phenyl group content: 17 mol% Average degree of polymerization: 70
[0146] (b2-3) Compound (CH 3 ) 3 SiO 1/2 4 mol % of trimethylsiloxane units represented by (CH 3 ) HSiO 2/2 Viscosity at 25°C: 0.02 Pa·s Average number of SiH groups per molecule: 48 Si—H group content: 1.5 mol / 100 g Phenyl group content: 0 mol % Average degree of polymerization: 50
[0147] (B3-1) Compound (CH 3 ) 2 (CH 2 =CH)SiO 1/2 48 mol % of dimethylvinylsiloxane units represented by (CH 3 ) SiO 3/2 49 mol % of methylsiloxane units represented by (CH 3 ) (CH3 O) SiO 2/2 An organosiloxane composed of 3 mol% of methylmethoxysiloxane units represented by the formula: Viscosity at 25°C: 0.03 Pa·s Alkenyl group content: 0.5 mol / 100 g
[0148] (B3-2) Compound (CH 3 ) 3 SiO 1/2 22 mol % of trimethylsiloxane units represented by (CH 3 ) 2 (CH 2 =CH)SiO 1/2 27 mol% of dimethylvinylsiloxane units represented by (CH 3 ) SiO 3/2 49 mol % of methylsiloxane units represented by (CH 3 ) (CH 3 O) SiO 2/2 An organosiloxane composed of 2 mol% of methylmethoxysiloxane units represented by the formula: Viscosity at 25°C: 0.03 Pa·s Alkenyl group content: 0.35 mol / 100 g
[0149] (C) Component (C-1) (CH 3 ) 3 SiO 1/2 4 mol % of trimethylsiloxane units represented by (CH 3 ) HSiO 2/2 Viscosity at 25°C: 0.02 Pa·s Average number of SiH groups per molecule: 48 Si—H group content: 1.5 mol / 100 g Average degree of polymerization: 50
[0150] Component (D) (D-1) Platinum-vinylsiloxane complex as a catalyst
[0151] Component (E) (E-1) A mixed solvent of toluene and hexane in a mass ratio of 1:1
[0152] (Component G) (G-1) Pot life extender: 3-methyl-1-butyn-3-ol (G-2) Pot life extender: 1-ethynylcyclohexanol
[0153] Examples 1 to 12, Comparative Examples 1 to 11 Using the above-described components (A) to (E) and (G) as raw materials, coating compositions were prepared according to the following procedure. Components (A), (B), (C), (E), and (G) were placed in a flask according to the blending ratios shown in Tables 1 to 6 and dissolved by stirring. Component (D) was added to the resulting solution so that the platinum content was 30 ppm relative to component (A), and the mixture was stirred and mixed to obtain a coating composition.
[0154] The obtained composition was applied to a 38 μm-thick PET film using an applicator to a solids thickness of 30 μm, and heated for 60 seconds in a hot air dryer at 130° C. to form a release agent layer (cured film), and the obtained release film (coated product) was used for evaluation. For evaluation of curability and adhesion, the release film immediately after heating was used, and for evaluation of release force and residual adhesion rate, the release film aged at 25° C. for 24 hours was used.
[0155] <Evaluation> [Curability (adhesion immediately after curing)] The release agent layer of the obtained release film was rubbed with a finger 10 times, and then the presence or absence of clouding and peeling was visually observed and evaluated according to the following criteria. A: No clouding or peeling was observed. B: Clouding was observed. C: Peeling was observed. The results are shown in Tables 1 to 6 below.
[0156] [Adhesion] The obtained release film was left to stand under certain conditions, and then the release agent layer was rubbed with a finger 10 times, and then the presence or absence of clouding and peeling was visually observed and evaluated according to the following criteria. A: No clouding or peeling was observed. B: Clouding was observed but no peeling was observed. C: Peeling was observed. The pressure-sensitive adhesive article was left to stand under three conditions: 25°C, 50% RH for one week, or 60°C, 90% RH for one day and one week. The results are shown in Tables 1 to 6 below.
[0157] [Peel Force] After aging, a solvent-based acrylic adhesive BPS-5127 (manufactured by Toyo Ink Co., Ltd.) was applied to the cured coating surface of the release film and then dried for 180 seconds in a dryer at 100°C. After drying, the film was left at room temperature for at least 10 minutes, and then a PET film was laminated and cut into pieces measuring 5.0 cm x 18 cm. A load was applied to the cut pieces by rolling a 2 kg roller back and forth once. After aging the cut pieces at room temperature for 3 hours, one end was peeled off, and the edge of the adhesive-coated PET film was pulled at an angle of 180 degrees to the release film at a peel rate of 0.3 m / min. The force required to peel ("peel force", N / 50 mm) was measured using a tensile tester (DSC-500 model, manufactured by Shimadzu Corporation). The results are shown in Tables 1 to 6 below.
[0158] [Residual Adhesion Rate] After aging, a 25 mm wide adhesive tape (Tesa 7475 tape, product name, manufactured by Tesa Tape, Inc.) was attached to the cured film surface side of the release film, and the tape was dried in a dryer at 70°C at 20 g / cm 2 After air-cooling for about 30 minutes, the tesa7475 tape was peeled from the release film and attached to a SUS stainless steel plate, and then pressed back and forth with a 2 kg tape roller once and left at 25°C for 30 minutes.The tesa7475 tape was then pulled at an angle of 180° and at a peeling rate of 0.3 m / min using a tensile tester, and the force (N / 25 mm) required to peel the tesa7475 tape from the SUS stainless steel plate, or adhesive strength F, was measured.
[0159] In addition, unused tesa 7475 tape was attached to a SUS stainless steel plate and treated in the same manner. 0 Then, (adhesive strength F / adhesive strength F 0 ) × 100 (%). The higher the residual adhesion rate, the smaller the effect on the adhesive surface of the adhesive tape due to contact with the release agent layer, and the more capable the release agent layer is of suppressing a decrease in the adhesive strength of the adhesive tape after peeling, and the better the release agent layer can be evaluated to be. The results are shown in Tables 1 to 6 below.
[0160] Note: Values without units are parts by mass. H / V molar ratio 1 is the value obtained by dividing the number of moles of SiH groups in C by the total number of moles of vinyl groups in A + B3, and is 0.5 to 15. H / V molar ratio 2 is the value obtained by dividing the number of moles of SiH groups in B2 by the number of moles of vinyl groups in B3. Adhesion 1 is the evaluation result after one week at 25°C and 50% RH. Adhesion 2 is the evaluation result after one day at 60°C and 90% RH. Adhesion 3 is the evaluation result after one week at 60°C and 90% RH.
[0161] Note: Values without units are parts by mass. H / V molar ratio 1 is the value obtained by dividing the number of moles of SiH groups in C by the total number of moles of vinyl groups in A + B3, and is 0.5 to 15. H / V molar ratio 2 is the value obtained by dividing the number of moles of SiH groups in B2 by the number of moles of vinyl groups in B3. Adhesion 1 is the evaluation result after one week at 25°C and 50% RH. Adhesion 2 is the evaluation result after one day at 60°C and 90% RH. Adhesion 3 is the evaluation result after one week at 60°C and 90% RH.
[0162] Note: Values without units are parts by mass. H / V molar ratio 1 is the value obtained by dividing the number of moles of SiH groups in C by the total number of moles of vinyl groups in A + B3, and is 0.5 to 15. H / V molar ratio 2 is the value obtained by dividing the number of moles of SiH groups in B2 by the number of moles of vinyl groups in B3. Adhesion 1 is the evaluation result after one week at 25°C and 50% RH. Adhesion 2 is the evaluation result after one day at 60°C and 90% RH. Adhesion 3 is the evaluation result after one week at 60°C and 90% RH.
[0163] Note: Values without units are parts by mass. H / V molar ratio 1 is the value obtained by dividing the number of moles of SiH groups in C by the total number of moles of vinyl groups in A + B3, and is 0.5 to 15. H / V molar ratio 2 is the value obtained by dividing the number of moles of SiH groups in B2 by the number of moles of vinyl groups in B3. Adhesion 1 is the evaluation result after one week at 25°C and 50% RH. Adhesion 2 is the evaluation result after one day at 60°C and 90% RH. Adhesion 3 is the evaluation result after one week at 60°C and 90% RH.
[0164] Note: Values without units are parts by mass. H / V molar ratio 1 is the value obtained by dividing the number of moles of SiH groups in C by the total number of moles of vinyl groups in A + B3, and is 0.5 to 15. H / V molar ratio 2 is the value obtained by dividing the number of moles of SiH groups in B2 by the number of moles of vinyl groups in B3. Adhesion 1 is the evaluation result after one week at 25°C and 50% RH. Adhesion 2 is the evaluation result after one day at 60°C and 90% RH. Adhesion 3 is the evaluation result after one week at 60°C and 90% RH.
[0165] Note: Values without units are parts by mass. H / V molar ratio 1 is the value obtained by dividing the number of moles of SiH groups in C by the total number of moles of vinyl groups in A + B3, and is 0.5 to 15. H / V molar ratio 2 is the value obtained by dividing the number of moles of SiH groups in B2 by the number of moles of vinyl groups in B3. Adhesion 1 is the evaluation result after one week at 25°C and 50% RH. Adhesion 2 is the evaluation result after one day at 60°C and 90% RH. Adhesion 3 is the evaluation result after one week at 60°C and 90% RH.
[0166] Tables 1 to 3 above show the results of Examples 1 to 12 of the present invention, and Tables 4 to 6 show the results of Comparative Examples 1 to 11. The results in Tables 1 to 3 show that the compositions of Examples 1 to 12 of the present invention were excellent in curability and exhibited excellent adhesion to substrates, and in many of the examples, release agent layers (cured films) were formed that were able to maintain this excellent adhesion for long periods of time even under severe environments such as high temperatures and high humidity. The results also show that the incorporation of an adhesion improver did not increase the release force, indicating that a release agent layer was provided that did not significantly impair the adhesive properties of the pressure-sensitive adhesive tape.
[0167] On the other hand, the compositions of Comparative Examples 1 and 11 did not contain the component (B). The composition of Comparative Example 2 did not contain the compound (B1). The composition of Comparative Example 4 did not contain the compound (B2). The composition of Comparative Example 6 did not contain the compound (B3). As a result, the release agent layers obtained from the compositions of Comparative Examples 1, 2, 4, 6, and 11 were unable to maintain adhesion to the substrate for an extended period of time under the harsh environment of 60°C and 90% RH. These results demonstrate that in order to maintain adhesion to the substrate for an extended period of time under the harsh environment of 60°C and 90% RH, all of the compounds (B1), (B2), and (B3) must be blended.
[0168] Comparative Example 3 was a composition in which the amount of the (B1) compound was too much, Comparative Example 5 was a composition in which the amount of the (B2) compound was too much, and Comparative Example 7 was a composition in which the amount of the (B3) compound was too much. As a result, the release agent layers obtained from the compositions of Comparative Examples 3 and 5 had a heavy release force, and the composition of Comparative Example 7 had reduced curability.
[0169] Examples 11 and 12 are compositions in which the blending ratios of compound (B2) and compound (B3) in Examples 1 and 2 were changed, and the value obtained by dividing the number of moles of SiH groups in compound (B2) by the number of moles of vinyl groups in compound (B3) was 1.5, which was smaller than the 3.8 in Examples 1 and 2. As a result, the release agent layers obtained from the compositions of Examples 11 and 12 were able to maintain adhesion to substrates for long periods of time under the harsh environment of 60°C and 90% RH, but were slightly inferior to the release agent layers obtained from the compositions of Examples 1 and 2.
[0170] The compound (b1-3) used in Comparative Example 8 had an average degree of polymerization of 2. As a result, the release agent layer obtained from the composition of Comparative Example 8 was unable to maintain adhesion to the substrate for a long period of time under severe conditions.
[0171] The (b1-4) compound used in Comparative Example 9 and the (b1-5) compound used in Comparative Example 10 were organosiloxanes composed only of monofunctional siloxane units and difunctional siloxane units, and differed from the (B1-1) and (B1-2) compounds, which were organosiloxanes composed of trifunctional siloxane units and tetrafunctional siloxane units, and did not contain silanol groups or alkoxy groups. As a result, the release agent layers obtained from the compositions of Comparative Examples 9 and 10 were unable to maintain adhesion to the substrate for a long period of time under the harsh environment of 60°C and 90% RH. Furthermore, the (B1-2) compound used in Example 8 differed from the (B1-1) compound in that it was composed only of trifunctional siloxane units and did not contain tetrafunctional siloxane units. As a result, the release agent layer obtained from the composition of Example 8 was able to maintain adhesion to the substrate for a long period of time even under the harsh environment of 60°C and 90% RH, but was slightly inferior to the release agent layer obtained from the composition of Example 7.
[0172] This specification includes the following aspects: [1]: An addition-curable silicone composition for release sheets, comprising: (A) 100 parts by mass of an organopolysiloxane having at least two alkenyl groups per molecule, the alkenyl group content being 0.001 to 0.2 mol / 100 g, and having a 30% by mass toluene dilution viscosity at 25°C of 0.001 to 70 Pa·s; (B) a component including the following compounds (B1), (B2), and (B3): (B1) 0.1 to 8 parts by mass of an organopolysiloxane containing per molecule 10 mol % or more siloxane units having a glycidyl group and / or glycidoxy group bonded to a silicon atom via a carbon atom, containing 0.002 to 0.02 mol / 100 g of silanol groups, and containing 0.5 to 2.5 mol / 100 g of alkoxy groups, and having an average degree of polymerization of 3 to 50; (B2) an organohydrogensiloxane having at least three silicon-bonded hydrogen atoms per molecule, an average degree of polymerization of 10 to 200, and 5 to 20 mol % of the substituents being aryl groups: 0.05 to 2.0 parts by mass; (B3) an organopolysiloxane having an alkenyl group content of 0.3 mol / 100 g or more and a viscosity at 25°C of 0.01 to 1 Pa s: 0.05 to 3.0 parts by mass; (C) an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms per molecule, other than the (B2) compound: the number of moles of silicon-bonded hydrogen atoms in component (C) corresponds to 0.5 to 15 times the number of moles of alkenyl groups in the composition; (D) a platinum group metal catalyst: a catalytic amount; (E) an organic solvent: 0 to 20,000 parts by mass; [2]: The addition-curable silicone composition for release sheets, characterized in that the compound (B3) is a compound represented by the general formula (I) above. 9 (3-g1) R 8 g1 SiO 1 / 2 Siloxane units (M R8R9 Units), R 9 SiO 3 / 2 Siloxane units (T R9 units) (wherein R 8 are independently an alkenyl group, and R 9are independently unsubstituted or halogen atom- or cyano group-substituted monovalent hydrocarbon groups that do not contain aliphatic unsaturated bonds, and g1 is a number from 0 to 3. R8R9 Unit / T R9 The molar ratio of the units is 2 / 8 to 8 / 2, and the molecular end is M R8R9 The silicone composition for release sheets according to the above [1], characterized in that the (B1) compound is an organopolysiloxane which is a partial hydrolysis condensate of an organoalkoxysilane represented by the following general formula (1-1) and at least one of organoalkoxysilanes represented by the following general formulas (1-2), (1-3), and (1-4), or a mixture thereof. (wherein R1 may be the same or different and represent an unsubstituted or substituted hydrocarbon group of 1 to 10 carbon atoms which does not have an aliphatic unsaturated bond and which may contain an oxygen atom, or a hydrogen atom; R12 represents an unsubstituted or substituted hydrocarbon group of 1 to 20 carbon atoms; and n is an integer from 3 to 10.) [4]: The silicone composition for release sheets according to [3] above, characterized in that the (B1) compound is a partial hydrolysis condensate of an organoalkoxysilane mixture which contains organoalkoxysilanes represented by the above general formulas (1-1) and (1-4) as essential components and organoalkoxysilanes represented by the above general formulas (1-2) and (1-3) as optional components, and is an organopolysiloxane having a linear, branched or cyclic siloxane structure, or a mixture thereof. [5]: The silicone composition for release sheets according to any one of [1] to [4] above, wherein the compound (B2) is an organohydrogensiloxane represented by the following general formula (2-1) or (2-2), or a mixture thereof: (R12) 3 SiO-{(R12)HSiO} m {(R12) 2 SiO} n -Si(R12) 3 ...(2-1) (R12) 2HSiO-{(R12)HSiO} m {(R12) 2 SiO} n -SiH(R12) 2 ...(2-2) (wherein R12 may be the same or different and are unsubstituted or substituted hydrocarbon groups having 1 to 20 carbon atoms, and aryl groups account for 5 to 20 mol% of the total number of substituents, calculated by adding together the H groups directly bonded to Si and R12, and m + n is an integer from 2 to 198.) [6]: A silicone composition for release sheets according to any one of [1] to [5] above, characterized in that the (B2) compound and the (B3) compound are blended in such a manner that the number of moles of hydrogen atoms bonded to silicon atoms in the (B2) compound divided by the number of moles of alkenyl groups in the (B3) compound is 1.6 or more parts by mass. [7]: A release sheet obtained by coating a paper substrate or a film substrate with the silicone composition for release sheets according to any one of [1] to [6] above, followed by curing.
[0173] The present invention is not limited to the above-described embodiments, which are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and that provides similar effects is included within the technical scope of the present invention.
Claims
1. An addition-curing silicone composition for release sheets, comprising: (A) 100 parts by mass of an organopolysiloxane having at least two alkenyl groups in one molecule, the alkenyl group content being 0.001 to 0.2 mol / 100 g, and having a 30% by mass toluene dilution viscosity at 25°C of 0.001 to 70 Pa·s; (B) a component including the following compounds (B1), (B2), and (B3): (B1) 0.1 to 8 parts by mass of an organopolysiloxane containing in one molecule at least 10 mol % of siloxane units having a glycidyl group and / or glycidoxy group bonded to a silicon atom via a carbon atom, containing 0.002 to 0.02 mol / 100 g of silanol groups, and containing 0.5 to 2.5 mol / 100 g of alkoxy groups, and having an average degree of polymerization of 3 to 50; (B2) an organohydrogensiloxane having at least three hydrogen atoms bonded to silicon atoms per molecule, an average degree of polymerization of 10 to 200, and in which 5 to 20 mol % of the substituents are aryl groups: 0.05 to 2.0 parts by mass; (B3) an organopolysiloxane having an alkenyl group content of 0.3 mol / 100 g or more and a viscosity at 25° C. of 0.01 to 1 Pa·s: 0.05 to 3.0 parts by mass; (C) an organohydrogenpolysiloxane other than the compound (B2) having at least two hydrogen atoms bonded to silicon atoms per molecule: the number of moles of hydrogen atoms bonded to silicon atoms in component (C) corresponds to 0.5 to 15 times the number of moles of alkenyl groups in the composition; (D) a platinum group metal catalyst: a catalytic amount; (E) an organic solvent: 0 to 20,000 parts by mass; 1. An addition-curable silicone composition for release sheets, comprising:
2. The compound (B3) is R 9 (3-g1) R 8 g1 SiO 1 / 2 Siloxane unit (M R8R9 Units), R 9 SiO 3 / 2 Siloxane unit (T R9 Units) (wherein R 8 are independently an alkenyl group; R 9 are independently an unsubstituted or halogen- or cyano-substituted monovalent hydrocarbon group that does not contain an aliphatic unsaturated bond, and g1 is a number from 0 to 3. R8R9 Unit / T R9 The molar ratio of the units is 2 / 8 to 8 / 2, and the molecular end is M R8R9 2. The silicone composition for use in a release sheet according to claim 1, which is an organopolysiloxane in which the monomer units are either aryl groups or aryl groups, or a portion of the monomer units are terminated as silanol groups or alkoxy groups.
3. The silicone composition for release sheets according to claim 1, characterized in that the compound (B1) is an organopolysiloxane which is a partial hydrolysis condensation product of an organoalkoxysilane represented by the following general formula (1-1) and at least one of organoalkoxysilanes represented by the following general formulas (1-2), (1-3), and (1-4), or a mixture thereof. (In the formula, R1 may be the same or different and is a hydrogen atom or an unsubstituted or substituted hydrocarbon group having 1 to 10 carbon atoms and no aliphatic unsaturated bond, which may contain an oxygen atom; R12 is an unsubstituted or substituted hydrocarbon group having 1 to 20 carbon atoms; and n is an integer from 3 to 10.) 4. The silicone composition for release sheets according to claim 3, characterized in that the (B1) compound is a partial hydrolysis condensate of an organoalkoxysilane mixture containing organoalkoxysilanes represented by the above general formulas (1-1) and (1-4) as essential components and organoalkoxysilanes represented by the above general formulas (1-2) and (1-3) as optional components, and is an organopolysiloxane having a linear, branched or cyclic siloxane structure, or a mixture thereof.
5. The silicone composition for release sheets according to claim 1, wherein the compound (B2) is an organohydrogensiloxane represented by the following general formula (2-1) or (2-2), or a mixture thereof: (R12) 3 SiO-{(R12)HSiO} m {(R12) 2 SiO} n -Si(R12) 3 ...(2-1) (R12) 2 HSiO-{(R12)HSiO} m {(R12) 2 SiO} n -SiH(R12) 2 (In the formula, R12 may be the same or different and is an unsubstituted or substituted hydrocarbon group having 1 to 20 carbon atoms, 5 to 20 mol % of the total number of substituents, which is the sum of H groups directly bonded to Si and R12, are aryl groups, and m+n is an integer of 2 to 198.) 6. The silicone composition for release sheets according to claim 1, characterized in that the (B2) compound and the (B3) compound are blended in such a way that the number of moles of hydrogen atoms bonded to silicon atoms in the (B2) compound divided by the number of moles of alkenyl groups in the (B3) compound is 1.6 or more parts by mass.
7. A release sheet obtained by applying the silicone composition for release sheets according to any one of claims 1 to 6 to a paper or film substrate and curing the composition.
Citation Information
Patent Citations
Silicone composition for release film
JP2007009072A
silicone release coating composition
JP2008520804A
Silicone composition for release film
JP2011236289A
Crosslinkable silicone composition for producing a non-stick coating for a flexible substrate and an adhesion promoting additive contained in this composition
JP2018538372A
Heavy release additive for release sheet, organopolysiloxane composition for release sheet, and release sheet
WO2016060084A1
Cited By
Composition set for use in thermally conductive silicone compositions
JP2026138390A