Film for latex inks

The film for latex ink, with a latex ink receiving layer containing an active energy ray-curable compound and a polymeric dispersant, addresses the challenge of achieving both substrate and ink adhesion, resulting in enhanced printing performance.

WO2024247170A1PCT designated stage expired Publication Date: 2024-12-05LINTEC CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/020305
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing latex ink films struggle to achieve both excellent substrate adhesion and ink adhesion, with a latex ink receiving layer formed from active energy ray-curable compounds often showing good substrate adhesion but poor ink adhesion.

Method used

A film with a laminated structure featuring a latex ink receiving layer composed of an active energy ray-curable compound and a polymeric dispersant with acidic or basic functional groups, which enhances both substrate and ink adhesion.

Benefits of technology

The film achieves improved ink adhesion while maintaining strong substrate adhesion, making it suitable for printing applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023020305_05122024_PF_FP_ABST
    Figure JP2023020305_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a film for latex inks which includes a latex-ink-receiving layer formed from an actinic-ray-curable compound and having excellent adhesion to the substrate and excellent ink adhesion thereto. The problem is solved with a film having a laminate structure comprising a latex-ink-receiving layer (X) and a substrate (Y) laminated on each other, the latex-ink-receiving layer (X) being formed from a composition (x1) comprising an actinic-ray-curable compound (A) and a specific dispersant (B).
Need to check novelty before this filing date? Find Prior Art

Description

Latex ink film

[0001] The present invention relates to a film for latex inks.

[0002] In recent years, printing methods using latex ink have been attracting attention (see, for example, Patent Document 1). Unlike solvent inks in which a pigment is dissolved in an organic solvent, latex inks are aqueous inks in which a pigment is dispersed in water together with latex (a polymer). Therefore, there is no emission of volatile organic compounds (VOCs) resulting from organic solvents, which is a problem when using solvent inks. Therefore, printed materials using latex inks have the advantage that they can be used safely in a variety of locations, such as restaurants, educational institutions, medical institutions, and commercial facilities.

[0003] Taking these advantages into consideration, the present applicant has proposed a film for latex ink in Patent Document 2. The film for latex ink described in Patent Document 2 includes a substrate and a printing coating layer to which latex ink is applied. The printing coating layer contains a material having a structure in which a polymeric material whose constituent monomers are vinyl chloride, vinyl acetate, and a crosslinkable monomer is crosslinked with a crosslinking agent. This results in a film for latex ink having a printing coating layer that has excellent adhesion to both the portion printed with latex ink and the substrate.

[0004] The "printing coating layer" in Patent Document 2 is referred to as the "latex ink-receiving layer" in this specification. That is, the "latex ink-receiving layer" refers to a layer to which latex ink is applied and which has the function of fixing the printed portion of the applied latex ink.

[0005] JP 2016-120719 A JP 2019-172877 A

[0006] In recent years, printing methods using latex inks have been widely adopted, and various requirements are also increasing for films for latex inks used in such methods. Therefore, there is a need for the development of a film for latex inks having a latex ink-receiving layer different from that described in Patent Document 2. Specifically, there is a need for the development of a film for latex inks having a latex ink-receiving layer formed using an actinic ray-curable compound.

[0007] Here, in a film for latex ink having a latex ink-receiving layer, it is required to ensure good adhesion between the latex ink-receiving layer and the substrate (hereinafter simply referred to as "substrate adhesion"), while also ensuring good adhesion between the latex ink-receiving layer and the area printed with latex ink (hereinafter simply referred to as "ink adhesion").

[0008] An object of the present invention is to provide a film for latex inks, which is formed from an active energy ray-curable compound and has a latex ink-receiving layer that is excellent in both substrate adhesion and ink adhesion.

[0009] The present inventors conducted extensive research to solve the above-mentioned problems and discovered that a latex ink-receiving layer formed from a composition containing an active energy ray-curable compound and a polymeric dispersant having one or more functional groups selected from the group consisting of acidic functional groups and basic functional groups can solve the above-mentioned problems. Based on this discovery, the present inventors conducted further research and completed the present invention. Specifically, the present invention relates to the following items [1] to [8]. [1] A film for latex inks, having a laminate structure in which a latex ink-receiving layer (X) and a substrate (Y) are laminated, the latex ink-receiving layer (X) being formed from a composition (x1) containing an active energy ray-curable compound (A) and a polymeric dispersant (B) having one or more functional groups selected from the group consisting of acidic functional groups and basic functional groups. [2] The film for latex inks according to item [1] above, in which the substrate (Y) contains a polyester resin. [3] The latex ink film according to [1] or [2] above, wherein the latex ink-receiving layer (X) is laminated on one surface of the substrate (Y), and a pressure-sensitive adhesive layer (Z) is provided on the other surface of the substrate (Y). [4] The latex ink film according to [3] above, wherein the adhesive surface of the pressure-sensitive adhesive layer (Z) is covered with a release liner. [5] The latex ink film according to any one of [1] to [4] above, which is used for printing using a latex ink containing an acrylic resin. [6] A method of use, comprising using the latex ink film according to any one of [1] to [5] above to form a printed section on the latex ink-receiving layer of the latex ink film according to any one of [1] to [5] above using latex ink. [7] A method for producing a printed matter, comprising the step of forming a printed section on the latex ink-receiving layer of the latex ink film according to any one of [1] to [5] above using latex ink. [8] A printed matter having a printed area printed with latex ink on the latex ink-receiving layer of the film for latex ink according to any one of [1] to [5] above.

[0010] According to the present invention, it is possible to provide a film for latex ink, which is formed from an active energy ray-curable compound and has a latex ink-receiving layer that is excellent in both substrate adhesion and ink adhesion.

[0011] 1 is a cross-sectional view showing one embodiment of a film for latex ink of the present invention.

[0012] As used herein, the term "active ingredient" refers to the components contained in the target composition, excluding diluting solvents such as water and organic solvents. Furthermore, as used herein, "(meth)acrylate" refers to both "acrylate" and "methacrylate." Furthermore, as used herein, the lower and upper limits of preferred numerical ranges (e.g., ranges of content, etc.) described in stages can be independently combined. For example, the description "preferably 10 to 90, more preferably 30 to 60" can be combined with the "preferable lower limit (10)" and the "more preferred upper limit (60)" to yield "10 to 60." Furthermore, as used herein, the numerical values ​​in the examples are numerical values ​​that can be used as upper or lower limits.

[0013] [Embodiments of Film for Latex Ink of the Present Invention] The film for latex ink of the present invention has a laminate structure in which a latex ink-receiving layer (X) and a substrate (Y) are laminated together. The latex ink-receiving layer (X) is formed from a composition (x1) containing an active energy ray-curable compound (A) and a polymer dispersant (B) having one or more functional groups selected from the group consisting of acidic functional groups and basic functional groups.

[0014] The present inventors conducted extensive research to solve the above-mentioned problems. First, they investigated latex ink-receiving layers formed solely from an actinic ray-curable compound. As a result, they found that while the layer exhibited good substrate adhesion, it also exhibited poor ink adhesion, making it impossible to achieve both excellent substrate adhesion and excellent ink adhesion. Therefore, the present inventors conducted further extensive research and found that a latex ink-receiving layer formed from a composition in which an actinic ray-curable compound is blended with a polymeric dispersant having one or more functional groups selected from the group consisting of acidic functional groups and basic functional groups, exhibits excellent substrate adhesion and excellent ink adhesion. Specifically, they found that forming a latex ink-receiving layer from a composition in which an actinic ray-curable compound is blended with a polymeric dispersant having one or more functional groups selected from the group consisting of acidic functional groups and basic functional groups, while maintaining good substrate adhesion similar to that of a latex ink-receiving layer formed solely from an actinic ray-curable compound, dramatically improves ink adhesion, thereby achieving both excellent substrate adhesion and excellent ink adhesion. Based on the above findings, the present inventors have further conducted various studies and have completed the present invention.

[0015] In the following description, the "active energy ray-curable compound (A)" will also be referred to as "component (A)." Furthermore, the "polymer dispersant (B) having one or more functional groups selected from the group consisting of acidic functional groups and basic functional groups" will also be simply referred to as "polymer dispersant (B)" or "component (B)."

[0016] The latex ink film of the present invention will be described in detail below with respect to its configuration, the components constituting the latex ink film (substrate, latex ink-receiving layer, adhesive layer, and release liner), the method for producing the latex ink film, and uses of the latex ink film.

[0017] [Configuration of Film for Latex Ink] The film for latex ink of the present invention has a laminated structure in which a latex ink-receiving layer (X) and a substrate (Y) are laminated.

[0018] Figure 1 shows a schematic cross-sectional view of one embodiment of the latex ink film of the present invention. The latex ink film 1 shown in Figure 1 has a laminate structure in which a latex ink-receiving layer (X) is laminated on one surface (Ya) of a substrate (Y). Here, as shown in Figure 1, the latex ink film of one embodiment of the present invention preferably has a pressure-sensitive adhesive layer (Z) provided on the other surface (Yb) of the substrate (Y). This allows the latex ink film to be suitably used as a pressure-sensitive adhesive film.

[0019] Although not shown, the adhesive surface of the pressure-sensitive adhesive layer (Z) may be covered with a release liner. The release liner may be peeled off when the pressure-sensitive adhesive layer (Z) is attached to an adherend, thereby exposing the adhesive surface of the pressure-sensitive adhesive layer (Z). Although not shown, a latex ink-receiving layer (X) may be provided on both the one surface (Ya) and the other surface (Yb) of the substrate (Y) without providing the pressure-sensitive adhesive layer (Z). Although not shown, another layer may be provided between the latex ink-receiving layer (X) and the substrate (Y). Examples of such another layer include an easy-adhesion layer.

[0020] [Components Constituting the Latex Ink Film] The latex ink film of the present invention has a latex ink-receiving layer (X) and a substrate (Y). As described above, the latex ink film of one embodiment of the present invention may further have a pressure-sensitive adhesive layer (Z) in addition to the latex ink-receiving layer (X) and the substrate (Y). In addition to the latex ink-receiving layer (X) and the substrate (Y), it may further have a pressure-sensitive adhesive layer (Z) and a release liner. The latex ink-receiving layer (X), the substrate (Y), the pressure-sensitive adhesive layer (Z), and the release liner are described in detail below.

[0021] <Latex ink-receiving layer (X)> The latex ink film of the present invention has a latex ink-receiving layer (X). The latex ink-receiving layer (X) is the portion to which latex ink is applied and has the function of fixing the printed portion of the applied latex ink. The thickness of the latex ink-receiving layer (X) is not particularly limited, but is preferably 0.05 μm to 50 μm, more preferably 0.1 μm to 25 μm, and even more preferably 0.1 μm to 10 μm.

[0022] The latex ink-receiving layer (X) is formed from a composition (x1) containing an active energy ray-curable compound (A) and a polymer dispersant (B). By forming the latex ink-receiving layer (X) from the composition (x1) containing the active energy ray-curable compound (A) and a polymer dispersant (B), the latex ink-receiving layer (X) can have excellent substrate adhesion and ink adhesion.

[0023] In one embodiment of the present invention, the composition (x1) used to form the latex ink-receiving layer (X) may consist solely of component (A) and component (B). However, it may also contain other components in addition to component (A) and component (B) as long as the effects of the present invention are not impaired. Examples of such other components include a polymerization initiator (C). When component (A) is an ultraviolet-curable compound, a photopolymerization initiator (C1) is preferred. Other additives commonly used in ink-receiving layers, such as latex ink-receiving layers, include, for example, a reaction accelerator (catalyst), a surface conditioner, a plasticizer, a filler, and a colorant.

[0024] In one embodiment of the present invention, the total content of component (A) and component (B) is preferably more than 50% by mass, more preferably 55% by mass or more, even more preferably 60% by mass or more, still more preferably 70% by mass or more, even more preferably 80% by mass or more, and even more preferably 90% by mass or more, based on the total amount of active ingredients in composition (x1).

[0025] The active energy ray-curable compound (A) and polymer dispersant (B) contained in the composition (x1), as well as the polymerization initiator (C), which is a preferred component other than these components, will be described in detail below.

[0026] (Active Energy Ray-Curable Compound (A)) The composition (x1) used in the present invention contains an active energy ray-curable compound (A). In the present invention, the term "active energy ray" refers to electromagnetic waves or charged particle beams that have an energy quantum, such as ultraviolet rays and electron beams.

[0027] Examples of the active energy ray-curable compound (A) include polyfunctional (meth)acrylate monomers, (meth)acrylate prepolymers, and active energy ray-curable polymers. Among these, it is preferable to use one or more compounds selected from the group consisting of polyfunctional (meth)acrylate monomers and (meth)acrylate prepolymers.

[0028] Examples of polyfunctional (meth)acrylate monomers include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, caprolactone-modified dicyclopentenyl di(meth)acrylate, ethylene oxide-modified phosphate di(meth)acrylate, arylated cyclohexyl di(meth)acrylate, isocyanurate di(meth)acrylate, and trimethylolpropane tri(meth)acrylate. Examples of the polyfunctional (meth)acrylate monomer include dipentaerythritol tri(meth)acrylate, propionic acid-modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide-modified trimethylolpropane tri(meth)acrylate, tris(acryloxyethyl)isocyanurate, pentaerythritol tetra(meth)acrylate, propionic acid-modified dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ethylene oxide-modified dipentaerythritol hexa(meth)acrylate, and caprolactone-modified dipentaerythritol hexa(meth)acrylate. One type of polyfunctional (meth)acrylate monomer may be used alone, or two or more types may be used in combination.

[0029] Examples of (meth)acrylate prepolymers include polyester acrylate prepolymers, epoxy acrylate prepolymers, urethane acrylate prepolymers, and polyol acrylate prepolymers. Polyester acrylate prepolymers can be obtained, for example, by esterifying the hydroxyl groups of a polyester oligomer having hydroxyl groups at both ends, obtained by condensation of a polycarboxylic acid and a polyhydric alcohol, with (meth)acrylic acid, or by esterifying the terminal hydroxyl groups of an oligomer obtained by adding an alkylene oxide to a polycarboxylic acid with (meth)acrylic acid. Epoxy acrylate prepolymers can be obtained, for example, by reacting (meth)acrylic acid with the oxirane ring of a relatively low-molecular-weight bisphenol epoxy resin or novolac epoxy resin to esterify it. Urethane acrylate prepolymers can be obtained, for example, by esterifying a polyurethane oligomer, obtained by reaction of a polyether polyol or polyester polyol with a polyisocyanate, with (meth)acrylic acid. The polyol acrylate prepolymer can be obtained by esterifying the hydroxyl groups of a polyether polyol with (meth)acrylic acid. The (meth)acrylate prepolymer may be used alone or in combination of two or more.

[0030] Commercially available polyfunctional (meth)acrylate monomers and (meth)acrylate prepolymers include, for example, Beamset (registered trademark) manufactured by Arakawa Chemical Industries, Ltd., Aronix (registered trademark) manufactured by Toagosei Co., Ltd., Viscoat (registered trademark) manufactured by Osaka Organic Chemical Industry Co., Ltd., and NK Ester (registered trademark) manufactured by Shin-Nakamura Chemical Co., Ltd. From the viewpoint of productivity of the latex ink film, it is preferable that the active energy ray is ultraviolet light. Therefore, it is preferable that the active energy ray-curable compound (A) is an ultraviolet-curable compound.

[0031] (Polymer Dispersant (B)) The composition (x1) used in the present invention contains a polymer dispersant (B) having one or more functional groups selected from the group consisting of acidic functional groups and basic functional groups. The inclusion of the polymer dispersant (B) in the composition (x1) dramatically improves the ink adhesion of the latex ink-receiving layer (X) formed from the composition (x1), thereby improving both the substrate adhesion and ink adhesion of the latex ink-receiving layer (X). While the polymer dispersant (B) is generally used to disperse pigments and the like, the inventors' studies have surprisingly found that the polymer dispersant (B) has the effect of dramatically improving the ink adhesion of the latex ink-receiving layer (X).

[0032] Examples of the acidic functional group contained in the polymer dispersant (B) include a carboxyl group (including a carboxyl anhydride group formed by dehydration condensation of two carboxyl groups), a phosphoric acid group, a sulfonic acid group, or a salt group thereof. The polymer dispersant (B) may contain one type of acidic functional group alone or two or more types of acidic functional groups.

[0033] Examples of the basic functional group contained in the polymer dispersant (B) include primary, secondary, or tertiary amino groups, quaternary ammonium bases, and groups derived from nitrogen-containing heterocycles such as pyridine, pyrimidine, and pyrazine. The polymer dispersant (B) may contain one type of basic functional group alone or two or more types of basic functional groups.

[0034] The polymer dispersant (B) is preferably a copolymer containing a structural unit derived from a compound having one or more functional groups selected from the group consisting of an acidic functional group and a basic functional group, and a structural unit derived from a hydrophobic monomer. Examples of the hydrophobic monomer include (meth)acrylic acid esters [(meth)acrylic acid C such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, and stearyl (meth)acrylate]. 1-20(meth)acrylic monomers such as alkyl, cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate, aryl (meth)acrylates such as phenyl (meth)acrylate, aralkyl (meth)acrylates such as benzyl (meth)acrylate and 2-phenylethyl (meth)acrylate; styrene-based monomers such as styrene, α-methylstyrene, and vinyltoluene; α-C 2-20 Examples of suitable hydrophobic monomers include olefins (ethylene, propylene, 1-butene, isobutylene, 1-hexene, 1-octene, 1-dodecene, etc.); and vinyl carboxylic acid ester monomers such as vinyl acetate and vinyl butyrate. When producing the copolymer, one hydrophobic monomer may be used alone, or two or more may be used in combination. Furthermore, when producing the copolymer, one compound having one or more functional groups selected from the group consisting of acidic functional groups and basic functional groups may be used alone, or two or more may be used in combination.

[0035] The acid value of the polymer dispersant (B) is preferably 1 mgKOH / g to 200 mgKOH / g, more preferably 1 mgKOH / g to 180 mgKOH / g, and even more preferably 1 mgKOH / g to 160 mgKOH / g. When the acid value of the polymer dispersant (B) is within the above range, the ink adhesion of the latex ink-receiving layer (X) formed from the composition (x1) is more likely to be improved, and therefore, both substrate adhesion and ink adhesion can be easily achieved. The acid value of the polymer dispersant (B) can be measured, for example, in accordance with JIS K0070:1992.

[0036] The amine value of the polymer dispersant (B) is preferably 1 mgKOH / g to 200 mgKOH / g, more preferably 1 mgKOH / g to 180 mgKOH / g, and even more preferably 2 mgKOH / g to 160 mgKOH / g. When the amine value of the polymer dispersant (B) is within the above range, the ink adhesion of the latex ink-receiving layer (X) formed from the composition (x1) is more likely to be improved, and therefore, both substrate adhesion and ink adhesion can be easily achieved. The amine value of the polymer dispersant (B) can be measured, for example, in accordance with JIS K7237:1995.

[0037] Commercially available polymer dispersants (B) include, for example, FLOLENE (registered trademark) manufactured by Kyoeisha Chemical Co., Ltd., DISPERBYK (registered trademark) manufactured by BYK Japan K.K., and AJISPER (registered trademark) manufactured by Ajinomoto Fine-Techno Co., Ltd. The polymer dispersants (B) may be used singly or in combination of two or more.

[0038] (Ratio of Component (B) to Component (A)) From the viewpoint of making it easier to improve the effects of the present invention, the ratio of component (B) to component (A) [(B) / (A)] is preferably 1 / 100 to 50 / 100, more preferably 1 / 100 to less than 50 / 100, even more preferably 3 / 100 to 40 / 100, still more preferably 4 / 100 to 30 / 100, and even more preferably 5 / 100 to 20 / 100.

[0039] (Polymerization initiator (C)) The composition (x1) used in the present invention preferably contains a polymerization initiator (C). As the polymerization initiator (C), a general polymerization initiator used when curing the active energy ray-curable compound (A) can be used as appropriate. Here, as described above, from the viewpoint of productivity of the latex ink film, the active energy ray is preferably ultraviolet light, and the active energy ray-curable compound (A) is preferably an ultraviolet light-curable compound. When the active energy ray-curable compound (A) is an ultraviolet light-curable compound, the polymerization initiator (C) is preferably a photopolymerization initiator (C1). As the photopolymerization initiator (C1), a general photopolymerization initiator used when curing an ultraviolet light-curable compound with ultraviolet light can be used as appropriate. Specific examples include 1-hydroxycyclohexyl phenyl ketone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzyl diphenyl sulfide, tetramethylthiuram monosulfide, azobisisobutyronitrile, benzyl, dibenzyl, diacetyl, β-chloroanthraquinone, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 2,4,6-trimethylzoyldiphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, and α-hydroxyacetophenone.

[0040] The content of the polymerization initiator (C) is preferably 0.1 to 10 parts by mass based on 100 parts by mass of the active energy ray-curable compound (A).

[0041] <Substrate (Y)> The film for latex ink of the present invention has a substrate (Y). The substrate (Y) supports the latex ink-receiving layer (X) and also functions as a support for supporting a printed portion formed on the latex ink-receiving layer (X).

[0042] The substrate (Y) is not particularly limited, but is preferably a resin film. The substrate (Y) being a resin film improves the rigidity and flexibility of the film for latex ink, thereby improving the handling properties of the film for latex ink. This is also advantageous from the viewpoint of reducing the production cost and weight of the film for latex ink.

[0043] Here, the substrate (Y) is preferably a transparent resin film, which allows a printed matter having a printed portion formed on the latex ink-receiving layer of the film for latex ink to be suitably used as glass decoration in stores, showrooms, offices, etc.

[0044] Examples of resins constituting the resin film include polyester-based resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyolefin resins such as polyethylene and polypropylene; polystyrene; acrylonitrile-butadiene-styrene copolymer; cellulose triacetate; polycarbonate; urethane resins such as polyurethane and acrylic-modified polyurethane; polymethylpentene; polysulfone; polyether ether ketone; polyethersulfone; polyphenylene sulfide; polyimide-based resins such as polyetherimide and polyimide; polyamide-based resins; acrylic resins; fluorine-based resins, etc. Among these, from the viewpoint of easily improving the adhesion between the latex ink-receiving layer (X) and the substrate (Y), polyester-based resins and polyolefin-based resins are preferred, polyester-based resins are more preferred, and polyethylene terephthalate is even more preferred.

[0045] The resin film may be composed of only one type of resin, or may be composed of two or more types of resin. When the resin film is composed of two or more types of resin, it is preferably a multi-layered structure. Furthermore, the uppermost layer of the multi-layered structure (the layer in contact with the latex ink-receiving layer (X)) is preferably a polyester-based resin, more preferably polyethylene terephthalate, from the viewpoint of easily improving the adhesion between the latex ink-receiving layer (X) and the substrate (Y).

[0046] The resin film may be unstretched or may be stretched uniaxially, such as longitudinally or transversely, or biaxially.

[0047] In addition, the resin film may contain, together with these resins, additives for the substrate, such as a surface conditioner, a plasticizer, an ultraviolet absorber, a light stabilizer, a colorant, etc. The content of the additives for the substrate is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less, based on the total amount of the substrate (Y).

[0048] The thickness of the substrate (Y) is not particularly limited, but is preferably 15 μm to 300 μm, more preferably 30 μm to 200 μm.

[0049] <Adhesive Layer (Z)> The film for latex ink of one embodiment of the present invention may have an adhesive layer (Z). By having the adhesive layer (Z), the film for latex ink of one embodiment of the present invention can be suitably used as an adhesive film.

[0050] The adhesive constituting the adhesive layer is not particularly limited, and examples thereof include acrylic adhesives, urethane adhesives, and silicone adhesives.

[0051] The thickness of the pressure-sensitive adhesive layer (Z) is not particularly limited, but from the viewpoint of improving the handleability when using the film for latex ink as a pressure-sensitive adhesive film, it is preferably 5 μm to 100 μm, more preferably 10 μm to 70 μm, and even more preferably 15 μm to 50 μm.

[0052] <Release Liner> The film for latex ink of one embodiment of the present invention may have a release liner together with the pressure-sensitive adhesive layer (Z). By covering the adhesive surface of the pressure-sensitive adhesive layer (Z) of the film for latex ink of one embodiment of the present invention with a release liner, the adhesive surface of the pressure-sensitive adhesive layer (Z) can be suitably protected during transportation and storage of the film for latex ink.

[0053] The release liner is not particularly limited, and release liners commonly used in the field of adhesive films can be used as appropriate. Examples of release liners include laminates in which a release layer is provided on the surface of a film substrate or a paper substrate. Examples of film substrates include polyester resins such as polyethylene terephthalate, and polyolefin resins such as polyethylene resins and polypropylene resins. Examples of paper substrates include papers such as fine paper, kraft paper, and glassine paper. Examples of materials constituting the release layer include silicone, long-chain alkyl resins, and fluorine-based resins.

[0054] The thickness of the release liner is not particularly limited, but is preferably 10 μm to 150 μm, more preferably 20 μm to 130 μm, and even more preferably 30 μm to 100 μm.

[0055] [Method for Producing Film for Latex Ink] The method for producing the film for latex ink of the present invention is not particularly limited, and may be appropriately selected depending on the configuration of the film for latex ink.

[0056] <Method of Forming Latex Ink Receiving Layer (X)> A preferred method of forming the latex ink receiving layer (X) is to apply the composition (x1) to one surface (Ya) of the substrate (Y) to form a coating film, dry the coating film, and then cure it with active energy rays to form the latex ink receiving layer (X). In order to improve the workability of application to the substrate (Y), the composition (x1) is preferably further diluted with a dilution solvent to form a solution.

[0057] Examples of dilution solvents include water and organic solvents such as methyl ethyl ketone, acetone, ethyl acetate, tetrahydrofuran, dioxane, cyclohexane, n-hexane, toluene, xylene, n-propanol, and isopropanol. When composition (x1) is a solution, the concentration of the active ingredient is preferably 10 to 50% by mass.

[0058] Examples of the method for applying the composition (x1) include Mayer bar coating, gravure coating, roll coating, knife coating, and die coating.

[0059] The composition (x1) is applied to one surface (Ya) of the substrate (Y) to form a coating film, and then the coating film is dried to remove the dilution solvent from the coating film (drying step). Heating conditions for drying the coating film include, for example, a drying temperature of 60°C to 120°C and a drying time of 30 seconds to 3 minutes.

[0060] After drying the coating film, the coating film is irradiated with active energy rays to cure (polymerize) the active energy ray-curable compound (A) (active energy ray irradiation step). The active energy ray is preferably ultraviolet light. When ultraviolet light is used as the active energy ray, the irradiation conditions for the ultraviolet light are an integrated dose (integrated light amount) of 5 to 1200 mJ / cm. 2 is preferred, and 50 to 500 mJ / cm 2 The ultraviolet light can be irradiated using, for example, a high-pressure mercury lamp, an electrodeless UV lamp, a xenon lamp, an LED, or the like as an ultraviolet light source.

[0061] <Method of Forming Pressure-Sensitive Adhesive Layer (Z)> When the film for latex ink of one embodiment of the present invention has a pressure-sensitive adhesive layer (Z), the pressure-sensitive adhesive layer (Z) is formed on the other surface (Yb) of the substrate (Y) on which the latex ink-receiving layer (X) is not formed. The pressure-sensitive adhesive layer (Z) is formed, for example, by applying a composition for forming the pressure-sensitive adhesive layer (pressure-sensitive adhesive layer-forming composition) to the other surface (Yb) of the substrate (Y). Alternatively, the pressure-sensitive adhesive layer (Z) may be formed by applying the pressure-sensitive adhesive layer-forming composition to the release surface of a release liner, and then the pressure-sensitive adhesive layer (Z) may be laminated (transferred) to the other surface (Yb) of the substrate (Y). The method of applying the pressure-sensitive adhesive layer-forming composition is the same as that described above for composition (x1).

[0062] [Uses of Latex Ink Film, etc.] The latex ink film of the present invention is preferably used for printing using latex ink. Therefore, according to the present invention, there is provided a method of using the latex ink film to form a printed section on the latex ink-receiving layer of the latex ink film using latex ink. Also, according to the present invention, there is provided a method for producing a printed item, which includes a step of forming a printed section on the latex ink-receiving layer of the latex ink film using latex ink. Furthermore, according to the present invention, there is provided a printed item having a printed section printed with latex ink on the latex ink-receiving layer of the latex ink film.

[0063] Below, we will explain the latex ink used to form a printed area on the latex ink-receiving layer of the latex ink film of the present invention, and then we will explain the method for forming a printed area on the latex ink-receiving layer of the latex ink film of the present invention.

[0064] <Latex Ink> Latex ink contains a liquid dispersion medium and a dispersoid composed of a material containing at least a resin, dispersed (emulsified and / or suspended) in the dispersion medium. Latex ink has a low environmental impact. Another advantage of latex ink is that it can produce deep colors with a thin layer. The latex particles that make up latex ink contain a binder (resin), which is generally advantageous in improving the adhesion of the pigment colorant to the recording medium. Another advantage is that it can be printed on demand using an inkjet method. It is also preferable that the latex ink is a water-based ink. Water-based inks are safer and have a lower environmental impact because they suppress the generation of volatile organic compounds caused by organic solvents.

[0065] (Resin) The resin contained in the latex ink is not particularly limited, but examples include vinyl resins, acrylic resins, styrene resins, alkyd resins, polyester resins, polyurethane resins, silicone resins, fluorine-based resins, epoxy resins, phenoxy resins, polyolefin resins, and modified resins thereof (e.g., modified resins modified to be water-soluble). One or more selected from these may be used in combination. Among these, acrylic resins, styrene resins, water-soluble polyurethane resins, water-soluble polyester resins, and water-soluble acrylic resins are preferred, with acrylic resins being more preferred. The latex ink used in the latex ink film of one embodiment of the present invention is preferably a latex ink containing an acrylic resin, from the viewpoint of further improving adhesion between the latex ink-receiving layer (X) and the printed area. The resin content in the latex ink is preferably 1% by mass to 20% by mass, more preferably 2% by mass to 10% by mass, based on the total amount of the latex ink.

[0066] (Dispersion Medium) The latex ink contains water as a dispersion medium. The content of the dispersion medium (water) in the latex ink is preferably 50% by mass to 98% by mass, more preferably 60% by mass to 97% by mass, and even more preferably 70% by mass to 96% by mass, based on the total mass of the latex ink.

[0067] (Colorant) Latex inks usually contain a colorant. Various dyes, pigments, etc. can be used as the colorant. The content of the colorant in the latex ink is preferably 0.1% by mass to 20% by mass, and more preferably 0.2% by mass to 10% by mass, based on the total mass of the latex ink.

[0068] (Other Components) The latex ink may contain components other than those described above (other components), such as dispersants, antifungals, antirust agents, pH adjusters, surfactants, plasticizers, UV absorbers, and light stabilizers.

[0069] <Formation of Printed Section> The printed section using latex ink is formed by applying the latex ink onto the latex ink-receiving layer (X) of the latex ink film. The latex ink is preferably a latex ink containing an acrylic resin, from the viewpoint of further improving adhesion between the latex ink-receiving layer (X) and the printed section. The method for applying the latex ink is not particularly limited, and various printing methods can be used, but inkjet printing is preferred. Examples of inkjet printing methods include piezo printing and thermal jet printing. The film for latex ink may be heated when applying the latex ink. The heating temperature is not particularly limited, but is preferably 40°C to 90°C. This method results in a printed matter having a printed section using latex ink on the latex ink-receiving layer (X) of the latex ink film. The latex ink is preferably a latex ink containing an acrylic resin, from the viewpoint of further improving adhesion between the latex ink-receiving layer (X) and the printed section.

[0070] The present invention will be specifically described with reference to the following examples, but the present invention is not limited to these examples.

[0071] [Methods for measuring various physical properties] The methods for measuring various physical properties in the present examples are as follows: (1) Thickness of each layer The thickness of each layer was measured using a constant pressure thickness gauge manufactured by Teclock Corporation (model number: "PG-02J", standard specifications: JIS K6783:1994, JIS Z1702:1994, JIS Z1709:1995).

[0072] [Examples 1 to 15, Comparative Example 1] Inkjet printing sheets provided with latex ink films of Examples 1 to 15 and Comparative Example 1 were prepared by the following procedure.

[0073] <Preparation of Composition (x1)> The composition (x1) was prepared using the active energy ray-curable compound (A), polymer dispersant (B), and photopolymerization initiator (C1) shown below.

[0074] (Active energy ray-curable compound (A)) Beamset AQ-19 (manufactured by Arakawa Chemical Industries, Ltd.) was used. Beamset AQ-19 is a multifunctional urethane acrylate prepolymer, and is a compound that undergoes radical polymerization and three-dimensional curing when irradiated with an electron beam or ultraviolet light.

[0075] (Polymer Dispersant (B)) The following polymer dispersants (B)-1 to (B)-9 were used. The acid values ​​and amine values ​​of the following polymer dispersants (B)-1 to (B)-9 are shown in Table 1. The acid values ​​and amine values ​​shown are all from the catalog.・"Polymer dispersant (B)-1": Manufactured by Kyoeisha Chemical Co., Ltd., product name "FLOWLEN G-700" ・"Polymer dispersant (B)-2": Manufactured by Kyoeisha Chemical Co., Ltd., product name "FLOWLEN GW-1500" ・"Polymer dispersant (B)-3": Manufactured by Kyoeisha Chemical Co., Ltd., product name "FLOWLEN AF-1000" ・"Polymer dispersant (B)-4": Manufactured by BYK Japan Co., Ltd., product name "DISPERBYK-2001" ・"Polymer dispersant (B)-5": Manufactured by BYK Japan Co., Ltd., product name "DISPERBYK-2013" ・"Polymer dispersant (B)-6": Manufactured by BYK Japan Co., Ltd., product name "DISPERBYK-199" ・"Polymer dispersant (B)-7": Manufactured by Kyoeisha Chemical Co., Ltd., product name "FLOWLEN DOPA-17HF" "Polymer dispersant (B)-8": Manufactured by BYK Japan Co., Ltd., product name "DISPERBYK-109" "Polymer dispersant (B)-9": Manufactured by BYK Japan Co., Ltd., product name "DISPERBYK-2061"

[0076] (Polymerization initiator (C)) α-hydroxyacetophenone was used as a photopolymerization initiator (C1).

[0077] <Preparation of Inkjet Printing Sheet> A polyethylene terephthalate sheet (thickness: 50 μm) with an easy-adhesion layer was prepared as the substrate (Y). The active energy ray-curable compound (A), dispersant (B), and polymerization initiator (C) were mixed in the amounts shown in Table 1 (the amounts are calculated as active ingredients; Comparative Example 1 does not include dispersant (B)), and diluted with a dilution solvent (a 1:2 (mass ratio) mixture of water and isopropanol) to a solids (active ingredient) concentration of 10 mass % to prepare composition (x1). The resulting composition (x1) was applied to the substrate (Y) so that the thickness after drying was 1.8 μm or 3.6 μm. Next, the solvent contained in the composition (x1) applied to the substrate (Y) was removed by heating at 70°C for 1 minute using a hot air dryer, and then ultraviolet light having a peak wavelength of 365 nm was applied at an integrated light intensity of 400 mJ / cm. 2 The resulting film was irradiated with light and cured. This formed a latex ink-receiving layer (X) with a thickness of 1.8 μm or 3.6 μm, yielding a film for latex ink. Next, an acrylic pressure-sensitive adhesive composition was applied to the release agent side of the release liner so that the dried film would have a thickness of 20 μm, and the composition was heated at 90°C for 1 minute using a hot air dryer to remove the solvent contained in the acrylic pressure-sensitive adhesive composition, thereby forming an acrylic pressure-sensitive adhesive layer. Thereafter, the acrylic pressure-sensitive adhesive layer formed on the release liner was bonded to the surface of the substrate (Y) opposite the surface from which the latex ink-receiving layer (X) was formed, yielding a sheet for inkjet printing.

[0078] <Evaluation> (1) Evaluation of Adhesion of Substrate (Y) to Latex Ink-Receiving Layer (X) (Substrate Adhesion) Inkjet printing sheets equipped with the latex ink films of Examples 1 to 15 and Comparative Example 1 were left standing for 24 hours in an environment of 23°C and 50% relative humidity to prepare test samples. A 10 cm x 24 mm piece of Nichiban Cellotape (registered trademark) was then attached to the surface of the test sample on which the latex ink-receiving layer (X) was formed. The tape was then peeled off to check the remaining state of the latex ink-receiving layer (X) and evaluate it according to the following criteria: 1: Residual rate less than 20% 2: Residual rate 20% or more but less than 40% 3: Residual rate 40% or more but less than 60% 4: Residual rate 60% or more but less than 90% 5: Residual rate 90% or more The higher the residual rate, the better the adhesion of the latex ink-receiving layer (X) to the substrate. In this example, a rating of 4 or more was considered a pass.

[0079] (2) Evaluation of Ink Adhesion For each of the inkjet printing sheets provided with the latex ink film of Examples 1 to 15 and Comparative Example 1, a predetermined test pattern was printed on the surface of the latex ink-receiving layer (X) by the inkjet method using a latex ink (HP832, manufactured by Hewlett-Packard) with an inkjet printer (HP Latex 700W, manufactured by Hewlett-Packard). The inkjet printing sheets with the predetermined test pattern printed on the surface of the latex ink-receiving layer (X) were then left to stand for one day in an environment of 23°C and 50% relative humidity to prepare test samples. A 100 mm x 24 mm piece of Nichiban Cellotape (registered trademark) was then attached to the side of the test sample on which the printed portion was formed. The remaining area (remaining area / total area) of the printed portion after the tape was removed was determined and evaluated according to the following criteria. 1: Residual rate less than 20% 2: Residual rate 20% or more and less than 40% 3: Residual rate 40% or more and less than 60% 4: Residual rate 60% or more and less than 90% 5: Residual rate 90% or more The higher the residual rate, the better the ink adhesion of the latex ink-receiving layer (X). In this example, a rating of 4 or more was considered to be acceptable.

[0080] The results are shown in Table 1. In Table 1, "-" for the acid value and amine value indicates that the value is not listed in the catalog.

[0081]

[0082] Table 1 reveals the following: The latex ink-receiving layers (X) provided in the inkjet printing sheets of Examples 1 to 15 are excellent in both substrate adhesion and ink adhesion. On the other hand, the latex ink-receiving layer (X) provided in the inkjet printing sheet of Comparative Example 1 is excellent in substrate adhesion but poor in ink adhesion.

[0083] 1: film for latex ink; X: latex ink receiving layer; Y: substrate; Ya: one surface of substrate; Yb: other surface of substrate; Z: adhesive layer

Claims

1. A film for latex ink, having a laminated structure in which a latex ink-receiving layer (X) and a substrate (Y) are laminated, the latex ink-receiving layer (X) being formed from a composition (x1) containing an active energy ray-curable compound (A) and a polymer dispersant (B) having one or more functional groups selected from the group consisting of acidic functional groups and basic functional groups.

2. The film for latex ink according to claim 1, wherein the substrate (Y) comprises a polyester-based resin.

3. The film for latex ink according to claim 1 or 2, wherein the latex ink receiving layer (X) is laminated on one surface of the substrate (Y), and an adhesive layer (Z) is provided on the other surface of the substrate (Y).

4. The film for latex inks according to claim 3, wherein the adhesive surface of said adhesive layer (Z) is covered with a release liner.

5. The film for latex ink according to any one of claims 1 to 4, which is used for printing using latex ink containing an acrylic resin.

6. A method of using the film for latex ink according to any one of claims 1 to 5 to form a printed portion on the latex ink receiving layer of the film for latex ink using latex ink.

7. A method for producing a printed matter, comprising a step of forming a printed portion on the latex ink-receiving layer of the film for latex ink according to any one of claims 1 to 5 using latex ink.

8. A printed matter having a printed portion printed with latex ink on the latex ink receiving layer of the film for latex ink according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Ink jet recording sheet and optical data recording medium

    JP2004025481A

  • Ink for transfer printing and transfer printing method

    JP2014094992A

  • Translucent sheet and decorative glass

    WO2017169844A1