Wafer processing method and wafer processing system
The described wafer processing method using hydrogen, nitrogen, and fluorine gases, combined with chlorine gas etching, addresses the challenges of conventional silicon etching technologies by achieving high-precision and uniform etching of silicon films, improving manufacturing efficiency and reducing surface roughness.
Patent Information
- Application Number
- PCT/JP2023/020475
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-06-01
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional silicon atomic layer etching technologies face challenges such as difficulty in horizontal processing due to ionic environments, potential roughness from ion sputtering, narrow self-limiting ALE windows, and inefficiencies in continuous etching processes, which affect the precision and efficiency of semiconductor device manufacturing.
A wafer processing method involving the use of hydrogen, nitrogen, and fluorine gases to form modified layers on silicon films, followed by desorption steps, and the application of chlorine gas to achieve precise etching, allowing for the removal of natural oxide films and isotropic etching of silicon with improved control and precision.
This method enables high-precision removal of natural oxide films and etching of silicon with reduced surface roughness and expanded process windows, enhancing the efficiency and precision of semiconductor device manufacturing by allowing for uniform etching across complex three-dimensional structures without the need for wafer transfer.
Smart Images

Figure JP2023020475_05122024_PF_FP_ABST
Abstract
Description
Wafer processing method and wafer processing system
[0001] The present invention relates to a wafer processing method and a wafer processing system.
[0002] In the field of semiconductor devices, efforts to reduce power consumption and increase memory capacity are driving further miniaturization and higher integration through three-dimensional stacking of device structures. Stacked three-dimensional devices have more complex, three-dimensional structures than conventional devices, and their manufacture often relies on isotropic etching, which allows etching in the lateral direction relative to the wafer surface. Meanwhile, progress in miniaturization is also increasing the need for lateral processing technology at the atomic layer level, and the development of this technology is crucial.
[0003] Atomic layer etching (ALE) is known as a processing technology at the atomic layer level. Patent Document 1 (JP-A-2005-102666) discloses a method for etching a material on a substrate. The method disclosed in Patent Document 1 includes specifying process conditions for an atomic layer etching process of a material using a modifying gas and a removing gas, and performing the atomic layer etching process on the material on the substrate as follows: exposing the substrate to a modifying gas to modify the surface of the material, where the modifying gas has a modification energy and a desorption energy relative to the material to be etched; exposing the modified surface to a removing gas to ignite a plasma to remove the modified surface, where the modification energy is smaller than the desorption energy, and the desorption energy is smaller than the surface binding energy of the material. Patent Document 1 specifically discloses a silicon atomic layer etching (ALE) technology, in which chlorine gas is used to generate plasma and SiCl is removed from the silicon surface. x After forming the altered layer, a wafer bias was applied and SiCl x The layer removal cycle is repeated. Atomic layer etching of silicon is realized by searching for a self-limiting ALE window (hereinafter also referred to as "ALE window"), where the etching rate changes depending on the bias voltage.
[0004] On the other hand, a process for removing a native oxide film is required before etching silicon. Patent Document 2 discloses a method for removing a silicon oxide film formed on the surface of a workpiece W, which uses HF and NH 3 The present invention discloses a removal step for removing the silicon oxide film by using a gas and setting the processing temperature within a range of 150 to 200°C.
[0005] US Patent Application Publication No. 2020 / 0118835 JP 2010-109335 A
[0006] The silicon ALE technology disclosed in Patent Document 1 does not fully consider the following three points. First, since processing is performed in an ion environment, horizontal processing is difficult. Second, there is a concern that roughness may occur due to ion sputtering. Third, the self-limiting ALE window is narrow.
[0007] Furthermore, the technique for etching silicon native oxide films disclosed in Patent Document 2 removes the silicon native oxide film, but does not consider the silicon etching process after removal. Therefore, when continuing to etch silicon, it is necessary to transfer the semiconductor wafer to another apparatus, which poses a problem in the efficiency of semiconductor device manufacturing.
[0008] That is, in the silicon etching process of the above-mentioned conventional technology, the problem of removing the native oxide film on the silicon and isotropically etching the silicon layer, and controlling the etching amount over the entire surface of the three-dimensional structure with high precision and uniformity was not taken into consideration.
[0009] The present invention was made in consideration of the problems of the conventional techniques, and has an object to provide a technique that can remove native oxide films and perform silicon etching with high precision.
[0010] In order to solve the above problems, one representative wafer processing method of the present invention is a wafer processing method in which a semiconductor wafer having a silicon film formed on its upper surface is placed in a processing chamber and the silicon film is processed, and includes the steps of: supplying hydrogen, nitrogen, and fluorine gas particles to an oxide film formed on the surface of the silicon film to form a first modified layer; a first desorption step of heating the first modified layer to desorb it; after the first desorption step, supplying chlorine gas particles to the silicon film to form a second modified layer; and a second desorption step of heating the second modified layer to desorb it.
[0011] According to the present invention, it is possible to remove a native oxide film and perform etching of silicon with high precision. Problems, configurations, and effects other than those described above will become apparent from the description of the following embodiments.
[0012] FIG. 1 is a schematic diagram of an etching step in a semiconductor device manufacturing process. FIG. 2 is a schematic diagram of an etching processing apparatus. FIG. 3A is a process schematic diagram of the etching method of this embodiment. FIG. 3B is a process schematic diagram of the etching method of this embodiment. FIG. 4 is a graph showing experimental results of the relationship between etching amount and cycle dependency in the etching method of this embodiment. FIG. 5A is a graph showing test results regarding the dependency of the etching amount of polysilicon by the etching process of this embodiment on the irradiation time of fluorine radicals, nitrogen radicals, and hydrogen radicals in step (a) of FIG. 3B. FIG. 5B is a graph showing test results regarding the dependency of the etching amount of polysilicon by the etching process of this embodiment on the adsorption time of chlorine radicals in step (b) of FIG. 3B. FIG. 6 is a graph showing the dependency of the etching amount of polysilicon and oxide film on the number of cycles when steps (a) to (d) of FIG. 3B are repeated. FIG. 7 is a schematic diagram of the configuration of a wafer processing system that executes the wafer processing method of this embodiment.
[0013] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Note that the present invention is not limited to this embodiment. In addition, in the description of the drawings, the same parts are designated by the same reference numerals.
[0014] In this disclosure, the term "native oxide film" refers to an oxide film other than an intentionally formed oxide film. This term is intended to distinguish it from oxide films formed by thermal oxidation of silicon, oxide films formed by CVD (Chemical Vapor Deposition), and oxide films formed using oxygen radicals. The term "native oxide film" also refers to an oxide film that is not formed in the intended location, such as an oxide film formed on a surface perpendicular to the wafer's main surface when attempting to form an oxide film parallel to the wafer's main surface. The term "window" refers to appropriate process conditions for a certain process. The term "upper" refers to the vertically upward direction when a plate-like member or layer is placed horizontally. The term "lower" refers to the vertically downward direction when a plate-like member or layer is placed horizontally. For example, when illustrating a plate-like member or a layer included in a plate-like member, the surfaces shown at the top or bottom of the drawing may be referred to as the "upper surface" or "lower surface."
[0015] (Conventional Example) An example of a silicon film to be etched and its pattern processing will be described using FIG. 1 . FIG. 1 is a schematic diagram of an etching process in a semiconductor device manufacturing process. FIG. 1( a) is a diagram showing an example of a cross section of an etching target. FIG. 1( b) is a diagram showing the target after etching. As shown in FIG. 1( a), the silicon film 4 to be etched is, for example, a silicon film formed on a wafer Wf. The silicon film 4 has an uneven shape formed in a direction perpendicular to the main surface of the wafer Wf, resulting in a so-called trench structure. The width of the convex portion of the trench (the length in the direction parallel to the main surface of the wafer Wf) is W1. The silicon nitride film 1 is a film formed from a compound of silicon and nitrogen. The silicon oxide film 2 is a film formed from a compound of silicon and oxygen. The silicon nitride film 1 and the silicon oxide film 2 have a predetermined pattern shape and function as a mask (hard mask) in the etching process. In addition, a native oxide film 3 is formed on the surface of the silicon film 4. In addition, the native oxide film 3 is formed on the surface of the silicon film 4 due to the influence of oxygen and moisture. The silicon oxide film 2 is an oxide film that is intentionally formed to function as a mask, whereas the native oxide film 3 is an oxide film that is unintentionally formed.
[0016] 1B shows an ideal etching process. Because the etching is isotropic, the grooves are enlarged in a direction parallel to the main surface of the wafer Wf. The width W2 of the convex portion is smaller than the width W1 before the process. Furthermore, the native oxide film 3 is also removed to the extent that it was formed, while the shape of the silicon film 4 is maintained.
[0017] However, in reality, it is difficult to obtain the shape shown in Figure 1(b). If the etching process is performed without removing the native oxide film 3, the surface roughness of the silicon film 4 will worsen, which may adversely affect the electrical characteristics of the semiconductor device.
[0018] (Configuration of Etching Processing Apparatus) The overall configuration of the etching processing apparatus 100 will be outlined with reference to FIG. 2. FIG. 2 is a schematic diagram of the etching processing apparatus 100. The processing chamber 34 is composed of a base chamber (vacuum vessel) 37, in which a wafer stage 10 for placing a wafer 9 is installed. A plasma source (ICP plasma source) using an ICP (Inductively Coupled Plasma) discharge method is installed above the processing chamber 34. The ICP plasma source is used to generate reactive gases by plasma, and is used to clean the inner walls of the chamber and to process film layers to be processed on wafers.
[0019] A cylindrical discharge tube 12 constituting an ICP plasma source is installed above a processing chamber 34, and an ICP coil 11 is installed outside the discharge tube 12. A high-frequency power supply 35 is connected to the ICP coil 11 via a matching device 36, and high-frequency power is supplied for plasma generation. The frequency of the high-frequency power is in the frequency band of several tens of megahertz, such as 13.56 MHz. A top plate 13 is installed above the discharge tube 12. A gas dispersion plate 14 and a shower plate 15 are installed below the top plate 13, and processing gas is introduced into the discharge tube 12 via the gas dispersion plate 14 and the shower plate 15.
[0020] The supply flow rate of the process gas is adjusted by a mass flow controller 30 installed for each gas type. In addition, a gas distributor 31 is installed downstream of the mass flow controller 30, and the flow rate and combination of the gas supplied to the center of the discharge tube 12 and the gas supplied to the outer periphery are independently controlled and supplied. This allows for detailed control of the spatial distribution of the partial pressure of the process gas. Note that in FIG. 2, argon (Ar) gas, nitrogen (N 2 ) gas, hydrogen (H 2 ) gas, sulfur hexafluoride (SF 6 ) gas, difluoromethane (CH 2 F 2 ) gas, oxygen (O 2 ) gas, chlorine (Cl 2 ) gas is used as the process gas, other gases may be used.
[0021] An exhaust mechanism 20 is connected to the bottom of the processing chamber 34 via a vacuum exhaust pipe 19 in order to reduce the pressure in the processing chamber 34. The exhaust mechanism 20 is configured, for example, by a turbomolecular pump, a mechanical booster pump, or a dry pump, but is not limited to these. In addition, a pressure adjustment mechanism 21 is installed on the vacuum exhaust pipe 19 in order to adjust the pressure in the processing chamber 34.
[0022] An IR lamp unit for heating the wafer 9 is installed above the wafer stage 10. The IR lamp unit includes an IR lamp 60, a reflector 61 that reflects IR light, and an IR light transmitting window 72. Here, the IR lamps 60 are circular (circular shaped) IR lamps 60-1, 60-2, and 60-3.
[0023] The IR lamps 60 emit light (herein referred to as IR light) mainly ranging from visible light to infrared light. In this example, three circles of IR lamps 60-1, 60-2, and 60-3 are arranged concentrically, but two circles, or four or more circles may also be used. A reflector 61 is installed above the IR lamps 60 to reflect the IR light downward (toward the wafer placement direction).
[0024] An IR lamp power supply 73 is connected to the IR lamp 60 , and a high frequency cut filter 74 is installed midway between the IR lamp and the power supply 73 to prevent high frequency power noise from entering the IR lamp power supply 73 .
[0025] The IR lamp power supply 73 is also provided with a function for independently controlling the power supplied to the IR lamps 60-1, 60-2, and 60-3, making it possible to adjust the radial distribution of the amount of heat applied to the wafer (some of the wiring is not shown).
[0026] A flow path 27 is formed in the center of the IR lamp unit. An ion shielding plate 26 with a plurality of holes is installed in this flow path 27 to suppress ions and electrons generated in the plasma and to allow neutral gases and neutral radicals to pass through and irradiate the wafer.
[0027] A coolant flow path 39 for cooling the wafer stage 10 is formed inside the wafer stage 10, and a chiller 38 circulates and supplies the coolant through the flow path 39. In addition, in order to fix the wafer 9 by electrostatic attraction, a plate-shaped electrode plate 40 is embedded in the wafer stage 10 and is connected to a DC power supply.
[0028] In addition, in order to efficiently cool the wafer 9, helium (He) gas with a flow rate adjusted by a mass flow controller 32 can be supplied between the backside of the wafer 9 and the wafer stage 10. In addition, in order to prevent the backside of the wafer 9 from being scratched when heating or cooling is performed while the wafer 9 is being adsorbed, the surface (wafer mounting surface) of the wafer stage 10 is coated with a resin such as polyimide. Furthermore, a thermocouple 70 for measuring the temperature of the wafer stage 10 is installed inside the wafer stage 10, and this thermocouple 70 is connected to a thermocouple thermometer 71.
[0029] (Etching Process) The wafer processing method of this embodiment will be described with reference to FIGS. 3A and 3B. In the wafer processing method, a semiconductor wafer having a silicon film (silicon film 4) formed on its upper surface, which is the processing target, is placed in a processing chamber and the silicon film is processed. FIGS. 3A and 3B are process schematic diagrams of the etching processing method of this embodiment. FIGS. 3A and 3B show a portion of the cross-sectional structure of the processing target, and are schematically represented using atoms that constitute the processing target. In the step shown in FIG. 3A, a native oxide film is removed, and in the step shown in FIG. 3B, an etching process of the processing target film is performed. The processing shown in FIGS. 3A and 3B is performed with the wafer 9 still mounted on the wafer stage 10.
[0030] Step (a) of FIG. 3A shows the initial state of a silicon film 4, which is a silicon film to be processed. A native oxide film 3 is a native oxide film formed in advance on the surface of the silicon film 4. The silicon film 4 is a silicon layer underlying the native oxide film 3. The silicon film 4 is composed of regularly arranged silicon atoms. The native oxide film 3 is composed of silicon atoms on the surface of the silicon film 4 and oxygen atoms attached to cover the silicon atoms on the surface. In the present disclosure, the two film types, the native oxide film 3 and the silicon film 4, are etched in a consistent manner using the same equipment. Detailed process steps are described below.
[0031] The silicon film 4 is not limited to being formed on the upper surface of the wafer 9, but may also be a silicon film formed on the wafer 9. Furthermore, when the wafer 9 is a silicon wafer, the silicon film 4 may be the surface of the wafer 9. Although FIGS. 3A and 3B show a silicon film 4 formed on the upper surface of the wafer 9 and a gas being supplied from the upper surface of the silicon film 4, the silicon film 4 may also be a film formed on the side surface of a trench structure, as shown in FIG. 4 . That is, the present disclosure applies not only to a native oxide film 3 formed in a direction parallel to the main surface of the wafer 9, but also to a native oxide film 3 formed in a direction perpendicular to the main surface of the wafer 9. Furthermore, the native oxide film 3 in the present disclosure is assumed to be formed under conditions in which the wafer is placed in a processing chamber 34 during a semiconductor manufacturing process. Because the thickness of the native oxide film 3 has been found to be approximately 1 nanometer (nm), which is known to correspond to the thickness of one atomic layer, it is represented as a single layer of film in FIG. 3A .
[0032] Step (b) of FIG. 3A shows a process of supplying hydrogen, nitrogen, and fluorine gas particles to an oxide film previously formed on the surface of a silicon film to form a first modified layer. The first modified layer also contains ammonium silicofluoride. In step (b) of FIG. 3A, sulfur hexafluoride gas, nitrogen gas, and hydrogen gas are first supplied and introduced into the discharge region 50. Then, the high-frequency power supply 35 is turned on to supply high-frequency power, forming plasma in the discharge region 50. Fluorine (F) radicals, nitrogen (N) radicals, and hydrogen (H) radicals generated in the plasma are supplied to the processing chamber 34 via the flow path 27 and the ion shielding plate 26 and adsorbed onto the surface of the wafer 9. The fluorine radicals, nitrogen radicals, and hydrogen radicals react with the native oxide film 3 to modify the native oxide film 3, and ammonium silicofluoride (NH), a compound containing silicon, nitrogen, fluorine, and hydrogen, is deposited on the surface of the silicon film 4. 4 ) 2 SiF 6 A layer (first modified layer) 5 is formed.
[0033] Step (c) of FIG. 3A shows a first desorption step in which the first modified layer 5 is heated and desorbed. In the first desorption step, heating is performed by irradiating the processing chamber 34 with electromagnetic waves. Specifically, in step (c) of FIG. 3A, argon (Ar) is supplied as an inert gas, the high-frequency power supply 35 is turned on to form plasma in the discharge region 50, and the IR lamp 60 irradiates infrared (IR) rays to heat the wafer 9. This method thermally decomposes and desorbs the first modified layer 5 formed on the surface of the silicon film 4, thereby etching (removing) the native oxide film 3. The temperature of the wafer 9 during this reaction is preferably 150° C. or higher. In other words, the silicon film 4 is heated to 150° C. or higher. The IR lamp is then turned off, and the wafer is cooled by supplying helium (He) gas for wafer cooling to the backside of the wafer 9, restoring the temperature of the wafer 9 to the temperature of the wafer stage 10. This is to prevent diffusion of silicon atoms from the surface of the silicon film 4 .
[0034] 3A and 3B, a purging step of evacuating the inside of the processing chamber 34 to reduce the pressure may be included. The purging step is performed by operating the exhaust mechanism 20.
[0035] After the native oxide film removal process from step (a) in FIG. 3A to step (c) in FIG. 3A is performed, the silicon film 4 etching process from step (a) in FIG. 3B to step (d) in FIG. 3B is performed.
[0036] Step (a) of FIG. 3B is a step subsequent to step (c) of FIG. 3A (the first desorption step). In step (a) of FIG. 3B, a layer (damaged layer 6) with hydrogen, nitrogen, or fluorine particles attached thereto is formed on the surface of the silicon film 4. Specifically, in step (a) of FIG. 3B, first, sulfur hexafluoride gas, nitrogen gas, and hydrogen gas, the same gas system as in step (b) of FIG. 3A, are supplied and introduced into the discharge region 50. Next, the high-frequency power supply 35 is turned on to supply high-frequency power, thereby forming plasma in the discharge region 50. Fluorine radicals, nitrogen radicals, and hydrogen radicals generated in the plasma are supplied to the processing chamber 34 via the flow path 27 and the ion shielding plate 26 and adsorbed onto the surface of the wafer 9. The fluorine radicals, nitrogen radicals, and hydrogen radicals react with the silicon film 4, forming the damaged layer 6. Then, the gas containing fluorine, nitrogen, and hydrogen atoms remaining in the gas phase is evacuated (purged).
[0037] Although the same gas system is used in step (a) of FIG. 3B and step (b) of FIG. 3A, adjusting the flow rate ratio of sulfur hexafluoride gas, nitrogen gas, and hydrogen gas can increase the selectivity for native oxide film that may be generated during silicon layer etching in steps (a) to (d) of FIG. 3B. FIG. 4 shows an example of the amount of oxide film etched before and after adjusting the flow rate ratio of sulfur hexafluoride gas, nitrogen gas, and hydrogen gas in steps (a) of FIG. 3B and (b) of FIG. 3A. FIG. 4 is a graph showing experimental results of the relationship between the amount of etching and cycle dependency in the etching method of this embodiment. By adjusting the flow rate ratio, it is possible to almost completely suppress the generation of native oxide film, as shown in the graph of FIG. 3B(a) in FIG. 4.
[0038] Step (b) of FIG. 3B is a step that follows the first desorption step. Step (b) of FIG. 3B shows a step of supplying chlorine gas particles to the silicon film to form a second modified layer. Specifically, in step (b) of FIG. 3B, first, a gas containing chlorine atoms (chlorine (Cl)) is supplied to the discharge region 50. 2 ) gas, boron trichloride (BCl 3 ) gas, etc.) is introduced. The high-frequency power supply 35 is turned on to supply high-frequency power, and plasma is formed in the discharge region 50. Chlorine (Cl) radicals generated in the plasma are supplied to the processing chamber 34 via the flow path 27 and the ion shielding plate 26 and are adsorbed onto the surface of the wafer 9. The chlorine radicals react with the damaged layer 6 to form a layer of a compound containing silicon, fluorine, hydrogen, nitrogen, and chlorine (second modified layer) 7. The high-frequency power supply 35 is then turned off to stop plasma generation. The gas containing chlorine atoms remaining in the gas phase is then evacuated.
[0039] Step (c) of FIG. 3B shows a second desorption step in which the second modified layer is heated to desorb it. In the second desorption step, the heating is performed by irradiating electromagnetic waves. Specifically, in step (c) of FIG. 3B, argon (Ar) gas, which is an inert gas, is supplied, the high-frequency power supply 35 is turned on to form plasma in the discharge region 50, and the wafer is heated by the IR lamp 60. This method thermally decomposes and desorbs the second modified layer 7 formed on the surface of the silicon film 4, thereby removing the second modified layer 7 as shown in step (d) of FIG. 3B.
[0040] 3B and 3C, a purging step of evacuating the inside of the processing chamber 34 to reduce the pressure may be included. The purging step is performed by operating the exhaust mechanism 20.
[0041] (Process Conditions) Fig. 5A is a graph showing test results regarding the dependence of the etching amount of polysilicon by the etching process of this embodiment on the irradiation time of fluorine radicals, nitrogen radicals, and hydrogen radicals in step (a) of Fig. 3B. Fig. 5B is a graph showing test results regarding the dependence of the etching amount of polysilicon by the etching process of this embodiment on the adsorption time of chlorine radicals in step (b) of Fig. 3B.
[0042] As shown in Fig. 5A, the amount of etching performed between the formation of the second modified layer 7 (step (a) in Fig. 3B) and the desorption (step (d) in Fig. 3B) saturates at about 1.2 nm when the radical irradiation time in step (a) in Fig. 3B is in the range of 5 (s) to 30 (s). Also, as shown in Fig. 5B, the amount of etching performed between the formation of the second modified layer 7 (step (a) in Fig. 3B) and the desorption (step (d) in Fig. 3B) saturates at about 1.5 nm when the adsorption time, which is the time for adsorbing chlorine radicals to the damaged layer 6 in step (b) in Fig. 3B, is in the range of 10 (s) to 30 (s).
[0043] Therefore, when the irradiation time in FIG. 3B(a) is set to a range of 5 (s) to 30 (s) and the adsorption time in FIG. 3B(b) is set to a range of 10 (s) to 30 (s), uniform etching capable of removing one atomic layer can be performed.
[0044] When etching a pattern with a complex structure, such as a deep groove structure, it is necessary to increase the radical irradiation time and adsorption time so that the radicals can reach the film to be processed. On the other hand, if the radical irradiation time and adsorption time are increased too much, deposition may occur and the surface roughness may worsen. Therefore, it is desirable to adjust the radical irradiation time and adsorption time according to the structure of the target pattern.
[0045] According to the wafer processing method of the present disclosure, a silicon film is processed by performing a cycle consisting of multiple steps, including the step of forming a second modified layer and the second desorption step, multiple times. Specifically, the surface of the silicon film 4 is exposed by going through steps (a) to (d) of FIG. 3B . If the desired etching amount is not achieved, the process returns to step (a) of FIG. 3B and repeats steps (a) to (d) of FIG. 3B to ultimately achieve the desired etching amount. FIG. 6 shows the dependence of the etching amount of polysilicon and oxide film on the number of cycles when steps (a) to (d) of FIG. 3B are repeated. The circle indicated by point 301 represents the test result of the etching amount of polysilicon, and the square indicated by point 302 represents the test result of the etching amount of oxide film. The dashed line 401 represents the result of linear regression of the etching amount test result for polysilicon. The test results are shown by a dashed line 401 that passes through the circle marks that represent the measurement results. As shown by the dashed line 401, polysilicon can be etched linearly as the number of cycles increases. Furthermore, since the amount of oxide film etched does not increase even when the number of cycles is increased, polysilicon can be selectively etched.
[0046] In the present invention, examples have been described using polysilicon samples as an example of a silicon layer, but similar effects can be obtained with single-crystal silicon layers or amorphous silicon layers. Figure 6 shows a comparison of the etching amount of a silicon layer according to the present invention and that of a polysilicon sample. Point 303 represents the etching amount of a single-crystal silicon layer processed under the same conditions.
[0047] 7 is a schematic diagram of a wafer processing system 200 that executes the wafer processing method of this embodiment. The wafer processing system 200 includes the etching processing apparatus 100 and a control device 500. The control device 500 includes at least one processor 501 and at least one memory 502.
[0048] The control device 500 acquires the temperature from the thermocouple thermometer 71. The control device 500 also controls the operations of the exhaust mechanism 20, the pressure adjustment mechanism 21, the high frequency power supply 35, the mass flow controllers 30, 32, and 33, the chiller 38, and the IR lamp power supply 73. In addition, the control device 500 is connected to sensors (not shown) and controls power supplies and the like in order to control the operations of the etching processing device 100.
[0049] The memory 502 stores a program that, when executed by the processor 501, causes the etching processing apparatus 100 to perform the wafer processing method described in this embodiment.
[0050] 6, the wafer processing method of the present disclosure enables linear etching by increasing the number of cycles, thereby achieving self-limiting atomic layer etching of the silicon film.
[0051] Furthermore, according to the wafer processing method of the present disclosure, the etching process of the silicon film is performed in a radical environment, particularly as shown in steps (a) and (b) of FIG. 3B. Because processing in an ion environment can be avoided, it is possible to easily process the wafer in a direction parallel to the main surface of the wafer, in addition to processing in a direction perpendicular to the main surface of the wafer. Furthermore, it is possible to provide a margin for the radical irradiation time and adsorption time, which are conditions for achieving a uniform etching amount, thereby ensuring a process window. Because the irradiation time and adsorption time are parameters that are relatively easy to control, it is easy to address the deterioration of surface roughness. Furthermore, according to the wafer processing method of the present disclosure, since the same processing gas is used, removal of the native oxide film and atomic layer etching of the silicon film can be performed in the same etching processing apparatus. There is no need to transport the wafer, which avoids a loss of efficiency in semiconductor device manufacturing.
[0052] As described above, according to the present invention, the native oxide film can be removed and silicon etching can be performed with high precision.
[0053] In this embodiment, the IR lamps 60 are used to heat the wafer, but the heating method is not limited to this.
[0054] Furthermore, the present invention is not limited to the above-described embodiments, but includes various modifications. For example, the above-described embodiments have been described in detail to clearly explain the present invention, and the present invention is not necessarily limited to those including all of the described configurations. Furthermore, it is possible to replace part of the configuration of one embodiment with the configuration of another embodiment, and it is also possible to add the configuration of another embodiment to the configuration of one embodiment. Furthermore, it is also possible to add, delete, or replace part of the configuration of each embodiment with other configurations.
[0055] The present invention is not limited to the following embodiments: (Aspect 1) A processing method for etching a native oxide film formed on silicon and a silicon layer, comprising the steps of: placing the wafer on a wafer stage in a processing chamber inside a vacuum vessel; supplying fluorine, nitrogen, and hydrogen radicals to the wafer to form a modified layer on the native oxide film; heating the wafer to desorb and remove the modified layer formed on the native oxide film; supplying fluorine, nitrogen, and hydrogen radicals to the wafer to form a modified layer on the silicon surface after the native oxide film has been removed; supplying chlorine radicals to the wafer to further modify the modified layer formed on the silicon surface, and desorbing and removing the modified layer formed by chlorine radical adsorption by heating and inert gas plasma discharge; and repeating the steps of forming a modified layer on the silicon and desorbing and removing the modified layer formed. (Aspect 2) The etching method according to Aspect 1, wherein the steps of supplying fluorine, nitrogen, and hydrogen radicals to the wafer to form a modified layer on the native oxide film and supplying fluorine, nitrogen, and hydrogen radicals to the wafer to form a modified layer on the silicon surface after the native oxide film has been removed utilize the same gas system containing fluorine, nitrogen, and hydrogen radicals, but maintain a selectivity to other films by adjusting the gas flow rate ratio. (Aspect 3) The etching processing apparatus according to Aspect 1, wherein the modified layer formed on the silicon surface is a layer of a compound containing silicon, fluorine, nitrogen, hydrogen, and chlorine. (Aspect 4) The etching processing method according to Aspect 1, wherein silicon oxide film etching including native oxide film etching and silicon etching are performed in the same apparatus.
[0056] 1: silicon nitride film, 2: silicon oxide film, 3: native oxide film, 4: silicon film, 5: first modified layer, 6: damaged layer, 7: second modified layer, 9: wafer, 10: wafer stage, 11: ICP coil, 12: discharge tube, 13: top plate, 14: gas dispersion plate, 15: shower plate, 19: vacuum exhaust piping, 20: exhaust mechanism, 21: pressure adjustment mechanism, 26: ion shielding plate, 27: flow path, 30, 32, 33: mass flow controller, 34: processing chamber, 35: high frequency power supply, 36: matching machine, 37: base chamber, 38: chiller, 39: flow path, 40: electrode plate, 50: discharge area, 60: IR lamp, 61: reflector, 70: thermocouple, 71: thermocouple thermometer, 72: IR light transmission window, 73: IR lamp power supply, 74: high frequency cut filter, 100: etching processing apparatus, 200: wafer processing system, 500: control apparatus, 501: processor, 502: memory
Claims
1. A wafer processing method in which a semiconductor wafer having a silicon film formed on its upper surface is placed in a processing chamber and the silicon film is processed, the wafer processing method comprising the steps of: supplying hydrogen, nitrogen and fluorine gas particles to an oxide film formed on the surface of the silicon film to form a first modified layer; a first desorption step of heating the first modified layer to desorb it; a step of supplying chlorine gas particles to the silicon film after the first desorption step to form a second modified layer; and a second desorption step of heating the second modified layer to desorb it.
2. A wafer processing method according to claim 1, comprising performing a cycle of a plurality of steps including the step of forming the second modified layer and the second desorption step a plurality of times to process the silicon film.
3. A wafer processing method according to claim 1 or 2, wherein the heating is performed by irradiating the inside of the processing chamber with electromagnetic waves in the first or second desorption step.
4. A wafer processing method according to claim 1 or 2, wherein the silicon film is heated to 150° C. or higher in the first desorption step.
5. A wafer processing method according to claim 1 or 2, wherein the first modified layer contains ammonium silicofluoride.
6. A wafer processing method according to claim 1 or 2, wherein a layer of hydrogen, nitrogen or fluorine particles adhering to the surface of the silicon film is formed after the first desorption step.
7. A wafer processing method as defined in claim 1 or 2, comprising a purging step of evacuating the inside of the processing chamber to reduce pressure between the step of forming the first modified layer and the first desorption step, or between the step of forming the second modified layer and the second desorption step.
8. A wafer processing method for placing a semiconductor wafer having a silicon film formed thereon in a processing chamber and processing the silicon film, the wafer processing method comprising: a step of supplying hydrogen, nitrogen and fluorine gas particles to the silicon film to form a first modified layer; a step of supplying chlorine gas particles to the first modified layer to form a second modified layer; and a second desorption step of heating the second modified layer to desorb the second modified layer.
9. A wafer processing method according to claim 8, comprising the steps of: forming the second modified layer and the second desorption step forming one cycle; and performing the cycle a number of times to process the silicon film.
10. A wafer processing method as defined in claim 8 or 9, comprising a purging step of evacuating the inside of the processing chamber to reduce pressure between the step of forming the first modified layer and the step of forming the second modified layer, or between the step of forming the second modified layer and the desorption step.
11. A wafer processing system for placing a semiconductor wafer having a silicon film formed on an upper surface thereof in a processing chamber and processing the silicon film, the wafer processing system comprising: an etching processing device; a processor; and a memory having a program, the program being configured to cause the etching processing device to perform the wafer processing method recited in claim 1 when executed by the processor.
Citation Information
Patent Citations
Light emission monitoring method, substrate processing method, and substrate processing apparatus
JP2020092135A
Etching method and etching equipment
JP2020115498A
Etching processing method and etching processing apparatus
JP2020115538A
Etching method and etching device
JP2020205304A