Zn-al-mg-si-based plated steel sheet

The Zn-Al-Mg-Si plated steel sheet, with its unique composition and surface structure, enhances corrosion resistance in both appearance and joint areas with aluminum alloys, addressing the challenges of conventional zinc plating in corrosive environments and zinc resource depletion.

WO2024247424A1PCT designated stage expired Publication Date: 2024-12-05JFE STEEL CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/008333
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-03-05
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

There is a need for improved corrosion resistance, particularly in appearance and joint areas, for plated steel sheets, especially when in contact with aluminum alloy parts, as conventional zinc plating methods are insufficient in modern corrosive environments and zinc resource depletion is a concern.

Method used

A Zn-Al-Mg-Si plated steel sheet with a specific composition and structure, including a ternary eutectic structure and a high density of acicular Si alloy phase on the surface, enhances corrosion resistance by forming a sacrificial protective film and improving adhesion and workability.

Benefits of technology

The Zn-Al-Mg-Si plated steel sheet demonstrates excellent appearance corrosion resistance and improved corrosion resistance at dissimilar mating parts with aluminum alloys, effectively addressing the limitations of conventional zinc plating in harsh environments and resource conservation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008333_05122024_PF_FP_ABST
    Figure JP2024008333_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a Zn-Al-Mg-Si-based plated steel sheet which has excellent appearance corrosion resistance and excellent heterojoint-portion corrosion resistance in a portion in which a flat portion and a processed portion contact an aluminum alloy. This Zn-Al-Mg-Si-based plated steel sheet comprises a base steel sheet and a plating layer formed on at least one surface of the base steel sheet, and is characterized in that the plating layer has a composition containing, in terms of mass%, 0.50-3.00% Mg, 0.10-3.00% Al, 0.010-0.20% Si, and up to 0.30% Fe, the remainder comprising Zn and unavoidable impurities, and has a Zn-Al-MgZn2 ternary eutectic structure, and that, in a backscattered electron image with a magnification of 5,000 times obtained by irradiating the surface of the plating layer with an electron beam at an acceleration voltage of 7.0 kV using a scanning electron microscope, acicular Mg2Si-alloy-phase grains having a major-axis dimension of 0.5 μm or greater are present on the Zn-Al-MgZn2 ternary eutectic structure at a number density of 100,000 grains / mm2 or higher.
Need to check novelty before this filing date? Find Prior Art

Description

Zn-Al-Mg-Si plated steel sheet

[0001] The present invention relates to a Zn-Al-Mg-Si plated steel sheet.

[0002] Zinc plating, which inhibits iron corrosion through sacrificial corrosion protection, is excellent in rust prevention performance and economy, and is widely used to manufacture steel materials with high corrosion resistance. In particular, hot-dip galvanized steel materials, in which a plating layer is formed by immersing steel materials in molten zinc, have a simpler manufacturing process and are cheaper than electrogalvanized steel materials, and therefore demand for hot-dip galvanized steel materials is increasing across industries such as automobiles, home appliances, and building materials. However, due to the worsening of air pollution and corrosive environments associated with industrial advancement and the depletion of zinc resources due to a significant increase in zinc use, there has been a demand for plated steel materials that are more corrosion-resistant than conventional zinc plating and that also require less zinc.

[0003] Patent Document 1 discloses a Zn-Al-Mg plated steel material in which elements such as aluminum (Al) and magnesium (Mg) are added to zinc (Zn) to improve the corrosion resistance of the steel material. Patent Document 2 reports that adding silicon (Si) to a Zn-Al-Mg plated layer improves the corrosion resistance of the plated steel material at the flat and edge surfaces compared to conventional Zn-Al-Mg plated steel sheets. Patent Document 3 reports that adding Si to the plated layer of a Zn-Al-Mg plated steel sheet and concentrating Si at the interface between the plated layer and the base steel sheet imparts fracture toughness to the plated layer and improves corrosion resistance after processing.

[0004] Japanese Patent Application Laid-Open No. 4-147955 Japanese Patent Application Laid-Open No. 2005-82834 Japanese Patent Application Laid-Open No. 2021-508771

[0005] However, further improvements in the external corrosion resistance and corrosion resistance of joints of plated steel sheets have been required.In addition, as the use of aluminum alloy sheets and aluminum die-castings in automobile bodies has increased in order to drastically reduce the weight of automobiles, corrosion resistance at joints between plated steel sheet members and aluminum alloy members has become a new required property, and corrosion resistance at joints between plated steel sheet members and aluminum alloy members has been desired.

[0006] In view of the above problems, an object of the present invention is to provide a Zn-Al-Mg-Si plated steel sheet that has excellent appearance corrosion resistance and excellent corrosion resistance at dissimilar joints where the flat plate portion and the processed portion come into contact with an aluminum alloy.

[0007] As a result of intensive research to solve the above problems, the present inventors have found the following: 2 The formation of the Si alloy phase in the surface layer of the plating layer can improve the corrosion resistance of the appearance and the corrosion resistance of dissimilar joints at the contact points between the flat plate portion and the processed portion and the aluminum alloy. 2 and N 2 By using a mixed gas consisting of Mg 2 The Si alloy phase can be formed in the surface layer of the plating layer.

[0008] That is, the gist and configuration of the present invention are as follows.

[0009] [1] A steel sheet having a base steel sheet and a coating layer formed on at least one surface of the base steel sheet, wherein the coating layer contains, in mass%, Mg: 0.50 to 3.00%, Al: 0.10 to 3.00%, Si: 0.010 to 0.20%, and Fe: 0.30% or less, with the balance being Zn and unavoidable impurities, and a Zn-Al-MgZn 2 and a ternary eutectic structure, wherein the Zn—Al—MgZn ternary eutectic structure is found in a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 7.0 kV using a scanning electron microscope. 2 On the ternary eutectic structure, needle-shaped Mg 2 The number density of the Si alloy phase is 100,000 pieces / mm 2 Zn-Al-Mg-Si based plated steel sheet characterized by the presence of the above.

[0010] [2] In a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope, 2 Needle-shaped Mg with a long side length of 0.5 μm or more, which exists on the ternary eutectic structure2 The number density of the Si alloy phase is 1000 pieces / mm 2 The Zn-Al-Mg-Si plated steel sheet according to the above [1], which is as follows:

[0011] According to the present invention, it is possible to provide a Zn-Al-Mg-Si plated steel sheet that has excellent corrosion resistance in appearance and corrosion resistance in dissimilar joints at contact points between the flat plate portion and the processed portion and the aluminum alloy.

[0012] 1A is a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of a plating layer with an electron beam at an accelerating voltage of 7.0 kV in one example of the present invention, and 1B to 1C are Mg distribution, Si distribution, Al distribution, and Zn distribution, respectively, obtained by composition analysis using EDS.

[0013] Hereinafter, an embodiment of the Zn-Al-Mg-Si plated steel sheet according to the present invention will be described. Note that the embodiment described below is an example of the present invention, and the configuration of the present invention is not limited to this specific example.

[0014] A Zn-Al-Mg-Si based plated steel sheet according to one embodiment of the present invention comprises a base steel sheet and a plating layer formed on at least one surface of the base steel sheet. The plating layer contains, by mass%, 0.50 to 3.00% Mg, 0.10 to 3.00% Al, 0.010 to 0.20% Si, and 0.30% or less Fe, with the balance being Zn and unavoidable impurities. 2 Furthermore, in a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 7.0 kV using a scanning electron microscope, the Zn—Al—MgZn ternary eutectic structure is 2 On the ternary eutectic structure, needle-shaped Mg 2 The number density of the Si alloy phase is 100,000 pieces / mm 2 The presence of more than one

[0015] The type of the substrate steel sheet used in the present invention is not particularly limited, and for example, a hot-rolled steel sheet or hot-rolled steel strip that has been pickled and descaled, or a cold-rolled steel sheet or cold-rolled steel strip obtained by cold-rolling such a hot-rolled steel sheet or hot-rolled steel strip, can be used. There is also no particular limit to the thickness of the substrate steel sheet, but it is preferably 0.7 to 2.0 mm.

[0016] Next, the composition of the Zn-Al-Mg-Si based plating layer in the present invention will be described.

[0017] If the Mg content in the plating layer is less than 0.50% by mass, the effect of improving the corrosion resistance of dissimilar joints at the contact points between the flat plate portion and the processed portion and the aluminum alloy is insufficient. Therefore, the Mg content in the plating layer is set to 0.50% by mass or more, and preferably 1.00% by mass or more. On the other hand, if the Mg content in the plating layer exceeds 3.00% by mass, brittle lumpy MgZn alloys are formed. 2 A phase is formed, which makes the plating layer brittle and reduces adhesion, and there is a risk of deterioration in workability and corrosion resistance of the processed part. Therefore, the Mg content in the plating layer is set to 3.00 mass% or less, and preferably 2.50 mass% or less.

[0018] If the Al content in the plating layer is less than 0.10% by mass, the effect of improving the corrosion resistance of dissimilar joints at the contact points between the flat plate portion and the processed portion and the aluminum alloy is insufficient. Therefore, the Al content in the plating layer is set to 0.10% by mass or more, and preferably 0.50% by mass or more. On the other hand, if the Al content in the plating layer exceeds 3.00% by mass, swelling from scratches that occur after painting of the plated steel sheet becomes large, and the appearance corrosion resistance deteriorates. Therefore, the Al content in the plating layer is set to 3.00% by mass or less, and preferably 2.00% by mass or less.

[0019] When the content of Si in the plating layer is 0.010 mass% or more, Mg is contained in the plating layer together with Mg. 2 The formation of a Si alloy phase contributes to improving the corrosion resistance of the coating layer. This is thought to be due to the following action: 2 Because the Si alloy phase is active, it reacts with water in a corrosive environment and decomposes, forming the Zn-Al-MgZn alloy described below. 2In the ternary eutectic coating structure, Zn phase, Al phase and MgZn 2 The metal structure containing one or more of the alloy phases is sacrificially protected from corrosion. At the same time, the resulting Mg corrosion product forms a protective film, suppressing further corrosion. This improves the corrosion resistance of dissimilar joints at the contact points between the flat plate portion and the processed portion and the aluminum alloy. To achieve the above effect, the Si content in the plating layer is set to 0.010 mass% or more, and preferably 0.050 mass% or more. On the other hand, if the Si content in the plating layer exceeds 0.20 mass%, a large amount of Mg will penetrate into the plating layer. 2 Si alloy phase is formed. Mg 2 Since the Si alloy phase is brittle, if a large amount of Si alloy is formed inside the plating layer, external stress can cause cracks inside the plating layer. As a result, the plating layer is prone to cracking during forming, and the corrosion resistance of the dissimilar joint at the contact point between the processed part and the aluminum alloy is reduced. Therefore, the Si content in the plating layer is set to 0.20 mass% or less, and preferably 0.15 mass% or less.

[0020] If the Fe content in the coating layer exceeds 0.30 mass%, the growth of an alloy layer formed at the interface between the base steel sheet and the coating layer increases, resulting in a decrease in workability. Therefore, the Fe content in the coating layer is set to 0.30 mass% or less, and preferably 0.20 mass% or less. On the other hand, the lower limit of the Fe content in the coating layer is not particularly limited, and may be 0.00 mass%.

[0021] The remainder of the composition of the plating layer other than those mentioned above consists of Zn and unavoidable impurities.

[0022] Next, the structure of the Zn-Al-Mg-Si based plating layer will be described. 2 It has a ternary eutectic coating structure, and Mg 2 The coating structure further contains a Zn phase, an Al phase, or an MgZn phase. 2 An alloy phase may be included.

[0023] Mg in Zn-Al-Mg-Si based plating layer 2The Si alloy phase contributes to improving corrosion resistance, but if it exists in large quantities deep inside the coating layer, it may cause the Mg 2 Stress concentration occurs in the Si alloy phase, which promotes the initiation and growth of cracks and reduces corrosion resistance after processing. 2 It is preferable that the Si alloy phase is located near the surface of the plating layer. To achieve this, it is necessary to control the Si content in the plating bath components and to use a reducing gas as the wiping gas. If such control is insufficient, Mg 2 The Si alloy phase may be present in a small amount in the surface layer of the plating layer, resulting in a deterioration in corrosion resistance, or may be present in a large amount even inside the plating layer, resulting in a decrease in corrosion resistance after processing.

[0024] In the present invention, Mg 2 The phrase "the Si alloy phase is formed in the surface layer of the plating layer" means that the Si alloy phase is not formed in the surface layer of the plating layer in a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 7.0 kV using a scanning electron microscope. 2 On the ternary eutectic structure, needle-shaped Mg 2 This means that a Si alloy phase is observed. 2 In order to obtain the corrosion resistance improving effect of the Si alloy phase, Mg formed in the surface layer of the plating layer 2 The number density of the Si alloy phase is 100,000 pieces / mm 2 or more, 150,000 pieces / mm 2 It is preferable that the number of particles is 200,000 or more per mm. 2 On the other hand, Mg formed on the surface of the plating layer is more preferably 100% or more. 2 Although there is no upper limit to the number density of the Si alloy phase, even if an appropriate wiping gas is used, the number density of the plating layer produced using the plating bath composition of the present invention cannot be increased to 650,000 pieces / mm 2 Since it is difficult to exceed this number density, the number density is usually 650,000 pieces / mm 2 The following is the result.

[0025] In the present invention, Mg 2The phrase "the Si alloy phase is formed inside the plating layer" means that the surface of the plating layer is irradiated with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope, and in a backscattered electron image at a magnification of 5000 times, a Zn-Al-MgZn 2 On the ternary eutectic structure, needle-shaped Mg 2 This means that a Si alloy phase is observed. 2 The number density of the Si alloy phase is 1000 pieces / mm 2 When the thickness is less than 100 μm, the corrosion resistance after processing is favorably obtained. 2 The number density of the Si alloy phase is 1000 pieces / mm 2 It is preferable that the number of particles is 750 or less per mm 2 More preferably, the number is 500 or less per mm 2 More preferably, the number is 0 or less per mm 2 It is most preferable that:

[0026] 1(a) to (e) show backscattered electron images (5000x magnification) and EDS analysis results observed when the surface of the plating layer of a Zn-Al-Mg-Si-plated steel sheet manufactured in one embodiment of the present invention was irradiated with an electron beam using a scanning electron microscope at an accelerating voltage of 7.0 kV. FIG. 1(a) is a backscattered electron image of the Zn-Al-Mg-Si-plated layer, and (b) to (e) are Mg distribution, Si distribution, Al distribution, and Zn distribution, respectively, obtained by composition analysis using EDS. As shown in FIGS. 1(a) to (e), Mg 2 The Si alloy phase has a needle-like shape where the Mg and Si compositions overlap, and the Zn-Al-MgZn 2 It can be seen that it is in a ternary eutectic structure.

[0027] [Method for manufacturing Zn-Al-Mg-Si plated steel sheet] Next, a method for manufacturing a Zn-Al-Mg-Si plated steel sheet according to one embodiment of the present invention will be described. The method for manufacturing a Zn-Al-Mg-Si plated steel sheet according to one embodiment of the present invention comprises the steps of immersing a substrate steel sheet in a coating bath containing, by mass %, 0.50 to 3.00% Mg, 0.10 to 3.00% Al, 0.010 to 0.20% Si, and 0.30% or less Fe, with the balance consisting of Zn and unavoidable impurities, thereby subjecting the substrate steel sheet to a coating treatment, and, after the coating treatment, subjecting the substrate steel sheet to gas wiping to adjust the adhesion weight of the coating layer formed on the substrate steel sheet. Furthermore, the gas wiping step is performed by applying H 2 and N 2 The method for cooling the plated steel sheet after gas wiping is not particularly limited, and various methods such as air cooling, air-water cooling, and water cooling can be applied.

[0028] In the method for producing a Zn—Al—Mg—Si plated steel sheet according to the present invention, the base steel sheet to be plated is the same as that described above for the base steel sheet.

[0029] When annealing heat treatment is performed on the base steel sheet before plating treatment, H in the furnace atmosphere during annealing 2 When the concentration is 1% by volume or more, oxides on the surface of the base steel sheet can be suitably reduced. 2 The concentration is preferably 1% by volume or more. 2 When the concentration is 10% by volume or less, the manufacturing cost can be suitably reduced. 2 The concentration is preferably 10% by volume or less. 2 and the remainder is N 2 The temperature of the annealing heat treatment is not particularly limited, but is preferably 600 to 850° C. The time of the annealing heat treatment is also not particularly limited, but is preferably 10 to 60 seconds.

[0030] The coating bath used in the production of the Zn-Al-Mg-Si coated steel sheet according to the present invention has a composition containing, by mass%, 0.50 to 3.00% Mg, 0.10 to 3.00% Al, 0.010 to 0.20% Si, and 0.30% or less Fe, with the balance consisting of Zn and unavoidable impurities. The explanation of each component in the coating bath is the same as the explanation of each component of the coating layer described above. The component composition of the coating bath is equivalent to the component composition of the applied coating layer.

[0031] The coating weight of the plating layer in the plating process is set to 15 g / m from the viewpoint of corrosion resistance. 2 It is preferable that the content is 30 g / m or more. 2 On the other hand, the coating weight of the plating layer is more preferably 100 g / m or more. 2 When the coating weight of the plating layer is 100 g / m or less, the manufacturing cost can be suitably reduced. 2 It is preferable that the temperature of the plating bath during plating treatment is 430 to 540°C. If the temperature of the plating bath is less than 430°C, the fluidity of the plating bath will decrease, which may hinder uniform plating deposition. Therefore, the temperature of the plating bath is preferably 430°C or higher. On the other hand, if the temperature of the plating bath exceeds 540°C, there is a risk of an increase in oxides on the surface of the plating bath due to oxidation of Mg in the plating bath, and erosion of the refractory material in the plating bath by Al and Mg. Therefore, the temperature of the plating bath is preferably 540°C or lower, more preferably 530°C or lower.

[0032] Mg 2 In order to form the Si alloy phase in the surface layer of the coating layer and not to form much inside the coating layer, it is important that the wiping gas has reducing properties. 2 and N 2 Conventionally, in the production of hot-dip galvanized steel sheets, air or N has been used as the wiping gas from the viewpoint of economy. 2 The present inventors have found that, in particular, in the production of the Si-containing Zn—Al—Mg—Si-plated steel sheet of the present invention, the O contained in the wiping gas is2 The inventors have found that the surface layer of the plating is oxidized by the H of the wiping gas, and as a result, the desired corrosion resistance may not be obtained. 2 The lower the concentration, the more difficult it is to suppress the formation of oxides on the surface of the substrate steel sheet. As a result, the oxides formed on the surface of the substrate steel sheet are converted into Mg in the surface layer of the coating layer. 2 It has been found that this prevents the formation of Si alloy phases and promotes their formation within the plating layer.

[0033] Wiping gas H 2 When the concentration is 1% by volume or more, Mg is present in the surface layer of the plating layer. 2 The Si alloy phase is suitably formed, and the effect of contributing to the improvement of corrosion resistance is suitably obtained. 2 The concentration is preferably 1% by volume or more. 2 When the concentration is 5% by volume or more, oxide formation on the surface of the substrate steel sheet is suitably suppressed, and Mg 2 The formation of a Si alloy phase inside the plating layer is effectively suppressed. 2 When the concentration is 10% by volume or less, the manufacturing cost can be suitably reduced. 2 The concentration is preferably 10% by volume or less. The wiping is preferably performed in an atmospheric environment.

[0034] For steps and conditions not described in the present invention, conventional methods can be used.

[0035] All Zn-Al-Mg-Si plated steel sheets were produced as samples using a 0.8 mm thick ultra-low carbon cold rolled steel sheet as the base steel sheet using hot dip plating equipment. Each sample was plated using variously changed plating bath compositions, and the plating bath temperature was set to 450°C, which is 30°C higher than the solidification start temperature estimated from the Zn-Al-Mg-Si quaternary equilibrium phase diagram. The base steel sheet was then plated using H 2 (5% by volume) + N 2The steel sheet was heated in an atmosphere, and the temperature of the base steel sheet when immersed in the coating bath was set to the same temperature as the coating bath temperature, and hot-dip coating was performed in the coating bath for 1 second. Thereafter, the thickness of the coating layer was reduced to 7 μm (50 g / m) by adjusting the flow rate of the wiping gas. 2 The plating bath composition, the wiping gas composition, and the plating layer composition are shown in Table 1. The wiping was performed in an air atmosphere.

[0036]

[0037] Each sample of the obtained Zn—Al—Mg—Si plated steel sheet was sheared to a size of 10 × 20 mm. The plating layer of the sheared sample was observed from the surface of the plated steel sheet using a scanning electron microscope to determine the Zn—Al—MgZn 2 The presence or absence of a ternary eutectic structure was confirmed. During the observation, composition analysis by EDS revealed that Zn phase, Al phase, and MgZn 2 The structure is composed of three phases of the alloy phase, and when the same surface is analyzed by XRD, Zn phase, Al phase, and MgZn phase are found. 2 If alloy phase is confirmed, it is Zn-Al-MgZn 2 "Yes" indicates the presence of a ternary eutectic structure, and "Zn phase, Al phase, and MgZn phase" indicates the presence of a ternary eutectic structure. 2 The structure does not consist of three phases of the alloy phase, and when the same surface is analyzed by XRD, the Zn phase, Al phase, and MgZn phase are not observed. 2 If any of the alloy phases is not confirmed, Zn-Al-MgZn 2 The absence of a crystal structure is indicated as "none" in Table 1.

[0038] The plating layer of the sheared sample was observed from the surface of the plated steel sheet using a scanning electron microscope to determine whether Mg existed in the surface and interior of the plating layer. 2 The state of the Si alloy phase was observed, and the number density was evaluated. 2 The number density of the Si alloy phase was evaluated from a backscattered electron image (5000x magnification) observed when irradiating an electron beam at an acceleration voltage of 7.0 kV. 2The number density of the Si alloy phase was evaluated from a backscattered electron image (5000x magnification) observed when irradiating an electron beam at an accelerating voltage of 15.0 kV.

[0039] [Appearance Corrosion Resistance] Next, to evaluate the appearance corrosion resistance of the resulting Zn-Al-Mg-Si plated steel sheets after painting, each sample was sheared to a size of 70 × 80 mm, phosphate-treated under the same conditions, and then electrocoated (the coating thickness was constant at 15 μm). A cross-shaped cut was made on the painted surface using a blade, and then a corrosion test was performed. The depth of the cut reached the surface of the base steel. After 90 cycles of corrosion testing according to SAE J2334 (2016), the blister width from the cross-shaped cut on the painted surface was measured, and the maximum blister width was used for evaluation. A blister width of less than 3 mm was evaluated as "◎", a blister width of 3 mm or more but less than 5 mm was evaluated as "○", a blister width of 5 mm or more but less than 7 mm was evaluated as "△", and a blister width of 7 mm or more was evaluated as "×". A blister width of ◎ or ◯ was considered a pass, and a blister width of △ or × was considered a fail.

[0040] [Corrosion Resistance of Flat Plate Dissimilar Joints] Next, to evaluate the corrosion resistance of flat plate dissimilar joints of Zn-Al-Mg-Si-plated steel sheets, each sample was sheared to a size of 80 × 80 mm and then bolted to an Al alloy (A6061, Al-0.6Si-1Mg-based) sheared to a size of 40 × 40 mm to prepare a flat plate dissimilar joint sample of Zn-Al-Mg-Si-plated steel sheet and Al alloy. In this case, all surfaces except the joint surface were covered with resin tape. The dissimilar joint samples were then subjected to a corrosion test according to SAE J2334 (2016). The corrosion amount of the Al alloy after 20 cycles of the corrosion test was evaluated. The amount of Al corrosion was determined in accordance with ISO 8407:2021 by immersing the flat plate dissimilar joint samples in a 60% by mass aqueous nitric acid solution at room temperature to remove aluminum-based corrosion products, and then calculating the difference between the weight before the test and the weight after the corrosion products were removed. Corrosion amount: 5g / m 2 If it is less than 5g / m, mark it as "◎" 2 10g / m or more 2 If it is less than 10 g / m, it is marked as "○" 2 15g / m or more 2 If it is less than 15 g / m, it is marked as "△" 2In the above cases, the result was marked with "X" and shown in Table 1. A rating of ⊚ or ◯ was considered to be a pass, and a rating of △ or × was considered to be a fail.

[0041] [Corrosion Resistance of Processed Dissimilar Joints] Next, the corrosion resistance of processed dissimilar joints of Zn-Al-Mg-Si plated steel sheets was evaluated. Each sample was sheared to a size of 70 × 120 mm and mechanically joined at two points to an Al alloy sheared to a size of 40 × 90 mm using a mechanical clinch (5 mmφ) to create a processed section. A processed dissimilar joint sample of Zn-Al-Mg-Si plated steel sheet and Al alloy was prepared. In this case, the surfaces other than the joint surface were phosphate treated under the same conditions, followed by electrodeposition coating (with a constant coating thickness of 15 μm). The processed dissimilar joint samples were then subjected to a corrosion test according to SAE J2334 (2016). The corrosion level of the Al alloy after 20 cycles of the corrosion test was evaluated. The amount of Al corrosion was determined in accordance with ISO 8407:2021 by immersing a dissimilar processed sample in a 60 mass% aqueous nitric acid solution at room temperature to remove corrosion products mainly composed of aluminum, and then calculating the difference between the weight before the test and the weight after the corrosion products were removed. 2 If it is less than 5g / m, mark it as "◎" 2 10g / m or more 2 If it is less than 10 g / m, it is marked as "○" 2 15g / m or more 2 If it is less than 15 g / m, it is marked as "△" 2 In the above cases, the result was marked with "X" and shown in Table 1. A rating of ⊚ or ◯ was considered to be a pass, and a rating of △ or × was considered to be a fail.

[0042] As shown in Table 1, when observed at an accelerating voltage of 7.0 kV, the Mg 2 The number density of the Si alloy phase is 100,000 pieces / mm 2 The above-mentioned invention examples were excellent in corrosion resistance of appearance, corrosion resistance of dissimilar joints of flat plate parts, and corrosion resistance of dissimilar joints of processed parts. 2 It was found that the presence of a large amount of Si alloy phase in the surface layer of the plating layer has an advantageous effect on the corrosion resistance of the appearance, the corrosion resistance of the flat plate dissimilar joint, and the corrosion resistance of the processed dissimilar joint. 2 The number density of the Si alloy phase is 500 pieces / mm2 is less than or equal to Mg 2 The inventive examples, which had a small amount of Si alloy phase inside the plating layer, achieved more favorable evaluation results. In contrast, the comparative examples, which were outside the scope of the present invention, were inferior to the inventive examples in any of the corrosion resistance of the appearance, the corrosion resistance of the flat portion dissimilar joint, and the corrosion resistance of the processed portion dissimilar joint.

[0043] According to the present invention, it is possible to provide a Zn-Al-Mg-Si plated steel sheet that has excellent corrosion resistance in appearance and excellent corrosion resistance in dissimilar joints at contact points between the flat plate portion and the processed portion and the aluminum alloy.

Claims

1. A steel sheet having a base steel sheet and a plating layer formed on at least one side of the base steel sheet, the plating layer containing, in mass%, Mg: 0.50 to 3.00%, Al: 0.10 to 3.00%, Si: 0.010 to 0.20%, Fe: 0.30% or less, with the balance being Zn and unavoidable impurities, and a Zn-Al-MgZn 2 and a ternary eutectic structure, wherein the Zn-Al-MgZn ternary eutectic structure is obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 7.0 kV using a scanning electron microscope and observing a backscattered electron image at a magnification of 5000 times. 2 On the ternary eutectic structure, needle-like Mg 2 The number density of the Si alloy phase is 100,000 pieces / mm 2 The Zn-Al-Mg-Si plated steel sheet is characterized in that the above-mentioned components are present.

2. The Zn-Al-MgZn was identified in a backscattered electron image at a magnification of 5,000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope. 2 Needle-like Mg with a long side length of 0.5 μm or more that exists on the ternary eutectic structure 2 The number density of the Si alloy phase is 1000 pieces / mm 2 The Zn-Al-Mg-Si plated steel sheet according to claim 1, wherein:

Citation Information

Patent Citations

  • Production of hot-dip zn-mg-al coated steel sheet

    JP1992147955A

  • Highly corrosion-resistant hot-dip plating steel sheet and manufacturing method therefor

    JP2005082834A

  • Zinc alloy plated steel material with excellent corrosion resistance after processing and its manufacturing method

    JP2021508771A

  • Plated steel

    WO2018139619A1

  • Plated steel

    WO2018139620A1