Flux and solder paste
The flux composition for solder pastes, featuring rosin, specific polymers, and benzotriazole compounds, addresses cohesiveness and blackening issues in Sn-Bi soldering, ensuring reliable electrical connections and stability.
Patent Information
- Application Number
- PCT/JP2024/011860
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-03-26
- Publication Date
- 2024-12-05
AI Technical Summary
Solder pastes containing Sn and Bi alloys face issues with high cohesiveness during reflow soldering, leading to solder ball formation, and flux residues tend to blacken over time, reducing electrical reliability and stability.
A flux composition including rosin, a polymer with specific repeating units, monoalkylpropylene glycol, dicarboxylic acid, and a benzotriazole compound is used to enhance cohesiveness, prevent blackening, and improve stability by controlling the weight average molecular weight and content ratios of these components.
The flux composition achieves high cohesiveness of solder alloy powder during reflow, suppresses blackening of flux residues, and maintains stability over time, reducing solder ball formation and viscosity changes in the solder paste.
Smart Images

Figure JP2024011860_05122024_PF_FP_ABST
Abstract
Description
Flux and solder paste
[0001] This application claims priority to Japanese Patent Application No. 2023-090350, filed May 31, 2023, the contents of which are incorporated herein by reference.
[0002] When mounting electronic components, the components are generally fixed to a substrate and electrically connected to the substrate by soldering. Soldering uses flux, solder alloys, and solder pastes, which are mixtures of flux and solder alloy powder. Flux chemically removes metal oxides present on the metal surfaces of the objects to be soldered and on the solder alloy, allowing the migration of metal elements at the interface between the two. Therefore, soldering using flux forms an intermetallic compound between the two, resulting in a strong bond.
[0003] In soldering, methods such as flow soldering and reflow soldering are used depending on the size of the objects to be joined. In flow soldering, flux is first applied to a board on which components are mounted. Then, while the board on which components are mounted is being transported, molten solder is jetted from below and brought into contact with the surface to be soldered, thereby performing soldering. In reflow soldering, solder paste is first printed on the board. Next, components are mounted on the board, and the board on which components are mounted is heated in a heating furnace called a reflow furnace, thereby performing soldering.
[0004] In recent years, lead-free solder has been used in soldering due to its adverse environmental impact. Lead-free solder, which is primarily composed of Sn, has a high melting point and therefore must be heated to a higher temperature during soldering to melt it. The higher the temperature of the molten solder, the more oxides it is likely to produce. In response to this, solder alloys containing Sn and Bi, which allow soldering at lower temperatures, have come into use in order to reduce thermal damage to substrates and save energy. When using solder alloys containing Sn and Bi, since Bi is a metal element that is easily oxidized, fluxes that address this have been proposed (see, for example, Patent Document 1).
[0005] Patent No. 7075028
[0006] In solder paste, it is desirable that the solder alloy powder have high cohesion (i.e., are less likely to form solder balls) when melted during reflow soldering. The cohesion of solder alloy powder is evaluated according to "4.2 Solder Ball Test" in JIS Z 3284-4:2014. If the solder alloy powder has low cohesion during reflow, solder balls are more likely to form. These solder balls may short-circuit the electrical circuit on the board.
[0007] The present inventors have found through their research that dicarboxylic acids are effective as activators to be added to fluxes to reduce the cohesion of solder alloy powders. However, when a flux containing dicarboxylic acids is used in a solder paste, the flux residue at the soldered joints may blacken over time after reflow, potentially resulting in reduced electrical reliability. Further research by the present inventors has found that the combined use of a compound having a benzotriazole skeleton is effective in preventing this blackening of the flux residue. However, a flux using a dicarboxylic acid in combination with a compound having a benzotriazole skeleton presents a new problem: the compound having a benzotriazole skeleton is prone to precipitate in the flux over time.
[0008] The present invention has been made in view of the above circumstances, and provides a flux that exhibits high cohesion of solder alloy powder during reflow, suppresses blackening of flux residue, and is less likely to precipitate over time, resulting in good stability over time, and a solder paste using the flux.
[0009] In order to solve the above problems, the present invention employs the following configuration.
[0010] [1] A flux containing rosin, a polymer (P) having a repeating unit represented by the following general formula (p1), a solvent, a thixotropic agent, a dicarboxylic acid, and a compound having a benzotriazole skeleton:
[0011] [In the formula, R 1 is a methyl group or a hydrogen atom. 2 is a hydrocarbon group having 1 to 2 carbon atoms or a hydrogen atom.
[0012] [2] The flux according to [1] above, wherein the weight average molecular weight of the polymer (P) is 300 to 8000. [3] The flux according to [1] above or [2] above, wherein the content of the polymer (P) is 1 mass % or more and 15 mass % or less with respect to the total mass of the flux.
[0013] [4] The flux according to any one of [1] to [3], wherein the solvent includes a monoalkyl propylene glycol. [5] The flux according to [4], wherein the monoalkyl propylene glycol includes at least one selected from the group consisting of butyl propylene triglycol and butyl propylene diglycol.
[0014] [6] The flux according to [4] or [5], wherein the content of the monoalkyl propylene glycol is 5% by mass or more and 50% by mass or less with respect to the total mass of the flux.
[0015] [7] The flux according to any one of [4] to [6], wherein the mixing ratio of the polymer (P) and the monoalkyl propylene glycol is 0.05 or more as a mass ratio represented by polymer (P) / monoalkyl propylene glycol.
[0016] [8] The flux according to any one of [1] to [7], wherein the dicarboxylic acid is a compound represented by the following general formula (c1):
[0017] [In the formula, R represents an alkylene group having 1 to 10 carbon atoms, a phenylene group, or a single bond, provided that a methylene group constituting the alkylene group may be substituted with an oxygen atom.]
[0018] [9] The flux according to any one of [1] to [8], wherein the content of the dicarboxylic acid is 0.5 mass% or more and 7.5 mass% or less with respect to the total mass of the flux.
[0019]
[10] The flux according to any one of [1] to [9], wherein the compound having a benzotriazole skeleton is at least one selected from the group consisting of compounds represented by the following general formula (AZ1-1) and compounds represented by the following general formula (AZ1-2):
[0020] [In the formula, R 11 is an organic group or a hydrogen atom. 12 is a substituent. n1 represents an integer of 0 to 4. R 21 is an organic group or a hydrogen atom. 22 is a substituent. n2 represents an integer of 0 to 4.
[0021]
[11] The flux according to any one of [1] to
[10] , wherein the content of the compound having a benzotriazole skeleton is 1 mass% or more and 10 mass% or less with respect to the total mass of the flux.
[0022]
[12] The flux according to any one of [1] to
[11] , wherein a mixing ratio of the dicarboxylic acid and the compound having a benzotriazole skeleton is 0.2 or more and 3 or less as a mass ratio expressed as dicarboxylic acid / compound having a benzotriazole skeleton.
[0023]
[13] The flux according to any one of [1] to
[12] , wherein the rosin content is 10 mass % or more and 40 mass % or less with respect to the total mass of the flux.
[14] The flux according to any one of [1] to
[13] , wherein the rosin includes at least one selected from the group consisting of acrylic acid-modified hydrogenated rosin, hydrogenated rosin, and polymerized rosin.
[0024]
[15] The flux according to any one of [1] to
[14] , wherein the thixotropic agent contains polyamide.
[16] The flux according to any one of [1] to
[15] , wherein the content of the thixotropic agent is 2 mass % or more and 15 mass % or less with respect to the total mass of the flux.
[0025]
[17] The flux according to any one of [1] to
[16] , further containing a phenyl-substituted imidazole.
[0026]
[18] The flux according to any one of [1] to
[17] above, which does not contain a halogen compound.
[0027]
[19] A solder paste containing a solder alloy powder and the flux according to any one of [1] to
[18] .
[20] The solder paste according to
[19] , wherein the solder alloy powder is made of a solder alloy containing Sn and Bi.
[0028] According to the present invention, it is possible to provide a flux that exhibits high cohesion of solder alloy powder during reflow, suppresses blackening of flux residue, and is less likely to precipitate over time, resulting in good stability over time, and a solder paste using the flux.
[0029] Fig. 1 is a diagram showing a reflow profile in the evaluation of this example. Fig. 2 is a schematic diagram explaining the evaluation method for wetting and spreading properties in this example. Fig. 3 is a diagram showing the state of blackening of flux residue in [Evaluation of suppression of blackening of flux residue] in this example. Fig. 4 is a diagram showing the state of flux floating (separated) on the surface of the solder paste after a predetermined period of storage in [Evaluation of stability over time (flux separation over time)] in this example.
[0030] (Flux) One embodiment of the flux contains rosin, a polymer (P) having a repeating unit represented by the general formula (p1) described below, a solvent, a thixotropic agent, a dicarboxylic acid, a compound having a benzotriazole skeleton, and other components as necessary. The flux of this embodiment is characterized in that it employs the polymer (P) having a repeating unit represented by the general formula (p1) as a means for suppressing precipitation over time, i.e., precipitation of the compound having a benzotriazole skeleton.
[0031] <Rosin> The flux of the present embodiment contains rosin. In the present invention, the term "rosin" encompasses natural resins containing abietic acid as a main component, including a mixture of abietic acid and its isomers, and chemically modified natural resins (sometimes referred to as rosin derivatives).
[0032] The content of abietic acid in the natural resin is, for example, 40% by mass or more and 80% by mass or less relative to the natural resin. In this specification, the term "main component" refers to a component that, among components constituting a compound, is contained in the compound at a content of 40% by mass or more.
[0033] Representative isomers of abietic acid include neoabietic acid, palustric acid, levopimaric acid, etc. Examples of the "natural resins" include gum rosin, wood rosin, tall oil rosin, etc.
[0034] In the present invention, the term "chemically modified natural resin (rosin derivative)" includes the "natural resin" that has been subjected to one or more treatments selected from the group consisting of hydrogenation, dehydrogenation, neutralization, alkylene oxide addition, amidation, dimerization, oligomerization, esterification, and Diels-Alder cycloaddition.
[0035] Examples of rosin derivatives include purified rosin, modified rosin, etc. Modified rosins include hydrogenated rosin, polymerized rosin, polymerized hydrogenated rosin, disproportionated rosin, acid-modified rosin, rosin ester, acid-modified hydrogenated rosin, acid anhydride-modified hydrogenated rosin, acid-modified disproportionated rosin, acid anhydride-modified disproportionated rosin, phenol-modified rosin, and α,β-unsaturated carboxylic acid-modified products (acrylated rosin, maleated rosin, fumarated rosin, etc.), as well as purified products, hydrogenated products, and disproportionated products of the polymerized rosin, purified products, hydrogenated products, and disproportionated products of the α,β-unsaturated carboxylic acid-modified products, rosin alcohol, rosin amine, hydrogenated rosin alcohol, rosin ester, hydrogenated rosin ester, rosin soap, hydrogenated rosin soap, and acid-modified rosin soap.
[0036] Examples of rosin amines include dehydroabietylamine, dihydroabietylamine, etc. The rosin amine refers to a so-called disproportionated rosin amine.
[0037] In the flux of this embodiment, the rosin may be used alone or in a mixture of two or more types. The rosin preferably contains a rosin derivative, more preferably one or more selected from the group consisting of acid-modified rosin, hydrogenated rosin, polymerized rosin, acid-modified hydrogenated rosin, and rosin ester. It is even more preferable to contain one or more selected from the group consisting of acid-modified hydrogenated rosin, hydrogenated rosin, and polymerized rosin, and it is particularly preferable to contain at least acid-modified hydrogenated rosin. As the acid-modified hydrogenated rosin, acrylic acid-modified hydrogenated rosin is preferred. The rosin used in the flux of this embodiment may be acid-modified hydrogenated rosin alone, a combination of acid-modified hydrogenated rosin and hydrogenated rosin, a combination of hydrogenated rosin and polymerized rosin, or polymerized rosin alone.
[0038] The rosin content in the flux of this embodiment is preferably 10% by mass or more, more preferably 10% by mass to 40% by mass, even more preferably 15% by mass to 40% by mass, particularly preferably 20% by mass to 35% by mass, and most preferably 20% by mass to 30% by mass, relative to the total mass (100% by mass) of the flux. When the rosin content is equal to or greater than the lower limit of the preferred range, the wetting and spreading of the solder paste onto the lands is improved, and when the rosin content is equal to or less than the upper limit of the preferred range, flux residue is likely to be reduced.
[0039] <Polymer (P) Having Repeating Unit Represented by General Formula (p1)> The flux of this embodiment contains a polymer (P) (hereinafter also referred to as "component (P)") having a repeating unit represented by the following general formula (p1) (hereinafter also referred to as "repeating unit (p1)"). By containing component (P), precipitation of compounds having a benzotriazole skeleton in the flux is suppressed, and in the flux, precipitation over time is less likely to occur, improving the temporal stability.
[0040] [In the formula, R 1 is a methyl group or a hydrogen atom. 2 is a hydrocarbon group having 1 to 2 carbon atoms or a hydrogen atom.
[0041] <<Repeating Unit (p1)>> In the above formula (p1), R 1 is preferably a methyl group. 2 The hydrocarbon group having 2 carbon atoms in R may be a saturated hydrocarbon group (ethyl group) or an unsaturated hydrocarbon group (ethenyl group, ethynyl group). 2 is preferably a hydrocarbon group having 1 to 2 carbon atoms, more preferably a methyl group.
[0042] Specific examples of the repeating unit (p1) are shown below.
[0043]
[0044] The repeating unit (p1) contained in the component (P) may be used alone or in combination of two or more types. The repeating unit (p1) preferably contains at least one selected from the group consisting of repeating units represented by any of the above chemical formulas (p1-1), (p1-2), (p1-3), (p1-4), and (p1-5), more preferably contains at least one selected from the group consisting of repeating units represented by any of the above chemical formulas (p1-3), (p1-4), and (p1-5), and even more preferably contains at least one selected from the group consisting of repeating units represented by any of the above chemical formulas (p1-3) and (p1-4). The proportion of the repeating unit (p1) relative to the total (100 mol%) of all repeating units constituting the component (P) may be 10 mol% or more, 20 mol% or more, more than 50 mol%, or 100 mol% (i.e., a homopolymer).
[0045] <<Repeating Unit (p2)>> The component (P) may be a polymer having the repeating unit (p1) and another repeating unit (hereinafter also referred to as “repeating unit (p2)”). Examples of the repeating unit (p2) include a repeating unit derived from an alkene and a repeating unit derived from butadiene.
[0046] Specific examples of the repeating unit (p2) are shown below.
[0047]
[0048] The repeating unit (p2) contained in the component (P) may be a single type, or a combination of two or more types. The proportion of the repeating unit (p2) relative to the total (100 mol%) of all repeating units constituting the component (P) may be 50 mol% or more, 70 to 90 mol%, or 75 to 85 mol%.
[0049] In the flux of this embodiment, the (P) component may be used alone or in combination with two or more types. The (P) component used in this embodiment is a polymer having at least the repeating unit (p1), preferably a polymer having the repeating unit (p1) as the main component, more preferably a polymer in which the proportion of the repeating unit (p1) to the total (100 mol%) of all repeating units constituting the (P) component exceeds 50 mol%, and may also be a homopolymer consisting of the repeating unit (p1). Preferred (P) components include homopolymers consisting of repeating units represented by the chemical formula (p1-3), homopolymers consisting of repeating units represented by the chemical formula (p1-4), homopolymers consisting of repeating units represented by the chemical formula (p1-5), copolymers having repeating units represented by the chemical formula (p1-3) and repeating units represented by the chemical formula (p1-4), and copolymers having repeating units represented by the chemical formula (p1-5) and repeating units represented by the chemical formula (p2-4). Among these, one or more selected from the group consisting of a copolymer having a repeating unit represented by the chemical formula (p1-3) and a repeating unit represented by the chemical formula (p1-4), and a polymer having a repeating unit represented by the chemical formula (p1-5) are more preferred, and a copolymer having a repeating unit represented by the chemical formula (p1-3) and a repeating unit represented by the chemical formula (p1-4) (hereinafter also referred to as "copolymer (P34)") is even more preferred. As the copolymer (P34), a copolymer having a repeating unit represented by the chemical formula (p1-4) as a main component is preferred, and a copolymer in which the proportion of the repeating unit represented by the chemical formula (p1-4) exceeds 50 mol % relative to the total (100 mol %) of all repeating units constituting the copolymer (P34) is more preferred.
[0050] The component (P) used in this embodiment may be a synthesized product or a commercially available product. Examples of commercially available products include Nippon Oil Polybutene (manufactured by ENEOS Corporation), Indopol Polybutene (manufactured by INEOS Oligomers), NOF Polybutene (registered trademark) (manufactured by NOF Corporation); liquid polybutadiene NISSO-PB (manufactured by Nippon Soda Co., Ltd.), and polybutadiene-type liquid polymer Poly bd TM (PolyBD) (manufactured by Idemitsu Kosan Co., Ltd.), etc.
[0051] The weight average molecular weight (Mw) of the component (P) (measured by gel permeation chromatography (GPC) in terms of polystyrene) is preferably 200 to 10,000, more preferably 250 to 9,000, and even more preferably 300 to 8,000. The number average molecular weight (Mn) of the component (P) (measured by GPC in terms of polystyrene) is preferably 200 to 7,000, more preferably 250 to 6,000, and even more preferably 300 to 5,000. When the Mw and Mn of the component (P) are within the above-mentioned preferred ranges, precipitation of compounds having a benzotriazole skeleton in the flux is more easily suppressed, and stability over time (resistance to precipitation over time) is improved.
[0052] The content of the (P) component in the flux of this embodiment is preferably 1% by mass or more and 15% by mass or less, more preferably 2% by mass or more and 10% by mass or less, and even more preferably 3% by mass or more and 10% by mass or less, relative to the total mass (100% by mass) of the flux. When the content of the (P) component is equal to or greater than the lower limit of the above-mentioned preferred range, precipitation of compounds having a benzotriazole skeleton in the flux is easily suppressed, improving the stability over time (resistance to precipitation over time). When the content of the (P) component is equal to or less than the upper limit of the above-mentioned preferred range, the stability over time (resistance to flux separation over time) is easily improved.
[0053] <Solvent> The flux of this embodiment contains a solvent, such as water, alcohol-based solvents, glycol ether-based solvents, and terpineols.
[0054] Examples of alcohol-based solvents include isopropyl alcohol, 1,2-butanediol, 1,3-butanediol, isobornylcyclohexanol, 2,4-diethyl-1,5-pentanediol, 2,2-dimethyl-1,3-propanediol, 2,5-dimethyl-2,5-hexanediol, 2,5-dimethyl-3-hexyne-2,5-diol, 2,3-dimethyl-2,3-butanediol, 2-methylpentane-2,4-diol, 1,1,1-tris(hydroxymethyl)propane, 2-ethylhexylmethylpropane, 2,4 ...ethylhexylmethylpropane, 2,5-dimethyl-2,5-hexanediol, 2,5-dimethyl-3-hexyne-2,5-diol, 2,3-dimethyl-2,3-butanediol, 2-ethylhexylmethylpropane, 2,4-ethylhexylmethylpropane, 2,5-dimethyl-2,5-hexanediol, 2,5-dimethyl-3-hexyne-2,5-diol, 2,3-dimethyl-2,3-butanediol, 2-ethylhexylmethylpropane, 2,4-ethylhexylmethylpropane, 2,5-dimethyl-2,5-hexanediol, 2,5-dimethyl-3-hexyne-2,5-diol, 2,3-dimethyl-2,3-butanediol, 2-ethylhexylmethylpropane, 2,4-ethylhexylmethylpropane, 2,5-dimethyl- ethyl-2-hydroxymethyl-1,3-propanediol, 2,2'-oxybis(methylene)bis(2-ethyl-1,3-propanediol), 2,2-bis(hydroxymethyl)-1,3-propanediol, 1,2,6-trihydroxyhexane, 1-ethynyl-1-cyclohexanol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 2-hexyl-1-decanol, octanediol, and the like.
[0055] Examples of glycol ether solvents include diethylene glycol mono-2-ethylhexyl ether, ethylene glycol monophenyl ether, diethylene glycol monohexyl ether (hexyl diglycol: HeDG), diethylene glycol dibutyl ether, triethylene glycol monobutyl ether, triethylene glycol butyl methyl ether, tetraethylene glycol, tetraethylene glycol dimethyl ether; monoalkyl propylene glycols, and the like.
[0056] Examples of terpineols include α-terpineol, β-terpineol, γ-terpineol, terpineol mixtures (i.e., mixtures whose main component is α-terpineol and contain β-terpineol or γ-terpineol), etc. Other solvents include, for example, dioctyl sebacate, liquid paraffin, etc.
[0057] In the flux of this embodiment, the solvent may be used alone or in combination of two or more. Among the above, glycol ether solvents are preferred, and monoalkyl propylene glycol is more preferred because it is particularly effective in suppressing an increase in the viscosity of the solder paste. The monoalkyl propylene glycol preferably includes one or more selected from the group consisting of butyl propylene triglycol, butyl propylene diglycol, and butyl propylene (mono)glycol, and more preferably includes one or more selected from the group consisting of butyl propylene triglycol and butyl propylene diglycol.
[0058] The content of the solvent in the flux of this embodiment is the remainder of the flux and is determined depending on the contents of the other components. For example, the content of the solvent in the flux of this embodiment may be 30% by mass to 70% by mass, 35% by mass to 60% by mass, 35% by mass to 55% by mass, or 40% by mass to 50% by mass, relative to the total mass (100% by mass) of the flux.
[0059] When monoalkyl propylene glycol is selected as the solvent in the flux of this embodiment, the content of monoalkyl propylene glycol in the flux is preferably 5 to 50 mass %, more preferably 10 to 40 mass %, and even more preferably 15 to 35 mass %, relative to the total mass (100 mass %) of the flux. When the content of monoalkyl propylene glycol is equal to or greater than the lower limit of the preferred range, an increase in the viscosity of the solder paste is easily suppressed. When the content is equal to or less than the upper limit of the preferred range, precipitation of compounds having a benzotriazole skeleton in the flux is easily suppressed, improving stability over time (resistance to precipitation over time).
[0060] In the flux of this embodiment, from the viewpoint of temporal stability (resistance to precipitation over time), the mixing ratio of the polymer (P) to the monoalkyl propylene glycol, expressed as a mass ratio of polymer (P) / monoalkyl propylene glycol, is preferably 0.05 or more, and more preferably 0.10 to 3. When this mass ratio is within the above-mentioned preferred range, precipitation of the compound having a benzotriazole skeleton in the flux is easily suppressed, and temporal stability (resistance to precipitation over time) is improved.
[0061] In the flux of this embodiment, from the viewpoint of both suppressing an increase in the viscosity of the solder paste and achieving stability over time (resistance to precipitation over time), the mixing ratio of the polymer (P) to the monoalkyl propylene glycol, expressed as a mass ratio of polymer (P) / monoalkyl propylene glycol, is preferably 0.05 or more, more preferably 0.05 to 1.5, even more preferably 0.06 to 1.0, and particularly preferably 0.10 to 0.50. When this mass ratio is equal to or greater than the lower limit of the above-mentioned preferred range, precipitation of the compound having a benzotriazole skeleton in the flux is easily suppressed, improving stability over time (resistance to precipitation over time). When the mass ratio is equal to or less than the upper limit of the above-mentioned preferred range, an increase in the viscosity of the solder paste is easily suppressed.
[0062] <Thixotropic Agent> The flux of this embodiment contains a thixotropic agent. Examples of the thixotropic agent include an amide-based thixotropic agent, an ester-based thixotropic agent, and a sorbitol-based thixotropic agent.
[0063] Examples of amide-based thixotropic agents include monoamides, bisamides, and polyamides. Examples of monoamides include lauric acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, hydroxystearic acid amide, saturated fatty acid amide, oleic acid amide, erucic acid amide, unsaturated fatty acid amide, 4-methylbenzamide (p-toluamide), p-toluenemethane amide, aromatic amide, hexamethylene hydroxystearic acid amide, substituted amide, methylol stearic acid amide, methylol amide, and fatty acid ester amide. Examples of bisamides include ethylene bisfatty acid (fatty acid having 6 to 24 carbon atoms) amide, ethylene bishydroxyfatty acid (fatty acid having 6 to 24 carbon atoms) amide, hexamethylene bisfatty acid (fatty acid having 6 to 24 carbon atoms) amide, hexamethylene bishydroxyfatty acid (fatty acid having 6 to 24 carbon atoms) amide, and aromatic bisamide. Examples of fatty acids that are raw materials for the bisamides include stearic acid (number of carbon atoms: C18), oleic acid (number of carbon atoms: C18), lauric acid (number of carbon atoms: C12), etc. Examples of polyamides include saturated fatty acid polyamides, unsaturated fatty acid polyamides, aromatic polyamides, 1,2,3-propanetricarboxylic acid tris(2-methylcyclohexylamide), cyclic amide oligomers, and acyclic amide oligomers.
[0064] Examples of the cyclic amide oligomer include an amide oligomer obtained by cyclic polycondensation of a dicarboxylic acid and a diamine, an amide oligomer obtained by cyclic polycondensation of a tricarboxylic acid and a diamine, an amide oligomer obtained by cyclic polycondensation of a dicarboxylic acid and a triamine, an amide oligomer obtained by cyclic polycondensation of a tricarboxylic acid and a triamine, an amide oligomer obtained by cyclic polycondensation of a dicarboxylic acid, a tricarboxylic acid, and a diamine, an amide oligomer obtained by cyclic polycondensation of a dicarboxylic acid, a tricarboxylic acid, and a triamine, an amide oligomer obtained by cyclic polycondensation of a dicarboxylic acid, a diamine, and a triamine, an amide oligomer obtained by cyclic polycondensation of a tricarboxylic acid, a diamine, and a triamine, and an amide oligomer obtained by cyclic polycondensation of a dicarboxylic acid, a tricarboxylic acid, a diamine, and a triamine.
[0065] The acyclic amide oligomer may be an amide oligomer obtained by acyclic polycondensation of a monocarboxylic acid with a diamine and / or triamine, or an amide oligomer obtained by acyclic polycondensation of a dicarboxylic acid and / or tricarboxylic acid with a monoamine. In the case of an amide oligomer containing a monocarboxylic acid or a monoamine, the monocarboxylic acid or monoamine functions as a terminal molecule, resulting in an acyclic amide oligomer with a reduced molecular weight. Furthermore, when the acyclic amide oligomer is an amide compound obtained by acyclic polycondensation of a dicarboxylic acid and / or tricarboxylic acid with a diamine and / or triamine, it becomes an acyclic high-molecular-weight amide polymer. Furthermore, the acyclic amide oligomer also includes an amide oligomer obtained by acyclic condensation of a monocarboxylic acid with a monoamine.
[0066] Examples of ester-based thixotropic agents include ester compounds, and specific examples include hydrogenated castor oil and ethyl myristate.
[0067] Examples of sorbitol-based thixotropic agents include dibenzylidene-D-sorbitol, bis(4-methylbenzylidene)-D-sorbitol, (D-)sorbitol, monobenzylidene (-D-)sorbitol, and mono(4-methylbenzylidene)-(D-)sorbitol.
[0068] In the flux of this embodiment, the thixotropic agent may be used alone or in combination of two or more. Among the above, the thixotropic agent preferably includes one or more selected from the group consisting of amide-based thixotropic agents and ester-based thixotropic agents, and more preferably includes one or more selected from amide-based thixotropic agents. Among amide-based thixotropic agents, polyamide is more preferable because it is particularly likely to enhance stability over time (suppression of flux separation over time). Selecting polyamide is particularly effective when the content of component (P) is high (for example, 10% by mass or more relative to the total mass (100% by mass) of the flux).
[0069] The content of the thixotropic agent in the flux of this embodiment is preferably 2% by mass or more and 15% by mass or less, more preferably 4% by mass or more and 12% by mass or less, and even more preferably 5% by mass or more and 9% by mass or less, relative to the total mass (100% by mass) of the flux. When the content of the thixotropic agent is equal to or more than the lower limit of the above-mentioned preferred range, the stability over time (suppression of flux separation over time) is easily improved, while when the content is equal to or less than the upper limit of the above-mentioned preferred range, the initial viscosity of the solder paste is easily prevented from becoming too high.
[0070] <Dicarboxylic Acid> The flux of this embodiment contains a dicarboxylic acid. By selecting a dicarboxylic acid from among organic acids, the cohesion of the solder alloy powder is enhanced (the generation of solder balls is suppressed) when the solder alloy powder melts during reflow soldering. Examples of the dicarboxylic acid include dibasic carboxylic acids, and may be either aliphatic dicarboxylic acids or aromatic dicarboxylic acids.
[0071] Preferred dicarboxylic acids include compounds represented by the following general formula (c1).
[0072] [In the formula, R represents an alkylene group having 1 to 10 carbon atoms, a phenylene group, or a single bond, provided that a methylene group constituting the alkylene group may be substituted with an oxygen atom.]
[0073] In the formula (c1), the number of carbon atoms in the alkylene group for R is preferably 2 to 8. The alkylene group for R may be linear or branched, but is preferably linear. Examples of dicarboxylic acids include succinic acid, glutaric acid, diglycolic acid, adipic acid, sebacic acid, dodecanedioic acid, o-phthalic acid, m-phthalic acid (isophthalic acid), and p-phthalic acid (terephthalic acid).
[0074] In the flux of this embodiment, the dicarboxylic acid may be used alone or in combination of two or more. Among the above, the dicarboxylic acid is preferably an aliphatic dicarboxylic acid, more preferably a dicarboxylic acid in which R in the formula (c1) is an alkylene group having 2 to 8 carbon atoms, and among these, glutaric acid and adipic acid are more preferred, with adipic acid being particularly preferred.
[0075] The dicarboxylic acid content in the flux of this embodiment is preferably 0.5% by mass to 7.5% by mass, more preferably 1% by mass to 6% by mass, and even more preferably 2% by mass to 4% by mass, relative to the total mass (100% by mass) of the flux. If the dicarboxylic acid content is equal to or greater than the lower limit of the preferred range, the cohesion of the solder alloy powder during reflow is likely to be enhanced, while if the dicarboxylic acid content is equal to or less than the upper limit of the preferred range, an increase in the viscosity of the solder paste is likely to be suppressed.
[0076] <Compound Having a Benzotriazole Skeleton> The flux of this embodiment contains a compound having a benzotriazole skeleton (hereinafter also referred to as “component (AZ1)”). By containing component (AZ1), blackening of flux residue can be suppressed.
[0077] In this specification, the term "compound having a benzotriazole skeleton" refers to a compound in which a 5-membered heterocyclic ring containing three nitrogen atoms and a benzene ring form a condensed ring.
[0078] Examples of the component (AZ1) include a compound represented by the following general formula (AZ1-1) and a compound represented by the following general formula (AZ1-2).
[0079] [In the formula, R 11 is an organic group or a hydrogen atom. 12 is a substituent. n1 represents an integer of 0 to 4. R 21 is an organic group or a hydrogen atom. 22 is a substituent. n2 represents an integer of 0 to 4.
[0080] Regarding the compound represented by general formula (AZ1-1), R11 R is an organic group or a hydrogen atom, and is preferably a hydrogen atom. 11 is an organic group, examples of the organic group include a chain hydrocarbon group having 1 to 40 carbon atoms which may have a substituent, an alicyclic hydrocarbon group having 3 to 40 carbon atoms which may have a substituent, -R 101 -N(R 102a ) (R 102b Examples of the substituent include a carboxy group, a carbonyl group, a hydroxy group, an amino group, and a halogen atom.
[0081] R 11 When R is a chain hydrocarbon group, the chain hydrocarbon group may be linear or branched, and is preferably branched. The chain hydrocarbon group may be a saturated hydrocarbon group or an unsaturated hydrocarbon group, and is preferably a saturated hydrocarbon group. 11 is an alicyclic hydrocarbon group, the alicyclic hydrocarbon group may be a polycyclic group or a monocyclic group. As a monocyclic alicyclic hydrocarbon group, a group in which one or more hydrogen atoms have been removed from a monocycloalkane is preferred. As a polycyclic alicyclic hydrocarbon group, a group in which one or more hydrogen atoms have been removed from a polycycloalkane is preferred.
[0082] R 11 Ga-R 101 -N(R 102a ) (R 102b ), then R 101 may be, for example, a hydrocarbon group having 1 to 5 carbon atoms. 101 Examples of the hydrocarbon group in R include linear or branched aliphatic hydrocarbon groups, and preferably have 1 to 10 carbon atoms, more preferably 1 to 6, even more preferably 1 to 4, and most preferably 1 to 3. 101 The linear aliphatic hydrocarbon group in is preferably a linear alkylene group, specifically a methylene group [—CH 2 -], ethylene group [-(CH 2 ) 2 -], trimethylene group [-(CH 2 ) 3 -], tetramethylene group [-(CH2 ) 4 -], pentamethylene group [-(CH 2 ) 5 -] etc. 101 The branched aliphatic hydrocarbon group in is preferably a branched alkylene group, specifically, —CH(CH 3 ) -, -CH(CH 2 CH 3 ) -, -C(CH 3 ) 2 -, -C(CH 3 ) (CH 2 CH 3 ) -, -C(CH 3 ) (CH 2 CH 2 CH 3 ) -, -C(CH 2 CH 3 ) 2 alkylmethylene groups such as -; -CH(CH 3 ) CH 2 -, -CH(CH 3 ) CH(CH 3 ) -, -C(CH 3 ) 2 CH 2 -, -CH(CH 2 CH 3 ) CH 2 -, -C(CH 2 CH 3 ) 2 -CH 2 alkylethylene groups such as -; -CH(CH 3 ) CH 2 CH 2 -, -CH 2 CH (CH 3 ) CH 2 alkyltrimethylene groups such as -; -CH(CH 3 ) CH 2 CH 2 CH 2 -, -CH 2 CH (CH 3 ) CH 2 CH 2 and alkyl alkylene groups such as alkyl tetramethylene groups such as -.
[0083] R 102a and R102b may each independently be, for example, a chain hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, or a hydrogen atom. Examples of the substituent include those described above. 102a and R 102b When is a chain hydrocarbon group, the chain hydrocarbon group may be linear or branched. The chain hydrocarbon group is a saturated hydrocarbon group or an unsaturated hydrocarbon group, and is preferably a saturated hydrocarbon group.
[0084] R in the above general formula (AZ1-1) 12 Examples of R include hydrocarbon groups having 1 to 5 carbon atoms, carboxy groups, hydroxy groups, amino groups, and halogen atoms. 12 When R is a hydrocarbon group having 1 to 5 carbon atoms, the hydrocarbon group may be either a linear or branched chain. The hydrocarbon group may be a saturated hydrocarbon group or an unsaturated hydrocarbon group, with a saturated hydrocarbon group being preferred. 12 Examples of the hydrocarbon group in R include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an isopentyl group, a sec-pentyl group, a tert-pentyl group, and a neopentyl group, and a methyl group is preferred. 12 Examples of the halogen atom in R include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. 12 may be the same as or different from each other. n1 is preferably 0 or 1.
[0085] Examples of the compound represented by general formula (AZ1-1) include 1,2,3-benzotriazole, 5-methylbenzotriazole, 1-[N,N-bis(2-ethylhexyl)aminomethyl]benzotriazole, carboxybenzotriazole, 1-[N,N-bis(2-ethylhexyl)aminomethyl]methylbenzotriazole, and the like. Among these, one or more compounds selected from the group consisting of 1,2,3-benzotriazole and 5-methylbenzotriazole are preferred, and 1,2,3-benzotriazole is more preferred.
[0086] Regarding the compound represented by general formula (AZ1-2), R 21 is an organic group or a hydrogen atom. 21 is an organic group, examples of the organic group include an aromatic hydrocarbon group which may have a substituent, a chain hydrocarbon group having 1 to 40 carbon atoms which may have a substituent, and an alicyclic hydrocarbon group having 3 to 40 carbon atoms which may have a substituent, and an aromatic hydrocarbon group is preferred.
[0087] R 21 The chain hydrocarbon group and alicyclic hydrocarbon group in 11 The aromatic hydrocarbon group is a hydrocarbon group having at least one aromatic ring, and examples thereof include aromatic hydrocarbon rings such as benzene, naphthalene, anthracene, and phenanthrene, aromatic heterocycles in which some of the carbon atoms constituting the aromatic hydrocarbon ring are substituted with heteroatoms, and fused rings in which an aromatic hydrocarbon ring and an aromatic heterocycle are fused together. 21 When the aromatic hydrocarbon group in has a substituent, examples of the substituent include a hydrocarbon group having 1 to 20 carbon atoms, an aromatic hydrocarbon group, a carboxy group, a hydroxy group, an amino group, a halogen atom, etc., and a hydrocarbon group or a hydroxy group is preferred. When the substituent is a hydrocarbon group, examples of the hydrocarbon group include, for example, R 11 When the substituent is an aromatic hydrocarbon group, examples of the aromatic hydrocarbon group include those described above.
[0088] R in the above general formula (AZ1-2) 22 As the group, R in the above general formula (AZ1-1) 12 The compound represented by general formula (AZ1-2) may have a plurality of benzotriazole skeletons. Here, "a plurality" means, for example, 2 to 5, and preferably 2.
[0089] Examples of the compound represented by the general formula (AZ1-2) include 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-tert-amylphenyl)benzotriazole, 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-tert-octylphenol], 6-(2-benzotriazolyl)-4-tert-octyl-6'-tert-butyl-4'-methyl-2,2'-methylenebisphenol, and the like. Among these, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole is preferred.
[0090] In the flux of this embodiment, the (AZ1) component may be used alone or in a mixture of two or more. Among the above, the (AZ1) component is preferably one or more selected from the group consisting of 1,2,3-benzotriazole, 5-methylbenzotriazole, and 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and more preferably contains at least 1,2,3-benzotriazole. The (AZ1) component used in the flux of this embodiment may be 1,2,3-benzotriazole alone, 5-methylbenzotriazole alone, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole alone, a combination of 1,2,3-benzotriazole and 5-methylbenzotriazole, or a combination of 1,2,3-benzotriazole and 2-(2'-hydroxy-5'-methylphenyl)benzotriazole. Among these, it is more preferable to use 1,2,3-benzotriazole alone, a combination of 1,2,3-benzotriazole and 5-methylbenzotriazole, or a combination of 1,2,3-benzotriazole and 2-(2'-hydroxy-5'-methylphenyl)benzotriazole.
[0091] The content of the compound having a benzotriazole skeleton in the flux of this embodiment is preferably 1% by mass or more and 10% by mass or less, more preferably 1% by mass or more and 6% by mass or less, and even more preferably 3% by mass or more and 5% by mass or less, relative to the total mass (100% by mass) of the flux. When the content of the compound having a benzotriazole skeleton is equal to or more than the lower limit of the above-mentioned preferred range, blackening of the flux residue is easily suppressed, while when it is equal to or less than the upper limit of the above-mentioned preferred range, the wetting and spreading of the solder paste onto the lands is improved.
[0092] In the flux of this embodiment, the content of rosin is preferably 15% by mass or more, more preferably 20% by mass or more, and the content of the compound having a benzotriazole skeleton is preferably 6% by mass or less, more preferably 5% by mass or less, relative to the total mass (100% by mass) of the flux, whereby the wetting and spreading properties of the solder paste onto the lands tend to be improved.
[0093] In the flux of this embodiment, the mixing ratio of the dicarboxylic acid to the compound having a benzotriazole skeleton, expressed as a mass ratio of dicarboxylic acid / compound having a benzotriazole skeleton, is preferably 0.2 to 3, more preferably 0.4 to 2, even more preferably 0.5 to 1.5, and particularly preferably greater than 0.5 and less than 1.5. If this mass ratio is equal to or greater than the lower limit of the above-mentioned preferred range, the cohesion of the solder alloy powder during reflow is likely to be enhanced, and if it is equal to or less than the upper limit of the above-mentioned preferred range, blackening of the flux residue is likely to be suppressed.
[0094] <Other Components> The flux of the present embodiment may contain other components as needed in addition to the rosin, polymer (P), solvent, thixotropic agent, dicarboxylic acid, and compound having a benzotriazole skeleton described above. Examples of other components include an activator, a resin component other than rosin, a metal deactivator, a surfactant, a silane coupling agent, an antioxidant, and a colorant.
[0095] <<Activator>> Examples of the activator include amines, organic acids other than dicarboxylic acids, and halogen compounds.
[0096] Regarding amines, examples of amines include rosin amines, azoles, guanidines, alkylamine compounds, amino alcohol compounds, etc. Examples of rosin amines include those exemplified in the above <Rosin>.
[0097] Examples of azoles include 2-methylimidazole, 2-ethylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, and 1-cyanoethyl-2-ethylimidazole. ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl- s-Triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, 2-phenylimidazo Phosphorus, 2,4-diamino-6-vinyl-s-triazine, 2,4-diamino-6-vinyl-s-triazine isocyanuric acid adduct, 2,4-diamino-6-methacryloyloxyethyl-s-triazine, epoxy-imidazole adduct, 2-methylbenzimidazole, 2-octylbenzimidazole, 2-pentylbenzimidazole, 2-(1-ethylpentyl)benzimidazole, 2-nonylbenzimidazole, 2-(4-thiazolyl)benzimidazole, benzimidazole, 1,2,4-triazole, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-tert-amylphenyl)benzotriazole, 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-tert-octylphenol], 6-(2-benzotriazolyl)-4-tert-octyl-6'-tert-butyl-4'-methyl-2,2'-methylenebisphenol, 1,2,3-benzotriazolyl benzotriazole, 1-[N,N-bis(2-ethylhexyl)aminomethyl]benzotriazole, carboxybenzotriazole, 1-[N,N-bis(2-ethylhexyl)aminomethyl]methylbenzotriazole, 2,2'-[[(methyl-1H-benzotriazol-1-yl)methyl]imino]bisethanol, 1-(1',2'-dicarboxyethyl)benzotriazole, 1-(2,3-dicarboxypropyl)benzotriazole, 1-[(2-ethylhexylamino)methyl]benzotriazole, 2,6-bis[(1H-benzotriazol-1-yl)methyl]-4-methylphenol, 5-methylbenzotriazole, 5-phenyltetrazole, and the like.
[0098] Examples of guanidines include 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, 1-o-tolylbiguanide, 1,3-di-o-cumenylguanidine, and 1,3-di-o-cumenyl-2-propionylguanidine.
[0099] Examples of alkylamine compounds include ethylamine, triethylamine, ethylenediamine, triethylenetetramine, cyclohexylamine, hexadecylamine, and stearylamine.
[0100] Examples of the amino alcohol compound include alkanolamines such as 1-amino-2-propanol and N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine.
[0101] When using amines, one type may be used alone, or two or more types may be used in combination. Among the above, azoles and guanidines are preferably used as the amines. Among azoles, phenyl-substituted imidazoles are preferred, and 2-phenyl-4-methylimidazole is particularly preferred, as this helps to suppress an increase in the viscosity of the solder paste. Among guanidines, 1,3-di-o-tolylguanidine is particularly preferred. The amines used in the flux of this embodiment are preferably a combination of azoles and guanidines, such as a combination of 2-phenyl-4-methylimidazole and 1,3-di-o-tolylguanidine.
[0102] When an amine other than the above-mentioned compound having a benzotriazole skeleton is used, the content of the amine (excluding those corresponding to the above-mentioned compound having a benzotriazole skeleton) in the flux is preferably 4% by mass or more and 15% by mass or less, more preferably 5% by mass or more and 12% by mass or less, and even more preferably 6% by mass or more and 10% by mass or less, relative to the total amount (100% by mass) of the flux. When the amine content is equal to or greater than the lower limit of the above-mentioned preferred range, an increase in the viscosity of the solder paste is easily suppressed, while when the amine content is equal to or less than the upper limit of the above-mentioned preferred range, the cohesion of the solder alloy powder during reflow is easily enhanced.
[0103] Regarding organic acids other than dicarboxylic acids, examples of organic acids other than dicarboxylic acids include carboxylic acids and organic sulfonic acids. Examples of the carboxylic acids include aliphatic carboxylic acids and aromatic carboxylic acids. Examples of the aliphatic carboxylic acids include aliphatic monocarboxylic acids.
[0104] Examples of aliphatic monocarboxylic acids include caproic acid, enanthic acid, caprylic acid, pelargonic acid, isopelargonic acid, capric acid, caproleic acid, lauric acid (dodecanoic acid), undecanoic acid, linderic acid, tridecanoic acid, myristoleic acid, pentadecanoic acid, isopalmitic acid, palmitoleic acid, hiragonic acid, hydnocarpic acid, margaric acid, isostearic acid, elaidic acid, petroselinic acid, moroctic acid, eleostearic acid, talic acid, vaccenic acid, riminoleic acid, vernolic acid, sterculic acid, nonadecanoic acid, eicosanoic acid, stearic acid, 12-hydroxystearic acid, oleic acid, linoleic acid, linolenic acid, myristic acid, 2,2-bis(hydroxymethyl)propionic acid, 2,2-bis(hydroxymethyl)butanoic acid, and the like. Examples of aromatic carboxylic acids include salicylic acid, parahydroxyphenylacetic acid, benzoic acid, 2,3-dihydroxybenzoic acid, 2-quinolinecarboxylic acid, 3-hydroxybenzoic acid, p-anisic acid, picolinic acid, and 3-hydroxypicolinic acid.
[0105] Examples of organic sulfonic acids include aliphatic sulfonic acids, aromatic sulfonic acids, etc. Examples of aliphatic sulfonic acids include alkanesulfonic acids, alkanolsulfonic acids, etc.
[0106] Examples of alkane sulfonic acids include methanesulfonic acid, ethanesulfonic acid, 1-propanesulfonic acid, 2-propanesulfonic acid, 1-butanesulfonic acid, 2-butanesulfonic acid, pentanesulfonic acid, hexanesulfonic acid, decanesulfonic acid, dodecanesulfonic acid, etc. Examples of alkanol sulfonic acids include 2-hydroxyethane-1-sulfonic acid, 2-hydroxypropane-1-sulfonic acid, 2-hydroxybutane-1-sulfonic acid, 2-hydroxypentane-1-sulfonic acid, 1-hydroxypropane-2-sulfonic acid, 3-hydroxypropane-1-sulfonic acid, 4-hydroxybutane-1-sulfonic acid, 2-hydroxyhexane-1-sulfonic acid, 2-hydroxydecane-1-sulfonic acid, and 2-hydroxydodecane-1-sulfonic acid. Examples of aromatic sulfonic acids include 1-naphthalenesulfonic acid, 2-naphthalenesulfonic acid, p-toluenesulfonic acid, xylenesulfonic acid, p-phenolsulfonic acid, cresolsulfonic acid, sulfosalicylic acid, nitrobenzenesulfonic acid, sulfobenzoic acid, and diphenylamine-4-sulfonic acid.
[0107] When using an organic acid other than dicarboxylic acid, one type may be used alone or two or more types may be used in combination. However, in the flux of this embodiment, the effect of dicarboxylic acid is sufficiently high and from the viewpoint of reducing flux residue, it is preferable that no organic acid other than dicarboxylic acid is contained.
[0108] Regarding Halogen Compounds Examples of halogen compounds include amine hydrohalides and organic halogen compounds other than amine hydrohalides.
[0109] Amine hydrohalides are compounds obtained by reacting an amine with a hydrogen halide. Examples of the amine include aliphatic amines, azoles, and guanidines. Examples of the hydrogen halide include chlorine, bromine, and iodine hydrides. Examples of the aliphatic amine include ethylamine, diethylamine, triethylamine, and ethylenediamine. Examples of the guanidines and azoles include those exemplified in the above description of amines.
[0110] Examples of organic halogen compounds other than amine hydrohalides include halogenated aliphatic compounds. A halogenated aliphatic hydrocarbon group refers to an aliphatic hydrocarbon group in which some or all of the hydrogen atoms constituting the group have been substituted with halogen atoms. Examples of halogenated aliphatic compounds include halogenated aliphatic alcohols and halogenated heterocyclic compounds.
[0111] When a halogen compound is used, one type may be used alone, or two or more types may be used in combination. However, it is preferable that the flux of this embodiment does not contain a halogen compound, since this makes it easier to suppress an increase in the viscosity of the solder paste.
[0112] <<Resin Components Other Than Rosin>> Examples of resin components other than rosin-based resins include terpene resins, modified terpene resins, terpene phenolic resins, modified terpene phenolic resins, styrene resins, modified styrene resins, xylene resins, modified xylene resins, acrylic resins, polyethylene resins, acrylic-polyethylene copolymer resins, and epoxy resins. Examples of modified terpene resins include aromatic modified terpene resins, hydrogenated terpene resins, and hydrogenated aromatic modified terpene resins. Examples of modified terpene phenolic resins include hydrogenated terpene phenolic resins. Examples of modified styrene resins include styrene-acrylic resins and styrene-maleic acid resins. Examples of modified xylene resins include phenol-modified xylene resins, alkylphenol-modified xylene resins, phenol-modified resol-type xylene resins, polyol-modified xylene resins, and polyoxyethylene-added xylene resins.
[0113] <<Metal Deactivator>> Examples of metal deactivators include hindered phenol compounds and nitrogen compounds. The term "metal deactivator" as used herein refers to a compound that has the ability to prevent metals from deteriorating due to contact with certain compounds. A hindered phenol compound refers to a phenol compound having a bulky substituent (e.g., a branched or cyclic alkyl group such as a t-butyl group) on at least one of the ortho positions of the phenol. Examples of nitrogen compounds in metal deactivators include hydrazide nitrogen compounds, amide nitrogen compounds, triazole nitrogen compounds, and melamine nitrogen compounds.
[0114] <<Surfactants>> Examples of surfactants include nonionic surfactants and cationic surfactants. Examples of nonionic surfactants include aliphatic alcohol polyoxyethylene adducts, aromatic alcohol polyoxyethylene adducts, polyhydric alcohol polyoxyethylene adducts, aliphatic alcohol polyoxypropylene adducts, aromatic alcohol polyoxypropylene adducts, and polyhydric alcohol polyoxypropylene adducts. Examples of cationic surfactants include diamine-terminated polyethylene glycol, diamine-terminated polyethylene glycol-polypropylene glycol copolymers, aliphatic amine polyoxyethylene adducts, aromatic amine polyoxyethylene adducts, polyvalent amine polyoxyethylene adducts, and polyvalent amine polyoxypropylene adducts.
[0115] As explained above, the flux of this embodiment uses, in addition to rosin, a solvent, a thixotropic agent, a dicarboxylic acid, and a compound having a benzotriazole skeleton, a polymer (P) having a repeating unit represented by general formula (p1). The use of this polymer (P), although the reason is unclear, makes it possible to provide a flux that has good stability over time, with high cohesion of the solder alloy powder during reflow, suppressing blackening of the flux residue, and being less susceptible to precipitation over time.
[0116] Another embodiment of the flux contains a solvent containing monoalkyl propylene glycol. Use of this flux suppresses changes in the viscosity (thickening) of the solder paste. Furthermore, by controlling the mixing ratio of the monoalkyl propylene glycol and the polymer (P), it is possible to easily achieve both suppression of the precipitation of compounds having a benzotriazole skeleton in the flux and suppression of an increase in the viscosity of the solder paste.
[0117] (Solder Paste) One embodiment of the solder paste contains a solder alloy powder and the flux of the above-described embodiment. The solder alloy constituting the solder alloy powder can be a solder alloy of known composition. The solder alloy may be a solder containing only Sn, or a solder alloy such as Sn—Ag, Sn—Cu, Sn—Ag—Cu, Sn—Bi, or Sn—In, or an alloy of these to which Sb, Bi, In, Cu, Zn, As, Ag, Cd, Fe, Ni, Co, Au, Ge, or P is added. The solder alloy may be a Sn—Pb solder alloy or a Sn—Pb solder alloy to which Sb, Bi, In, Cu, Zn, As, Ag, Cd, Fe, Ni, Co, Au, Ge, or P is added. The solder alloy is preferably a solder alloy that does not contain Pb, and more preferably a solder alloy that contains Sn and Bi.
[0118] The soldering conditions in the soldering step may be appropriately set depending on the melting point of the solder alloy. For example, when a Sn—Ag—Cu solder alloy is used, the molten solder temperature is preferably 230 to 280° C., and more preferably 250 to 270° C. Alternatively, when a Sn—Bi solder alloy (a solder alloy containing Sn and Bi) is used, the molten solder temperature is preferably 170 to 220° C., and more preferably 180 to 200° C.
[0119] Flux Content: The flux content in the solder paste of this embodiment is preferably 5 to 30 mass % and more preferably 5 to 15 mass % relative to the total mass of the solder paste.
[0120] The solder paste of the present embodiment described above uses the flux of the above-described embodiment, which results in high cohesion of the solder alloy powder during reflow (suppressing the generation of solder balls) and suppressing blackening of the flux residue. In addition, the solder paste of the present embodiment provides good wetting and spreading properties onto the lands, suppresses changes in the viscosity (thickening) of the solder paste, and improves stability over time (suppressing flux separation over time). Furthermore, the solder paste of the present embodiment uses the flux of the above-described embodiment, which makes it particularly suitable for use when a solder alloy containing Sn and Bi (a so-called low-temperature solder) is used as the solder alloy powder.
[0121] As another embodiment of the flux and solder paste, the following configurations can also be adopted.
[0122]
[21] A flux containing rosin, a polymer (P) having a repeating unit represented by the following general formula (p1), a solvent, a thixotropic agent containing polyamide, a dicarboxylic acid represented by the following general formula (c1), and a compound having a benzotriazole skeleton selected from the group consisting of a compound represented by the following general formula (AZ1-1) and a compound represented by the following general formula (AZ1-2):
[0123] [In the formula, R 1 is a methyl group or a hydrogen atom. 2 is a hydrocarbon group having 1 to 2 carbon atoms or a hydrogen atom.
[0124] [In the formula, R represents an alkylene group having 1 to 10 carbon atoms, a phenylene group, or a single bond, provided that a methylene group constituting the alkylene group may be substituted with an oxygen atom.]
[0125] [In the formula, R 11 is an organic group or a hydrogen atom. 12 is a substituent. n1 represents an integer of 0 to 4. R 21 is an organic group or a hydrogen atom. 22 is a substituent. n2 represents an integer of 0 to 4.
[0126]
[22] The flux according to
[21] above, wherein the weight average molecular weight of the polymer (P) is 300 to 8000.
[23] The flux according to
[21] above or
[22] above, wherein the content of the polymer (P) is 1 mass % or more and 15 mass % or less with respect to the total mass of the flux.
[0127]
[24] The flux according to any one of
[21] to
[23] , wherein the solvent contains a monoalkyl propylene glycol.
[25] The flux according to
[24] , wherein the monoalkyl propylene glycol contains at least one selected from the group consisting of butyl propylene triglycol and butyl propylene diglycol.
[0128]
[26] The flux according to
[24] or
[25] , wherein the content of the monoalkyl propylene glycol is 5% by mass or more and 50% by mass or less with respect to the total mass of the flux.
[0129]
[27] The flux according to any one of
[24] to
[26] , wherein the mixing ratio of the polymer (P) and the monoalkyl propylene glycol is 0.05 or more as a mass ratio represented by polymer (P) / monoalkyl propylene glycol.
[0130]
[28] The flux according to any one of
[21] to
[27] , wherein the content of the dicarboxylic acid is 0.5 mass% or more and 7.5 mass% or less with respect to the total mass of the flux.
[29] The flux according to any one of
[21] to
[28] , wherein the content of the compound having a benzotriazole skeleton is 1 mass% or more and 10 mass% or less with respect to the total mass of the flux.
[0131]
[30] The flux according to any one of
[21] to
[29] , wherein a mixing ratio of the dicarboxylic acid and the compound having a benzotriazole skeleton is 0.2 or more and 3 or less as a mass ratio expressed as dicarboxylic acid / compound having a benzotriazole skeleton.
[0132]
[31] The flux according to any one of
[21] to
[30] , wherein the rosin content is 10 mass % or more and 40 mass % or less with respect to the total mass of the flux.
[32] The flux according to any one of
[21] to
[31] , wherein the rosin comprises at least one selected from the group consisting of acrylic acid-modified hydrogenated rosin, hydrogenated rosin, and polymerized rosin.
[0133]
[33] The flux according to any one of
[21] to
[32] , wherein the content of the thixotropic agent is 2 mass% or more and 15 mass% or less with respect to the total mass of the flux.
[0134]
[34] The flux according to
[21] , wherein, relative to the total mass (100 mass%) of the flux, the content of the rosin is 10 mass% or more and 40 mass% or less, the content of the polymer (P) is 1 mass% or more and 15 mass% or less, the content of the thixotropic agent is 2 mass% or more and 15 mass% or less, the content of the dicarboxylic acid is 0.5 mass% or more and 7.5 mass% or less, and the content of the compound having a benzotriazole skeleton is 1 mass% or more and 10 mass% or less.
[0135]
[35] The flux according to
[34] , wherein the weight average molecular weight of the polymer (P) is 300 to 8000.
[0136]
[36] The flux according to
[34] or
[35] , wherein the solvent contains a monoalkyl propylene glycol.
[37] The flux according to
[36] , wherein the monoalkyl propylene glycol contains at least one selected from the group consisting of butyl propylene triglycol and butyl propylene diglycol.
[0137]
[38] The flux according to
[36] or
[37] , wherein the content of the monoalkyl propylene glycol is 5% by mass or more and 50% by mass or less with respect to the total mass of the flux.
[0138]
[39] The flux according to any one of
[36] to
[38] , wherein the mixing ratio of the polymer (P) and the monoalkyl propylene glycol is 0.05 or more as a mass ratio represented by polymer (P) / monoalkyl propylene glycol.
[0139]
[40] The flux according to any one of
[34] to
[39] , wherein a mixing ratio of the dicarboxylic acid and the compound having a benzotriazole skeleton is 0.2 or more and 3 or less as a mass ratio expressed as dicarboxylic acid / compound having a benzotriazole skeleton.
[0140]
[41] The flux according to any one of
[34] to
[40] , wherein the rosin comprises at least one selected from the group consisting of acrylic acid-modified hydrogenated rosin, hydrogenated rosin, and polymerized rosin.
[0141]
[42] The flux according to any one of
[21] to
[41] above, further containing a phenyl-substituted imidazole.
[0142]
[43] The flux according to any one of
[21] to
[42] above, which does not contain a halogen compound.
[0143]
[44] A solder paste containing a solder alloy powder and the flux according to any one of
[21] to
[43] .
[45] The solder paste according to
[44] , wherein the solder alloy powder is made of a solder alloy containing Sn and Bi.
[0144] The present invention will be described below with reference to examples, but the present invention is not limited to the following examples.
[0145] <Preparation of Flux> (Examples 1 to 174, Comparative Examples 1 to 12) The fluxes of the examples and comparative examples were prepared with the compositions shown in Tables 1 to 31. In the tables, the content of each raw material indicates the ratio (mass%) to the total mass of the flux (100 mass%). The raw materials used are listed below.
[0146] Rosin: Acrylic acid modified hydrogenated rosin, hydrogenated rosin, and polymerized rosin were used.
[0147] Polymer (P) Having Repeating Units Represented by General Formula (p1) The following polybutenes (P1) to (P6) were used, which are copolymers having repeating units represented by the above chemical formula (p1-3) and repeating units represented by the chemical formula (p1-4). Polybutenes (P1) to (P6) are copolymers having a molecular structure of long-chain hydrocarbons, mainly isobutene, with some normal butene reacting. In addition, the following polybutadiene (P7) was used, which is a polymer having repeating units represented by the above chemical formula (p1-5). Polybutadiene (P7) is a homopolymer containing 90% or more repeating units represented by chemical formula (p1-5) and 10% or less repeating units represented by chemical formula (p2-4).
[0148] Polybutene (P1): weight average molecular weight 3370, number average molecular weight 1558; manufactured by ENEOS Corporation, trade name "Grade HV-300" Polybutene (P2): weight average molecular weight 345, number average molecular weight 332; manufactured by ENEOS Corporation, trade name "Grade LV-7" Polybutene (P3): weight average molecular weight 1130, number average molecular weight 689; manufactured by ENEOS Corporation, trade name "Grade HV-15" Polybutene (P4): weight average molecular weight 2114, number average molecular weight 944; manufactured by ENEOS Corporation, trade name "Grade HV-50" Polybutene (P5): weight average molecular weight 2578, number average molecular weight 1136; manufactured by ENEOS Corporation, trade name "Grade HV-100" Polybutene (P6): weight average molecular weight 7773, number average molecular weight 4808; manufactured by ENEOS Corporation, trade name "Grade HV-1900"
[0149] Polybutadiene (P7): weight average molecular weight 3991, number average molecular weight 2778; manufactured by Nippon Soda Co., Ltd., trade name "NISSO-PB B-2000"
[0150] [Method for measuring molecular weight of polymer (P)] The weight average molecular weight and number average molecular weight (in terms of polystyrene) of polymer (P) were measured by gel permeation chromatography (GPC) using a sample dissolved and diluted in tetrahydrofuran (THF). The measurement conditions were as follows:
[0151] Analytical apparatus: Waters e2695 Mobile phase: THF Column: Tosoh TSKguard column HXL (guard column) + Tosoh TSKgel G3000HXL + Tosoh TSKgel G2000HXL Column temperature: 40°C Flow rate: 1.0 (mL / min) Detector: RI detector, Po(+), Res(1.0 s) Injection volume: 50 μL Standard substance: Tosoh "GPC standard polystyrene kit PStQuick F" was used. Accordingly, the analysis results are converted into polystyrene equivalents.
[0152] Solvents: Butyl propylene triglycol, butyl propylene diglycol, butyl propylene (mono)glycol, and tetraethylene glycol dimethyl ether were used.
[0153] - Thixotropic agent: Polyamide and hydrogenated castor oil were used.
[0154] Dicarboxylic acids: Adipic acid, glutaric acid, diglycolic acid, succinic acid, sebacic acid, dodecanedioic acid, and phthalic acid were used.
[0155] - Monocarboxylic acid: Stearic acid was used.
[0156] Compounds having a benzotriazole skeleton: 1,2,3-benzotriazole, 5-methylbenzotriazole, and 2-(2'-hydroxy-5'-methylphenyl)benzotriazole were used.
[0157] Other Components Azoles and guanidines were used as amines. The azoles used were 2-ethylimidazole, 2-ethyl-4-methylimidazole, and 2-phenyl-4-methylimidazole. The guanidine used was 1,3-di-o-tolylguanidine.
[0158] <Preparation of Solder Paste> Each flux was mixed with the following solder alloy powder to prepare a solder paste. Each prepared solder paste contained 10.5 mass% flux and 89.5 mass% solder alloy powder. Solder alloy powder: Powder consisting of a solder alloy containing 58 mass% Bi and the remainder Sn. This solder alloy has a solidus temperature of 139°C and a liquidus temperature of 141°C. The size of the solder alloy powder (particle size distribution) satisfies symbol 4 in the powder size classification (Table 2) of JIS Z 3284-1:2014.
[0159] <Evaluation> As shown below, the following evaluations were performed: wettability, cohesion of the solder alloy powder (resistance to solder ball formation), stability over time (resistance to precipitation over time), change in viscosity of the solder paste (suppression of thickening), suppression of blackening of flux residue, and stability over time (flux separation over time). The results of these evaluations are shown in Tables 1 to 31.
[0160] The reflow profile used in the evaluation of this example is shown in Figure 1. The temperature inside the reflow furnace was increased from 50 to 130°C at a rate of 1.3 to 2.2°C / second. The temperature was maintained at 130 to 150°C for 60 to 90 seconds. The temperature was increased from 150 to 170°C at a rate of 0.4 to 1°C / second. After reaching 170°C, the temperature was allowed to cool and maintained for 30 to 90 seconds.
[0161] In each evaluation, the evaluation of the cohesion of the solder alloy powder (resistance to the generation of solder balls) was carried out in an atmosphere with an oxygen concentration of 1000 ppm. The other evaluations were carried out in the air.
[0162] [Evaluation of Wetting and Spreading Properties] In the evaluation of wetting and spreading properties, a Cu-OSP treated glass epoxy substrate was used as the substrate, with 41 lands, a land width of 0.27 mm, and a solder resist width of 0.37 mm.
[0163] Figure 2 is a schematic diagram illustrating the method for evaluating the wetting and spreading properties in this example. As shown in Figure 2, a single line of solder paste 20 was printed with a length of 0.3 mm and a mask thickness of 0.15 mm on top of lands 26 (light green) and solder resist 28 (dark green) formed on a substrate, and then reflow was performed. After reflow, the length of the solder alloy 22 that had spread and wetted the lands 26 was measured. The wetting and spreading properties were evaluated based on the following criteria.
[0164] Evaluation criteria Rank 1: The solder alloy 22 that has wetted and spread over the land 26 has an average length of 700 μm or more. Rank 2: The solder alloy 22 that has wetted and spread over the land 26 has an average length of 650 to less than 700 μm. Rank 3: The solder alloy 22 that has wetted and spread over the land 26 has an average length of 600 to less than 650 μm. Rank 4: The solder alloy 22 that has wetted and spread over the land 26 has an average length of less than 600 μm.
[0165] [Evaluation of cohesion of solder alloy powder (resistance to solder ball formation)] The cohesion of the solder alloy powder was evaluated as follows. A solder paste was printed on a ceramic plate with a diameter of 6.5 mm and a mask thickness of 0.20 mm, and reflow was performed. After reflow, the state of solder ball formation was confirmed. The cohesion of the solder alloy powder (resistance to solder ball formation) was evaluated based on the following criteria.
[0166] Evaluation criteria Rank 1: After melting, the solder alloy powder aggregates into one large sphere. Fewer than 15 solder alloy particles with a particle diameter of 150 μm or less were observed around the large sphere. Rank 2: After melting, the solder alloy powder aggregates into one large sphere. Fewer than 15 but less than 30 solder alloy particles with a particle diameter of 150 μm or less were observed around the large sphere. Rank 3: After melting, the solder alloy powder aggregates into one large sphere. Fewer than 30 but less than 40 solder alloy particles with a particle diameter of 150 μm or less were observed around the large sphere. Rank 4: After melting, the solder alloy powder aggregates into one large sphere. Fewer than 40 solder alloy particles with a particle diameter of 150 μm or less were observed around the large sphere, or solder alloy particles with a particle diameter exceeding 150 μm were observed, or non-aggregated solder alloy particles were observed.
[0167] [Evaluation of temporal stability (resistance to precipitation over time)] The temporal stability (resistance to precipitation over time) was evaluated as follows. The flux was stored at a temperature of 25°C and a relative humidity of 50%. After one week, one month, two months, and three months of storage, the flux was printed on a glass slide with a thickness of 100 μm to check for precipitation. The temporal stability (resistance to precipitation over time) was evaluated based on the following criteria.
[0168] Evaluation criteria Rank 1: No precipitate was observed after 3 months of storage. Rank 2: No precipitate was observed after 2 months of storage. Rank 3: No precipitate was observed after 1 month of storage. Rank 4: Precipitation was observed after 1 week of storage (i.e., precipitation occurred within 1 week).
[0169] [Evaluation of viscosity change (thickening suppression) of solder paste] Evaluation of viscosity change of the solder paste was carried out in accordance with JIS Z 3284-3:2014 "4.2 Viscosity characteristic test." A Malcom PCU-205 viscometer was used. The measurement conditions were a temperature of 25°C, a rotation speed of 10 rpm, and the initial viscosity was the viscosity 30 minutes after the start of measurement. The viscosity change (thickening suppression) of the solder paste was evaluated based on the following criteria.
[0170] Judgment criteria Rank 1: Viscosity 24 hours after the start of measurement is 1.05 times or less than the initial viscosity. Rank 2: Viscosity 12 hours after the start of measurement is 1.05 times or less than the initial viscosity. Rank 3: Viscosity 8 hours after the start of measurement is 1.05 times or less than the initial viscosity. Rank 4: Viscosity 8 hours after the start of measurement is more than 1.05 times the initial viscosity.
[0171] [Evaluation of suppression of blackening of flux residue] The suppression of blackening of flux residue was evaluated as follows. Solder paste was printed on a Cu-OSP substrate with a diameter of 5.0 mm and a mask thickness of 0.15 mm, and then left to stand for 2 hours at a temperature of 25°C and a relative humidity of 50%. Reflow was then performed, and the state of blackening of the flux residue was confirmed by binarization processing. The suppression of blackening of the flux residue was evaluated based on the following criteria. Figure 3 shows the state of blackened flux residue 34 remaining on the periphery of solder alloy 32 after reflow.
[0172] Judgment criteria In a plan view from above, Rank 1: The blackened area is 0% or more and less than 10% of the surface area of the flux residue 34. Rank 2: The blackened area is 10% or more and less than 30% of the surface area of the flux residue 34. Rank 3: The blackened area is 30% or more and less than 50% of the surface area of the flux residue 34. Rank 4: The blackened area is 50% or more of the surface area of the flux residue 34.
[0173] [Evaluation of temporal stability (flux separation over time)] The temporal stability (flux separation over time) was evaluated as follows. 2A container with a diameter of approximately 5.5 cm at the container opening was used. 500 g of solder paste was filled into this container and stored at a temperature of 25°C and a relative humidity of 50% for 7 days. After that, the area of the flux floating (separated) on the surface of the solder paste (the proportion of the separated flux occupying the container opening: area ratio) was confirmed. The stability over time (flux separation over time) was evaluated based on the following criteria. Figure 4 shows the state in which flux 44 is floating (separated) on the surface of solder paste 42 after the solder paste filled in container 40 has been stored for a predetermined period of time.
[0174] Judgment criteria Rank 1: No separation of flux 44. Rank 2: Separation of flux 44 occurred, with the separated flux 44 occupying more than 0% and less than 10% of the area of the container opening. Rank 3: Separation of flux 44 occurred, with the separated flux 44 occupying 10% or more and less than 30% of the area of the container opening. Rank 4: Separation of flux 44 occurred, with the separated flux 44 occupying 30% or more of the area of the container opening.
[0175]
[0176] From the results shown in Table 1, it can be confirmed that when the flux of Example 1 to which the present invention is applied is used, the cohesion of the solder alloy powder during reflow (less likely to generate solder balls) is high, the blackening of the flux residue is suppressed, and precipitation over time is less likely to occur, resulting in good stability over time.
[0177] On the other hand, when the flux of Comparative Example 1 lacking a dicarboxylic acid was used, the evaluation of the cohesion of the solder alloy powder was poor. When the flux of Comparative Example 4 containing a monocarboxylic acid instead of a dicarboxylic acid was used, the evaluation of the cohesion of the solder alloy powder was also poor. When the flux of Comparative Example 2 lacking a compound having a benzotriazole skeleton was used, the evaluation of the suppression of blackening of the flux residue was poor. When the flux of Comparative Example 3 lacking a polymer (P) was used, the evaluation of the stability over time (the resistance to precipitation over time) was poor.
[0178]
[0179] In Table 2, the results for the flux of Comparative Example 5 confirm that dicarboxylic acid is an effective activator for the flux in preventing the coagulation of the solder alloy powder, but on the other hand, the evaluation of suppressing blackening of the flux residue is poor. The results for the flux of Comparative Example 6 confirm that a compound having a benzotriazole skeleton is effective in preventing the blackening of the flux residue, but on the other hand, the evaluation of stability over time (resistance to precipitation over time) is poor. In contrast, the results for the fluxes of Examples 1 and 15 confirm that the use of polymer (P) in combination improves the evaluation of coagulation of the solder alloy powder, suppression of blackening of the flux residue, and stability over time (resistance to precipitation over time).
[0180]
[0181] In Table 3, a comparison of Example 1 and Example 34 confirms that the inclusion of monoalkylpropylene glycol as a solvent can further reduce the viscosity change of the solder paste (enhancing the effect of suppressing thickening). When the flux of Comparative Example 7, which lacks both polymer (P) and monoalkylpropylene glycol, was used, the evaluation results were poor in both stability over time (resistance to precipitation over time) and viscosity change of the solder paste (suppression of thickening).
[0182]
[0183]
[0184] The results shown in Tables 4 and 5 confirm that when the fluxes of Examples 1 to 15 to which the present invention is applied are used, the solder alloy powder exhibits high cohesion during reflow, the blackening of the flux residue is suppressed, and precipitation over time is unlikely to occur, resulting in good stability over time.Comparing Examples 1, 5, and 7, it can be confirmed that by using a monoalkyl propylene glycol selected from the group consisting of butyl propylene triglycol and butyl propylene diglycol as the solvent, the viscosity change of the solder paste can be further reduced (the effect of suppressing thickening can be enhanced).
[0185]
[0186]
[0187]
[0188]
[0189]
[0190]
[0191]
[0192] From the results shown in Tables 6 to 12, it can be confirmed that when the content of monoalkyl propylene glycol is 5% by mass or more, preferably 10% by mass or more, and more preferably more than 10% by mass, the change in viscosity of the solder paste can be made smaller (the effect of suppressing thickening can be improved).
[0193] From the results shown in Tables 6 to 12, it can be confirmed that when the mass ratio represented by polymer (P) / monoalkyl propylene glycol is 0.05 or more, precipitation of the compound having a benzotriazole skeleton in the flux is easily suppressed, and the temporal stability (the degree to which precipitation does not occur over time) is improved.
[0194]
[0195]
[0196] When the fluxes of Examples 59 to 70, which apply the present invention, are used, it can be confirmed that the cohesion of the solder alloy powder during reflow (resistance to the generation of solder balls) is high, blackening of the flux residue is suppressed, and precipitation over time is unlikely to occur, resulting in good stability over time.When the flux of Comparative Example 8, which lacks dicarboxylic acid, is used, the evaluation of the cohesion of the solder alloy powder was poor.
[0197]
[0198] When the fluxes of Examples 71 to 76 were used, it was confirmed that the solder alloy powder had high cohesion during reflow (less likely to form solder balls), the blackening of the flux residue was suppressed, and precipitation over time was less likely to occur, resulting in good stability over time.When the flux of Comparative Example 9, which lacked a compound having a benzotriazole skeleton, was used, the evaluation of the suppression of blackening of the flux residue was poor.
[0199]
[0200] When the fluxes of Examples 77 to 80 to which the present invention is applied are used, it can be confirmed that the cohesion of the solder alloy powder during reflow (less likely to generate solder balls) is high, the blackening of the flux residue is suppressed, and precipitation over time is less likely to occur, resulting in good stability over time.
[0201]
[0202] When the fluxes of Examples 81 to 90 to which the present invention is applied are used, it can be confirmed that the cohesion of the solder alloy powder during reflow (resistance to the generation of solder balls) is high, blackening of the flux residue is suppressed, and precipitation over time is unlikely to occur, resulting in good stability over time.When the flux of Comparative Example 10, which lacks polymer (P), is used, the evaluation of stability over time (resistance to precipitation over time) was poor.
[0203]
[0204]
[0205]
[0206]
[0207]
[0208]
[0209]
[0210] When the fluxes of Examples 91 to 133 to which the present invention is applied are used, it can be confirmed that the cohesion of the solder alloy powder during reflow (resistance to the generation of solder balls) is high, blackening of the flux residue is suppressed, and precipitation over time is unlikely to occur, resulting in good stability over time.When the flux of Comparative Example 11, which lacks polymer (P), is used, the evaluation of stability over time (resistance to precipitation over time) was poor.
[0211]
[0212]
[0213]
[0214]
[0215]
[0216]
[0217]
[0218] When the fluxes of Examples 134 to 174 to which the present invention is applied are used, it can be confirmed that the cohesion of the solder alloy powder during reflow (resistance to the generation of solder balls) is high, blackening of the flux residue is suppressed, and precipitation over time is unlikely to occur, resulting in good stability over time.When the flux of Comparative Example 12, which lacks polymer (P), is used, the evaluation of stability over time (resistance to precipitation over time) was poor.
[0219] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to these embodiments. Addition, omission, substitution, and other modifications of the configuration are possible within the scope of the spirit of the present invention. The present invention is not limited by the above description, but is limited only by the scope of the appended claims.
[0220] 20 solder paste, 22 solder alloy, 26 land, 28 solder resist, 32 solder alloy, 34 flux residue, 40 container, 42 solder paste, 44 flux
Claims
1. A flux comprising: rosin; a polymer (P) having a repeating unit represented by the following general formula (p1); a solvent; a thixotropic agent containing polyamide; a dicarboxylic acid represented by the following general formula (c1); and a compound having a benzotriazole skeleton selected from the group consisting of a compound represented by the following general formula (AZ1-1) and a compound represented by the following general formula (AZ1-2). [In the formula, R 1 is a methyl group or a hydrogen atom. 2 is a hydrocarbon group having 1 to 2 carbon atoms or a hydrogen atom. [In the formula, R represents an alkylene group having 1 to 10 carbon atoms, a phenylene group, or a single bond. However, a methylene group constituting the alkylene group may be substituted with an oxygen atom.] [In the formula, R 11 R is an organic group or a hydrogen atom. 12 is a substituent. n1 represents an integer of 0 to 4. R 21 R is an organic group or a hydrogen atom. 22 is a substituent. n2 represents an integer of 0 to 4.] 2. The flux according to claim 1, wherein the weight average molecular weight of the polymer (P) is 300 to 8,000.
3. The flux according to claim 1, wherein the content of the polymer (P) is 1 mass % or more and 15 mass % or less with respect to the total mass of the flux.
4. The flux of claim 1, wherein the solvent comprises a monoalkyl propylene glycol.
5. The flux according to claim 4, wherein the monoalkyl propylene glycol comprises at least one member selected from the group consisting of butyl propylene triglycol and butyl propylene diglycol.
6. The flux according to claim 4, wherein the content of the monoalkyl propylene glycol is 5% by mass or more and 50% by mass or less based on the total mass of the flux.
7. The flux according to claim 4, wherein a mixing ratio of the polymer (P) to the monoalkyl propylene glycol is 0.05 or more as a mass ratio expressed as polymer (P) / monoalkyl propylene glycol.
8. The flux according to claim 1, wherein the content of the dicarboxylic acid is 0.5 mass % or more and 7.5 mass % or less based on the total mass of the flux.
9. The flux according to claim 1, wherein the content of the compound having a benzotriazole skeleton is 1 mass % or more and 10 mass % or less with respect to the total mass of the flux.
10. The flux according to claim 1, wherein a mixing ratio of the dicarboxylic acid to the compound having a benzotriazole skeleton is from 0.2 to 3 in mass ratio (dicarboxylic acid / compound having a benzotriazole skeleton).
11. The flux according to claim 1, wherein the rosin content is 10 mass % or more and 40 mass % or less with respect to the total mass of the flux.
12. The flux according to claim 1, wherein the rosin comprises at least one selected from the group consisting of acrylic acid modified hydrogenated rosin, hydrogenated rosin, and polymerized rosin.
13. The flux according to claim 1, wherein the content of the thixotropic agent is 2 mass % or more and 15 mass % or less with respect to the total mass of the flux.
14. The flux of claim 1 further comprising a phenyl-substituted imidazole.
15. The flux of claim 1 which is halide-free.
16. A solder paste comprising a solder alloy powder and the flux according to any one of claims 1 to 15.
17. The solder paste according to claim 16, wherein the solder alloy powder is made of a solder alloy containing Sn and Bi.
Citation Information
Patent Citations
Impact tool
JP2023090350A
Flux and method for manufacturing joint body
JP7075028B1
Flux for resin flux-cored solder, flux for flux coat solder, flux-cored solder and flux coat solder
JP2018202465A
Solder composition and electronic substrate
JP2022054100A
Flux and solder paste
JP7141009B1