Thermally conductive composition, thermally conductive sheet using same, and production method therefor
The thermally conductive composition, featuring a matrix resin and specific particle combinations, addresses the issue of high plasticity in conventional sheets by achieving high thermal conductivity and low plasticity, ensuring effective heat dissipation and moldability in thermally conductive sheets.
Patent Information
- Application Number
- PCT/JP2024/014209
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-11-17
- Filing Date
- 2024-04-08
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional thermally conductive compositions and sheets face the challenge of increased thermal conductivity leading to poor moldability due to high plasticity, as adding large amounts of conductive particles deteriorates moldability.
A thermally conductive composition comprising a matrix resin, thermosetting resin, curing catalyst, and a combination of alumina and aluminum nitride particles with specific size distributions and ratios, which is vacuum-defoamed, rolled, and cured to form a sheet with high thermal conductivity and low plasticity.
The solution achieves a thermally conductive sheet with high thermal conductivity (14 W/m·K or more) and low plasticity, enabling good moldability and continuous sheet molding, suitable for use as a thermal interface material.
Smart Images

Figure JP2024014209_05122024_PF_FP_ABST
Abstract
Description
Thermally conductive composition, thermally conductive sheet using the same, and method for manufacturing the same
[0001] The present invention relates to a thermally conductive composition suitable for being interposed between a heat-generating portion of an electric or electronic component or the like and a heat sink, a thermally conductive sheet using the same, and a method for producing the same.
[0002] In recent years, the performance of semiconductors such as CPUs has improved dramatically, resulting in enormous increases in the amount of heat generated. For this reason, heat-generating electronic components are fitted with heat sinks, and thermally conductive sheets are used to improve adhesion between the semiconductor and the heat sink. As devices become smaller, more powerful, and more highly integrated, thermally conductive sheets are required to be soft and have high thermal conductivity. Patent documents 1 to 4, among others, have proposed thermally conductive sheets. Furthermore, the present applicant has proposed a thermally conductive sheet with high thermal conductivity in Patent document 5.
[0003] JP 2021-518466 A Re-table 2020-137970 A Re-table 2018-088416 A JP 2016-216523 A Patent No. 7061736 A
[0004] However, conventional thermally conductive compositions and thermally conductive sheets using the same have the problem that increasing the thermal conductivity increases the plasticity of the composition, resulting in poor moldability. This is because increasing the thermal conductivity requires adding a large amount of thermally conductive particles, which increases the plasticity of the composition and deteriorates moldability.
[0005] In order to solve the above-mentioned conventional problems, the present invention provides a thermally conductive composition having high thermal conductivity, low plasticity of the composition, and good moldability, as well as a thermally conductive sheet using the same and a method for producing the same.
[0006] The thermally conductive composition of the present invention is a thermally conductive composition comprising a matrix resin (component A) made of a thermosetting resin, a curing catalyst, and thermally conductive particles, the thermally conductive particles comprising the following components B and C: (1) component B: alumina having a D50 (median diameter) of 0.01 μm or more and less than 1 μm in a cumulative particle size distribution on a volume basis is contained in an amount of 220 to 500 parts by mass per 100 parts by mass of the matrix resin, and the following components B-1 and B-2 are contained: component B-1: alumina having a D50 (median diameter) of 0.01 μm or more and less than 0.3 μm, a BET specific surface area of 9 m 2 / g or more is 30 to 100 mass% relative to 100 mass% of component B, component B-2: alumina having a D50 (median diameter) of 0.3 μm or more and less than 1 μm is 0 to 70 mass% relative to 100 mass% of component B, (2) component C: contains 1900 to 2500 mass parts of aluminum nitride having a D50 (median diameter) of 0.01 μm or more and 150 μm or less relative to 100 mass parts of matrix resin, and contains the following components C-1 and C-2, component C-1: D50 (median diameter) is 0.01 μm or more and less than 30 μm, component C-2: D50 (median diameter) is 30 μm or more and 150 μm or less.
[0007] The thermally conductive sheet of the present invention is characterized in that the thermally conductive composition is formed into a sheet. The method for producing the thermally conductive sheet of the present invention comprises vacuum degassing the thermally conductive composition, rolling it, forming it into a sheet, and then heat curing it to produce the thermally conductive sheet.
[0008] By using the above composition, the present invention can provide a thermally conductive composition having high thermal conductivity, low plasticity, and good moldability, and a thermally conductive sheet using the same. Specifically, by specifying the type, particle size, and amount of conductive particles, a thermally conductive composition having high thermal conductivity, low plasticity, and good moldability can be obtained. Specifically, the plasticity of the thermally conductive composition after degassing before curing is preferably less than 100, and the preferred thermal conductivity is 14 W / m·K or higher. Furthermore, the method for producing a thermally conductive sheet of the present invention enables continuous sheet molding because the composition has low plasticity and good moldability.
[0009] Fig. 1 is a schematic cross-sectional view showing a method for using a thermally conductive sheet according to one embodiment of the present invention. Figs. 2A and 2B are schematic explanatory views showing a method for measuring the thermal conductivity of a sample according to one embodiment of the present invention.
[0010] The present invention relates to a thermally conductive composition comprising a matrix resin, a curing catalyst, and thermally conductive particles. The matrix resin is preferably a thermosetting resin such as silicone rubber, silicone gel, acrylic rubber, fluororubber, epoxy resin, phenolic resin, unsaturated polyester resin, melamine resin, acrylic resin, silicone resin, or fluororesin. Among these, silicone is preferred, and examples thereof include elastomers, gels, putties, and greases. Any method, such as peroxide, addition, or condensation, may be used for the silicone curing system. Silicone is preferred because of its high heat resistance. Furthermore, addition reaction type resins are preferred because they are non-corrosive to the surrounding area, emit minimal by-products outside the system, and cure deeply.
[0011] The thermally conductive particles are as follows for 100 parts by mass of matrix resin (component A): (1) Component B: 220 to 500 parts by mass of alumina having a D50 (median diameter) of 0.01 μm or more and less than 1 μm in the cumulative particle size distribution on a volume basis is added for 100 parts by mass of matrix resin. The preferred amount is 230 to 480 parts by mass, and more preferably 240 to 440 parts by mass. Component B also includes the following components B-1 and B-2: Component B-1: D50 (median diameter) of 0.01 μm or more and less than 0.3 μm, BET specific surface area of 9 m 2 / g or more of alumina is 30 to 100 mass % relative to 100 mass % of component B. The preferred D50 (median diameter) is 0.1 μm or more and less than 0.3 μm. The preferred BET specific surface area is 9 to 20 m 2 / g, and more preferably 10 to 18m 2 / g. The BET specific surface area is measured according to the standards of JIS R 1626-1996. Component B-2: Alumina having a D50 (median diameter) of 0.3 μm or more and less than 1 μm accounts for 0 to 70 mass% of Component B (100 mass%). The preferred D50 (median diameter) is 0.3 μm or more and 1.0 μm or less. (2) Component C: Aluminum nitride having a D50 (median diameter) of 0.01 μm or more and 150 μm or less is added in an amount of 1900 to 2500 mass parts per 100 mass parts of matrix resin. The preferred D50 (median diameter) is 0.1 μm or more and 120 μm or less. The preferred amount added is 1920 to 2400 mass parts, and more preferably 1940 to 2300 mass parts. Component C includes the following components C-1 and C-2. C-1 component: D50 (median diameter) is 0.01 μm or more and less than 30 μm. C-2 component: D50 (median diameter) is 30 μm or more and 150 μm or less.
[0012] In the present invention, the thermally conductive particles are a mixture of multiple types of inorganic particles with different average particle sizes, which allows the thermally conductive inorganic particles with smaller particle sizes to be embedded between the larger particles, resulting in a nearly close-packed state, resulting in a thermally conductive composition with high thermal conductivity, low plasticity, and good moldability.
[0013] The ratio of the C-1 component to the C-2 component, in terms of mass ratio, is preferably C-2 component ≦ C-1 component, and more preferably C-2 component < C-1 component. This results in a thermally conductive composition with high thermal conductivity, low plasticity, and good moldability. Furthermore, the plasticity of the thermally conductive composition after vacuum degassing before curing is preferably less than 100, more preferably 10 to 99, even more preferably 20 to 99, and particularly preferably 30 to 99. This results in a thermally conductive composition with low plasticity and good moldability. Plasticity is measured in accordance with JIS K 6300-3, ISO 2007:1991 using a Wallace plastometer at a measurement temperature of 25°C. The thickness (t) of a sample compressed between two metal plates at a constant load (100 N) for a constant time (15 seconds) is divided by the thickness (t) before compression to obtain plasticity (P = t / t × 100). A smaller P indicates greater flexibility. Note that a smaller plasticity (P) value is synonymous with a lower plasticity.
[0014] The thermal conductivity of the cured product of the thermally conductive composition is preferably 14 W / m K or more, more preferably 14 to 20 W / m K, and even more preferably 14.5 to 20 W / m K. This provides high thermal conductivity and makes the composition suitable for use as a heat dissipation sheet: TIM (Thermal Interface Material).
[0015] The cured product of the thermally conductive composition preferably has a SHORE 00 hardness of 75 or less, more preferably 10 to 75, and even more preferably 15 to 72. This provides good conformability to heat generating bodies and heat dissipating bodies (heat sinks).
[0016] The matrix resin is preferably at least one selected from addition-curable silicone polymers, peroxide-curable silicone polymers, and condensation-curable silicone polymers.
[0017] Preferably, 0.1 to 10 parts by mass, more preferably 0.5 to 7 parts by mass, of a silane coupling agent is added to 100 parts by mass of the matrix resin. The silane coupling agent coats the surface of the thermally conductive particles (surface treatment), making them easier to fill into the matrix resin (plasticizer function), and also has the effect of preventing the curing catalyst from being adsorbed onto the thermally conductive particles, preventing curing inhibition. This is useful for storage stability. The silane coupling agent is R(CH3) a Si(OR') 4-a (R is an unsubstituted or substituted organic group having 1 to 20 carbon atoms, R' is an alkyl group having 1 to 4 carbon atoms, and a is 0 or 1), or a partial hydrolyzate thereof. a Si(OR') 4-a Examples of alkoxysilane compounds (hereinafter simply referred to as "silanes") represented by the formula (R is an unsubstituted or substituted organic group having 1 to 20 carbon atoms, R' is an alkyl group having 1 to 4 carbon atoms, and a is 0 or 1) include methyltrimethoxysilane, ethyltrimethoxysilane, propyltrimethoxysilane, butyltrimethoxysilane, pentyltrimethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, octyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, dodecyltrimethoxysilane, dodecyltriethoxysilane, hexadecyltrimethoxysilane, hexadecyltriethoxysilane, octadecyltrimethoxysilane, and octadecyltriethoxysilane. These silane compounds can be used alone or in combination.
[0018] At least one component selected from the group consisting of alumina (aluminum oxide) as component B and aluminum nitride as component C is preferably in the form of irregularly pulverized particles. Irregularly pulverized particles are readily available. Hereinafter, "irregularly pulverized" may also be simply referred to as "irregular."
[0019] The thermally conductive composition of the present invention is preferably formed into a sheet to be a thermally conductive sheet, which is highly versatile and suitable as a TIM. The thickness of the thermally conductive sheet is preferably in the range of 0.2 to 10 mm.
[0020] In the method for producing a thermally conductive sheet of the present invention, the thermally conductive composition is vacuum degassed, rolled, formed into a sheet, and then heat-cured to form a thermally conductive sheet. Vacuum degassing involves reducing the pressure of the thermally conductive composition (compound) to -0.08 to -0.1 Pa and leaving it for approximately 5 to 10 minutes to degas the composition. Rolling can be performed by roll rolling or press working, but roll rolling is preferred because it allows for continuous production.
[0021] The thermally conductive composition preferably has a breakdown voltage (JIS K6249) of 7 to 16 kV / mm, thereby providing a thermally conductive sheet with high electrical insulation.
[0022] The volume resistivity (JIS K6249) of the thermally conductive composition is 10 10 ~10 14 It is preferable that the resistance is Ω·cm, which makes it possible to provide a thermally conductive sheet with high electrical insulation properties.
[0023] As an example of the present invention, in the case of an addition reaction type silicone composition (uncured composition), a compound having the following composition is preferred. A. Matrix Resin The matrix resin contains the following (A1) and (A2). (A1) Base Polymer Component: A linear organopolysiloxane containing at least two silicon-bonded alkenyl groups per molecule. (A2) Crosslinking Component: An organohydrogenpolysiloxane containing at least two silicon-bonded hydrogen atoms per molecule may contain an organopolysiloxane having no reactive groups other than components (A1) and (A2) in an amount less than 1 mole per mole of silicon-bonded alkenyl groups in component A. For example, unreacted silicone oil, such as dimethylpolysiloxane, is used. In this specification, the total amount of base polymer component (A1), crosslinking component (A2), unreacted silicone oil, and silane coupling agent is 100 parts by mass. B. Thermally Conductive Particles: As described above. C. Platinum-based metal catalyst: 0.01 to 1000 ppm by mass relative to the matrix resin. D. Other additives: silane coupling agent, curing retarder, colorant, etc.; optional amounts.
[0024] Each component is described below. (1) Base Polymer Component (Component A1) The base polymer component is an organopolysiloxane containing two or more silicon-bonded alkenyl groups per molecule. This organopolysiloxane contains two silicon-bonded alkenyl groups per molecule, such as vinyl or allyl groups, each having 2 to 8 carbon atoms, preferably 2 to 6 carbon atoms. From the standpoint of workability and curability, a viscosity of 10 to 1,000,000 mPa·s at 25°C, and particularly 100 to 100,000 mPa·s, is desirable. Specifically, an organopolysiloxane is used that contains two or more silicon-bonded alkenyl groups per molecule, each alkenyl group being represented by the following general formula (Chemical Formula 1): The side chains are linear organopolysiloxanes blocked with alkyl groups. A viscosity of 10 to 1,000,000 mPa·s at 25°C is desirable from the viewpoint of workability and curability. This linear organopolysiloxane may also contain a small amount of branched structure (trifunctional siloxane units) in the molecular chain.
[0025]
[0026] In the formula, R 1 are the same or different unsubstituted or substituted monovalent hydrocarbon groups that do not contain aliphatic unsaturated bonds, and R 2 is an alkenyl group, and k is 0 or a positive integer. 1Examples of unsubstituted or substituted monovalent hydrocarbon groups having no aliphatic unsaturated bonds include those having 1 to 10 carbon atoms, and particularly preferably 1 to 6 carbon atoms, and specific examples thereof include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, cyclohexyl, octyl, nonyl, and decyl, aryl groups such as phenyl, tolyl, xylyl, and naphthyl, aralkyl groups such as benzyl, phenylethyl, and phenylpropyl, and groups in which some or all of the hydrogen atoms of these groups have been substituted with halogen atoms such as fluorine, bromine, and chlorine, or with cyano groups, such as halogen-substituted alkyl groups such as chloromethyl, chloropropyl, bromoethyl, and trifluoropropyl, and cyanoethyl groups. 2 The alkenyl group in (A1) preferably has 2 to 6 carbon atoms, particularly 2 to 3 carbon atoms. Specific examples include vinyl, allyl, propenyl, isopropenyl, butenyl, isobutenyl, hexenyl, and cyclohexenyl groups, with vinyl being preferred. In general formula (1), k is generally 0 or a positive integer satisfying 0≦k≦10,000, preferably 5≦k≦2,000, and more preferably 10≦k≦1,200. The organopolysiloxane of component A1 may also be used in combination with an organopolysiloxane having three or more, typically 3 to 30, and preferably about 3 to 20, alkenyl groups bonded to silicon atoms having 2 to 8 carbon atoms, particularly 2 to 6 carbon atoms, such as vinyl or allyl groups, per molecule. The molecular structure may be linear, cyclic, branched, or three-dimensionally networked. Preferably, the polymer is a linear organopolysiloxane whose main chain is composed of repeating diorganosiloxane units and whose molecular chain is terminally blocked with triorganosiloxy groups, and whose viscosity at 25°C is 10 to 1,000,000 mPa·s, and particularly 100 to 100,000 mPa·s.
[0027] The alkenyl group may be bonded to any part of the molecule. For example, it may be bonded to a silicon atom at the molecular chain terminal or a non-terminal (mid-chain) location. Among these, a linear organopolysiloxane having one to three alkenyl groups on each of the silicon atoms at both molecular chain terminals, as represented by the following general formula (Chemical Formula 2), is preferred from the viewpoints of workability, curability, etc., and has at least one alkenyl group (e.g., as a substituent in a diorganosiloxane unit) bonded to a non-terminal (mid-chain) silicon atom, as described above. Furthermore, this linear organopolysiloxane may contain a small amount of branched structures (trifunctional siloxane units) in the molecular chain.
[0028]
[0029] In the formula, R 3 are the same or different unsubstituted or substituted monovalent hydrocarbon groups, and at least one is an alkenyl group. 4 are the same or different unsubstituted or substituted monovalent hydrocarbon groups that do not contain aliphatic unsaturated bonds, and R 5 is an alkenyl group, and l and m are 0 or positive integers. 3The monovalent hydrocarbon group preferably has 1 to 10 carbon atoms, particularly 1 to 6 carbon atoms, and specific examples thereof include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, cyclohexyl, octyl, nonyl, and decyl; aryl groups such as phenyl, tolyl, xylyl, and naphthyl; aralkyl groups such as benzyl, phenylethyl, and phenylpropyl; alkenyl groups such as vinyl, allyl, propenyl, isopropenyl, butenyl, hexenyl, cyclohexenyl, and octenyl; and groups in which some or all of the hydrogen atoms of these groups have been substituted with halogen atoms such as fluorine, bromine, and chlorine, or with cyano groups, such as halogen-substituted alkyl groups such as chloromethyl, chloropropyl, bromoethyl, and trifluoropropyl, and cyanoethyl groups. 4 The monovalent hydrocarbon group of R preferably has 1 to 10 carbon atoms, particularly 1 to 6 carbon atoms. 1 Specific examples of R include the same as those of R, except that alkenyl groups are not included. 5 The alkenyl group of the formula (1) is preferably an alkenyl group having 2 to 6 carbon atoms, particularly preferably having 2 to 3 carbon atoms. 2 Examples of l and m are the same as those shown in the above, and a vinyl group is preferred. l and m are generally 0 or a positive integer satisfying 0 < l + m ≦ 10000, preferably 5 ≦ l + m ≦ 2000, more preferably 10 ≦ l + m ≦ 1200, and are integers satisfying 0 < l / (l + m) ≦ 0.2, preferably 0.0011 ≦ l / (l + m) ≦ 0.1.
[0030] (2) Crosslinking Component (Component A2) The organohydrogenpolysiloxane of Component A2 of the present invention acts as a crosslinking agent, forming a cured product through an addition reaction (hydrosilylation) between the SiH groups in this component and the alkenyl groups in Component A. Any organohydrogenpolysiloxane may be used as long as it has two or more hydrogen atoms bonded to silicon atoms (i.e., SiH groups) per molecule. The molecular structure of this organohydrogenpolysiloxane may be linear, cyclic, branched, or a three-dimensional network structure, but those with a number of silicon atoms per molecule (i.e., degree of polymerization) of 2 to 1000, and particularly about 2 to 300, can be used.
[0031] The position of the silicon atom to which the hydrogen atom is bonded is not particularly limited, and it may be at the end of the molecular chain or at a non-end of the molecular chain (in the middle of the molecular chain). In addition, the organic group bonded to the silicon atom other than a hydrogen atom is R in the general formula (Chemical Formula 1). 1 and unsubstituted or substituted monovalent hydrocarbon groups having no aliphatic unsaturated bonds, similar to those shown above.
[0032] Examples of organohydrogenpolysiloxanes of component A2 include those with the following structures:
[0033] In the above formula, R 6 are the same or different alkyl groups, phenyl groups, epoxy groups, acryloyl groups, methacryloyl groups, alkoxy groups, or hydrogen atoms, and at least two of them are hydrogen atoms. L is an integer of 0 to 1,000, particularly an integer of 0 to 300, and M is an integer of 1 to 200.
[0034] (3) Catalyst Component (Component C) The catalyst component of Component C can be a catalyst used in hydrosilylation reactions. Examples include platinum black, platinic chloride, chloroplatinic acid, reaction products of chloroplatinic acid with monohydric alcohols, complexes of chloroplatinic acid with olefins or vinylsiloxanes, platinum-based catalysts such as platinum bisacetoacetate, palladium-based catalysts, and rhodium-based catalysts. Two-component room-temperature-curing silicone polymers contain a platinum-group metal catalyst, but the additional platinum-group metal catalyst is used to control the curing rate.
[0035] (4) Thermally conductive particles (component B and component C) In the present invention, it is preferable to use three or more types of inorganic particles with different average particle sizes in combination as the thermally conductive particles. When three types are used, they are component B-1, component C-1, and component C-2, and when four types are used, component B-2 is added to these. In this way, the thermally conductive inorganic particles with smaller particle sizes are buried between the larger particles, allowing for filling in a state close to close packing, thereby increasing thermal conductivity.
[0036] (5) Other Additives The composition of the present invention may contain other components as needed. For example, heat resistance improvers such as red iron oxide, titanium oxide, and cerium oxide, flame retardant assistants, and cure retarders may be added. Organic or inorganic pigments may be added for coloring or toning purposes. The above-mentioned silane coupling agents may also be added.
[0037] The following description will be made with reference to the drawings. In the following drawings, the same reference numerals indicate the same parts. FIG. 1 is a schematic cross-sectional view of a heat dissipation structure 10 incorporating a thermally conductive sheet according to one embodiment of the present invention. The thermally conductive sheet 11b dissipates heat generated by an electronic component 13, such as a semiconductor device. The thermally conductive sheet 11b is fixed to a main surface 12a of the heat spreader 12 facing the electronic component 13, and is sandwiched between the electronic component 13 and the heat spreader 2. The thermally conductive sheet 11a is sandwiched between the heat spreader 12 and a heat sink 15. The thermally conductive sheets 11a and 11b, together with the heat spreader 2, constitute a heat dissipation member that dissipates heat from the electronic component 13. The heat spreader 12 is formed, for example, in the shape of a rectangular plate, and has a main surface 12a facing the electronic component 13 and a sidewall 12b extending along the outer periphery of the main surface 12a. The heat spreader 2 has a thermally conductive sheet 11b on a main surface 12a surrounded by side walls 12b, and a heat sink 15 on another surface 12c opposite to the main surface 12a, with the thermally conductive sheet 11a interposed therebetween. The electronic component 13 is, for example, a semiconductor element such as a BGA, and is mounted on a wiring board 14.
[0038] The present invention will be described below using examples, but is not limited to these examples. Various parameters were measured by the methods described below.
[0039] <Thermal Conductivity> The thermal conductivity of the thermally conductive silicone rubber sheet was measured using a hot disk (compliant with ISO 22007-2:2008). As shown in Figure 2A, this thermal conductivity measuring device 1 sandwiches a polyimide film sensor 2 between two samples 3a and 3b, applies a constant power to the sensor 2, and generates a constant amount of heat, analyzing the thermal characteristics from the temperature rise of the sensor 2. The sensor 2 has a 7 mm diameter tip 4 and, as shown in Figure 2B, has a double spiral electrode structure with an applied current electrode 5 and a resistance value electrode (temperature measurement electrode) 6 located at the bottom. The thermal conductivity is calculated using the following equation (Equation 1): <Hardness> The hardness of the thermally conductive silicone rubber sheet was measured in accordance with SHORE 00. <Plasticity> Plasticity was measured using a Wallace plastometer in accordance with JIS K 6300-3 and ISO 2007:1991. The plasticity was determined by dividing the thickness (t) of the sample after compressing it between two metal plates at a constant load (100 N) for a constant time (15 seconds) at a measurement temperature of 23°C by the thickness (t0) before compression (P0 = t / t0 × 100). A smaller plasticity (P0) value indicates greater flexibility. The pre-vacuum plasticity is the plasticity of the compound after preparation. The post-degassing plasticity is the plasticity after the compound is prepared and degassed for 5 minutes at a reduced pressure of -0.1 Pa. Since the compound is degassed before being molded into a sheet, the post-degassing plasticity is important. <BET Specific Surface Area> The BET specific surface area of the thermally conductive particles was measured according to the standard of JIS R 1626-1996. The larger the BET specific surface area, the smaller the D50 (median diameter) of the cumulative particle size distribution based on the volume of the thermally conductive particles.
[0040] (Examples 1 to 5, Comparative Examples 1 to 5) 1. Material Components (1) Polyorganosiloxane (Component A) A commercially available two-component room-temperature curing silicone polymer (silicone component) containing polyorganosiloxane was used. One component (Component A) contains a base polymer component (Component A1 of Component A) and a platinum group metal catalyst, while the other component (Component B) contains an organohydrogenpolysiloxane, which is a base polymer component (Component A1 of Component A) and a crosslinker component (Component A2 of Component A). The mass ratio of Components A and B was A:B = 100:100. (2) Thermally Conductive Particles (Component B) The thermally conductive particles listed in Table 1 were used. The average particle size was measured by laser diffraction light scattering and was the D50 (median diameter) of the cumulative particle size distribution on a volume basis. An example of this measuring instrument is the LA-950S2 laser diffraction / scattering particle distribution analyzer manufactured by Horiba, Ltd. The number before μm in the table is the average particle size of each particle. (3) Thermally conductive particles (component C) The thermally conductive particles listed in Table 1 were used. The average particle size is the D50 (median diameter) of the cumulative particle size distribution based on volume, as measured by the laser diffraction / light scattering method. An example of this measuring instrument is the LA-950S2 laser diffraction / scattering particle distribution analyzer manufactured by Horiba, Ltd. The number before μm in the table is the average particle size of each particle. Also, AlN in the table is an abbreviation for aluminum nitride. (4) Platinum group metal catalyst (component C) A platinum-vinyldisiloxane complex was used as an additional platinum group metal catalyst. As mentioned above, the two-component room-temperature curing silicone polymer (silicone component) contains a platinum group metal catalyst. When preparing the silicone composition of each example, an additional platinum group metal catalyst was added to ensure that the polyorganosiloxane was sufficiently cured. (5) Additive 1 Dimethylpolysiloxane was used as the unreacted silicone oil (viscosity at 25°C using a Brooklyn Field type rotational viscometer SP No. 2: 100 mm 2 / s) was used. (6) Additive 2 Decyltrimethoxysilane was used as a silane coupling agent.
[0041] 2. Compound The amounts of each material shown in Table 1 were weighed out and placed in a mixer to form a compound. In Table 1, the amount of each material is listed in parts by mass, assuming 100 parts by mass (100 g) of the silicone component (two-component room-temperature-curing silicone polymer). This compound was degassed for 5 minutes under a reduced pressure of -0.1 Pa.
[0042] 3. Sheet Molding The compound was sandwiched between release-treated polyethylene terephthalate (PET) films and rolled using a constant-speed roll at 23°C, a roll speed of 0.5 m / min, and a thickness of 2.0 mm to obtain a thermally conductive silicone rubber sheet. The moldability was evaluated as "possible" if molding was possible under the above conditions, and "NG" if not. The above conditions and results are shown in Tables 1 and 2. Tables 1 and 2 show the amount of each component added when the total of the base polymer component (A1), crosslinking component (A2), unreacted silicone oil, and silane coupling agent is 100 parts by mass.
[0043]
[0044]
[0045] As shown in Tables 1 and 2, it was confirmed that Examples 1 to 5 had high thermal conductivity and low plasticity after degassing (plasticity before curing). In contrast, in Comparative Example 1, the absence of component B-1 increased plasticity, and molding processability was poor. In Comparative Example 2, the absence of component B-1 increased plasticity even though the BET specific surface area was large, and molding processability was poor. In Comparative Example 3, component B was below the lower limit, so plasticity increased and molding processability was poor. In Comparative Example 4, component B exceeded the upper limit, and thermal conductivity decreased. In Comparative Example 5, component C was below the lower limit, and thermal conductivity decreased.
[0046] The thermally conductive composition and thermally conductive sheet of the present invention are suitable as a thermal interface material (TIM) that is placed between a heat-generating portion of an electric or electronic part and a heat sink.
[0047] REFERENCE SIGNS LIST 1 Thermal conductivity measuring device 2 Sensor 3a, 3b Sample 4 Sensor tip 5 Electrode for applied current 6 Electrode for resistance value (electrode for temperature measurement) 10 Heat dissipation structure 11a, 11b Thermally conductive sheet 12 Heat spreader 13 Electronic component 14 Wiring board 15 Heat sink
Claims
1. A thermally conductive composition comprising a matrix resin (component A) made of a thermosetting resin, a curing catalyst, and thermally conductive particles, the thermally conductive particles comprising the following components B and C: (1) Component B: Alumina having a volume-based cumulative particle size distribution D50 (median diameter) of 0.01 μm or more and less than 1 μm is contained in an amount of 220 to 500 parts by mass per 100 parts by mass of the matrix resin, and comprising the following components B-1 and B-2: Component B-1: Alumina having a D50 (median diameter) of 0.01 μm or more and less than 0.3 μm and a BET specific surface area of 9 m 2 / g or more is 30 to 100 mass% relative to 100 mass% of component B, component B-2: alumina having a D50 (median diameter) of 0.3 μm or more and less than 1 μm is 0 to 70 mass% relative to 100 mass% of component B, (2) component C: containing 1900 to 2500 mass parts of aluminum nitride having a D50 (median diameter) of 0.01 μm or more and 150 μm or less relative to 100 mass parts of matrix resin, and containing the following components C-1 and C-2: component C-1: D50 (median diameter) is 0.01 μm or more and less than 30 μm, and component C-2: D50 (median diameter) is 30 μm or more and 150 μm or less.
2. The thermally conductive composition according to claim 1, wherein the mass ratio of component C-1 to component C-2 is such that component C-2≦component C-1.
3. The thermally conductive composition according to claim 1 or 2, wherein the thermal conductivity of the cured product of the thermally conductive composition is 14 W / m·K or more.
4. The thermally conductive composition according to any one of claims 1 to 3, wherein the cured product of the thermally conductive composition has a SHORE 00 hardness of 75 or less.
5. The thermally conductive composition according to any one of claims 1 to 4, wherein the matrix resin is at least one selected from the group consisting of addition-curing silicone polymers, peroxide-curing silicone polymers, and condensation-curing silicone polymers.
6. The thermally conductive composition according to any one of claims 1 to 5, further comprising 0.1 to 10 parts by mass of a silane coupling agent per 100 parts by mass of the matrix resin.
7. A thermally conductive composition according to any one of claims 1 to 6, wherein at least one component selected from the group consisting of alumina as component B and aluminum nitride as component C is in the form of irregularly pulverized particles.
8. A thermally conductive sheet, characterized in that the thermally conductive composition according to any one of claims 1 to 7 is formed into a sheet.
9. The thermally conductive sheet according to claim 8, wherein the thickness of the thermally conductive sheet is in the range of 0.2 to 10 mm.
10. A method for producing a thermally conductive sheet, comprising vacuum degassing the thermally conductive composition according to any one of claims 1 to 7, rolling it, forming it into a sheet, and then heat curing it to produce a thermally conductive sheet.
Citation Information
Patent Citations
Composition for thermal conducive grease, thermal conductive grease and heat dissipating member
JP2016216523A
Light-emitting panel and building wall
JP2018088416A
Absorbent article
JP2020137970A
Silicone polymer and composition containing same
JP2021518466A
Thermally conductive sheet and manufacturing method thereof
JP7061736B1