Packaging material and method for manufacturing packaging material
The packaging material, featuring a hydrophilic resin barrier layer and a polyol-isocyanate adhesive layer, enhances lamination strength and oxygen barrier properties while minimizing residual solvent, effectively addressing the limitations of conventional materials in terms of recycling and environmental impact.
Patent Information
- Application Number
- PCT/JP2024/016419
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2024-04-26
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional packaging materials face challenges in achieving excellent lamination strength and oxygen barrier properties after bending, while also minimizing residual solvent content, particularly due to issues with chlorine-based coatings and the limitations of single-material recycling concepts.
A packaging material comprising a base material, a barrier layer with a hydrophilic resin, and an adhesive layer containing a polyol and isocyanate curing agent, with a specific Permacol value and unit area mass, along with an optional inorganic layered filler, to enhance lamination strength and reduce residual solvent.
The solution provides packaging materials with improved lamination strength and oxygen barrier properties after bending, while significantly reducing residual solvent content, thus addressing environmental and recycling concerns.
Smart Images

Figure JPOXMLDOC01-APPB-M000001 
Figure JPOXMLDOC01-APPB-M000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Packaging material and method for manufacturing packaging material
[0001] The present invention relates to packaging materials and methods for manufacturing packaging materials.
[0002] Conventionally, aluminum foil or aluminum-deposited packaging materials have been widely used for packaging materials that require oxygen barrier properties, such as food packaging materials. However, in recent years, in response to environmental issues and other factors, there has been a growing movement toward aluminum-free packaging materials due to social demands for thinner packaging materials, simplified lamination, and recyclability.
[0003] Furthermore, in order to provide a packaging material with barrier properties without using aluminum, a film in which a PVDC (polyvinylidene chloride) layer is formed on a plastic film exhibits high oxygen barrier properties not only under low humidity but also under high humidity conditions, and also has a relatively high barrier property against water vapor. However, when PVDC is incinerated during waste disposal, the chlorine released from the PVDC generates chlorine gas and dioxins, which can have a significant adverse effect on the environment and human health, so a transition to other materials is desired.
[0004] Furthermore, when recycling plastic packaging materials, the idea of "mono-material" has been proposed, in which all the base materials constituting the plastic packaging material are made of the same type of base material, such as polypropylene. This is an idea that makes packaging materials easier to recycle, but using only a single base material poses issues with oxygen barrier properties, and using conventional aluminum would hinder recycling, while using coating agents such as PVDC could lead to damage to recycling equipment due to chlorine gas released at high temperatures.
[0005] Known examples of chlorine-free gas barrier materials include laminates that use an adhesive layer that has been imparted with gas barrier properties, or a coated film in which a thermoplastic resin film is coated with polyvinyl alcohol or the like. Patent Document 1 discloses an example of a laminate that uses an adhesive layer that has been imparted with gas barrier properties, which has a structure of PET (polyethylene terephthalate) / ester-based adhesive layer / CPP (non-oriented polypropylene), in which the Permacol value of the resin composition for a gas barrier cured product used to form the ester-based adhesive layer is 44 to 60. However, in order to impart sufficient barrier properties to a laminate using only an adhesive layer, the adhesive layer must have a large mass per unit area, which poses the problem of residual solvent.
[0006] As an example of a laminate using a coated film, a laminate film having a structure of OPP (biaxially oriented polypropylene) / urethane anchor coat layer / vinyl alcohol barrier layer / adhesive layer / CPP has been disclosed (Patent Documents 2 and 3). However, even in this laminate film, the adhesive layer has a large mass per unit area, and there is a problem of residual solvent.
[0007] Furthermore, when the laminates described in Patent Documents 1 to 3 are used as packaging materials, there are likely to be problems with oxygen barrier properties after folding.
[0008] JP 2013-129780 A JP 2007-136984 A JP 2001-129915 A
[0009] An object of the present disclosure is to provide a packaging material that has excellent lamination strength and oxygen barrier properties after folding, and has little residual solvent.
[0010] As a result of extensive research into the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by using the following packaging material, and have thus achieved the present invention.
[0011] That is, the present invention relates to the following [1] to
[10] .
[0012] [1] A packaging material having a substrate 1, a barrier layer, an adhesive layer, and a substrate 2, wherein the barrier layer contains a hydrophilic resin, the adhesive layer is a layer containing a cured product of a polyol and an isocyanate curing agent (I), the Permacol value of the polyol is 25 to 60, and the unit area mass of the adhesive layer is 1.0 to 4.5 g / m 2 and the olefin content of the packaging material is 80 mass% or more of the total mass of the packaging material.
[0013] [2] The packaging material according to [1], wherein the hydrophilic resin is a polyvinyl alcohol-based resin.
[0014] [3] The packaging material according to [1] or [2], wherein the barrier layer further contains an inorganic layered filler.
[0015] [4] The mass per unit area of the barrier layer is 0.7 g / m 2 The packaging material according to any one of [1] to [3] above.
[0016] [5] The packaging material according to any one of [1] to [4], wherein the polyol has a polyester structure.
[0017] [6] The packaging material according to any one of [1] to [5], wherein the ratio of the mass per unit area of the barrier layer to the mass per unit area of the adhesive layer is 70:30 to 15:85.
[0018] [7] The packaging material according to any one of [1] to [6], further comprising an anchor coat layer, wherein the anchor coat layer contains a urethane resin.
[0019] [8] The packaging material according to [7], wherein the urea bond concentration of the urethane resin is 0.1 to 1.3 mmol / g.
[0020] [9] The packaging material according to any one of [1] to [8], wherein the substrate 1 and the substrate 2 contain a polyolefin resin.
[0021]
[10] A method for producing a packaging material having a substrate 1, a barrier layer, an adhesive layer, and a substrate 2 in this order, the method comprising the steps of applying a barrier coating agent to form a barrier layer, and applying a reactive adhesive to form an adhesive layer, wherein the barrier layer contains a hydrophilic resin, the adhesive layer is a layer made of a reactive adhesive containing a polyol and an isocyanate curing agent (I), the Permacol value of the polyol is 25 to 60, and the unit area mass of the adhesive layer is 1.0 to 4.5 g / m 2 wherein the olefin content of the packaging material is 80 mass% or more of the total mass of the packaging material.
[0022] The present disclosure makes it possible to provide a packaging material that is excellent in lamination strength and oxygen barrier properties after folding, and has little residual solvent.
[0023] The following describes in detail the embodiments of the present disclosure, but the described embodiments or explanations of the requirements are examples of the embodiments of the present disclosure, and the present disclosure is not limited to these contents as long as it does not deviate from the gist of the disclosure.
[0024] [Packaging Material] The packaging material has a substrate 1, a barrier layer, an adhesive layer, and a substrate 2, in which the barrier layer contains a hydrophilic resin, the adhesive layer is a layer containing a cured product of a polyol and an isocyanate curing agent (I), the Permacol value of the polyol-derived structure is 25 to 60, and the unit area mass of the adhesive layer is 1.0 to 4.5 g / m 2 and the olefin content of the packaging material is 80% by mass or more of the total mass of the packaging material. The packaging material of the present disclosure can be suitably used to form flexible packaging packages, packaging bags, etc. The packaging material of the present disclosure may be used alone or in combination with other materials. The packaging material may also form a packaging container. The olefin content of the packaging material is preferably 80% by mass or more of the total mass of the packaging material, and more preferably 90 to 99% by mass. When the olefin content of the packaging material is within the above range, residual solvent can be further reduced.
[0025] In methods such as dry lamination for forming an adhesive layer, the adhesive is applied to a substrate or the like in a state dissolved in an organic solvent. However, depending on the application conditions and lamination configuration, there is a concern that the organic solvent may penetrate into the substrate or the like during application, resulting in a large amount of residual solvent. The packaging material of the present disclosure has a barrier layer with a specific configuration, and the adhesive layer has a polyol-derived structure with a specific Permacol value. This not only improves barrier properties, but also significantly reduces residual solvent due to the combined effect of the barrier layer, adhesive layer, and olefin content of the packaging material. One consideration is that this effect is due to the promotion of volatilization of the organic solvent derived from the adhesive layer and the prevention of penetration of the organic solvent into the substrate 1. Due to these effects, the packaging material of the present disclosure has excellent laminate strength, residual solvent, and oxygen barrier properties after folding.
[0026] Specific examples of the configuration of the packaging material include, but are not limited to, the following configurations. A configuration having a substrate 1, a barrier layer, and an adhesive layer in this order is preferred, and a configuration having a substrate 1, an anchor coat layer, a barrier layer, an adhesive layer, and a substrate 2 in this order is more preferred. In the following configuration notations, " / " indicates the boundary between layers. For example, the adhesive layer may be one formed from an adhesive used in dry lamination, which is a conventionally known method. (1) Substrate 1 / barrier layer / adhesive layer / substrate 2 (2) Substrate 1 / printing layer / barrier layer / adhesive layer / substrate 2 (3) Substrate 1 / anchor coat layer / barrier layer / adhesive layer / substrate 2 (4) Substrate 1 / printing layer / anchor coat layer / barrier layer / adhesive layer / substrate 2 (5) Substrate 1 / printing layer / anchor coat layer / barrier layer / adhesive layer / intermediate substrate / adhesive layer / substrate 2 (6) Printing layer / substrate 1 / anchor coat layer / barrier layer / adhesive layer / substrate 2 In the above configuration examples, substrate 1, intermediate substrate, and substrate 2 may be the same or different, and their names are determined by their positional relationship.
[0027] The substrate 1, intermediate substrate, and substrate 2 may each be a single layer, may be laminated with the same or different plastic substrates, or may be laminated with a substrate different from the plastic substrate. In the case of a laminated substrate, it may include an adhesive layer. The "substrate different from the plastic substrate" may be a paper substrate or the like, and any type of substrate may be used. The method for laminating the substrates is not particularly limited, and includes conventionally known methods such as coextrusion, heat fusion, and pressure bonding via an adhesive layer.
[0028] [Substrate 1] The substrate 1 is not particularly limited, and examples thereof include paper substrates such as medium-density paper, wood-free paper, impregnated paper, cardboard, and kraft paper. Examples of plastic substrates include polyethylenes such as biaxially oriented polypropylene (OPP), non-oriented polypropylene (CPP), low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), medium-density polyethylene (MDPE), and high-density polyethylene (HDPE), polyolefin substrates such as acid-modified polyethylene, acid-modified polypropylene, and copolymer polypropylene, polyethylene terephthalate, polycarbonate, polylactic acid, polystyrene, AS resin, ABS resin, nylon, polyamide, polyvinyl chloride, polyvinylidene chloride, and cellophane. Substrates made of composite materials of the above may also be used. In addition, the substrate may be vapor-deposited with an inorganic compound such as silica, alumina, or aluminum, or may be coated with polyethylene, polyvinyl alcohol, or the like, or may be corona-treated.
[0029] In particular, the substrate 1 is preferably a polyolefin substrate. The polyolefin substrate is preferably at least one selected from the group consisting of polyethylene such as biaxially oriented polypropylene (OPP), non-oriented polypropylene (CPP), low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), medium-density polyethylene (MDPE), and high-density polyethylene (HDPE), acid-modified polyethylene, acid-modified polypropylene, and copolymer polypropylene. The thickness of the substrate 1 is not particularly limited, and in consideration of processability into packaging containers, it may be preferably 5 μm or more and 150 μm or less, more preferably 10 μm or more and 70 μm or less.
[0030] [Substrate 2] The substrate 2 is not particularly limited, but in one embodiment, a polyolefin resin, particularly one having heat-sealing properties, can be suitably used. Examples of suitable substrates include corona-treated biaxially oriented polypropylene (OPP) film, high-density polyethylene film (HDPE), unoriented polypropylene (CPP) film, linear low-density polyethylene (LLDPE) film, and polyethylene resin films formed by melt coating. The substrate 2 may also be coated with a heat-sealing agent. The thickness of the substrate 2 is not particularly limited, but is preferably 5 to 150 μm, more preferably 10 to 70 μm, from the viewpoint of processability during packaging container production.
[0031] [Intermediate Substrate] The packaging material of the present disclosure may have an intermediate substrate for purposes such as improving rigidity. Specific examples of the intermediate substrate, like substrate 1 and substrate 2, are preferably plastic substrates primarily containing polyolefin resin as a raw material. Examples include polyolefin resins such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), ethylene-vinyl acetate copolymer, propylene homopolymer, and ethylene-propylene copolymer. Alternatively, the intermediate substrate may be a composite substrate manufactured by co-extrusion. Furthermore, it is more preferable that the intermediate substrate is made of the same (same) material as substrate 1 and substrate 2. Examples of materials of the same (same) type include combinations of polypropylene and polyethylene, etc.
[0032] [Barrier Layer] The barrier layer is disposed for the purposes of imparting oxygen barrier properties to the packaging material and reducing residual solvents through the integrated effect with other components, and the barrier layer contains a hydrophilic resin. The barrier layer is preferably formed from a barrier coating agent described below.
[0033] The mass per unit area of the barrier layer is 0.7 to 5 g / m 2 It is preferable that the density is 0.8 to 3 g / m 2 More preferably, it is 0.9 to 1.5 g / m 2 It is more preferable that the mass per unit area of the barrier layer is 0.7 g / m 2When the unit area mass of the barrier layer is 5 g / m or more, the residual solvent can be reduced, and the oxygen barrier property after folding is also improved. Normally, when the unit area mass of the barrier layer is increased, the amount of organic solvent that may be contained in the composition for forming the barrier layer increases, and it is expected that the amount of residual solvent in the packaging material will also increase. However, in the case of the packaging material of the present disclosure, the barrier layer acts to prevent the organic solvent from migrating from the adhesive layer to the substrate 1, and it is presumed that the integrated effect with other components further reduces the residual solvent. On the other hand, when the unit area mass of the barrier layer is 5 g / m or more, the residual solvent can be reduced. 2 When the ratio is equal to or less than 1, the laminate strength is improved.
[0034] <Hydrophilic Resin> A hydrophilic resin refers to a resin that is miscible with water. Examples of hydrophilic resins include polyvinyl alcohol-based resins (including ethylene-vinyl alcohol copolymer resins), aqueous acrylic resins, aqueous styrene-acrylic resins, aqueous styrene-maleic acid resins, aqueous urethane resins, aqueous polylactic acid resins, polyvinylpyrrolidone, starch, methyl cellulose, carboxymethyl cellulose, and modified resins thereof. These hydrophilic resins can be used alone or in combination of two or more. Among the above, it is preferable that the hydrophilic resin includes a polyvinyl alcohol-based resin.
[0035] The content of the hydrophilic resin in the barrier layer is preferably 30 to 95% by mass, more preferably 55 to 90% by mass, and even more preferably 70 to 80% by mass. When the content is within the above range, the oxygen barrier property after bending can be further improved.
[0036] <Polyvinyl alcohol-based resin> The polyvinyl alcohol-based resin may be any resin having a structural unit derived from vinyl alcohol, and preferably further contains a structural unit derived from ethylene. Examples of the polyvinyl alcohol-based resin include polyvinyl alcohol resin and ethylene-vinyl alcohol copolymer resin, with polyvinyl alcohol resin and / or ethylene-vinyl alcohol copolymer resin being preferred, and ethylene-vinyl alcohol copolymer resin being more preferred.
[0037] The content of ethylene-derived structural units in the ethylene-vinyl alcohol copolymer resin is preferably 1 to 40 mol%, more preferably 3 to 20 mol%, and even more preferably 5 to 15 mol%. When the content of ethylene-derived structural units is within the above range, the oxygen barrier property after bending is improved. The degree of polymerization of the polyvinyl alcohol resin is preferably 100 to 3,000, and more preferably 500 to 2,400. When within the above range, the oxygen barrier property after bending is improved.
[0038] The polyvinyl alcohol resin may have a modified functional group, and examples of the functional group include, but are not limited to, a carbonyl group, a silicon group, etc. Furthermore, the polyvinyl alcohol resin may be crosslinked with a crosslinking agent, and examples of the crosslinking agent include known crosslinking agents such as an isocyanate crosslinking agent, an epoxy crosslinking agent, a melamine crosslinking agent, an oxazoline crosslinking agent, and a silane coupling crosslinking agent, and the oxazoline crosslinking agent and the silane coupling crosslinking agent are preferred.
[0039] The degree of saponification of the polyvinyl alcohol resin is expressed by the following formula (1), and is preferably 80 mol% or more, more preferably 90 mol%, and even more preferably 95 mol%. When it is in the above range, the oxygen barrier property after bending is improved. (Formula 1) Saponification degree: (number of hydroxyl groups) / {(number of hydroxyl groups)+(number of acetate groups)}×100 [mol%]
[0040] Examples of polyvinyl alcohol resins that can be used include Kuraray Poval R series (polyvinyl alcohol resins manufactured by Kuraray Co., Ltd.), Kuraray Eval L104B and F104B (ethylene-vinyl alcohol copolymer resins manufactured by Kuraray Co., Ltd.), and the like.
[0041] <Inorganic Layered Filler> The barrier layer preferably further contains an inorganic layered filler. The inorganic layered filler referred to here is an inorganic filler that forms a layered structure, and is particularly preferably one that swells and / or cleaves in a solvent. The mass ratio of the hydrophilic resin to the inorganic layered filler is preferably 9:1 to 4:6, more preferably 8:2 to 5:5, and even more preferably 8:2 to 6:4. When the mass ratio is within the above range, the oxygen barrier property after bending is improved.
[0042] The average particle size of the inorganic layered filler measured by a laser light scattering method is preferably 0.1 to 30 μm, more preferably 0.5 to 15 μm, even more preferably 1 to 10 μm, and particularly preferably 1.5 to 5 μm. In the present disclosure, the average particle size is measured using an MT3300EX II manufactured by Microtrac MRB.
[0043] The aspect ratio of the inorganic layered filler is preferably 10 to 2000, more preferably 50 to 1000, and even more preferably 200 to 700. The aspect ratio refers to a value measured using a scanning electron microscope (SEM), and in the present disclosure is measured using a JEOL JSM-7800F.
[0044] The specific surface area of the inorganic layered filler is 0.5 to 250 m 2 / g, and 1 to 100m 2 / g, and more preferably 3 to 50m 2 / g, and more preferably 5 to 30m 2 The specific surface area is a value calculated from the amount of nitrogen gas adsorbed by the BET method, and in the present disclosure, is measured using a TriStar II manufactured by Shimadzu Corporation.
[0045] Preferred examples of inorganic layered fillers include montmorillonite, beidellite, saponite, hectorite, sauconite, vermiculite, mica, paragonite, lepidolite, margarite, clintonite, anandite, chlorite, donbassite, sudoite, cookeite, clinochlore, chamosite, nimite, tetrasilylic mica, talc, pyrophyllite, nacrite, kaolinite, halloysite, chrysotile, sodium taeniolite, xanthophyllite, antigorite, dickite, and hydrotalcite. Montmorillonite is preferably one or more selected from the group consisting of kaolin, montmorillonite, and mica, and more preferably montmorillonite. Montmorillonite has high water absorption and high viscosity after swelling due to its layered structure, which allows resins to easily penetrate between the layers of the layered filler, thereby contributing to improving the oxygen barrier properties of the packaging material after folding.
[0046] These inorganic layered fillers may be naturally occurring or artificially synthesized or modified, or may be those treated with an organic substance such as an onium salt.
[0047] The content of the inorganic layered filler is preferably 1 to 40% by mass, more preferably 10 to 35% by mass, and even more preferably 20 to 30% by mass, based on 100% by mass of the barrier layer.
[0048] <Montmorillonite> The montmorillonite is represented by the following formula 2. Bentonite, which contains montmorillonite as the main component and further contains minerals such as quartz and feldspar, can also be preferably used. (Formula 2) M a Si 4 (Al 2-a Mg a ) O 10 (OH) 2 ・nH 2 O (In formula 2, M represents a sodium cation, and a is 0.25 to 0.60. The number of water molecules bonded to the ion-exchangeable cations between layers can vary depending on the type of cation, humidity, and other conditions. Therefore, in the formula, nH 2 It is represented by O.)
[0049] Montmorillonite also includes isomorphous ion-substituted products of magnesian montmorillonite, iron montmorillonite, and iron magnesian montmorillonite, which are represented by the following formulas (3) to (5), and these may also be used. (Formula 3) M a Si 4 (Al 1.67-a Mg 0.5+a ) O 10 (OH) 2 ・nH 2 O (Formula 4) M a Si 4 (Fe 2-a 3+ Mg a ) O 10 (OH) 2 ・nH 2 O (Formula 5) M a Si 4 (Fe 1.67-a 3+ Mg 0.5+a ) O 10 (OH) 2 ・nH 2 O (In formulas 3 to 5, M represents a sodium cation, and a is 0.25 to 0.60.)
[0050] Montmorillonite usually contains cations between its layers, the content of which varies depending on the place of origin. Examples of such ions include inorganic cations such as sodium ions, calcium ions, magnesium ions, and potassium ions, and organic cations such as quaternary ammonium ions. From the viewpoint of affinity for water, inorganic cations are preferred, and sodium ions and / or calcium ions are more preferred. It is also preferable to use montmorillonite that has been purified by water treatment.
[0051] The average particle size of montmorillonite is preferably 0.1 to 10 μm, more preferably 1 to 5 μm, and even more preferably 1.5 to 3 μm. The particle aspect ratio of montmorillonite is preferably 10 to 2,000, more preferably 100 to 1,000, and even more preferably 300 to 700. The specific surface area of montmorillonite is preferably 1 to 250 m. 2 / g, and 1 to 100m 2 / g, and more preferably 3 to 50m 2 / g, and more preferably 5 to 30m 2 It is particularly preferred that the SiO2 content is 1 / g.
[0052] The average thickness of the montmorillonite particles is preferably 0.05 to 30 nm, more preferably 0.1 to 10 nm, and even more preferably 0.5 to 3 nm. The average major axis of the montmorillonite particles is preferably 0.01 to 5 μm, more preferably 0.05 to 3 μm, and even more preferably 0.1 to 1 μm. Here, the average thickness and average major axis of the particles refer to values measured using an atomic force microscope (AFM), and in the present disclosure, measurements are performed using an AFM100Plus manufactured by Hitachi High-Technologies Corporation.
[0053] As the montmorillonite, commercially available products such as Kunipia-F and Kunipia-G (manufactured by Kunimine Industries Co., Ltd.) can be used.
[0054] <Kaolin> Kaolin is a type of kaolinite (Al 2 O 3 2SiO 2 ・H 2 O) or halloysite Al 2 O 3 2SiO 2 ・2H 2 The main component is O, and it may be a natural product or a synthetic product. Also, depending on the manufacturing method, there are dry kaolin, wet kaolin, calcined kaolin, etc., but it is not limited to any one of them.
[0055] From the viewpoint of oxygen barrier properties after folding, the average particle size of kaolin is preferably 0.1 to 30 μm, more preferably 0.2 to 20 μm, and even more preferably 0.3 to 10 μm. The aspect ratio of kaolin is preferably 10 to 1,000, more preferably 30 to 500, and even more preferably 50 to 200. The specific surface area of kaolin is 1 to 250 m. 2 / g, and 1 to 100m 2 / g, and more preferably 3 to 50m 2 / g, and more preferably 5 to 30m2 It is particularly preferred that the SiO2 content is 1 / g.
[0056] As the kaolin, commercially available products such as Barisurf HX (manufactured by Imerys), NN kaolin clay, and ST kaolin clay (manufactured by Takehara Chemical Industry Co., Ltd.) can be used.
[0057] <Mica> Both natural and synthetic mica can be used. Natural mica is a scaly base material made by crushing mica ore, and the particle size and aspect ratio can be controlled by mechanical crushing or cleavage by calcination. Synthetic mica is a type of mica made of SiO 2 , MgO, Al 2 0 3 , K. 2 SiF 6 , Na 2 SiF 6 These include those synthesized by heating industrial raw materials such as KMg, melting them at a high temperature of about 1500°C, and then cooling and crystallizing them. Compared to natural mica, these have fewer impurities and are uniform in size and thickness. 3 AlSi 3 O 10 F 2 ), potassium tetrasilicic mica (KMg 2.5 AlSi 4 O 10 F 2 ), sodium tetrasilicic mica (NaMg 2.5 AlSi 4 O 10 F 2 ), Na taeniolite (NaMg 2 LiSi 4 O 10 F 2 ), LiNa taeniolite (LiMg 2 LiSi 4 O 10 F 2 From the viewpoint of dispersibility, synthetic mica, which is easily cleaved by intercalation, is preferred.
[0058] From the viewpoint of oxygen barrier properties after folding, the average particle size of the mica is preferably 30 μm or less, more preferably 1 to 25 μm, and even more preferably 5 to 15 μm. The aspect ratio of the mica is preferably 30 to 200, more preferably 70 to 170, and even more preferably 100 to 150. The specific surface area of the mica is 1 to 250 m. 2 / g, and 1 to 100m 2 / g, and more preferably 3 to 50m 2 / g, and more preferably 5 to 30m 2 It is particularly preferred that the SiO2 content is 1 / g.
[0059] As the mica, commercially available products such as Mica Powder TM series, Mica Powder NCF series (manufactured by Yamaguchi Mica Co., Ltd.), L60M, L100M (manufactured by Seishin Enterprise Co., Ltd.) can be used.
[0060] <Additives that can be contained in the barrier layer> The barrier layer can contain known additives such as an isocyanate compound, a silane coupling agent, a dispersant, a stabilizer, a viscosity adjuster, and a colorant, as long as the effects of the present disclosure are not impaired.
[0061] <Barrier Coating Agent> The barrier coating agent for forming the barrier coating layer preferably contains a hydrophilic resin and an aqueous solvent. Furthermore, each component of the inorganic layered filler can be added to the coating agent either alone or in combination, and additives can be added as needed. The barrier coating agent can be obtained, for example, by charging a resin solution in which a hydrophilic resin is dissolved or dispersed in an aqueous solvent, the aqueous solvent, and, if necessary, the optional components described above, into a mixer equipped with a stirring blade, rotor, or the like, followed by mixing and stirring. The stirring speed is not particularly limited, and can be set at 50 to 2000 rpm.
[0062] <Aqueous Solvent> The barrier coating agent preferably contains an aqueous solvent. The main component of the aqueous solvent is preferably water, but a hydrophilic organic solvent can be used in addition to water. Specifically, alcohol-based organic solvents, glycol-based organic solvents, etc. can be added depending on the printing conditions (speed, plate depth, design, drying temperature, etc.). Here, "the main component is water" means that the water content is the highest in the aqueous solvent. Furthermore, a hydrophilic organic solvent refers to one that is liquid at 25°C and has a solubility in water at 25°C of 1% by mass or more.
[0063] Examples of the alcohol-based organic solvent include methanol, ethanol, propanol, isopropanol, isobutanol, normal butanol, tertiary butanol, hexanol, octanol, and decanol.
[0064] Examples of the glycol-based organic solvent include acetylene diol, ethylene glycol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, ethylene glycol monooctyl ether, diethylene glycol, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, triethylene glycol, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, triethylene glycol monopropyl ether, triethylene glycol monobutyl ether, propylene glycol, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monobutyl ether, tripropylene glycol, tripropylene glycol monomethyl ether, tripropylene glycol monoethyl ether, tripropylene glycol monopropyl ether, tripropylene glycol monobutyl ether, and dibutyl glycol. These may be used alone or in combination of two or more.
[0065] <Formation of Barrier Layer> The barrier layer can be formed, for example, by printing a barrier coating agent on the anchor coat layer and then removing the volatile components. Examples of printing methods include conventionally known methods such as gravure printing, flexographic printing, dipping, roll coating, screen printing, and spraying. The gravure printing method is preferred. For example, the agent is diluted with a diluting solvent to a viscosity and concentration suitable for gravure printing, and then supplied to each printing unit alone or in a mixture, and applied. The barrier coat layer can then be obtained by fixing the coating by drying in an oven or the like.
[0066] [Adhesive Layer] The adhesive layer is a layer containing a cured product of a polyol and an isocyanate curing agent (I). The adhesive layer can be formed, for example, by coating a two-component reactive adhesive, which is a mixture of a polyol having a Permacol value of 25 to 60 and an isocyanate curing agent (I), on the barrier layer, followed by drying and curing. The adhesive is preferably in the form of a dry laminate adhesive.
[0067] The mass per unit area of the adhesive layer is 1.0 to 4.5 g / m 2 and 1.5 to 4.3 g / m 2 is preferably 2.0 to 4.0 g / m 2 When the content is in the above range, the oxygen barrier property after bending is further improved and the residual solvent is further reduced.
[0068] Furthermore, the ratio of the unit area mass of the barrier layer to the unit area mass of the adhesive layer is preferably 70:30 to 15:85, more preferably 55:45 to 22.5:77.5, and even more preferably 40:60 to 20:80. When the ratio of the unit area mass of the barrier layer to the unit area mass of the adhesive layer is within the above range, the oxygen barrier property after bending is further improved and the residual solvent is further reduced.
[0069] <Permacol value of polyol>
[0070] The Permacol value of the polyol is 25 to 60, preferably 27 to 50, and more preferably 30 to 40. When the Permacol value is 25 or more, the oxygen barrier property after bending is improved. When the Permacol value is 60 or less, the laminate strength is improved and the residual solvent is reduced.
[0071] In the present disclosure, the Permacol value of a polyol refers to the Permacol value of the residue excluding the terminal OH group of the polyol. The Permacol value correlates with gas permeability as shown in (Equation 6), and the larger the Permacol value, the smaller the gas permeability. (Equation 6) P = A × exp(-S × Π) P: gas permeability A: constant specific to each gas (oxygen: 5.0 × 10 -9 ) S: A constant specific to each gas (oxygen: 0.112) Π: Permacol value
[0072] The Permacol value of a polyol can be calculated using the following (Equation 7), and the Permacol value Pn specific to the polymer segment n in (Equation 7) can be the value described in Table 1 of JP 2013-129780 A. (Equation 7) Pn: Permacol value specific to polymer segment n Mn: number of moles of polymer segment n
[0073] <Permacol Value of Cured Product of Polyol and Isocyanate Curing Agent (I)>
[0074] The Permacol value of the cured product of the polyol and the isocyanate curing agent is 30 to 70, preferably 35 to 60, and more preferably 40 to 50. When the Permacol value is 30 or more, the oxygen barrier property after bending is improved. When the Permacol value is 70 or less, the laminate strength is improved and the residual solvent is reduced.
[0075] In the present disclosure, the Permacol value of a cured product of a polyol and an isocyanate curing agent (I) refers to the Permacol value of the residue excluding the terminal OH group of the polyol and the isocyanate curing agent (I). The Permacol value of a cured product of a polyol and an isocyanate curing agent (I) can be calculated using the following (Equation 8), and the Permacol value Pm specific to the isocyanate segment m in (Equation 8) can be the values listed in Tables 3 to 7 of JP 2013-129780 A. The isocyanate group of the isocyanate segment is converted to a carbamate group for calculation. (Equation 8) Pn: Permacol value specific to polymer segment n Pm: Permacol value specific to isocyanate segment m Mn: Number of moles of polymer segment n Mm: Number of moles of isocyanate segment n
[0076] <Polyol> The polyol may be any polyol as long as it satisfies a Permacol value of 25 to 60, and examples thereof include polyester polyol, polyether polyol, polyurethane polyol, polyesteramide polyol, acrylic polyol, polycarbonate polyol, polycaprolactone polyol, polyvalerolactone polyol, polyolefin polyol, polyhydroxyalkane, castor oil, and mixtures thereof, as well as ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-5-pentanediol, 1,6-hexanediol, and the like. Examples of suitable polyols include glycols such as 1,4-cyclohexanediol, neopentyl glycol, methylpentane glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, bishydroxyethoxybenzene, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, and triethylene glycol; polyalkylene glycols having a number-average molecular weight of 200 to 3,000; trifunctional or tetrafunctional aliphatic alcohols such as glycerin, trimethylolpropane, and pentaerythritol; and polyols obtained by adding the above-mentioned glycols or polyols to the above-mentioned trifunctional or tetrafunctional aliphatic alcohols. These may be used alone or in combination of two or more. Among these, polyester polyols and polyether polyols are preferred, and polyester polyols are more preferred. The mass ratio of polyester polyol in the polyol is preferably 50 to 100 mass%, more preferably 70 to 100 mass%, and even more preferably 90 to 100 mass%, based on 100 mass% of the polyol. Within the above ranges, oxygen barrier properties after bending are further improved, and residual solvent is further reduced.
[0077] Examples of the polyester polyol include aromatic dibasic acids such as terephthalic acid, isophthalic acid, phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, and naphthalenedicarboxylic acid; aliphatic dibasic acids such as adipic acid, azelaic acid, sebacic acid, succinic acid, glutaric acid, and maleic anhydride; alicyclic dibasic acids such as itaconic anhydride; and dialkyl esters thereof, or mixtures thereof (hereinafter also referred to as carboxyl group components), and ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, triethylene glycol, butylene glycol, neopentyl glycol, dineopentyl glycol, trimethylolpropane, glycerin, 1,6-hexanediol, 1,4- Examples of suitable hydroxyl group components include polyester polyols obtained by esterifying diols such as butanediol, 1,4-cyclohexanedimethanol, 3-methyl-1,5-pentanediol, 3,3'-dimethylolheptane, 1,9-nonanediol, polyoxyethylene glycol, polyoxypropylene glycol, polytetramethylene ether glycol, polyether polyol, polycarbonate polyol, polyolefin polyol, acrylic polyol, and polyurethane polyol, or mixtures thereof (hereinafter also referred to as hydroxyl group components); and polyester polyols obtained by ring-opening polymerization of lactones such as polycaprolactone, polyvalerolactone, and poly(β-methyl-γ-valerolactone). Two or more of the above carboxyl group components and hydroxyl group components may be used in combination. Among these, aromatic dibasic acids and aliphatic dibasic acids are preferred, and aromatic dibasic acids are even more preferred. When the above components are included, oxygen barrier properties and low residual solvent after bending are further improved. Among aromatic dibasic acids, isophthalic acid and terephthalic acid are preferred, and isophthalic acid is more preferred, and among aliphatic dibasic acids, succinic acid, adipic acid and sebacic acid are preferred, and sebacic acid is even more preferred. As a combination of the dibasic acids, a combination of an aromatic dibasic acid and an aliphatic dibasic acid is preferred, and a combination of isophthalic acid and sebacic acid, or a combination of terephthalic acid and sebacic acid is more preferred, and a combination of isophthalic acid and sebacic acid is even more preferred.
[0078] The content of the aromatic dibasic acid-derived structure in the polyester polyol is preferably 5 to 75% by mass, more preferably 15 to 55% by mass, and even more preferably 25 to 35% by mass. Within this range, the oxygen barrier property after bending and low residual solvent are further improved. Furthermore, the content of the linear dibasic acid-derived structure in the polyester polyol is preferably 1 to 60% by mass, more preferably 5 to 40% by mass, and even more preferably 10 to 20% by mass. Within this range, the oxygen barrier property after bending is further improved and residual solvent is further reduced.
[0079] Examples of the polyether polyol include polyether diols and polyether triols, such as polyether diols obtained by polymerizing an oxirane compound such as ethylene oxide, propylene oxide, butylene oxide, or tetrahydrofuran using water, ethylene glycol, propylene glycol, or a bifunctional low-molecular-weight polyol as an initiator; and polyether triols obtained by polymerizing an oxirane compound such as ethylene oxide, propylene oxide, butylene oxide, or tetrahydrofuran using a low-molecular-weight triol such as trimethylolpropane or glycerin as an initiator.
[0080] The polyol containing a structural unit derived from a polyester polyol or a structural unit derived from a polyether polyol may be a polyester urethane polyol or a polyether urethane polyol obtained by further reacting the polyester polyol or polyether polyol with a diisocyanate, or may be further reacted with an acid anhydride. Examples of the diisocyanate include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, 1,5-naphthalene diisocyanate, hexamethylene diisocyanate, and hydrogenated diphenylmethane diisocyanate. Examples of the acid anhydride include pyromellitic anhydride, mellitic anhydride, trimellitic anhydride, and trimellitic ester anhydride. Examples of trimellitic ester anhydrides include ethylene glycol bisanhydrotrimellitate and propylene glycol bisanhydrotrimellitate.
[0081] The mass average molecular weight (Mw) of the polyol is preferably 2,000 to 80,000, more preferably 5,000 to 60,000, and even more preferably 10,000 to 60,000. Furthermore, by using a polyol having a molecular weight distribution (Mw / Mn) of 1.5 to 10, the leveling properties during adhesive application and the lamination strength between layers can be improved. In particular, when the polyol contains structural units derived from polyether polyol, the molecular weight distribution (Mw / Mn) is preferably 3.0 to 10.0, more preferably 3.0 to 8.0. When the polyol contains structural units derived from polyester polyol, the molecular weight distribution (Mw / Mn) is preferably 1.5 to 5.0, more preferably 2.0 to 4.0.
[0082] The acid value of the polyol is not particularly limited, but is preferably 0 to 50 mgKOH / g, more preferably 0 to 40 mgKOH / g. The hydroxyl value of the polyol is not particularly limited, but is preferably 1 to 200 mgKOH / g, more preferably 3 to 150 mgKOH / g.
[0083] (Isocyanate Curing Agent (I)) The isocyanate curing agent (I) functions as a curing agent for the reactive adhesive, and is suitable for use in ordinary two-component reactive adhesives. Any isocyanate curing agent can be used as long as it contains a functional group reactive with a hydroxyl group. The presence of an isocyanate group increases the adhesive strength and cohesive force of the adhesive, and also enables curing at low temperatures around room temperature.
[0084] The isocyanate curing agent (I) is preferably a diisocyanate or a urethane prepolymer which is a reaction product of a diisocyanate and a polyol, and various known aromatic, aliphatic, or alicyclic diisocyanates can be used as the diisocyanate. For example, 1,5-naphthylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl isocyanate, dialkyldiphenylmethane diisocyanate, tetraalkyldiphenylmethane diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, tolylene diisocyanate, butane-1,4-diisocyanate, hexamethylene diisocyanate, isopropylene diisocyanate, methylene diisocyanate, 2,2, Examples of such diisocyanates include 4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, cyclohexane-1,4-diisocyanate, xylylene diisocyanate, isophorone diisocyanate, lysine diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, methylcyclohexane diisocyanate, m-tetramethylxylylene diisocyanate, and dimer diisocyanate in which the carboxyl groups of dimer acid are converted to isocyanate groups. These may be used alone or in combination of two or more.
[0085] As the isocyanate curing agent (I), a urethane prepolymer having an isocyanate group at its terminal can be suitably used. Among them, from the viewpoints of preventing yellowing and imparting flexibility to improve laminate strength, it is preferable to use aliphatic diisocyanates such as hexamethylene diisocyanate and xylylene diisocyanate, and alicyclic diisocyanates such as isophorone diisocyanate, and from the viewpoint of achieving both retort resistance and retort resistance, it is preferable to use trifunctional or higher polyisocyanate compounds such as adducts of trimethylolpropane, isocyanurates, and biurets.
[0086] In the adhesive layer, the functional group equivalent ratio NCO / OH between the hydroxyl groups derived from the polyol and the isocyanate groups derived from the isocyanate resin is preferably 1.5 to 8.0, and more preferably 2.0 to 5.0. Other components known for adhesives can be blended into the base resin or curing agent of the adhesive.
[0087] (Reaction Accelerator) The adhesive may contain, for example, a reaction accelerator. Examples of reaction accelerators include metal catalysts such as dibutyltin diacetate, dibutyltin dilaurate, dioctyltin dilaurate, and dibutyltin dimaleate; tertiary amines such as 1,8-diaza-bicyclo(5,4,0)undecene-7 and 1,5-diazabicyclo(4,3,0)nonene-5,6-dibutylamino-1,8-diazabicyclo(5,4,0)undecene-7; reactive tertiary amines such as triethanolamine; and titanium-, zinc-, and bismuth-based accelerators. These accelerators may be used alone or in any combination of two or more. Among these, the use of titanium-, zinc-, or bismuth-based accelerators is preferred because they provide excellent aging effects for the adhesive and excellent durability of the packaging material against the contents.
[0088] (Silane Coupling Agent) The adhesive may contain a silane coupling agent, particularly from the viewpoint of improving adhesive strength to metal-based materials such as metal foil. Examples of silane coupling agents include trialkoxysilanes having a vinyl group, such as vinyltriethoxysilane and vinyltriethoxysilane; trialkoxysilanes having an amino group, such as 3-aminopropyltriethoxysilane and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane; and trialkoxysilanes having a glycidyl group, such as 3-glycidoxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)-ethyltrimethoxysilane, and 3-glycidoxypropyltriethoxysilane. These can be used alone or in any combination of two or more. The content of the silane coupling agent is preferably 0.1 to 5% by mass, more preferably 0.2 to 3% by mass, based on the total polyol component. By using the silane coupling agent in the above range, adhesive strength, particularly to metal-based materials, can be further improved.
[0089] (Phosphoric Acid or Phosphoric Acid Derivative) The adhesive may contain phosphoric acid or a phosphoric acid derivative, particularly from the viewpoint of improving adhesive strength to metal materials such as metal foil. The phosphoric acid may be any phosphoric acid having at least one free oxygen acid, such as hypophosphorous acid, phosphorous acid, orthophosphoric acid, or hypophosphoric acid; or condensed phosphoric acids such as metaphosphoric acid, pyrophosphoric acid, tripolyphosphoric acid, polyphosphoric acid, or ultraphosphoric acid. Phosphoric acid derivatives include, for example, phosphoric acids partially esterified with alcohols, while leaving at least one free oxygen acid. Examples of such alcohols include aliphatic alcohols such as methanol, ethanol, ethylene glycol, and glycerin; and aromatic alcohols such as phenol, xylenol, hydroquinone, catechol, and phloroglucinol. These may be used alone or in any combination of two or more. The content of phosphoric acid or a derivative thereof is preferably 0.01 to 10% by mass, more preferably 0.05 to 5% by mass, and even more preferably 0.05 to 1% by mass, based on the solid content of the two-component reactive adhesive.
[0090] (Leveling Agent, Antifoaming Agent) The adhesive may contain a known leveling agent or antifoaming agent. Examples of leveling agents include polyether-modified polydimethylsiloxane, polyester-modified polydimethylsiloxane, aralkyl-modified polymethylalkylsiloxane, polyester-modified hydroxyl group-containing polydimethylsiloxane, polyetherester-modified hydroxyl group-containing polydimethylsiloxane, acrylic copolymer, methacrylic copolymer, polyether-modified polymethylalkylsiloxane, acrylic acid alkyl ester copolymer, methacrylic acid alkyl ester copolymer, and lecithin. Examples of antifoaming agents include silicone resin, silicone solution, and copolymers of alkyl vinyl ether, acrylic acid alkyl ester, and methacrylic acid alkyl ester. These can be used alone or in any combination of two or more. The content of each of the leveling agent and antifoaming agent is preferably 0.001 to 1 mass%, more preferably 0.005 to 0.5 mass%, based on the solids content of the two-component reactive adhesive.
[0091] (Other Additives) Various additives may be blended into the adhesive as long as they do not impair the effects of the present disclosure. Examples of additives include inorganic fillers such as silica, alumina, mica, talc, aluminum flakes, and glass flakes, layered inorganic compounds, stabilizers (antioxidants, heat stabilizers, UV absorbers, hydrolysis inhibitors, etc.), rust inhibitors, thickeners, plasticizers, antistatic agents, lubricants, antiblocking agents, colorants, fillers, crystal nucleating agents, and catalysts for adjusting the curing reaction.
[0092] (Organic Solvent Used in Adhesive) The adhesive may be diluted with a solvent to adjust the viscosity to an appropriate level. Suitable organic solvents used in reactive adhesives are those that are inactive to the polyisocyanate component, such as esters such as ethyl acetate, ketones such as methyl ethyl ketone, and aromatic hydrocarbons such as toluene and xylene, and can be selected as appropriate.
[0093] [Anchor Coat Layer] The packaging material of the present disclosure preferably further includes an anchor coat layer. The anchor coat layer preferably includes a urethane resin. The anchor coat layer is preferably located between the substrate 1 and the barrier layer, and can be formed using an anchor coat agent described below.
[0094] The unit area mass of the anchor coat layer is 0.1 to 5 g / m 2 It is preferable that the density is 0.15 to 3 g / m 2 More preferably, it is 0.2 to 1 g / m 2 When the unit area mass of the anchor coat layer is within the above range, the oxygen barrier property and laminate strength when folded are improved. From the viewpoint of improving the oxygen barrier property and laminate strength after folding, the mass ratio of the anchor coat layer to the barrier layer is preferably 0.1:1 to 2:1, more preferably 0.15:1 to 1:1, and even more preferably 0.2:1 to 0.6:1.
[0095] <Urethane Resin> The urethane resin preferably has a urea bond. Examples of the urethane resin having a urea bond include a urethane urea resin obtained by reacting a terminal isocyanate urethane prepolymer made of a polyol and a polyisocyanate with a polyamine chain extender, and these resins are preferably used.
[0096] The content of the urethane resin is preferably 20 to 90% by mass, more preferably 40 to 85% by mass, and even more preferably 60 to 80% by mass, based on the total mass of the anchor coat layer, since this further improves the oxygen barrier property after bending.
[0097] (Urea Bond Concentration) When the urethane resin has a urea bond, the urea bond concentration is preferably 0.1 to 1.3 mmol / g, more preferably 0.3 to 1.15 mmol / g, and even more preferably 0.6 to 0.9 mmol / g. When the urea bond concentration of the urethane resin is 0.1 mmol / g or more, the laminate strength and oxygen barrier property after bending are further improved. When the urea bond concentration of the urethane resin is 1.3 mmol / g or less, the laminate strength, residual solvent, and oxygen barrier property after bending are further improved.
[0098] Here, the urea bond concentration is a value expressed as follows: When a prepolymer having a terminal isocyanate group is synthesized under conditions such that (number of moles of NCO / number of moles of OH)>1, and then chain-extended with polyamine to give a urethane resin having an amino group at its terminal, the urea bond concentration is expressed by the following (Equation 9): (Equation 9) Urea bond concentration (mmol / g)=[total number of moles of isocyanate groups (mmol)-total number of moles of hydroxyl groups (mmol)] / total mass of solids (g)
[0099] When a prepolymer having a terminal isocyanate group is synthesized under conditions such that (number of moles of NCO / number of moles of OH) > 1, and then chain-extended with a polyamine to give a urethane resin having an isocyanate group at its terminal, the urea bond concentration is expressed by the following (Equation 10): (Equation 10) Urea bond concentration (mmol / g) = (total number of moles of amino groups (mmol)) / total mass of solids (g) Here, the total number of moles of amino groups refers to the total number of moles of primary or secondary amino groups contained in the polyamine used to react with the prepolymer having a terminal isocyanate group to generate urea bonds.
[0100] (Urethane Bond Concentration) The urethane bond concentration of the urethane resin is preferably 0.1 to 1.3 mmol / g, more preferably 0.3 to 1.15 mmol / g, and even more preferably 0.6 to 0.9 mmol / g. When the urethane bond concentration of the urethane resin is within the above range, the oxygen barrier property and laminate strength after bending are improved.
[0101] Here, the urethane bond concentration is a value expressed as follows. When (number of moles of NCO / number of moles of OH) > 1 in the raw materials constituting the urethane resin, the urethane bond concentration is expressed by the following (Equation 11): (Equation 11) Urethane bond concentration (mmol / g) = total number of moles of hydroxyl groups (mmol) / total mass of solids (g) Here, the total number of moles of hydroxyl groups refers to the total number of moles of hydroxyl groups contained in polyols and the like used in the reaction to form urethane. Additionally, the total solids refers to the total mass of non-volatile components that become the urethane resin. When (number of moles of NCO / number of moles of OH) < 1 in the raw materials constituting the urethane resin, the urethane bond concentration is expressed by the following (Equation 12).
[0102] (Equation 12) Urethane bond concentration (mmol / g) = total number of moles of isocyanate groups (mmol) / total mass of solids (g) Here, the total number of moles of isocyanate groups refers to the total number of moles of isocyanate groups contained in the polyisocyanate used in the reaction to form urethane.
[0103] The mass average molecular weight of the urethane resin is preferably 10,000 to 100,000, more preferably 20,000 to 85,000, and even more preferably 30,000 to 70,000. When the mass average molecular weight of the urethane resin is within the above range, the oxygen barrier properties after bending are improved.
[0104] The glass transition temperature of the urethane resin is preferably −80 to 20° C., more preferably −60 to 0° C., and even more preferably −40 to −5° C. When the glass transition temperature of the urethane resin is within the above range, the oxygen barrier property after bending is improved.
[0105] The amine value of the urethane resin is preferably 0.5 to 20 mgKOH / g, and more preferably 1 to 15 mgKOH / g. When the amine value of the urethane resin is within the above range, the oxygen barrier property after bending is improved.
[0106] The hydroxyl value of the urethane resin is preferably 0.5 to 30 mgKOH / g, and more preferably 1 to 20 mgKOH / g. When the hydroxyl value of the urethane resin is within the above range, the oxygen barrier property after bending is improved.
[0107] The urethane resin preferably contains a structural unit derived from a polyester polyol, and the content thereof is preferably 5 to 80 mass %, more preferably 30 to 70 mass %, based on 100 mass % of the urethane resin solid content. When the content of the structural unit derived from a polyester polyol is within the above range, the oxygen barrier property after bending is improved.
[0108] The method for producing the urethane resin is not particularly limited, and any known method can be used. For example, a urethane resin obtained by reacting a urethane prepolymer having a terminal isocyanate, which is composed of a polyol and a polyisocyanate, with a polyamine and, if necessary, a polymerization terminator, is preferred.
[0109] More specifically, known methods can be used, such as a prepolymer method in which a polyol and a polyisocyanate are reacted (urethanization reaction) at a temperature of 50°C to 150°C, optionally using a solvent inert to isocyanate groups, and if necessary, using a urethanization catalyst, to produce a prepolymer having an isocyanate group at its terminal, and then this prepolymer is reacted with a polyamine at 10°C to 60°C to obtain a urethane resin, or a one-shot method in which a high molecular weight polyol, a polyisocyanate, and a polyamine (and, if necessary, a polymerization terminator) are reacted in one step to obtain a urethane resin. Polyamine can also be used in the urethanization reaction of a polyol and a polyisocyanate.
[0110] Examples of polyols include polyester polyols, polyether polyols, polycaprolactone diols, polycarbonate polyols, polyolefin polyols, castor oil polyols, hydrogenated castor oil polyols, dimer diols, and hydrogenated dimer diols. Of these, polyester polyols are preferred.
[0111] Examples of polyester polyols include condensates obtained by esterification of dibasic acids and diols. Examples of dibasic acids include adipic acid, phthalic anhydride, isophthalic acid, terephthalic acid, maleic acid, fumaric acid, succinic acid, oxalic acid, malonic acid, pimelic acid, azelaic acid, sebacic acid, suberic acid, glutaric acid, 1,4-cyclohexyldicarboxylic acid, dimer acid, and hydrogenated dimer acid. Among these, sebacic acid and adipic acid are particularly preferred. Examples of diols include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,3-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2-methyl-1,3-propanediol, 3,3,5-trimethylpentanediol, 2,4-diethyl-1,5-pentanediol, 1,12-octadecanediol, 1,2-alkanediol, 1,3-alkanediol, 1-monoglyceride, 2-monoglyceride, 1-monoglycerin ether, 2-monoglycerin ether, dimer diol, and hydrogenated dimer diol. Among these, polyester polyols composed of a diol having a branched structure and a dibasic acid are preferred. The term "branched structure" refers to a diol having an alkyl side chain in which at least one hydrogen atom of the alkylene group contained in the diol is substituted with an alkyl group, and examples thereof include propylene glycol, 1,3-butanediol, 2-methyl-1,3-propanediol, neopentyl glycol, 1,4-pentanediol, 3-methyl-1,5-pentanediol, 2,5-hexanediol, 2-methyl-1,4-pentanediol, 2,4-diethyl-1,5-pentanediol, 2-butyl-2-ethyl-1,3-propanediol, 2-methyl-1,8-octanediol, 2,2,4-trimethyl-1,3-pentanediol, and 2,2,4-trimethyl-1,6-hexanediol. These polyester polyols are particularly preferred because they improve printability, printing effects, and laminate strength. These polyester polyols can be used alone or in combination.It is also possible to use polyester polyol in combination with a polyol having three or more hydroxyl groups and / or a polycarboxylic acid having three or more carboxyl groups.
[0112] The number average molecular weight of the polyester polyol is preferably 500 to 10,000. The number average molecular weight of the polyol is calculated by (Equation 13). The acid value of the polyester polyol is preferably 1.0 mg KOH / g or less, and more preferably 0.5 mg KOH / g or less. (Equation 13) Number average molecular weight of polyol = 1000 x 56.1 x hydroxyl group valence / hydroxyl group value
[0113] In the production of the urethane resin, the polyol may contain a low-molecular-weight diol. Such low-molecular-weight diols preferably have a molecular weight of 50 to 800, and examples thereof include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,3-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2-methyl-1,3-propanediol, 3,3,5-trimethylpentanediol, 2,4-diethyl-1,5-pentanediol, 1,12-octadecanediol, 1,2-alkanediol, 1,3-alkanediol, 1-monoglyceride, 2-monoglyceride, 1-monoglycerin ether, 2-monoglycerin ether, dimer diol, and hydrogenated dimer diol.
[0114] Examples of polyisocyanates include various known aromatic diisocyanates, aliphatic diisocyanates, alicyclic diisocyanates, etc. that are commonly used in the production of urethane resins. Specific examples include 1,5-naphthylene diisocyanate, 4,4'-diphenylmethane diisocyanate (MDI), 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl isocyanate, dialkyldiphenylmethane diisocyanate, tetraalkyldiphenylmethane diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, tolylene diisocyanate, butane-1,4-diisocyanate, hexamethylene diisocyanate, isopropylene diisocyanate, methylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, and lysine diisocyanate. Examples of suitable polyisocyanates include cyclohexane-1,4-diisocyanate, xylylene diisocyanate, isophorone diisocyanate, dimeryl diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, methylcyclohexane diisocyanate, norbornane diisocyanate, m-tetramethylxylylene diisocyanate, 4,4-diphenylmethane diisocyanate, bis-chloromethyl-diphenylmethane-diisocyanate, 2,6-diisocyanato-benzyl chloride, and dimer diisocyanates in which the carboxyl groups of dimer acids are converted to isocyanate groups. These may be trimers to form an isocyanurate ring structure. These polyisocyanates may be used alone or in combination of two or more. Among these, tolylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, hexamethylene diisocyanate, and isocyanurates of hexamethylene diisocyanate are preferred.
[0115] The polyamine preferably has a molecular weight of 500 or less, but is not limited to the following, and examples thereof include diamines and polyfunctional amines, such as ethylenediamine, propylenediamine, hexamethylenediamine, pentamethylenediamine, isophoronediamine, dicyclohexylmethane-4,4'-diamine, and p-phenylenediamine, as well as diamines having a hydroxyl group such as 2-hydroxyethylethylenediamine, 2-hydroxyethylpropyldiamine, 2-hydroxyethylpropylenediamine, di-2-hydroxyethylethylenediamine, di-2-hydroxyethylenediamine, di-2-hydroxyethylpropylenediamine, 2-hydroxypropylethylenediamine, di-2-hydroxypropylethylenediamine, and di-2-hydroxypropylethylenediamine. These polyamines can be used alone or in combination of two or more. In particular, the urethane resin preferably contains a structural unit derived from a trifunctional or higher polyfunctional polyamine. Specific examples of polyfunctional polyamines include diethylenetriamine, iminobispropylamine (IBPA, 3,3'-diaminodipropylamine), triethylenetetramine, N-(3-aminopropyl)butane-1,4-diamine (spermidine), 6,6-iminodihexylamine, 3,7-diazanonane-1,9-diamine, and N,N'-bis(3-aminopropyl)ethylenediamine. The polyfunctional polyamine preferably has three amino groups. Furthermore, it is preferable to use it in combination with a diamine. Among these, isophoronediamine, hexamethylenediamine, and iminobispropylamine are preferred.
[0116] The ratio of the total number of moles of amino groups in the polyamine to the number of moles of isocyanate groups in the prepolymer is preferably 1.01 to 2.00, more preferably 1.03 to 1.06.
[0117] Monovalent active hydrogen compounds can also be used as polymerization terminators to stop excessive reactions. Examples of such compounds include, but are not limited to, monoamine compounds having primary or secondary amino groups, such as dialkylamines (e.g., di-n-butylamine) and amino alcohols (e.g., 2-ethanolamine). Furthermore, when introducing carboxyl groups into the urethane resin, amino acids (e.g., glycine, L-alanine) can be used as polymerization terminators. When using a polymerization terminator, the chain extension reaction can be carried out using the polymerization terminator together with a chain extender (polyamine). Alternatively, the polymerization can be terminated by adding the polymerization terminator alone after a certain amount of chain extension reaction has been carried out using the chain extender. While molecular weight control is possible without the use of a polymerization terminator, in this case, adding a prepolymer to a solution containing the chain extender is preferred from the standpoint of reaction control. Amino alcohols are preferred as polymerization terminators, and their content is preferably 0.01 to 2.0% by mass relative to 100% by mass of the urethane resin.
[0118] In producing the prepolymer, the amounts of polyol and polyisocyanate are preferably such that the NCO / OH ratio, which is the ratio of the number of moles of isocyanate groups in the polyisocyanate to the total number of moles of hydroxyl groups in the polymer polyol, is in the range of 1.1 to 3.0, more preferably 1.3 to 2.5.
[0119] In addition, it is preferable to use an organic solvent for synthesizing the prepolymer in terms of reaction control. As the organic solvent, an organic solvent inactive to an isocyanate group is preferable, and examples thereof include ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ethers such as dioxane and tetrahydrofuran; and esters such as ethyl acetate, butyl acetate, and propyl acetate. These can be used alone or as a mixed solvent of two or more kinds.
[0120] Furthermore, a catalyst can be used in synthesizing the prepolymer. Examples of the catalyst include tertiary amine catalysts such as triethylamine and dimethylaniline, and metal catalysts such as tin and zinc. These catalysts can usually be used in the range of 0.001 to 1 mol % based on the polyol compound.
[0121] <Resins used in combination with urethane resin> The anchor coat layer preferably contains, in addition to the urethane resin, a vinyl chloride resin, and a co-used resin such as a polyvinyl acetal resin, a cellulose resin, or a polyamide resin. The co-used resin is preferably a vinyl chloride resin and / or a polyvinyl acetal resin, and more preferably a vinyl chloride resin. The mass ratio of the urethane resin to the co-used resin is preferably 3:7 to 9.9:0.1, more preferably 5:5 to 9.5:0.5, and even more preferably 7:3 to 9:1.
[0122] <Vinyl chloride resin> Vinyl chloride resins include a structure obtained by polymerizing a monomer having an unsaturated double bond (excluding vinyl chloride) and a vinyl chloride monomer. Suitable examples of the vinyl chloride resin include vinyl chloride-acrylic copolymer resin and vinyl chloride-vinyl acetate copolymer resin.
[0123] <Vinyl chloride-acrylic copolymer resin> A vinyl chloride-acrylic copolymer resin is primarily composed of a copolymer of vinyl chloride and an acrylic monomer, and the acrylic monomer is a monomer having an acrylic group or a methacrylic group, and preferably contains an acrylic monomer having a hydroxyl group. (Hereinafter, "acrylic or methacrylic" may be referred to as "(meth)acrylic.") The vinyl chloride-acrylic copolymer resin may be a block copolymer or random copolymer of vinyl chloride and an acrylic monomer, or a graft copolymer in which an acrylic monomer is grafted onto the side chain of polyvinyl chloride.
[0124] The weight average molecular weight of the vinyl chloride-acrylic copolymer resin is preferably 10,000 to 100,000, and more preferably 30,000 to 70,000. The glass transition temperature of the vinyl chloride-acrylic copolymer resin is preferably 50 to 90°C, more preferably 55 to 85°C, and even more preferably 65 to 80°C. The hydroxyl acid value of the vinyl chloride-acrylic copolymer resin is preferably 10 to 120 mgKOH / g, more preferably 20 to 110 mgKOH / g, even more preferably 30 to 100 mgKOH / g, and particularly preferably 40 to 80 mgKOH / g. The content of vinyl chloride-derived structures in the vinyl chloride-acrylic copolymer resin is preferably 70 to 95% by mass based on 100% by mass of the vinyl chloride-acrylic copolymer resin solids content.
[0125] Examples of (meth)acrylic monomers having a hydroxyl group include hydroxyalkyl (meth)acrylates, such as hydroxyalkyl (meth)acrylate esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate; glycol mono(meth)acrylates such as polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, and 1,4-cyclohexanedimethanol mono(meth)acrylate; caprolactone-modified (meth)acrylates; and hydroxyethyl acrylamide. Among these, 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 2-hydroxypropyl (meth)acrylate are preferred. These can be used alone or in combination of two or more.
[0126] The (meth)acrylic monomer may contain a (meth)acrylic acid alkyl ester. The number of carbon atoms in the alkyl group in the (meth)acrylic acid alkyl ester is preferably 1 to 20. Examples of the alkyl acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, tetradecyl (meth)acrylate, hexadecyl (meth)acrylate, and octadecyl (meth)acrylate. The alkyl group may have an aromatic ring structure substituted with an aryl group or the like. These may be used alone or in combination of two or more.
[0127] As the vinyl chloride-acrylic copolymer resin, for example, commercially available products such as Solbin A Type Series (manufactured by Shin-Etsu Chemical Co., Ltd.) can be used.
[0128] <Vinyl Chloride-Vinyl Acetate Copolymer Resin> A vinyl chloride-vinyl acetate copolymer resin is a resin obtained by copolymerizing at least vinyl chloride and vinyl acetate. Its mass average molecular weight is preferably 5,000 to 100,000, and more preferably 20,000 to 70,000. The content of structures derived from vinyl acetate monomers in 100% by mass of the solids content of the vinyl chloride-vinyl acetate copolymer resin is preferably 1 to 30% by mass, and the content of structures derived from vinyl chloride monomers is preferably 70 to 95% by mass. Furthermore, since the vinyl chloride-vinyl acetate copolymer resin has improved solubility in organic solvents, it is more preferable that it contains hydroxyl groups derived from vinyl alcohol resulting from a saponification reaction or copolymerization, and its hydroxyl value is preferably 20 to 200 mgKOH / g. Furthermore, the glass transition temperature of the vinyl chloride-vinyl acetate copolymer resin is preferably 50°C to 90°C.
[0129] As the vinyl chloride-acrylic copolymer resin, commercially available products such as Solbin C type series (manufactured by Shin-Etsu Chemical Co., Ltd.) can be used.
[0130] <Polyvinyl acetal resin> Polyvinyl acetal resins are acetalized by reacting polyvinyl alcohol with an aldehyde such as butyraldehyde, and preferably contain vinyl alcohol units, vinyl acetate units, and acetal ring units. For the acetalization reaction, known aldehydes such as formaldehyde and acetaldehyde can be used, and two or more aldehydes can also be used. Examples of polyvinyl acetal resins include polyvinyl formal, polyvinyl acetal, and polyvinyl butyral, and polyvinyl butyral is preferred.
[0131] The content of acetal rings in the polyvinyl acetal resin is preferably 60 to 90% by mass, based on 100% by mass of the polyvinyl acetal resin. When the content of acetal rings is within the above range, laminate strength is further improved. The content of vinyl alcohol units in the polyvinyl acetal resin is preferably 5 to 30% by mass, and more preferably 15 to 25% by mass, based on 100% by mass of the polyvinyl acetal resin. When the content of vinyl alcohol units is within the above range, laminate strength is further improved. The content of vinyl acetate units in the polyvinyl acetal resin is preferably 0.5 to 10% by mass, and more preferably 1 to 5% by mass, based on 100% by mass of the polyvinyl acetal resin. When the content of vinyl acetate units is within the above range, laminate strength is further improved.
[0132] The weight average molecular weight of the polyvinyl acetal resin is preferably 25,000 to 200,000, more preferably 40,000 to 150,000, and even more preferably 70,000 to 120,000. When the weight average molecular weight of the polyvinyl acetal resin is within the above range, the laminate strength is improved. The glass transition temperature of the polyvinyl acetal resin is preferably 50 to 80°C, and more preferably 60 to 75°C. When the glass transition temperature of the polyvinyl acetal resin is within the above range, the laminate strength is improved.
[0133] As the polyvinyl acetal resin, commercially available products such as the Mobital series (manufactured by Kuraray Co., Ltd., polyvinyl butyral resin), the S-Lec KX series (manufactured by Sekisui Chemical Co., Ltd., polyvinyl acetal resin), and the Vinylec series (manufactured by JNC Corporation, polyvinyl formal) can be used.
[0134] <Inorganic Pigment> The anchor coat layer preferably contains an inorganic pigment, since this improves the oxygen barrier property after bending. Examples of inorganic pigments include titanium oxide, zinc oxide, zinc sulfide chromium oxide, aluminum particles, mica, bronze powder, chrome vermilion, yellow lead, cadmium yellow, cadmium red, ultramarine, Prussian blue, red iron oxide, yellow iron oxide, iron black, silica, barium sulfate, kaolin clay, calcium carbonate, and magnesium carbonate are preferred, and silica is particularly preferred.
[0135] The content of the inorganic pigment is preferably 0.5 to 15% by mass, more preferably 1 to 10% by mass, and even more preferably 3 to 7% by mass, relative to 100% by mass of the anchor coat layer.
[0136] <Isocyanate Curing Agent (I')> In order to improve the lamination strength and oxygen barrier properties after bending, the anchor coat layer preferably contains a cured product derived from the isocyanate curing agent (I'). That is, the anchor coating agent for forming the anchor coat layer preferably contains the isocyanate curing agent (I'). When the anchor coating agent contains the isocyanate curing agent (I'), it reacts with a urethane resin or the like, or the isocyanate curing agent (I') reacts with itself to form a cured product. The cured product is formed by the reaction between the urethane resin and the isocyanate curing agent (I'). That is, it preferably has a structure derived from the urethane resin and a structure derived from the isocyanate curing agent (I'). The isocyanate curing agent (I') may be the same as or different from the <Isocyanate Curing Agent (I)> described in [Adhesive Layer].
[0137] Examples of the isocyanate curing agent (I') include aromatic isocyanate curing agents such as m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 3,3'-dimethyl-4,4'-biphenylene diisocyanate, 3,3'-dimethoxy-4,4'-biphenylene diisocyanate, 3,3'-dichloro-4,4'-biphenylene diisocyanate, 1,5-naphthalene diisocyanate, 1,5-tetrahydronaphthalene diisocyanate, xylylene diisocyanate, and tetramethylxylylene diisocyanate; tetramethylene diisocyanate, 1,6-hexamethylene diisocyanate, dodecamethylene diisocyanate, and trimethylhexamethylene diisocyanate. aliphatic isocyanate curing agents such as cyclohexane-1,4-diisocyanate, hydrogenated xylylene diisocyanate, lysine diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, and 3,3'-dimethyl-4,4'-dicyclohexylmethane diisocyanate; alicyclic isocyanate curing agents such as cyclohexane-1,4-diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, methylcyclohexane diisocyanate, and norbornane diisocyanate; and adduct-type isocyanate curing agents, which are adducts of the above-mentioned isocyanate curing agents and polyhydric alcohols. Among these, aliphatic isocyanate curing agents are preferred, adduct type aliphatic isocyanate curing agents are more preferred, and trifunctional adduct type aliphatic isocyanate curing agents are even more preferred.
[0138] Examples of the polyhydric alcohol include 1,2-propylene glycol (dihydric), diethylene glycol (dihydric), dipropylene glycol (dihydric), 1,3-butanediol (dihydric), neopentyl glycol (dihydric), trimethylolpropane (trihydric), 2,2,4-trimethyl-1,3-pentanediol (trihydric), polyethylene glycol (polyhydric), and polypropylene glycol (polyhydric), with trimethylolpropane being preferred. A trifunctional adduct-type aliphatic isocyanate is obtained by reacting a trihydric alcohol with an aliphatic isocyanate curing agent. A suitable example of the adduct-type aliphatic isocyanate curing agent is the reaction product of 1,6-hexamethylene diisocyanate and trimethylolpropane.
[0139] As the isocyanate curing agent (I'), commercially available products can be used, for example, 24A-100, 22A-75, TPA-100, TSA-100, TSS-100, TAE-100, TKA-100, P301-75E, E402-808, E405-70B, AE700-100, D101, D201, A201H (manufactured by Asahi Kasei Corporation), Mytec Y260A (manufactured by Mitsubishi Chemical Corporation), Coronate CORONATE HX, Coronate CORONATE HL, Coronate CORONATE L (manufactured by Nippon Polyurethane Co., Ltd.), Desmodur N75MPA / X (manufactured by Bayer AG).
[0140] In the anchor coat layer, in the cured product composed of a urethane resin and an isocyanate curing agent (I'), the mass ratio of the structural units derived from the urethane resin to the structural units derived from the isocyanate curing agent (I') is preferably 99:1 to 70:30, more preferably 98:2 to 80:20, and even more preferably 95:5 to 85:15. When a co-resin is contained in addition to the urethane resin, the mass ratio of the total amount of the urethane resin and the co-resin to the isocyanate curing agent (I') is preferably 99:1 to 70:30, more preferably 98:2 to 80:20, and even more preferably 95:5 to 85:15. When the mass ratio of the resin to the isocyanate curing agent (I') is within the above range, the oxygen barrier properties and laminate strength after bending are improved.
[0141] <Additives> The anchor coat layer preferably contains known additives or structures derived from additives. Examples of the additives include pigment derivatives, dispersants, wetting agents, adhesion aids, leveling agents, antifoaming agents, antistatic agents, trapping agents, antiblocking agents, waxes, silane coupling agents, and water.
[0142] <Anchor Coating Agent> When the anchor coating layer is formed using an anchor coating agent, the anchor coating agent preferably contains a urethane resin. Furthermore, in order to improve the handling of the anchor coating agent and the oxygen barrier properties after bending, optional components such as organic solvents, co-resins, inorganic pigments, and additives can be added to the anchor coating agent alone or in combination.
[0143] The anchor coating agent can be obtained, for example, by charging a resin solution prepared by dissolving a resin in an organic solvent and an organic solvent into a mixer equipped with a stirring blade, rotor, etc. There are no particular restrictions on the stirring speed, and the mixture can be stirred at 50 to 2000 rpm.
[0144] <Organic Solvent> Examples of organic solvents that can be used in the anchor coating agent include non-aromatic organic solvents such as hydrocarbons such as methylcyclohexane and ethylcyclohexane; ketones such as acetone, methyl ethyl ketone (MEK), and methyl isobutyl ketone; esters such as ethyl acetate, n-propyl acetate, and butyl acetate; and alcohols such as methanol, ethanol, propanol, isopropanol (IPA), and butanol. The organic solvent may be appropriately selected taking into consideration factors such as reducing the amount of solvent remaining in the coating after printing, and may be used alone or in combination of two or more. The content of the organic solvent is preferably 30 to 95% by mass, more preferably 50 to 90% by mass, and particularly preferably 70 to 85% by mass, of 100% by mass of the anchor coating agent.
[0145] In one embodiment, the anchor coating agent preferably contains a glycol ether-based solvent to improve laminate strength. Examples of glycol ether-based solvents include, but are not limited to, ethylene glycol ethers and propylene glycol ethers. Among these, propylene glycol monomethyl ether, diethylene glycol monoethyl ether, and diethylene glycol monobutyl ether are preferred, with diethylene glycol monoethyl ether being more preferred. The glycol ether-based solvent preferably accounts for 5 to 25% by mass, and particularly preferably 5 to 15% by mass, of 100% by mass of the organic solvent in the anchor coating agent.
[0146] <Formation of Anchor Coat Layer> The anchor coat layer can be formed, for example, by printing an anchor coating agent on the substrate 1 and then removing the volatile components. Examples of printing methods include conventionally known methods such as gravure printing, flexographic printing, dipping, roll coating, screen printing, and spraying. The gravure printing method is preferred; for example, the agent is diluted with a diluting solvent to a viscosity and concentration suitable for gravure printing, and then supplied to each printing unit alone or in a mixture, and printed. The anchor coat layer can then be obtained by fixing the coating by drying in an oven or the like.
[0147] [Printed Layer] The packaging material of the present disclosure may have a printed layer. The printed layer preferably contains a resin and a colorant. The printed layer can be a layer that displays any design, pattern, letter, symbol, etc. for the purpose of providing decoration or aesthetic appeal; indicating the contents, expiration date, manufacturer or seller, etc. The printed layer may also be a solid printed layer that does not have any design, pattern, letter, symbol, etc. The method for forming the printed layer is not particularly limited, and it can be formed using, for example, printing ink. The printed layer may have a single-layer structure or a multi-layer structure, and may be provided as a surface layer.
[0148] [Method for Producing Packaging Material] The method for producing a packaging material according to the present disclosure is a method for producing a packaging material having a substrate 1, a barrier layer, an adhesive layer, and a substrate 2, and includes a step of applying a barrier coating agent to form a barrier layer, and a step of applying a reactive adhesive to form an adhesive layer, wherein the barrier layer contains a hydrophilic resin, the adhesive layer is a layer made of a reactive adhesive containing a polyol and an isocyanate curing agent (I), the Permacol value of the polyol is 25 to 60, and the unit area mass of the adhesive layer is 1.0 to 4.5 g / m 2 and the olefin content of the packaging material is 80 mass % or more of the total mass of the packaging material.
[0149] The present disclosure will be described in detail below with reference to examples, but the present disclosure is not limited to these examples. In this specification, parts and % represent parts by mass and % by mass unless otherwise noted.
[0150] <Hydroxyl value> The hydroxyl value is the number of milligrams of potassium hydroxide required to neutralize acetic acid bonded to hydroxyl groups when 1 g of a sample is acetylated, and was measured by the method described in JIS K 0070. <Acid value> The acid value is the number of milligrams of potassium hydroxide required to neutralize free fatty acids, resin acids, etc. contained in 1 g of a sample, and was measured by the method described in JIS K 0070.
[0151] <Amine Value> The amine value is the amount of potassium hydroxide (mg) equivalent to the amount of hydrochloric acid required to neutralize the amino groups contained in 1 g of sample, and was measured in accordance with JIS K 0070. 0.5 to 2 g of sample was precisely weighed (sample solids: S g), and 50 mL of a 60 / 40 (mass ratio) mixed solution of methanol and methyl ethyl ketone was added to the precisely weighed sample for dissolution. Bromophenol blue was added as an indicator to the resulting solution, and the resulting solution was titrated with a 0.2 mol / L ethanolic hydrochloric acid solution (titer: f). The point at which the solution changed color from green to yellow was defined as the endpoint, and the titration volume (A mL) at this point was used to calculate the amine value according to the following formula (13): (Formula 13) Amine value = (A × f × 0.2 × 56.108) / S [mg KOH / g]
[0152] <Weight average molecular weight> The weight average molecular weight was determined by measuring the molecular weight distribution using a gel permeation chromatography (GPC) apparatus (HLC-8220 manufactured by Tosoh Corporation) and calculating the molecular weight as a converted value using polystyrene as a standard substance. The measurement conditions are shown below. Column: The following columns were connected in series and used. TSKgel Super AW2500 manufactured by Tosoh Corporation TSKgel Super AW3000 manufactured by Tosoh Corporation TSKgel Super AW4000 manufactured by Tosoh Corporation TSKgelguard column Super AWH manufactured by Tosoh Corporation Detector: RI (differential refractometer) Measurement conditions: Column temperature 40°C Eluent: tetrahydrofuran Flow rate: 1.0 mL / min
[0153] <Glass Transition Temperature (Tg)> The glass transition temperature was determined by differential scanning calorimetry (DSC). Measurements were performed using a Rigaku DSC8231 at a temperature range of -70 to 250°C and a heating rate of 10°C / min. The midpoint (inflection point) of the baseline shift due to the glass transition in the DSC curve was taken as the glass transition temperature.
[0154] <Measurement of unit area mass of each layer> <Anchor coat layer> In the examples described later, for an intermediate laminate obtained during the production of a laminate, five 10 cm square pieces were cut out from the component part of substrate 1 / anchor coat layer, and five 10 cm square pieces were cut out from substrate 1. The mass of each sample was measured, and the unit area mass of the anchor coat layer was calculated using the following (Equation 14). Note that a uniaxially stretched polyethylene film (MDOPE) with a thickness of 20 μm was used as substrate 1. (Equation 14) The unit area mass (g / m) of the anchor coat layer was calculated using the following (Equation 14) 2 ) = (1 m of 5 samples of [substrate 1 / anchor coat layer] 2 Average mass per 1 m of 5 samples of substrate 1 2 average mass per
[0155] <Layers other than anchor coat layer> For layers other than the anchor coat layer, the unit area mass was calculated in the same manner as for the anchor coat layer, except that the calculation formula and the location where the sample was cut out were different. Note that a low-density polyethylene film (LLDPE) with a thickness of 40 μm was used as the substrate 2. (Equation 15) The unit area mass (g / m) of the barrier layer was calculated using the formula: 2 ) = (1 m of 5 samples of [substrate 1 / anchor coat layer / barrier layer] 2 Average mass per 1 m of 5 samples of [Substrate 1 / anchor coat layer] 2 (Average mass per unit area) (Equation 16) Mass per unit area of adhesive layer (g / m 2 ) = (1 m of 5 samples of [substrate 1 / anchor coat layer / barrier layer / adhesive layer / substrate 2] 2 (average mass per 1 m of 5 samples of [substrate 1 / anchor coat layer / barrier layer]) 2 (average mass per 1 m of 5 samples of substrate 2) + (average mass per 1 m of 5 samples of substrate 2) 2 (average mass per unit)
[0156] <Calculation of Olefin Content in Packaging> The olefin content in the packaging material can be calculated using the following formula 17. (Formula 17) Olefin content in packaging material (%) = (1 m of packaging material) 2 Polyolefin resin mass contained per 1 m of packaging material 2 As an example of calculation, in a structure of [substrate 1 / anchor coat layer / barrier layer / adhesive layer / substrate 2], 2 Mass of polyolefin resin contained per m of base material 1 = (1 m of base material 1) 2 (mass per m of anchor coat layer) × (olefin content in substrate 1) + (1 m of anchor coat layer) 2 (mass per 1 m of barrier layer) × (olefin content in anchor coat layer) + (1 m of barrier layer) 2 (mass per 1 m of adhesive layer) × (olefin content in barrier layer) + (1 m of adhesive layer) 2 (mass per m of substrate 2) × (olefin content in adhesive layer) + (1 m of substrate 2) 2 (mass per 1 m of packaging material) × (olefin content in base material 2) 2 Mass per m of substrate 1 = 2Mass per m of anchor coat layer) + (1 m of anchor coat layer 2 Mass per m of barrier layer) + (1 m of barrier layer 2 Mass per meter of adhesive layer 2 Mass per m of substrate 2) + (1 m of substrate 2) 2 The olefin content in the packaging material can be calculated using Equation 17. 2 The mass per unit area of the substrate may be measured directly or calculated using the substrate thickness and substrate specific gravity as shown in the following formula 18. For other layers, the mass per unit area can be obtained by the method described above in <Measurement of unit area mass of each layer>. (Formula 18) 2 Mass per unit (g / m 2 ) = Base material film thickness (μm) × Base material specific gravity (g / cm 3 )
[0157] (Synthesis of Polyol) <Synthesis Example 1> Polyol PO1 150 parts of ethylene glycol, 350 parts of diethylene glycol, 350 parts of isophthalic acid, and 150 parts of sebacic acid were charged into a reaction vessel equipped with a stirrer, thermometer, reflux condenser, dropping tank, and nitrogen gas inlet tube, and an esterification reaction was carried out at 240 ° C. After a predetermined amount of water was distilled off, the pressure was gradually reduced to 1 mmHg or less and a deglycolization reaction was carried out at 250 ° C. for 5 hours to obtain a polyester polyol. This polyester polyol was diluted with ethyl acetate to a nonvolatile content of 60% to obtain a polyol PO1 solution. The weight average molecular weight of polyol PO1 was 23,000, the number average molecular weight was 13,500, and the Permacol value was 36.0.
[0158] Synthesis Example 2: Polyol PO2: 420 parts of neopentyl glycol, 373 parts of sebacic acid, and 187 parts of adipic acid were charged into a reaction vessel equipped with a stirrer, thermometer, reflux condenser, dropping tank, and nitrogen gas inlet tube, and an esterification reaction was carried out at 240°C. After a predetermined amount of water was distilled off, the pressure was gradually reduced to 1 mmHg or less and a deglycolization reaction was carried out at 250°C for 5 hours. Next, 10 parts of isophorone diisocyanate was added and reacted at 150°C for 2 hours. Further, 10 parts of trimellitic anhydride was added and reacted at 180°C for 2 hours to obtain a polyesterurethane polyol. This polyesterurethane polyol was diluted with ethyl acetate to a nonvolatile content of 60%, yielding a polyol PO2 solution. The polyol PO2 had a mass average molecular weight of 25,000, a number average molecular weight of 11,400, and a Permacol value of 25.9.
[0159] Synthesis Example 3 Polyol PO3 Polyol PO3 was obtained in the same manner as in Synthesis Example 2, except that the raw materials and blending ratios shown in Table 1 were used.
[0160] Synthesis Examples 4 to 6, Comparative Synthesis Example 1 Polyols PO4 to PO6 and PO8 Polyols PO4 to PO6 and PO8 were obtained in the same manner as in Synthesis Example 1, except that the raw materials and blending ratios shown in Table 1 were used.
[0161] Synthesis Example 7 Polyol PO7 A reaction vessel equipped with a stirrer, thermometer, reflux condenser, dropping tank, and nitrogen gas inlet tube was charged with 150 parts of a bifunctional polypropylene glycol having a number average molecular weight of approximately 2,000, 700 parts of a bifunctional polypropylene glycol having a number average molecular weight of approximately 400, 150 parts of a trifunctional polypropylene glycol having a number average molecular weight of approximately 400, and 350 parts of tolylene diisocyanate, and the mixture was heated at 80-90°C for 5 hours with stirring under a nitrogen gas stream to carry out a urethanization reaction, yielding a polyetherurethane polyol. 0.1 parts of phosphoric acid and 0.2 parts of DYNASYLAN GLYMO (EVONIK, 3-glycidoxypropyltrimethoxysilane) were added to the resulting polyetherurethane polyol, and the solids concentration was adjusted to 60% with ethyl acetate to yield a polyol PO7 solution. Polyol PO7 has a weight average molecular weight of 36,000, a number average molecular weight of 10,000, and a Permacol value of 38.8.
[0162] Comparative Synthesis Example 2 Polyol PO9 398 parts of ethylene glycol was added to a reaction vessel equipped with a stirrer, a nitrogen gas inlet tube, a cooling condenser, and a dropping funnel, and the mixture was stirred while heated to 70°C. 602 parts of xylylene diisocyanate was slowly added dropwise thereto over 1 hour. After the dropwise addition, stirring was continued at 70°C for 3 hours, yielding a polyol with a molecular weight of 312 to which 2 moles of ethylene oxide had been added. The polyol PO9 had a mass average molecular weight of 500, a number average molecular weight of 312, and a Permacol value of 79.6.
[0163]
[0164] (Isocyanate Curing Agents) Isocyanate Curing Agent I1: Takenate D-103H (manufactured by Mitsui Chemicals, Inc., solid content: 75%, adduct of toluene diisocyanate and trimethylolpropane, solvent: ethyl acetate) Isocyanate Curing Agent I2: Duranate 22A-75PX (manufactured by Asahi Kasei Corporation, biuret of hexamethylene diisocyanate, solid content: 75%, solvent: ethyl acetate)
[0165] Preparation Example 1 Isocyanate Curing Agent I3 38 parts of Takenate D-103H and 62 parts of Duranate 22A-75PX were mixed with stirring to obtain isocyanate curing agent I3.
[0166] Preparation Example 2 Isocyanate Curing Agent I4 38 parts of Takenate D-103H, 29 parts of Duranate 22A-75PX, and 33 parts of Takenate D-110NB (manufactured by Mitsui Chemicals, Inc., solids content 75%, adduct of xylene diisocyanate and trimethylolpropane, solvent: ethyl acetate) were mixed with stirring to obtain isocyanate curing agent I4.
[0167] Synthesis Example 8 Isocyanate Curing Agent I5 23 parts of bifunctional polypropylene glycol having a number average molecular weight of approximately 2,000, 18 parts of bifunctional polypropylene glycol having a number average molecular weight of approximately 400, 2 parts of trifunctional polypropylene glycol having a number average molecular weight of approximately 400, and 30 parts of 4,4'-diphenylmethane diisocyanate were charged into a reaction vessel and heated at 70 to 80°C for 7 hours with stirring under a nitrogen gas stream to carry out a urethane reaction. After completion of the reaction, 7 parts of a trimethylolpropane adduct of tolylene diisocyanate were mixed in. The mixture was diluted with ethyl acetate to a solids concentration of 75%, yielding a polyisocyanate solution containing polyether urethane polyisocyanate. 80 parts of the polyisocyanate solution and 20 parts of Desmodur L75 (manufactured by Sumika Covestro Urethane Co., Ltd., a trimethylolpropane adduct of toluene diisocyanate, NCO group content 13%, solids concentration 75%) were mixed to prepare an isocyanate curing agent I5 solution.
[0168] Preparation Example 3 Isocyanate Curing Agent I6 38 parts of Takenate D-103H and 62 parts of Takenate D-110NB were mixed with stirring to obtain isocyanate curing agent I6.
[0169] (Synthesis of Urethane Resin) <Synthesis Example 9> Urethane Resin PU1 Ethyl acetate 120.6 parts, 153.7 parts of polyester polyol having a number average molecular weight of 2,000 which is a condensate of 3-methyl-1,5-pentanediol (MPD) and adipic acid (AdA) (hereinafter referred to as "MPD / AdA 2000"), 27.9 parts of polyester polyol having a number average molecular weight of 5,000 which is a condensate of 3-methyl-1,5-pentanediol (MPD) and adipic acid (AdA) (hereinafter referred to as "MPD / AdA 5000"), 12.4 parts of polypropylene glycol having a number average molecular weight of 700 (hereinafter referred to as "PPG 700"), 35.0 parts of polypropylene glycol having a number average molecular weight of 2,000 (hereinafter referred to as "PPG 2000"), isophorone diisocyanate (hereinafter referred to as "IPDI") The mixture was mixed with 52.3 parts of the urethane prepolymer and reacted at 90°C for 5 hours under a nitrogen atmosphere to obtain a terminal isocyanate urethane prepolymer. Next, 279.6 parts of isopropanol, 299.7 parts of ethyl acetate, 2.1 parts of iminobispropylamine (IBPA), and 16.6 parts of isophorone diamine (IPDA) were stirred and mixed, and the resulting terminal isocyanate urethane prepolymer was gradually added at 40°C. The mixture was reacted at 80°C for 1 hour to obtain a solution of urethane resin PU1 with a solids content of 30% by mass, a urea bond concentration of 0.78 mmol / g, an amine value of 1.3 mgKOH / g, and a weight average molecular weight of 36,100.
[0170] Synthesis Examples 10 and 11 Urethane Resins PU2 and 3 Urethane resins PU2 and 3 were obtained in the same manner as in Synthesis Example 1, except that the raw materials and compounding ratios shown in Table 2 were used.
[0171]
[0172] (Production of Anchor Coating Agent) <Production Example 1> Anchor Coating Agent AC1 47 parts of urethane resin PU1 solution, 15 parts of vinyl chloride-vinyl acetate resin PVC1 solution (hydroxyl value: 154 mg KOH / g, mass average molecular weight: 28,000, glass transition temperature: 78°C, solids mass%=25%), 1 part of silica particles S1 (Mizukasil P-707, manufactured by Mizusawa Industrial Chemicals, Ltd., average particle size (laser scattering method): 4 μm, oil absorption: 250 ml / 100 g, solids mass%=100%), 1 part of chlorinated polypropylene (Superchron 390S, manufactured by Nippon Paper Industries Co., Ltd., solids mass%=50%), 0.5 parts of fatty acid amide solution (lauric acid amide, solids mass%=50%), 30.5 parts of mixed solvent (normal propyl acetate (NPAC) / isopropyl alcohol (IPA)=7 / 3), propylene glycol monomethyl ether 3 parts of the pigment dispersion and 2 parts of water were mixed and dispersed for 20 minutes in a bead mill to obtain a pigment dispersion. 20 parts of water were added to the obtained pigment dispersion and mixed with stirring to obtain anchor coating agent AC1.
[0173] <Production Examples 2 to 4> Anchor Coating Agents AC2 to 4 Anchor coating agents AC2 to 4 were obtained in the same manner as in Production Example 1, except that the raw materials and compounding ratios were changed to those shown in Table 3.
[0174]
[0175] (Production of Barrier Coating Agent) <Production Example 5> Barrier Coating Agent V1 6 parts of polyvinyl alcohol resin PVA1 (manufactured by Kuraray Co., Ltd., EXCEVAL AQ-4104, ethylene vinyl alcohol resin, ethylene content: 6 mol%, solids mass %=100%) and 92 parts of a mixed solvent (water / IPA=8 / 2) were heated with stirring, and heating and stirring were continued at 95°C for 1 hour. Thereafter, heating was stopped, and stirring was continued until the temperature returned to room temperature, thereby obtaining an aqueous solution of polyvinyl alcohol resin PVA1. Montmorillonite (swellable, average particle size: 2 μm, aspect ratio: 500, specific surface area: 13.1 m) was added to the aqueous solution of polyvinyl alcohol resin PVA1. 2 / g, particle thickness: 1 nm, average major axis: 500 nm, solid content mass %=100%) was added to the mixture, and the mixture was stirred to obtain barrier coating agent V1.
[0176] <Production Examples 6 to 13, Comparative Production Example 1> Barrier Coating Agents V2 to V10 Barrier coating agents V2 to V10 were obtained in the same manner as in Production Example 5, except that the raw materials and compounding ratios were changed as shown in Table 4. The properties of the raw materials used were as follows: Polyvinyl alcohol resin PVA2: Kuraray Co., Ltd., Kuraray Poval 28-98, polyvinyl alcohol, solids mass % = 100% Polyvinyl alcohol resin PVA3: Sekisui Chemical Co., Ltd., ULTILOC5003, amine-modified polyvinyl alcohol, solids mass % = 100% Acrylic resin A1: Nippon Shokubai Co., Ltd., AQUALIC HL415, mass average molecular weight 10,000, solids mass % = 45% Bentonite: BYK Corporation, CLOISITE-Na+ Mica: average particle size: 6 μm, aspect ratio 100, specific surface area 9 m 2 / g, solid content mass% = 100% Kaolin: average particle size 1.2 μm, aspect ratio 100, specific surface area 10 m 2 / g, solid content mass% = 100%
[0177]
[0178] (Production of Packaging Materials) Example 1 Packaging Material P1 100 parts of anchor coating agent AC1 was diluted with a mixed solvent (isopropyl alcohol / ethyl acetate) to a Zahn cup #3 (manufactured by Rigo Co., Ltd.) hardness of 15 seconds (25°C), and then 3 parts of isocyanate curing agent H1 (manufactured by Asahi Kasei Corporation, Duranate P-301-75E, hexamethylene diisocyanate-based (aliphatic), adduct type, solids content 50%) was added and mixed with stirring. Also, 100 parts of barrier coating agent V1 was diluted with a mixed solvent (isopropyl alcohol / water) to a Zahn cup #3 (manufactured by Rigo Co., Ltd.) hardness of 16 seconds (25°C). Then, a thickness of 20 μm and a specific gravity of 0.92 g / cm were applied. 3A gravure printing press equipped with a 15 μm deep gravure plate was used to print the diluted anchor coating agent AC1 containing the curing agent H1 onto the surface of a uniaxially stretched polyethylene film (MDOPE) at a printing speed of 50 m / min and an in-line oven temperature of 60°C to form an anchor coat layer. A gravure printing press equipped with a 30 μm deep gravure plate with a non-image area on one half of the plate was used to print the diluted barrier coating agent V1 twice to form a barrier layer, yielding an intermediate laminate p1 consisting of MDOPE (substrate 1) / anchor coat layer / barrier layer. Next, polyol PO1 was mixed with ethyl acetate, and then isocyanate curing agent I1 was added and mixed again to form an adhesive solution. The solids ratio of polyol PO1 to isocyanate curing agent I1 was 95 / 5, and the solids content of the adhesive solution was 23%. Thereafter, an adhesive solution was applied onto the barrier layer of the intermediate laminate p1 using a dry laminating machine equipped with a gravure plate with a plate depth of 60 μm, and the solvent was dried in an oven to form an adhesive layer. After that, a 40 μm thick, 0.91 g / cm specific gravity adhesive was applied onto the adhesive layer at a line speed of 40 m / min. 3 The resulting mixture was then kept at 40°C for 1 day to obtain a packaging material P1 having a structure of MDOPE (substrate 1) / anchor coat layer / barrier layer / adhesive layer / LLDPE (substrate 2). The unit area mass of the anchor coat layer of packaging material P1 was 0.4 g / m 2 , the mass per unit area of the barrier layer is 1.0 g / m 2 , the mass per unit area of the adhesive layer is 3.0 g / m 2 It was.
[0179] <Examples 2 to 22, Comparative Examples 1 to 7> Packaging materials P2 to 29 Packaging materials P2 to 29 were obtained in the same manner as in Example 1, except that the raw materials and coating conditions were changed as shown in Tables 5 and 6. The materials used were as follows: Thickness: 15 μm, specific gravity: 1.15 g / cm 3 Nylon film (NY)
[0180] Example 23 A packaging material P30 was produced in the same manner as in Example 1, except that no anchor coat layer was formed on the substrate 1. The evaluation results for each item described below were: laminate strength: 3, residual solvent: 4, oxygen barrier property after bending: 3.
[0181] (Evaluation) The packaging materials obtained in the above Examples and Comparative Examples were evaluated as follows. The results are shown in Tables 5 and 6.
[0182] <Laminate Strength> The laminates obtained in the above Examples and Comparative Examples were each cut into a rectangle 150 mm long and 15 mm wide, and substrate 1 was peeled off from substrate 2 at one end. Substrate 1 and substrate 2 were then each set in the chuck of a tensile tester, and the laminate strength in the 90° direction was measured and evaluated according to the following criteria. 3 to 5 are practically acceptable ranges. <Evaluation Criteria> 5: 1.5 N / 15 mm or more 4: 1.2 N / 15 mm or more but less than 1.5 N / 15 mm 3: 1.0 N / 15 mm or more but less than 1.2 N / 15 mm 2: 0.8 N / 15 mm or more but less than 1.0 N / 15 mm 1: Less than 0.8 N / 15 mm
[0183] <Residual Solvent> The obtained packaging material was cut into 10 rectangular pieces of 50 mm x 10 mm, placed in a headspace vial (manufactured by Agilent, 75.5 mm x 23 mm), and heated at 80°C for 30 minutes in a sealed state. After that, a certain amount of solvent vapor was taken out with a microsyringe, and the amount of volatile solvent was confirmed by gas chromatography (manufactured by GL Science, GC-4000), and evaluated according to the following criteria. Note that 3 to 5 are in the range where there is no problem in practical use. <Evaluation Criteria> 5: 2.0 mg / m 2 Less than 4: 2.0 mg / m 2 Above, 3.0mg / m 2 Less than 3: 3.0 mg / m 2 Above, 4.0mg / m 2 Less than 2: 4.0 mg / m 2 Above, 5.0mg / m 2 Less than 1: 5.0 mg / m 2 End
[0184] <Oxygen Barrier Property After Bending> The obtained packaging material was cut into a 100 mm square, and folded so that the surfaces of the base material 2 overlapped each other. A pressure of 1 kg / m was applied to the folded portion.2 The sample was unfolded and unfolded, and the oxygen transmission rate (OTR) was measured using an oxygen transmission rate measuring device OC-TRAN manufactured by MOCON Corporation in accordance with JIS K 7162 Method B (constant pressure method) at a temperature of 30°C and a relative humidity of 70%, and evaluated according to the following criteria. 3 to 5 are ranges that are acceptable for practical use. Evaluation criteria: 5: Oxygen transmission rate is 100 cc / m 2 / day / atm. 4: Oxygen permeability is less than 100 cc / m 2 / day / atm or more, 1000cc / m 2 / day / atm. 3: Oxygen permeability is less than 1000 cc / m 2 / day / atm or more, 1500cc / m 2 / day / atm. 2: Oxygen permeability is less than 1500 cc / m 2 / day / atm or more, 2000cc / m 2 / day / atm. 1: Oxygen permeability is less than 2000 cc / m 2 / day / atm or more.
[0185]
[0186]
[0187]
[0188] From the above results, Comparative Example 1 did not have a barrier layer, and therefore the residual solvent evaluation and oxygen barrier property after bending were poor. Comparative Example 2 did not have a barrier layer, and therefore the residual solvent evaluation and oxygen barrier property after bending were poor. Comparative Example 3 had a Permacol value of the polyol of less than 25, and therefore the oxygen barrier property after bending was poor. Comparative Example 4 had a Permacol value of the polyol of more than 60, and therefore the lamination strength and residual solvent evaluation were poor. Comparative Example 5 had an adhesive with a unit area mass of 1.0 g / m 2 In Comparative Example 6, the lamination strength and the oxygen barrier property after bending were poor. 2In Comparative Example 7, the olefin content in the packaging material was less than 80% by mass of the total mass of the packaging material, and therefore the residual solvent evaluation was poor. On the other hand, the packaging materials of the Examples have a barrier layer containing a hydrophilic resin, an adhesive layer having a structure derived from a polyol with a Permacol value of 25 to 60, and a unit area mass of the adhesive layer of 1.0 to 4.5 g / m 2 and the olefin content of the packaging material was 80 mass% or more of the total mass of the packaging material. Therefore, it was shown that the present disclosure can provide a packaging material that is excellent in lamination strength and oxygen barrier property after folding, and has little residual solvent.
[0189] Although the present invention has been described with reference to the above-mentioned several embodiments, the present invention is not limited to these several embodiments. Various modifications can be made to the configuration and details of the present invention within the scope of the present invention.
[0190] The disclosure of this application is related to the subject matter described in Japanese Patent Application No. 2023-088032, filed on May 29, 2023, the entire disclosure of which is incorporated herein by reference.
Claims
1. A packaging material having a substrate 1, a barrier layer, an adhesive layer, and a substrate 2, wherein the barrier layer contains a hydrophilic resin, the adhesive layer is a layer containing a cured product of a polyol and an isocyanate curing agent (I), the polyol has a Permacol value of 25 to 60, and the adhesive layer has a unit area mass of 1.0 to 4.5 g / m 2 The packaging material has an olefin content of 80 mass% or more based on the total mass of the packaging material.
2. The packaging material according to claim 1, wherein the hydrophilic resin is a polyvinyl alcohol-based resin.
3. The packaging material according to claim 1 or 2, wherein the barrier layer further comprises an inorganic layered filler.
4. The mass per unit area of the barrier layer is 0.7 g / m 2 The packaging material according to claim 1 or 2.
5. The packaging material according to claim 1 or 2, wherein the polyol has a polyester structure.
6. The packaging material according to claim 1 or 2, wherein the ratio of the mass per unit area of the barrier layer to the mass per unit area of the adhesive layer is from 70:30 to 15:
85.
7. The packaging material according to claim 1 or 2, further comprising an anchor coat layer, the anchor coat layer comprising a urethane resin.
8. The packaging material according to claim 7, wherein the urea bond concentration of the urethane resin is 0.1 to 1.3 mmol / g.
9. The packaging material according to claim 1 or 2, wherein substrate 1 and substrate 2 contain a polyolefin resin.
10. A method for producing a packaging material having a substrate 1, a barrier layer, an adhesive layer, and a substrate 2, comprising the steps of applying a barrier coating agent to form a barrier layer, and applying a reactive adhesive to form an adhesive layer, wherein the barrier layer contains a hydrophilic resin, the adhesive layer is a layer made of a reactive adhesive containing a polyol and an isocyanate curing agent (I), the polyol has a Permacol value of 25 to 60, and the adhesive layer has a unit area mass of 1.0 to 4.5 g / m 2 The packaging material has an olefin content of 80 mass% or more based on the total mass of the packaging material.
Citation Information
Patent Citations
Gas barrier film
JP2001129915A
Gas barrier laminated film
JP2007136984A
Gas barrier hardener resin composition and adhesive
JP2013129780A
Power feeding device and luminaire
JP2023088032A
Ultraviolet screening packaging material and ultraviolet screening packaging bag using it