Slurry composition for dielectric layers, dielectric layer, and capacitor
The slurry composition for dielectric layers, featuring a perovskite dielectric material and specific water-soluble polymers, addresses stability and redispersibility issues, ensuring uniformity and handling improvements in capacitor production.
Patent Information
- Application Number
- PCT/JP2024/017145
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-08
- Publication Date
- 2024-12-05
AI Technical Summary
The existing slurry compositions for dielectric layers in capacitor manufacturing face challenges with dispersion stability and redispersibility, leading to variations in capacitor performance and issues like blocking and powder falling, especially during long-term storage and handling.
A slurry composition containing a dielectric material with a perovskite structure, water-soluble polymers A and B with specific molecular weight ranges, and a solvent, which enhances dispersion stability, redispersibility, and provides excellent blocking and powder drop resistance, allowing for improved handling and uniformity in film thickness.
The proposed slurry composition ensures stable and uniform dielectric layers with enhanced handling properties, reducing performance variations and improving the efficiency of capacitor production by maintaining viscosity and preventing settling and powder loss.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure 00000047_0000
Abstract
Description
Slurry composition for dielectric layer, dielectric layer, and capacitor
[0001] The present invention relates to a slurry composition for a dielectric layer, a dielectric layer, and a capacitor.
[0002] Capacitors such as multilayer ceramic capacitors are generally manufactured using dielectric layers such as ceramic green sheets. The dielectric layers can be obtained, for example, by first preparing a slurry composition containing a binder, a dielectric material, and a solvent, then applying the slurry composition to a release substrate and drying it. The resulting dielectric layers are then stacked, and optionally subjected to degreasing (binder removal) and sintering to obtain a capacitor.
[0003] In recent years, in order to impart excellent characteristics to capacitors, development of slurry compositions used in the production of dielectric layers has been progressing. For example, Patent Document 1 proposes a slurry composition that can produce ceramic green sheets with little binder residue during binder removal treatment and excellent smoothness and ceramic particle density after binder removal treatment, the slurry composition containing a dispersion medium made of an organic solvent, ceramic powder having a predetermined average particle size, and a binder made of a predetermined (meth)acrylate copolymer.
[0004] Patent No. 6337628
[0005] Here, the slurry composition can be stored for a certain period of time (e.g., 7 days) after preparation, and from the viewpoint of uniformly applying the slurry composition and suppressing variations in capacitor performance, it is desirable that the slurry composition has little change in viscosity when comparing the viscosity after storage for a certain period of time with the viscosity immediately after preparation, and has excellent dispersion stability.
[0006] Furthermore, the slurry composition may be stored for a longer period (e.g., 30 days) than the above storage period. When the slurry composition is stored for such a long period, the dielectric material may settle in the slurry composition. As described above, from the viewpoint of uniformly applying the slurry composition and suppressing variations in the performance of the capacitor, it is desirable that the settled dielectric material be well redispersed when the slurry composition is stirred after long-term storage.
[0007] Therefore, an object of the present invention is to provide a slurry composition for a dielectric layer having excellent dispersion stability and redispersibility. Another object of the present invention is to provide a dielectric layer obtained by drying a coating film made of the above-mentioned slurry composition for a dielectric layer. Another object of the present invention is to provide a capacitor using the above-mentioned dielectric layer.
[0008] The present inventors have conducted extensive research with the aim of solving the above-mentioned problems, and have newly discovered that the above-mentioned problems can be solved by a slurry composition for a dielectric layer containing a predetermined dielectric material, two water-soluble polymers having predetermined weight-average molecular weights, and a solvent containing water, thereby completing the present invention.
[0009]
[0010] The present invention aims to advantageously solve the above-mentioned problems, and [1] provides a slurry composition for a dielectric layer, comprising a dielectric material having a perovskite structure, a water-soluble polymer A, a water-soluble polymer B, and a solvent, wherein the water-soluble polymer A has a weight-average molecular weight of 100,000 or more and 2,000,000 or less, the water-soluble polymer B has a weight-average molecular weight of 5,000 or more and 80,000 or less, and the solvent contains water. The slurry composition for a dielectric layer has excellent dispersion stability and redispersibility. Furthermore, after forming a dielectric layer on a release substrate, it is usually rolled up together with the release substrate. When rolled up, the dielectric layer is in close contact with the surface of the release substrate on the side where the dielectric layer is not formed (hereinafter, sometimes referred to as the "back surface of the release substrate"). If stored in this state, the dielectric layer may adhere to the back surface of the release substrate (so-called blocking). However, the use of the above-mentioned dielectric layer slurry composition can impart excellent blocking resistance to the dielectric layer. Furthermore, while there is a risk that the dielectric material contained in the dielectric layer may fall off from the dielectric layer (hereinafter, sometimes referred to as "powdering"), the use of the above-mentioned dielectric layer slurry composition can impart excellent powdering resistance to the dielectric layer. In this specification, the "weight average molecular weight" of water-soluble polymer A and water-soluble polymer B can be measured using the method described in the examples of this specification.
[0010] [2] In the dielectric layer slurry composition according to the above [1], the water-soluble polymer A preferably contains an ethylenically unsaturated acid monomer unit. If the water-soluble polymer A contains an ethylenically unsaturated acid monomer unit, the dispersion stability of the dielectric layer slurry composition and the powder shedding resistance of the dielectric layer can be improved.
[0011] [3] In the dielectric layer slurry composition according to [1] or [2] above, the content of the water-soluble polymer B is preferably 0.1 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the dielectric material. When the content of the water-soluble polymer B is equal to or more than the lower limit per 100 parts by mass of the dielectric material, the dispersion stability of the dielectric layer slurry composition can be improved. On the other hand, when the content of the water-soluble polymer B is equal to or less than the upper limit per 100 parts by mass of the dielectric material, the powder shedding resistance of the dielectric layer can be improved. Furthermore, the dielectric layer is provided with appropriate flexibility, which makes it easier to cut the dielectric layer and the laminate including the dielectric layer when fabricating a capacitor.
[0012] [4] In the dielectric layer slurry composition according to any one of [1] to [3] above, the content of the water-soluble polymer A is preferably 0.1 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the dielectric material. When the content of the water-soluble polymer A is equal to or more than the lower limit per 100 parts by mass of the dielectric material, the powder shedding resistance of the dielectric layer can be improved. On the other hand, when the content of the water-soluble polymer A is equal to or less than the upper limit per 100 parts by mass of the dielectric material, the dispersion stability of the dielectric layer slurry composition and the blocking resistance of the dielectric layer can be improved.
[0013] [5] In the slurry composition for a dielectric layer according to any one of [1] to [4] above, the mass ratio of the water-soluble polymer B to the water-soluble polymer A is preferably 0.01 or more and 1 or less. When the mass ratio of the water-soluble polymer B to the water-soluble polymer A is equal to or more than the lower limit, the dispersion stability of the slurry composition for a dielectric layer can be improved. On the other hand, when the mass ratio of the water-soluble polymer B to the water-soluble polymer A is equal to or less than the upper limit, the powder shedding resistance of the dielectric layer can be improved. In addition, the dielectric layer is provided with appropriate flexibility, which results in easy cutting of the dielectric layer and a laminate including the dielectric layer when fabricating a capacitor.
[0014] [6] It is preferable that the dielectric layer slurry composition according to any one of [1] to [5] above further contains a particulate polymer. If the dielectric layer slurry composition further contains a particulate polymer, the redispersibility of the dielectric layer slurry composition and the powder shedding resistance of the dielectric layer can be improved. In this specification, a "particulate polymer" refers to a polymer that has a particulate shape at least in the dielectric layer slurry composition. The particle shape of the particulate polymer can be confirmed, for example, by laser diffraction.
[0015] [7] In the slurry composition for a dielectric layer according to any one of the above [1] to [6], the pH is preferably 8 or more and 12 or less. If the pH is within the above range, the dispersion stability and redispersibility of the slurry composition for a dielectric layer can be improved. In this specification, the pH of the slurry composition for a dielectric layer can be measured using the method described in the examples of this specification.
[0016] Another object of the present invention is to advantageously solve the above-mentioned problems. [8] The present invention provides a dielectric layer formed by drying a coating film made of a dielectric layer slurry composition according to any one of [1] to [7] above. The dielectric layer is formed by drying a coating film made of a dielectric layer slurry composition having excellent dispersion stability and redispersibility, and therefore has excellent film thickness uniformity. The dielectric layer also has excellent resistance to powder shedding. The dielectric layer also has excellent blocking resistance, making it easy to handle, and as a result, capacitors can be produced efficiently.
[0017] Another object of the present invention is to advantageously solve the above-mentioned problems, and [9] the present invention is a capacitor using the dielectric layer of [8] above. The capacitor uses a dielectric layer with excellent film thickness uniformity, so performance variation is suppressed. The capacitor also uses a dielectric layer with excellent resistance to powder shedding, so it has excellent performance. The capacitor also uses a dielectric layer that is easy to handle, so it has excellent productivity.
[0018] According to the present invention, a slurry composition for a dielectric layer having excellent dispersion stability and redispersibility can be provided. Also, according to the present invention, a dielectric layer formed by drying a coating film made of the above-mentioned slurry composition for a dielectric layer can be provided. Also, according to the present invention, a capacitor formed using the above-mentioned dielectric layer can be provided.
[0019] 1 is a schematic cross-sectional view showing an example of a multilayer ceramic capacitor as a capacitor of the present invention.
[0020] Hereinafter, embodiments of the present invention will be described in detail. Hereinafter, the slurry composition for a dielectric layer of the present invention (hereinafter, sometimes simply referred to as "slurry composition") can be used to form a dielectric layer used in the manufacture of a capacitor or the like. The dielectric layer of the present invention is formed by drying a coating film made of the slurry composition of the present invention. The capacitor of the present invention is formed using a dielectric layer formed using the slurry composition of the present invention.
[0021] (Slurry Composition for Dielectric Layer) The slurry composition for a dielectric layer of the present invention comprises a dielectric material having a perovskite structure, a water-soluble polymer A, a water-soluble polymer B, and a solvent, and may optionally comprise a particulate polymer and a water-soluble plasticizer. In the slurry composition of the present invention, the weight-average molecular weight of the water-soluble polymer A is 100,000 or more and 2,000,000 or less, the weight-average molecular weight of the water-soluble polymer B is 5,000 or more and 80,000 or less, and the solvent comprises water. The slurry composition has excellent dispersion stability. This is presumably because, in a water-containing slurry composition, the two water-soluble polymers (water-soluble polymer A and water-soluble polymer B) having predetermined weight-average molecular weights maintain the dispersion state of the dielectric material well, thereby suppressing viscosity changes of the slurry composition over time. The slurry composition also has excellent redispersibility. The reason for this is presumably that when the dielectric material in the slurry composition settles due to long-term storage, the two water-soluble polymers (water-soluble polymer A and water-soluble polymer B) having the predetermined weight-average molecular weight effectively suppress aggregation of the dielectric material. Furthermore, the use of the above-mentioned slurry composition can impart excellent blocking resistance and powder shedding resistance to the dielectric layer. Furthermore, since the slurry composition of the present invention contains water as the solvent, the amount of organic solvent used can be reduced, thereby reducing the environmental impact.
[0022] The slurry composition of the present invention may optionally further contain components other than the dielectric material, water-soluble polymer A, water-soluble polymer B, solvent, particulate polymer, and water-soluble plasticizer (hereinafter, these may be referred to as "other components").
[0023] <Dielectric Material> In the slurry composition of the present invention, the dielectric material has a perovskite structure. Here, the "perovskite structure" refers to a structure represented by the general formula ABO 3 The term "dielectric material having a perovskite structure" means a structure represented by the general formula ABO in at least a part of the dielectric material. 3 It means that there is a structure represented by the following formula: The slurry composition may optionally further contain a dielectric material other than the dielectric material having a perovskite structure.
[0024] As a dielectric material having a perovskite structure, a ceramic material having a perovskite structure as a main phase is preferable. As the ceramic material, for example, barium titanate (BaTiO 3 ), calcium zirconate (CaZrO 3 ), calcium titanate (CaTiO 3 ), strontium titanate (SrTiO 3 ), Ba that forms a perovskite structure 1-x-y Ca x Sr y Ti 1-z Zr z O 3 (0≦x≦1, 0≦y≦1, 0≦z≦1), etc. Among these, barium titanate is preferred as a ceramic material having a perovskite structure as the main phase.
[0025] The average particle size of the dielectric material is preferably 0.01 μm or more, more preferably 0.02 μm or more, even more preferably 0.05 μm or more, even more preferably 0.08 μm or more, and preferably 1 μm or less, more preferably 0.8 μm or less, even more preferably 0.5 μm or less, even more preferably 0.3 μm or less, and even more preferably 0.2 μm or less. If the average particle size of the dielectric material is above the above lower limit, the powder shedding resistance of the dielectric layer can be improved. On the other hand, if the average particle size of the dielectric material is below the above upper limit, the dispersion stability of the slurry composition can be improved. In this specification, the average particle size of the dielectric material means the particle size at which the cumulative volume calculated from the smallest diameter side in the particle size distribution (volume basis) obtained by measurement using a laser diffraction method accounts for 50%.
[0026] The content of the dielectric material in the slurry composition is preferably 40% by mass or more, more preferably 50% by mass or more, and is preferably 80% by mass or less, more preferably 70% by mass or less, when all components in the slurry composition (including the solvent) are taken as 100% by mass.
[0027] <Water-Soluble Polymer A> In the slurry composition of the present invention, the water-soluble polymer A is a component that can function as a viscosity modifier and a binder, and has a weight-average molecular weight of 100,000 or more and 2,000,000 or less.
[0028] Here, examples of monomer units that the water-soluble polymer A may contain include ethylenically unsaturated acid monomer units and (meth)acrylic acid alkyl ester monomer units. Among these, the water-soluble polymer A preferably contains ethylenically unsaturated acid monomer units, since this can improve the dispersion stability of the slurry composition and the powder shedding resistance of the dielectric layer. The water-soluble polymer A may optionally contain monomer units other than the ethylenically unsaturated acid monomer units and the (meth)acrylic acid alkyl ester monomer units (hereinafter, sometimes referred to as "other monomer units A"). In this specification, "(meth)acrylic" means acrylic and / or methacrylic.
[0029] <<Ethylenically Unsaturated Acid Monomer Unit>> Examples of ethylenically unsaturated acid monomers that can form ethylenically unsaturated acid monomer units include carboxylic acid group-containing ethylenically unsaturated monomers, sulfonic acid group-containing ethylenically unsaturated monomers, and phosphoric acid group-containing ethylenically unsaturated monomers. Among these, carboxylic acid group-containing ethylenically unsaturated monomers and sulfonic acid group-containing ethylenically unsaturated monomers are preferred, and carboxylic acid group-containing ethylenically unsaturated monomers are more preferred, as they can further improve the dispersion stability of the slurry composition and the powder shedding resistance of the dielectric layer. That is, the water-soluble polymer A preferably contains at least one of a carboxylic acid group-containing ethylenically unsaturated monomer unit and a sulfonic acid group-containing ethylenically unsaturated monomer unit, and more preferably contains a carboxylic acid group-containing ethylenically unsaturated monomer unit.
[0030] Examples of carboxylic acid group-containing ethylenically unsaturated monomers capable of forming carboxylic acid group-containing ethylenically unsaturated monomer units include ethylenically unsaturated monocarboxylic acids and their derivatives, ethylenically unsaturated dicarboxylic acids and their acid anhydrides, and derivatives thereof. Examples of ethylenically unsaturated monocarboxylic acids include acrylic acid, methacrylic acid, and crotonic acid. Examples of ethylenically unsaturated monocarboxylic acid derivatives include 2-ethylacrylic acid, isocrotonic acid, α-acetoxyacrylic acid, β-trans-aryloxyacrylic acid, and α-chloro-β-E-methoxyacrylic acid. Examples of ethylenically unsaturated dicarboxylic acids include maleic acid, fumaric acid, and itaconic acid. Examples of ethylenically unsaturated dicarboxylic acid derivatives include methylmaleic acid, dimethylmaleic acid, phenylmaleic acid, chloromaleic acid, dichloromaleic acid, fluoromaleic acid, and maleic acid monoesters such as nonyl maleate, decyl maleate, dodecyl maleate, octadecyl maleate, and fluoroalkyl maleates. Examples of acid anhydrides of ethylenically unsaturated dicarboxylic acids include maleic anhydride, acrylic anhydride, methyl maleic anhydride, and dimethyl maleic anhydride. Furthermore, acid anhydrides that generate carboxylic acid groups upon hydrolysis can also be used as carboxylic acid group-containing ethylenically unsaturated monomers. Among these, ethylenically unsaturated monocarboxylic acids are preferred, and methacrylic acid is more preferred. That is, the water-soluble polymer A preferably contains an ethylenically unsaturated monocarboxylic acid unit, and more preferably contains a methacrylic acid unit.
[0031] Examples of sulfonic acid group-containing ethylenically unsaturated monomers capable of forming sulfonic acid group-containing ethylenically unsaturated monomer units include vinyl sulfonic acid, methyl vinyl sulfonic acid, (meth)allyl sulfonic acid, styrene sulfonic acid, (meth)acrylic acid-2-ethyl sulfonate, 2-acrylamido-2-methylpropanesulfonic acid, 3-allyloxy-2-hydroxypropanesulfonic acid, etc. In this specification, "(meth)allyl" means allyl and / or methallyl.
[0032] Examples of the phosphate group-containing ethylenically unsaturated monomer capable of forming the phosphate group-containing ethylenically unsaturated monomer unit include 2-(meth)acryloyloxyethyl phosphate, methyl-2-(meth)acryloyloxyethyl phosphate, ethyl-(meth)acryloyloxyethyl phosphate, vinylphosphonic acid, etc. In this specification, "(meth)acryloyl" means acryloyl and / or methacryloyl.
[0033] The content of the ethylenically unsaturated acid monomer units in the water-soluble polymer A is preferably 10% by mass or more, more preferably 15% by mass or more, even more preferably 20% by mass or more, even more preferably 25% by mass or more, and preferably 80% by mass or less, more preferably 75% by mass or less, even more preferably 70% by mass or less, even more preferably 50% by mass or less, and even more preferably 35% by mass or less, when the total amount of repeating units (total monomer units) contained in the water-soluble polymer A is taken as 100% by mass. If the content of the ethylenically unsaturated acid monomer units is equal to or greater than the lower limit specified above, the dispersion stability of the slurry composition and the powder shedding resistance of the dielectric layer can be improved. On the other hand, if the content of the ethylenically unsaturated acid monomer units is equal to or less than the upper limit specified above, when the total amount of monomer units contained in the water-soluble polymer A is taken as 100% by mass, the blocking resistance of the dielectric layer can be improved. In this specification, the content ratio of various repeating units (monomer units) in the polymer is 1 It can be measured using a nuclear magnetic resonance (NMR) method such as H-NMR.
[0034] <<(Meth)acrylic acid alkyl ester monomer unit>> In the slurry composition of the present invention, the water-soluble polymer A preferably contains a (meth)acrylic acid alkyl ester monomer unit. If the water-soluble polymer A contains a (meth)acrylic acid alkyl ester monomer unit, the dispersion stability of the slurry composition can be improved. Here, the (meth)acrylic acid alkyl ester monomer unit is a monomer unit that can be formed from a (meth)acrylic acid alkyl ester monomer. In this specification, the above-mentioned ethylenically unsaturated acid monomer unit is not included in the (meth)acrylic acid alkyl ester monomer unit.
[0035] Examples of (meth)acrylic acid alkyl ester monomers that can form (meth)acrylic acid alkyl ester monomer units include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, t-butyl acrylate, isobutyl acrylate, n-pentyl acrylate, isopentyl acrylate, hexyl acrylate, heptyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, nonyl acrylate, decyl acrylate, lauryl acrylate, n-tetradecyl acrylate, and stearyl acrylate. and alkyl methacrylate esters such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, t-butyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, isopentyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, nonyl methacrylate, decyl methacrylate, lauryl methacrylate, n-tetradecyl methacrylate, and stearyl methacrylate. These may be used alone or in combination of two or more. Among these, ethyl acrylate and n-butyl acrylate are preferred. That is, it is preferable that the water-soluble polymer A contains at least one of ethyl acrylate units and n-butyl acrylate units. It is more preferable that the water-soluble polymer A contains ethyl acrylate units and n-butyl acrylate units.
[0036] The content of (meth)acrylic acid alkyl ester monomer units in the water-soluble polymer A (the total content when two or more types of (meth)acrylic acid alkyl ester monomer units are contained) is preferably 20% by mass or more, more preferably 25% by mass or more, even more preferably 30% by mass or more, even more preferably 50% by mass or more, still more preferably 65% by mass or more, and preferably 90% by mass or less, more preferably 85% by mass or less, even more preferably 80% by mass or less, and even more preferably 75% by mass or less, when all repeating units (all monomer units) contained in the water-soluble polymer A are taken as 100% by mass.
[0037] <<Other Monomer Units A>> The other monomer units A are monomer units that can be formed by other monomers A. The other monomers A are not particularly limited as long as they are monomers copolymerizable with the above-mentioned ethylenically unsaturated acid monomers and (meth)acrylic acid alkyl ester monomers. Examples of the other monomers A include hydroxyl group-containing monomers; (meth)acrylamide monomers such as (meth)acrylamide; crosslinkable monomers (crosslinkable monomers) such as polyfunctional ethylenically unsaturated carboxylic acid ester monomers having two or more ethylenically unsaturated bonds (C=C) in the molecule, such as allyl glycidyl ether, allyl (meth)acrylate, and ethoxylated pentaerythritol tetraacrylate; olefins such as ethylene and propylene; halogen atom-containing monomers such as vinyl chloride and vinylidene chloride; methyl vinyl ether, ethyl vinyl ether, and butyl vinyl ether. vinyl ethers such as methyl vinyl ether, ...
[0038] Here, examples of the hydroxyl group-containing monomer include ethylenically unsaturated alcohols such as (meth)allyl alcohol, 3-butene-1-ol, and 5-hexene-1-ol; alkanol esters of ethylenically unsaturated carboxylic acids such as 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, di-2-hydroxyethyl maleate, di-4-hydroxybutyl maleate, and di-2-hydroxypropyl itaconate; and esters of ethylenically unsaturated carboxylic acids such as 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxyethyl methacrylate, di-4-hydroxybutyl maleate, and di-2-hydroxypropyl itaconate; 2 =CR 1 -COO-(Cq H 2q O) p -H (wherein p is an integer of 2 to 9, q is an integer of 2 to 4, R 1 represents hydrogen or a methyl group) and (meth)acrylic acid esters; mono(meth)acrylic acid esters of dihydroxy esters of dicarboxylic acids such as 2-hydroxyethyl-2'-(meth)acryloyloxyphthalate and 2-hydroxyethyl-2'-(meth)acryloyloxysuccinate; vinyl ethers such as 2-hydroxyethyl vinyl ether and 2-hydroxypropyl vinyl ether; mono(meth)allyl alkylene glycols such as (meth)allyl-2-hydroxyethyl ether, (meth)allyl-2-hydroxypropyl ether, (meth)allyl-3-hydroxypropyl ether, (meth)allyl-2-hydroxybutyl ether, (meth)allyl-3-hydroxybutyl ether, (meth)allyl-4-hydroxybutyl ether, and (meth)allyl-6-hydroxyhexyl ether. ethers; polyoxyalkylene glycol mono(meth)allyl ethers such as diethylene glycol mono(meth)allyl ether and dipropylene glycol mono(meth)allyl ether; mono(meth)allyl ethers of halogen- and hydroxy-substituted (poly)alkylene glycols such as glycerin mono(meth)allyl ether, (meth)allyl-2-chloro-3-hydroxypropyl ether and (meth)allyl-2-hydroxy-3-chloropropyl ether; mono(meth)allyl ethers of polyhydric phenols such as eugenol and isoeugenol and halogen-substituted products thereof; (meth)allyl thioethers of alkylene glycols such as (meth)allyl-2-hydroxyethyl thioether and (meth)allyl-2-hydroxypropyl thioether; 2-hydroxyethyl(meth)acrylamide, N-methylolacrylamide; etc. These may be used alone or in combination of two or more.
[0039] The content of the other monomer units A in the water-soluble polymer A is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 1% by mass or less, and even more preferably 0% by mass, i.e., the water-soluble polymer A does not contain any other monomer units A, when all repeating units (total monomer units) contained in the water-soluble polymer A are taken as 100% by mass.
[0040] <<Characteristics of Water-Soluble Polymer A>> The weight-average molecular weight of the water-soluble polymer A must be 100,000 or more, preferably 500,000 or more, and must be 2,000,000 or less, preferably 1,200,000 or less. If the weight-average molecular weight of the water-soluble polymer A is not less than the above-mentioned lower limit, the redispersibility of the slurry composition and the blocking resistance of the dielectric layer can be improved. On the other hand, if the weight-average molecular weight of the water-soluble polymer A is not more than the above-mentioned upper limit, the powder shedding resistance of the dielectric layer can be improved.
[0041] The water-soluble polymer A is not particularly limited, but the haze of the evaluation liquid calculated by the following procedure (hereinafter sometimes simply referred to as "haze") is preferably 60% or more, more preferably 65% or more. If the haze of the water-soluble polymer A is equal to or greater than the above lower limit, the dispersion stability and redispersibility of the slurry composition can be improved. The haze calculation procedure involves first adjusting the concentration and pH of an aqueous solution of the water-soluble polymer A to prepare an aqueous solution with a concentration of 10% and a pH of 6.5, and stirring the aqueous solution at 25°C for 1 hour to obtain an evaluation liquid. This evaluation liquid is transferred to a cell with an optical path length of 30 mm, and scattered light and total light transmitted light are measured using a haze meter, and the haze of the evaluation liquid is calculated according to the following formula (1): Haze (%) = Scattered light / Total light transmitted × 100 (1) The haze of the water-soluble polymer A can be adjusted appropriately depending on the type and ratio of monomers that can form the water-soluble polymer A.
[0042] The water-soluble polymer A preferably has a glass transition temperature of 0°C or higher, more preferably 5°C or higher, and preferably 100°C or lower, more preferably 80°C or lower. If the glass transition temperature of the water-soluble polymer A is above the lower limit, the blocking resistance of the dielectric layer can be improved. On the other hand, if the glass transition temperature of the water-soluble polymer A is below the upper limit, the dispersion stability of the slurry composition can be improved. In this specification, the glass transition temperature of the polymer can be measured according to the method described in the examples.
[0043] <<Content of Water-Soluble Polymer A>> The content of water-soluble polymer A is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, and preferably 20 parts by mass or less, and more preferably 15 parts by mass or less, relative to 100 parts by mass of the dielectric material. If the content of water-soluble polymer A is equal to or greater than the above-mentioned lower limit relative to 100 parts by mass of the dielectric material, the powder shedding resistance of the dielectric layer can be improved. On the other hand, if the content of water-soluble polymer A is equal to or less than the above-mentioned upper limit relative to 100 parts by mass of the dielectric material, the dispersion stability of the slurry composition and the blocking resistance of the dielectric layer can be improved.
[0044] <<Content of Water-Soluble Polymer A in the Entire Slurry Composition>> The content of water-soluble polymer A in the entire slurry composition (including the solvent) is preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 2% by mass or more, and is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less. If the content of water-soluble polymer A in the entire slurry composition is equal to or greater than the above-mentioned lower limit, the powder shedding resistance of the dielectric layer can be improved. On the other hand, if the content of water-soluble polymer A in the entire slurry composition is equal to or less than the above-mentioned upper limit, the dispersion stability of the slurry composition and the blocking resistance of the dielectric layer can be improved.
[0045] <<Method for Preparing Water-Soluble Polymer A>> The water-soluble polymer A can be obtained, for example, by polymerizing a monomer composition obtained by mixing the above-mentioned monomers with an arbitrary polymerization solvent using an arbitrary polymerization method. The polymerization method for the water-soluble polymer A is not limited, and any method, such as a solution polymerization method such as an aqueous solution polymerization method, a slurry polymerization method, a suspension polymerization method, a bulk polymerization method, or an emulsion polymerization method, can be used. Furthermore, addition polymerization such as ionic polymerization, radical polymerization, or living radical polymerization can be used as the polymerization reaction. Commonly used additives, such as a polymerization initiator, polymerization accelerator, emulsifier, dispersant, or chain transfer agent, can be used, and the amounts used can be the same as commonly used amounts. Among these, an aqueous solution polymerization method using water as the polymerization solvent is preferred because it does not require a solvent removal operation and the solvent is highly safe.
[0046] When water is used as a polymerization solvent and the above-mentioned monomer composition is polymerized in water to prepare an aqueous solution containing the water-soluble polymer A, it is preferable to adjust the pH of the aqueous solution after polymerization to 7 or more and 9 or less. This is because, if the obtained aqueous solution is neutralized to adjust the pH to within the above range, the viscosity stability of the slurry composition can be easily improved.
[0047] Here, the polymerization initiator that can be used in preparing the water-soluble polymer A is not particularly limited, and examples thereof include known polymerization initiators such as sodium persulfate, ammonium persulfate, and potassium persulfate. Among these, potassium persulfate is preferably used. The polymerization initiator may be used alone or in combination of two or more types in any ratio.
[0048] The polymerization accelerator is not particularly limited, and a known reducing polymerization accelerator, such as tetramethylethylenediamine, can be used. The polymerization accelerator may be used alone or in combination of two or more in any ratio.
[0049] <Water-Soluble Polymer B> In the slurry composition of the present invention, the water-soluble polymer B is a component that can function as a dispersant, and has a weight-average molecular weight of 5,000 or more and 80,000 or less.
[0050] Here, examples of the monomer units contained in the water-soluble polymer B include the same monomer units as those described in detail in the section "Water-soluble polymer A". Among these, the water-soluble polymer B preferably contains at least one of an ethylenically unsaturated acid monomer unit and an alkoxy polyalkylene glycol allyl ether unit, and more preferably contains both an ethylenically unsaturated acid monomer unit and an alkoxy polyalkylene glycol allyl ether unit, since this can improve the dispersibility of the slurry composition. The water-soluble polymer B is not particularly limited as long as it is a polymer having a weight-average molecular weight of 5,000 or more and 80,000 or less. For example, a polymer containing the same type of monomer unit as the water-soluble polymer A and having the same content ratio of each monomer unit can be used.
[0051] The ethylenically unsaturated acid monomer unit that the water-soluble polymer B can contain is preferably a carboxylic acid group-containing ethylenically unsaturated monomer unit, more preferably an acid anhydride unit of an ethylenically unsaturated dicarboxylic acid, and even more preferably a maleic anhydride unit.
[0052] A methoxypolyethylene glycol allyl ether unit is preferred as the alkoxy polyalkylene glycol allyl ether unit that can be contained in the water-soluble polymer B. The alkoxy polyalkylene glycol allyl ether that can form the alkoxy polyalkylene glycol allyl ether unit is usually one to which 5 to 20 moles of alkylene oxide have been added.
[0053] <<Characteristics of Water-Soluble Polymer B>> The weight-average molecular weight of the water-soluble polymer B must be 5,000 or more, preferably 10,000 or more, and must be 80,000 or less, preferably 50,000 or less, and more preferably 30,000 or less. If the weight-average molecular weight of the water-soluble polymer B is equal to or greater than the lower limit, the dispersion stability of the slurry composition can be improved. On the other hand, if the weight-average molecular weight of the water-soluble polymer B is equal to or less than the upper limit, the powder shedding resistance of the dielectric layer can be improved. In addition, the water-soluble polymer B imparts appropriate flexibility to the dielectric layer, which, as a result, makes it easier to cut the dielectric layer and the laminate including the dielectric layer when producing a capacitor.
[0054] <<Content of Water-Soluble Polymer B>> The content of water-soluble polymer B is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and even more preferably 3 parts by mass or less, based on 100 parts by mass of the dielectric material. If the content of water-soluble polymer B is equal to or greater than the lower limit above, based on 100 parts by mass of the dielectric material, the dispersion stability of the slurry composition can be improved. On the other hand, if the content of water-soluble polymer B is equal to or less than the upper limit above, based on 100 parts by mass of the dielectric material, the powder shedding resistance of the dielectric layer can be improved. In addition, the water-soluble polymer B imparts appropriate flexibility to the dielectric layer, which, as a result, facilitates cutting of the dielectric layer and a laminate including the dielectric layer when producing a capacitor.
[0055] <<Ratio of Water-Soluble Polymer B in the Entire Slurry Composition>> The ratio of water-soluble polymer B in the entire slurry composition (including the solvent) is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, even more preferably 0.3% by mass or more, and preferably 3% by mass or less, more preferably 1.5% by mass or less, and even more preferably 0.8% by mass or less. If the ratio of water-soluble polymer B in the entire slurry composition is equal to or greater than the above lower limit, the dispersion stability of the slurry composition can be improved. On the other hand, if the ratio of water-soluble polymer B in the entire slurry composition is equal to or less than the above upper limit, the powder shedding resistance of the dielectric layer can be improved. In addition, the dielectric layer is provided with appropriate flexibility, which results in easy cutting of the dielectric layer and a laminate including the dielectric layer when producing a capacitor.
[0056] <<Mass Ratio of Water-Soluble Polymer B to Water-Soluble Polymer A>> The mass ratio of water-soluble polymer B to water-soluble polymer A (water-soluble polymer B / water-soluble polymer A) is preferably 0.01 or more, more preferably 0.05 or more, even more preferably 0.1 or more, and preferably 1 or less, more preferably 0.5 or less, and even more preferably 0.3 or less. When the mass ratio of water-soluble polymer B to water-soluble polymer A is equal to or greater than the above lower limit, the dispersion stability of the slurry composition can be improved. On the other hand, when the mass ratio of water-soluble polymer B to water-soluble polymer A is equal to or less than the above upper limit, the powder shedding resistance of the dielectric layer can be improved. In addition, the dielectric layer is provided with appropriate flexibility, which results in easy cutting of the dielectric layer and a laminate including the dielectric layer when producing a capacitor.
[0057] <<Method for Preparing Water-Soluble Polymer B>> The method for preparing the water-soluble polymer B is not particularly limited, and the water-soluble polymer B can be prepared, for example, by the same method as that for the water-soluble polymer A. Note that, for example, by appropriately adjusting the type and amount of a chain transfer agent such as t-dodecyl mercaptan, the weight-average molecular weight of the water-soluble polymer B can be efficiently adjusted to fall within a predetermined range.
[0058] <Solvent> In the slurry composition of the present invention, the solvent contains water. From the viewpoint of reducing the environmental load, the content of water contained in the solvent is preferably 50 parts by mass or more, more preferably 80 parts by mass or more, and even more preferably 90 parts by mass or more, based on 100 parts by mass of all solvent components. From the viewpoint of safety and easy availability, the content of water contained in the solvent is particularly preferably 100 parts by mass, based on 100 parts by mass of all solvent components, i.e., the solvent is all water.
[0059] <Particulate Polymer> The slurry composition of the present invention preferably further contains a particulate polymer, as this can improve the redispersibility of the slurry composition and the powder-fall resistance of the dielectric layer.
[0060] The particulate polymer is a component that can function as a binder, imparting adhesiveness to the dielectric layer formed using the slurry composition and retaining materials contained in the dielectric layer (e.g., dielectric materials) from being detached from the dielectric layer. Here, the particulate polymer has a particulate shape in the slurry composition containing water as a solvent. The particulate polymer may be present in the dielectric layer while maintaining its particulate shape, or may be present in any non-particulate shape. The particulate polymer is preferably a water-insoluble polymer, as this can improve the dispersion stability of the slurry composition.
[0061] The particulate polymer is not particularly limited, and any polymer such as a conjugated diene polymer or an acrylic polymer can be used.
[0062] <<Conjugated Diene Polymer>> A conjugated diene polymer is a polymer containing a conjugated diene monomer unit. The conjugated diene polymer may optionally contain an aromatic vinyl monomer unit, an ethylenically unsaturated acid monomer unit, or a cyano group-containing monomer unit. Furthermore, the conjugated diene polymer may contain a monomer unit other than the conjugated diene monomer unit, the aromatic vinyl monomer unit, the ethylenically unsaturated acid monomer unit, and the cyano group-containing monomer unit (hereinafter, sometimes referred to as "other monomer unit B").
[0063] Examples of the conjugated diene polymer include copolymers containing aromatic vinyl monomer units and conjugated diene monomer units, such as styrene-butadiene copolymer (SBR), butadiene rubber (BR), isoprene rubber, acrylic rubber (NBR) (copolymers containing cyano group-containing monomer units and conjugated diene monomer units), and hydrogenated products thereof.
[0064] [Conjugated Diene Monomer Unit] The conjugated diene monomer unit is a monomer unit that can be formed by a conjugated diene monomer. Examples of conjugated diene monomers include 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, substituted linear conjugated pentadienes, and substituted and side-chain conjugated hexadienes. These may be used alone or in combination of two or more. Among these, 1,3-butadiene and 2-methyl-1,3-butadiene (isoprene) are preferred as the conjugated diene monomer, with 1,3-butadiene being more preferred.
[0065] The content of conjugated diene monomer units in the conjugated diene polymer is preferably 20% by mass or more, more preferably 25% by mass or more, and is preferably 60% by mass or less, more preferably 55% by mass or less, when all repeating units (all monomer units) contained in the conjugated diene polymer are taken as 100% by mass.
[0066] [Aromatic vinyl monomer unit] The aromatic vinyl monomer unit is a monomer unit that can be formed by an aromatic vinyl monomer. Examples of aromatic vinyl monomers include styrene, α-methylstyrene, vinyltoluene, and divinylbenzene. These may be used alone or in combination of two or more. Among these, styrene is preferred as the aromatic vinyl monomer.
[0067] The content of aromatic vinyl monomer units in the conjugated diene polymer is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 45% by mass or more, and is preferably 70% by mass or less, and more preferably 65% by mass or less, when all repeating units (all monomer units) contained in the conjugated diene polymer are taken as 100% by mass.
[0068] [Ethylenically unsaturated acid monomer unit] The ethylenically unsaturated acid monomer unit is a monomer unit that can be formed by an ethylenically unsaturated acid monomer. Examples of the ethylenically unsaturated acid monomer that can be used in the preparation of the conjugated diene polymer include the same monomers as those described in the above section "Ethylenically unsaturated acid monomer unit." These may be used alone or in combination of two or more. Among these, acrylic acid, methacrylic acid, itaconic acid, and vinyl sulfonic acid are more preferred as the ethylenically unsaturated acid monomer unit.
[0069] The content of the ethylenically unsaturated acid monomer units in the conjugated diene polymer is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, and is preferably 10% by mass or less, more preferably 5% by mass or less, when all repeating units (all monomer units) contained in the conjugated diene polymer are taken as 100% by mass.
[0070] [Cyano Group-Containing Monomer Unit] The cyano group-containing monomer unit is a monomer unit that can be formed by a cyano group-containing monomer. Examples of the cyano group-containing monomer include acrylonitrile and methacrylonitrile. These may be used alone or in combination of two or more in any ratio. Among these, acrylonitrile is preferred as the cyano group-containing monomer.
[0071] The cyano group-containing monomer units in the conjugated diene polymer preferably account for 5% by mass or more, more preferably 10% by mass or more, and preferably 25% by mass or less, more preferably 20% by mass or less, when all repeating units (all monomer units) contained in the conjugated diene polymer are taken as 100% by mass.
[0072] [Other Monomer Units B] The other monomer units B are monomer units that can be formed by other monomers B. The other monomers B are not particularly limited as long as they are copolymerizable with the monomers that can form the conjugated diene polymers described above. Examples of the other monomers B include amide group-containing monomers such as acrylamide and methacrylamide; crosslinkable monomers (crosslinkable monomers) such as allyl glycidyl ether and allyl (meth)acrylate; olefins such as ethylene and propylene; halogen atom-containing monomers such as vinyl chloride and vinylidene chloride; vinyl esters such as vinyl acetate, vinyl propionate, and vinyl butyrate; vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, and butyl vinyl ether; vinyl ketones such as methyl vinyl ketone, ethyl vinyl ketone, butyl vinyl ketone, hexyl vinyl ketone, and isopropenyl vinyl ketone; and N-vinylpyrrolidone. heterocycle-containing vinyl compounds such as vinylpyridine and vinylimidazole; amino group-containing monomers such as aminoethyl vinyl ether and dimethylaminoethyl vinyl ether; (meth)acrylic acid alkyl ester monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, and octyl (meth)acrylate such as 2-ethylhexyl (meth)acrylate; and the like. These other monomers B may be used singly or in combination of two or more.
[0073] The content of the other monomer units B in the conjugated diene polymer is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 1% by mass or less, and even more preferably 0% by mass, i.e., the conjugated diene polymer does not contain any other monomer units B, when all repeating units (total monomer units) contained in the conjugated diene polymer are taken as 100% by mass.
[0074] When a (meth)acrylic acid alkyl ester monomer is used to prepare the conjugated diene polymer, the content of the (meth)acrylic acid alkyl ester monomer unit is less than 50 mass % when the total amount of all repeating units (total monomer units) contained in the conjugated diene polymer is 100 mass %.
[0075] <<Acrylic Polymer>> The acrylic polymer is a polymer containing (meth)acrylic acid alkyl ester monomer units. The acrylic polymer may optionally contain aromatic vinyl monomer units, ethylenically unsaturated acid monomer units, and cyano group-containing monomer units. The acrylic polymer may also contain monomer units other than (meth)acrylic acid alkyl ester monomer units, aromatic vinyl monomer units, ethylenically unsaturated acid monomer units, and cyano group-containing monomer units (hereinafter, sometimes referred to as "other monomer units C"). Note that the acrylic polymer is typically a polymer containing 50% by mass or more of (meth)acrylic acid alkyl ester monomer units, with the total repeating units (total monomer units) contained in the acrylic polymer being 100% by mass, and is different from the above-mentioned conjugated diene polymers.
[0076] [(Meth)acrylic acid alkyl ester monomer unit] The (meth)acrylic acid alkyl ester monomer unit is a monomer unit that can be formed by a (meth)acrylic acid alkyl ester monomer. Examples of the (meth)acrylic acid alkyl ester monomer that can be used in the preparation of the acrylic polymer include the same monomers as those explained in the above section "(meth)acrylic acid alkyl ester monomer unit." These may be used alone or in combination of two or more.
[0077] The content of the (meth)acrylic acid alkyl ester monomer units in the acrylic polymer is 50% by mass or more, preferably 55% by mass or more, and is preferably 98% by mass or less, and more preferably 95% by mass or less, when all repeating units (all monomer units) contained in the acrylic polymer are taken as 100% by mass.
[0078] [Aromatic vinyl monomer unit] The aromatic vinyl monomer unit is a monomer unit that can be formed by an aromatic vinyl monomer. Examples of aromatic vinyl monomers that can be used to prepare the acrylic polymer include the same monomers as those described in the above section "Aromatic vinyl monomer unit". These may be used alone or in combination of two or more.
[0079] The content of aromatic vinyl monomer units in the acrylic polymer is preferably 10% by mass or more, and more preferably 20% by mass or more, and is preferably 50% by mass or less, and more preferably 40% by mass or less, when all repeating units (all monomer units) contained in the acrylic polymer are taken as 100% by mass.
[0080] [Ethylenically unsaturated acid monomer unit] The ethylenically unsaturated acid monomer unit is a monomer unit that can be formed by an ethylenically unsaturated acid monomer. Examples of the ethylenically unsaturated acid monomer unit that can be used to prepare the acrylic polymer include the same monomers as those described in the above section "Ethylenically unsaturated acid monomer unit". These may be used alone or in combination of two or more. Among these, acrylic acid, methacrylic acid, itaconic acid, and vinyl sulfonic acid are preferred as the ethylenically unsaturated acid monomer unit.
[0081] The content of the ethylenically unsaturated acid monomer units in the acrylic polymer is preferably 0.1% by mass or more, and more preferably 0.2% by mass or more, and is preferably 10% by mass or less, and more preferably 5% by mass or less, when all repeating units (all monomer units) contained in the acrylic polymer are taken as 100% by mass.
[0082] [Cyano Group-Containing Monomer Unit] The cyano group-containing monomer unit is a monomer unit that can be formed by a cyano group-containing monomer. Examples of cyano group-containing monomers that can be used to prepare the acrylic polymer include the same monomers as those described in the above section "Cyano Group-Containing Monomer Unit." These may be used alone or in combination of two or more types in any ratio.
[0083] The content of the cyano group-containing monomer units in the acrylic polymer is preferably 1% by mass or more, more preferably 3% by mass or more, and is preferably 10% by mass or less, and more preferably 8% by mass or less, when all repeating units (all monomer units) contained in the acrylic polymer are taken as 100% by mass.
[0084] [Other Monomer Units C] The other monomer units C are monomer units that can be formed by other monomers C. The other monomers C are not particularly limited as long as they are monomers that can be copolymerized with the above-mentioned monomers that can form the acrylic polymer. Examples of other monomers C include amide group-containing monomers such as acrylamide and methacrylamide; crosslinkable monomers (crosslinkable monomers) such as allyl glycidyl ether and allyl (meth)acrylate; olefins such as ethylene and propylene; halogen atom-containing monomers such as vinyl chloride and vinylidene chloride; vinyl esters such as vinyl acetate, vinyl propionate, and vinyl butyrate; vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, and butyl vinyl ether; vinyl ketones such as methyl vinyl ketone, ethyl vinyl ketone, butyl vinyl ketone, hexyl vinyl ketone, and isopropenyl vinyl ketone; heterocycle-containing vinyl compounds such as N-vinylpyrrolidone, vinylpyridine, and vinylimidazole; and amino group-containing monomers such as aminoethyl vinyl ether and dimethylaminoethyl vinyl ether. These may be used alone or in combination of two or more.
[0085] The content of the other monomer units C in the acrylic polymer is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 1% by mass or less, and even more preferably 0% by mass, i.e., the acrylic polymer does not contain any other monomer units C, when all repeating units (total monomer units) contained in the acrylic polymer are taken as 100% by mass.
[0086] <<Average Particle Diameter of Particulate Polymer>> The average particle diameter of the particulate polymer is preferably 0.01 μm or more, more preferably 0.02 μm or more, and preferably 1.0 μm or less, more preferably 0.8 μm or less, and even more preferably 0.5 μm or less. If the average particle diameter of the particulate polymer is equal to or greater than the above lower limit, the dispersion stability of the slurry composition can be improved. On the other hand, if the average particle diameter of the particulate polymer is equal to or less than the above upper limit, the blocking resistance of the dielectric layer can be improved. In this specification, the average particle diameter of the particulate polymer can be measured according to the method described in the examples.
[0087] <<Content of Particulate Polymer>> The content of the particulate polymer is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, and is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, relative to 100 parts by mass of the dielectric material.
[0088] <<Method for Preparing Particulate Polymer>> The polymerization method for the particulate polymer is not particularly limited, and any method such as solution polymerization, suspension polymerization, bulk polymerization, or emulsion polymerization may be used. Furthermore, addition polymerization such as ionic polymerization, radical polymerization, or living radical polymerization may be used as the polymerization reaction. Furthermore, polymerization solvents and additives such as emulsifiers, dispersants, polymerization initiators, and chain transfer agents that can be used in the polymerization may be commonly used ones, and the amounts used may also be commonly used amounts.
[0089] <Water-Soluble Plasticizer> The slurry composition of the present invention can improve the powder shedding resistance of the dielectric layer and impart appropriate flexibility to the dielectric layer, thereby facilitating cutting of the dielectric layer and the laminate including the dielectric layer when fabricating a capacitor. Therefore, it is preferable that the slurry composition further contains a water-soluble plasticizer. The molecular weight of the water-soluble plasticizer is usually 10 or more and 1,000 or less.
[0090] Examples of water-soluble plasticizers include polyhydric alcohols such as ethylene glycol, glycerin, trimethylolpropane, diethylene glycol, triethylene glycol, dipropylene glycol, pentaerythritol, sorbit, sorbitan, sucrose, etc. Among these, ethylene glycol and glycerin are preferred because they can improve the powder-fall resistance of the dielectric layer.
[0091] The content of the water-soluble plasticizer is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and preferably 5 parts by mass or less, and more preferably 3 parts by mass or less, per 100 parts by mass of the dielectric material. When the content of the water-soluble plasticizer is equal to or greater than the lower limit, per 100 parts by mass of the dielectric material, the powder shedding resistance of the dielectric layer can be improved. Furthermore, the dielectric layer is provided with appropriate flexibility, which makes it easier to cut the dielectric layer and the laminate including the dielectric layer when fabricating a capacitor. On the other hand, when the content of the water-soluble plasticizer is equal to or less than the upper limit, per 100 parts by mass of the dielectric material, the blocking resistance of the dielectric layer can be improved.
[0092] <Other Components> The slurry composition of the present invention may contain other components, such as the water-soluble polymer A, the water-soluble polymer B, and the additives used when polymerizing the particulate polymer.
[0093] <pH of Slurry Composition for Dielectric Layer> The pH of the slurry composition is preferably 8 or more, more preferably 8.5 or more, and is preferably 12 or less, more preferably 11.5 or less. If the pH is within the above range, the dispersion stability and redispersibility of the slurry composition can be improved.
[0094] <Solid content concentration of slurry composition for dielectric layer> The solid content concentration of the slurry composition is preferably 20% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more, and is preferably 90% by mass or less, and more preferably 80% by mass or less.
[0095] <Method for preparing slurry composition for dielectric layer> The above-mentioned slurry composition can be prepared by mixing the above-mentioned dielectric material, water-soluble polymer A, water-soluble polymer B, and solvent, as well as any particulate polymer, water-soluble plasticizer, and other components by a known method. Specifically, the slurry composition can be prepared by mixing the above-mentioned components using a mixer such as a ball mill, sand mill, bead mill, pigment disperser, crusher, ultrasonic disperser, homogenizer, planetary mixer, Filmix, or planetary-revolution mixer.
[0096] (Dielectric Layer) The dielectric layer of the present invention is formed by drying a coating film made from the above-described slurry composition of the present invention. The dielectric layer of the present invention is typically a dried film obtained by partially or completely removing the solvent from a coating film made from the slurry composition of the present invention. That is, the dielectric layer of the present invention comprises the above-described dielectric material, water-soluble polymer A, and water-soluble polymer B, and may optionally contain a solvent, a particulate polymer, a water-soluble plasticizer, and other components. Here, the dielectric layer of the present invention is formed by drying a coating film made from the slurry composition of the present invention, which has excellent dispersion stability and redispersibility, and therefore has excellent film thickness uniformity. Furthermore, the dielectric layer of the present invention is formed by drying a coating film made from the slurry composition of the present invention, and therefore has excellent powder shedding resistance. Furthermore, the dielectric layer of the present invention is formed by drying a coating film made from the slurry composition of the present invention, and therefore has excellent blocking resistance. Furthermore, because the dielectric layer of the present invention has excellent blocking resistance, it is easy to handle, resulting in efficient capacitor production.
[0097] The content of the dielectric material in the dielectric layer is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more, and is preferably 98% by mass or less, more preferably 95% by mass or less, and even more preferably 90% by mass or less, when all components in the dielectric layer are taken as 100% by mass.
[0098] The content of the water-soluble polymer A in the dielectric layer is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, and is preferably 20 parts by mass or less, and more preferably 15 parts by mass or less, based on 100 parts by mass of the dielectric material in the dielectric layer.
[0099] The content of the water-soluble polymer B in the dielectric layer is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and even more preferably 3 parts by mass or less, based on 100 parts by mass of the dielectric material in the dielectric layer.
[0100] The content of the particulate polymer in the dielectric layer is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, and is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, based on 100 parts by mass of the dielectric material in the dielectric layer.
[0101] The content of the water-soluble plasticizer in the dielectric layer is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, based on 100 parts by mass of the dielectric material in the dielectric layer.
[0102] The thickness of the dielectric layer is preferably 0.1 μm or more, more preferably 0.5 μm or more, and is preferably 10 μm or less, more preferably 5 μm or less.
[0103] The dielectric layer of the present invention may have a conductor layer formed on the dielectric layer. The conductor layer can be formed by various printing methods such as screen printing, gravure printing, stamp printing, inkjet printing, and offset printing using a pattern formed by these methods; vacuum deposition for forming a metal vapor deposition film; or the like. When the conductor layer is formed by a printing method, a conductive paste can be used. The conductive paste can be prepared by a conventionally known method, for example, by mixing a conductive powder such as a metal, a dispersant, a plasticizer, a solvent, etc. with a polyvinyl acetal resin.
[0104] <Method of Producing Dielectric Layer> The dielectric layer can be produced by applying the slurry composition of the present invention onto a release substrate and drying the formed coating film.
[0105] Here, the release substrate used when preparing the dielectric layer is preferably made of a flexible resin. Since the release substrate is made of a flexible resin, the release substrate (laminated film) on which the dielectric layer is formed by applying a slurry composition to the release substrate and drying it can be stored in a rolled state and supplied as needed. The release substrate is not particularly limited, and examples thereof include substrates containing resins such as polyesters such as polyethylene terephthalate and polyethylene naphthalate, polyethylene, polypropylene, polystyrene, polyimide, polyvinyl alcohol, and polyvinyl chloride.
[0106] The release substrate is preferably subjected to a surface treatment to improve releasability on the side on which the dielectric layer of the present invention is formed. The surface treatment is not particularly limited, and examples thereof include surface treatments using a release agent such as a silicone-based release agent, a fluorine-based release agent, or a wax-based release agent.
[0107] The thickness of the release substrate is not particularly limited, but is usually 20 μm or more and 100 μm or less.
[0108] The method for applying the slurry composition to the release substrate is not particularly limited, and examples thereof include known application methods using an applicator or various roll coaters such as a gravure coater and a comma coater (registered trademark).
[0109] The method for drying the coating film formed on the release substrate is not particularly limited, and for example, a known drying method using a hot air dryer can be mentioned. The drying conditions can be appropriately set depending on the content of the solvent in the coating film, the thickness of the coating film, etc., but the drying temperature is usually 80°C or higher and 150°C or lower, and the drying time is usually 3 minutes or higher and 60 minutes or lower.
[0110] When the dielectric layer of the present invention is used to manufacture a capacitor, a plurality of dielectric layers may be superimposed on one another and then thermocompression bonded. However, the dielectric layers may be peeled off from the release substrate either before or after the superimposition and thermocompression bonding of the dielectric layers.
[0111] (Capacitor) The capacitor of the present invention is formed using the dielectric layer of the present invention described above. The capacitor of the present invention is formed using the dielectric layer of the present invention, which has excellent film thickness uniformity, and therefore performance variation is suppressed. Furthermore, the capacitor of the present invention is formed using a dielectric layer that has excellent resistance to powder shedding, and therefore has excellent performance. Furthermore, the capacitor of the present invention is formed using a dielectric layer that is easy to handle, and therefore has excellent productivity.
[0112] Here, the capacitor of the present invention includes a capacitor obtained by sintering a laminate of overlapping dielectric layers (sintered product), and a capacitor obtained without sintering a laminate of overlapping dielectric layers (unsintered product). Examples of capacitors obtained by sintering the above-mentioned laminate include multilayer ceramic capacitors. Examples of capacitors obtained without sintering the above-mentioned laminate include laminated metallized film capacitors. Note that, below, a case where the capacitor is a multilayer ceramic capacitor will be described as an example, but the present invention is not limited to the following example.
[0113] The multilayer ceramic capacitor as the capacitor of the present invention usually comprises a layered dielectric, layered internal electrodes, and external electrodes, and the dielectric is formed by sintering the stacked dielectric layers of the present invention. Hereinafter, an example of a multilayer ceramic capacitor as the capacitor of the present invention will be described with reference to FIG.
[0114] FIG. 1 is a schematic cross-sectional view showing an example of a multilayer ceramic capacitor as a capacitor of the present invention. The multilayer ceramic capacitor 10 shown in FIG. 1 includes layered dielectrics 11 and layered internal electrodes 12 that are alternately stacked, and a pair of external electrodes 13 on the outside of the dielectrics 11 and the internal electrodes 12. One of the pair of internal electrodes 12 adjacent to each other along the stacking direction, sandwiching the dielectric 11 therebetween, is electrically connected to one of the pair of external electrodes 13 inside the multilayer ceramic capacitor 10, and the other of the pair of internal electrodes 12 adjacent to each other along the stacking direction, sandwiching the dielectric 11 therebetween, is electrically connected to the other of the pair of external electrodes 13 inside the multilayer ceramic capacitor 10. This results in a structure in which multiple capacitor elements are electrically connected in parallel between the pair of external electrodes 13. Note that the interface between the dielectric layers of the present invention that may be formed when the dielectric layers are stacked is not shown in FIG. 1 because the dielectric layers will disappear when they are integrated together by sintering.
[0115] The multilayer ceramic capacitor is not particularly limited and can be produced by a conventionally known method. For example, the multilayer ceramic capacitor can be produced by stacking a plurality of dielectric layers of the present invention, each having a conductive layer that can serve as an internal electrode, so that the dielectric layers and the conductive layers alternate, heat-pressing the stack to form a laminate, thermally decomposing and removing binder components and the like contained in the laminate (degreasing treatment), sintering the stack, and then forming external electrodes on the end faces of the sintered ceramic product obtained by sintering.
[0116] The degreasing treatment is usually carried out in a nitrogen atmosphere at a temperature of 300° C. to 500° C. The degreasing treatment time is usually 1 hour to 5 hours. The content of the binder component in the laminate after the degreasing treatment is usually 50 ppm or less.
[0117] The degreased laminate is usually sintered under an oxygen partial pressure of 10 -9 ~10 -12 MPa H 2 -N 2 -H 2 The sintering is carried out in a reducing atmosphere such as O gas at a temperature of 1000° C. to 1500° C. The sintering time for the laminate is usually 1 hour to 30 hours.
[0118] The external electrodes can be formed by applying an external electrode material to the end faces of the sintered ceramic product obtained by sintering and then baking the applied material. This allows, for example, a multilayer ceramic capacitor as shown in FIG. 1 to be obtained. Examples of the external electrode material include a Cu paste containing glass frit. Baking is usually performed in a nitrogen atmosphere at a temperature of 500°C or higher and 1500°C or lower. The surfaces of the external electrodes can also be plated with Ni, Sn, or the like.
[0119] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples. In the following description, "%" and "parts" representing amounts are based on mass unless otherwise specified. In addition, in a polymer produced by polymerizing multiple types of monomers, the proportion of a monomer unit formed by polymerizing a certain monomer in the polymer usually coincides with the ratio (feed ratio) of that monomer to all monomers used in the polymerization of the polymer, unless otherwise specified. In addition, the weight-average molecular weights of water-soluble polymer A and water-soluble polymer B, the glass transition temperature of water-soluble polymer A, the average particle size of the particulate polymer, the pH of the slurry composition, dispersion stability, redispersibility, blocking resistance, and powder shedding resistance were measured and evaluated according to the following procedures.
[0120] <Weight-average molecular weight of water-soluble polymer A and water-soluble polymer B> The weight-average molecular weight of water-soluble polymer A and water-soluble polymer B was measured by gel permeation chromatography (GPC). Specifically, the water-soluble polymer was first added to about 5 mL of eluent so that the solid concentration was about 0.5 g / L, and slowly dissolved at room temperature. After visually confirming the dissolution of the water-soluble polymer, the solution was gently filtered through a 0.45 μm filter to prepare a measurement sample, which was then used for measurement. Then, a calibration curve was prepared using a standard substance, and the weight-average molecular weight was calculated as a value converted from the standard substance. The measurement conditions were as follows. <<Measurement conditions>> Column: Showa Denko K.K., product name Shodex OHpak (SB-G, SB-807HQ, SB-806MHQ) Eluent: 0.1 M Tris buffer solution (0.1 M potassium chloride added) Flow rate: 0.5 mL / min Sample concentration: 0.05 g / L (solids concentration) Injection volume: 200 μL Column temperature: 40°C Detector: Differential refractive index detector RI (Tosoh Corporation, product name "RI-8020") Standard substance: Monodispersed pullulan (Showa Denko K.K.)
[0121] <Glass Transition Temperature of Water-Soluble Polymer A> An aqueous solution of water-soluble polymer A was dried for 3 days in an environment of 50% humidity and 25°C to obtain a film having a thickness of 1.0 mm. This film was dried at 60°C for 10 hours using a vacuum dryer. Thereafter, the glass transition temperature (°C) of the dried film was measured as a sample in accordance with JIS K7121 using a differential scanning calorimeter (DSC6220SII, manufactured by Nano Technology Corporation) under conditions of a measurement temperature of -100°C to 180°C and a heating rate of 5°C / min.
[0122] <Average Particle Diameter of Particulate Polymer> The average particle diameter of the particulate polymer was measured by a laser diffraction method as follows. First, a measurement sample was prepared by adjusting the solid content concentration of the polymer (particulate) dispersion prepared in the examples to 0.1% by mass. Then, in the particle size distribution (volume basis) measured using a laser diffraction particle size distribution analyzer (manufactured by Beckman Coulter, Inc., product name "LS-230"), the particle diameter D50 at which the cumulative volume calculated from the smallest diameter side reached 50% was taken as the average particle diameter.
[0123] <pH of Slurry Composition> A benchtop pH meter (F-51, manufactured by HORIBA) was calibrated with pH standard solutions (pH 4, pH 7, and pH 9), and then the pH of the slurry composition was measured using this. Note that in Comparative Example 2, the solvent for the slurry composition was toluene, so pH measurement was not performed.
[0124] <Dispersion Stability> The viscosity η0 of the slurry compositions produced in the examples and comparative examples was measured at 25°C and a rotation speed of 60 rpm using a Brookfield viscometer. Thereafter, the slurry compositions were left to stand at 25°C for 7 days, and the viscosity η1 was measured again in the same manner as above. Using the measured viscosities η0 and η1, the viscosity change rate α was calculated according to the following formula (2): Viscosity change rate α (%) = (η1 / η0) × 100 (2) Then, the dispersion stability was evaluated according to the following criteria: The viscosity change rate α is 100% or more, and the closer the viscosity change rate α is to 100%, the less the viscosity change of the slurry composition over time and the more excellent the dispersion stability. A: Viscosity change rate α is 100% or more and less than 150% B: Viscosity change rate α is 150% or more and less than 200% C: Viscosity change rate α is 200% or more
[0125] <Redispersibility> The viscosity η0 of the slurry compositions produced in the examples and comparative examples was measured using a Brookfield viscometer at 25°C and 60 rpm. The dielectric layer slurry compositions were then left to stand at 25°C for 30 days to allow the dielectric material to settle. The slurry compositions were then stirred (25°C, 60 rpm), and the viscosity η2 was measured again in the same manner as above. Using the measured viscosities η0 and η2, the viscosity change rate β was calculated according to the following formula (3): Viscosity change rate β (%) = (η2 / η0) × 100 (3) The redispersibility was then evaluated according to the following criteria: A viscosity change rate β of 100% or higher and a viscosity change rate α closer to 100% indicate that the dielectric layer slurry composition has better redispersibility. A: Viscosity change rate β is 100% or more and less than 150% B: Viscosity change rate β is 150% or more and less than 200% C: Viscosity change rate β is 200% or more D: Viscosity change rate β is less than 100% (redispersion is not possible due to settling of sediment)
[0126] <Blocking Resistance> The dielectric layer was peeled off from the release substrate with the dielectric layer produced in the Examples and Comparative Examples, and the peeled dielectric layer was cut into a square with a width of 5 cm and a length of 5 cm to prepare a test piece. A polyethylene terephthalate (PET) film was prepared, and the PET film and the test piece (dielectric layer) were overlapped, and the test piece was subjected to a pressure of 40°C and 10 kg / cm. 2 After leaving it for 24 hours, the adhesion state (blocking state) of the dielectric layer to the PET film was visually confirmed, and the blocking resistance was evaluated according to the following criteria: A: The dielectric layer does not block to the PET film. B: The dielectric layer blocks to the PET film but peels off. C: The dielectric layer blocks to the PET film and does not peel off.
[0127] <Powder Fall-Off Resistance> Five test specimens measuring 5 cm wide and 5 cm long were prepared from the release substrates with a dielectric layer produced in the Examples and Comparative Examples. The following operations and measurements were performed on each test specimen. First, the initial dielectric layer weight (P0) was measured for each test specimen. Next, 11 1 mm-wide cuts were made in the test specimen using a utility knife, and the powder that was generated during the cutting was gently brushed off. The dielectric layer weight (P1) after the cuts was measured. The amount of powder falling off of the dielectric layer was calculated according to the following formula (4): Amount of powder falling off of the dielectric layer (mass %) = {(P0 - P1) / P0} × 100 (4) The above operations and measurements were repeated five times, and the average amount of powder falling off of the dielectric layer for the five specimens was calculated. The powder fall-off resistance of the dielectric layer was evaluated according to the following criteria. The smaller the amount of powder falling off of the dielectric layer, the better the dielectric layer's resistance to powder falling off. A: The average amount of powder falling off the dielectric layer is less than 5.0% by mass. B: The average amount of powder falling off the dielectric layer is 5.0% by mass or more and less than 10.0% by mass. C: The average amount of powder falling off the dielectric layer is 10.0% by mass or more.
[0128] Example 1 Preparation of Aqueous Solution of Water-Soluble Polymer A A 5 MPa pressure vessel equipped with a stirrer was charged with 30 parts of methacrylic acid (ethylenically unsaturated acid monomer), 55 parts of ethyl acrylate ((meth)acrylic acid alkyl ester monomer), and 15 parts of n-butyl acrylate ((meth)acrylic acid alkyl ester monomer) as a monomer composition, as well as 0.6 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion-exchanged water, and 1 part of potassium persulfate as a polymerization initiator. After thorough stirring, the mixture was heated to 60°C to initiate polymerization. When the polymerization conversion rate reached 96%, the mixture was cooled to terminate the reaction, and an aqueous sodium hydroxide solution was added to adjust the pH to 4, thereby obtaining an aqueous solution of water-soluble polymer A. The weight-average molecular weight and glass transition temperature of the water-soluble polymer A were measured using the obtained aqueous solution of water-soluble polymer A. The results are shown in Table 1.
[0129] <Preparation of Water-Soluble Polymer B> As the water-soluble polymer B, "Marialim SC-0505K" (a copolymer α of methoxypolyethylene glycol (11 moles of ethylene oxide added) allyl ether and maleic anhydride) manufactured by NOF Corporation was prepared. The weight-average molecular weight of the water-soluble polymer B was measured using the water-soluble polymer B. The results are shown in Table 1.
[0130] <Preparation of Particulate Polymer Dispersion> A 5 MPa pressure vessel equipped with a stirrer was charged with 33 parts of 1,3-butadiene, 3.8 parts of itaconic acid, and 63.2 parts of styrene as the monomer composition, 0.4 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion-exchanged water, and 0.5 parts of potassium peroxodisulfate as a polymerization initiator. After thorough stirring, the mixture was heated to 50°C to initiate polymerization. When the polymerization conversion rate reached 96%, the mixture was cooled to terminate the reaction, yielding a mixture containing a polymer. A 5% aqueous sodium hydroxide solution was added to the polymer-containing mixture to adjust the pH to 8, and unreacted monomer was removed by heating under reduced pressure. The mixture was then cooled to 30°C or below to yield a dispersion containing a particulate polymer (styrene-butadiene copolymer). The solids concentration of the dispersion was 40%. The average particle size of the particulate polymer was measured using the resulting dispersion. The results are shown in Table 1.
[0131] <Preparation of Slurry Composition> 100 parts of barium titanate (manufactured by Sakai Chemical Industry Co., Ltd., "BT-01") having an average particle size (d50) of 0.1 μm as a dielectric material, 12.5 parts of the aqueous solution of water-soluble polymer A prepared above (containing 5 parts of water-soluble polymer A), 1 part of water-soluble polymer B prepared above, and 25 parts of water as a solvent were stirred at 500 rpm for 20 hours using a bead mill (manufactured by Imex Co., Ltd., "RMB-01") together with 100 parts of zirconia beads (manufactured by Nikkato Corporation) having a particle size of 0.1 mm as mixing beads. Thereafter, 32 parts of water was further added, and the mixture was stirred at 500 rpm for 10 hours. The zirconia beads were filtered off, and a dispersion of barium titanate was prepared. To 142.5 parts of the barium titanate dispersion (containing 100 parts of barium titanate), 25 parts of the particulate polymer dispersion prepared above (containing 10 parts of particulate polymer) and 2 parts of glycerin as a water-soluble plasticizer were added, and the mixture was stirred at 1000 rpm for 3 minutes using a planetary centrifugal mixer to prepare a slurry composition (solid concentration 60%). The pH of the obtained slurry composition was measured, and the dispersion stability and redispersibility were evaluated. The results are shown in Table 1.
[0132] <Preparation of Dielectric Layer> The slurry composition obtained above was applied to a release-treated film (PET38AL-5, manufactured by Lintec Corporation) measuring 100 mm wide x 100 mm long using a gravure coater so that the thickness of the dielectric layer after drying would be approximately 1.0 μm, and the film was dried at 100°C for 5 minutes in the atmosphere to prepare a dielectric layer on the release substrate (ceramic green sheet method). The resulting release substrate with the dielectric layer was used to evaluate blocking resistance and powder shedding resistance. The results are shown in Table 1.
[0133] (Example 2) Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in the preparation of the aqueous solution of water-soluble polymer A, the heating temperature during polymerization was changed from 60°C to 80°C, and in the preparation of the slurry composition, the amount of each component was adjusted so that the solid content concentration of the slurry composition was 66%. The results are shown in Table 1.
[0134] (Example 3) Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in the preparation of the aqueous solution of water-soluble polymer A, the heating temperature during polymerization was changed from 60°C to 40°C, and in the preparation of the slurry composition, the amount of each component was adjusted so that the solid content concentration of the slurry composition was 55%. The results are shown in Table 1.
[0135] (Example 4) In preparing the slurry composition, the amount of water-soluble polymer B used was changed from 1 part to 0.1 part, and the amount of each component was adjusted so that the solid content concentration of the slurry composition was 62%. Except for this, various operations, measurements, and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1.
[0136] (Example 5) In preparing the slurry composition, the amount of water-soluble polymer B used was changed from 1 part to 3.5 parts, and the amount of each component was adjusted so that the solid content concentration of the slurry composition was 58%. Except for this, various operations, measurements, and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1.
[0137] (Example 6) In preparing the slurry composition, various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that the water-soluble plasticizer and the particulate polymer were not added and the amounts of each component were adjusted so that the solid content concentration of the slurry composition was 58%. The results are shown in Table 1.
[0138] Example 7 Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in preparing the water-soluble polymer B, "Marialim AKM-0531" (a copolymer β of methoxypolyethylene glycol (9 moles of ethylene oxide added) allyl ether and maleic anhydride) manufactured by NOF Corporation was prepared instead of "Marialim SC-0505K" manufactured by NOF Corporation, and in preparing the slurry composition, the amount of each component was adjusted so that the solids concentration of the slurry composition would be 62%. The results are shown in Table 1.
[0139] (Example 8) Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in preparing the water-soluble polymer B, instead of "Marialim SC-0505K" manufactured by NOF Corporation, the water-soluble polymer B was prepared by the preparation method described below, and in preparing the slurry composition, the amount of each component was adjusted so that the solids concentration of the slurry composition would be 62%. The results are shown in Table 1.
[0140] <Preparation of Water-Soluble Polymer B> A 5 MPa pressure vessel equipped with a stirrer was charged with the monomer composition: 30 parts of methacrylic acid (ethylenically unsaturated acid monomer), 55 parts of ethyl acrylate ((meth)acrylic acid alkyl ester monomer), and 15 parts of n-butyl acrylate ((meth)acrylic acid alkyl ester monomer), as well as 0.6 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion-exchanged water, 1 part of potassium persulfate as a polymerization initiator, and 1 part of t-dodecyl mercaptan (TDM) as a chain transfer agent. After thorough stirring, the mixture was heated to 60°C to initiate polymerization. When the polymerization conversion rate reached 96%, the mixture was cooled to terminate the reaction, and an aqueous sodium hydroxide solution was added to adjust the pH to 4, yielding an aqueous solution of polymer γ as water-soluble polymer B. The weight-average molecular weight of the water-soluble polymer B was measured using the resulting aqueous solution of water-soluble polymer B. The results are shown in Table 1.
[0141] (Comparative Example 1) In the preparation of the aqueous solution of water-soluble polymer A, the heating temperature during polymerization was changed from 60°C to 90°C, and in the preparation of the slurry composition, the amount of the aqueous solution of water-soluble polymer A used was changed to 22.5 parts (containing 9 parts of water-soluble polymer A), no water-soluble plasticizer and no particulate polymer were added, and the amounts of each component were adjusted so that the solids concentration of the slurry composition was 66%. Various operations, measurements, and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1.
[0142] Comparative Example 2 Except for preparing a slurry composition as follows, various operations, measurements, and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1.
[0143] <Preparation of Slurry Composition> First, the water-soluble polymer A in the aqueous solution was dried to obtain a dried product of the water-soluble polymer A. Next, 100 parts of barium titanate (manufactured by Sakai Chemical Industry Co., Ltd., "BT-01") having an average particle size (d50) of 0.1 μm as a dielectric material, 5 parts of the water-soluble polymer A, 1 part of the water-soluble polymer B, and 60 parts of toluene as a solvent were mixed with 100 parts of zirconia beads (manufactured by Nikkato Corporation) having a particle size of 0.1 mm as mixing beads, and stirred at 500 rpm for 2 hours using a bead mill (manufactured by Imex Co., Ltd., "RMB-01"). Then, 141 parts of toluene was further added, and the mixture was stirred at 500 rpm for 1 hour. The zirconia beads were filtered off to prepare a slurry composition.
[0144] In Table 1 below, "MAA" represents a methacrylic acid unit, "EA" represents an ethyl acrylate unit, "BA" represents an n-butyl acrylate unit, and "SBR" represents a styrene-butadiene copolymer.
[0145]
[0146] As is clear from Table 1, the slurry compositions of the examples are excellent in dispersion stability and redispersibility.
[0147] According to the present invention, a slurry composition for a dielectric layer having excellent dispersion stability and redispersibility can be provided. Also, according to the present invention, a dielectric layer formed by drying a coating film made of the above-mentioned slurry composition for a dielectric layer can be provided. Also, according to the present invention, a capacitor formed using the above-mentioned dielectric layer can be provided.
[0148] 10: Multilayer ceramic capacitor 11: Dielectric 12: Internal electrode 13: External electrode
Claims
1. A slurry composition for a dielectric layer comprising a dielectric material having a perovskite structure, a water-soluble polymer A, a water-soluble polymer B, and a solvent, wherein the weight average molecular weight of the water-soluble polymer A is 100,000 or more and 2,000,000 or less, the weight average molecular weight of the water-soluble polymer B is 5,000 or more and 80,000 or less, and the solvent comprises water.
2. The slurry composition for a dielectric layer according to claim 1, wherein said water-soluble polymer A contains an ethylenically unsaturated acid monomer unit.
3. A slurry composition for a dielectric layer according to claim 1, wherein the content of the water-soluble polymer B is 0.1 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the dielectric material.
4. A slurry composition for a dielectric layer according to claim 1, wherein the content of the water-soluble polymer A is 0.1 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the dielectric material.
5. A slurry composition for a dielectric layer according to claim 1, wherein a mass ratio of said water-soluble polymer B to said water-soluble polymer A is 0.01 or more and 1 or less.
6. The dielectric layer slurry composition of claim 1, further comprising a particulate polymer.
7. The slurry composition for a dielectric layer according to claim 1, having a pH of 8 or more and 12 or less.
8. A dielectric layer obtained by drying a coating film made of the slurry composition for a dielectric layer according to any one of claims 1 to 7.
9. A capacitor comprising the dielectric layer according to claim 8.
Citation Information
Patent Citations
Manufacture of aluminum nitirde green sheet
JP1985180954A
Ceramic green sheet and manufacture
JP1988147853A
Additive for molding ceramics
JP1993070212A
Ceramic slurry composition
JP1999268959A
Ceramic green sheet for laminated electronic parts
JP2001247375A