Sandwich structure body, and integrally-molded body using same
The sandwich structure with fiber-reinforced skin layers and a core layer featuring porous and resin-rich layers, combined with a thermoplastic resin layer and resin member, addresses the need for higher strength and rigidity in electronic device casings, achieving a lightweight and thin-walled design for portable devices.
Patent Information
- Application Number
- PCT/JP2024/017963
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-15
- Publication Date
- 2024-12-05
AI Technical Summary
Current integrated molded bodies used in electronic devices require further enhancement for higher strength, rigidity, and thinner wall thickness to accommodate the increasing demand for smaller and lighter portable devices.
A sandwich structure with skin layers made of fiber-reinforced resin containing continuous reinforcing fibers and a core layer with a three-layer structure, including porous layers on both sides of a resin-rich layer, and a thermoplastic resin layer on the outer surface, along with a resin member integrated at the thin wall portion, forming a stepped portion with a specific angle boundary.
This configuration results in a lightweight, high-strength, and high-rigidity integrated molded body, enabling further thinning while maintaining structural integrity, suitable for applications like personal computer housings.
Smart Images

Figure JP2024017963_05122024_PF_FP_ABST
Abstract
Description
Sandwich structure and integrally molded body using the same
[0001] The present invention relates to a sandwich structure suitable for applications requiring light weight, high strength, high rigidity and thin wall thickness, and used as components or housings for personal computers, office automation equipment, mobile phones, etc., and to an integrally molded product using the same.
[0002] Currently, as electrical and electronic devices such as personal computers, office automation equipment, audiovisual equipment, mobile phones, telephones, facsimiles, home appliances, toys, etc. become more portable, there is a demand for them to be smaller and lighter. To achieve this, miniaturization of components inside the housing and thinning of the housing are required.
[0003] Patent Document 1 discloses an integrated molded body in which at least a portion of the plate end of a sandwich structure consisting of a core layer made of discontinuous reinforcing fibers and thermoplastic resin and a surface layer (skin layer) made of continuous fibers and resin is used as a joint, and another structure is arranged at the joint, and the sandwich structure has a region in which the porosity of the core layer in the main body part other than the joint is lower than the porosity of the core layer at the joint, and the integrated molded body is suitable for housing applications that require light weight, high strength, high rigidity, and thin wall thickness.
[0004] JP 2016-49649 A
[0005] However, although the integrally molded body described in Patent Document 1 contributes to thinner walls and higher rigidity, in order to achieve the current trend of further reducing the thickness of housings, it is essential to make the integrally molded body even more rigid.
[0006] Therefore, an object of the present invention is to provide an integrally molded body that can achieve high strength, high rigidity, light weight, and thin wall thickness.
[0007] In order to solve the above problems, the present invention employs the following configurations: [1] A sandwich structure in which skin layers made of a fiber-reinforced resin containing continuous reinforcing fibers and a resin are arranged on both sides of a core layer containing discontinuous reinforcing fibers and a thermoplastic resin, wherein at least a portion of the core layer has a three-layer structure in which porous layers are arranged on both sides of a resin-rich layer, and the thickness of the resin-rich layer in the three-layer structure is 1 to 60% of the thickness of the core layer. [2] The sandwich structure according to [1], in which the porous layer is formed by expanding a porous layer precursor containing discontinuous reinforcing fibers and a thermoplastic resin by 1.1 to 7.0 times in the thickness direction. [3] An integrally molded body formed by forming a thermoplastic resin layer on one outer surface of the sandwich structure according to [1] or [2], and bonding and integrating the thermoplastic resin layer with a resin member arranged on the outer peripheral edge side of the sandwich structure, wherein the sandwich structure has a stepped portion with a difference in thickness and a thick portion with a constant thickness in at least a part of the outer peripheral edge, the stepped portion has a thin portion with a porosity lower than the fiber volume content of the porous layer constituting the thick portion, and the resin member and the thermoplastic resin layer are bonded at the thin portion. [4] The integrally molded body according to [3], wherein the stepped portion has a boundary portion connecting the thick portion and the thin portion, and the surface of the boundary portion forms an angle of 1 to 30° with the surface of the skin layer.
[0008] According to the present invention, when used in the housing of a personal computer or the like, it is possible to obtain an integrally molded body that is lightweight, thin, high in strength and high in rigidity.
[0009] 7 is a schematic side view showing a sandwich structure according to one embodiment of the present invention. FIG. 8 is a schematic plan view showing a core layer consisting of a matrix resin and reinforcing fibers with a three-dimensional network structure that constitutes the sandwich structure of FIG. 1. FIG. 9 is a schematic side view showing the vicinity of a joint of an integrally molded body according to one embodiment of the present invention. FIG. 10 is a perspective view of an integrally molded body having a step portion according to another embodiment of the present invention. FIG. 11 is a schematic view showing recycled fibers used in the resin member of the integrally molded body of FIG. 3. FIG. 12 is a schematic side view of an integrally molded body having an arch shape according to yet another embodiment of the present invention. FIG. 13 is a perspective view of an integrally molded body obtained by injection molding a resin member onto the sandwich structure of the present invention. FIG. 14 is a schematic side view showing the vicinity of a joint formed by injection molding a resin member onto the outer surface of the non-design surface side of the integrally molded body of FIG. 15. FIG. 16 is a schematic side view showing the vicinity of a joint formed by providing a thermoplastic resin layer on the outer surface of the non-design surface side of the integrally molded body of FIG. 16. FIG. 17 is a schematic side view showing the manner of a resin-rich layer in a thick portion, a step portion, and a thin portion according to another embodiment of the present invention.
[0010] Hereinafter, embodiments of the present invention will be described with reference to the drawings. Note that the present invention is not limited in any way by the drawings or examples. In this specification, the notation "a to b" in the description of a range of values means a to b, unless otherwise specified.
[0011] The sandwich structure according to the present invention is a sandwich structure in which skin layers having fiber-reinforced resin members made of continuous reinforcing fibers and resin are arranged on both sides of a core layer, and porous layers containing discontinuous reinforcing fibers and thermoplastic resin are formed on both sides of a resin-rich layer formed in the center of the core layer, the thickness of the resin-rich layer is 1 to 60% of the thickness of the core layer, and the outer surface of the porous layer is bonded to the skin layer.
[0012] FIG. 1 shows a schematic side view of a sandwich structure according to an embodiment of the present invention. The sandwich structure 100 according to the present invention comprises skin layers 110, each having a fiber-reinforced resin member made of continuous reinforcing fibers and a resin, disposed on both sides of a core layer 120. The core layer 120 is formed of porous layers 122 containing discontinuous reinforcing fibers and a thermoplastic resin, on both sides of a resin-rich layer 121 formed in the center of the core layer 120. The resin-rich layer 121 has a thickness of 1 to 60% of the thickness of the core layer 120, and the outer surface of the porous layer 122 is bonded to the skin layer 110. By providing the resin-rich layer 121 within the core layer 120, the shear stress of the core layer 120 itself is increased, making the sandwich structure 100 stronger. This allows for even thinner walls when used in, for example, a personal computer housing.
[0013] Examples of reinforcing fibers that can be used in the sandwich structure 100 of the present invention include metal fibers such as aluminum fibers, brass fibers, and stainless steel fibers; inorganic fibers such as polyacrylonitrile (PAN), rayon, lignin, and pitch-based carbon fibers and graphite fibers; glass fibers, silicon carbide fibers, silicon nitride fibers, alumina fibers, silicon carbide fibers, and boron fibers; and organic fibers such as aramid fibers, polyparaphenylene benzobisoxazole (PBO) fibers, polyphenylene sulfide fibers, polyester fibers, acrylic fibers, nylon fibers, and polyethylene fibers. These reinforcing fibers may be used alone or in combination of two or more.
[0014] Of these, carbon fibers are preferred as the reinforcing fibers used in the skin layer 110 constituting the sandwich structure 100 from the viewpoints of specific strength, specific rigidity, and light weight, and carbon fibers (including graphite fibers) such as polyacrylonitrile (PAN)-based carbon fibers, rayon-based carbon fibers, lignin-based carbon fibers, and pitch-based carbon fibers, which have excellent specific strength and specific rigidity, are preferably used. In the present invention, polyacrylonitrile (PAN)-based carbon fibers are preferred from the viewpoints of cost and processability.
[0015] Furthermore, either a thermoplastic resin or a thermosetting resin can be used as the resin used for the skin layer 110. There are no particular limitations on the thermoplastic resin, and any of the thermoplastic resins exemplified below can be used. For example, polyester resins such as polyethylene terephthalate (PET) resin, polybutylene terephthalate (PBT) resin, polytrimethylene terephthalate (PTT) resin, polyethylene naphthalate (PEN resin), and liquid crystal polyester resin; polyolefin resins such as polyethylene (PE resin), polypropylene (PP resin), and polybutylene resin; polyarylene sulfide resins such as polyoxymethylene (POM) resin, polyamide (PA) resin, and polyphenylene sulfide (PPS) resin; polyketone (PK) resin, polyether ketone (PEK) resin, polyether ether ketone (PEEK) resin, polyether ketone ketone (PEKK) resin, polyether nitrile (PEN) resin, and polytetrafluoroethylene resin. Examples of the resin include crystalline resins such as fluorine-based resins, liquid crystal polymers (LCPs), and styrene-based resins, as well as amorphous resins such as polycarbonate (PC) resin, polymethyl methacrylate (PMMA) resin, polyvinyl chloride (PVC) resin, polyphenylene ether (PPE) resin, polyimide (PI) resin, polyamideimide (PAI) resin, polyetherimide (PEI) resin, polysulfone (PSU) resin, polyethersulfone resin, and polyarylate (PAR) resin, as well as thermoplastic resins selected from phenol-based resins, phenoxy resins, and thermoplastic elastomers such as polystyrene-based resins, polyurethane-based resins, polybutadiene-based resins, polyisoprene-based resins, and acrylonitrile-based resins, as well as copolymers and modified products thereof.
[0016] Among these, polyolefin resins are preferred from the viewpoint of the lightness of the resulting molded article, polyamide resins are preferred from the viewpoint of strength, amorphous resins such as polycarbonate resins, styrene-based resins, and modified polyphenylene ether-based resins are preferred from the viewpoint of surface appearance, polyarylene sulfide resins are preferred from the viewpoint of heat resistance, and polyether ether ketone resins are preferred from the viewpoint of continuous use temperature. The thermoplastic resins exemplified above may contain impact resistance improvers such as elastomers or rubber components, other fillers, and additives, as long as the purpose of the present invention is not impaired. Examples of these additives include inorganic fillers, flame retardants, conductivity imparting agents, crystal nucleating agents, ultraviolet absorbers, antioxidants, vibration dampers, antibacterial agents, insect repellents, deodorizing agents, color inhibitors, heat stabilizers, mold release agents, antistatic agents, plasticizers, lubricants, colorants, pigments, dyes, foaming agents, foam control agents, and coupling agents.
[0017] When the resin constituting the skin layer 110 is a thermosetting resin, preferred examples include unsaturated polyester resin, vinyl ester resin, epoxy resin, phenol (resol type) resin, urea-melamine resin, polyimide resin, maleimide resin, and benzoxazine resin. A blend of two or more of these resins may also be used. Among these, epoxy resins are particularly preferred from the viewpoint of the mechanical properties and heat resistance of the molded body. When using an epoxy resin, it is preferred that it be included as the main component of the resin used in order to exhibit its excellent mechanical properties, and specifically, it is preferred that it be included in an amount of 60% by weight or more of the resin composition.
[0018] From the viewpoint of ease of handling, it is preferable to use a prepreg, which is a base material in which reinforcing fibers are pre-impregnated with resin, for the skin layer 110 .
[0019] When carbon fibers are used as the reinforcing fibers constituting the sandwich structure 100, the tensile modulus is preferably in the range of 200 to 1000 GPa from the viewpoint of the rigidity of the sandwich structure 100, and more preferably in the range of 400 to 900 GPa from the viewpoint of the handleability of the prepreg. If the tensile modulus of the carbon fiber is less than 200 GPa, the rigidity of the sandwich structure may be poor, while if it is greater than 1000 GPa, the crystallinity of the carbon fiber must be increased, making it difficult to manufacture the carbon fiber. A tensile modulus of the carbon fiber within the above range is preferable in terms of further improving the rigidity of the sandwich structure and improving the manufacturability of the carbon fiber. The tensile modulus of the carbon fiber can be measured by a strand tensile test according to JIS R7301-1986.
[0020] When carbon fibers are used as the reinforcing fibers constituting the skin layers of the sandwich structure 100, the density is 1.6 g / cm in the case of polyacrylonitrile (PAN)-based carbon fibers. 3 2.0g / cm or more 3 From the viewpoint of improving rigidity, 1.8 g / cm 3 2.0g / cm or more 3 In the case of pitch-based carbon fiber, 2.0 g / cm 3 2.5g / cm or more 3 From the viewpoint of cost, 2.0 g / cm 3 2.3g / cm or more 3 In the present invention, polyacrylonitrile (PAN)-based carbon fibers are preferred because of their excellent processability.
[0021] These fibers may be surface-treated, such as by coating with a metal, by using a coupling agent, by using a sizing agent, or by applying an additive.
[0022] Furthermore, in the present invention, the sandwich structure 100 includes a skin layer 110 and a core layer 120 in a layered configuration, and it is preferable that two or more prepregs (two layers) are laminated per skin layer 110.
[0023] The prepregs constituting each skin layer 110 can be freely set and laminated according to the desired rigidity, thickness, strength, etc. of the sandwich structure 100. From the viewpoint of the thickness of the sandwich structure 100, the thickness per prepreg is preferably 0.05 to 1.00 mm. More preferably, from the viewpoint of the degree of freedom in lamination design, the thickness is preferably 0.05 to 0.20 mm.
[0024] A woven fiber substrate can also be used for the skin layer of the sandwich structure 100. A woven fiber substrate is a substrate in which continuous reinforcing fiber bundles, each consisting of 1,000 continuous reinforcing fibers, are used as warp and weft threads, and two sets of threads are crossed at substantially right angles using a loom. A bundle of 1,000 continuous reinforcing fibers is generally called a 1K, a bundle of 3,000 fibers is called a 3K, and a bundle of 12,000 fibers is called a 12K.
[0025] The fiber woven substrate is preferably at least one woven fabric selected from plain weave, twill weave, satin weave, and satin weave. Since the fiber woven substrate has a characteristic fiber pattern, by using a fiber woven substrate that highlights the characteristic fiber pattern as the outermost layer (design surface side) of the sandwich structure, an integrated molded body that exhibits a novel surface pattern can be obtained. The continuous reinforcing fiber bundles are preferably 1K to 24K, and more preferably 1K to 6K from the viewpoint of the stability of the fiber pattern during processing.
[0026] Furthermore, when a fiber woven fabric substrate is used for the skin layer 110 of the sandwich structure 100, the core layer 120 acts as a cushion, making it possible to reduce the size of spots of resin deficiency called "pits" at the intersections of the warp and weft threads. 2 Preferably less than 0.2 mm 2 is less than.
[0027] Furthermore, the type of thermoplastic resin constituting the resin-rich layer 121 of the core layer 120 of the sandwich structure 100 is not particularly limited, and any of the thermoplastic resins exemplified below can be used. For example, polyester resins such as polyethylene terephthalate (PET) resin, polybutylene terephthalate (PBT) resin, polytrimethylene terephthalate (PTT) resin, polyethylene naphthalate (PEN resin), and liquid crystal polyester resin; polyolefin resins such as polyethylene (PE resin), polypropylene (PP resin), and polybutylene resin; polyarylene sulfide resins such as polyoxymethylene (POM) resin, polyamide (PA) resin, and polyphenylene sulfide (PPS) resin; polyketone (PK) resin, polyether ketone (PEK) resin, polyether ether ketone (PEEK) resin, polyether ketone ketone (PEKK) resin, polyether nitrile (PEN) resin, and polytetrafluoroethylene resin. Examples of the resin include crystalline resins such as fluorine-based resins, liquid crystal polymers (LCPs), and styrene-based resins, as well as amorphous resins such as polycarbonate (PC) resin, polymethyl methacrylate (PMMA) resin, polyvinyl chloride (PVC) resin, polyphenylene ether (PPE) resin, polyimide (PI) resin, polyamideimide (PAI) resin, polyetherimide (PEI) resin, polysulfone (PSU) resin, polyethersulfone resin, and polyarylate (PAR) resin, as well as thermoplastic resins selected from phenol-based resins, phenoxy resins, and thermoplastic elastomers such as polystyrene-based resins, polyurethane-based resins, polybutadiene-based resins, polyisoprene-based resins, and acrylonitrile-based resins, as well as copolymers and modified products thereof.
[0028] Among these, polyolefin resins are preferred from the viewpoint of the light weight of the resulting integrally molded body, polyamide resins are preferred from the viewpoint of strength, amorphous resins such as polycarbonate resins, styrene-based resins, and modified polyphenylene ether-based resins are preferred from the viewpoint of surface appearance, polyarylene sulfide resins are preferred from the viewpoint of heat resistance, and polyether ether ketone resins are preferably used from the viewpoint of continuous use temperature.
[0029] Furthermore, from the viewpoint of bonding strength, it is preferable that the thermoplastic resin constituting the core layer 120 of the sandwich structure 100 and the thermoplastic resin constituting the resin-rich layer 121 are the same type of resin.
[0030] The exemplified thermoplastic resins may contain impact resistance improvers such as elastomers or rubber components, other fillers, and additives, provided that the object of the present invention is not impaired. Examples of these include inorganic fillers, flame retardants, conductivity imparting agents, crystal nucleating agents, ultraviolet absorbers, antioxidants, vibration dampers, antibacterial agents, insect repellents, deodorizing agents, color inhibitors, heat stabilizers, release agents, antistatic agents, plasticizers, lubricants, colorants, pigments, dyes, foaming agents, foam control agents, and coupling agents.
[0031] It is important that the porous layers 122 of the core layer 120, which are arranged on both sides of the resin-rich layer 121, are made of a porous base material made of discontinuous reinforcing fibers and a thermoplastic resin.
[0032] The discontinuous reinforcing fibers constituting the porous layer 122 can be the same as the reinforcing fibers used in the skin layer 110 described above.
[0033] Here, continuous fibers and discontinuous reinforcing fibers are defined. Continuous fibers refer to reinforcing fibers contained in the skin layers constituting a sandwich structure that are arranged substantially continuously over the entire length or width of the sandwich structure, while discontinuous reinforcing fibers refer to reinforcing fibers that are intermittently broken. Generally, fibers used as unidirectional fiber-reinforced resins in which reinforcing fibers aligned in one direction are impregnated with resin fall under the category of continuous fibers, while reinforcing fibers contained in SMC (sheet molding compound) substrates used in press molding, pellet materials used in injection molding, etc. fall under the category of discontinuous reinforcing fibers.
[0034] The thermoplastic resin used in the porous layer 122 can be the same as the thermoplastic resin used in the resin-rich layer 121 described above. Alternatively, as shown in FIG. 2 , the thermoplastic resin may be present as a matrix resin with a three-dimensional network structure. The thermoplastic resin is expanded in a planar manner in the area surrounded by the contour formed by the annularly arranged discontinuous reinforcing fibers 125 in the three-dimensional network structure composed of the discontinuous reinforcing fibers 125, and forms a plurality of holes 126. The contour formed by the annularly arranged discontinuous reinforcing fibers 125 is not limited to the hexagon shown in FIG. 2 , but may also be a polygon such as a triangle or a square. The formation of such holes 126 makes the thermoplastic resin that spreads in a planar manner less likely to break in the stretching direction when stretched, and the bond between the discontinuous reinforcing fibers 125 can be maintained, making it possible to bond the discontinuous reinforcing fibers 125 more firmly than if the holes 126 were not formed in the thermoplastic resin. Furthermore, the thermoplastic resin having a plurality of holes 126 can be stretched more greatly, increasing the porosity of the porous layer 122, which is expected to further reduce the weight. By adopting such a structure, the rigidity of the sandwich structure 100 can be increased.
[0035] Furthermore, by providing a high-density resin-rich portion 121 in the center of the core layer 120 of the sandwich structure 100, it is possible to increase the shear strength of the sandwich structure 100. Furthermore, by arranging low-density porous layers 122 on both sides of the resin-rich layer 121, it is possible to achieve both strength and weight reduction.
[0036] Here, the resin-rich layer 121 will be defined. The resin-rich layer refers to a layer in which a thermoplastic resin is filled into the mesh of a three-dimensional network structure formed by discontinuous reinforcing fibers 125, and there are no voids. When the thickness of the core layer 120 is constant, the resin-rich layer 121 is formed near the center of the core layer 120 in the thickness direction. When the thickness of the core layer 120 varies, at least a portion of the core layer 120 may have a porous layer 122, that is, the core layer 120 may be composed of only the resin-rich layer 121.
[0037] It is also important that the thickness of the resin-rich layer 121 is 1 to 60% of the thickness of the core layer 120. A thickness within this range makes it possible to obtain a strong sandwich structure 100. From the viewpoint of adhesion between the skin layer 110 and the core layer 120, the thickness is preferably 1 to 30%, and more preferably 3 to 20%.
[0038] From the viewpoint of reducing weight, the specific gravity of the sandwich structure 100 is preferably 0.5 to 1.4.
[0039] In the present invention, the porous layer 122 is preferably formed by expanding a porous layer precursor containing discontinuous reinforcing fibers and a thermoplastic resin by 1.1 to 7.0 times in the thickness direction. From the viewpoint of ensuring the thickness and lightness of the core layer 120, the expansion is preferably 2.0 to 7.0 times, and more preferably 2.9 to 7.0 times.
[0040] Furthermore, in the present invention, one surface of the sandwich structure 100 is a design surface 100a and the other surface is a non-design surface 100b, a thermoplastic resin layer 300 is provided on the outer surface of the non-design surface 100b, and a resin member 200 injected onto the outer periphery of the sandwich structure 100 and the thermoplastic resin layer 300 are bonded together, and it is preferable that the sandwich structure 100 has a thin-walled sandwich structure (thin-walled portion 151) at least at a portion of its end portion having a void ratio lower than the fiber volume content of the sandwich structure 100, and the resin member 200 is bonded only to the thin-walled sandwich structure (thin-walled portion) 151.
[0041] 3 shows an integrated molded body 1000 in which one surface of a sandwich structure 100 is a designed surface 100a and the other surface is a non-design surface 100b, a thermoplastic resin layer 130 is provided on the outer surface of the non-design surface 100b side, and a resin member 200 is injected onto the outer periphery of the sandwich structure 100 to form an integrated body. By joining the outer peripheral side portion of the sandwich structure 100 and the thermoplastic resin layer 130, the reliability of the joining can be improved.
[0042] Here, the type of thermoplastic resin layer 130 is not limited as long as it is one of the thermoplastic resins listed for the resin-rich layer 121. Among them, resins such as polycarbonate resin, styrene-based resin, and modified polyphenylene ether-based resin are preferred from the viewpoints of adhesiveness and formability.
[0043] 4, the sandwich structure 100 has a stepped portion 150 with a difference in thickness at least at a portion of the end and a thick portion 160 with no change in thickness, and the stepped portion 150 has a thin portion 151 with a porosity lower than the fiber volume content of the porous layer 122 that constitutes the thick portion 160, and a boundary portion 152 connecting the thick portion 160 and the thin portion 151. It is preferable that the resin member 200 is bonded to the entire outer periphery of the thin portion 151. By forming an integrated molded body 1000 in which the resin member 200 is bonded to the entire outer periphery of the thin portion 151, the thickness can be further reduced and the reliability of the bond can be improved.
[0044] Furthermore, in the present invention, the resin member 200 is preferably bonded to the entire outer periphery of the sandwich structure 100. By forming a bonded portion with the resin member 200 along the entire outer periphery of the sandwich structure 100, high bonding strength and a thin wall can be achieved for the entire integrally molded body 1000. Here, the type of resin member 200 is not limited as long as it is a thermoplastic resin listed for the resin-rich layer 121 described above. Among these, resins such as polycarbonate resin, styrene-based resin, and modified polyphenylene ether-based resin are preferred from the viewpoints of adhesion to the thermoplastic resin layer 130 and moldability.
[0045] Furthermore, the resin member 200 also contains a thermoplastic resin, and when the sandwich structure 100 has a thermoplastic resin layer 130 on the non-design surface 100b, a joint structure can be formed in which the thermoplastic resin of the resin member 200 melts and bonds with the thermoplastic resin of the thermoplastic resin layer 130. This allows for a higher joint strength to be achieved as the integrally molded body 1000. The melt-bonded joint structure refers to a joint structure in which the members are melted by heat and then solidified by cooling.
[0046] In addition, from the viewpoint of reducing warpage of the integrally molded body 1000, it is preferable that the resin member 200 contains reinforcing fibers.
[0047] The reinforcing fibers used in the resin member 200 are preferably carbon fiber and glass fiber from the viewpoint of the strength of the resin member. Glass fiber is more preferable, and the use of glass fiber can impart the resin member with the function of a radio wave transmitting member.
[0048] Here, it is preferable that the reinforcing fibers are discontinuous reinforcing fibers, and the weight average fiber length of the discontinuous reinforcing fibers is preferably 0.3 to 3 mm.
[0049] As a method for measuring the fiber length of discontinuous reinforcing fibers, for example, there is a method of directly removing the discontinuous reinforcing fibers from the integrally molded body 1000 and measuring them by microscopic observation. When resin is attached to the discontinuous reinforcing fibers, the resin is dissolved using a solvent that dissolves only the resin attached to the discontinuous reinforcing fibers, and the remaining discontinuous reinforcing fibers are filtered and measured by microscopic observation (dissolution method). In addition, when there is no solvent that dissolves the resin, only the resin is burned off in a temperature range where the discontinuous reinforcing fibers do not oxidize and lose weight, and the discontinuous reinforcing fibers are separated and measured by microscopic observation (burn-off method). 400 discontinuous reinforcing fibers are randomly selected, and their lengths are measured to the nearest 1 μm using an optical microscope to determine the fiber length and its ratio.
[0050] The discontinuous reinforcing fibers used in the resin member 200 do not need to be virgin materials, and may be fiber-reinforced plastic pieces obtained by crushing fiber-reinforced plastic made of a thermoplastic resin or a thermosetting resin having a melting point sufficiently higher than that of the injected resin, or fibers obtained from fiber-reinforced plastic pieces that have been crushed, classified, and heat-treated for recycling. More preferably, from the viewpoint of reducing waste to be landfilled, recycled fibers obtained by crushing, classifying, and heat-treating waste fiber-reinforced plastic made of a thermosetting resin are preferred.
[0051] Also, as shown in Figure 5, some of the recycled fibers may be dispersed in the form of single threads, and another part of the reinforcing fibers may not be dispersed but may be randomly arranged in the form of a converging portion 210 made up of multiple single threads.
[0052] Furthermore, a resin different from the thermoplastic resin used in the resin member 200 may be attached to the surface of the single yarn constituting the converging portion 210. It is preferable that the amount of the resin attached is 0.1 to 30 parts by mass per 100 parts by mass of the reinforcing fibers included in the converging portion 210.
[0053] In the present invention, the weight fiber content of the discontinuous reinforcing fibers contained in the resin member 200 is preferably 1 to 60% by weight. This increases the bonding strength with the sandwich structure and reduces warpage of the integrated molded body. If it is less than 1% by weight, it may be difficult to ensure the strength of the sandwich structure 100, and if it exceeds 60% by weight, the filling of the resin member may be partially insufficient during injection molding. From the viewpoint of moldability of the resin member, it is preferably 5 to 55% by weight, more preferably 8 to 50% by weight, and even more preferably 12 to 45% by weight.
[0054] The boundary surface connecting the sandwich structure 100 and the thin sandwich structure (thin portion) 151 preferably has an angle of 1 to 30° with respect to the in-plane direction of the skin layer 120 of the sandwich structure 100 .
[0055] Specifically, the angle θ of the inclined surface of the step portion 150 relative to the in-plane direction of the skin layer 120 (the direction parallel to the surface of the skin layer 120) is preferably 1 to 30° from the standpoint of the formability of the sandwich structure 100 and ensuring its thickness, more preferably 2 to 30°, and even more preferably 3.5 to 30°.
[0056] Modified examples of the integrally molded body 1000 according to the present invention will be described below.
[0057] First, the arch-shaped integrally molded body 1000 will be described with reference to FIG.
[0058] From the viewpoint of ensuring space for inserting internal components, the integrated molded body 1000 according to the present invention preferably has a concave portion extending from the non-design surface 100b toward the design surface 100a in a portion of the non-design surface 100b. In this case, it is preferable that at least a portion of the concave portion is a curved surface, and it is more preferable that the entire surface is a curved surface from the viewpoint of ease of molding. In a plan view, it is preferable that 50% or more of the entire non-design surface 100b form a concave portion, more preferably a partial or entire curved surface, and even more preferable that the curved shape is continuously curved as described above. The area of the curved portion is more preferably 80% or more, even more preferably 90% or more, of the exposed area of the sandwich structure 100, and it is particularly preferable that the curved portion is formed over the entire area. In this case, it is preferable that the areas other than the concave portion are flat.
[0059] In the present invention, it is preferable that the height difference 300 between the horizontal extension line from the maximum height portion of the design surface 100a of the sandwich structure 100 and the horizontal extension line from the minimum height portion of the design surface 100a is greater than 0 mm and not more than 5 mm. If the height difference 300 is 0 mm (completely flat), interference with internal components may occur when the sandwich structure 100 has a thickness of a certain level or more. On the other hand, if the height difference 300 exceeds 5 mm, interference with internal components may be avoided, but when viewed from the design surface 100a, the convex shape may be noticeable, which may be disadvantageous in terms of appearance.
[0060] The preferred range of the height difference 300 varies depending on the part and purpose of use in the integrally molded body 1000, but is preferably 4 mm or less, and more preferably 2 mm or less, in consideration of appearance, etc. From the viewpoint of ensuring an internal component insertion space, a range of more than 0 mm and 0.5 mm or less is preferred, and from the viewpoints of ensuring an internal component insertion space and appearance, a range of more than 0 mm and 0.1 mm or less is more preferred, and a range of more than 0 mm and 0.05 mm or less is even more preferred.
[0061] From the viewpoint of prioritizing securing space for inserting internal components and providing a certain thickness to the sandwich structure 100, the height difference 300 is preferably 1 mm or more. Regarding the convex shape of the design surface 100a, the specific proportion of the area of the design surface where the convex portion is formed in a plan view is the same as the preferred proportion for the concave portion on the non-design surface 100b. As with the concave portion on the non-design surface 100b, it is preferable that at least a portion of the area is a curved surface. More preferably, as with the non-design surface 100b, a certain area is a curved surface, and the convex portion continuously rises from the periphery in the in-plane direction of the sandwich structure 100 toward the center or a position shifted from the center. One optimal embodiment is for one curved convex portion to be formed over the entire area of the design surface 100a.
[0062] 7, 8, and 9, it is also preferable to separate the separate member 400 from the sandwich structure 100 before injecting the resin member 200, place the separate member 400 on the outer periphery of the sandwich structure 100, and then injection-molde the resin member 200 into the gap between the sandwich structure 100 and the separate member 400. This is an effective means for realizing low warpage of the integrated molding 1200.
[0063] As the separate member 400, a fiber-reinforced resin frame made of reinforcing fibers and resin is preferred from the viewpoint of the strength and rigidity of the integrally molded body 1200. The reinforcing fibers constituting the separate member 400 can be the same as those used in the resin member 200 described above. From the viewpoint of increasing the strength of the separate member 400, glass fiber and carbon fiber are preferred, and from the viewpoint of antenna performance, glass fiber is preferred. On the other hand, although carbon fiber is inferior to glass fiber in antenna performance, it can be used effectively to improve strength and rigidity.
[0064] In the present invention, the maximum thickness of the sandwich structure 100 is preferably 0.3 mm to 2.0 mm. If it is less than 0.3 mm, the rigidity of the integrally molded body 1200 is likely to be insufficient. If it exceeds 2.0 mm, the lightness may be impaired. From the viewpoint of lightness and rigidity, the maximum thickness is more preferably 0.7 mm to 1.5 mm. The maximum thickness is the value measured at the thickest part of the sandwich structure 100.
[0065] In the present invention, the porous layer 122 formed of the discontinuous reinforcing fibers and thermoplastic resin that constitute the core layer 120 preferably has a porosity such that the porosity of the porous layer 122 at the joints 190 is different from the porosity of the porous layer 122 in regions other than the joints 190, from the viewpoint of the rigidity of the integrally molded body 1000. Furthermore, it is preferable that the porosity of the porous layer 122 at the joints 190 is lower than the porosity of the porous layer 122 in regions other than the joints 190.
[0066] Furthermore, in the present invention, by forming the sandwich structure 100 in a rectangular shape when viewed from above, the area of the resin member 200 is reduced, thereby achieving low warpage in the integral molding.
[0067] The integrally molded article using the sandwich structure of the present invention can be effectively used for automobile interiors and exteriors, electrical and electronic equipment housings, bicycles, structural materials for sporting goods, aircraft interior materials, transport boxes, etc. Among these, it can be particularly used for personal computer housings (for example, notebook computer housings with a side length of 200 mm to 500 mm, or even 200 mm to 400 mm) for which there is a high demand for lighter and thinner sizes.
[0068] 100 Sandwich structure 100a Design surface 100b Non-design surface 110 Skin layer 120 Core layer 121 Resin-rich layer 122 Porous layer 125 Discontinuous reinforcing fibers 126 Hole 130 Thermoplastic resin layer 150 Step portion 151 Thin portion 152 Boundary portion 160 Thick portion 190 Joint portion 200 Resin member 210 Converging portion 300 Height difference 400 Separate member 1000, 1200 Integrated molded body θ Angle of inclined surface
Claims
1. A sandwich structure in which skin layers made of fiber-reinforced resin containing continuous reinforcing fibers and resin are arranged on both sides of a core layer containing discontinuous reinforcing fibers and a thermoplastic resin, wherein at least a portion of the core layer has a three-layer structure in which a porous layer is arranged on both sides of a resin-rich layer, and the thickness of the resin-rich layer in the three-layer structure is 1 to 60% of the thickness of the core layer.
2. The sandwich structure according to claim 1, wherein the porous layer is formed by expanding a porous layer precursor containing discontinuous reinforcing fibers and a thermoplastic resin by 1.1 to 7.0 times in the thickness direction.
3. An integrated molded body formed by forming a thermoplastic resin layer on one outer surface of the sandwich structure described in claim 1 or 2, and bonding and integrating a resin member arranged on the outer peripheral end side of the sandwich structure with the thermoplastic resin layer, characterized in that the sandwich structure has a step portion with a thickness difference and a thick-walled portion of constant thickness on at least a part of the outer peripheral end, the step portion has a thin-walled portion with a porosity lower than the fiber volume content of the porous layer constituting the thick-walled portion, and the resin member and the thermoplastic resin layer are bonded at the thin-walled portion.
4. An integrally molded body as described in claim 3, wherein the step portion has a boundary portion connecting the thick portion and the thin portion, and the surface of the boundary portion forms an angle of 1 to 30 degrees with the surface of the skin layer.
Citation Information
Patent Citations
Sandwich structure
JP2012000890A
Laminate with bending rigidity, molded product from the laminate, and method for manufacturing the same.
JP2014508055A
Integrally molded body and method for producing same
WO2018142971A1