Resin composition for ink modification, modifier for gravure ink, and gravure ink

The combination of ethylene-vinyl ester and acrylic block copolymers in a specific mass ratio and composition improves the fluidity and solubility of gravure inks in ester solvents, addressing the fluidity issues of ethylene-vinyl ester copolymers alone and maintaining transparency without the need for additional fillers.

WO2024247769A1PCT designated stage expired Publication Date: 2024-12-05DOW MITSUI POLYCHEMICALS CO LTD

Patent Information

Application Number
PCT/JP2024/018391
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2024-05-17
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Gravure inks using ethylene-vinyl ester copolymers alone exhibit decreased fluidity when dissolved in ester solvents, which is a concern for environmental toluene-free formulations.

Method used

A resin composition combining ethylene-vinyl ester copolymers with acrylic block copolymers, where the total content of both is between 70% to 100% by mass, with specific ranges for vinyl acetate content and melt mass flow rates, enhances solubility and fluidity in ester solvents.

Benefits of technology

The composition ensures excellent fluidity and solubility in ester solvents while reducing the need for inorganic fillers, thereby maintaining transparency and preventing blocking, even with reduced vinyl acetate content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

Provided is a resin composition for ink modification, the resin composition containing an ethylene-vinyl ester copolymer A and an acrylic block copolymer B, wherein the total content of the ethylene-vinyl ester copolymer A and the acrylic block copolymer B is more than 70 mass% and not more than 100 mass% on the basis of the total mass of the resin composition for ink modification.
Need to check novelty before this filing date? Find Prior Art

Description

Resin composition for modifying ink, gravure ink modifier, and gravure ink

[0001] The present disclosure relates to a resin composition for modifying ink, a modifier for gravure ink, and gravure ink.

[0002] Among ethylene-vinyl acetate copolymers (EVA) and other ethylene-vinyl ester copolymers, EVA, which has a particularly high content of structural units derived from vinyl acetate (VA), has excellent adhesive properties and is therefore used as a modifier for gravure inks. Among various organic solvents for gravure inks, toluene is particularly inexpensive, has suitable drying properties during printing, and has high solubility for resins, additives, and the like. However, in light of recent environmental concerns, toluene-free organic solvents, which do not use toluene, are becoming more common in various countries, and a shift from toluene to ester-based solvents such as ethyl acetate is underway (see, for example, Patent Document 1).

[0003] Japanese Patent Application Laid-Open No. 2006-131843

[0004] When an ethylene-vinyl ester copolymer such as EVA is used alone as the resin component of an ink modifying resin composition, the fluidity of the ink modifying resin composition dissolved in an ester solvent tends to decrease.

[0005] An object of the present disclosure is to provide a resin composition for modifying ink and a gravure ink that have excellent flowability when dissolved in an ester-based solvent.

[0006] Specific means for solving the above problems include the following aspects. <1> A resin composition for modifying ink, comprising an ethylene-vinyl ester copolymer A and an acrylic block copolymer B, wherein the total content of the ethylene-vinyl ester copolymer A and the acrylic block copolymer B is more than 70% by mass and not more than 100% by mass, relative to the total mass of the resin composition for modifying ink. <2> The resin composition for modifying ink according to <1>, wherein the ethylene-vinyl ester copolymer A comprises an ethylene-vinyl acetate copolymer. <3> The resin composition for modifying ink according to <2>, wherein the content of structural units derived from vinyl acetate contained in the ethylene-vinyl acetate copolymer is 28% by mass to 48% by mass, relative to the total mass of the ethylene-vinyl acetate copolymer. <4> The resin composition for modifying ink according to any one of <1> to <3>, wherein the melt mass flow rate of the ethylene-vinyl ester copolymer A at 190°C under a load of 2160 g, as measured in accordance with JIS K7210:1999, is 0.1 g / 10 min to 800 g / 10 min. <5> The resin composition for modifying ink according to any one of <1> to <4>, wherein the melt mass flow rate of the acrylic block copolymer B at 190°C under a load of 2160 g, as measured in accordance with JIS K7210:1999, is 0.01 g / 10 min to 100 g / 10 min. <6> The resin composition for modifying ink according to any one of <1> to <5>, wherein the hardness of the acrylic block copolymer B, as measured in accordance with ISO 7619-1 (Type A), is 5 to 150. <7> The ink modifying resin composition according to any one of <1> to <6>, wherein the acrylic block copolymer B comprises at least one selected from the group consisting of copolymer 1 comprising a block chain consisting of structural units derived from methyl methacrylate and a block chain consisting of structural units derived from n-butyl acrylate, and copolymer 2 comprising a block chain consisting of structural units derived from methyl methacrylate, a block chain consisting of structural units derived from n-butyl acrylate, and a block chain consisting of structural units derived from 2-ethylhexyl acrylate. <8> The ink modifying resin composition according to any one of <1> to <7>, wherein the acrylic block copolymer B has not been subjected to an antiblocking treatment.<9> The ink modifying resin composition according to any one of <1> to <8>, wherein the solubility parameter of the acrylic block copolymer B is 8.5 or more. <10> The ink modifying resin composition according to any one of <1> to <9>, wherein the melt mass flow rate of the ink modifying resin composition measured in accordance with JIS K7210:1999 at 190°C under a load of 2160 g is 0.1 g / 10 min to 800 g / 10 min. <11> The ink modifying resin composition according to any one of <1> to <10>, wherein the content of structural units derived from vinyl acetate contained in the ink modifying resin composition is 10% by mass to 48% by mass. <12> The ink modifying resin composition according to any one of <1> to <11>, wherein when a mixture prepared by adding 20 parts by mass of the ink modifying resin composition to 80 parts by mass of a 1:1 (mass ratio) mixed solution of normal propyl acetate and ethyl acetate is shaken at 30°C and 85 rpm (revolutions per minute), the time until the ink modifying resin composition is completely dissolved in the mixed solution is less than 12 hours. <13> The ink modifying resin composition according to any one of <1> to <12>, wherein a mixture prepared by adding 20 parts by mass of the ink modifying resin composition to 80 parts by mass of a 1:1 (mass ratio) mixed solution of normal propyl acetate and ethyl acetate is shaken at 30°C and 85 rpm until the ink modifying resin composition is completely dissolved in the mixed solution, and then the mixture is allowed to stand at 23°C for 24 hours. The solution viscosity measured using a B-type viscometer shown below is 1 mPa s to 8000 mPa s. Device name: BROOKFIELD DIGITAL VISCOMETER Device manufacturer: Brookfield Engineering Laboratories, Inc. Model: RVTDV-II Measurement temperature: 23°C <14> A gravure ink modifier comprising the ink modifying resin composition according to any one of <1> to <13>. <15> A gravure ink comprising the ink modifying resin composition according to any one of <1> to <13>.

[0007] According to the present disclosure, it is possible to provide a resin composition for modifying ink and a gravure ink that have excellent flowability when dissolved in an ester-based solvent.

[0008] In this disclosure, a numerical range indicated using "to" indicates a range that includes the numerical values ​​before and after "to" as the minimum and maximum values, respectively. In this disclosure, when multiple substances corresponding to each component are present, the amount of each component refers to the total amount of the multiple substances unless otherwise specified. In the numerical ranges described in stages in this disclosure, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in stages, or may be replaced with a value shown in an example.

[0009] [Ink modifying resin composition] The ink modifying resin composition of the present disclosure comprises an ethylene-vinyl ester copolymer A and an acrylic block copolymer B, and the total content of the ethylene-vinyl ester copolymer A and the acrylic block copolymer B is more than 70 mass % and not more than 100 mass % based on the total mass of the ink modifying resin composition.

[0010] An ink modifying resin composition containing ethylene-vinyl ester copolymer A and acrylic block copolymer B has excellent fluidity when dissolved in an ester solvent compared to when ethylene-vinyl ester copolymer A is used alone.

[0011] Furthermore, as a method for increasing the solubility of ethylene-vinyl ester copolymer A (particularly ethylene-vinyl acetate copolymer) in ester solvents, there is a method for increasing the content of structural units derived from vinyl esters (particularly vinyl acetate) in ethylene-vinyl ester copolymer A. However, when the content of structural units derived from vinyl esters (particularly vinyl acetate) is increased, the tackiness of ethylene-vinyl ester copolymer A (particularly ethylene-vinyl acetate copolymer) also increases, which causes a problem of increased susceptibility to blocking.

[0012] The ink modifying resin composition of the present disclosure uses an acrylic block copolymer B, so that solubility in ester-based solvents can be favorably ensured even when the content of structural units derived from vinyl esters (particularly vinyl acetate) is reduced. Therefore, the ink modifying resin composition of the present disclosure easily achieves both solubility in ester-based solvents and blocking suppression. Furthermore, the amount of inorganic fillers, anti-blocking agents such as particulate polymers used to suppress blocking can be reduced, so that when the ink modifying resin composition is dissolved in an ester-based solvent, the decrease in transparency of the ink modifying resin composition can be suppressed.

[0013] In the ink modifying resin composition of the present disclosure, the total content of the ethylene-vinyl ester copolymer A and the acrylic block copolymer B is more than 70% by mass and 100% by mass or less, preferably 80% by mass to 100% by mass, and more preferably 90% by mass to 100% by mass, based on the total mass of the ink modifying resin composition.

[0014] (Ethylene-vinyl ester copolymer A) The resin composition for modifying ink of the present disclosure contains ethylene-vinyl ester copolymer A. The ethylene-vinyl ester copolymer A is a polymer obtained by copolymerizing ethylene and a vinyl ester, and is not particularly limited as long as it is a polymer containing structural units derived from ethylene and structural units derived from a vinyl ester. The ethylene-vinyl ester copolymer A may be a random copolymer, a block copolymer, or an alternating copolymer.

[0015] Examples of the ethylene-vinyl ester copolymer A include ethylene-vinyl acetate copolymer, ethylene-vinyl propionate copolymer, ethylene-vinyl butyrate copolymer, ethylene-vinyl stearate copolymer, etc. The ethylene-vinyl ester copolymer A may be used alone or in combination of two or more.

[0016] From the viewpoint of solubility in an ester solvent, the content of the structural units derived from ethylene is preferably 30% by mass to 95% by mass, more preferably 40% by mass to 94% by mass, more preferably 46% by mass to 84% by mass, more preferably 48% by mass to 80% by mass, more preferably 52% by mass to 72% by mass, more preferably 54% by mass to 68% by mass, and more preferably 56% by mass to 60% by mass, relative to the total mass of the ethylene-vinyl ester copolymer A.

[0017] From the viewpoint of solubility in an ester solvent, the content of structural units derived from vinyl ester (preferably the content of structural units derived from vinyl acetate) is preferably 5% by mass to 70% by mass, more preferably 6% by mass to 60% by mass, more preferably 14% by mass to 54% by mass, more preferably 20% by mass to 52% by mass, more preferably 28% by mass to 48% by mass, more preferably 32% by mass to 46% by mass, and more preferably 40% by mass to 44% by mass, relative to the total mass of ethylene-vinyl ester copolymer A.

[0018] The ethylene-vinyl ester copolymer A may be a copolymer consisting only of structural units derived from ethylene and structural units derived from vinyl ester, or may further contain structural units derived from other monomers other than ethylene and vinyl ester.

[0019] Examples of other monomers besides ethylene and vinyl esters include unsaturated hydrocarbons such as propylene, butene, 1,3-butadiene, pentene, 1,3-pentadiene, and 1-hexene; oxides such as vinyl sulfate and vinyl nitrate; halogen compounds such as vinyl chloride and vinyl fluoride; vinyl group-containing primary and secondary amine compounds; carbon monoxide; and sulfur dioxide.

[0020] The content of structural units derived from monomers other than ethylene and vinyl ester that can be contained in the ethylene-vinyl ester copolymer A may be 0% by mass to 10% by mass, or 0% by mass to 5% by mass, relative to the total mass of the ethylene-vinyl ester copolymer A.

[0021] The method for producing the ethylene-vinyl ester copolymer A is not particularly limited, and it can be produced by a known method. For example, it can be obtained by radical copolymerization of each polymerization component under high temperature and high pressure. It can be produced by either an autoclave method or a tubular method. Furthermore, commercially available ethylene-vinyl ester copolymer A may be used.

[0022] The melt mass flow rate (MFR) of the ethylene-vinyl ester copolymer A measured in accordance with JIS K7210:1999 at 190°C under a load of 2160 g is preferably 0.1 g / 10 min to 800 g / 10 min, more preferably 1 g / 10 min to 300 g / 10 min, more preferably 10 g / 10 min to 200 g / 10 min, more preferably 30 g / 10 min to 150 g / 10 min, more preferably 50 g / 10 min to 100 g / 10 min, and even more preferably 70 g / 10 min to 90 g / 10 min.

[0023] The content of ethylene-vinyl ester copolymer A contained in the ink modifying resin composition is preferably 10% by mass to 90% by mass, more preferably 15% by mass to 85% by mass, and even more preferably 20% by mass to 80% by mass, based on the total mass of the resin components contained in the ink modifying resin composition.

[0024] The ethylene-vinyl ester copolymer A preferably contains an ethylene-vinyl acetate copolymer. In this case, the content of the ethylene-vinyl acetate copolymer may be 50% by mass to 100% by mass, 70% by mass to 100% by mass, or 90% by mass to 100% by mass, based on the total mass of the ethylene-vinyl ester copolymer A.

[0025] (Acrylic Block Copolymer B) The resin composition for modifying ink of the present disclosure contains an acrylic block copolymer B. The acrylic block copolymer B is a block copolymer having a polymer block that is a soft segment and a polymer block that is a hard segment. The acrylic block copolymer B may be used alone or in combination of two or more types.

[0026] The acrylic block copolymer B contains an acrylic monomer (a monomer having an acryloyl group or a methacryloyl group) as a monomer component constituting at least one polymer block of the soft segment and the hard segment.

[0027] The acrylic monomer constituting the soft segment is preferably an acrylic ester. That is, the polymer block of the soft segment is preferably an acrylic ester polymer block (b1). Examples of the acrylic ester include acrylic esters having a hydrocarbon group that may have an alkoxy group (particularly, an alkyl acrylate ester that may have an alkoxy group), such as methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, n-pentyl acrylate, isopentyl acrylate, n-hexyl acrylate, cyclohexyl acrylate, 2-ethylhexyl acrylate, pentadecyl acrylate, dodecyl acrylate, isobornyl acrylate, phenyl acrylate, benzyl acrylate, phenoxyethyl acrylate, and 2-methoxyethyl acrylate. The hydrocarbon group in the acrylic ester may be an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, an aromatic hydrocarbon group, or a group in which two or more of these are bonded. The acrylic monomers may be used alone or in combination.

[0028] As the acrylic monomer constituting the acrylic ester polymer block (b1), from the viewpoint of achieving better fluidity and impact resistance of molded articles, preferred are acrylic esters having a hydrocarbon group with 1 to 22 carbon atoms (preferably 1 to 10, more preferably 1 to 4 carbon atoms). From the same viewpoint, the hydrocarbon group in the acrylic ester is preferably an aliphatic hydrocarbon. Therefore, the acrylic ester is particularly preferably an alkyl acrylate, more preferably n-butyl acrylate and 2-ethylhexyl acrylate, and even more preferably n-butyl acrylate.

[0029] The acrylic monomer constituting the acrylic ester polymer block (b1) may include an acrylic monomer other than the acrylic ester having a hydrocarbon group optionally containing an alkoxy group. Examples of the other acrylic monomer include acrylic esters having a crosslinkable functional group, such as 2-hydroxyethyl acrylate, glycidyl acrylate, and allyl acrylate; methacrylic esters constituting hard segments; and carboxyl group-containing monomers, such as methacrylic acid and acrylic acid. Furthermore, the monomer component constituting the soft segment may further include other monomers, such as aromatic vinyl compounds; vinyl cyanide monomers, such as acrylonitrile and methacrylonitrile; and olefins. The proportion of the acrylic ester having a hydrocarbon group optionally containing an alkoxy group in the acrylic ester polymer block (b1) is preferably 90% by mass or more, more preferably 95% by mass or more, based on the total mass of the monomer components constituting the acrylic ester polymer block (b1). The upper limit of the aforementioned proportion is not particularly limited, as long as it is 100% by mass or less.

[0030] The glass transition temperature of the acrylic acid ester polymer block (b1) is not particularly limited, but is preferably from -100°C to 20°C, more preferably from -80°C to 0°C, and even more preferably from -60°C to -40°C.

[0031] The acrylic monomer constituting the hard segment is preferably a methacrylic acid ester. That is, the polymer block that constitutes the hard segment is preferably a methacrylic acid ester polymer block (b2). Examples of the methacrylic acid ester include methacrylic acid esters having a hydrocarbon group that may have an alkoxy group (particularly, alkyl methacrylates that may have an alkoxy group), such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, n-pentyl methacrylate, isopentyl methacrylate, n-hexyl methacrylate, cyclohexyl methacrylate, 2-ethylhexyl methacrylate, pentadecyl methacrylate, dodecyl methacrylate, isobornyl methacrylate, phenyl methacrylate, benzyl methacrylate, phenoxyethyl methacrylate, and 2-methoxyethyl methacrylate. The hydrocarbon group in the methacrylic acid ester may be any of an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, an aromatic hydrocarbon group, and a group in which two or more of these are bonded. The acrylic monomers may be used alone or in combination of two or more.

[0032] As the acrylic monomer constituting the methacrylic acid ester polymer block (b2), from the viewpoint of obtaining a molded article with better impact resistance and heat resistance, a methacrylic acid ester having a hydrocarbon group with 1 to 22 carbon atoms (preferably 1 to 10, more preferably 1 to 4 carbon atoms) is preferred. From the same viewpoint, the hydrocarbon group in the methacrylic acid ester is preferably an aliphatic hydrocarbon. Therefore, as the methacrylic acid ester, an alkyl methacrylate is preferred, and methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, tert-butyl methacrylate, 2-ethylhexyl methacrylate, cyclohexyl methacrylate, and isobornyl methacrylate are more preferred, with methyl methacrylate being particularly preferred.

[0033] The acrylic monomer constituting the methacrylic acid ester polymer block (b2) may include an acrylic monomer other than the methacrylic acid ester having a hydrocarbon group optionally containing an alkoxy group. Examples of the other acrylic monomer include methacrylic acid esters having a crosslinkable functional group, such as 2-hydroxyethyl methacrylate, glycidyl methacrylate, and allyl methacrylate; acrylic acid esters constituting soft segments; and carboxyl group-containing monomers, such as methacrylic acid and acrylic acid. The monomer components constituting the methacrylic acid ester polymer block (b2) may further include other monomers, such as aromatic vinyl compounds; vinyl cyanide monomers, such as acrylonitrile and methacrylonitrile; and olefins. The proportion of the methacrylic acid ester having a hydrocarbon group optionally containing an alkoxy group in the methacrylic acid ester polymer block (b2) is preferably 90% by mass or more, more preferably 95% by mass or more, based on the total mass of the monomer components constituting the methacrylic acid ester polymer block (b2). The upper limit of the aforementioned proportion is not particularly limited, as long as it is 100% by mass or less.

[0034] The acrylic block copolymer B preferably contains at least one selected from the group consisting of copolymer 1 containing a block chain made of structural units derived from methyl methacrylate and a block chain made of structural units derived from n-butyl acrylate, and copolymer 2 containing a block chain made of structural units derived from methyl methacrylate, a block chain made of structural units derived from n-butyl acrylate, and a block chain made of structural units derived from 2-ethylhexyl acrylate, and more preferably contains copolymer 1 containing a block chain made of structural units derived from methyl methacrylate and a block chain made of structural units derived from n-butyl acrylate.

[0035] The glass transition temperature of the methacrylic acid ester polymer block (b2) is not particularly limited, but is preferably 30°C to 180°C, more preferably 60°C to 160°C, and even more preferably 100°C to 120°C.

[0036] The acrylic block copolymer B may have another polymer block (b3) other than the acrylic acid ester polymer block (b1) and the methacrylic acid ester polymer block (b2). The other polymer block is composed of a monomer component other than an acrylic acid ester and a methacrylic acid ester. Examples of monomers constituting the other polymer block include α-olefins such as ethylene, propylene, 1-butene, isobutylene, and 1-octene; conjugated dienes such as butadiene, isoprene, and myrcene; aromatic vinyl monomers such as styrene, α-methylstyrene, p-methylstyrene, and m-methylstyrene; vinyl acetate, vinylpyridine, acrylonitrile, methacrylonitrile, vinyl ketone, vinyl chloride, vinylidene chloride, vinylidene fluoride, acrylamide, methacrylamide, ε-caprolactone, and valerolactone.

[0037] The bonding form of each polymer block constituting the acrylic block copolymer B is not particularly limited, and examples thereof include linear, branched, and radial. Examples of the bonding form include linear structures such as the {(b1)-(b2)}n structure, the {(b1)-(b2)}n-(b1) structure, the (b2)-{(b1)-(b2)}n structure, the (b2)-{(b1)-(b2)}n-(b3) structure, and the (b3)-(b2)-{(b1)-(b2)}n-(b3) structure; and the {(b1)-(b2)}nZ structure (where n is a natural number and Z represents a coupling agent residue). From the viewpoint of achieving better dispersibility of the ethylene-vinyl ester copolymer A in the ink modifying resin composition, a linear structure is preferred, and it is more preferable to use a triblock copolymer in which the methacrylic acid ester polymer block (b2) is bonded to both ends of the acrylic acid ester polymer block (b1).

[0038] The weight-average molecular weight of the acrylic block copolymer B is preferably 10,000 to 200,000, and more preferably 15,000 to 150,000. When the weight-average molecular weight of the acrylic block copolymer B is 10,000 or more, the melt viscosity is appropriate and the melt-kneadability with the ethylene-vinyl ester copolymer A is good. When the weight-average molecular weight is 200,000 or less, an increase in melt viscosity can be suppressed. The weight-average molecular weight of each of the acrylic acid ester polymer block (b1) and the methacrylic acid polymer block (b2) in the acrylic block copolymer B is preferably 2,000 to 100,000, and more preferably 5,000 to 80,000.

[0039] The total content of the acrylic acid ester polymer blocks (b1) in the acrylic block copolymer B is preferably 35% by mass to 95% by mass, more preferably 40% by mass to 95% by mass, and even more preferably 45% by mass to 90% by mass, relative to the total mass of the acrylic block copolymer B. When the content is 35% by mass or more, the fluidity is improved. When the content is 95% by mass or less, the ink modifying resin composition is less likely to stick. From the same viewpoint, the total content of the methacrylic acid ester polymer blocks (b2) in the acrylic block copolymer B is preferably 5% by mass to 65% by mass, more preferably 5% by mass to 60% by mass, and even more preferably 10% by mass to 55% by mass, relative to the total mass of the acrylic block copolymer B.

[0040] The total content of the acrylic acid ester polymer block (b1) and the methacrylic acid ester polymer block (b2) in the acrylic block copolymer B is preferably 60% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more, based on the total mass of the acrylic block copolymer B. The upper limit of the aforementioned proportion is not particularly limited, as long as it is 100% by mass or less.

[0041] The molecular weight distribution (weight average molecular weight (Mw) / number average molecular weight (Mn)) of the acrylic block copolymer B is preferably 1.01 or more and less than 1.50, more preferably 1.01 to 1.35, and even more preferably 1.01 to 1.20.

[0042] The hardness of the acrylic block copolymer B measured in accordance with ISO 7619-1 (Type A) is preferably 5 to 150, more preferably 10 to 120, and even more preferably 60 to 100.

[0043] The melt mass flow rate (MFR) of the acrylic block copolymer B measured in accordance with JIS K7210:1999 at 190°C under a load of 2160 g is preferably 0.01 g / 10 min to 100 g / 10 min, more preferably 0.1 g / 10 min to 60 g / 10 min, still more preferably 1 g / 10 min to 50 g / 10 min, and even more preferably 1 g / 10 min to 30 g / 10 min.

[0044] The content of the acrylic block copolymer B contained in the ink modifying resin composition is preferably 10% by mass to 90% by mass, more preferably 15% by mass to 85% by mass, and more preferably 20% by mass to 80% by mass, based on the total mass of the resin components contained in the ink modifying resin composition.

[0045] The acrylic block copolymer B may have a functional group such as a hydroxyl group, a carboxyl group, an acid anhydride group, or an amino group in the molecular chain or at the molecular chain terminal, if necessary.

[0046] The acrylic block copolymer B may or may not be subjected to an anti-blocking treatment. From the viewpoint of the transparency of the ink modifying resin composition when the ink modifying resin composition is dissolved in an ester solvent, it is preferable that the acrylic block copolymer B is not subjected to an anti-blocking treatment.

[0047] The solubility parameter of the acrylic block copolymer B is preferably 8.5 or more, more preferably 9.0 or more. The upper limit of the solubility parameter of the acrylic block copolymer B is not particularly limited, and may be, for example, 15.0 or less, or 12.0 or less.

[0048] A commercially available product may be used as the acrylic block copolymer B. Examples of commercially available acrylic block copolymer B include Kuraly LA2140, LA2330, LA3320, LA2250, LA2270, LA4285, and LA1892 manufactured by Kuraray Co., Ltd. One of these commercially available products may be used alone, or two or more of them may be used in combination.

[0049] (Shape of ink modifying resin composition) The shape of the ink modifying resin composition of the present disclosure is not particularly limited. From the viewpoints of ease of removal from a storage location, ease of supply to a molding device, etc., ease of transportation, ease of measurement, etc., the ink modifying resin composition is preferably in the form of pellets.

[0050] The melt mass flow rate of the ink modifying resin composition measured in accordance with JIS K7210:1999 at 190 ° C. and a load of 2160 g is preferably 0.1 g / 10 min to 800 g / 10 min, more preferably 0.5 g / 10 min to 300 g / 10 min, more preferably 1 g / 10 min to 100 g / 10 min, and even more preferably 2 g / 10 min to 80 g / 10 min.

[0051] The content of vinyl acetate-derived structural units contained in the ink modifying resin composition of the present disclosure may be 10% by mass to 48% by mass, or 10% by mass to 40% by mass.

[0052] In the ink modifying resin composition of the present disclosure, when 20 parts by mass of the ink modifying resin composition is added to 80 parts by mass of a 1:1 (mass ratio) mixed solution of normal propyl acetate and ethyl acetate, and the mixture is shaken at 30°C and 85 rpm, it is preferable that the time until the ink modifying resin composition is completely dissolved in the mixed solution (complete dissolution time) is less than 12 hours. The complete dissolution time may be less than 10 hours or less than 6 hours.

[0053] In the ink modifying resin composition of the present disclosure, a mixture prepared by adding 20 parts by mass of the ink modifying resin composition to 80 parts by mass of a 1:1 (mass ratio) mixed solution of normal propyl acetate and ethyl acetate is shaken at 30 ° C. and 85 rpm until the ink modifying resin composition is completely dissolved in the mixed solution. After leaving to stand at 23 ° C. for 24 hours, the solution viscosity measured using a B-type viscometer shown below is preferably less than 8500 mPa s, more preferably 8000 mPa s or less, more preferably 4000 mPa s or less, more preferably less than 2000 mPa s, more preferably 1500 mPa s or less, even more preferably 1200 mPa s or less, and particularly preferably 1000 mPa s or less. The lower limit of the solution viscosity is not particularly limited, and may be, for example, 1 mPa·s or more, 5 mPa·s or more, 10 mPa·s or more, or 30 mPa·s or more. Device name: BROOKFIELD DIGITAL VISCOMETER Device manufacturer: Brookfield Engineering Laboratories, Inc. Model: RVTDV-II Measurement temperature: 23°C

[0054] (Other Components) The resin composition for modifying ink of the present disclosure may contain other components as needed. Examples of other components include liquid coating agents, powder coating agents such as inorganic fillers, pigments, dyes, antioxidants, lubricants, weathering agents, anti-blocking agents other than the powder coating agents described above, heat stabilizers, UV stabilizers, flame retardants, and flame retardant assistants.

[0055] The use of the ink modifying resin composition of the present disclosure is not particularly limited, and it can be used, for example, as a gravure ink modifier. The gravure ink modifier is not particularly limited as long as it is prepared using the ink modifying resin composition described above. The gravure ink modifier may, for example, include an ink modifying resin composition containing an ethylene-vinyl ester copolymer A, an acrylic block copolymer B, and, as necessary, other components.

[0056] [Gravure Ink] The gravure ink of the present disclosure includes the aforementioned resin composition for modifying ink of the present disclosure. The gravure ink may contain components contained in general gravure inks other than the aforementioned resin composition for modifying ink of the present disclosure, for example, resin components other than the resin composition for modifying ink, solvents, colorants, other components, etc.

[0057] Examples of the solvent include aliphatic cyclic hydrocarbon solvents, ketone solvents, ester solvents, alcohol solvents, glycol ether solvents, etc. One solvent may be used alone, or two or more solvents may be used in combination. The solvent preferably includes an ester solvent, and examples of the ester solvent include methyl acetate, ethyl acetate, normal propyl acetate, isopropyl acetate, and butyl acetate.

[0058] Examples of colorants include pigments and dyes.

[0059] Other components include antioxidants, lubricants, weathering agents, antiblocking agents, heat stabilizers, ultraviolet stabilizers, flame retardants, flame retardant assistants, dispersants, antistatic agents, plasticizers, olefin waxes, surfactants, etc.

[0060] Examples of the present disclosure will be described below, but the present disclosure is not limited to the following examples.

[0061] In the examples and comparative examples, the following ethylene-vinyl ester copolymer A and acrylic block copolymer B were used. <Ethylene-Vinyl Ester Copolymer A> A-1: ​​EVA (content of structural units derived from vinyl acetate: 42% by mass; MFR: 80 g / 10 min at 190°C under a load of 2160 g, measured in accordance with JIS K7210:1999) <Acrylic Block Copolymer B> B-1: KURARITY LA4285 (block copolymer of a block chain (MMA chain) composed of structural units derived from methyl methacrylate (MMA) and a block chain (nBA chain) composed of structural units derived from n-butyl acrylate (nBA); MMA chain content: 50% by mass; nBA chain content: 50% by mass; MFR: 1.5 g / 10 min at 190°C under a load of 2160 g, measured in accordance with JIS K7210:1999, measured at 190°C under a load of 2160 g, measured at 95, hardness: 95, measured in accordance with ISO 7619-1 (Type A); no anti-blocking treatment, manufactured by Kuraray Co., Ltd.) B-2: Kurariti LA2250 (block copolymer of MMA chains and nBA chains, MMA chain content = 30 mass%, nBA chain content = 70 mass%, MFR = 25 g / 10 min at 190 ° C under a load of 2160 g as measured in accordance with JIS K7210:1999, hardness = 65 as measured in accordance with ISO 7619-1 (Type A), anti-blocking treated, manufactured by Kuraray Co., Ltd.) B-3: Kurariti LA3320 (block copolymer of MMA chains and nBA chains, MMA chain content = 15 mass%, nBA chain content = 85 mass%, MFR = 6.2 g / 10 min at 190 ° C under a load of 2160 g as measured in accordance with JIS K7210:1999, Hardness measured in accordance with JIS No. 7619-1 (Type A) = 13, anti-blocking treated, manufactured by Kuraray Co., Ltd.

[0062] [Examples 1 to 7 and Comparative Example 1] <Preparation of ink modifying resin composition P> The materials were pre-mixed in the blending ratios shown in Table 1, and then charged into a twin-screw extruder with a screw diameter of 30 mm, melt-kneaded, and granulated to prepare pellets of ink modifying resin composition P. Blanks in Table 1 indicate that the material was not blended.

[0063] The content of vinyl acetate-derived structural units in the ink modifying resin composition P prepared above was calculated from the content of vinyl acetate-derived structural units in the ethylene-vinyl ester copolymer A used as a raw material, and the content of ethylene-vinyl ester copolymer A when the entire ink modifying resin composition P was taken as 100% by mass. The MFR of the ink modifying resin composition P prepared above at 190°C and a load of 2160 g was measured in accordance with JIS K 7210:1999. The results are shown in Table 1.

[0064] <Solvent Solubility> 20 g of pellets of the ink modifying resin composition P were added to 80 g of a 1:1 (mass ratio) mixed solution of normal propyl acetate and ethyl acetate to prepare a mixture. The mixture was shaken at 30°C and 85 rpm using an incubator (EYELA Tokyo Rikakikai Co., Ltd., UNI THERMO SHAKER NTS-3000), and the time until the pellets of the ink modifying resin composition P were completely dissolved was measured. The solvent solubility of the pellets of the ink modifying resin composition P was evaluated based on the transparency, hue, presence of suspended matter, and presence of precipitate after complete dissolution, and was evaluated according to the following criteria. The results are shown in Table 1. -Transparency Evaluation Criteria- A: The mixture after shaking was transparent. B: The mixture after shaking was translucent. Translucent and nearly uniform. -Hue Evaluation Criteria- A: The mixture after shaking was colorless. B: The mixture after shaking was not colorless. - Evaluation criteria for floating matter - A: Floating matter was observed in the mixture after shaking. B: No floating matter was observed in the mixture after shaking. - Evaluation criteria for sediment - A: Sediment was observed in the mixture after shaking. B: No sediment was observed in the mixture after shaking.

[0065] <Flowability> 20 g of pellets of the ink modifying resin composition P produced were added to 80 g of a 1:1 (mass ratio) mixed solution of normal propyl acetate and ethyl acetate to prepare a mixture. The mixture was dissolved by shaking at 30°C and 85 rpm using an incubator (EYELA Tokyo Rikakikai Co., Ltd., UNI THERMO SHAKER NTS-3000). After allowing to stand at 23°C for 24 hours, the solution viscosity was measured using the following Brookfield Digital Viscometer. The results are shown in Table 1. Device name: BROOKFIELD DIGITAL VISCOMETER Device manufacturer: Brookfield Engineering Laboratories, Inc. Model: RVTDV-II Measurement temperature: 23°C Flowability was evaluated according to the following criteria. -Evaluation criteria- A: Less than 2000 mPa·s B: 2000 mPa·s or more and less than 8500 mPa·s C: 8500 mPa·s or more

[0066]

[0067] As is clear from Table 1, the ink modifying resin compositions P of Examples 1 to 3 were good in transparency, hue, presence or absence of suspended matter, presence or absence of sediment, and fluidity. The ink modifying resin compositions P of Examples 4 to 7 were good in hue, presence or absence of suspended matter, presence or absence of sediment, and fluidity, but were translucent. On the other hand, Comparative Example 1 was good in transparency, hue, presence or absence of suspended matter, and presence or absence of sediment, but had poor fluidity.

[0068] The disclosure of Japanese Patent Application No. 2023-087987, filed on May 29, 2023, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.

Claims

1. An ink modifying resin composition comprising an ethylene-vinyl ester copolymer A and an acrylic block copolymer B, wherein the total content of the ethylene-vinyl ester copolymer A and the acrylic block copolymer B is more than 70 mass% and not more than 100 mass% based on the total mass of the ink modifying resin composition.

2. The resin composition for modifying ink according to claim 1, wherein the ethylene-vinyl ester copolymer A comprises an ethylene-vinyl acetate copolymer.

3. A resin composition for modifying ink according to claim 2, wherein the content of constituent units derived from vinyl acetate contained in the ethylene-vinyl acetate copolymer is 28% by mass to 48% by mass relative to the total mass of the ethylene-vinyl acetate copolymer.

4. The resin composition for modifying ink according to claim 1, wherein the melt mass flow rate of the ethylene-vinyl ester copolymer A measured in accordance with JIS K7210:1999 at 190°C under a load of 2160 g is 0.1 g / 10 min to 800 g / 10 min.

5. The resin composition for modifying ink according to claim 1, wherein the melt mass flow rate of the acrylic block copolymer B measured in accordance with JIS K7210:1999 at 190°C under a load of 2160 g is 0.01 g / 10 min to 100 g / 10 min.

6. A resin composition for modifying ink according to claim 1, wherein the hardness of the acrylic block copolymer B measured in accordance with ISO 7619-1 (Type A) is 5 to 150.

7. The ink modifying resin composition according to claim 1, wherein the acrylic block copolymer B comprises at least one selected from the group consisting of copolymer 1 comprising a block chain consisting of structural units derived from methyl methacrylate and a block chain consisting of structural units derived from n-butyl acrylate, and copolymer 2 comprising a block chain consisting of structural units derived from methyl methacrylate, a block chain consisting of structural units derived from n-butyl acrylate, and a block chain consisting of structural units derived from 2-ethylhexyl acrylate.

8. The resin composition for modifying ink according to claim 1, wherein the acrylic block copolymer B has not been subjected to an anti-blocking treatment.

9. The resin composition for modifying ink according to claim 1, wherein the solubility parameter of the acrylic block copolymer B is 8.5 or more.

10. The ink modifying resin composition according to claim 1, wherein the melt mass flow rate of the ink modifying resin composition measured in accordance with JIS K7210:1999 at 190°C and a load of 2160 g is 0.1 g / 10 min to 800 g / 10 min.

11. A resin composition for modifying ink according to claim 1, wherein the content of structural units derived from vinyl acetate contained in the resin composition for modifying ink is 10% by mass to 48% by mass.

12. A resin composition for modifying ink as described in claim 1, wherein when a mixture prepared by adding 20 parts by mass of the resin composition for modifying ink to 80 parts by mass of a 1:1 (mass ratio) mixed solution of normal propyl acetate and ethyl acetate is shaken under conditions of 30°C and 85 rpm, the time it takes for the resin composition for modifying ink to completely dissolve in the mixed solution is less than 12 hours.

13. The ink modifying resin composition according to claim 1, wherein a mixture prepared by adding 20 parts by mass of the ink modifying resin composition to 80 parts by mass of a 1:1 (mass ratio) mixed solution of normal propyl acetate and ethyl acetate is shaken at 30°C and 85 rpm until the ink modifying resin composition is completely dissolved in the mixed solution, and then the mixture is allowed to stand at 23°C for 24 hours, and the solution viscosity measured using a B-type viscometer shown below is 1 mPa·s to 8000 mPa·s. Apparatus name: BROOKFIELD DIGITAL VISCOMETER Apparatus manufacturer: Brookfield Engineering Laboratories, Inc. Model: RVTDV-II Measurement temperature: 23°C 14. A gravure ink modifier comprising the resin composition for modifying ink according to any one of claims 1 to 13.

15. A gravure ink comprising the resin composition for modifying ink according to any one of claims 1 to 13.

Citation Information

Patent Citations

  • JP1973043029A

  • Aqueous dispersion

    JP2002080687A

  • Resin pellet, method for producing resin pellet, and solar cell sealing material

    WO2013172396A1

  • Resin pellet, resin pellet manufacturing method, and gravure ink

    WO2020196044A1

Cited By

  • Resin composition for plating, and plated molded article

    JP2022080834A

  • Resin composition for plating and plated molded product

    JP7733504B2