Resin composition, cured product, laminate, method for producing cured product, method for producing laminate, method for producing semiconductor device, and semiconductor device
The resin composition, featuring a heterocycle-containing polymer precursor and a pyridine/pyridinium salt-generating compound, addresses the challenge of low pattern resolution in semiconductor manufacturing by enhancing solubility and cyclization, resulting in improved adhesion and heat resistance.
Patent Information
- Application Number
- PCT/JP2024/018772
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2024-05-22
- Publication Date
- 2024-12-05
AI Technical Summary
Current resin compositions used in semiconductor manufacturing face challenges in achieving high resolution when forming patterns of cured products, particularly due to limitations in the interaction between heterocycle-containing polymer precursors and exposure processes.
A resin composition incorporating a heterocycle-containing polymer precursor, a compound that generates a pyridine or pyridinium salt structure upon light or heat exposure, and an organometallic complex, along with a polymerization initiator, which enhances pattern resolution through improved solubility and cyclization reactions.
The resin composition achieves improved pattern resolution, adhesion, and heat resistance by altering the absorption spectrum of the compound, inhibiting precursor interactions, and forming coordination bonds, thereby maintaining film thickness and preventing substrate corrosion.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Resin composition, cured product, laminate, method for manufacturing cured product, method for manufacturing laminate, method for manufacturing semiconductor device, and semiconductor device
[0001] The present invention relates to a resin composition, a cured product, a laminate, a method for producing a cured product, a method for producing a laminate, a method for producing a semiconductor device, and a semiconductor device.
[0002] Nowadays, resin materials produced from resin compositions containing resins are being utilized in various fields. For example, heterocycle-containing polymers such as polyimides have excellent heat resistance and insulating properties and are therefore used in a variety of applications. Examples of such applications include, but are not limited to, insulating films, encapsulants, or protective films for semiconductor devices used for packaging. They are also used as base films or coverlays for flexible substrates.
[0003] For example, in the above-mentioned applications, heterocycle-containing polymers such as polyimides are used in the form of resin compositions containing heterocycle-containing polymer precursors such as polyimide precursors. Such resin compositions can be applied to a substrate, for example, by coating to form a photosensitive film, and then, as necessary, by performing exposure, development, heating, etc., to form a cured product on the substrate. The heterocycle-containing polymer precursors such as polyimide precursors are cyclized, for example, by heating, to form heterocycle-containing polymers such as polyimides in the cured product. Since the resin compositions can be applied by known coating methods, for example, they have excellent manufacturing adaptability, such as a high degree of design freedom in the shape, size, application position, etc., of the applied resin composition. In addition to the high performance of heterocycle-containing polymers such as polyimides, the industrial application of the above-mentioned resin compositions is increasingly expected from the viewpoint of such excellent manufacturing adaptability.
[0004] For example, Patent Document 1 describes a heat-resistant negative photoresist composition containing a resin component made of a polyimide precursor having a specific structure and a compound of a specific structure that exhibits basicity upon irradiation with actinic rays. Patent Document 2 describes a photosensitive polyimide resin composition containing a polyimide resin precursor having a specific repeating unit and a weight-average molecular weight of 20,000 to 100,000, a dihydropyridine compound of a specific structure, and a hexaarylbiimidazole compound of a specific structure.
[0005] JP-A No. 06-075376 JP-A No. 08-254831
[0006] When a resin composition containing a heterocycle-containing polymer precursor is exposed to light and developed to produce a pattern of a cured product, there is a demand for an improvement in the resolution of the resulting pattern.
[0007] The present invention aims to provide a resin composition that has excellent resolution when forming a pattern of a cured product, a cured product obtained by curing the resin composition, a laminate including the cured product, a method for producing the cured product, a method for producing the laminate, a method for producing a semiconductor device including the method for producing the cured product, and a semiconductor device including the cured product.
[0008] Representative embodiments of the present invention are described below. <1> A resin composition comprising: a heterocycle-containing polymer precursor; a compound A that generates a compound having at least one of a pyridine structure and a pyridinium salt structure upon the action of light or heat; an organometallic complex; and a polymerization initiator. <2> The resin composition according to <1>, wherein the organometallic complex is a metal complex having one or more π-conjugated moieties containing a nitrogen atom. <3> A resin composition comprising: a heterocycle-containing polymer precursor; a compound A that generates a compound having at least one of a pyridine structure and a pyridinium salt structure upon the action of light or heat; and a polymerization initiator, wherein the content of a Group 4 element in the composition is 0.010 to 5.0 mass% based on the total solids content of the composition. <4> A resin composition comprising: a heterocycle-containing polymer precursor; a compound A that generates a compound having at least one of a pyridine structure and a pyridinium salt structure upon the action of light or heat; a base generator other than the compound A; and a polymerization initiator. <5> The resin composition according to <4>, wherein the content of the base generator is 1 to 1,000 parts by mass relative to 100 parts by mass of the content of the compound A. <6> The resin composition according to any one of <1> to <5>, wherein the compound A includes a compound represented by the following formula (A-1): In formula (A-1), R 1 is a hydrogen atom or any organic group, and R 2 , R 3 , R 4 and R 5 are each independently a hydrogen atom, a halogen atom, or any organic group, and R 6 is a halogen atom or any organic group. 1 is a hydrogen atom, and R 4 and R 5 are each independently —C(═O)O—R 7 , a cyano group or —C(═O)—R 7 and R 7 is a hydrocarbon group which may have a substituent, and R 6 <8> The resin composition according to <6>, wherein R in formula (A-1) is an aromatic group having an electron-withdrawing group as a substituent. 6When the electron-withdrawing group in is a nitro group, R 6 The resin composition according to <7>, wherein the compound A is a heterocycle-containing polymer precursor, and the compound A is a polymerization initiator. In formula (A-2), R 1 is a hydrogen atom or any organic group, and R 2 , R 3 , R 4 , R 5 are each independently a hydrogen atom, a halogen atom, or any organic group, and Ar 1 is an aromatic group having an electron-withdrawing group as a substituent, and when the electron-withdrawing group is a nitro group, Ar 1has only one nitro group. <10> The resin composition according to any one of <1> to <5> and <9>, wherein the content of the compound A is 0.10 to 30 parts by mass relative to 100 parts by mass of the heterocycle-containing polymer precursor. <11> The resin composition according to any one of <1> to <5> and <9>, wherein the heterocycle-containing polymer precursor is a polyimide precursor. <12> The resin composition according to <11>, wherein the cyclization rate of the polyimide precursor is 2 to 70%. <13> The resin composition according to any one of <1> to <5> and <9>, wherein the heterocycle-containing polymer precursor has a weight average molecular weight in terms of polystyrene of less than 20,000. <14> The resin composition according to any one of <1> to <5> and <9>, further comprising a polymerizable compound. <15> The resin composition according to any one of <1> to <5> and <9>, further comprising a urea compound. <16> The resin composition according to any one of <1> to <5> and <9>, further comprising a compound having at least one of a pyridine structure and a pyridinium salt structure. <17> A cured product obtained by curing the resin composition according to any one of <1> to <5> and <9>. <18> The cured product according to <17>, which is a film having a thickness of less than 10 μm. <19> A laminate comprising two or more layers made of the cured product according to <17>, and a metal layer between any two adjacent layers made of the cured product. <20> A method for producing a cured product, comprising a film-forming step of applying the resin composition according to any one of <1> to <5> and <9> onto a substrate to form a film. <21> A method for producing the cured product according to <20>, comprising an exposure step of selectively exposing the film to light and a development step of developing the film with a developer to form a pattern. <22> A method for producing the cured product according to <20>, comprising a heating step of heating the film at 50 to 450°C. <23> A method for producing a laminate, comprising the method for producing the cured product according to <20>. <24> A method for producing a semiconductor device, comprising the method for producing the cured product according to <20>. <25> A semiconductor device, comprising the cured product according to <17>.
[0009] According to the present invention, there are provided a resin composition having excellent resolution when forming a pattern of a cured product, a cured product obtained by curing the resin composition, a laminate including the cured product, a method for producing the cured product, a method for producing the laminate, a method for producing a semiconductor device including the method for producing the cured product, and a semiconductor device including the cured product.
[0010] The following describes the main embodiments of the present invention. However, the present invention is not limited to the explicitly described embodiments. In this specification, a numerical range expressed using the symbol "to" means a range that includes the numerical values before and after "to" as the lower and upper limits, respectively. In this specification, the term "process" refers not only to an independent process but also to a process that cannot be clearly distinguished from other processes as long as the process achieves its intended effect. In the description of a group (atomic group), a notation that does not specify whether it is substituted or unsubstituted encompasses both unsubstituted groups (atomic groups) and substituted groups (atomic groups). For example, the term "alkyl group" encompasses not only unsubstituted alkyl groups (unsubstituted alkyl groups) but also substituted alkyl groups (substituted alkyl groups). In this specification, unless otherwise specified, "exposure" includes not only exposure using light but also exposure using particle beams such as electron beams and ion beams. In addition, examples of light used for exposure include actinic rays or radiation such as the bright line spectrum of a mercury lamp, far ultraviolet light typified by excimer lasers, extreme ultraviolet light (EUV light), X-rays, and electron beams. As used herein, "(meth)acrylate" refers to either or both of "acrylate" and "methacrylate," "(meth)acrylic" refers to either or both of "acrylic" and "methacrylic," and "(meth)acryloyl" refers to either or both of "acryloyl" and "methacryloyl." In the structural formulae herein, Me represents a methyl group, Et represents an ethyl group, Bu represents a butyl group, and Ph represents a phenyl group. As used herein, the term "total solid content" refers to the total mass of all components of the composition excluding the solvent. Furthermore, as used herein, the term "solid content concentration" refers to the mass percentage of the components other than the solvent relative to the total mass of the composition. As used herein, the weight average molecular weight (Mw) and number average molecular weight (Mn) are values measured using gel permeation chromatography (GPC) and are defined as polystyrene equivalent values, unless otherwise specified.In this specification, the weight-average molecular weight (Mw) and number-average molecular weight (Mn) can be determined, for example, by using an HLC-8220GPC (manufactured by Tosoh Corporation) and guard columns HZ-L, TSKgel Super HZM-M, TSKgel Super HZ4000, TSKgel Super HZ3000, and TSKgel Super HZ2000 (all manufactured by Tosoh Corporation) connected in series. Unless otherwise specified, these molecular weights are measured using THF (tetrahydrofuran) as the eluent. However, when THF is not suitable as the eluent, for example, due to low solubility, NMP (N-methyl-2-pyrrolidone) can also be used. Furthermore, unless otherwise specified, detection in GPC measurement is assumed to be performed using a UV (ultraviolet) detector at a wavelength of 254 nm. In this specification, when the positional relationship of each layer constituting a laminate is described as "above" or "below," it is sufficient that another layer is above or below the reference layer among the multiple layers being considered. In other words, a third layer or element may be interposed between the reference layer and the other layer, and the reference layer and the other layer do not need to be in contact with each other. Unless otherwise specified, the direction in which layers are stacked on the substrate is referred to as "above." Alternatively, if a resin composition layer is present, the direction from the substrate to the resin composition layer is referred to as "above," and the opposite direction is referred to as "below." Note that such vertical directions are defined for convenience in this specification, and in actual embodiments, the "above" direction in this specification may differ from the vertically upward direction. In this specification, unless otherwise specified, the composition may contain two or more compounds corresponding to each component contained in the composition. Unless otherwise specified, the content of each component in the composition means the total content of all compounds corresponding to that component. In this specification, unless otherwise specified, the temperature is 23° C., the atmospheric pressure is 101,325 Pa (1 atmosphere), and the relative humidity is 50% RH. In this specification, a combination of preferred embodiments is a more preferred embodiment.
[0011] (Resin Composition) A resin composition according to a first aspect of the present invention (hereinafter also simply referred to as the "first resin composition") comprises a heterocycle-containing polymer precursor, compound A that generates a compound having at least one of a pyridine structure and a pyridinium salt structure upon the action of light or heat, an organometallic complex, and a polymerization initiator. A resin composition according to a second aspect of the present invention (hereinafter also simply referred to as the "second resin composition") comprises a heterocycle-containing polymer precursor, compound A that generates a compound having at least one of a pyridine structure and a pyridinium salt structure upon the action of light or heat, and a polymerization initiator, wherein the content of the Group 4 element in the composition is 0.010 to 5.0 mass% based on the total solids content of the composition. A resin composition according to a third aspect of the present invention (hereinafter also simply referred to as the "third resin composition") comprises a heterocycle-containing polymer precursor, compound A that generates a compound having at least one of a pyridine structure and a pyridinium salt structure upon the action of light or heat, a base generator other than compound A, and a polymerization initiator. A resin composition according to a fourth aspect of the present invention (hereinafter also simply referred to as the "fourth resin composition") comprises a heterocycle-containing polymer precursor, a compound A represented by formula (A-2), and a polymerization initiator. Hereinafter, the first resin composition, the second resin composition, the third resin composition, and the fourth resin composition will be collectively referred to simply as the "resin composition." Hereinafter, the compound A contained in the first resin composition will be referred to as the "first compound A," the compound A contained in the second resin composition will be referred to as the "second compound A," the compound A contained in the third resin composition will be referred to as the "third compound A," and the compound A contained in the fourth resin composition will be referred to as the "fourth compound A." Hereinafter, when simply referred to as "compound A," it refers to all of the first compound A, the second compound A, the third compound A, and the fourth compound A.
[0012] The resin composition of the present invention is preferably used to form a photosensitive film that is subjected to exposure and development, and is preferably used to form a film that is subjected to exposure and development using a developer containing an organic solvent. The resin composition of the present invention can be used, for example, to form an insulating film for a semiconductor device, an interlayer insulating film for a redistribution layer, a stress buffer film, etc., and is preferably used to form an interlayer insulating film for a redistribution layer. Furthermore, the resin composition of the present invention is preferably used to form a photosensitive film that is subjected to negative development. In the present invention, negative development refers to development in which non-exposed areas are removed by development in exposure and development, and positive development refers to development in which exposed areas are removed by development. As the exposure method, the developer, and the development method, for example, the exposure method described in the exposure step and the developer and development method described in the development step in the description of the method for producing a cured product described below can be used.
[0013] The resin composition of the present invention has excellent resolution when forming a pattern of the cured product. The mechanism by which this effect is achieved is unknown, but is presumed to be as follows.
[0014] The resin composition according to the first aspect of the present invention comprises a heterocycle-containing polymer precursor, a compound A that generates a compound having at least one of a pyridine structure and a pyridinium salt structure upon the action of light or heat, an organometallic complex, and a polymerization initiator. Compound A undergoes structural change to a compound having at least one of a pyridine structure and a pyridinium salt structure upon the action of light or heat, thereby changing its absorption spectrum. For example, if compound A is a compound that absorbs light at 365 nm, its molar absorption coefficient at 365 nm decreases as it absorbs light and changes to a pyridine form. Therefore, in patterning by exposure using a composition containing a polymerization initiator, the exposure contrast between exposed and unexposed areas is increased, and resolution is thought to be improved. This is presumably because light is absorbed by compound A in the unexposed areas that are exposed by slight leaking light around the exposed areas. Furthermore, in the exposed areas, irradiation with a certain amount of exposure reduces the amount of light absorbed by compound A, thereby sufficiently curing the film and maintaining a high film thickness after development of the patterned area. In addition, compound A forms hydrogen bonds with the heterocycle-containing polymer precursor, thereby inhibiting interactions between the heterocycle-containing polymer precursors, and is therefore thought to improve the solubility in the developer in the unexposed areas. Furthermore, in the composition, the hydrogen bonds between the above-mentioned compound A and the heterocycle-containing polymer precursor are thought to increase the solubility of the heterocycle-containing polymer precursor in the composition. Thus, it can be said that the inclusion of compound A in the resin composition improves the resolution of the patterned portion. Meanwhile, since the compound having at least one of a pyridine structure and a pyridinium salt structure after structural change has basicity, it is thought to promote the cyclization reaction of the cyclized resin precursor, thereby improving the elongation at break. Furthermore, neutralizing the acid component in the cured film is thought to prevent corrosion of the metal substrate and improve adhesion after a heat resistance test. Furthermore, the organometallic complex decomposes during a heating process or the like to form a coordinate bond with the resin in the film, thereby improving the heat resistance and elongation at break of the film. Therefore, adhesion after a heat resistance test can also be improved.Although there is a concern that organometallic complexes may react with basic compounds in the composition and decompose, it is believed that decomposition in the composition can be suppressed when combined with the non-basic Compound A. For this reason, it is presumed that the resolution, adhesion after heat resistance testing, and elongation at break can be improved to high levels while suppressing a decrease in the stability of the composition.
[0015] A resin composition according to a second aspect of the present invention comprises a heterocycle-containing polymer precursor, a compound A that generates a compound having at least one of a pyridine structure and a pyridinium salt structure upon the action of light or heat, and a polymerization initiator, wherein the content of the Group 4 element in the composition is 0.010 to 5.0 mass% based on the total solids content of the composition. In the second aspect, the inclusion of the same compound A as in the first aspect is believed to improve resolution and adhesion after a heat resistance test. Here, atoms belonging to the Group 4 element form coordinate bonds with the resin in the film during a heating process or the like, thereby improving the heat resistance and elongation at break of the film. As a result, adhesion after a heat resistance test is improved.
[0016] A resin composition according to a third aspect of the present invention comprises a heterocycle-containing polymer precursor, compound A that generates a compound having at least one of a pyridine structure and a pyridinium salt structure upon the action of light or heat, a base generator other than compound A, and a polymerization initiator. As described above, the inclusion of compound A improves the resolution of the film in an embodiment in which exposure and development are performed. Further inclusion of another base generator here effectively promotes cyclization of the resin, significantly improving the elongation at break and adhesion after a heat resistance test.
[0017] The resin composition according to the fourth aspect of the present invention contains a compound A represented by formula (A-2) and a polymerization initiator. As described above, the inclusion of compound A improves the resolution of the film in the embodiment in which exposure and development are performed. Here, formula (A-2) in the resin composition according to the fourth aspect further includes Ar 1The fourth aspect excludes an embodiment containing two nitro groups. This suppresses the polymerization inhibiting effect of compound A, making it easier for polymerization by the polymerization initiator to proceed quickly. Therefore, it is believed that the resin composition according to the fourth aspect further improves the resolution of the film in an embodiment in which exposure and development are performed.
[0018] Here, Patent Documents 1 and 2 do not describe the combined use of a first compound A and an organometallic complex in a composition containing a polymerization initiator. Furthermore, Patent Documents 1 and 2 do not describe the inclusion of a second compound A in a composition containing a polymerization initiator, and the content of the Group 4 element in the composition being 0.010 to 5.0 mass% relative to the total solids content of the composition. Furthermore, Patent Documents 1 and 2 do not describe the combined use of a first compound A and a base generator other than the first compound A in a composition containing a polymerization initiator. In addition, Patent Documents 1 and 2 do not describe the use of a fourth compound A in a composition containing a polymerization initiator.
[0019] The components contained in the resin composition of the present invention will be described in detail below.
[0020] <Heterocycle-Containing Polymer Precursor> The resin composition of the present invention contains a heterocycle-containing polymer precursor. The heterocycle-containing polymer precursor refers to a resin that undergoes a change in chemical structure in response to an external stimulus to become a heterocycle-containing polymer. A resin that undergoes a change in chemical structure in response to heat to become a heterocycle-containing polymer is preferred, and a resin that undergoes a ring-closing reaction in response to heat to form a ring structure to become a heterocycle-containing polymer is more preferred. The heterocycle-containing polymer is preferably a resin that contains an imide ring structure or an oxazole ring structure in its main chain structure. In the present invention, the term "main chain" refers to the relatively longest bonding chain in the resin molecule, and the term "side chain" refers to other bonding chains. Examples of heterocycle-containing polymers include polyimide, polybenzoxazole, and polyamideimide. Examples of heterocycle-containing polymer precursors include polyimide precursors, polybenzoxazole precursors, and polyamideimide precursors. That is, the resin composition preferably contains, as the heterocycle-containing polymer precursor, at least one resin selected from the group consisting of polyimide precursors, polybenzoxazole precursors, and polyamideimide precursors. The resin composition preferably contains a polyimide precursor as the heterocycle-containing polymer precursor.
[0021] The heterocycle-containing polymer precursor preferably has a polymerizable group, more preferably a radically polymerizable group. When the heterocycle-containing polymer precursor has a radically polymerizable group, the resin composition of the present invention preferably contains a radical polymerization initiator, more preferably contains a radical polymerization initiator and a radical crosslinking agent. If necessary, it can further contain a sensitizer. From such a resin composition, for example, a negative photosensitive film can be formed.
[0022] [Polyimide Precursor] The polyimide precursor used in the present invention is not particularly limited in type, but preferably contains a repeating unit represented by the following formula (2). In formula (2), A 1 and A 2 are each independently an oxygen atom or —NR z represents -, and R 111 represents a divalent organic group, and R 115represents a tetravalent organic group, R 113 and R 114 each independently represents a hydrogen atom or a monovalent organic group; R z represents a hydrogen atom or a monovalent organic group.
[0023] A in formula (2) 1 and A 2 are each independently an oxygen atom or —NR z -, and an oxygen atom is preferred. z represents a hydrogen atom or a monovalent organic group, and preferably a hydrogen atom. 111 represents a divalent organic group. Examples of the divalent organic group include groups containing a linear or branched aliphatic group, a cyclic aliphatic group, and an aromatic group, and a linear or branched aliphatic group having 2 to 20 carbon atoms, a cyclic aliphatic group having 3 to 20 carbon atoms, an aromatic group having 3 to 20 carbon atoms, or a group consisting of a combination thereof is preferred, and a group containing an aromatic group having 6 to 20 carbon atoms is more preferred. The linear or branched aliphatic group may have a hydrocarbon group in the chain substituted with a group containing a heteroatom, and the cyclic aliphatic group and aromatic group may have a hydrocarbon group in the ring substituted with a group containing a heteroatom. R in formula (2) 111 Examples of the group include groups represented by -Ar- and -Ar-L-Ar-, and the group represented by -Ar-L-Ar- is preferred, where each Ar is independently an aromatic group, L is a single bond, an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a fluorine atom, -O-, -CO-, -S-, or -SO 2 - or -NHCO-, or a group consisting of a combination of two or more of the above. The preferred ranges for these are as described above.
[0024] R 111 is preferably derived from a diamine. Examples of diamines used in the production of the polyimide precursor include linear or branched aliphatic, cyclic aliphatic, or aromatic diamines. Only one type of diamine may be used, or two or more types may be used. Specifically, R 111is preferably a diamine containing a linear or branched aliphatic group having 2 to 20 carbon atoms, a cyclic aliphatic group having 3 to 20 carbon atoms, an aromatic group having 3 to 20 carbon atoms, or a group consisting of a combination thereof, and more preferably a diamine containing an aromatic group having 6 to 20 carbon atoms. The linear or branched aliphatic group may have a hydrocarbon group in the chain substituted with a group containing a heteroatom, and the cyclic aliphatic group and aromatic group may have a hydrocarbon group in the ring substituted with a group containing a heteroatom. Examples of groups containing an aromatic group include the following.
[0025] In the formula, A represents a single bond or a divalent linking group, and is selected from the group consisting of a single bond, an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a fluorine atom, —O—, —C(═O)—, —S—, and —SO 2 -, -NHCO-, or a group selected from a combination thereof, and is preferably a single bond, an alkylene group having 1 to 3 carbon atoms which may be substituted with a fluorine atom, -O-, -C(=O)-, -S-, or -SO 2 - is more preferably a group selected from -CH 2 -, -O-, -S-, -SO 2 -, -C(CF 3 ) 2 - or -C(CH 3 ) 2 In the formula, * represents a bonding site to another structure.
[0026] Specific examples of diamines include 1,2-diaminoethane, 1,2-diaminopropane, 1,3-diaminopropane, 1,4-diaminobutane, and 1,6-diaminohexane; 1,2- or 1,3-diaminocyclopentane, 1,2-, 1,3-, or 1,4-diaminocyclohexane, 1,2-, 1,3-, or 1,4-bis(aminomethyl)cyclohexane, bis-(4-aminocyclohexyl)methane, bis-(3-aminocyclohexyl)methane, 4,4'-diamino-3,3'-dimethylcyclohexylmethane, and isophoronediamine; m- or p-phenylenediamine, diaminotoluene, 4,4'- or 3,3'-diaminobiphenyl, 4,4'-diaminodiphenyl ether, 3,3-diaminodiphenyl ether, 4,4'- or 3,3'-diaminodiphenylmethane, 4,4'- or 3,3'-diaminodiphenyl sulfone, 4,4'- or 3,3'-diaminodiphenyl sulfide, 4,4'- or 3,3'-diaminobenzophenone, 3 ,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dimethoxy-4,4'-diaminobiphenyl, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis(3-hydroxy-4-aminophenyl)propane, 2,2-bis(3-hydroxy-4-aminophenyl)hexafluoropropane parafluoropropane, 2,2-bis(3-amino-4-hydroxyphenyl)propane, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, bis(3-amino-4-hydroxyphenyl)sulfone, bis(4-amino-3-hydroxyphenyl)sulfone, 4,4'-diaminoparaterphenyl, 4,4'-bis(4-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(2-aminophenoxy)phenyl]sulfone, 1,4-bis(4-aminophenoxy)benzene, 9,10-bis(4-aminophenyl)anthracene, 3,3'-dimethyl-4,4'-diaminodiphenylsulfone, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenyl)benzene, 3,3'-diethyl-4,4'-diaminodiphenylmethane, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 4,4'-diaminooctafluorobiphenyl, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 9,9-bis(4-aminophenyl)-10-hydroanthracene, 3,3',4,4'-tetraaminobiphenyl, 3,3',4,4'-tetraaminodiphenyl ether fluorene, 1,4-diaminoanthraquinone, 1,5-diaminoanthraquinone, 3,3-dihydroxy-4,4'-diaminobiphenyl, 9,9'-bis(4-aminophenyl)fluorene, 4,4'-dimethyl-3,3'-diaminodiphenyl sulfone, 3,3',5,5'-tetramethyl-4,4'-diaminodiphenylmethane, 2,4- and 2,5-diaminocumene, 2,5-dimethyl-p-phenylenediamine, acetoguanamine, 2,3,5,6-tetramethyl-p-phenylenediamine, 2,4,6-trimethyl-m-phenylenediamine bis(3-aminopropyl)tetramethyldisiloxane, bis(p-aminophenyl)octamethylpentasiloxane, 2,7-diaminofluorene, 2,5-diaminopyridine, 1,2-bis(4-aminophenyl)ethane, diaminobenzanilide, esters of diaminobenzoic acid, 1,5-diaminonaphthalene, diaminobenzotrifluoride, 1,3-bis(4-aminophenyl)hexafluoropropane, 1,4-bis(4-aminophenyl)octafluorobutane, 1,5-bis(4-aminophenyl)decafluoropentane, 1,7-bis(4-aminophenyl)tetradecafluoroheptane, 2,2-bis[4-(3-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis[4-(2-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)-3,5-dimethylphenyl]hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)-3,5-bis(trifluoromethyl)phenyl]hexafluoropropane, p-bis(4-amino-2-trifluoromethylphenoxy)benzene, 4,At least one diamine selected from 4'-bis(4-amino-2-trifluoromethylphenoxy)biphenyl, 4,4'-bis(4-amino-3-trifluoromethylphenoxy)biphenyl, 4,4'-bis(4-amino-2-trifluoromethylphenoxy)diphenyl sulfone, 4,4'-bis(3-amino-5-trifluoromethylphenoxy)diphenyl sulfone, 2,2-bis[4-(4-amino-3-trifluoromethylphenoxy)phenyl]hexafluoropropane, 3,3',5,5'-tetramethyl-4,4'-diaminobiphenyl, 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl, 2,2',5,5',6,6'-hexafluorotolidine, and 4,4'-diaminoquaterphenyl can be mentioned.
[0027] Also preferred are the diamines (DA-1) to (DA-18) described in paragraphs 0030 to 0031 of WO 2017 / 038598.
[0028] Also preferably used are diamines having two or more alkylene glycol units in the main chain described in paragraphs 0032 to 0034 of WO 2017 / 038598.
[0029] R 111 is preferably represented by -Ar-L-Ar- from the viewpoint of flexibility of the resulting organic film, wherein each Ar is independently an aromatic group, and L is an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a fluorine atom, -O-, -CO-, -S-, or -SO 2 Ar is preferably a phenylene group, and L is preferably an aliphatic hydrocarbon group having 1 or 2 carbon atoms which may be substituted with a fluorine atom, -O-, -CO-, -S-, or -SO 2 The aliphatic hydrocarbon group here is preferably an alkylene group.
[0030] Also, R 111From the viewpoint of i-line transmittance, it is preferable that is a divalent organic group represented by the following formula (51) or formula (61). In particular, from the viewpoint of i-line transmittance and ease of availability, it is more preferable that is a divalent organic group represented by formula (61). Formula (51) In formula (51), R 50 ~R 57 are each independently a hydrogen atom, a fluorine atom, or a monovalent organic group, and R 50 ~R 57 At least one of R is a fluorine atom, a methyl group, or a trifluoromethyl group, and * each independently represents a bonding site with the nitrogen atom in formula (2). 50 ~R 57 Examples of the monovalent organic group include an unsubstituted alkyl group having 1 to 10 carbon atoms (preferably 1 to 6 carbon atoms) and a fluorinated alkyl group having 1 to 10 carbon atoms (preferably 1 to 6 carbon atoms). In formula (61), R 58 and R 59 are each independently a fluorine atom, a methyl group, or a trifluoromethyl group, and * each independently represents a bonding site with the nitrogen atom in formula (2). Examples of diamines that give the structure of formula (51) or formula (61) include 2,2'-dimethylbenzidine, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 2,2'-bis(fluoro)-4,4'-diaminobiphenyl, and 4,4'-diaminooctafluorobiphenyl. These may be used alone or in combination of two or more.
[0031] Also, R 111 is also preferably a group represented by the following formula (71). 111 is more preferably a group represented by the following formula (72). In formula (71), A 1 ~A 3are each independently a single bond or a divalent linking group, * represents a bonding site with the nitrogen atom in formula (2), and the four benzene rings described in formula (71) may each have a hydrogen atom substituted with a substituent. In this specification, a bond crossing a side of a ring structure means that one of the hydrogen atoms in the ring structure is substituted. In formula (72), * represents a bonding site with the nitrogen atom in formula (2).
[0032] In formula (71), A 1 ~A 3 represents an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a fluorine atom, —O—, —C(═O)—, —S—, —S(═O) 2 Preferably, it is -, -NHC(=O)-, or a group consisting of a combination of two or more thereof, more preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a fluorine atom, -O-, -C(=O)-, or a group consisting of a combination of two or more thereof, and even more preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a fluorine atom or -O-. In particular, A 1 and A 3 is preferably —O—. 2 is preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a fluorine atom. 1 and A 3 is —O—, and A 2 -C(CH 3 ) 2 The number of carbon atoms in the aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a fluorine atom is not particularly limited, but is preferably 1 to 6, and more preferably 1 to 4. Specific examples of the aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a fluorine atom include -CH 2 -, -C(CH 3 ) 2 -, -C(CF 3 ) 2 -, among which -C(CH 3 ) 2- is preferred. Examples of the substituents on the four benzene rings described in formula (71) include a fluorine atom and a hydrocarbon group having 1 to 10 carbon atoms in which a hydrogen atom may be substituted with a fluorine atom. An embodiment in which all of the four benzene rings described in formula (71) are unsubstituted is also one of the preferred embodiments of the present invention.
[0033] Also, R 111 is also preferably a group represented by the following formula (81). 111 is more preferably a group represented by the following formula (82). In formula (81), A 1 and A 2 are each independently a single bond or a divalent linking group, * represents a bonding site to the nitrogen atom in formula (2), and in the three benzene rings described in formula (81), each hydrogen atom may be substituted with a substituent. In formula (82), * represents a bonding site to the nitrogen atom in formula (2).
[0034] In formula (81), A 1 and A 2 each independently represents an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a fluorine atom, —O—, —C(═O)—, —S—, —S(═O) 2 -, -NHC(=O)-, or a group consisting of a combination of two or more thereof is preferred, an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a fluorine atom, -O-, -C(=O)-, or a group consisting of a combination of two or more thereof is more preferred, an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a fluorine atom or -O- is even more preferred, and -C(CH 3 ) 2 It is particularly preferred that -.
[0035] R in formula (2) 115 represents a tetravalent organic group. As the tetravalent organic group, a tetravalent organic group containing an aromatic ring is preferred, and a group represented by the following formula (5) or formula (6) is more preferred. In formula (5) or formula (6), * each independently represents a bonding site to another structure. In formula (5), R 112represents a single bond or a divalent linking group, and is a single bond, or an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a fluorine atom, -O-, -CO-, -S-, -SO 2 -, -NHCO-, and a group selected from a combination thereof are preferred, and a single bond, an alkylene group having 1 to 3 carbon atoms which may be substituted with a fluorine atom, -O-, -CO-, -S-, and -SO 2 - is more preferably a group selected from -CH 2 -, -C(CF 3 ) 2 -, -C(CH 3 ) 2 -, -O-, -CO-, -S- and -SO 2 It is more preferably a divalent group selected from the group consisting of -.
[0036] Also, R 115 is also preferably a group represented by the following formula (7). 115 is more preferably a group represented by the following formula (7-2). In formula (7), A 1 ~A 3 are each independently a single bond or a divalent linking group, * represents a bonding site with the carbonyl group in formula (2), and the hydrogen atoms of each of the four benzene rings described in formula (7) may be substituted with a substituent. In formula (7-2), * represents a bonding site with the carbonyl group in formula (2).
[0037] In formula (7), A 1 ~A 3 and a preferred embodiment of the substituent on the benzene ring is A in the above formula (7-1). 1 ~A 3 and the preferred embodiments of the substituents on the benzene ring are the same as those.
[0038] R 115 Specifically, R may be a tetracarboxylic acid residue remaining after removal of the anhydride group from a tetracarboxylic dianhydride. 115The tetracarboxylic acid dianhydride may contain only one kind or two or more kinds of tetracarboxylic acid dianhydride residues as a structure corresponding to the formula (I). The tetracarboxylic acid dianhydride is preferably represented by the following formula (I): In formula (O), R 115 represents a tetravalent organic group. 115 The preferred range of R in formula (2) is 115 The same applies to the preferred range.
[0039] Specific examples of tetracarboxylic dianhydrides include pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfidetetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-diphenylmethanetetracarboxylic dianhydride, 2,2 2,3,3',4'-diphenylmethanetetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-benzophenonetetracarboxylic dianhydride, 4,4'-oxydiphthalic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,4,5,7-naphthalenetetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 2,2-bis(2, 1,3-diphenylhexafluoropropane-3,3,4,4-tetracarboxylic dianhydride, 1,4,5,6-naphthalenetetracarboxylic dianhydride, 2,2',3,3'-diphenyltetracarboxylic dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 1,2,4,5-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 1,8,9,10-phenanthrenetetracarboxylic dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, 1,2,3,4-benzenetetracarboxylic dianhydride, and alkyl and alkoxy derivatives having 1 to 6 carbon atoms thereof.
[0040] Further, tetracarboxylic dianhydrides (DAA-1) to (DAA-5) described in paragraph 0038 of WO 2017 / 038598 are also preferred examples.
[0041] In formula (2), R 111 and R 115 At least one of R may have an OH group. 111Examples of the amino acid residue include residues of bisaminophenol derivatives.
[0042] R in formula (2) 113 and R 114 each independently represents a hydrogen atom or a monovalent organic group. The monovalent organic group preferably contains a linear or branched alkyl group, a cyclic alkyl group, an aromatic group, or a polyalkyleneoxy group. 113 and R 114 Preferably, at least one of R contains a polymerizable group, and more preferably, both of R 113 and R 114 It is also preferable that at least one of the groups contains two or more polymerizable groups. The polymerizable group is a group capable of undergoing a crosslinking reaction by the action of heat, radicals, or the like, and a radically polymerizable group is preferred. Specific examples of the polymerizable group include a group having an ethylenically unsaturated bond, an alkoxymethyl group, a hydroxymethyl group, an acyloxymethyl group, an epoxy group, an oxetanyl group, a benzoxazolyl group, a blocked isocyanate group, and an amino group. The radically polymerizable group possessed by the polyimide precursor is preferably a group having an ethylenically unsaturated bond. Examples of the group having an ethylenically unsaturated bond include a vinyl group, an allyl group, an isoallyl group, a 2-methylallyl group, a group having an aromatic ring directly bonded to a vinyl group (e.g., a vinylphenyl group), a (meth)acrylamide group, a (meth)acryloyloxy group, and a group represented by the following formula (III), with a group represented by the following formula (III) being preferred.
[0043]
[0044] In formula (III), R 200 represents a hydrogen atom, a methyl group, an ethyl group, or a methylol group, and is preferably a hydrogen atom or a methyl group. In formula (III), * represents a bonding site with another structure. In formula (III), R 201 represents an alkylene group having 2 to 12 carbon atoms, —CH 2 CH(OH)CH 2 -, a cycloalkylene group or a polyalkyleneoxy group. 201Examples of the alkylene group include an ethylene group, a propylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, an octamethylene group, and a dodecamethylene group; a 1,2-butanediyl group, a 1,3-butanediyl group; a —CH 2 CH(OH)CH 2 alkylene groups such as ethylene and propylene; 2 CH(OH)CH 2More preferred are alkylene groups such as ethylene and propylene, or polyalkyleneoxy groups. In the present invention, a polyalkyleneoxy group refers to a group in which two or more alkyleneoxy groups are directly bonded. The alkylene groups in the multiple alkyleneoxy groups contained in the polyalkyleneoxy group may be the same or different. When a polyalkyleneoxy group contains multiple alkyleneoxy groups with different alkylene groups, the arrangement of the alkyleneoxy groups in the polyalkyleneoxy group may be a random arrangement, a block arrangement, or an arrangement having an alternating pattern. The number of carbon atoms in the alkylene group (including the number of carbon atoms in the substituent if the alkylene group has a substituent) is preferably 2 or more, more preferably 2 to 10, even more preferably 2 to 6, even more preferably 2 to 5, even more preferably 2 to 4, even more preferably 2 or 3, and particularly preferably 2. The alkylene group may also have a substituent. Preferred substituents include alkyl groups, aryl groups, and halogen atoms. The number of alkyleneoxy groups contained in the polyalkyleneoxy group (the number of repeating polyalkyleneoxy groups) is preferably 2 to 20, more preferably 2 to 10, and even more preferably 2 to 6. From the viewpoint of solvent solubility and solvent resistance, the polyalkyleneoxy group is preferably a polyethyleneoxy group, a polypropyleneoxy group, a polytrimethyleneoxy group, a polytetramethyleneoxy group, or a group in which multiple ethyleneoxy groups and multiple propyleneoxy groups are bonded, more preferably a polyethyleneoxy group or a polypropyleneoxy group, and even more preferably a polyethyleneoxy group. In the group in which multiple ethyleneoxy groups and multiple propyleneoxy groups are bonded, the ethyleneoxy groups and propyleneoxy groups may be arranged randomly, in blocks, or in an alternating pattern. The preferred embodiments of the number of repeating ethyleneoxy groups and the like in these groups are as described above.
[0045] In formula (2), R 113is a hydrogen atom, or R 114 When is a hydrogen atom, the polyimide precursor may form a counter salt with a tertiary amine compound having an ethylenically unsaturated bond. An example of such a tertiary amine compound having an ethylenically unsaturated bond is N,N-dimethylaminopropyl methacrylate.
[0046] In formula (2), R 113 and R 114 At least one of the groups may be a polarity conversion group such as an acid-decomposable group. The acid-decomposable group is not particularly limited as long as it is decomposed by the action of an acid to generate an alkali-soluble group such as a phenolic hydroxy group or a carboxy group. Preferred examples include an acetal group, a ketal group, a silyl group, a silyl ether group, and a tertiary alkyl ester group. From the viewpoint of exposure sensitivity, an acetal group or a ketal group is more preferred. Specific examples of the acid-decomposable group include a tert-butoxycarbonyl group, an isopropoxycarbonyl group, a tetrahydropyranyl group, a tetrahydrofuranyl group, an ethoxyethyl group, a methoxyethyl group, an ethoxymethyl group, a trimethylsilyl group, a tert-butoxycarbonylmethyl group, and a trimethylsilyl ether group. From the viewpoint of exposure sensitivity, an ethoxyethyl group or a tetrahydrofuranyl group is preferred.
[0047] The polyimide precursor preferably contains fluorine atoms in its structure. The fluorine atom content in the polyimide precursor is preferably 10% by mass or more and 20% by mass or less.
[0048] Furthermore, for the purpose of improving adhesion to the substrate, the polyimide precursor may be copolymerized with an aliphatic group having a siloxane structure. Specific examples include embodiments using bis(3-aminopropyl)tetramethyldisiloxane, bis(p-aminophenyl)octamethylpentasiloxane, or the like as the diamine.
[0049] The repeating unit represented by formula (2) is preferably a repeating unit represented by formula (2-A). That is, it is preferable that at least one of the polyimide precursors used in the present invention is a precursor having a repeating unit represented by formula (2-A). When the polyimide precursor contains a repeating unit represented by formula (2-A), it becomes possible to further widen the width of the exposure latitude. Formula (2-A) In formula (2-A), A 1 and A 2 represents an oxygen atom, R 111 and R 112 each independently represents a divalent organic group; R 113 and R 114 each independently represents a hydrogen atom or a monovalent organic group; R 113 and R 114 At least one of the groups is a group containing a polymerizable group, and it is preferred that both of the groups are groups containing a polymerizable group.
[0050] A 1 , A 2 , R 111 , R 113 and R 114 are each independently A in formula (2). 1 , A 2 , R 111 , R 113 and R 114 The same definition and preferred range are also true. 112 is R in formula (5). 112 The same applies to the preferred range.
[0051] The polyimide precursor may contain one type of repeating unit represented by formula (2), or may contain two or more types. It may also contain a structural isomer of the repeating unit represented by formula (2). The polyimide precursor may also contain other types of repeating units in addition to the repeating unit of formula (2).
[0052] In one embodiment of the polyimide precursor of the present invention, the content of the repeating unit represented by formula (2) is 50 mol% or more of all repeating units. The total content is more preferably 70 mol% or more, even more preferably 90 mol% or more, and particularly preferably more than 90 mol%. The upper limit of the total content is not particularly limited, and all repeating units in the polyimide precursor except for the terminal repeating units may be repeating units represented by formula (2).
[0053] The polystyrene-equivalent weight-average molecular weight (Mw) of the polyimide precursor is preferably 5,000 to 100,000, more preferably 10,000 to 50,000, and even more preferably 15,000 to 40,000. The number-average molecular weight (Mn) of the polyimide precursor is preferably 2,000 to 40,000, more preferably 3,000 to 30,000, and even more preferably 4,000 to 20,000. Another preferred embodiment of the present invention is a polystyrene-equivalent weight-average molecular weight of less than 20,000. In this case, the lower limit of the weight-average molecular weight is preferably 5,000 or more, more preferably 8,000 or more. The polystyrene-equivalent molecular weight dispersity of the polyimide precursor is preferably 1.5 or more, more preferably 1.8 or more, and even more preferably 2.0 or more. The upper limit of the molecular weight dispersity of the polyimide precursor is not particularly specified, but is preferably 7.0 or less, more preferably 6.5 or less, and even more preferably 6.0 or less. In this specification, the molecular weight dispersity is a value calculated by weight average molecular weight / number average molecular weight. When the resin composition contains multiple types of polyimide precursors as heterocycle-containing polymer precursors, it is preferable that the weight average molecular weight, number average molecular weight, and dispersity of at least one polyimide precursor are within the above ranges. It is also preferable that the weight average molecular weight, number average molecular weight, and dispersity calculated by treating the multiple types of polyimide precursors as a single resin are each within the above ranges.
[0054] - Cyclization rate (imidization rate) - From the viewpoint of the film strength, insulating properties, etc. of the resulting organic film, the cyclization rate (imidization rate) of the polyimide precursor is preferably 60% or less, more preferably 50% or less, and even more preferably 40% or less. The lower limit of the cyclization rate is not particularly limited and may be 0%, but is preferably 1% or more, and more preferably 2% or more. The cyclization rate is measured, for example, by the following method. The infrared absorption spectrum of the polyimide precursor is measured, and the absorption peak at 1377 cm -1 Next, the polyimide precursor is heat-treated at 350° C. for 1 hour, and then the infrared absorption spectrum is measured again to determine the peak intensity P1 around 1377 cm -1 The peak intensity P2 around the peak intensity P1 is measured. The cyclization rate of the polyimide precursor can be calculated using the obtained peak intensities P1 and P2 according to the following formula: Cyclization rate (%) = (peak intensity P1 / peak intensity P2) x 100
[0055] [Polybenzoxazole Precursor] Examples of the polybenzoxazole precursor include the compounds described in paragraphs 0073 to 0095 of WO 2022 / 145355. The above descriptions are incorporated herein by reference.
[0056] [Polyamideimide Precursor] Examples of the polyamideimide precursor include the compounds described in paragraphs 0104 to 0119 of WO 2022 / 145355. The above descriptions are incorporated herein by reference.
[0057] [Method for Producing Polyimide Precursor, etc.] The polyimide precursor, etc., is produced, for example, by the method described in paragraphs 0134 to 0136 of WO 2022 / 145355. The above description is incorporated herein by reference.
[0058] [Content] The content of the heterocycle-containing polymer precursor in the resin composition of the present invention is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and even more preferably 50% by mass or more, based on the total solid content of the resin composition. Furthermore, the content of the resin in the resin composition of the present invention is preferably 99.5% by mass or less, more preferably 99% by mass or less, even more preferably 98% by mass or less, even more preferably 97% by mass or less, and even more preferably 95% by mass or less, based on the total solid content of the resin composition. The resin composition of the present invention may contain only one type of heterocycle-containing polymer precursor, or may contain two or more types. When two or more types are contained, the total amount is preferably within the above range.
[0059] The resin composition of the present invention preferably contains at least two resins. Specifically, the resin composition of the present invention may contain a total of two or more heterocycle-containing polymer precursors and other resins described later, or may contain two or more heterocycle-containing polymer precursors. However, it is preferable to contain two or more heterocycle-containing polymer precursors. When the resin composition of the present invention contains two or more heterocycle-containing polymer precursors, for example, a polyimide precursor having a structure derived from a dianhydride (R 115 ) preferably contains two or more different polyimide precursors.
[0060] <Other Resins> The resin composition of the present invention may contain the heterocycle-containing polymer precursor described above and other resins different from the heterocycle-containing polymer precursor (hereinafter simply referred to as "other resins"). Examples of other resins include polyimide, polybenzoxazole, polyamideimide, phenolic resin, polyamide, epoxy resin, polysiloxane, resins containing a siloxane structure, (meth)acrylic resin, (meth)acrylamide resin, urethane resin, butyral resin, styryl resin, polyether resin, polyester resin, etc. Examples of polyimide, polybenzoxazole, and polyamideimide include those described in paragraphs 0050 to 0077, 0101 to 0108, and 0125 to 0138 of WO 2023 / 026892, respectively. For example, by further adding a (meth)acrylic resin, a resin composition with excellent coatability can be obtained, and a pattern (cured product) with excellent solvent resistance can be obtained. For example, instead of or in addition to the polymerizable compound described later, a polymerizable compound having a weight average molecular weight of 20,000 or less and a high polymerizable group value (for example, a polymerizable compound having a molar content of 1×10 per 1 g of resin) may be used. -3 By adding a (meth)acrylic resin (having a molecular weight of 1000 to 1000 mol / g or more) to the resin composition, it is possible to improve the coatability of the resin composition and the solvent resistance of the pattern (cured product).
[0061] When the resin composition of the present invention contains other resins, the content of the other resins is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, even more preferably 1% by mass or more, even more preferably 2% by mass or more, even more preferably 5% by mass or more, and even more preferably 10% by mass or more, based on the total solid content of the resin composition. When the resin composition of the present invention contains other resins, the content of the other resins is preferably 80% by mass or less, more preferably 75% by mass or less, even more preferably 70% by mass or less, even more preferably 60% by mass or less, and even more preferably 50% by mass or less, based on the total solid content of the resin composition. A preferred embodiment of the resin composition of the present invention may also be an embodiment in which the content of the other resin is low. In the above embodiment, the content of the other resin is preferably 20% by mass or less, more preferably 15% by mass or less, even more preferably 10% by mass or less, even more preferably 5% by mass or less, and even more preferably 1% by mass or less, based on the total solid content of the resin composition. The lower limit of the content is not particularly limited, as long as it is 0% by mass or more. The resin composition of the present invention may contain only one type of other resin, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0062] <Compound A> The first resin composition of the present invention contains a first compound A. The second resin composition of the present invention contains a second compound A. The third resin composition of the present invention contains a third compound A. The first compound A, the second compound A, and the third compound A are compounds that generate a compound having at least one of a pyridine structure and a pyridinium salt structure by the action of light or heat. The compound generated from compound A is not particularly limited as long as it is a compound that generates a compound having at least one of a pyridine structure and a pyridinium salt structure.
[0063] In the present invention, the pyridine structure refers to a structure represented by the following formula (P), and the pyridinium salt structure refers to a salt structure formed by a cation represented by the following formula (Ps) and a counter anion, where * indicates a bonding site to other structures. Preferred embodiments of the compound having at least one of a pyridine structure and a pyridinium salt structure will be described in detail below.
[0064] [Confirmation of generation of a compound having at least one of a pyridine structure and a pyridinium salt structure by the action of light or heat] Whether or not a compound in the resin composition of the present invention generates a compound having at least one of a pyridine structure and a pyridinium salt structure by the action of light is determined by the following method: The resin composition of the present invention is exposed to light with a wavelength of 190 to 800 nm at an exposure intensity of 25 W / cm under conditions of 1 atmosphere and 25°C. 2 After irradiating for 60 seconds under the conditions 1 The increase in the amount of pyridine structure and pyridinium salt structure is quantified by a method such as H-NMR, and if the increase in the amount of the pyridine structure and pyridinium salt structure relative to the total molar amount of the compounds contained in the composition before exposure is 0.01 mass% or more based on the total solid content of the resin composition, the resin composition is determined to contain a compound that generates a compound having at least one of a pyridine structure and a pyridinium salt structure when acted upon by light. Which compound contained in the resin composition is the compound that generates a compound having at least one of a pyridine structure and a pyridinium salt structure when acted upon by light can be determined by the following method: 1This can be determined by analyzing the pyridine structure and pyridinium salt structure using methods such as H-NMR. Furthermore, if the structure of the compound cannot be determined by the above analysis, the structure of the compound can also be determined by analyzing the structure of the compound whose content is reduced from the resin composition before and after exposure. The increase is preferably 0.1 mol% or more, more preferably 0.5 mol% or more. The upper limit of the increase is not particularly limited, but can be, for example, 100 mol% or less. Furthermore, from the viewpoint of resolution, it is preferable that compound A generates a compound having at least one of a pyridine structure and a pyridinium salt structure upon the action of light having a wavelength to which the polymerization initiator contained in the resin composition of the present invention is sensitive. In particular, it is preferable that compound A generates a compound having at least one of a pyridine structure and a pyridinium salt structure upon the action of light having a wavelength of 300 to 450 nm. Another preferred embodiment of the present invention is that compound A generates a compound having at least one of a pyridine structure and a pyridinium salt structure upon the action of light having a wavelength of 365 nm.
[0065] Whether or not a compound in the resin composition of the present invention generates a compound having at least one of a pyridine structure and a pyridinium salt structure under the action of heat can be determined by the following method: The resin composition of the present invention is heated from 25°C to 250°C under 1 atmosphere and maintained at 250°C for 3 hours. 1 The increase in the amount of pyridine structure and pyridinium salt structure in the resin composition is quantified by H-NMR, and if the increase in the amount of pyridine structure and pyridinium salt structure relative to the total molar amount of compounds contained in the resin composition before heating is 0.01 mass% or more based on the total solid content of the resin composition, the resin composition is determined to contain a compound that generates a compound having at least one of a pyridine structure and a pyridinium salt structure upon the action of heat. Which compound contained in the resin composition is the compound that generates a compound having at least one of a pyridine structure and a pyridinium salt structure upon the action of heat can be determined by 1This can be determined by analyzing the structure of a compound containing a pyridine structure or a pyridinium salt structure using a method such as H-NMR. Furthermore, if the structure of the compound cannot be determined by the above analysis, the structure of the compound can also be determined by analyzing the structure of the compound whose content is reduced from the resin composition before and after heating. The increase is preferably 0.1 mol% or more, and more preferably 0.5 mol% or more. The upper limit of the increase is not particularly limited, but can be, for example, 100 mol% or less.
[0066] [Formula (A-1)] The first compound A, the second compound A and the third compound A preferably include a compound represented by the following formula (A-1). In formula (A-1), R 1 is a hydrogen atom or any organic group, and R 2 , R 3 , R 4 and R 5 are each independently a hydrogen atom, a halogen atom, or any organic group, and R 6 is a halogen atom or any organic group.
[0067] The compound represented by formula (A-1) generates a pyridine structure as shown below when exposed to light or heat, for example. 12 ~R 16 each independently represents a hydrogen atom or an arbitrary organic group. Preferred embodiments of formula (Py-1) will be described later.
[0068] In formula (A-1), R 1 is preferably a hydrogen atom. 1 When is an organic group, it is preferably a hydrocarbon group, more preferably an alkyl group.
[0069] In formula (A-1), R 2 and R 3are each independently preferably a hydrocarbon group, more preferably an alkyl group or an aromatic hydrocarbon group, further preferably an alkyl group or a phenyl group, and particularly preferably an alkyl group. The alkyl group is preferably an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 4 carbon atoms, and further preferably a methyl group, an ethyl group, or an isopropyl group.
[0070] In formula (A-1), R 4 and R 5 are each independently —C(═O)O—R 7 , a cyano group or —C(═O)—R 7 is preferably —C(═O)O—R 7 It is more preferable that R 7 is a hydrocarbon group which may have a substituent, and is preferably an alkyl group which may have a substituent. 7 is a substituent, R of the structure represented by formula (A-1) 4 or R 5 may include a group where is —C(═O)O— or —C(═O)—.
[0071] In formula (A-1), R 6 is preferably an aromatic group having an electron-withdrawing group as a substituent. Examples of the electron-withdrawing group include a nitro group, a halogeno group, a haloalkyl group, a cyano group, and —C(═O)O—R 8 , —C(═O)—R 8 , —C(═O)OH, etc. 8 is a hydrocarbon group which may have a substituent, and is preferably an alkyl group which may have a substituent. The halogeno group is preferably —F, —Cl or —Br. Among these, R 6The electron-withdrawing group in is preferably a nitro group or a halogeno group, more preferably a nitro group. The electron-withdrawing group may be bonded to the aromatic group without a linking group, or may be bonded via a linking group such as an alkenyl group. The aromatic group may further have a group different from the electron-withdrawing group as a substituent. The aromatic group may be an aromatic hydrocarbon group or an aromatic heterocyclic group, but is preferably a 6-membered monocyclic aromatic group, more preferably a phenyl group. Here, from the viewpoint of exposure sensitivity and resolution, R 6 When the electron-withdrawing group in is a nitro group, R 6 It is preferred that there is only one nitro group therein.
[0072] Below, R 6 Specific examples of preferred structures are given below, but the present invention is not limited to these.
[0073] Among these, R in formula (A-1) 1 is a hydrogen atom, and R 4 and R 5 are each independently —C(═O)O—R 7 , a cyano group or —C(═O)—R 7 and R 7 is a hydrocarbon group which may have a substituent, and R 6 is preferably an aromatic group having an electron-withdrawing group as a substituent.
[0074] [Formula (A-1-1)] Compound A may also be a compound represented by the following formula (A-1-1). In formula (A-1-1), R 1 is a hydrogen atom or any organic group, and R 2 , R 3 and R 4 are each independently a hydrogen atom, a halogen atom, or any organic group, and R 6 represents a halogen atom or any organic group, L represents an n-valent linking group, n represents an integer of 1 or more, and when n is 2 or more, n R 1 may be the same or different, and n R 2may be the same or different, and n R 3 may be the same or different, and n R 4 may be the same or different, and n R 6 may be the same or different.
[0075] In formula (A-1-1), R 1 , R 2 , R 3 , R 4 and R 6 A preferred embodiment of the formula (A-1) is 1 , R 2 , R 3 , R 4 and R 6 In formula (A-1-1), L is preferably an n-valent hydrocarbon group, and more preferably an n-valent saturated aliphatic hydrocarbon group. In formula (A-1-1), n is preferably an integer of 1 to 10, more preferably an integer of 1 to 6, and even more preferably an integer of 1 to 3.
[0076] [Formula (A-2)] The fourth compound A is a compound represented by the following formula (A-2): The first compound A, the second compound A and the third compound A are preferably compounds represented by the following formula (A-2). In formula (A-2), R 1 is a hydrogen atom or any organic group, and R 2 , R 3 , R 4 , R 5 are each independently a hydrogen atom, a halogen atom, or any organic group, and Ar 1 is an aromatic group having an electron-withdrawing group as a substituent, and when the electron-withdrawing group is a nitro group, Ar 1 has only one nitro group.
[0077] In formula (A-2), R 1 , R 2 , R 3 , R 4 , R 5 A preferred embodiment of the formula (A-1) is 1 , R2 , R 3 , R 4 , R 5 In formula (A-2), Ar 1 In a preferred embodiment, when the electron-withdrawing group is a nitro group, Ar 1 R in formula (A-1) is the same as R in formula (A-1), except that R has only one nitro group. 6 is the same as the preferred embodiment when is an aromatic group having an electron-withdrawing group as a substituent.
[0078] [Formula (A-2-1)] Compound A may also be a compound represented by the following formula (A-2-1). In formula (A-2-1), R 1 is a hydrogen atom or any organic group, and R 2 , R 3 and R 4 are each independently a hydrogen atom, a halogen atom, or any organic group, and Ar 1 is an aromatic group having an electron-withdrawing group as a substituent, and when the electron-withdrawing group is a nitro group, Ar 1 has only one nitro group, L represents an n-valent linking group, n represents an integer of 1 or more, and when n is 2 or more, there are n R 1 may be the same or different, and n R 2 may be the same or different, and n R 3 may be the same or different, and n R 4 may be the same or different, and n Ar 1 may be the same or different.
[0079] In formula (A-2-1), R 1 , R 2 , R 3 , R 4 and Ar 1 A preferred embodiment of the formula (A-2) is 1 , R 2 , R 3 , R 4 and Ar 1In formula (A-2-1), L is preferably an n-valent hydrocarbon group, and more preferably an n-valent saturated aliphatic hydrocarbon group. In formula (A-2-1), n is preferably an integer of 1 to 10, more preferably an integer of 1 to 6, and even more preferably an integer of 1 to 3.
[0080] [Compound Having a Pyridine Structure] In the present invention, the compound having a pyridine structure generated from compound A is preferably a compound represented by the following formula (Py-1). In formula (Py-1), R 12 , R 13 , R 14 , R 15 and R 16 are each independently a hydrogen atom, a halogen atom, or any organic group. Here, for example, it is preferable that compound A becomes a compound represented by formula (Py-1) through intramolecular oxidation-reduction. In addition, a certain compound A may be reduced by another compound A or further another compound to become formula (Py-1). For example, when compound A is a compound represented by formula (A-1), R included in formula (A-1) 1 ~R 6 is reduced, and the dihydropyridine ring structure contained in formula (A-1) is oxidized to form the pyridine ring structure in formula (Py-1). 12 , R 13 , R 14 , R 15 and R 16 A preferred embodiment of the formula (A-1) is 2 , R 3 , R 4 , R 5 and R 6 or the structures obtained by reducing these. Among these, R 6 is reduced, and the dihydropyridine ring structure contained in formula (A-1) is oxidized to form the pyridine ring structure in formula (Py-1). 12 , R 13 , R 14 and R15 A preferred embodiment of the formula (A-1) is 2 , R 3 , R 4 and R 5 and R in formula (Py-1) is the same as the preferred embodiment of 16 A preferred embodiment of the formula (A-1) is 6 Here, it is preferable that R in formula (A-1) is a reduced structure. 6 is a group containing a nitro group, R in formula (Py-1) 16 is R 6 It is preferable that the nitro group in the formula (A-1) is changed to a nitroso group. 6 is a group containing a halogen atom, R in formula (Py-1) 16 is R 6 It is preferable that the halogen atom in R in formula (A-1) is substituted with —H. 6 -C(=O)O-R 8 When the group represented by the formula (Py-1) is contained, R 16 is R 6 -C(=O)O-R in 8 is preferably a group in which is changed to —C(═O)OH.
[0081] When compound A is a compound represented by formula (A-2), R in formula (Py-1) 12 , R 13 , R 14 and R 15 A preferred embodiment of the formula (A-2) is 2 , R 3 , R 4 and R 5 In addition, when compound A is a compound represented by formula (A-2), a preferred embodiment is the same as that of R 16 is an aromatic group having an electron-withdrawing group as a substituent after reduction, when the compound A is a compound represented by formula (A-1), R in formula (Py-1) 16 This is the same as the preferred embodiment of the above.
[0082] Among these, in formula (Py-1), R 12 , R 13 , R 14and R 15 are each independently a hydrogen atom, a halogen atom, or any organic group, and R 6 is preferably a hydrogen atom or any organic group. 12 , R 13 , R 14 and R 15 A preferred embodiment of the formula (1-1) is R 2 , R 3 , R 4 and R 5 In this embodiment, R 16 is preferably an aromatic group, more preferably an aromatic group having a nitroso group, a halogeno group, or a carboxy group as a substituent, and even more preferably an aromatic group having a nitroso group as a substituent. These substituents may be bonded to the aromatic group without a linking group, or may be bonded via a linking group such as an alkenyl group. The aromatic group may further have a group different from the substituent group as a substituent. The aromatic group may be an aromatic hydrocarbon group or an aromatic heterocyclic group, but is preferably a 6-membered monocyclic aromatic group, and more preferably a phenyl group.
[0083] Specific examples of structural changes in Compound A are shown below.
[0084] The compound having a pyridine structure is also preferably a compound represented by the following formula (Py-1-1): In formula (Py-1-1), R 12 , R 13 , R 14 and R 16 are each independently a hydrogen atom, a halogen atom, or any organic group, n represents an integer of 1 or more, L represents a linking group having a valence of n+m, and n R 12 may be the same or different, and n R 13 may be the same or different, and n R 14 may be the same or different, and n R 16 may be the same or different, R1 is a hydrogen atom or any organic group, and R 2 , R 3 and R 4 are each independently a hydrogen atom, a halogen atom, or any organic group, and R 6 is a halogen atom or any organic group, m is an integer of 0 or more, and when m is 2 or more, m R 1 may be the same or different, and m R 2 may be the same or different, and m R 3 may be the same or different, and m R 4 may be the same or different, and m R 6 may be the same or different.
[0085] In formula (Py-1-1), R 12 , R 13 , R 14 and R 16 A preferred embodiment of the formula (Py-1) is R 12 , R 13 , R 14 and R 16 In formula (Py-1-1), R 1 , R 2 , R 3 , R 4 and R 6 A preferred embodiment of the formula (A-1-1) is R 1 , R 2 , R 3 , R 4 and R 6 In formula (Py-1-1), L is preferably a hydrocarbon group having a valence of n+m, and more preferably a saturated aliphatic hydrocarbon group having a valence of n+m. In formula (Py-1-1), n is preferably an integer of 1 to 10, more preferably an integer of 1 to 6, and even more preferably an integer of 1 to 3. In formula (Py-1-1), m is preferably an integer of 0 to 5, more preferably an integer of 0 to 3, and even more preferably an integer of 0 to 2. An embodiment in which m is 0 is also one of the preferred embodiments of the present invention.
[0086] [Compound Having a Pyridinium Salt Structure] In the present invention, the compound having a pyridinium salt structure generated from compound A is preferably a compound having a salt structure composed of a cation represented by the following formula (Py-2) and a counter anion. The counter anion may be present in formula (Py-2) or as another compound. In formula (Py-2), R 11 is a hydrogen atom or any organic group, and R 12 , R 13 , R 14 and R 15 are each independently a hydrogen atom, a halogen atom, or any organic group, and R 16 is a hydrogen atom or any organic group. 11 A preferred embodiment of the formula (A-1) is 1 In formula (Py-2), R 12 ~R 16 In each of the preferred embodiments, R 12 ~R 16 The preferred embodiments are the same as those of the above. 16 When has a carboxy group, it may be a carboxylate anion. This carboxylate anion may be a counter anion of the pyridinium cation in formula (Py-2).
[0087] The compound having a pyridinium salt structure is also preferably a compound having a salt structure composed of a cation represented by the following formula (Py-2-2) and a counter anion. In formula (Py-2-2), R 11 is a hydrogen atom or any organic group, and R 12 , R 13 , R 14 and R 16 are each independently a hydrogen atom, a halogen atom, or any organic group, n represents an integer of 1 or more, L represents a linking group having a valence of n+m, and n R 11 may be the same or different, and n R 12 may be the same or different, and n R13 may be the same or different, and n R 14 may be the same or different, and n R 16 may be the same or different, R 1 is a hydrogen atom or any organic group, and R 2 , R 3 and R 4 are each independently a hydrogen atom, a halogen atom, or any organic group, and R 6 is a halogen atom or any organic group, m is an integer of 0 or more, and when m is 2 or more, m R 1 may be the same or different, and m R 2 may be the same or different, and m R 3 may be the same or different, and m R 4 may be the same or different, and m R 6 may be the same or different.
[0088] In formula (Py-2-2), R 11 , R 12 , R 13 , R 14 and R 16 A preferred embodiment of the formula (Py-2) is R 11 , R 12 , R 13 , R 14 and R 16 In formula (Py-2-2), R 1 , R 2 , R 3 , R 4 and R 6 A preferred embodiment of the formula (A-1-1) is R 1 , R 2 , R 3 , R 4 and R 6In formula (Py-2-2), L is preferably a hydrocarbon group having a valence of n+m, and more preferably a saturated aliphatic hydrocarbon group having a valence of n+m. In formula (Py-2-2), n is preferably an integer of 1 to 10, more preferably an integer of 1 to 6, and even more preferably an integer of 1 to 3. In formula (Py-2-2), m is preferably an integer of 0 to 5, more preferably an integer of 0 to 3, and even more preferably an integer of 0 to 2. An embodiment in which m is 0 is also one of the preferred embodiments of the present invention.
[0089] [Compound Having a Pyridine Structure and a Pyridinium Salt Structure] In the present invention, the compound having a pyridine structure and a pyridinium salt structure generated from compound A is also preferably a compound having a salt structure constituted by a cation represented by the following formula (Py-3) and a counter anion: In formula (Py-3), R 11 is a hydrogen atom or any organic group, and R 12 , R 13 , R 14 and R 16 are each independently a hydrogen atom, a halogen atom, or any organic group; n represents an integer of 1 or more; m represents an integer of 1 or more; L represents an (n+m+i)-valent linking group; and m R 11 may be the same or different, and n+m R 12 may be the same or different, and n+m R 13 may be the same or different, and n+m R 14 may be the same or different, and n+m R 16 may be the same or different, R 1 is a hydrogen atom or any organic group, and R 2 , R 3 and R 4 are each independently a hydrogen atom, a halogen atom, or any organic group, and R 6 is a halogen atom or any organic group, and i represents an integer of 0 or more. When i is 2 or more, there are i R 1may be the same or different, and there are i R 2 may be the same or different, and there are i R 3 may be the same or different, and there are i R 4 may be the same or different, and there are i R 6 may be the same or different.
[0090] In formula (Py-3), R 11 , R 12 , R 13 , R 14 and R 16 A preferred embodiment of the formula (Py-2) is R 11 , R 12 , R 13 , R 14 and R 16 In formula (Py-3), R 1 , R 2 , R 3 , R 4 and R 6 A preferred embodiment of the formula (A-1-1) is R 1 , R 2 , R 3 , R 4 and R 6 In formula (Py-3), L is preferably an n+m+i valent hydrocarbon group, and more preferably an n+m+i valent saturated aliphatic hydrocarbon group. In formula (Py-3), n is preferably an integer of 1 to 10, more preferably an integer of 1 to 6, and even more preferably an integer of 1 to 3. In formula (Py-3), m is preferably an integer of 1 to 10, more preferably an integer of 1 to 6, and even more preferably an integer of 1 to 3. In formula (Py-3), i is preferably an integer of 0 to 5, more preferably an integer of 0 to 3, and even more preferably an integer of 0 to 2. An embodiment in which i is 0 is also one of the preferred embodiments of the present invention.
[0091] [Molecular Weight] The molecular weight of compound A is preferably 250 to 1,500, more preferably 280 to 1,000, and even more preferably 300 to 800.
[0092] [Synthesis Method] Compound A can be synthesized, for example, by the method described in the Examples below. Alternatively, other known synthesis methods may be used, and the synthesis method is not particularly limited.
[0093] [Specific Examples] Specific examples of Compound A are not particularly limited, but include the compounds used in the examples described below.
[0094] [Content] The content of compound A relative to the total solid content of the resin composition of the present invention is preferably 0.05 to 30% by mass. The lower limit is more preferably 0.1% by mass or more, even more preferably 0.3% by mass or more, and particularly preferably 0.5% by mass or more. The upper limit is more preferably 20% by mass or less, even more preferably 15% by mass or less, and particularly preferably 10% by mass or less. Furthermore, when the content of the heterocycle-containing polymer precursor is taken as 100 parts by mass, the content of compound A is preferably 0.10 to 30 parts by mass, preferably 0.20 to 30 parts by mass, more preferably 0.50 to 20 parts by mass, and even more preferably 1.0 to 10 parts by mass. One type of compound A may be used alone, or two or more types may be used in combination. When two or more types are used in combination, the total amount thereof is preferably within the above range.
[0095] <Compound Having At Least One of a Pyridine Structure and a Pyridinium Salt Structure> The resin composition of the present invention may contain a compound having at least one of a pyridine structure and a pyridinium salt structure. A preferred embodiment of the compound having at least one of a pyridine structure and a pyridinium salt structure is the same as the preferred embodiment of the compound having at least one of a pyridine structure and a pyridinium salt structure generated from the above-mentioned compound A.
[0096] The content of the compound having at least one of a pyridine structure and a pyridinium salt structure relative to the total mass of the resin composition of the present invention is preferably 0.0001 to 0.010 mass%, more preferably 0.0002 to 0.009 mass%, and even more preferably 0.0005 to 0.008 mass%.
[0097] <Organometallic Complex> The first resin composition of the present invention contains an organometallic complex. The second resin composition, the third resin composition, and the fourth resin composition of the present invention preferably contain an organometallic complex. The organometallic complex is preferably a compound containing a Group 4 element. The compound containing a Group 4 element is preferably a compound containing titanium, zirconium, or hafnium, and more preferably a compound containing titanium. Furthermore, the compound containing a Group 4 element is preferably an organometallic complex, and more preferably an organotitanium complex.
[0098] Specific examples of titanium-containing compounds are shown below in I) to VII): I) Titanium chelate compounds: Among these, titanium chelates having two or more alkoxy groups are more preferred because they provide a negative photosensitive resin composition with good storage stability and a good pattern. Specific examples include titanium bis(triethanolamine) diisopropoxide, titanium di(n-butoxide) bis(2,4-pentanedionate), titanium diisopropoxide bis(2,4-pentanedionate), titanium diisopropoxide bis(tetramethylheptanedionate), titanium diisopropoxide bis(ethylacetoacetate), etc.
[0099] II) Tetraalkoxytitanium compounds: for example, titanium tetra(n-butoxide), titanium tetraethoxide, titanium tetra(2-ethylhexoxide), titanium tetraisobutoxide, titanium tetraisopropoxide, titanium tetramethoxide, titanium tetramethoxypropoxide, titanium tetramethylphenoxide, titanium tetra(n-nonyloxide), titanium tetra(n-propoxide), titanium tetrastearyloxide, titanium tetrakis[bis{2,2-(allyloxymethyl)butoxide}], etc.
[0100] III) Titanocene compounds: for example, pentamethylcyclopentadienyltitanium trimethoxide, bis(η 5 -2,4-cyclopentadien-1-yl)bis(2,6-difluorophenyl)titanium, bis(η 5 -2,4-cyclopentadien-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, and the like.
[0101] IV) Monoalkoxytitanium compounds: For example, titanium tris(dioctylphosphate) isopropoxide, titanium tris(dodecylbenzenesulfonate) isopropoxide, etc.
[0102] V) Titanium oxide compounds: For example, titanium oxide bis(pentanedionate), titanium oxide bis(tetramethylheptanedionate), phthalocyanine titanium oxide, etc.
[0103] VI) Titanium tetraacetylacetonate compounds: For example, titanium tetraacetylacetonate.
[0104] VII) Titanate coupling agents: for example, isopropyl tridodecylbenzenesulfonyl titanate.
[0105] Among the above I) to VII), it is preferable that the titanium-containing compound is at least one compound selected from the group consisting of I) titanium chelate compounds, II) tetraalkoxytitanium compounds, and III) titanocene compounds, from the viewpoint of exhibiting better chemical resistance. In particular, titanium diisopropoxide bis(ethylacetoacetate), titanium tetra(n-butoxide), and bis(η 5 3-(1H-pyrrol-1-yl)phenyl)titanium is preferred.
[0106] Furthermore, the organometallic complex is preferably a metal complex having one or more π-conjugated moieties containing a nitrogen atom (hereinafter also referred to as a "specific metal complex"). Here, the nitrogen atom is preferably directly bonded to a metal atom in the specific metal complex. The bond is not particularly limited, but is preferably a coordinate bond. Furthermore, the π-conjugated moiety may have only one nitrogen atom or may have two or more nitrogen atoms. When two or more nitrogen atoms are present, it is preferable that one of the nitrogen atoms is directly bonded to a metal atom in the specific metal complex. Here, the specific metal complex may have only one or two or more π-conjugated moieties containing a nitrogen atom, but it is preferable that the specific metal complex has one to two π-conjugated moieties.
[0107] The π-conjugated moiety containing a nitrogen atom preferably has a structure represented by the following formula (Co-1). In formula (Co-1), X 1 ~X 3 each independently represents -C(-*)= or -N=, * represents a bonding site to another structure, and # represents a bonding site to a metal atom.
[0108] In formula (Co-1), X 1 ~X 3 each independently represents -C(-*)= or -N=, and it is preferable that at least one represents -C(-*)=, and it is more preferable that at least two represent -C(-*)=.
[0109] In formula (Co-1), at least two structures bonded to * may be bonded to form a ring structure. The ring structure may be an aliphatic ring structure or an aromatic ring structure, but is preferably an aromatic ring structure.
[0110] It is also preferable to include a compound represented by the following formula (T-1) as the specific metal complex. In formula (T-1), M is titanium, zirconium, or hafnium, l1 is an integer of 0 to 2, l2 is 0 or 1, l1 + l2 × 2 is an integer of 0 to 2, m is an integer of 0 to 4, n is an integer of 0 to 2, l1 + l2 + m + n × 2 = 4, and R 11 are each independently a substituted or unsubstituted cyclopentadienyl group, a substituted or unsubstituted alkoxy group, or a substituted or unsubstituted phenoxy group; R 12 is a substituted or unsubstituted hydrocarbon group, R 2 are each independently a group containing a structure represented by the following formula (T-2), and R 3 are each independently a group containing a structure represented by the following formula (T-2), A are each independently an oxygen atom or a sulfur atom. In formula (T-2), X 1 ~X 3 each independently represents -C(-*)= or -N=, * represents a bonding site to another structure, and # represents a bonding site to a metal atom.
[0111] In formula (T-1), from the viewpoint of storage stability of the composition, M is preferably titanium. In formula (T-1), an embodiment in which l1 and l2 are 0 is also one of the preferred embodiments of the present invention. In formula (T-1), m is preferably 2 or 4, and more preferably 2. In formula (T-1), n is preferably 1 or 2, and more preferably 1. Here, it is also preferable that in formula (T-1), l1 and l2 are 0, and m is 0, 2, or 4.
[0112] In formula (T-1), from the viewpoint of the stability of the specific metal complex, R 11 is preferably a substituted or unsubstituted cyclopentadienyl ligand. 11The cyclopentadienyl group, alkoxy group and phenoxy group in the formula (I) may be substituted, but an embodiment in which they are unsubstituted is also one of the preferred embodiments of the present invention.
[0113] In formula (T-1), R 12 is preferably a hydrocarbon group having 1 to 20 carbon atoms, and more preferably a hydrocarbon group having 2 to 10 carbon atoms. 12 The hydrocarbon group in may be either an aliphatic hydrocarbon group or an aromatic hydrocarbon group, but an aromatic hydrocarbon group is preferred. The aliphatic hydrocarbon group may be either a saturated aliphatic hydrocarbon group or an unsaturated aliphatic hydrocarbon group, but a saturated aliphatic hydrocarbon group is preferred. The aromatic hydrocarbon group is preferably an aromatic hydrocarbon group having 6 to 20 carbon atoms, more preferably an aromatic hydrocarbon group having 6 to 10 carbon atoms, and even more preferably a phenylene group. R 12 The substituent in R is preferably a monovalent substituent, such as a halogen atom. 12 When R is an aromatic hydrocarbon group, it may have an alkyl group as a substituent. 12 is preferably an unsubstituted phenylene group. 12 The phenylene group in is preferably a 1,2-phenylene group.
[0114] In formula (T-1), m is 2 or more, and R 2 If two or more are included, 2 In formula (T-1), n is 2 or more, and R 3 If two or more are included, 3 The structures may be the same or different.
[0115] In formula (T-2), X 1 ~X 3 each independently represents -C(-*)= or -N=, and it is preferable that at least one represents -C(-*)=, and it is more preferable that at least two represent -C(-*)=.
[0116] When the resin composition contains an organometallic complex, the content is preferably 0.05 to 10 parts by mass, and more preferably 0.1 to 5 parts by mass, per 100 parts by mass of the heterocycle-containing polymer precursor. When the content is 0.05 parts by mass or more, heat resistance and chemical resistance are improved, and when it is 10 parts by mass or less, storage stability is improved.
[0117] <Group 4 Element Content> In the second resin composition of the present invention, the content of the Group 4 element in the composition is 0.010 to 5.0 mass% based on the total solid content of the composition. In the first, third, and fourth resin compositions of the present invention, the content of the Group 4 element in the composition is preferably 0.050 to 4.0 mass% based on the total solid content of the composition. The Group 4 element is contained in the composition of the present invention, for example, as the above-mentioned organometallic complex or its decomposition product. The content of the Group 4 element is quantified by comparing the results of measurement by ICP-MS (inductively coupled plasma mass spectrometry) with a calibration curve prepared using samples containing the Group 4 element at known concentrations. In particular, in the resin composition of the present invention, the content of the Group 4 element is preferably 0.010 to 5.0 mass%, more preferably 0.050 to 4.0 mass%, based on the total solid content of the composition.
[0118] <Polymerizable Compound> The resin composition of the present invention preferably further contains a polymerizable compound. Examples of the polymerizable compound include a radical crosslinking agent and other crosslinking agents.
[0119] [Radical Crosslinking Agent] The resin composition of the present invention preferably contains a radical crosslinking agent. The radical crosslinking agent is a compound having a radical polymerizable group. The radical polymerizable group is preferably a group containing an ethylenically unsaturated bond. Examples of the group containing an ethylenically unsaturated bond include a vinyl group, an allyl group, a vinylphenyl group, a (meth)acryloyl group, a maleimide group, and a (meth)acrylamide group. Among these, a (meth)acryloyl group, a (meth)acrylamide group, and a vinylphenyl group are preferred, and from the viewpoint of reactivity, a (meth)acryloyl group is more preferred.
[0120] The radical crosslinking agent is preferably a compound having one or more ethylenically unsaturated bonds, more preferably a compound having two or more ethylenically unsaturated bonds. The radical crosslinking agent may have three or more ethylenically unsaturated bonds. The compound having two or more ethylenically unsaturated bonds is preferably a compound having 2 to 15 ethylenically unsaturated bonds, more preferably a compound having 2 to 10 ethylenically unsaturated bonds, and even more preferably a compound having 2 to 6 ethylenically unsaturated bonds. From the viewpoint of the film strength of the obtained pattern (cured product), it is also preferable that the resin composition of the present invention contains a compound having two ethylenically unsaturated bonds and the compound having three or more ethylenically unsaturated bonds.
[0121] The molecular weight of the radical crosslinking agent is preferably 2,000 or less, more preferably 1,500 or less, and even more preferably 900 or less. The lower limit of the molecular weight of the radical crosslinking agent is preferably 100 or more.
[0122] Specific examples of radical crosslinking agents include unsaturated carboxylic acids (e.g., acrylic acid, methacrylic acid, itaconic acid, crotonic acid, isocrotonic acid, maleic acid, etc.), their esters, and amides. Preferred are esters of unsaturated carboxylic acids and polyhydric alcohol compounds, and amides of unsaturated carboxylic acids and polyamine compounds. Also suitable are addition reaction products of unsaturated carboxylic acid esters or amides having a nucleophilic substituent such as a hydroxyl group, amino group, or sulfanyl group with monofunctional or polyfunctional isocyanates or epoxies, and dehydration condensation reaction products of monofunctional or polyfunctional carboxylic acids. Also suitable are addition reaction products of unsaturated carboxylic acid esters or amides having an electrophilic substituent such as an isocyanate group or an epoxy group with monofunctional or polyfunctional alcohols, amines, or thiols, and substitution reaction products of unsaturated carboxylic acid esters or amides having a leaving substituent such as a halogeno group or a tosyloxy group with monofunctional or polyfunctional alcohols, amines, or thiols. As another example, it is also possible to use a group of compounds in which the above-mentioned unsaturated carboxylic acids are replaced with unsaturated phosphonic acids, vinylbenzene derivatives such as styrene, vinyl ethers, allyl ethers, etc. Specific examples can be found in paragraphs 0113 to 0122 of JP 2016-027357 A, the contents of which are incorporated herein by reference.
[0123] The radical crosslinking agent is preferably a compound having a boiling point of 100°C or higher under normal pressure. Examples of compounds having a boiling point of 100°C or higher under normal pressure include the compounds described in paragraph 0203 of WO 2021 / 112189, the contents of which are incorporated herein by reference.
[0124] Other preferred radical crosslinking agents include the radical polymerizable compounds described in paragraphs 0204 to 0208 of WO 2021 / 112189, the contents of which are incorporated herein by reference.
[0125] Preferred radical crosslinking agents include dipentaerythritol triacrylate (commercially available products include KAYARAD D-330 (manufactured by Nippon Kayaku Co., Ltd.)), dipentaerythritol tetraacrylate (commercially available products include KAYARAD D-320 (manufactured by Nippon Kayaku Co., Ltd.) and A-TMMT (manufactured by Shin-Nakamura Chemical Co., Ltd.)), dipentaerythritol penta(meth)acrylate (commercially available products include KAYARAD D-310 (manufactured by Nippon Kayaku Co., Ltd.)), and dipentaerythritol hexa(meth)acrylate (commercially available products include KAYARAD DPHA (manufactured by Nippon Kayaku Co., Ltd.) and A-DPH (manufactured by Shin-Nakamura Chemical Co., Ltd.)), and structures in which the (meth)acryloyl group is bonded via an ethylene glycol residue or a propylene glycol residue. Oligomers of these agents can also be used.
[0126] Commercially available radical crosslinking agents include, for example, SR-494, a tetrafunctional acrylate having four ethyleneoxy chains, SR-209, 231, and 239, which are difunctional methacrylates having four ethyleneoxy chains (all manufactured by Sartomer Corporation), DPCA-60, a hexafunctional acrylate having six pentyleneoxy chains, and TPA-330, a trifunctional acrylate having three isobutyleneoxy chains (all manufactured by Nippon Kayaku Co., Ltd.), and urethane oligomers such as Examples of such an ester include UAS-10 and UAB-140 (manufactured by Nippon Paper Industries Co., Ltd.), NK Ester M-40G, NK Ester 4G, NK Ester M-9300, NK Ester A-9300, and UA-7200 (manufactured by Shin-Nakamura Chemical Co., Ltd.), DPHA-40H (manufactured by Nippon Kayaku Co., Ltd.), UA-306H, UA-306T, UA-306I, AH-600, T-600, and AI-600 (manufactured by Kyoeisha Chemical Co., Ltd.), and Blenmar PME400 (manufactured by NOF Corporation).
[0127] Suitable radical crosslinking agents include urethane acrylates such as those described in JP-B No. 48-041708, JP-A No. 51-037193, JP-B No. 02-032293, and JP-B No. 02-016765, and urethane compounds having an ethylene oxide skeleton such as those described in JP-B No. 58-049860, JP-B No. 56-017654, JP-B No. 62-039417, and JP-B No. 62-039418. Compounds having an amino structure or a sulfide structure in the molecule, such as those described in JP-A Nos. 63-277653, 63-260909, and JP-A No. 01-105238, can also be used as radical crosslinking agents.
[0128] The radical crosslinking agent may be a radical crosslinking agent having an acid group such as a carboxy group or a phosphate group. The radical crosslinking agent having an acid group is preferably an ester of an aliphatic polyhydroxy compound and an unsaturated carboxylic acid, and more preferably a radical crosslinking agent obtained by reacting a non-aromatic carboxylic anhydride with an unreacted hydroxy group of an aliphatic polyhydroxy compound to provide an acid group. Particularly preferred is a radical crosslinking agent obtained by reacting a non-aromatic carboxylic anhydride with an unreacted hydroxy group of an aliphatic polyhydroxy compound to provide an acid group, in which the aliphatic polyhydroxy compound is pentaerythritol or dipentaerythritol. Examples of commercially available products include polybasic acid-modified acrylic oligomers M-510 and M-520 manufactured by Toagosei Co., Ltd.
[0129] The acid value of the radical crosslinking agent having an acid group is preferably 0.1 to 300 mgKOH / g, more preferably 1 to 100 mgKOH / g. When the acid value of the radical crosslinking agent is within the above range, the agent has excellent handleability in production and developability. Furthermore, the agent has good polymerizability. The acid value is measured in accordance with the description of JIS K 0070:1992.
[0130] As the radical crosslinking agent, a radical crosslinking agent having at least one selected from the group consisting of a urea bond and a urethane bond (hereinafter also referred to as "crosslinking agent U") is also preferred. In the present invention, the urea bond is a radical crosslinking agent having at least one selected from the group consisting of *-NR N —C(═O)—NR N- is a bond represented by *, and R N each independently represents a hydrogen atom or a monovalent organic group, and * represents a bonding site with a carbon atom. In the present invention, the urethane bond is *—O—C(═O)—NR N - is a bond represented by *, and R N represents a hydrogen atom or a monovalent organic group, and * represents a bonding site with a carbon atom. The inclusion of crosslinker U in a resin composition may improve chemical resistance, resolution, and the like. While the mechanism by which this effect is achieved is unclear, it is thought that, for example, a portion of crosslinker U thermally decomposes during curing by heating or the like, generating amines, which then promote the cyclization of heterocycle-containing polymer precursors such as polyimide precursors. Crosslinker U may have only one urea bond or urethane bond, one or more urea bonds and one or more urethane bonds, no urethane bonds but two or more urea bonds, or no urea bonds but two or more urethane bonds. The total number of urea bonds and urethane bonds in crosslinker U is 1 or more, preferably 1 to 10, more preferably 1 to 4, and even more preferably 1 or 2. When crosslinker U does not have a urethane bond, the number of urea bonds in crosslinker U is 1 or more, preferably 1 to 10, more preferably 1 to 4, and even more preferably 1 or 2. When the crosslinking agent U does not have a urea bond, the number of urethane bonds in the crosslinking agent U is 1 or more, preferably 1 to 10, more preferably 1 to 4, and even more preferably 1 or 2.
[0131] The radical polymerizable group in the crosslinking agent U is not particularly limited, but examples thereof include a vinyl group, an allyl group, a (meth)acryloyl group, a (meth)acryloxy group, a (meth)acrylamide group, a vinylphenyl group, and a maleimide group. A (meth)acryloxy group, a (meth)acrylamide group, a vinylphenyl group, or a maleimide group is preferred, and a (meth)acryloxy group is more preferred. When the crosslinking agent U has two or more radical polymerizable groups, the structures of the respective radical polymerizable groups may be the same or different. The number of radical polymerizable groups in the crosslinking agent U may be only one or may be two or more, preferably 1 to 10, more preferably 1 to 6, and particularly preferably 1 to 4. The radical polymerizable group value (mass of the compound per mole of radical polymerizable group) in the crosslinking agent U is preferably 150 to 400 g / mol. From the viewpoint of chemical resistance of the cured product, the lower limit of the radical polymerizable group value is more preferably 200 g / mol or more, even more preferably 210 g / mol or more, even more preferably 220 g / mol or more, even more preferably 230 g / mol or more, still more preferably 240 g / mol or more, and particularly preferably 250 g / mol or more. From the viewpoint of developability, the upper limit of the radical polymerizable group value is more preferably 350 g / mol or less, even more preferably 330 g / mol or less, and particularly preferably 300 g / mol or less. In particular, the polymerizable group value of crosslinking agent U is preferably 210 to 400 g / mol, and more preferably 220 to 400 g / mol.
[0132] Specific examples of the crosslinking agent U are shown below, but the crosslinking agent U is not limited to these.
[0133] From the viewpoints of pattern resolution and film stretchability, the resin composition preferably uses a bifunctional methacrylate or acrylate. Specific compounds include triethylene glycol diacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, tetraethylene glycol diacrylate, PEG (polyethylene glycol) 200 diacrylate, PEG 200 dimethacrylate, PEG 600 diacrylate, PEG 600 dimethacrylate, polytetraethylene glycol diacrylate, polytetraethylene glycol dimethacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, neopentyl glycol diacrylate, neopentyl glycol dimethacrylate, 3-methyl-1,5-pentanediol diacrylate, 1,6-hexyl ... Examples of usable radical crosslinkers include xanediol diacrylate, 1,6-hexanediol dimethacrylate, dimethylol-tricyclodecane diacrylate, dimethylol-tricyclodecane dimethacrylate, ethylene oxide (EO) adduct diacrylate of bisphenol A, propylene oxide (PO) adduct dimethacrylate of bisphenol A, propylene oxide (PO) adduct dimethacrylate of bisphenol A, 2-hydroxy-3-acryloyloxypropyl methacrylate, EO-modified isocyanuric acid diacrylate, EO-modified isocyanuric acid dimethacrylate, and other bifunctional acrylates and bifunctional methacrylates having urethane bonds. Two or more of these may be mixed and used as needed. For example, PEG200 diacrylate refers to polyethylene glycol diacrylate with a formula weight of approximately 200 for the polyethylene glycol chain. From the viewpoint of suppressing warpage of the pattern (cured product), the resin composition of the present invention preferably uses a monofunctional radical crosslinker as the radical crosslinker.Preferred examples of monofunctional radical crosslinking agents include (meth)acrylic acid derivatives such as n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, carbitol (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, N-methylol (meth)acrylamide, glycidyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, and polypropylene glycol mono(meth)acrylate; N-vinyl compounds such as N-vinylpyrrolidone and N-vinylcaprolactam; and allyl glycidyl ether. Preferred monofunctional radical crosslinking agents include compounds having a boiling point of 100°C or higher under normal pressure in order to suppress volatilization before exposure. Other examples of bifunctional or higher radical crosslinking agents include allyl compounds such as diallyl phthalate and triallyl trimellitate.
[0134] When a radical crosslinking agent is contained, the content of the radical crosslinking agent is preferably more than 0% by mass and not more than 60% by mass, based on the total solid content of the resin composition. The lower limit is more preferably 5% by mass or more. The upper limit is more preferably 50% by mass or less, and even more preferably 30% by mass or less.
[0135] The radical crosslinking agent may be used alone or in combination of two or more. When two or more types are used in combination, the total amount thereof is preferably within the above range.
[0136] [Other Crosslinking Agents] The resin composition of the present invention preferably contains another crosslinking agent different from the radical crosslinking agent described above. The other crosslinking agent refers to a crosslinking agent other than the radical crosslinking agent described above. It is preferably a compound having multiple groups in its molecule that promote the reaction of forming a covalent bond with other compounds in the composition or their reaction products upon exposure to light by the photoacid generator or photobase generator described above. It is preferable that the compound have multiple groups in its molecule that promote the reaction of forming a covalent bond with other compounds in the composition or their reaction products under the action of an acid or base. The acid or base is preferably an acid or base generated from a photoacid generator or photobase generator during the exposure step. Examples of other crosslinking agents include the compounds described in paragraphs 0179 to 0207 of WO 2022 / 145355. The above descriptions are incorporated herein by reference.
[0137] [Polymerization initiator] The resin composition of the present invention contains a polymerization initiator. The polymerization initiator may be a thermal polymerization initiator or a photopolymerization initiator, but it is particularly preferable to contain a photopolymerization initiator. The photopolymerization initiator is preferably a photoradical polymerization initiator. There are no particular restrictions on the photoradical polymerization initiator, and it can be appropriately selected from known photoradical polymerization initiators. For example, a photoradical polymerization initiator that is photosensitive to light in the ultraviolet to visible range is preferred. Alternatively, it may be an activator that reacts with a photoexcited sensitizer to generate active radicals.
[0138] The photoradical polymerization initiator has a capacity of at least about 50 L·mol within a wavelength range of about 240 to 800 nm (preferably 330 to 500 nm). -1 ・cm -1 The molar absorption coefficient of the compound can be measured using a known method. For example, it is preferable to measure the molar absorption coefficient using an ultraviolet-visible spectrophotometer (Varian Cary-5 spectrophotometer) at a concentration of 0.01 g / L using ethyl acetate as a solvent.
[0139] Any known compound can be used as the photoradical polymerization initiator. Examples include halogenated hydrocarbon derivatives (e.g., compounds having a triazine skeleton, compounds having an oxadiazole skeleton, compounds having a trihalomethyl group, etc.), acylphosphine compounds such as acylphosphine oxide, hexaarylbiimidazole, oxime compounds such as oxime derivatives, organic peroxides, thio compounds, ketone compounds, aromatic onium salts, ketoxime ethers, α-aminoketone compounds such as aminoacetophenone, α-hydroxyketone compounds such as hydroxyacetophenone, azo compounds, azide compounds, metallocene compounds, organic boron compounds, and iron arene complexes. For details of these compounds, please refer to paragraphs
[0165] to
[0182] of JP 2016-027357 A and paragraphs
[0138] to
[0151] of WO 2015 / 199219 A, the contents of which are incorporated herein by reference. Further, paragraphs 0065 to 0111 of JP 2014-130173 A, compounds described in Japanese Patent No. 6301489, MATERIAL STAGE 37 to 60p, vol. 19, No. 3,2019 described peroxide-based photopolymerization initiators, photopolymerization initiators described in WO 2018 / 221177, photopolymerization initiators described in WO 2018 / 110179, photopolymerization initiators described in JP 2019-043864 A, photopolymerization initiators described in JP 2019-044030 A, peroxide-based initiators described in JP 2019-167313 A can be mentioned, the contents of which are incorporated herein by reference.
[0140] Examples of ketone compounds include the compounds described in paragraph 0087 of JP 2015-087611 A, the contents of which are incorporated herein by reference. As a commercially available product, Kayacure-DETX-S (manufactured by Nippon Kayaku Co., Ltd.) is also preferably used.
[0141] In one embodiment of the present invention, a hydroxyacetophenone compound, an aminoacetophenone compound, or an acylphosphine compound can be suitably used as the photoradical polymerization initiator. More specifically, for example, an aminoacetophenone-based initiator described in JP-A-10-291969 or an acylphosphine oxide-based initiator described in Japanese Patent No. 4225898 can be used, the contents of which are incorporated herein by reference.
[0142] Examples of α-hydroxyketone initiators that can be used include Omnirad 184, Omnirad 1173, Omnirad 2959, and Omnirad 127 (all manufactured by IGM Resins B.V.), IRGACURE 184 (IRGACURE is a registered trademark), DAROCUR 1173, IRGACURE 500, IRGACURE-2959, and IRGACURE 127 (all manufactured by BASF).
[0143] Examples of α-aminoketone initiators that can be used include Omnirad 907, Omnirad 369, Omnirad 369E, and Omnirad 379EG (all manufactured by IGM Resins B.V.), and IRGACURE 907, IRGACURE 369, and IRGACURE 379 (all manufactured by BASF).
[0144] As the aminoacetophenone initiator, acylphosphine oxide initiator, and metallocene compound, for example, compounds described in paragraphs 0161 to 0163 of WO 2021 / 112189 can also be suitably used. The contents of this specification are incorporated herein by reference.
[0145] As the photoradical polymerization initiator, an oxime compound is more preferably used. By using an oxime compound, it is possible to more effectively improve the exposure latitude. An oxime compound is particularly preferred because it has a wide exposure latitude (exposure margin) and also functions as a photocuring accelerator.
[0146] Specific examples of the oxime compound include compounds described in JP-A-2001-233842, compounds described in JP-A-2000-080068, compounds described in JP-A-2006-342166, compounds described in J. C. S. Perkin II (1979, pp. 1653-1660), compounds described in J. C. S. Perkin II (1979, pp. 156-162), compounds described in Journal of Photopolymer Science and Technology (1995, pp.202-232) described compounds, compounds described in JP-A-2000-066385, compounds described in JP-T-2004-534797, compounds described in JP-A-2017-019766, compounds described in Japanese Patent No. 6065596, compounds described in WO 2015 / 152153, compounds described in WO 2017 / 051680, compounds described in JP-A-2017-198865, compounds described in paragraphs 0025 to 0038 of WO 2017 / 164127, compounds described in WO 2013 / 167515 and the like, the contents of which are incorporated herein.
[0147] Preferred oxime compounds include, for example, compounds having the following structure: 3-(benzoyloxy(imino))butan-2-one, 3-(acetoxy(imino))butan-2-one, 3-(propionyloxy(imino))butan-2-one, 2-(acetoxy(imino))pentan-3-one, 2-(acetoxy(imino))-1-phenylpropan-1-one, 2-(benzoyloxy(imino))-1-phenylpropan-1-one, 3-((4-toluenesulfonyloxy)imino)butan-2-one, and 2-(ethoxycarbonyloxy(imino))-1-phenylpropan-1-one. In the resin composition, it is particularly preferable to use an oxime compound as a photoradical polymerization initiator. The oxime compound as a photoradical polymerization initiator has a linking group of >C=N-O-C(=O)- in the molecule.
[0148]
[0149] Commercially available oxime compounds include IRGACURE OXE 01, IRGACURE OXE 02, IRGACURE OXE 03, and IRGACURE OXE 04 (manufactured by BASF), ADEKA OPTOMER N-1919 (manufactured by ADEKA Corporation, photoradical polymerization initiator 2 described in JP 2012-014052 A), TR-PBG-304, TR-PBG-305 (manufactured by Changzhou Strong Electronic New Materials Co., Ltd.), ADEKA ARCLES NCI-730, NCI-831, and ADEKA ARCLES NCI-930 (manufactured by ADEKA Corporation), DFI-091 (manufactured by Daito ChemiX Co., Ltd.), and SpeedCure PDO (SARTOMER Also, an oxime compound having the following structure can be used.
[0150] When the resin composition contains a photopolymerization initiator, the content thereof is preferably 0.1 to 30% by mass, more preferably 0.1 to 20% by mass, even more preferably 0.5 to 15% by mass, and even more preferably 1.0 to 10% by mass, based on the total solid content of the resin composition. Only one type of photopolymerization initiator may be contained, or two or more types may be contained. When two or more types of photopolymerization initiators are contained, the total amount is preferably within the above range. Note that the photopolymerization initiator may also function as a thermal polymerization initiator, and therefore crosslinking by the photopolymerization initiator may be further promoted by heating in an oven, hot plate, or the like.
[0151] [Sensitizer] The resin composition may contain a sensitizer. The sensitizer absorbs specific actinic radiation and becomes electronically excited. The electronically excited sensitizer comes into contact with a thermal radical polymerization initiator, a photoradical polymerization initiator, or the like, and undergoes electron transfer, energy transfer, heat generation, and other actions. This causes the thermal radical polymerization initiator or the photoradical polymerization initiator to undergo a chemical change and decompose, generating a radical, acid, or base. Usable sensitizers include benzophenone-based, Michler's ketone-based, coumarin-based, pyrazole azo-based, anilino azo-based, triphenylmethane-based, anthraquinone-based, anthracene-based, anthrapyridone-based, benzylidene-based, oxonol-based, pyrazolotriazole azo-based, pyridone azo-based, cyanine-based, phenothiazine-based, pyrrolopyrazole azomethine-based, xanthene-based, phthalocyanine-based, benzopyran-based, and indigo-based compounds.Examples of the sensitizer include Michler's ketone, 4,4'-bis(diethylamino)benzophenone, 2,5-bis(4'-diethylaminobenzal)cyclopentane, 2,6-bis(4'-diethylaminobenzal)cyclohexanone, 2,6-bis(4'-diethylaminobenzal)-4-methylcyclohexanone, 4,4'-bis(dimethylamino)chalcone, 4,4'-bis(diethylamino)chalcone, p-dimethylaminocinnamylideneindanone, p-dimethylaminobenzylideneindanone, and Non, 2-(p-dimethylaminophenylbiphenylene)benzothiazole, 2-(p-dimethylaminophenylvinylene)benzothiazole, 2-(p-dimethylaminophenylvinylene)isonaphthothiazole, 1,3-bis(4'-dimethylaminobenzal)acetone, 1,3-bis(4'-diethylaminobenzal)acetone, 3,3'-carbonyl-bis(7-diethylaminocoumarin), 3-acetyl-7-dimethylaminocoumarin, 3-ethoxycarbonyl-7-dimethylaminocoumarin Phosphorus, 3-benzyloxycarbonyl-7-dimethylaminocoumarin, 3-methoxycarbonyl-7-diethylaminocoumarin, 3-ethoxycarbonyl-7-diethylaminocoumarin (ethyl 7-(diethylamino)coumarin-3-carboxylate), N-phenyl-N'-ethylethanolamine, N-phenyldiethanolamine, N-p-tolyldiethanolamine, N-phenylethanolamine, 4-morpholinobenzophenone, isoamyl dimethylaminobenzoate, isoamyl diethylaminobenzoate Examples of sensitizing dyes include soamyl, 2-mercaptobenzimidazole, 1-phenyl-5-mercaptotetrazole, 2-mercaptobenzothiazole, 2-(p-dimethylaminostyryl)benzoxazole, 2-(p-dimethylaminostyryl)benzothiazole, 2-(p-dimethylaminostyryl)naphtho(1,2-d)thiazole, 2-(p-dimethylaminobenzoyl)styrene, diphenylacetamide, benzanilide, N-methylacetanilide, and 3',4'-dimethylacetanilide. Other sensitizing dyes may also be used. For details of sensitizing dyes, please refer to the descriptions in paragraphs 0161 to 0163 of JP-A-2016-027357, the contents of which are incorporated herein by reference.
[0152] When the resin composition contains a sensitizer, the content of the sensitizer is preferably 0.01 to 20 mass %, more preferably 0.1 to 15 mass %, and still more preferably 0.5 to 10 mass %, based on the total solid content of the resin composition. The sensitizer may be used alone or in combination of two or more types.
[0153] [Chain Transfer Agent] The resin composition of the present invention may contain a chain transfer agent. Chain transfer agents are defined, for example, in the Third Edition of the Polymer Dictionary (edited by the Society of Polymer Science, 2005), pages 683-684. Examples of chain transfer agents include those having -S-S-, -SO 2 Examples of compounds that can be used include compounds having -S-, -N-O-, SH, PH, SiH, and GeH, and dithiobenzoates, trithiocarbonates, dithiocarbamates, and xanthate compounds having a thiocarbonylthio group used in RAFT (Reversible Addition Fragmentation Chain Transfer) polymerization. These compounds can donate hydrogen to low-activity radicals to generate radicals, or can be oxidized and then deprotonated to generate radicals. Thiol compounds are particularly preferred.
[0154] In addition, the chain transfer agent may be a compound described in paragraphs 0152 to 0153 of WO 2015 / 199219, the contents of which are incorporated herein by reference.
[0155] When the resin composition contains a chain transfer agent, the content of the chain transfer agent is preferably 0.01 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, and even more preferably 0.5 to 5 parts by mass, relative to 100 parts by mass of the total solid content of the resin composition. Only one type of chain transfer agent may be used, or two or more types may be used. When two or more types of chain transfer agents are used, the total content thereof is preferably within the above range.
[0156] In another preferred embodiment of the present invention, the resin composition of the present invention contains two or more polymerization initiators. Specifically, the resin composition of the present invention preferably contains a photopolymerization initiator and a thermal polymerization initiator described below, or the above-mentioned photoradical polymerization initiator and the above-mentioned photoacid generator.
[0157] By including a photopolymerization initiator and a thermal polymerization initiator described below, pattern formation by exposure becomes possible, and radical polymerization also proceeds more easily during curing by a heating step described below, which may improve performance such as chemical resistance. When a photopolymerization initiator and a thermal polymerization initiator described below are included, the content of the thermal polymerization initiator is preferably 20 to 70% by mass, and more preferably 30 to 60% by mass, relative to the total content of the photopolymerization initiator and the thermal polymerization initiator.
[0158] Inclusion of a photoradical polymerization initiator and a photoacid generator may improve performance such as resolution. When a photopolymerization initiator and a photoacid generator are included, the content ratio of the photoacid generator relative to the total content of the photopolymerization initiator and the photoacid generator is preferably 20 to 70 mass %, more preferably 30 to 60 mass %.
[0159] [Thermal Polymerization Initiator] Examples of the thermal polymerization initiator include a thermal radical polymerization initiator. A thermal radical polymerization initiator is a compound that generates radicals by thermal energy and initiates or promotes the polymerization reaction of a polymerizable compound. Addition of a thermal radical polymerization initiator can also promote the polymerization reaction of the resin and the polymerizable compound, thereby further improving solvent resistance.
[0160] Specific examples of the thermal radical polymerization initiator include compounds described in paragraphs 0074 to 0118 of JP-A-2008-063554, the contents of which are incorporated herein by reference.
[0161] When a thermal polymerization initiator is contained, the content thereof is preferably 0.1 to 30 mass% relative to the total solid content of the resin composition, more preferably 0.1 to 20 mass%, and even more preferably 0.5 to 15 mass%. The resin composition may contain only one type of thermal polymerization initiator, or may contain two or more types. When two or more types of thermal polymerization initiators are contained, the total amount is preferably in the above range.
[0162] <Base Generator Other Than Compound A> The third resin composition of the present invention contains a base generator other than Compound A (hereinafter also referred to as "other base generator"). The first, second, and fourth resin compositions of the present invention preferably contain another base generator. Here, the base generator is a compound capable of generating a base by physical or chemical action. Preferred base generators include thermal base generators and photobase generators. By containing a thermal base generator in the resin composition, for example, the cyclization reaction of the heterocycle-containing polymer precursor can be promoted by heating, and the mechanical properties and chemical resistance of the cured product can be improved, resulting in excellent performance as an interlayer insulating film for a rewiring layer included in a semiconductor package. The other base generator may be an ionic base generator or a nonionic base generator. Examples of bases generated from the other base generator include secondary amines and tertiary amines. The other base generator is not particularly limited, and known base generators can be used. Examples of known base generators include carbamoyl oxime compounds, carbamoyl hydroxylamine compounds, carbamic acid compounds, formamide compounds, acetamide compounds, carbamate compounds, benzyl carbamate compounds, nitrobenzyl carbamate compounds, sulfonamide compounds, imidazole derivative compounds, amine imide compounds, pyridine derivative compounds, α-aminoacetophenone derivative compounds, quaternary ammonium salt derivative compounds, iminium salts, pyridinium salts, α-lactone ring derivative compounds, amine imide compounds, phthalimide derivative compounds, and acyloxyimino compounds. Specific examples of non-ionic base generators include the compounds described in paragraphs 0249 to 0275 of WO 2022 / 145355. The above descriptions are incorporated herein by reference.
[0163] Other base generators include, but are not limited to, the following compounds:
[0164]
[0165] The molecular weight of the nonionic base generator is preferably 800 or less, more preferably 600 or less, and even more preferably 500 or less. The lower limit is preferably 100 or more, more preferably 200 or more, and even more preferably 300 or more.
[0166] Specific preferred compounds for the ionic base generator include, for example, the compounds described in paragraphs 0148 to 0163 of WO 2018 / 038002.
[0167] Specific examples of ammonium salts include, but are not limited to, the following compounds:
[0168] Specific examples of iminium salts include, but are not limited to, the following compounds:
[0169] As the other base generator, an amine in which the amino group is protected with a t-butoxycarbonyl group is preferred from the viewpoints of storage stability and generating a base by deprotection during curing.
[0170] Examples of amine compounds protected by a t-butoxycarbonyl group include ethanolamine, 3-amino-1-propanol, 1-amino-2-propanol, 2-amino-1-propanol, 4-amino-1-butanol, 2-amino-1-butanol, 1-amino-2-butanol, 3-amino-2,2-dimethyl-1-propanol, 4-amino-2-methyl-1-butanol, valinol, 3-amino-1,2-propanediol, and 2-amino-1,3-propanediol. alcohol, tyramine, norephedrine, 2-amino-1-phenyl-1,3-propanediol, 2-aminocyclohexanol, 4-aminocyclohexanol, 4-aminocyclohexaneethanol, 4-(2-aminoethyl)cyclohexanol, N-methylethanolamine, 3-(methylamino)-1-propanol, 3-(isopropylamino)propanol, N-cyclohexylethanolamine, α-[2-(methylamino)ethyl]benzyl alcohol, diethanolamine diamine, diisopropanolamine, 3-pyrrolidinol, 2-pyrrolidinemethanol, 4-hydroxypiperidine, 3-hydroxypiperidine, 4-hydroxy-4-phenylpiperidine, 4-(3-hydroxyphenyl)piperidine, 4-piperidinemethanol, 3-piperidinemethanol, 2-piperidinemethanol, 4-piperidineethanol, 2-piperidineethanol, 2-(4-piperidyl)-2-propanol, 1,4-butanolbis(3-aminopropyl)ethanol ter, 1,2-bis(2-aminoethoxy)ethane, 2,2'-oxybis(ethylamine), 1,14-diamino-3,6,9,12-tetraoxatetradecane, 1-aza-15-crown-5-ether, diethylene glycol bis(3-aminopropyl)ether, 1,11-diamino-3,6,9-trioxaundecane, or compounds in which the amino group of an amino acid or a derivative thereof is protected with a t-butoxycarbonyl group, but are not limited to these.
[0171] When the resin composition contains another base generator, the content of the other base generator is preferably 0.1 to 50 parts by mass per 100 parts by mass of the resin in the resin composition. The lower limit is more preferably 0.3 parts by mass or more, and even more preferably 0.5 parts by mass or more. The upper limit is more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, even more preferably 10 parts by mass or less, even more preferably 5 parts by mass or less, and particularly preferably 4 parts by mass or less. Furthermore, when the content of the compound A is taken as 100 parts by mass, the content of the base generator is preferably 1.0 to 1000 parts by mass, more preferably 5.0 to 900 parts by mass, and even more preferably 10.0 to 800 parts by mass. One or more types of the other base generators can be used. When two or more types are used, the total amount is preferably within the above range.
[0172] <Solvent> The resin composition of the present invention preferably contains a solvent. Any known solvent can be used as the solvent. The solvent is preferably an organic solvent. Examples of the organic solvent include compounds such as esters, ethers, ketones, cyclic hydrocarbons, sulfoxides, amides, ureas, and alcohols.
[0173] Examples of esters include ethyl acetate, n-butyl acetate, isobutyl acetate, hexyl acetate, amyl formate, isoamyl acetate, butyl propionate, isopropyl butyrate, ethyl butyrate, butyl butyrate, methyl lactate, ethyl lactate, γ-butyrolactone, ε-caprolactone, δ-valerolactone, γ-valerolactone, alkyl alkyloxyacetates (for example, methyl alkyloxyacetate, ethyl alkyloxyacetate, butyl alkyloxyacetate (for example, methyl methoxyacetate, ethyl methoxyacetate, butyl methoxyacetate, methyl ethoxyacetate, ethyl ethoxyacetate, etc.)), 3-alkyloxypropionic acid alkyl esters (for example, methyl 3-alkyloxypropionate, ethyl 3-alkyloxypropionate (for example, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, etc.)), 2-alkyloxypropionic acid alkyl esters ...alkyloxypropionate, ethyl 3-alkyloxypropionate, 2-alkyloxypropionic acid alkyl esters (for example, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, etc.)), 2-alkyloxypropionic acid alkyl esters (for example, methyl 3-alkyloxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, etc.)), 2-alkyloxypropionic acid alkyl esters (for example, methyl 3- Preferred examples thereof include alkyl esters of alkyloxypropionates (e.g., methyl 2-alkyloxypropionate, ethyl 2-alkyloxypropionate, propyl 2-alkyloxypropionate (e.g., methyl 2-methoxypropionate, ethyl 2-methoxypropionate, propyl 2-methoxypropionate, methyl 2-ethoxypropionate, ethyl 2-ethoxypropionate)), methyl 2-alkyloxy-2-methylpropionate and ethyl 2-alkyloxy-2-methylpropionate (e.g., methyl 2-methoxy-2-methylpropionate, ethyl 2-ethoxy-2-methylpropionate), methyl pyruvate, ethyl pyruvate, propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, methyl 2-oxobutanoate, ethyl 2-oxobutanoate, ethyl hexanoate, ethyl heptanoate, dimethyl malonate, and diethyl malonate.
[0174] Suitable examples of ethers include ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol ethyl methyl ether, diethylene glycol butyl methyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol dimethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether, ethylene glycol monobutyl ether acetate, diethylene glycol ethyl methyl ether, propylene glycol monopropyl ether acetate, and dipropylene glycol dimethyl ether.
[0175] Suitable examples of ketones include methyl ethyl ketone, cyclohexanone, cyclopentanone, 2-heptanone, 3-heptanone, 3-methylcyclohexanone, levoglucosenone, and dihydrolevoglucosenone.
[0176] Suitable examples of cyclic hydrocarbons include aromatic hydrocarbons such as toluene, xylene, and anisole, and cyclic terpenes such as limonene.
[0177] A preferred example of the sulfoxides is dimethyl sulfoxide.
[0178] Preferred examples of the amides include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, N,N-dimethylisobutyramide, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, N-formylmorpholine, and N-acetylmorpholine.
[0179] Preferred examples of ureas include N,N,N',N'-tetramethylurea and 1,3-dimethyl-2-imidazolidinone.
[0180] Examples of alcohols include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 1-pentanol, 1-hexanol, benzyl alcohol, ethylene glycol monomethyl ether, 1-methoxy-2-propanol, 2-ethoxyethanol, diethylene glycol monoethyl ether, diethylene glycol monohexyl ether, triethylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether, polyethylene glycol monomethyl ether, polypropylene glycol, tetraethylene glycol, ethylene glycol monobutyl ether, ethylene glycol monobenzyl ether, ethylene glycol monophenyl ether, methylphenyl carbinol, n-amyl alcohol, methyl amyl alcohol, and diacetone alcohol.
[0181] From the viewpoint of improving the properties of the coated surface, it is also preferable to mix two or more kinds of solvents.
[0182] In the present invention, one solvent selected from methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl cellosolve acetate, ethyl lactate, diethylene glycol dimethyl ether, butyl acetate, methyl 3-methoxypropionate, 2-heptanone, cyclohexanone, cyclopentanone, γ-butyrolactone, γ-valerolactone, 3-methoxy-N,N-dimethylpropionamide, toluene, dimethyl sulfoxide, ethyl carbitol acetate, butyl carbitol acetate, N-methyl-2-pyrrolidone, propylene glycol methyl ether, propylene glycol methyl ether acetate, levoglucosenone, and dihydrolevoglucosenone, or a mixed solvent composed of two or more solvents, is preferred. Particularly preferred are a combination of dimethyl sulfoxide and γ-butyrolactone, a combination of dimethyl sulfoxide and γ-valerolactone, a combination of 3-methoxy-N,N-dimethylpropionamide and γ-butyrolactone, a combination of 3-methoxy-N,N-dimethylpropionamide, γ-butyrolactone and dimethyl sulfoxide, or a combination of N-methyl-2-pyrrolidone and ethyl lactate. An embodiment in which toluene is further added to these combined solvents in an amount of approximately 1 to 10% by mass, based on the total mass of the solvent, is also a preferred embodiment of the present invention. In particular, from the viewpoint of the storage stability of the resin composition, an embodiment in which γ-valerolactone is included as a solvent is also a preferred embodiment of the present invention. In such an embodiment, the content of γ-valerolactone relative to the total mass of the solvent is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more. The upper limit of the above content is not particularly limited and may be 100% by mass. The content may be determined in consideration of the solubility of components such as the heterocycle-containing polymer precursor contained in the resin composition.Furthermore, when dimethyl sulfoxide and γ-valerolactone are used in combination, the solvent preferably contains 60 to 90% by mass of γ-valerolactone and 10 to 40% by mass of dimethyl sulfoxide, more preferably 70 to 90% by mass of γ-valerolactone and 10 to 30% by mass of dimethyl sulfoxide, and even more preferably 75 to 85% by mass of γ-valerolactone and 15 to 25% by mass of dimethyl sulfoxide, relative to the total mass of the solvent.
[0183] From the viewpoint of coatability, the content of the solvent is preferably an amount such that the total solids concentration of the resin composition of the present invention is 5 to 80 mass%, more preferably an amount such that the total solids concentration is 5 to 75 mass%, even more preferably an amount such that the total solids concentration is 10 to 70 mass%, and even more preferably an amount such that the total solids concentration is 20 to 70 mass%. The solvent content may be adjusted depending on the desired thickness of the coating film and the coating method. When two or more solvents are contained, the total amount of the solvents is preferably within the above range.
[0184] <Metal adhesion improver> The resin composition of the present invention preferably contains a metal adhesion improver from the viewpoint of improving adhesion to metal materials used in electrodes, wiring, etc. Examples of metal adhesion improvers include silane coupling agents having an alkoxysilyl group, aluminum-based adhesion aids, titanium-based adhesion aids, compounds having a sulfonamide structure, compounds having a thiourea structure, phosphoric acid derivative compounds, β-ketoester compounds, amino compounds, etc. However, compounds corresponding to the above-mentioned compound A are not considered to be metal adhesion improvers and silane coupling agents as referred to herein.
[0185] [Silane Coupling Agent] Examples of silane coupling agents include the compounds described in paragraph 0316 of WO 2021 / 112189 and the compounds described in paragraphs 0067 to 0078 of JP 2018-173573 A, the contents of which are incorporated herein by reference. It is also preferable to use two or more different silane coupling agents, as described in paragraphs 0050 to 0058 of JP 2011-128358 A. It is also preferable to use the following compounds as the silane coupling agent. In the formula below, Me represents a methyl group, and Et represents an ethyl group. Furthermore, the following R represents a structure derived from a blocking agent in a blocked isocyanate group. The blocking agent may be selected depending on the desorption temperature, and examples include alcohol compounds, phenol compounds, pyrazole compounds, triazole compounds, lactam compounds, and active methylene compounds. For example, caprolactam is preferred from the viewpoint of achieving a desorption temperature of 160 to 180°C. Commercially available products of such compounds include X-12-1293 (manufactured by Shin-Etsu Chemical Co., Ltd.).
[0186]
[0187] Other silane coupling agents include, for example, vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, N-2- Examples of suitable silane coupling agents include (aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, tris-(trimethoxysilylpropyl)isocyanurate, 3-ureidopropyltrialkoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, and 3-trimethoxysilylpropylsuccinic anhydride. These may be used alone or in combination of two or more. Furthermore, oligomeric compounds having multiple alkoxysilyl groups may also be used as silane coupling agents. Examples of such oligomeric compounds include compounds containing a repeating unit represented by the following formula (S-1): In formula (S-1), R S1 represents a monovalent organic group, R S2 represents a hydrogen atom, a hydroxy group or an alkoxy group, and n represents an integer of 0 to 2. S1is preferably a structure containing a polymerizable group. Examples of the polymerizable group include a group having an ethylenically unsaturated bond, an epoxy group, an oxetanyl group, a benzoxazolyl group, a blocked isocyanate group, and an amino group. Examples of the group having an ethylenically unsaturated bond include a vinyl group, an allyl group, an isoallyl group, a 2-methylallyl group, a group having an aromatic ring directly bonded to a vinyl group (for example, a vinylphenyl group), a (meth)acrylamide group, and a (meth)acryloyloxy group. A vinylphenyl group, a (meth)acrylamide group, or a (meth)acryloyloxy group is preferred, a vinylphenyl group or a (meth)acryloyloxy group is more preferred, and a (meth)acryloyloxy group is even more preferred. R S2 is preferably an alkoxy group, more preferably a methoxy group or an ethoxy group. n represents an integer of 0 to 2, preferably 1. Here, the structures of the multiple repeating units represented by formula (S-1) contained in the oligomer-type compound may be the same. Here, of the multiple repeating units represented by formula (S-1) contained in the oligomer-type compound, it is preferable that n is 1 or 2 in at least one, more preferably that n is 1 or 2 in at least two, and even more preferably that n is 1 in at least two. Such oligomer-type compounds can be commercially available products, and an example of a commercially available product is KR-513 (manufactured by Shin-Etsu Chemical Co., Ltd.).
[0188] It is also preferable to use, as the silane coupling agent, a compound having a structure in which a hydrogen atom in the alkoxy group of the alkoxysilyl group is substituted with an organic group having at least one atom selected from an oxygen atom, a nitrogen atom, and a sulfur atom. Examples of such compounds include the following compounds.
[0189] [Aluminum-Based Adhesion Aid] Examples of aluminum-based adhesion aids include aluminum tris(ethylacetoacetate), aluminum tris(acetylacetonate), and ethylacetoacetate aluminum diisopropylate.
[0190] Other metal adhesion improvers that can be used include the compounds described in paragraphs 0046 to 0049 of JP-A-2014-186186 and the sulfide-based compounds described in paragraphs 0032 to 0043 of JP-A-2013-072935, the contents of which are incorporated herein by reference.
[0191] The content of the metal adhesion improver is preferably 0.01 to 30 parts by mass, more preferably 0.1 to 10 parts by mass, and even more preferably 0.5 to 5 parts by mass, relative to 100 parts by mass of the heterocycle-containing polymer precursor. By ensuring that the content is equal to or greater than the above lower limit, the adhesion between the pattern and the metal layer is improved, and by ensuring that the content is equal to or less than the above upper limit, the heat resistance and mechanical properties of the pattern are improved. Only one type of metal adhesion improver may be used, or two or more types may be used. When two or more types are used, it is preferable that the total amount is within the above range.
[0192] <Compound X1> The resin composition of the present invention may contain compound X1. Compound X1 is a compound having at least one structure selected from the group consisting of a 1,3-dicarbonyl structure and a β-hydroxycarbonyl structure, and having a molecular weight of 1,000 or less. Here, the 1,3-dicarbonyl structure refers to a structure represented by formula (DC-1) below, and the β-hydroxycarbonyl structure refers to a structure represented by formula (HC-1) below.
[0193] In formula (DC-1) or formula (HC-1), * and # each represent a bonding site with another structure. Here, * is preferably a bonding site with a carbon atom, an oxygen atom, a nitrogen atom, or a sulfur atom. Also, # is preferably a bonding site with a hydrogen atom or a carbon atom. Here, the structure represented by (DC-1) above may be an enol type as shown in formula (DC-2) below. Also, the structure represented by (HC-1) above may be an enol type as shown in formula (HC-2) below. In formula (DC-2) or formula (HC-2), * and # each represent a bonding site to another structure. * is preferably a bonding site to a carbon atom, oxygen atom, nitrogen atom, or sulfur atom. Also, # is preferably a bonding site to a hydrogen atom or carbon atom.
[0194] It is preferable that compound X1 does not contain a metal atom in its structure. The metal atom here does not include metalloid atoms such as silica atoms. Furthermore, it is preferable that compound X1 is not coordinated to a metal atom in the resin composition.
[0195] [Molecular Weight] The molecular weight of compound X1 is 1,000 or less, preferably 100 to 500, more preferably 100 to 400, even more preferably 100 to 350, particularly preferably 100 to 300, and even more preferably 100 to 250.
[0196] [Specific Examples] Specific examples of compound X1 include, but are not limited to, compounds having the following structures.
[0197] [Content] The content of compound X1 relative to the total solid content of the resin composition of the present invention is preferably 0.01 to 30% by mass. The lower limit is more preferably 0.02% by mass or more, even more preferably 0.05% by mass or more, and particularly preferably 0.10% by mass or more. The upper limit is more preferably 20% by mass or less, even more preferably 10% by mass or less, and particularly preferably 5% by mass or less. An embodiment in which the content is 1% by mass or less is also one of the preferred embodiments of the present invention. One type of compound X1 may be used alone, or two or more types may be used in combination. When two or more types are used in combination, the total amount thereof preferably falls within the above range.
[0198] <Compound X2> The resin composition of the present invention preferably contains compound X2. Compound X2 is a compound represented by the following formula (B-1). In formula (B-1), R B1 represents a tertiary alkyl group, R B2 each independently represents a hydrogen atom or an organic group.
[0199] In formula (B-1), R B1 represents a tertiary alkyl group, and is preferably a group represented by the following formula (B1-1), more preferably a t-butyl group.
[0200] In formula (B1-1), R B3 each independently represents an alkyl group, and * represents a bonding site with the benzene ring in formula (B-1). B3 are each independently preferably an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 4 carbon atoms, still more preferably a methyl group or an ethyl group, and particularly preferably a methyl group. The alkyl group is preferably a linear alkyl group.
[0201] In formula (B-1), R B2 is an organic group, R B2 is preferably a hydrocarbon group or a group represented by a combination of a hydrocarbon group and a ring structure. The hydrocarbon group is preferably an aliphatic saturated hydrocarbon group or a group represented by a combination of an aliphatic hydrocarbon group and an aromatic hydrocarbon group. The ring structure may be either an aromatic ring structure or an aliphatic ring structure, but is preferably an aliphatic ring structure, and more preferably an isocyanuric ring structure.
[0202] The molecular weight of compound X2 is preferably 100 to 2,000, more preferably 150 to 1,000, and even more preferably 200 to 800.
[0203] Specific examples of the compound represented by formula (B-1) include, but are not limited to, 2,6-di-tert-butyl-4-methylphenol, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, N,N '-Hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], 3,3',3",5,5',5"-hexa-tert-butyl-a,a',a"-(mesitylene-2,4,6-triyl)tri-p-cresol, ethylene bis(oxyethylene) bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], hexamethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], hydroxyphenyl)propionate, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,6-di-tert-butyl-4-(4,6-bis(octylthio)-1,3,5-triazin-2-ylamino)phenol, 4,4',4"-(1-methylpropanyl-3-ylidene)tris(6-tert-butyl-m-cresol), 6,6'-di-tert-butyl 4,4'-butylidene-m-cresol, 3,9-bis[2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane, t-butylhydroquinone, di-t-butyl-p-cresol, 4,4-thiobis(3-methyl-6-t-butylphenol), 2,2'-methylenebis(4-methyl-6-t-butylphenol), and the like.
[0204] The content of compound X2 relative to the total solid content of the resin composition of the present invention is preferably 0.1 to 5% by mass. The lower limit is more preferably 0.2% by mass or more, and even more preferably 0.3% by mass or more. The upper limit is more preferably 3% by mass or less, and even more preferably 1% by mass or less. Compound X2 may be used alone or in combination with two or more types. When two or more types are used in combination, the total amount is preferably in the above range.
[0205] <Compound X3> From the viewpoint of improving developability, the resin composition of the present invention preferably contains a compound represented by the following formula (X-3). In formula (X-3), R X1 represents a hydrogen atom or an alkyl group, and n is an integer of 1 to 10. In formula (X-3), R X1 is preferably a hydrogen atom or an alkyl group having 1 to 15 carbon atoms, more preferably a hydrogen atom or an alkyl group having 1 to 12 carbon atoms, still more preferably a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and particularly preferably a hydrogen atom, a methyl group, or an ethyl group.
[0206] Specific examples of compound X3 include 4-hydroxybutyric acid, methyl 4-hydroxybutyrate, ethyl 4-hydroxybutyrate, propyl 4-hydroxybutyrate, isopropyl 4-hydroxybutyrate, butyl 4-hydroxybutyrate, pentyl 4-hydroxybutyrate, hexyl 4-hydroxybutyrate, heptyl 4-hydroxybutyrate, octyl 4-hydroxybutyrate, nonyl 4-hydroxybutyrate, and decyl 4-hydroxybutyrate.
[0207] The content of the compound X3 is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, based on 100 parts by mass of the heterocycle-containing polymer precursor.
[0208] <Migration Inhibitor> The resin composition of the present invention preferably further contains a migration inhibitor. By containing a migration inhibitor, for example, when the resin composition is applied to a metal layer (or metal wiring) to form a film, it is possible to effectively inhibit metal ions derived from the metal layer (or metal wiring) from migrating into the film. The migration inhibitor referred to here does not include compounds corresponding to the above-mentioned Compound X1 or Compound X2.
[0209] The migration inhibitor is not particularly limited, but examples thereof include compounds having a heterocycle (pyrrole ring, furan ring, thiophene ring, imidazole ring, oxazole ring, thiazole ring, pyrazole ring, isoxazole ring, isothiazole ring, tetrazole ring, pyridine ring, pyridazine ring, pyrimidine ring, pyrazine ring, piperidine ring, piperazine ring, morpholine ring, 2H-pyran ring, 6H-pyran ring, triazine ring), thioureas and compounds having a sulfanyl group, hindered phenol compounds, salicylic acid derivative compounds, and hydrazide derivative compounds. In particular, triazole compounds such as 1,2,4-triazole, benzotriazole, 3-amino-1,2,4-triazole, and 3,5-diamino-1,2,4-triazole, and tetrazole compounds such as 1H-tetrazole, 5-phenyltetrazole, and 5-amino-1H-tetrazole are preferably used.
[0210] As the migration inhibitor, an ion trapping agent that traps anions such as halogen ions can also be used.
[0211] Other migration inhibitors include the rust inhibitors described in paragraph 0094 of JP-A-2013-015701, the compounds described in paragraphs 0073 to 0076 of JP-A-2009-283711, the compounds described in paragraph 0052 of JP-A-2011-059656, the compounds described in paragraphs 0114, 0116 and 0118 of JP-A-2012-194520, and the compounds described in paragraph 0166 of WO 2015 / 199219. The contents of this specification are incorporated herein by reference.
[0212] Specific examples of the migration inhibitor include the following compounds.
[0213]
[0214] When the resin composition of the present invention contains a migration inhibitor, the content of the migration inhibitor is preferably 0.01 to 5.0 mass%, more preferably 0.05 to 2.0 mass%, and even more preferably 0.1 to 1.0 mass%, based on the total solid content of the resin composition.
[0215] The migration inhibitor may be one kind or two or more kinds. When two or more kinds of migration inhibitors are used, the total amount thereof is preferably within the above range.
[0216] <Polymerization inhibitor> The resin composition of the present invention preferably contains a polymerization inhibitor. Examples of the polymerization inhibitor include phenolic compounds, quinone compounds, amino compounds, N-oxyl free radical compounds, nitro compounds, nitroso compounds, heteroaromatic ring compounds, and metal compounds. The polymerization inhibitor referred to here does not include compounds corresponding to the above-mentioned Compound X1 or Compound X2.
[0217] Specific examples of the polymerization inhibitor include the compounds described in paragraph 0310 of WO 2021 / 112189, p-hydroquinone, o-hydroquinone, 4-hydroxy-2,2,6,6-tetramethylpiperidine 1-oxyl free radical, phenoxazine, 1,4,4-trimethyl-2,3-diazabicyclo[3.2.2]non-2-ene-N,N-dioxide, and the like, the contents of which are incorporated herein by reference.
[0218] When the resin composition of the present invention contains a polymerization inhibitor, the content of the polymerization inhibitor is preferably 0.01 to 20 mass%, more preferably 0.02 to 15 mass%, and even more preferably 0.05 to 10 mass%, based on the total solid content of the resin composition.
[0219] The polymerization inhibitor may be one kind or two or more kinds. When two or more kinds of polymerization inhibitors are used, the total amount thereof is preferably within the above range.
[0220] [Urea Compound, Carbodiimide Compound, Isourea Compound] From the viewpoint of elongation at break and adhesion to a metal or resin layer, the resin composition of the present invention may contain at least one compound (hereinafter also referred to as "urea compound, etc.") selected from the group consisting of compounds having a urea bond (urea compound), compounds having a carbodiimide structure (carbodiimide compound), and compounds having an isourea bond (isourea compound). Among these, it is preferable that the resin composition of the present invention further contains a compound having a urea bond. The urea compound, etc. referred to here does not include the above-mentioned compound A, the above-mentioned polymerizable compound, or compounds corresponding to silane coupling agents. The urea compound generates a primary or secondary amine upon thermal decomposition. This amine promotes cyclization of the heterocycle-containing polymer precursor upon heating. However, due to the high nucleophilicity of the amine, side reactions such as addition reactions to the resin may occur during curing of the composition, inhibiting cyclization of the heterocycle-containing polymer precursor. In the present invention, a compound containing at least one of a pyridine structure and a pyridinium salt structure is generated from compound A. These compounds have low nucleophilicity, making them less likely to undergo the above-mentioned side reactions, and are highly compatible with resins, making them more likely to remain in the film, promoting the cyclization of the resin gently over a long period of time. On the other hand, the above-mentioned amines may have higher basicity and may be more likely to promote cyclization. It is believed that the combined use of these compounds that generate bases with different properties can promote the cyclization of the resin with high efficiency, achieving excellent elongation at break. Examples of urea compounds include compounds represented by the following formula (UR-1), examples of carbodiimide compounds include compounds represented by the following formula (UR-2), and examples of isourea compounds include compounds represented by the following formula (UR-3).
[0221] In formula (UR-1), formula (UR-2) or formula (UR-3), R 11 and R 12 each independently represents an aliphatic hydrocarbon group having 1 to 7 carbon atoms which may have a substituent, R 21 and R 22each independently represents an aliphatic hydrocarbon group having 1 to 7 carbon atoms which may have a substituent, R 31 and R 32 each independently represents an aliphatic hydrocarbon group having 1 to 7 carbon atoms which may have a substituent, R 33 represents an aliphatic hydrocarbon group having 1 to 7 carbon atoms which may have a substituent. 11 and R 12 are each independently preferably an unsubstituted aliphatic hydrocarbon group having 1 to 7 carbon atoms, or an aliphatic hydrocarbon group having 1 to 7 carbon atoms and having at least one substituent selected from the group consisting of a primary amine salt structure, a secondary amine salt structure, a tertiary amino group, a tertiary amine salt structure, and a quaternary ammonium group, and more preferably an unsubstituted aliphatic hydrocarbon group having 1 to 7 carbon atoms. 11 and R 12 The unsubstituted aliphatic hydrocarbon group having 1 to 7 carbon atoms in the formula (I) is preferably an unsubstituted saturated aliphatic hydrocarbon group having 1 to 7 carbon atoms, more preferably an unsubstituted saturated aliphatic hydrocarbon group having 2 to 7 carbon atoms, and even more preferably an ethyl group, an isopropyl group, a t-butyl group, or a cyclohexyl group.
[0222] In formula (UR-1), R 11 and R 12 may each independently be an aliphatic hydrocarbon group having 2 to 7 carbon atoms and having at least one substituent selected from the group consisting of a hydroxy group, an alkoxy group, a thiol group, and an alkylthio group. The aliphatic hydrocarbon group having 2 to 7 carbon atoms may have two or more of the above-mentioned substituents, but it is also preferable that it have only one of the above-mentioned substituents.
[0223] In formula (UR-2), R 21 and R 22 each independently represents an aliphatic hydrocarbon group having 1 to 7 carbon atoms which may have a substituent. 21 and R 22 is preferably an unsubstituted aliphatic hydrocarbon group having 1 to 7 carbon atoms, or an aliphatic hydrocarbon group having 1 to 7 carbon atoms and having an amino group or a quaternary ammonium group as a substituent, and more preferably an unsubstituted aliphatic hydrocarbon group having 1 to 7 carbon atoms. 21 and R22 Preferred embodiments of the unsubstituted aliphatic hydrocarbon group having 1 to 7 carbon atoms or the substituted aliphatic hydrocarbon group having 1 to 7 carbon atoms in the above formula are respectively represented by R 11 and R 12 This is similar to what was shown in the explanation of .
[0224] In formula (UR-3), R 31 and R 32 is preferably an unsubstituted aliphatic hydrocarbon group having 1 to 7 carbon atoms, or an aliphatic hydrocarbon group having 1 to 7 carbon atoms and having an amino group or a quaternary ammonium group as a substituent, and more preferably an unsubstituted aliphatic hydrocarbon group having 1 to 7 carbon atoms. 31 and R 32 Preferred embodiments of the unsubstituted aliphatic hydrocarbon group having 1 to 7 carbon atoms or the substituted aliphatic hydrocarbon group having 1 to 7 carbon atoms in the above formula are respectively represented by R 11 and R 12 This is similar to what was shown in the explanation of .
[0225] In formula (UR-3), R 33 represents an aliphatic hydrocarbon group having 1 to 7 carbon atoms which may have a substituent, and is preferably an unsubstituted aliphatic hydrocarbon group having 1 to 7 carbon atoms, more preferably an unsubstituted saturated aliphatic hydrocarbon group having 1 to 7 carbon atoms, and even more preferably an unsubstituted saturated aliphatic hydrocarbon group having 1 to 4 carbon atoms. 33 As the alkyl group, a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group or a t-butyl group is preferred, and an ethyl group is more preferred.
[0226] Specific examples of the urea compound include, but are not limited to, dicyclohexylurea, diisopropylurea, dicyclohexylcarbodiimide, diisopropylcarbodiimide, dicyclohexylisourea, and diisopropylisourea.
[0227] The total content of the urea compound and the like is preferably 0.1 to 10.0 parts by mass, more preferably 0.5 to 8.0 parts by mass, and even more preferably 1.0 to 6.0 parts by mass, per 100 parts by mass of the heterocycle-containing polymer precursor. The urea compound and the like may be used alone or in combination of two or more types. When two or more types of bases are used in combination in the base-containing treatment liquid, it is preferable that the total content thereof is within the above range.
[0228] <Light absorber> The resin composition of the present invention preferably contains a compound (light absorber) whose absorbance at the exposure wavelength is reduced by exposure. Examples of the light absorber include the compounds described in paragraphs 0159 to 0183 of WO 2022 / 202647 and the compounds described in paragraphs 0088 to 0108 of JP 2019-206689 A. The contents of these compounds are incorporated herein by reference.
[0229] The content of the light absorber relative to the total solid content of the resin composition of the present invention is not particularly limited, but is preferably 0.1 to 20 mass%, more preferably 0.5 to 10 mass%, and even more preferably 1 to 5 mass%.
[0230] <Other Additives> The resin composition of the present invention may contain various additives, as needed, within the scope of obtaining the effects of the present invention, such as surfactants, higher fatty acid derivatives, thermal polymerization initiators, inorganic particles, ultraviolet absorbers, organic titanium compounds, antioxidants, photoacid generators, anti-aggregation agents, phenolic compounds, other polymer compounds, plasticizers, and other auxiliary agents (e.g., antifoaming agents, flame retardants, etc.). By appropriately incorporating these components, it is possible to adjust properties such as film physical properties. For details of these components, please refer to, for example, the descriptions in paragraphs 0183 and after of JP 2012-003225 A (corresponding to paragraph 0237 of U.S. Patent Application Publication No. 2013 / 0034812 ), and the descriptions in paragraphs 0101 to 0104 and 0107 to 0109 of JP 2008-250074 A, the contents of which are incorporated herein by reference. When these additives are blended, the total content thereof is preferably 3% by mass or less of the solid content of the resin composition of the present invention. Examples of these other additives include the compounds described in paragraphs 0316 to 0358 of WO 2022 / 145355. The above descriptions are incorporated herein by reference.
[0231] <Characteristics of Resin Composition> The viscosity of the resin composition of the present invention can be adjusted by the solid content concentration of the resin composition. 2 / s~12,000mm 2 / s is preferred, and 2,000 mm 2 / s~10,000mm 2 / s is more preferable, and 2,500 mm 2 / s~8,000mm 2 Within the above range, it is easy to obtain a highly uniform coating film. 2 If the thickness is more than 12,000 mm / s, it is easy to apply the coating to a thickness required for an insulating film for rewiring, for example. 2 If the viscosity is less than 1 / s, a coating film with excellent surface condition can be obtained.
[0232] <Restrictions on substances contained in the resin composition> The water content of the resin composition of the present invention is preferably less than 2.0% by mass, more preferably less than 1.5% by mass, and even more preferably less than 1.0% by mass. If it is less than 2.0%, the storage stability of the resin composition is improved. Methods for maintaining the water content include adjusting the humidity under storage conditions and reducing the porosity of the storage container during storage.
[0233] From the viewpoint of insulating properties, the metal content of the resin composition of the present invention is preferably less than 5 mass ppm (parts per million), more preferably less than 1 mass ppm, and even more preferably less than 0.5 mass ppm. Examples of metals include sodium, potassium, magnesium, calcium, iron, copper, chromium, and nickel, but metals contained as complexes of organic compounds and metals are excluded. When multiple metals are contained, the total amount of these metals is preferably within the above range.
[0234] Furthermore, examples of methods for reducing metal impurities unintentionally contained in the resin composition of the present invention include selecting raw materials with a low metal content as raw materials for constituting the resin composition of the present invention, filtering the raw materials for constituting the resin composition of the present invention, and lining the inside of the apparatus with polytetrafluoroethylene or the like to perform distillation under conditions that minimize contamination as much as possible.
[0235] Considering the use of the resin composition of the present invention as a semiconductor material, the content of halogen atoms is preferably less than 500 ppm by mass, more preferably less than 300 ppm by mass, and even more preferably less than 200 ppm by mass, from the viewpoint of wiring corrosion. In particular, those present in the form of halogen ions are preferably less than 5 ppm by mass, more preferably less than 1 ppm by mass, and even more preferably less than 0.5 ppm by mass. Examples of halogen atoms include chlorine atoms and bromine atoms. It is preferable that the total of chlorine atoms and bromine atoms, or chlorine ions and bromine ions, is within the above-mentioned range. Preferred methods for adjusting the content of halogen atoms include ion exchange treatment.
[0236] A conventionally known container can be used as a container for storing the resin composition of the present invention. For the purpose of preventing impurities from being mixed into the raw materials or the resin composition of the present invention, it is also preferable to use a multi-layer bottle whose inner wall is made of six types of six resin layers, or a bottle with a seven-layer structure made of six types of resin. Examples of such containers include the container described in JP 2015-123351 A.
[0237] <Cured Product of Resin Composition> A cured product of the resin composition can be obtained by curing the resin composition of the present invention. The cured product of the present invention is a cured product obtained by curing the resin composition. The resin composition is preferably cured by heating, with a heating temperature of 120°C to 400°C being more preferred, 140°C to 380°C being even more preferred, and 170°C to 350°C being particularly preferred. The form of the cured product of the resin composition is not particularly limited and can be selected depending on the application, such as a film, rod, sphere, or pellet. In the present invention, the cured product is preferably in the form of a film. By patterning the resin composition, the shape of the cured product can be selected depending on the application, such as forming a protective film on a wall surface, forming via holes for electrical conductivity, adjusting impedance, capacitance, or internal stress, or imparting heat dissipation functionality. The film thickness of the cured product (film made of the cured product) is preferably 0.5 μm or more and 150 μm or less. Another preferred embodiment of the present invention is a film of the cured product with a thickness of less than 10 μm. In the above embodiment, the thickness is preferably 0.5 μm or more, and more preferably 1.0 μm or more. The shrinkage percentage when the resin composition of the present invention is cured is preferably 50% or less, more preferably 45% or less, and even more preferably 40% or less. Here, the shrinkage percentage refers to the percentage of volume change before and after curing of the resin composition, and can be calculated using the following formula: Shrinkage percentage [%] = 100 - (volume after curing / volume before curing) x 100
[0238] <Characteristics of cured product of resin composition> The imidization reaction rate of the cured product of the resin composition of the present invention is preferably 70% or more, more preferably 80% or more, and even more preferably 90% or more. If it is 70% or more, the cured product may have excellent mechanical properties. The elongation at break of the cured product of the resin composition of the present invention is preferably 30% or more, more preferably 40% or more, and even more preferably 50% or more. The glass transition temperature (Tg) of the cured product of the resin composition of the present invention is preferably 180°C or more, more preferably 210°C or more, and even more preferably 230°C or more.
[0239] <Preparation of Resin Composition> The resin composition of the present invention can be prepared by mixing the above-mentioned components. The mixing method is not particularly limited, and can be carried out by a conventionally known method. Examples of the mixing method include mixing with a stirring blade, mixing with a ball mill, and mixing by rotating a tank. The temperature during mixing is preferably 10 to 30°C, more preferably 15 to 25°C.
[0240] Filtration using a filter is preferably performed to remove foreign matter such as dust and fine particles from the resin composition of the present invention. The filter pore size is, for example, preferably 5 μm or less, more preferably 1 μm or less, even more preferably 0.5 μm or less, and even more preferably 0.1 μm or less. The filter material is preferably polytetrafluoroethylene, polyethylene, or nylon. When the filter material is polyethylene, HDPE (high-density polyethylene) is more preferable. The filter may be pre-washed with an organic solvent. In the filter filtration process, multiple types of filters may be connected in series or parallel. When multiple types of filters are used, filters with different pore sizes or materials may be combined. An example of a connection mode is a mode in which an HDPE filter with a pore size of 1 μm is connected in series as the first stage and an HDPE filter with a pore size of 0.2 μm is connected in series as the second stage. Various materials may also be filtered multiple times. When filtration is performed multiple times, circulating filtration may be used. Filtration may also be performed under pressure. When filtering under pressure, the pressure to be applied is preferably 0.01 MPa or more and 1.0 MPa or less, more preferably 0.03 MPa or more and 0.9 MPa or less, even more preferably 0.05 MPa or more and 0.7 MPa or less, and even more preferably 0.05 MPa or more and 0.5 MPa or less. In addition to filtering using a filter, a process of removing impurities using an adsorbent may be performed. Filter filtration and a process of removing impurities using an adsorbent may be combined. Known adsorbents can be used as the adsorbent. Examples include inorganic adsorbents such as silica gel and zeolite, and organic adsorbents such as activated carbon. After filtering using a filter, the resin composition filled in a bottle may be subjected to a degassing process by placing it under reduced pressure.
[0241] (Method for producing a cured product) The method for producing a cured product of the present invention preferably includes a film-forming step in which a resin composition is applied to a substrate to form a film. The method for producing a cured product more preferably includes the film-forming step, an exposure step in which the film formed in the film-forming step is selectively exposed to light, and a development step in which the film exposed in the exposure step is developed using a developer to form a pattern. The method for producing a cured product particularly preferably includes the film-forming step, the exposure step, the development step, and at least one of a heating step in which the pattern obtained in the development step is heated and a post-development exposure step in which the pattern obtained in the development step is exposed to light. The method for producing a cured product also preferably includes the film-forming step and a step of heating the film. Details of each step are described below.
[0242] <Film Forming Step> The resin composition of the present invention can be used in a film forming step of applying the resin composition to a substrate to form a film. The method for producing a cured product of the present invention preferably includes a film forming step of applying the resin composition to a substrate to form a film.
[0243] [Substrate] The type of substrate can be appropriately determined depending on the application and is not particularly limited. Examples of substrates include semiconductor production substrates such as silicon, silicon nitride, polysilicon, silicon oxide, and amorphous silicon, quartz, glass, optical films, ceramic materials, vapor deposition films, magnetic films, reflective films, metal substrates such as Ni, Cu, Cr, and Fe (for example, substrates formed from metal and substrates on which a metal layer is formed by, for example, plating or vapor deposition), paper, SOG (Spin On Glass), TFT (Thin Film Transistor) array substrates, mold substrates, and plasma display panel (PDP) electrode plates. Substrates are particularly preferably semiconductor production substrates, with silicon substrates, Cu substrates, and mold substrates being more preferred. These substrates may have a surface layer such as an adhesion layer or an oxide layer formed by hexamethyldisilazane (HMDS) or the like. The shape of the substrate is not particularly limited and may be circular or rectangular. The size of the substrate is preferably, for example, a diameter of 100 to 450 mm, more preferably 200 to 450 mm, if it is circular. If it is rectangular, the length of the short side is preferably, for example, 100 to 1000 mm, more preferably 200 to 700 mm. As the substrate, for example, a plate-shaped, preferably a panel-shaped substrate (substrate) is used.
[0244] When a film is formed by applying a resin composition to the surface of a resin layer (for example, a layer made of a cured product) or the surface of a metal layer, the resin layer or the metal layer serves as the substrate.
[0245] Coating is preferred as a means for applying the resin composition to a substrate. Specific application methods include dip coating, air knife coating, curtain coating, wire bar coating, gravure coating, extrusion coating, spray coating, spin coating, slit coating, and inkjet coating. From the viewpoint of uniformity of film thickness, spin coating, slit coating, spray coating, or inkjet coating is preferred, and from the viewpoint of uniformity of film thickness and productivity, spin coating and slit coating are more preferred. By adjusting the solid content concentration of the resin composition and coating conditions depending on the application method, a film of the desired thickness can be obtained. In addition, the coating method can be appropriately selected depending on the shape of the substrate. For circular substrates such as wafers, spin coating, spray coating, inkjet coating, etc. are preferred, and for rectangular substrates, slit coating, spray coating, inkjet coating, etc. are preferred. In the case of spin coating, for example, it can be applied at a rotation speed of 500 to 3,500 rpm for about 10 seconds to 3 minutes. Alternatively, a method can be used in which a coating film formed by applying the coating composition to a temporary support using the above-described application method is transferred onto the substrate. Regarding the transfer method, the preparation methods described in paragraphs 0023 and 0036 to 0051 of JP-A No. 2006-023696 and paragraphs 0096 to 0108 of JP-A No. 2006-047592 can be suitably used. A step of removing excess film from the edge of the substrate may also be performed. Examples of such a step include edge bead rinsing (EBR) and back rinsing. A pre-wetting step may also be employed in which various solvents are applied to the substrate before applying the resin composition to improve the wettability of the substrate.
[0246] <Drying Step> After the film-forming step (layer-forming step), the film may be subjected to a step (drying step) of drying the formed film (layer) to remove the solvent. That is, the method for producing a cured product of the present invention may include a drying step of drying the film formed in the film-forming step. The drying step is preferably carried out after the film-forming step and before the exposure step. The drying temperature of the film in the drying step is preferably 50 to 150°C, more preferably 70 to 130°C, and even more preferably 90 to 110°C. Drying may also be carried out under reduced pressure. The drying time is, for example, 30 seconds to 20 minutes, preferably 1 to 10 minutes, and more preferably 2 to 7 minutes.
[0247] <Exposure Step> The film may be subjected to an exposure step in which the film is selectively exposed to light. The method for producing a cured product may include an exposure step in which the film formed in the film formation step is selectively exposed to light. Selective exposure means that a portion of the film is exposed to light. Furthermore, selective exposure forms exposed regions (exposed portions) and unexposed regions (unexposed portions) in the film. The exposure dose is not particularly limited as long as it can cure the resin composition of the present invention, but for example, it is 50 to 10,000 mJ / cm2 in terms of exposure energy at a wavelength of 365 nm. 2 is preferred, and 200 to 8,000 mJ / cm 2 is more preferred.
[0248] The exposure wavelength can be appropriately determined within the range of 190 to 1,000 nm, and is preferably 240 to 550 nm.
[0249] The exposure wavelengths, in relation to the light source, are: (1) semiconductor laser (wavelengths 830 nm, 532 nm, 488 nm, 405 nm, 375 nm, 355 nm, etc.); (2) metal halide lamp; (3) high-pressure mercury lamp, g-line (wavelength 436 nm), h-line (wavelength 405 nm), i-line (wavelength 365 nm), broad (three wavelengths of g, h, and i-line); (4) excimer laser, KrF excimer laser (wavelength 248 nm), ArF excimer laser (wavelength 193 nm), F 2Examples of such light include excimer laser (wavelength 157 nm), (5) extreme ultraviolet light; EUV (wavelength 13.6 nm), (6) electron beam, and (7) YAG laser second harmonic 532 nm and third harmonic 355 nm. For the resin composition of the present invention, exposure with a high-pressure mercury lamp is particularly preferred, and exposure with i-line is more preferred from the viewpoint of exposure sensitivity. The exposure method is not particularly limited as long as it is a method that exposes at least a portion of the film made of the resin composition of the present invention, and examples thereof include exposure using a photomask and exposure by laser direct imaging.
[0250] <Post-Exposure Bake Step> The film may be subjected to a heating step (post-exposure bake step) after exposure. That is, the method for producing a cured product of the present invention may include a post-exposure bake step in which the film exposed in the exposure step is heated. The post-exposure bake step can be carried out after the exposure step and before the development step. The heating temperature in the post-exposure bake step is preferably 50°C to 140°C, more preferably 60°C to 120°C. The heating time in the post-exposure bake step is preferably 30 seconds to 300 minutes, more preferably 1 minute to 10 minutes. The temperature rise rate in the post-exposure bake step from the temperature at the start of heating to the maximum heating temperature is preferably 1 to 12°C / min, more preferably 2 to 10°C / min, and even more preferably 3 to 10°C / min. The temperature rise rate may also be changed as appropriate during heating. The heating means in the post-exposure bake step is not particularly limited, and known hot plates, ovens, infrared heaters, etc. may be used. It is also preferable to carry out the heating in an atmosphere of low oxygen concentration by flowing an inert gas such as nitrogen, helium, or argon.
[0251] <Development step> The above-mentioned film after exposure may be subjected to a development step in which it is developed using a developer to form a pattern. That is, the method for producing a cured product of the present invention may include a development step in which the film exposed in the exposure step is developed using a developer to form a pattern. By carrying out development, one of the exposed and unexposed parts of the film is removed to form a pattern. Here, development in which the unexposed parts of the film are removed in the development step is called negative development, and development in which the exposed parts of the film are removed in the development step is called positive development.
[0252] [Developer] The developer used in the development step may be an aqueous alkaline solution or a developer containing an organic solvent.
[0253] When the developer is an alkaline aqueous solution, examples of the basic compound that can be contained in the alkaline aqueous solution include inorganic alkalis, primary amines, secondary amines, tertiary amines, and quaternary ammonium salts. Preferred are TMAH (tetramethylammonium hydroxide), potassium hydroxide, sodium carbonate, sodium hydroxide, sodium silicate, sodium metasilicate, ammonia, ethylamine, n-propylamine, diethylamine, di-n-butylamine, triethylamine, methyldiethylamine, dimethylethanolamine, triethanolamine, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, tetrapentylammonium hydroxide, tetrahexylammonium hydroxide, tetraoctylammonium hydroxide, ethyltrimethylammonium hydroxide, butyltrimethylammonium hydroxide, methyltriamylammonium hydroxide, dibutyldipentylammonium hydroxide, dimethylbis(2-hydroxyethyl)ammonium hydroxide, trimethylphenylammonium hydroxide, trimethylbenzylammonium hydroxide, triethylbenzylammonium hydroxide, pyrrole, and piperidine, and more preferred is TMAH. The content of the basic compound in the developer is preferably from 0.01 to 10% by mass, more preferably from 0.1 to 5% by mass, and even more preferably from 0.3 to 3% by mass, based on the total mass of the developer.
[0254] When the developer contains an organic solvent, the organic solvent may be a compound described in paragraph
[0387] of WO 2021 / 112189, the contents of which are incorporated herein by reference. Suitable examples of alcohols include methanol, ethanol, propanol, isopropanol, butanol, pentanol, octanol, diethylene glycol, propylene glycol, methyl isobutyl carbinol, and triethylene glycol, and suitable examples of amides include N-methylpyrrolidone, N-ethylpyrrolidone, and dimethylformamide.
[0255] When the developer contains an organic solvent, the organic solvent may be used alone or in combination. In the present invention, a developer containing at least one selected from the group consisting of cyclopentanone, γ-butyrolactone, dimethyl sulfoxide, N-methyl-2-pyrrolidone, and cyclohexanone is particularly preferred, a developer containing at least one selected from the group consisting of cyclopentanone, γ-butyrolactone, and dimethyl sulfoxide is more preferred, and a developer containing cyclopentanone is particularly preferred.
[0256] When the developer contains an organic solvent, the content of the organic solvent relative to the total mass of the developer is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more. Alternatively, the content may be 100% by mass.
[0257] When the developer contains an organic solvent, the developer may further contain at least one of a basic compound and a base generator. When at least one of the basic compound and the base generator in the developer permeates into the pattern, the performance of the pattern, such as breaking elongation, may be improved.
[0258] As the basic compound, from the viewpoint of reliability when it remains in the film after curing (adhesion to the substrate when the cured product is further heated), an organic base is preferred. As the basic compound, a basic compound having an amino group is preferred, and primary amines, secondary amines, tertiary amines, ammonium salts, tertiary amides, etc. are preferred. However, to promote the imidization reaction, primary amines, secondary amines, tertiary amines, or ammonium salts are preferred, secondary amines, tertiary amines, or ammonium salts are more preferred, secondary amines or tertiary amines are even more preferred, and tertiary amines are particularly preferred. As the basic compound, from the viewpoint of the mechanical properties (elongation at break) of the cured product, it is preferred that it is difficult for the amount remaining to decrease before heating due to vaporization, etc., is preferred. Therefore, the boiling point of the basic compound is preferably 30°C to 350°C at normal pressure (101,325 Pa), more preferably 80°C to 270°C, and even more preferably 100°C to 230°C. The boiling point of the basic compound is preferably higher than the temperature obtained by subtracting 20° C. from the boiling point of the organic solvent contained in the developer, and more preferably higher than the boiling point of the organic solvent contained in the developer. For example, when the boiling point of the organic solvent is 100° C., the boiling point of the basic compound used is preferably 80° C. or higher, and more preferably 100° C. or higher. The developer may contain only one type of basic compound, or may contain two or more types.
[0259] Specific examples of the basic compound include ethanolamine, diethanolamine, triethanolamine, ethylamine, diethylamine, triethylamine, hexylamine, dodecylamine, cyclohexylamine, cyclohexylmethylamine, cyclohexyldimethylamine, aniline, N-methylaniline, N,N-dimethylaniline, diphenylamine, pyridine, butylamine, isobutylamine, dibutylamine, tributylamine, dicyclohexylamine, DBU (diazabicycloundecene), DABCO (1,4-diazabicyclo[2.2.2]octane), N,N-diisopropylethylamine, tetramethylammonium hydroxide, tetrabutylammonium hydroxide, ethylenediamine, butanediamine, 1,5-diamino Examples of the alkyl ester include pentane, N-methylhexylamine, N-methyldicyclohexylamine, trioctylamine, N-ethylethylenediamine, N,N-diethylethylenediamine, N,N,N',N'-tetrabutyl-1,6-hexanediamine, spermidine, diaminocyclohexane, bis(2-methoxyethyl)amine, piperidine, methylpiperidine, dimethylpiperidine, piperazine, tropane, N-phenylbenzylamine, 1,2-dianilinoethane, 2-aminoethanol, toluidine, aminophenol, hexylaniline, phenylenediamine, phenylethylamine, dibenzylamine, pyrrole, N-methylpyrrole, N,N,N,N-tetramethylethylenediamine, and N,N,N,N-tetramethyl-1,3-propanediamine.
[0260] The preferred embodiments of the base generator are the same as those of the base generator contained in the composition described above. In particular, the base generator is preferably a thermal base generator.
[0261] When the developer contains at least one of a basic compound and a base generator, the content of the basic compound or base generator is preferably 10% by mass or less, more preferably 5% by mass or less, based on the total mass of the developer. The lower limit of the content is not particularly limited, but is preferably, for example, 0.1% by mass or more. When the basic compound or base generator is solid in the environment in which the developer is used, the content of the basic compound or base generator is also preferably 70 to 100% by mass, based on the total solid content of the developer. The developer may contain only one type of basic compound or base generator, or two or more types. When two or more types of at least one of the basic compound and base generator are used, the total content thereof is preferably within the above-mentioned range.
[0262] The developer may further contain other components, such as known surfactants and known defoaming agents.
[0263] [Method of Supplying Developer] The method of supplying the developer is not particularly limited as long as it can form the desired pattern, and includes a method of immersing a substrate on which a film has been formed in the developer, puddle development in which the developer is supplied to the film formed on the substrate using a nozzle, and a method of continuously supplying the developer. The type of nozzle is not particularly limited, and examples include a straight nozzle, a shower nozzle, and a spray nozzle. From the viewpoints of the permeability of the developer, the removability of non-image areas, and production efficiency, a method of supplying the developer using a straight nozzle or a method of continuously supplying the developer using a spray nozzle is preferred, and from the viewpoint of the permeability of the developer to the image areas, a method of supplying using a spray nozzle is more preferred. In addition, a process may be adopted in which the developer is continuously supplied using a straight nozzle, the substrate is spun to remove the developer from the substrate, and after spin drying, the developer is continuously supplied again using a straight nozzle, and the substrate is spun to remove the developer from the substrate, or this process may be repeated multiple times. Methods of supplying the developer in the development process include a process in which the developer is continuously supplied to the substrate, a process in which the developer is kept substantially stationary on the substrate, a process in which the developer is vibrated on the substrate using ultrasound or the like, and a combination thereof.
[0264] The development time is preferably 10 seconds to 10 minutes, more preferably 20 seconds to 5 minutes. The temperature of the developer during development is not particularly limited, but is preferably 10 to 45°C, more preferably 18 to 30°C.
[0265] In the developing step, after the treatment with the developer, the pattern may be further washed (rinsed) with a rinse liquid. Alternatively, a method may be employed in which a rinse liquid is supplied before the developer in contact with the pattern is completely dried.
[0266] [Rinse Liquid] When the developer is an alkaline aqueous solution, for example, water can be used as the rinse liquid. When the developer is a developer containing an organic solvent, for example, a solvent different from the solvent contained in the developer (for example, water, an organic solvent different from the organic solvent contained in the developer) can be used as the rinse liquid.
[0267] When the rinse solution contains an organic solvent, examples of the organic solvent include the same organic solvents as those exemplified when the developer contains an organic solvent. The organic solvent contained in the rinse solution is preferably different from the organic solvent contained in the developer, and more preferably an organic solvent that has a lower solubility for the pattern than the organic solvent contained in the developer.
[0268] When the rinse solution contains an organic solvent, the organic solvent may be used alone or in combination of two or more. The organic solvent is preferably cyclopentanone, γ-butyrolactone, dimethyl sulfoxide, N-methylpyrrolidone, cyclohexanone, PGMEA, or PGME, more preferably cyclopentanone, γ-butyrolactone, dimethyl sulfoxide, PGMEA, or PGME, and even more preferably cyclohexanone or PGMEA.
[0269] When the rinse solution contains an organic solvent, the organic solvent preferably accounts for 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more of the total mass of the rinse solution, and may also account for 100% by mass of the total mass of the rinse solution.
[0270] The rinse solution may contain at least one of a basic compound and a base generator. Although not particularly limited, when the developer contains an organic solvent, an embodiment in which the rinse solution contains the organic solvent and at least one of a basic compound and a base generator is also one of the preferred embodiments of the present invention. Examples of the basic compound and base generator contained in the rinse solution include the compounds exemplified as the basic compound and base generator that may be contained when the developer contains an organic solvent, and the same applies to preferred embodiments. The basic compound and base generator contained in the rinse solution may be selected taking into consideration the solubility in the solvent in the rinse solution, etc.
[0271] When the rinse solution contains at least one of a basic compound and a base generator, the content of the basic compound or base generator is preferably 10% by mass or less, and more preferably 5% by mass or less, based on the total mass of the rinse solution. The lower limit of the content is not particularly limited, but is preferably 0.1% by mass or more, for example. When the basic compound or base generator is solid in the environment in which the rinse solution is used, the content of the basic compound or base generator is also preferably 70 to 100% by mass, based on the total solid content of the rinse solution. When the rinse solution contains at least one of a basic compound and a base generator, the rinse solution may contain only one type of at least one of the basic compound and the base generator, or may contain two or more types. When at least one of the basic compound and the base generator is two or more types, the total content thereof is preferably within the above-mentioned range.
[0272] The rinse liquid may further contain other components, such as known surfactants and known defoaming agents.
[0273] [Method of Supplying Rinse Liquid] The method of supplying the rinse liquid is not particularly limited as long as it can form a desired pattern, and examples thereof include a method of immersing the substrate in the rinse liquid, a method of supplying the rinse liquid to the substrate by puddling, a method of supplying the rinse liquid to the substrate by showering, and a method of continuously supplying the rinse liquid onto the substrate by means of a straight nozzle or the like. From the viewpoints of the permeability of the rinse liquid, the removability of non-image areas, and production efficiency, methods of supplying the rinse liquid using a shower nozzle, straight nozzle, spray nozzle, etc. are available, and a method of continuously supplying using a spray nozzle is preferred, and from the viewpoint of the permeability of the rinse liquid into the image areas, a method of supplying using a spray nozzle is more preferred. The type of nozzle is not particularly limited, and examples include a straight nozzle, shower nozzle, spray nozzle, etc. That is, the rinsing step is preferably a step of supplying or continuously supplying the rinse liquid to the exposed film using a straight nozzle, and more preferably a step of supplying the rinse liquid using a spray nozzle. The method of supplying the rinse liquid in the rinsing step may include a step of continuously supplying the rinse liquid to the substrate, a step of keeping the rinse liquid substantially stationary on the substrate, a step of vibrating the rinse liquid on the substrate by ultrasonic waves or the like, and a combination of these steps.
[0274] The rinsing time is preferably 10 seconds to 10 minutes, more preferably 20 seconds to 5 minutes. The temperature of the rinsing liquid during rinsing is not particularly limited, but is preferably 10 to 45°C, more preferably 18 to 30°C.
[0275] The developing step may include a step of contacting the pattern with a treatment liquid after treatment with a developer or after washing the pattern with a rinse liquid. Alternatively, a method may be employed in which the treatment liquid is supplied before the developer or rinse liquid in contact with the pattern is completely dried.
[0276] The treatment liquid may include a treatment liquid containing at least one of water and an organic solvent, and at least one of a basic compound and a base generator. Preferred aspects of the organic solvent, the basic compound, and the base generator are the same as the preferred aspects of the organic solvent, the basic compound, and the base generator used in the rinse liquid described above. The treatment liquid can be supplied to the pattern using the same method as the rinse liquid described above, and preferred aspects are also the same.
[0277] The content of the basic compound or base generator in the treatment liquid is preferably 10% by mass or less, and more preferably 5% by mass or less, relative to the total mass of the treatment liquid. There is no particular limitation on the lower limit of the content, but it is preferably, for example, 0.1% by mass or more. Furthermore, when the basic compound or base generator is solid in the environment in which the treatment liquid is used, the content of the basic compound or base generator is also preferably 70 to 100% by mass, relative to the total solid content of the treatment liquid. When the treatment liquid contains at least one of a basic compound and a base generator, the treatment liquid may contain only one type of at least one of the basic compound and the base generator, or may contain two or more types. When there are two or more types of at least one of the basic compound and the base generator, it is preferable that the total amount thereof is within the above-mentioned range.
[0278] <Heating Step> The pattern obtained by the development step (or the pattern after rinsing, if a rinsing step is performed) may be subjected to a heating step in which the pattern obtained by the development step is heated. That is, the method for producing a cured product of the present invention may include a heating step in which the pattern obtained by the development step is heated. Furthermore, the method for producing a cured product of the present invention may include a heating step in which a pattern obtained by another method without performing a development step, or a film obtained by a film formation step, is heated. In the heating step, a resin such as a polyimide precursor is cyclized to form a resin such as a polyimide. Furthermore, crosslinking of unreacted crosslinkable groups in the heterocycle-containing polymer precursor or a crosslinking agent other than the heterocycle-containing polymer precursor also proceeds. The heating temperature (maximum heating temperature) in the heating step is preferably 50 to 450°C, more preferably 150 to 350°C, even more preferably 150 to 250°C, even more preferably 160 to 250°C, and particularly preferably 160 to 230°C.
[0279] The heating step is preferably a step in which the cyclization reaction of the polyimide precursor is promoted within the pattern by the action of a base or the like generated from the base generator due to heating.
[0280] The heating step is preferably carried out at a temperature increase rate of 1 to 12°C / min from the temperature at the start of heating to the maximum heating temperature. The temperature increase rate is more preferably 2 to 10°C / min, and even more preferably 3 to 10°C / min. By setting the temperature increase rate to 1°C / min or more, it is possible to prevent excessive volatilization of the acid or solvent while ensuring productivity, and by setting the temperature increase rate to 12°C / min or less, it is possible to alleviate residual stress in the cured product. In addition, in the case of an oven capable of rapid heating, it is preferable to increase the temperature from the temperature at the start of heating to the maximum heating temperature at a temperature increase rate of 1 to 8°C / sec, more preferably 2 to 7°C / sec, and even more preferably 3 to 6°C / sec.
[0281] The temperature at the start of heating is preferably 20°C to 150°C, more preferably 20°C to 130°C, and even more preferably 25°C to 120°C. The temperature at the start of heating refers to the temperature at the start of the process of heating up to the maximum heating temperature. For example, when the resin composition of the present invention is applied to a substrate and then dried, the temperature is the temperature of the film (layer) after this drying, and it is preferable to raise the temperature from, for example, a temperature 30 to 200°C lower than the boiling point of the solvent contained in the resin composition.
[0282] The heating time (heating time at the maximum heating temperature) is preferably from 5 to 360 minutes, more preferably from 10 to 300 minutes, and even more preferably from 15 to 240 minutes.
[0283] In particular, when forming a multilayer laminate, from the viewpoint of interlayer adhesion, the heating temperature is preferably 30° C. or higher, more preferably 80° C. or higher, even more preferably 100° C. or higher, and particularly preferably 120° C. or higher. The upper limit of the heating temperature is preferably 350° C. or lower, more preferably 250° C. or lower, and even more preferably 240° C. or lower.
[0284] Heating may be performed in stages. For example, the temperature may be increased from 25°C to 120°C at a rate of 3°C / min, held at 120°C for 60 minutes, increased from 120°C to 180°C at a rate of 2°C / min, and held at 180°C for 120 minutes. It is also preferable to treat the film while irradiating it with ultraviolet light, as described in U.S. Pat. No. 9,159,547. Such a pretreatment step can improve the film's properties. The pretreatment step may be performed for a short period of time, preferably from 10 seconds to 2 hours, more preferably from 15 seconds to 30 minutes. The pretreatment step may be performed in two or more steps. For example, a first pretreatment step may be performed in the range of 100 to 150°C, followed by a second pretreatment step in the range of 150 to 200°C. Furthermore, cooling may be performed after heating. In this case, the cooling rate is preferably from 1 to 5°C / min.
[0285] The heating step is preferably carried out in an atmosphere of low oxygen concentration by flowing an inert gas such as nitrogen, helium, or argon, or by carrying out the heating step under reduced pressure, in order to prevent decomposition of the heterocycle-containing polymer precursor. The oxygen concentration is preferably 50 ppm (volume ratio) or less, more preferably 20 ppm (volume ratio) or less. The heating means in the heating step is not particularly limited, and examples thereof include a hot plate, an infrared oven, an electric heating oven, a hot air oven, and an infrared oven.
[0286] <Post-development exposure step> The pattern obtained in the development step (if a rinsing step is performed, the pattern after rinsing) may be subjected to a post-development exposure step in which the pattern obtained in the development step is exposed to light, instead of or in addition to the heating step. That is, the method for producing a cured product of the present invention may include a post-development exposure step in which the pattern obtained in the development step is exposed to light. The method for producing a cured product of the present invention may include a heating step and a post-development exposure step, or may include only one of the heating step and the post-development exposure step. The post-development exposure step can promote, for example, a reaction in which cyclization of a polyimide precursor or the like progresses due to exposure of a photobase generator, or a reaction in which elimination of an acid-decomposable group progresses due to exposure of a photoacid generator. In the post-development exposure step, it is sufficient that at least a portion of the pattern obtained in the development step is exposed, but it is preferable that the entire pattern is exposed. The exposure dose in the post-development exposure step is 50 to 20,000 mJ / cm in terms of exposure energy at a wavelength to which the photosensitive compound has sensitivity. 2 is preferred, and 100 to 15,000 mJ / cm 2 The post-development exposure step can be carried out using, for example, the light source used in the exposure step described above, and it is preferable to use broadband light.
[0287] <Metal Layer Forming Step> The pattern obtained by the developing step (preferably subjected to at least one of a heating step and a post-development exposure step) may be subjected to a metal layer forming step of forming a metal layer on the pattern. That is, the method for producing a cured product of the present invention preferably includes a metal layer forming step of forming a metal layer on the pattern obtained by the developing step (preferably subjected to at least one of a heating step and a post-development exposure step).
[0288] The metal layer is not particularly limited, and existing metal species can be used. Examples include copper, aluminum, nickel, vanadium, titanium, chromium, cobalt, gold, tungsten, tin, silver, and alloys containing these metals. Copper and aluminum are more preferred, and copper is even more preferred.
[0289] The method for forming the metal layer is not particularly limited, and existing methods can be applied. For example, the methods described in JP 2007-157879 A, JP 2001-521288 A, JP 2004-214501 A, JP 2004-101850 A, U.S. Patent No. 7,888,181 B2, and U.S. Patent No. 9,177,926 B2 can be used. Examples of suitable methods include photolithography, PVD (physical vapor deposition), CVD (chemical vapor deposition), lift-off, electroplating, electroless plating, etching, printing, and combinations of these. More specifically, examples include patterning methods that combine sputtering, photolithography, and etching, and patterning methods that combine photolithography and electroplating. Preferred plating methods include electroplating using a copper sulfate or copper cyanide plating solution.
[0290] The thickness of the metal layer is preferably 0.01 to 50 μm, more preferably 1 to 10 μm, at the thickest part.
[0291] <Applications> Fields to which the method for producing a cured product of the present invention or the cured product can be applied include insulating films for electronic devices, interlayer insulating films for rewiring layers, stress buffer films, etc. Other examples include sealing films, substrate materials (base films, coverlays, and interlayer insulating films for flexible printed circuit boards), and the etching of insulating films for packaging applications such as those described above. For these applications, reference can be made to, for example, Science & Technology Co., Ltd.'s "High Performance Polyimide and Application Technology" (April 2008), edited by Masaaki Kakimoto, CMC Technical Library "Fundamentals and Development of Polyimide Materials" (November 2011), and Japan Polyimide and Aromatic Polymer Research Association's "Latest Polyimide Fundamentals and Applications" (NTS, August 2010).
[0292] The method for producing the cured product of the present invention, or the cured product of the present invention, can also be used for producing printing plates such as offset printing plates or screen printing plates, for etching molded parts, for producing protective lacquers and dielectric layers in electronics, especially microelectronics, etc.
[0293] (Laminate and method for manufacturing laminate) The laminate of the present invention refers to a structure having a plurality of layers each made of the cured product of the present invention. The laminate is a laminate including two or more layers each made of the cured product, and may be a laminate including three or more layers. At least one of the two or more layers each made of the cured product contained in the laminate is a layer made of the cured product of the present invention, and from the viewpoint of suppressing shrinkage of the cured product or deformation of the cured product associated with the shrinkage, it is also preferable that all of the layers made of the cured product contained in the laminate are layers made of the cured product of the present invention.
[0294] That is, the method for producing a laminate of the present invention preferably includes the method for producing a cured product of the present invention, and more preferably includes repeating the method for producing a cured product of the present invention multiple times.
[0295] The laminate of the present invention preferably includes two or more layers made of a cured product and a metal layer between any of the layers made of the cured product. The metal layer is preferably formed by the metal layer-forming step. That is, the method for producing a laminate of the present invention preferably further includes a metal layer-forming step of forming a metal layer on a layer made of a cured product between multiple cured product production processes. A preferred embodiment of the metal layer-forming step is as described above. Examples of the laminate include a laminate having at least a layer structure in which three layers are stacked in this order: a layer made of a first cured product, a metal layer, and a layer made of a second cured product. It is preferred that both the layer made of the first cured product and the layer made of the second cured product are layers made of the cured product of the present invention. The resin composition of the present invention used to form the layer made of the first cured product and the resin composition of the present invention used to form the layer made of the second cured product may have the same composition or different compositions. The metal layer in the laminate of the present invention is preferably used as metal wiring, such as a rewiring layer.
[0296] <Lamination Step> The method for producing a laminate of the present invention preferably includes a lamination step. The lamination step is a series of steps including performing at least one of (a) a film formation step (layer formation step), (b) an exposure step, (c) a development step, and (d) a heating step and a post-development exposure step again on the surface of the pattern (resin layer) or the metal layer in this order. However, at least one of (a) the film formation step and (d) the heating step and the post-development exposure step may be repeated. Furthermore, after at least one of (d) the heating step and the post-development exposure step, (e) a metal layer formation step may be included. It goes without saying that the lamination step may further include the above-mentioned drying step or the like as appropriate.
[0297] When a further lamination step is performed after the lamination step, a surface activation treatment step may be further performed after the exposure step, the heating step, or the metal layer forming step. An example of the surface activation treatment is a plasma treatment. Details of the surface activation treatment will be described later.
[0298] The lamination step is preferably performed 2 to 20 times, more preferably 2 to 9 times. For example, a structure having 2 to 20 resin layers, such as resin layer / metal layer / resin layer / metal layer / resin layer / metal layer, is preferred, and a structure having 2 to 9 resin layers is even more preferred. Each of the layers may be the same or different in composition, shape, film thickness, etc.
[0299] In the present invention, a particularly preferred embodiment is one in which, after providing a metal layer, a cured product (resin layer) of the resin composition of the present invention is further formed so as to cover the metal layer.Specific examples include an embodiment in which the steps of (a) film formation step, (b) exposure step, (c) development step, (d) at least one of a heating step and a post-development exposure step, and (e) metal layer formation step are repeated in this order, or an embodiment in which the steps of (a) film formation step, (d) at least one of a heating step and a post-development exposure step, and (e) metal layer formation step are repeated in this order.By alternately performing the lamination step of laminating the resin composition layer (resin layer) of the present invention and the metal layer formation step, the resin composition layer (resin layer) of the present invention and the metal layer can be alternately laminated.
[0300] (Surface Activation Treatment Step) The method for producing a laminate of the present invention preferably includes a surface activation treatment step in which at least a portion of the metal layer and the resin composition layer are surface-activated. The surface activation treatment step is usually performed after the metal layer formation step, but after the development step (preferably after at least one of the heating step and the post-development exposure step), the resin composition layer may be surface-activated before the metal layer formation step. The surface activation treatment may be performed only on at least a portion of the metal layer, or only on at least a portion of the resin composition layer after exposure, or may be performed on at least a portion of both the metal layer and the resin composition layer after exposure. The surface activation treatment is preferably performed on at least a portion of the metal layer, and it is preferable to perform the surface activation treatment on part or all of the region of the metal layer on which the resin composition layer is to be formed. In this way, by performing the surface activation treatment on the surface of the metal layer, adhesion with the resin composition layer (film) provided on the surface can be improved. The surface activation treatment is also preferably performed on part or all of the resin composition layer (resin layer) after exposure. In this way, by performing the surface activation treatment on the surface of the resin composition layer, adhesion with the metal layer or resin layer provided on the surface that has been surface-activated can be improved. In particular, when negative development is performed, when the resin composition layer is cured, it is less susceptible to damage due to surface treatment and adhesion is likely to be improved. The surface activation treatment can be carried out, for example, by the method described in paragraph 0415 of International Publication No. 2021 / 112189. The contents of this specification are incorporated herein.
[0301] (Semiconductor device and manufacturing method thereof) The present invention also discloses a semiconductor device comprising the cured product or laminate of the present invention. The present invention also discloses a manufacturing method for a semiconductor device comprising the manufacturing method for the cured product or the manufacturing method for the laminate of the present invention. Specific examples of semiconductor devices using the resin composition of the present invention to form an interlayer insulating film for a rewiring layer can be found in paragraphs 0213 to 0218 and FIG. 1 of JP 2016-027357 A, the contents of which are incorporated herein by reference.
[0302] The present invention will be explained in more detail below with reference to examples. The materials, amounts used, ratios, processing details, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. Unless otherwise specified, "parts" and "%" are based on mass.
[0303] <Method for producing heterocycle-containing polymer precursor> [Synthesis Example 1: Synthesis of heterocycle-containing polymer precursor (resin 1)] 23.48 g of 4,4'-oxydiphthalic dianhydride (ODPA) and 22.27 g of bisphthalic dianhydride (BPDA) were placed in a separable flask, and 39.69 g of 2-hydroxyethyl methacrylate (HEMA) and 136.83 g of tetrahydrofuran were added and stirred at room temperature (25°C). 24.66 g of pyridine was added with stirring to obtain a reaction mixture. After the heat generation due to the reaction had ceased, the mixture was allowed to cool to room temperature and left to stand for 16 hours. Next, under ice cooling, a solution of 62.46 g of dicyclohexylcarbodiimide (DCC) dissolved in 61.57 g of tetrahydrofuran was added to the reaction mixture over 40 minutes with stirring, followed by a suspension of 27.42 g of 4,4'-diaminodiphenyl ether (DADPE) in 119.73 g of tetrahydrofuran, which was added over 60 minutes with stirring. After further stirring at room temperature for 2 hours, 7.17 g of ethyl alcohol was added and stirred for 1 hour, followed by the addition of 136.83 g of tetrahydrofuran. The precipitate formed in the reaction mixture was removed by filtration to obtain a reaction solution. The resulting reaction solution was added to 716.21 g of ethyl alcohol to produce a precipitate consisting of a crude polymer. The resulting crude polymer was filtered off and dissolved in 403.49 g of tetrahydrofuran to obtain a crude polymer solution. The resulting crude polymer solution was added dropwise to 8470.26 g of water to precipitate the polymer. The resulting precipitate was filtered off and then vacuum dried to obtain 80.3 g of powdered Resin 1. The molecular weight of Resin 1 was measured by gel permeation chromatography (standard polystyrene equivalent) and found to have a weight average molecular weight (Mw) of 20,000. 1 By H-NMR, it was confirmed that the structure of Resin 1 was a structure represented by the following formula (P-1).
[0304] Synthesis Example 2A: Synthesis of Heterocycle-Containing Polymer Precursor (Resin 2A) 21.2 g of 4,4'-oxydiphthalic anhydride, 18.0 g of 2-hydroxyethyl methacrylate, 23.9 g of pyridine, and 250 mL of diglyme (diethylene glycol dimethyl ether) were mixed and stirred at 60°C for 4 hours to synthesize a diester of 4,4'-oxydiphthalic acid and 2-hydroxyethyl methacrylate. The reaction mixture was then cooled to -10°C, and 17.0 g of thionyl chloride was added over 60 minutes while maintaining the temperature at -10±5°C. After dilution with 50 mL of N-methylpyrrolidone, a solution of 12.6 g of 4,4'-diaminodiphenyl ether in 100 mL of N-methylpyrrolidone was added dropwise to the reaction mixture over 60 minutes at -10±5°C, and the mixture was stirred at room temperature for 2 hours. Thereafter, 10.0 g of ethanol was added and the mixture was stirred at room temperature for 1 hour. Next, 6,000 g of water was added to precipitate the polyimide precursor, and the precipitate (water-polyimide precursor mixture) was stirred for 15 minutes. The precipitate (solid polyimide precursor) after stirring was collected by filtration and dissolved in 500 g of tetrahydrofuran. 6,000 g of water (poor solvent) was added to the resulting solution to precipitate the polyimide precursor, and the precipitate (water-polyimide precursor mixture) was stirred for 15 minutes. The precipitate (solid polyimide precursor) after stirring was again filtered and dried at 45°C under reduced pressure for 3 days. 46.6 g of the dried powder was dissolved in 419.6 g of tetrahydrofuran, and then 2.3 g of triethylamine was added and the mixture was stirred at room temperature for 35 minutes. Then, 3,000 g of ethanol was added, and the precipitate was collected by filtration. The resulting precipitate was dissolved in 281.8 g of tetrahydrofuran. 17.1 g of water and 46.6 g of ion exchange resin UP6040 (AmberTec) were added thereto and stirred for 4 hours. The ion exchange resin was then removed by filtration, and the resulting polymer solution was added to 5,600 g of water to obtain a precipitate. The precipitate was collected by filtration and dried under reduced pressure at 45°C for 24 hours to obtain 45.1 g of resin 2A. 1H-NMR confirmed that the structure of Resin 2A was the structure represented by the following formula (P-2). The molecular weight of Resin 2A was measured by gel permeation chromatography (standard polystyrene equivalent), and the weight average molecular weight (Mw) was found to be 20,000. Furthermore, by appropriately adjusting the equivalent weight of 4,4'-diaminodiphenyl ether, Resin 2A with Mw of 5,000, 8,000, 10,000, 15,000, 30,000, 50,000, or 100,000 was also synthesized.
[0305] Synthesis Example 2B: Synthesis of heterocycle-containing polymer precursor (resin 2B) Resin 2B having a structure represented by the following formula (P-2) was synthesized in the same manner as in Synthesis Example 1, except that the compounds used were appropriately changed. 1 By H-NMR, it was confirmed that the structure of Resin 2B was a structure represented by the following formula (P-2): Mw of Resin 2B was 20,000.
[0306] [Synthesis Examples 3 to 13: Synthesis of heterocycle-containing polymer precursors (resins 3 to 13)] Resins 3 to 13, each having a structure represented by any one of the following formulas (P-3) to (P-13), were synthesized in the same manner as in Synthesis Example 1, except that the compounds used were changed appropriately. The Mw of resins 3 to 13 was all 20,000. 1 By H-NMR, it was confirmed that the structures of Resin 3 to Resin 13 were structures represented by the following formulas (P-3) to (P-13), respectively.
[0307]
[0308] Synthesis Example 14: Synthesis of Polyimide (Resin 14) Synthesis Example AA-1 48.65 g (225 mmol) of 3,3'-dihydroxybenzidine and 375 mL of dimethylformamide were mixed in a 1 L flask. Under ice cooling, 98.21 g (450 mmol) of di-t-butyl dicarbonate was added dropwise. After the addition was complete, the mixture was stirred at 60°C for 5 hours. After the reaction was completed and the mixture was cooled to room temperature, 35 mg of 2,2,6,6-tetramethylpiperidine 1-oxyl free radical, 68.68 g (450 mmol) of p-chloromethylstyrene, 74.63 g (540 mmol) of potassium carbonate, and 8.96 g (54.0 mmol) of potassium iodide were added, and the mixture was stirred at 60°C for 3 hours. After the reaction was completed, the mixture was filtered by suction filtration, and the filtrate was added dropwise to 500 mL of water. White crystals were precipitated, and the precipitated solid was collected by suction filtration. The obtained white solid was purified by recrystallization at 60°C using 1000 mL of acetone. 125 g (yield 85.6%) of the following intermediate AA-1a was obtained. The structure of AA-1a is shown below. 1 This was confirmed by H-NMR spectrum. 1 H-NMR (BRUKER, AVANCE NEO 400): δ(ppm,DMSO-d6)8.04-7.94(s,2H), 7.75-7.64(d,2H), 7.56-7.42(m,8H), 7.27-7.20(d,2H), 7.19-7.12(d,2H), 6.79-6.64(2H), 5.89-5.77(2H), 5.30-5.15(6H), 1.49-1.43(s,18H)
[0309] 75.0 g (115.6 mmol) of (AA-1a) and 500 mL of methylene chloride were mixed in a 1 L flask. 131.8 g (1156 mmol) of trifluoroacetic acid was added at room temperature, and then the mixture was stirred at 40°C for 5 hours. After the reaction was completed, 250 mL of methanol was added dropwise under ice cooling, followed by 117.0 g (1156 mmol) of triethylamine. Pale yellow crystals were precipitated, and the precipitated solid was collected by suction filtration. The precipitate was suspended and washed in 750 mL of methanol, yielding 40.5 g (73% yield) of (AA-1). The structure of AA-1 is shown below. The following structure is 1This was confirmed by H-NMR spectrum. 1 H-NMR (BRUKER, AVANCE NEO 400): δ(ppm,DMSO-d6)7.53-7.45(s,8H), 7.05-6.98(d,2H), 6.92-6.85(d,2H), 6.79-6.63(4H), 5.89-5.78(d,2H), 5.29-5.22(d,2H), 5.20-5.13(s,4H), 4.92-4.64(4H)
[0310] Synthesis Example AT-1 AT-1 was obtained in the same manner as in Synthesis Example AA-1, except that 3,3'-dihydroxybenzidine was replaced with p-methoxyphenol. The structure of AT-1 is shown below. 1 This was confirmed by H-NMR spectrum. 1 H-NMR (BRUKER, AVANCE NEO 400): δ(ppm,DMSO-d6)7.52-7.42(d,2H), 7.42-7.32(d,2H), 6.80-6.63(3H), 6.54-6.43(d,2H), 5.92-5.77(1H), 5.30-5.19(1H), 4.95-4.89(s,2H), 4.68-4.54(2H)
[0311] Synthesis Example 1 Synthesis of Polyimide (Resin 14) 30.0 g (57.64 mmol) of 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride and 0.08 g of 2,2,6,6-tetramethylpiperidine 1-oxyl free radical were dissolved in 120 g of N-methylpyrrolidone (NMP) to obtain a solution. Next, 9.93 g (24.2 mmol) of 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 10.86 g (24.2 mmol) of AA-1, and 1.30 g (5.76 mmol) of AT-1 were dissolved in 100 g of NMP and added dropwise to the above solution over 1 hour at a temperature of 0 to 10 °C. After stirring at 25 °C for 60 minutes, 18.2 g of pyridine and 14.7 g of acetic anhydride were added and reacted at 80 °C for 4 hours. After completion of the reaction, the mixture was cooled to 25 °C and diluted with 200 g of tetrahydrofuran. Next, the reaction solution was added dropwise to a mixture of 2.0 L of methanol and 0.5 L of water, stirred for 15 minutes, and then the polyimide resin was filtered. Next, the resin was reslurried in 1 L of water, filtered, and then reslurried again in 1 L of methanol, filtered, and dried under reduced pressure at 40 °C for 10 hours. Next, the dried resin was dissolved in 250 g of tetrahydrofuran, and 40 g of ion exchange resin (MB-1: manufactured by Organo Corporation) was added and stirred for 4 hours. The ion exchange resin was removed by filtration, and then the polyimide resin was precipitated in 2 liters of methanol and stirred for 15 minutes. The polyimide resin was collected by filtration and dried at 45°C under reduced pressure for 1 day to obtain a polyimide resin (resin 14). The weight average molecular weight of the obtained resin 14 was 20,000. The polyimide (resin 1) is a resin having a repeating unit represented by the following formula (P-14). The structure of the repeating unit is: 1 The molar ratio was determined from the H-NMR spectrum. In the following structure, the subscripts of the repeating units indicate the molar ratio of each repeating unit.
[0312] Examples and Comparative Examples In each example, the components listed in the table below were mixed to obtain a resin composition. In the comparative example, the components listed in the table below were mixed to obtain a comparative composition. Specifically, the content (amount) of each component listed in the table other than the solvent was the amount (parts by mass) listed in the "Parts by Mass" column of each column in the table. The solvent content (amount) was adjusted so that the solids concentration of the composition was the value (% by mass) of "Solids Concentration" in the table, and the ratio (mass ratio) of the content of each solvent to the total mass of solvents was the ratio listed in the "Ratio" column in the table. The obtained resin composition and comparative composition were pressure-filtered using a polytetrafluoroethylene filter with a pore width of 0.8 μm. The "Content X" column lists the content of a compound having at least one of a pyridine structure and a pyridinium salt structure relative to the total mass of the resin composition. In the table, "-" indicates that the composition does not contain the corresponding component.
[0313]
[0314]
[0315]
[0316]
[0317]
[0318]
[0319]
[0320]
[0321]
[0322]
[0323]
[0324]
[0325]
[0326] Details of each component listed in the table are as follows:
[0327] [Resins] Resins 1 to 14: Resins 1 to 14 obtained in the above synthesis examples
[0328] [Monomers (polymerizable compounds)] M-1 to M-4: Compounds having the following structures DPHA: Dipentaerythritol hexaacrylate
[0329] [Polymerization initiators or photoacid generators] I-1 to I-9: Compounds having the following structures
[0330] [Compound A and base generator] A-1 to A-42: Compounds having the following structure, A-1 to A-42 are compounds that fall under Compound A. AR-1 to AR-5: Compounds having the following structure, AR-1 to AR-5 are compounds that do not fall under Compound A.
[0331] Synthesis Example A-11: Synthesis of Compound A-11 In a flask, 2.00 g (9.56 mmol, 1.0 eq.) of methyl 4-formyl-3-nitrobenzoate, 2.22 g (2.0 eq.) of methyl acetoacetate, 1.11 g (1.5 eq.) of ammonium acetate, and 6.88 g (1.1 mol / L) of ethanol were stirred at 80°C and reacted for 6 hours. The solution was air-cooled to room temperature, and the precipitate was removed by filtration under reduced pressure. 20 mL of water was added to the filtrate, and the mixture was extracted three times with 13.0 g of ethyl acetate. The organic layers were combined, and then washed once with an aqueous solution of 1.58 g of sodium thiosulfate dissolved in 20 mL of water, followed by two separate washes with 20 mL of water. The organic layer was dried over sodium sulfate, and the solid was removed by filtration. The solvent was then distilled off under reduced pressure from the filtrate, yielding a crude product. This was purified by silica gel chromatography to obtain 1.59 g of solid A-11 (yield 41%). 1H-NMR (400MHz, DMSO-d6) δ=9.09 (s, 1H), 8.20 (d, 1H, J= 2 Hz), 8.14 (dd, 1H, J= 8 Hz, 2 Hz), 7.64 (d, 1H, J= 8 Hz), 5.56 (s, 1H), 3.86 (s, 3H), 3.44 (s, 6H), 2.26 (s, 6H).
[0332] Furthermore, A-1, A-3, A-4, A-5, A-7, A-8, and A-9 were commercially available from Tokyo Chemical Industry Co., Ltd., A-2 and A-6 were commercially available from Fujifilm Wako Pure Chemical Industries, Ltd., and A-10 and A-12 to A-42 were synthesized by the same method as A-11 described above.
[0333] [Polymerization inhibitors] B-1 to B-5, E-9: Compounds having the following structures
[0334] [Silane Coupling Agents (Metal Adhesion Improvers)] C-1 to C-7: Compounds having the following structures.
[0335] [Migration inhibitors] D-1 to D-3: Compounds having the following structure
[0336] [Additives] E-1 to E-6, E-10 to E-20: Compounds having the following structures E-7: Ester of 2,2',3,3'-tetrahydro-3,3,3',3'-tetramethyl-1,1'-spirobi(1H-indene)-5,5',6,6',7,7'hexanol and 1,2-naphthoquinone-(2)-diazo-5-sulfonic acid E-8: The following synthetic product
[0337] <Additive: Synthesis of Diazonaphthoquinone Compound E-8> 29.72 g (70 mmol) of 4,4'-(1-(2-(4-hydroxyphenyl)-2-propyl)phenyl)ethylidene)bisphenol (Tris-PA, manufactured by Honshu Chemical Industry Co., Ltd.) was added to a flask. Subsequently, 46.93 g (174.9 mmol) of 1,2-naphthoquinone diazide-5-sulfonic acid chloride and 17.9 g of triethylamine were dissolved in 300 g of acetone with stirring, and the solution was added dropwise to the flask using a dropping funnel over 30 minutes, followed by stirring for 30 minutes at an internal temperature of 30°C. Subsequently, hydrochloric acid was added dropwise, and the mixture was stirred for an additional 30 minutes. Next, a solution of 1,640 g of pure water and 30 g of hydrochloric acid was prepared in a beaker, and the filtrate obtained by filtering the hydrochloride salt from the reaction solution was added dropwise to the solution. The precipitate was filtered, washed with water, and vacuum-dried at 40°C for 50 hours to obtain diazonaphthoquinone compound E-8.
[0338] [Solvents] NMP: N-methyl-2-pyrrolidone EL: ethyl lactate DMSO: dimethyl sulfoxide GBL: γ-butyrolactone GVL: γ-valerolactone MDMPA: 3-methoxy-N,N-dimethylpropanamide Toluene: toluene
[0339] <Evaluation> [Evaluation of Adhesion After Heat Resistance Test] The resin composition or comparative composition prepared in each Example and Comparative Example was applied in the form of a layer on a copper substrate by spin coating, to form a resin composition layer or comparative composition layer. The copper substrate on which the obtained resin composition layer or comparative composition layer was formed was dried on a hot plate at 100°C for 5 minutes, to form a resin composition layer or comparative composition layer on the copper substrate with a uniform thickness as shown in the "Film Thickness (µm)" column in the table. The resin composition layer or comparative composition layer on the copper substrate was then heated at 500 mJ / cm 2In the examples marked with "CP" in the "Developer" column of the table, a photomask having a 100-μm square unmasked portion was formed, and in the examples marked with "TMAH" in the "Developer" column of the table, a photomask having a 100-μm square masked portion was formed, and exposure was performed with light having the exposure wavelength (nm) shown in the "Exposure Wavelength (nm)" column of the table. In the examples marked with "M" in the "Exposure Conditions" column, exposure was performed using a stepper as the light source. In the examples marked with "D" in the "Exposure Conditions" column, laser direct imaging exposure was performed over a 100-μm square area using a direct exposure device (Adtec DE-6UH III) as the light source without using a photomask. Thereafter, development was performed for 60 seconds with the developer shown in the table to obtain a 100-μm square resin layer. The "CP" in the table refers to cyclopentanone, and the "TMAH" in the table refers to a 2.38% by mass aqueous solution of tetramethylammonium hydroxide. In the examples where a numerical value is listed in the "Cure Temperature" column, the exposed resin composition layer was heated at a heating rate of 10 ° C. / min under a nitrogen atmosphere using a hot plate. After reaching the temperature listed in the "Cure Temperature (° C.)" column of the table, the temperature was maintained for the "Cure Time (min)" period in the table to obtain a cured product. In the examples where "IR" is listed in the "Cure Temperature (° C.)" column, the resin film obtained in each example was heated at a heating rate of 10 ° C. / min under a nitrogen atmosphere using an infrared lamp heating device (manufactured by Advance Riko Co., Ltd., RTP-6). After reaching 230 ° C., the temperature was maintained for the "Cure Time (min)" period in the table to obtain a cured product. The copper substrate with the obtained cured product was left in a chamber at 175°C under atmospheric pressure for 192 hours. The shear strength of a 100 μm square cured product on the copper substrate was measured using a bond tester (CondorSigma, manufactured by XYZTEC Corporation) in an environment of 25°C and 65% relative humidity (RH), and evaluated according to the following evaluation criteria. The evaluation results are shown in the column "Adhesion after heat resistance test" in the table. The greater the shear strength, the better the adhesion of the cured film after the heat resistance test. -Evaluation criteria- A: The shear strength exceeded 30 gf. B: The shear strength was greater than 25 gf but not more than 30 gf.C: The shear force was greater than 20 gf and not more than 25 gf. D: The shear force was not more than 20 gf. 1 gf is 0.00980665 N.
[0340] [Evaluation of Resolution] In each Example and Comparative Example, a cured product was obtained in the same manner as in the "Evaluation of Adhesion After Heat Resistance Test" above, except that the photomask or laser direct imaging exposure range was set so that the exposed area was a line and space pattern in 1-μm increments from 5 μm to 25 μm. The line pattern of the obtained cured product was observed using a scanning electron microscope (SEM) to determine the minimum line width. Evaluation was performed according to the following evaluation criteria, and the evaluation results are shown in the "Resolution" column in the table. The smaller the minimum line width formed, the better the resolution. Evaluation Criteria: A: The minimum line width of the line and space pattern formed was less than 10 μm. B: The minimum line width of the line and space pattern formed was 10 μm or more but less than 15 μm. C: The minimum line width of the line and space pattern formed was 15 μm or more but less than 20 μm. D: The minimum line width of the line and space pattern formed was 20 μm or more, or no pattern was obtained.
[0341] [Evaluation of Elongation at Break] In each Example and Comparative Example, cured products were obtained in the same manner as in the "Evaluation of Adhesion After Heat Resistance Test" above, except that the photomask or laser direct imaging exposure range was set so that the exposed area was a rectangular region 3 mm wide and 30 mm long. The cured resin composition layer (cured product) was immersed in a 4.9% by mass aqueous solution of hydrofluoric acid, and the cured product was peeled off from the silicon wafer. The longitudinal elongation of the peeled cured product (test piece with a sample width of 3 mm and a sample length of 30 mm) was measured using a tensile tester (Tensilon) at a crosshead speed of 300 mm / min under an environment of 25°C and 65% RH (relative humidity) in accordance with JIS-K6251. Each measurement was performed five times, and the arithmetic mean value of the elongation at break (elongation at break) of the test piece over the five measurements was used as an index value. Evaluation was performed according to the following evaluation criteria, and the evaluation results are shown in the "Elongation at Break" column in the table. The higher the index value, the better the film strength of the cured product. -Evaluation criteria- A: The index value was 65% or more. B: The index value was 60% or more and less than 65%. C: The index value was 55% or more and less than 60%. D: The index value was less than 55%.
[0342] From the above results, it can be seen that the resin composition of the present invention has excellent resolution when forming a pattern of a cured product. The comparative composition according to Comparative Example 1 does not contain a compound corresponding to Compound A. It can be seen that the cured product formed from such a comparative composition has poor resolution. The comparative composition according to Comparative Example 2 does not contain an organometallic complex, has a Group 4 element content of less than 0.010 mass%, does not contain a base generator other than Compound A, and does not contain a compound corresponding to Formula (A-2). It can be seen that the cured product formed from such a comparative composition has poor resolution.
[0343] Example 201 The resin composition used in Example 1 was applied in the form of a layer by spin coating to the surface of the thin copper layer of a resin substrate having a thin copper layer formed on its surface. The resulting layer was dried at 100°C for 5 minutes to form a 20 μm-thick photosensitive film, which was then exposed using a stepper (Nikon Corporation, NSR1505 i6). The exposure was performed at a wavelength of 365 nm through a mask (a binary mask with a 1:1 line-and-space pattern and a line width of 10 μm). After the exposure, the film was developed with cyclopentanone for 2 minutes and rinsed with PGMEA for 30 seconds to obtain a layer pattern. The temperature was then increased at a rate of 10°C / min in a nitrogen atmosphere until it reached 230°C, at which point it was maintained at 230°C for 180 minutes to form an interlayer insulating film for a redistribution layer. This interlayer insulating film for a redistribution layer had excellent insulating properties. Furthermore, a semiconductor device was manufactured using this interlayer insulating film for a redistribution layer, and it was confirmed to operate without any problems.
Claims
1. A resin composition comprising: a heterocycle-containing polymer precursor; compound A that generates a compound having at least one of a pyridine structure and a pyridinium salt structure by the action of light or heat; an organometallic complex; and a polymerization initiator.
2. The resin composition according to claim 1, wherein the organometallic complex is a metal complex having one or more π-conjugated sites containing a nitrogen atom.
3. A resin composition comprising: a heterocycle-containing polymer precursor; compound A which generates a compound having at least one of a pyridine structure and a pyridinium salt structure by the action of light or heat; and a polymerization initiator, wherein the content of a Group 4 element in the composition is 0.010 to 5.0 mass% based on the total solid content of the composition.
4. A resin composition comprising: a heterocycle-containing polymer precursor; compound A that generates a compound having at least one of a pyridine structure and a pyridinium salt structure by the action of light or heat; a base generator other than compound A; and a polymerization initiator.
5. The resin composition according to claim 4, wherein the content of the base generator is 1 to 1,000 parts by mass when the content of the compound A is 100 parts by mass.
6. The resin composition according to any one of claims 1 to 5, wherein the compound A comprises a compound represented by the following formula (A-1): In formula (A-1), R 1 is a hydrogen atom or any organic group, R 2 , R 3 , R 4 and R 5 are each independently a hydrogen atom, a halogen atom, or any organic group; R 6 is a halogen atom or any organic group.
7. R in formula (A-1) 1 is a hydrogen atom, R 4 and R 5 each independently represents -C(=O)O-R 7 , a cyano group or -C(=O)-R 7 and R 7 is a hydrocarbon group which may have a substituent, R 6The resin composition according to claim 6 , wherein is an aromatic group having an electron-withdrawing group as a substituent.
8. R in formula (A-1) 6 When the electron-withdrawing group in is a nitro group, R 6 The resin composition according to claim 7, having only one nitro group therein.
9. A resin composition comprising a heterocycle-containing polymer precursor, a compound A represented by the following formula (A-2), and a polymerization initiator: In formula (A-2), R 1 is a hydrogen atom or any organic group, R 2 , R 3 , R 4 , R 5 are each independently a hydrogen atom, a halogen atom, or any organic group; Ar 1 is an aromatic group having an electron-withdrawing group as a substituent, and when the electron-withdrawing group is a nitro group, Ar 1 has only one nitro group.
10. A resin composition according to any one of claims 1 to 5 and 9, wherein the content of compound A is 0.10 to 30 parts by mass when the content of the heterocycle-containing polymer precursor is 100 parts by mass.
11. The resin composition according to any one of claims 1 to 5 and 9, wherein the heterocycle-containing polymer precursor is a polyimide precursor.
12. The resin composition according to claim 11, wherein the cyclization rate of the polyimide precursor is 2 to 70%.
13. The resin composition according to any one of claims 1 to 5 and 9, wherein the heterocycle-containing polymer precursor has a weight average molecular weight in terms of polystyrene of less than 20,000.
14. The resin composition according to any one of claims 1 to 5 and 9, further comprising a polymerizable compound.
15. The resin composition according to any one of claims 1 to 5 and 9, further comprising a urea compound.
16. The resin composition according to any one of claims 1 to 5 and 9, further comprising a compound having at least one of a pyridine structure and a pyridinium salt structure.
17. A cured product obtained by curing the resin composition according to any one of claims 1 to 5 and 9.
18. The cured product according to claim 17, which is a film having a thickness of less than 10 μm.
19. A laminate comprising two or more layers of the cured product according to claim 17, and including a metal layer between any two of the layers of the cured product.
20. A method for producing a cured product, comprising a film-forming step of applying the resin composition according to any one of claims 1 to 5 and 9 onto a substrate to form a film.
21. The method for producing a cured product according to claim 20, comprising an exposure step of selectively exposing the film to light, and a development step of developing the film with a developer to form a pattern.
22. A method for producing a cured product according to claim 20, comprising a heating step of heating the film at 50 to 450°C.
23. A method for producing a laminate, comprising the method for producing a cured product according to claim 20.
24. A method for producing a semiconductor device, comprising the method for producing the cured product according to claim 20.
25. A semiconductor device comprising the cured product according to claim 17.
Citation Information
Patent Citations
Resin composition, cured product, multilayer body, method for producing cured product, and semiconductor device