Aqueous pigment dispersion, inkjet ink, and method for producing printed matter

The aqueous pigment dispersion with a high crosslinking rate of the crosslinked polymer addresses the stability and ejection performance issues in inkjet inks by ensuring the resin remains adsorbed to the pigment, enhancing storage stability and printability under temperature changes.

WO2024247862A1PCT designated stage expired Publication Date: 2024-12-05DIC CORP

Patent Information

Application Number
PCT/JP2024/018929
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-01
Filing Date
2024-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing inkjet inks face challenges in maintaining storage stability and ink ejection performance, especially under temperature changes, due to the trade-off between crosslinking treatment for stability and potential nozzle clogging from aggregated polymers.

Method used

An aqueous pigment dispersion is developed with a crosslinked polymer derived from a water-soluble dispersion resin having an anionic group and a crosslinking agent with two or more epoxy groups, achieving a crosslinking rate exceeding 80%, which enhances storage stability and ink ejection properties while preventing polymer aggregation.

Benefits of technology

The solution provides inkjet inks with excellent storage stability and printability, even under temperature fluctuations, by ensuring the dispersion resin remains adsorbed to the pigment, thus maintaining inkjet performance and preventing nozzle clogging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Provided is an aqueous pigment dispersion which comprises water, a pigment and a crosslinked polymer. The crosslinked polymer is a product of a reaction between a crosslinking agent and a dispersing resin having an anionic group. The dispersing resin having an anionic group is water-soluble and has an acid value of 181-220 mg KOH / g. The crosslinking agent is a water-soluble compound having two or more epoxy groups. The crosslinking rate of the crosslinked polymer is more than 80%. The aqueous pigment dispersion maintains excellent storage stability even in high temperature environments or in environments having significant changes in temperature, and can be used to produce an inkjet ink having excellent printability.
Need to check novelty before this filing date? Find Prior Art

Description

Aqueous pigment dispersion, inkjet ink, and method for producing printed matter

[0001] The present invention relates to an aqueous pigment dispersion, an inkjet ink, and a method for producing a printed matter.

[0002] Inkjet recording is a method of printing characters and images by ejecting ink droplets directly from extremely fine nozzles onto a recording medium. This method has the advantages of low noise and easy operability, and it is also easy to produce color images. For these reasons, inkjet recording is used not only as an output device in offices and homes, but also for industrial purposes.

[0003] In order to prevent ink ejection defects such as nozzle clogging, deflection of ink droplets, and droplet separation, inks used in the inkjet recording method are required to have excellent storage stability and be resistant to increases in viscosity over time and sedimentation of pigments, etc. Furthermore, when manufactured inks are transported, they may be stored at high or low temperatures, and it is necessary for the inks to be ones that do not cause sedimentation of pigments, etc., even when subjected to temperature changes.

[0004] Known examples of aqueous pigment dispersions with excellent storage stability include crosslinked polymer particles for inkjet recording, which are obtained by dispersing a pigment in a water-soluble polymer having an anionic group and a water-insoluble polymer having an anionic group, and then crosslinking the polymers with a crosslinking agent, and aqueous dispersions using the same (see, for example, Patent Document 1).

[0005] However, even when the dispersion is subjected to a crosslinking treatment as described above, the storage stability is highly dependent on the type of dispersing resin and crosslinking agent, as well as the conditions of the crosslinking reaction, and if the combination is not appropriate, sufficient storage stability may not be obtained at high temperatures or when exposed to repeated high and low temperatures.

[0006] Furthermore, as a result of strengthening the crosslinking treatment to improve storage stability, there is a concern that even dispersion resins that are not adsorbed to the pigment in the dispersion may crosslink with each other, resulting in a high molecular weight. Crosslinked polymers that are not adsorbed to the pigment tend to aggregate, which can cause ink ejection problems such as nozzle clogging.

[0007] As described above, in dispersions that have been subjected to a crosslinking treatment, there is a trade-off between storage stability and ink ejection properties, and there is a demand for the development of dispersions that achieve both of these.

[0008] JP 2009-49595 A

[0009] The problem to be solved by the present invention is to provide an aqueous pigment dispersion that can be used to produce an inkjet ink that maintains excellent storage stability even at high temperatures or in environments with large temperature changes, has excellent ink ejection properties, and is also excellent in printability.

[0010] The present invention solves the above-mentioned problems by providing an aqueous pigment dispersion comprising water, a pigment, and a crosslinked polymer, wherein the crosslinked polymer is a reaction product of a dispersing resin having an anionic group and a crosslinking agent, the dispersing resin having an anionic group is water-soluble and has an acid value of 181 to 220 mgKOH / g, the crosslinking agent is a water-soluble compound having two or more epoxy groups, and the crosslinking rate of the crosslinked polymer exceeds 80%.

[0011] According to the aqueous pigment dispersion of the present invention, it is possible to obtain an inkjet ink and a printed matter that maintain excellent storage stability, have excellent ink ejection properties, and are also excellent in printability.

[0012] The aqueous pigment dispersion of the present invention comprises water, a pigment, and a crosslinked polymer, the crosslinked polymer being a reaction product of a dispersing resin having an anionic group and a crosslinking agent, and the crosslinked polymer having a crosslinking rate of more than 80%. The dispersing resin having an anionic group is water-soluble and has an acid value of 181 to 220 mgKOH / g. The crosslinking agent is a water-soluble compound having two or more epoxy groups.

[0013] (Water) The water used in the present invention can be, for example, pure water or ultrapure water such as ion-exchanged water, ultrafiltered water, reverse osmosis water, distilled water, etc. The water is used in an amount of preferably 25% by mass to 90% by mass, more preferably 35% by mass to 85% by mass, and even more preferably 55% by mass to 75% by mass, based on the total amount of the aqueous pigment dispersion.

[0014] (Pigment) As the pigment, for example, organic pigments and inorganic pigments that are usually used in aqueous gravure ink, aqueous flexographic ink, aqueous offset ink, or aqueous inkjet ink can be used.

[0015] The pigment may include one or both of an organic pigment and an inorganic pigment, and both an unacid-treated pigment and an acid-treated pigment can be used.

[0016] Examples of inorganic pigments that can be used include iron oxide and carbon black produced by a contact method, a furnace method, a thermal method, or the like.

[0017] Examples of organic pigments that can be used include azo pigments (azo lake, insoluble azo pigment, condensed azo pigment, chelate azo pigment, etc.), polycyclic pigments (e.g., phthalocyanine pigment, perylene pigment, perinone pigment, anthraquinone pigment, quinacridone pigment, dioxazine pigment, thioindigo pigment, isoindolinone pigment, quinophthalone pigment, etc.), lake pigments (e.g., basic dye-type chelate, acid dye-type chelate), nitro pigments, nitroso pigments, and aniline black.

[0018] Examples of pigments (black pigments) that can be used in black inks include C.I. Pigment Black 1, 6, 7, 8, 10, 26, 27, and 28. Among these, C.I. Pigment Black 7 is preferably used. Specific examples of black pigments include No. 2200, No. 2300, No. 2350, No. 2600, No. 650B, No. 750B, No. 850, No. 900, No. 950, No. 960, No. 970, No. 980, No. 990, No. 995B, No. 1000, No. 3030B, No. 3050B, No. 3230B, No. 3400B, and No. 1000, all manufactured by Mitsubishi Chemical Corporation. No. 25B, No. 30, No. 33, No. 40, No. 44, No. 45, No. 45L, No. 47, No. 52, MA7, MA8, MA77, MA100, MA230, MA600, MCF88, etc.; No. 5500, No. 4500, No. 4400, No. 5500 manufactured by Tokai Carbon Co., Ltd.; 8500 etc.; Raven760UP, Raven780UP, Raven860UP, Raven900P, Rav manufactured by BILRA en1000P, Raven1060P, Raven1080UP, Raven1255, Raven2000, Raven2350 ULTRA, Raven2500 ULTRA, Raven2800 ULTRA, Raven2900 ULTRA, Raven3000 ULTRA, Raven3500, Raven5000 ULTRA II, Raven5000 ULTRA 3. Raven UV ULTRA, Conductex SC ULTRA, Conductex K ULTRA etc;Regal 330R, Regal 400R, Regal 660R, Mogul L, Mogul 700, Monarch 700, Monarch 717, Monarch 800, Monarch 880, Monarch 900, Monarch 1000, Monarch 1100, Monarch 1300, Monarch 1400, BLACK PEARLS 800, BLACK PEARLS 880, BLACK PEARLS 1000, BLACK PEARLS 1300, BLACK PEARLS 2000, BLACK PEARLS 4040, BLACK PEARLS 4350, BLACK PEARLS 4560i, BLACK PEARLS 4750, VULCAN XC72, VULCAN XC72R, VULCAN 9A32, ELFTTEX 570, ELFTTEX P100, ELFTTEX TP, etc. manufactured by Cabot Corporation;Orion Engineered Carbon's Color Black FW1, Color Black FW2, Color Black FW2V, Color Black FW18, Color Black FW171, Color Black FW182, Color Black FW200, Color Black FW285, Color Black S150, Color Black S160, Color Black S170, Printex 30, Printex 35, Printex 40, Printex 45, Printex U, Printex V, and Printex 1400U, Printex 150T, Printex 55, Printex 70, Printex 75, Printex 80, Printex F80, Printex F85, Printex 90, Printex 95, Printex 300, Printex P beads, Printex L6, Special Black 6, Special Black 5, Special Black 4, Special Black 4A, Special Black 350, Special Black 550, NIPEX 35, NIPEX 75, NIPEX 90, NIPEX 150, NIPEX 160, NIPEX 160IQ, NIPEX 170, NIPEX 170IQ, NIPEX 180, NIPEX 180IQ, NIPEX 1601IQ, HIBLACK 50L, HIBLACK 600L, HIBLACK F890B, HIBLACK 930L, HIBLACK 970LB, Nerox 305, Nerox 500, Nerox 505, Nerox 600, Nerox 605, and the like.

[0019] Specific examples of pigments (yellow pigments) that can be used in yellow inks include C.I. Pigment Yellow 1, 2, 12, 13, 14, 16, 17, 73, 74, 75, 83, 93, 95, 97, 98, 109, 110, 114, 120, 128, 129, 138, 150, 151, 154, 155, 174, 180, and 185.

[0020] Specific examples of pigments (magenta pigments) that can be used in magenta inks include C.I. Pigment Red 5, 7, 12, 48 (Ca), 48 (Mn), 57 (Ca), 57:1, 112, 122, 123, 146, 149, 150, 168, 176, 184, 185, 202, 209, 254, 269, 282, and the like; C.I. Pigment Violet 19, and the like. Specific examples of magenta pigments include Quindo Magenta 228-2120, Fastogen Super Magenta RGT, Fastogen Super Magenta RTS, Fastgen Super Magenta RY, Cinquasia Magenta D4550J, and Cinquasia Magenta D4500J, all manufactured by DIC Corporation; and FUJI FAST CARMINE 520, FUJI FAST CARMINE 522-1D, Fuji Fast Carmine 580S, and FUJI FAST CARMINE 590-4, all manufactured by Fuji Color Co., Ltd. RED 9800, FUJI FAST CARMINE 6005; Ink Jet Magenta E5B 02 manufactured by Heubach; and the like.

[0021] Specific examples of pigments (cyan pigments) that can be used in cyan inks include C.I. Pigment Blue 1, 2, 3, 15, 15:3, 15:4, 15:6, 16, 22, 60, 63, and 66. Of these, C.I. Pigment Blue 15:3 is preferably used. Specific examples of cyan pigments include FSJ-SD, TGR, TGR-J, TGR-SD, SBG-SD, KET BLUE 111, and Heliogen Blue L 7101 F, all manufactured by DIC Corporation; and CYANINE BLUE 3023-A, all manufactured by Sanyo Pigment Co., Ltd.

[0022] Specific examples of pigments (white pigments) that can be used in white ink include alkaline earth metal sulfates, carbonates, finely powdered silicic acid, silicas such as synthetic silicates, calcium silicate, alumina, alumina hydrate, titanium oxide, zinc oxide, talc, clay, and the like.

[0023] The pigment is preferably used in an amount of 10% by mass to 25% by mass, based on the total amount of the aqueous pigment dispersion, and is preferably used in an amount of 12% by mass to 20% by mass, in order to obtain an aqueous pigment dispersion that can suppress aggregation over time and has excellent storage stability.

[0024] In the present invention, the pigment is preferably a quinacridone pigment, as this allows the effects of the present invention to be optimally exhibited. Examples of quinacridone pigments include compounds represented by the following general formula (1): Xn-Q-Ym(1) (wherein Q represents a quinacridone residue or a quinacridonequinone residue, X and Y represent a hydrogen atom, a methyl group, a chloro group, or a methoxy group, and n and m represent integers of 1 to 4). Specific examples thereof include dimethylquinacridone pigments such as 2,9-dimethylquinacridone, 3,10-dimethylquinacridone, and 4,11-dimethylquinacridone (C.I. Pigment Red 122, etc.), dichloroquinacridone pigments such as 2,9-dichloroquinacridone, 3,10-dichloroquinacridone, and 4,11-dichloroquinacridone (C.I. Pigment Red 202, C.I. Pigment Red 209, etc.), unsubstituted quinacridone pigments (C.I. Pigment Violet 19, etc.), dimethoxyquinacridone pigments such as 2,9-dimethoxyquinacridone, 3,10-dimethoxyquinacridone, and 4,11-dimethoxyquinacridone, quinacridonequinone pigments, and mixtures or solid solutions of at least two or more pigments selected from these pigments. The pigment may be a dry pigment in the form of powder, granules or lumps, or may be in the form of a wet cake or slurry. Among the above quinacridone pigments, C.I. Pigment Red 122 is preferred.

[0025] A quinacridone pigment solid solution refers to a pigment containing two quinacridone pigments selected from an unsubstituted quinacridone pigment, a dimethylquinacridone pigment, and a dichloroquinacridone pigment, forming a mixed layer in which one quinacridone pigment is dissolved in the other crystalline phase. In other words, the solid solution does not contain single crystals of the quinacridone pigment. Whether the solid solution is a solid solution or a mixture of the single crystals can be easily determined by powder X-ray diffraction. Among these, a solid solution of an unsubstituted quinacridone pigment and a dimethylquinacridone pigment is preferred. In the quinacridone pigment solid solution, the weight ratios of [unsubstituted quinacridone pigment / dimethylquinacridone pigment], [unsubstituted quinacridone pigment / dichloroquinacridone pigment], and [dimethylquinacridone pigment / dichloroquinacridone pigment] are preferably 5 / 95 to 95 / 5, more preferably 10 / 90 to 90 / 10, from the viewpoints of ejection reliability, print density, saturation, etc. In particular, the weight ratio of [unsubstituted quinacridone pigment / dimethylquinacridone pigment] is preferably 5 / 95 to 40 / 60, more preferably 10 / 90 to 30 / 70. The quinacridone pigment solid solution may be in the form of a powder, granule, or block dry pigment, or may be in the form of a wet cake or slurry.

[0026] The use of quinacridone pigments in particular in the present invention allows the effects of the present invention to be optimally achieved. While the reason for this is unclear, the inventors speculate as follows: As can be seen from the quinacridone molecular skeleton, the vertical direction of the molecular plane exhibits aromatic properties and is highly hydrophobic. However, the lateral direction is extremely weaker in aromaticity due to the presence of carbonyl and amino groups, and as a result, the hydrophobicity is thought to be weaker compared to the vertical direction. Therefore, quinacridone pigments tend to be difficult to stabilize with the hydrophobic functional groups that serve as the adsorption groups of the dispersing resin. As a result, dissociation of the dispersing resin is likely to occur, and quinacridone pigments tend to have poor ink storage stability, particularly when the ink is subjected to repeated temperature increases and decreases. In the present invention, the quinacridone pigment is dispersed using a dispersing resin having an anionic group, and then the dispersing resin is crosslinked, thereby increasing the molecular weight of the dispersing resin and preventing the dispersing resin from detaching from the quinacridone pigment. This is thought to result in good storage stability, particularly when the ink is subjected to repeated temperature increases and decreases.

[0027] The aqueous pigment dispersion of the present invention preferably does not contain a pigment derivative. Generally, pigment derivatives are added to pigments that tend to have poor storage stability, such as quinacridone pigments, to improve their storage stability. However, pigment derivatives that are not adsorbed to the pigment may aggregate together, reducing the ejection performance of the inkjet printer and adversely affecting the storage stability of the ink when the ink is repeatedly heated and cooled. The aqueous pigment dispersion of the present invention can improve the storage stability of dispersions of pigments that have relatively poor storage stability, such as quinacridone pigments, without using a pigment derivative, and can also suppress the adverse effects of the pigment derivative on the ink.

[0028] (Crosslinked Polymer) The aqueous pigment dispersion of the present invention contains a crosslinked polymer, which is a reaction product of a dispersing resin having an anionic group and a crosslinking agent.

[0029] The crosslinked polymer is preferably formed, for example, by producing an aqueous pigment dispersion containing the pigment, the dispersing resin, water, and the like, and then mixing the aqueous pigment dispersion with the crosslinking agent to react the carboxyl groups of the dispersing resin having an anionic group with the epoxy groups of the crosslinking agent.

[0030] (Crosslinking Rate of Crosslinked Polymer) The crosslinked polymer contained in the aqueous pigment dispersion of the present invention has a crosslinking rate of more than 80%. Here, the crosslinking rate is a value that can be calculated using the following calculation formula (2) from the amount of crosslinking agent used, the number of moles of reactive groups, the amount of polymer used, and the number of moles of reactive groups of the polymer that can react with the reactive groups of the crosslinking agent. Crosslinking rate (mol %) = 100 × [number of moles of reactive groups in crosslinking agent] / [number of moles of carboxyl groups in the dispersion resin] Formula (2) In formula (2), the "number of moles of reactive groups in the crosslinking agent" is the value obtained by dividing the weight of the crosslinking agent used by the equivalent weight of the reactive groups. In other words, it is calculated by multiplying the number of moles of crosslinking agent used by the number of reactive groups in one molecule of the crosslinking agent.

[0031] When the crosslinking rate exceeds 80%, the storage stability of the ink and the storage stability when the ink is repeatedly heated and cooled can be improved. Furthermore, in order to maintain good ink ejection properties, the crosslinking rate is preferably more than 80% and less than 90%. When the crosslinking rate is less than 90%, the anionic groups remaining in the dispersion resin without undergoing the crosslinking reaction also contribute to dispersion stability, thereby improving the storage stability.

[0032] Furthermore, it is preferable to use a crosslinked polymer having anionic groups in a range of 0.2 to 2.5 mmol / g relative to the total amount of the crosslinked polymer. By using a crosslinked polymer having anionic groups in this range, it is possible to obtain an aqueous pigment dispersion and an ink containing the same with excellent storage stability. It is more preferable to use a crosslinked polymer with anionic groups in an amount in a range of 0.3 to 2.0 mmol / g relative to the total amount of the crosslinked polymer, in order to further improve the storage stability of the aqueous pigment dispersion and ink.

[0033] When the reaction product of the dispersing resin and the crosslinking agent is used as the crosslinked polymer, a part of the anionic groups of the dispersing resin reacts with the epoxy groups of the crosslinking agent and is consumed. Therefore, the amount of the anionic groups relative to the total amount of the crosslinked polymer refers to the amount of the anionic groups remaining in the reaction product of the dispersing resin and the crosslinking agent.

[0034] (Dispersion Resin Having Anionic Groups) The dispersion resin having anionic groups used in the present invention is water-soluble and has an acid value of 181 to 220 mgKOH / g. Here, in the present invention, "the dispersion resin is water-soluble" means that the neutralized dispersion resin neutralized with NaOH dissolves in an amount of 10 g or more in 100 g of water. If the dispersion resin is water-soluble, the pigment can be dispersed without using an organic solvent, particularly an ester solvent or a ketone solvent, in the dispersion step, eliminating the need for a step of removing the organic solvent. Furthermore, residual organic solvent that cannot be completely removed does not adversely affect storage stability or storage stability during repeated temperature increases and decreases.

[0035] The dispersing resin having an anionic group used in the present invention has an acid value of 181 to 220 mgKOH / g. The acid value is preferably 181 to 210 mgKOH / g, and more preferably 185 to 205 mgKOH / g. When the acid value is within the above range, an aqueous pigment dispersion can be obtained that is excellent in storage stability by preventing pigment aggregation and sedimentation over time, and also has good jetting properties, resulting in excellent printability. Furthermore, when the ink composition contains a large amount of surfactant or solvent, the ink tends to have poor storage stability when repeatedly heated and cooled. However, when the acid value is within the above range, even such an ink has good storage stability when repeatedly heated and cooled.

[0036] The weight-average molecular weight of the dispersion resin having an anionic group used in the present invention is preferably 10,000 to 50,000, more preferably 13,000 to 50,000, even more preferably 13,000 to 30,000, and particularly preferably 13,000 to 25,000. When the weight-average molecular weight is within the above range, the dispersion stability is good, and the storage stability and storage stability during repeated temperature increases and decreases are also good. Furthermore, free dispersion resins are less likely to form aggregates, reducing the risk that such aggregates will adversely affect inkjet ejection performance.

[0037] The content of the dispersing resin having an anionic group in the aqueous pigment dispersion of the present invention is preferably in the range of 10% by mass to 34% by mass, and more preferably in the range of 15% by mass to 30% by mass, relative to the total amount of the pigment. In other words, the ratio of dispersing resin having an anionic group to pigment is preferably 0.10 to 0.40, more preferably 0.12 to 0.40, even more preferably 0.15 to 0.40, and particularly preferably 0.18 to 0.30.

[0038] Examples of the dispersing resin having an anionic group include acrylic resins such as acrylic acid-acrylic acid ester copolymers, styrene-acrylic acid copolymers, styrene-methacrylic acid copolymers, styrene-methacrylic acid-acrylic acid ester copolymers, styrene-α-methylstyrene-acrylic acid copolymers, styrene-α-methylstyrene-acrylic acid-acrylic acid ester copolymers, and other styrene-acrylic resins, such as styrene-maleic acid copolymers, styrene-maleic anhydride copolymers, and vinylnaphthalene-acrylic acid copolymers, as well as salts of these resins. Examples of the dispersing resin include the Acrydic series from DIC Corporation and the Hiros-X series from Seiko PMC Corporation. The compounds exemplified as polymer (G) in WO 2018 / 190139 can also be used as the dispersing resin. The dispersing resin having an anionic group may also be referred to simply as a dispersing resin.

[0039] Among these, it is preferable to use a styrene-acrylic acid copolymer or a styrene-methacrylic acid copolymer as the dispersing resin having an anionic group, since the pigment can be stably dispersed in water.

[0040] As the dispersing resin having an anionic group, it is preferable to use one in which a part or all of the anionic groups have been neutralized with a neutralizing agent.

[0041] The neutralizing agent may be, for example, an alkali metal hydroxide or an amine compound, and the use of an alkali metal hydroxide is preferred in order to further improve the dispersion stability immediately after production of the aqueous pigment dispersion of the present invention and the storage stability. Furthermore, the use of an alkali metal hydroxide can also maintain good ejection properties.

[0042] Examples of the alkali metal hydroxide include lithium hydroxide, sodium hydroxide, potassium hydroxide, and cesium hydroxide, with sodium hydroxide and potassium hydroxide being preferred, and potassium hydroxide being more preferred.

[0043] The neutralizing agent is preferably used so that the neutralization rate calculated by the following formula is 100% or less, in order to prevent the pigment from settling or flocculating over time and to obtain an aqueous pigment dispersion with excellent storage stability. The neutralization rate refers to a value calculated based on the formula [100 × (molar equivalents of hydroxyl groups in alkali metal hydroxide / molar equivalents of anionic groups in the dispersing resin)].

[0044] (Crosslinking Agent) The crosslinking agent used in the present invention is a water-soluble compound having two or more epoxy groups. Examples of the crosslinking agent include polyglycidyl ethers such as ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, glycerin triglycidyl ether, glycerol polyglycidyl ether, polyglycerol polyglycidyl ether, trimethylolpropane polyglycidyl ether, sorbitol polyglycidyl ether, pentaerythritol polyglycidyl ether, resorcinol diglycidyl ether, and neopentyl glycol diglycidyl ether. These crosslinking agents may be used alone or in combination of two or more.

[0045] Among these, it is preferable to use a crosslinking agent having an epoxy group and an oxyethylene structure in order to further improve the storage stability of the aqueous pigment dispersion. Specifically, it is preferable to use ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerol polyglycidyl ether, or trimethylolpropane polyglycidyl ether, and it is more preferable to use ethylene glycol diglycidyl ether.

[0046] The crosslinking agent may be a compound having two or more epoxy groups. It is preferable to use a crosslinking agent having two to four epoxy groups in order to further improve the storage stability of the aqueous pigment dispersion, and it is more preferable to use a crosslinking agent having two epoxy groups in order to more easily achieve both the storage stability of the ink, the storage stability when the ink is repeatedly heated and cooled, and the ejection properties of the ink.

[0047] Furthermore, as the crosslinking agent, it is preferable to use a compound having epoxy groups at both ends, and it is more preferable to use a compound having epoxy groups only at both ends. By using a compound having epoxy groups at both ends as a crosslinking agent, the dispersion resin can be favorably crosslinked, and even if the dispersion resin that did not contribute to pigment dispersion is crosslinked, good ejection properties are likely to be maintained. Furthermore, using a compound having epoxy groups only at both ends is more preferable because it allows the crosslinking density to be favorably controlled, making it easier to achieve both ink storage stability and ink ejection properties when the ink is repeatedly heated and cooled.

[0048] The amount of epoxy groups contained in the crosslinking agent is expressed by the epoxy equivalent. The epoxy equivalent is the molecular weight of the epoxy compound divided by the number of epoxy groups; the smaller this value, the shorter the distance between crosslinking points. The epoxy equivalent of the crosslinking agent is preferably 100 to 400, more preferably 100 to 350, and even more preferably 100 to 300. If the epoxy equivalent is 100 or less, the distance between crosslinking points is too short, making it impossible to crosslink dispersed resins together. On the other hand, if the epoxy equivalent is too high, dispersed resins that are farther apart will be crosslinked to form a crosslinked structure, which will cause the ink to thicken.

[0049] The crosslinking agent is water-soluble. Here, "the crosslinking agent is a water-soluble compound" means that the crosslinking agent has a water solubility of 50% or more. The water solubility is preferably 60% or more, more preferably 70% or more, even more preferably 80% or more, and particularly preferably 90% or more. The higher the water solubility of the crosslinking agent, the less likely the pigment particle size will increase when the dispersion resin is crosslinked, thereby suppressing pigment aggregation. The water solubility (%) refers to the dissolution rate (mass%) when 10 parts by mass of an epoxy compound is dissolved in 90 parts by mass of water at room temperature (25°C). Specifically, it can be measured by the following procedure. At room temperature (25°C), 90 parts of ion-exchanged water and 10 parts of a crosslinking agent are added to a glass tube (25 mmφ x 250 mmh), and the glass tube is allowed to stand for 1 hour in a thermostatic bath adjusted to a water temperature of 25°C. The glass tube is then vigorously shaken for 1 minute and then allowed to stand again in the thermostatic bath for 10 minutes. Next, the undissolved matter is weighed, and the water solubility (mass %) is calculated.

[0050] The crosslinking agent is preferably used in a range of 4.0 mmol / g or less, more preferably 3.8 mmol / g or less, and even more preferably 2.3 mmol / g or more and 3.6 mmol / g or less, relative to the total amount of the dispersing resin, in order to obtain an aqueous pigment dispersion having even better storage stability.

[0051] The aqueous pigment dispersion of the present invention can contain, as needed, a water-soluble solvent, a preservative, a viscosity modifier, a pH modifier, a chelating agent, a plasticizer, an antioxidant, an ultraviolet absorber, etc. The chelating agent can reduce the content of metal ions derived from the pigment contained in the aqueous pigment dispersion.

[0052] Next, a method for producing an aqueous pigment dispersion of the present invention will be described. The present invention also provides a method for producing an aqueous pigment dispersion comprising water, a pigment, and a crosslinked polymer, the crosslinked polymer being obtained by crosslinking a dispersing resin having an anionic group with a crosslinking agent, the dispersing resin having an anionic group being water-soluble and having an acid value of 181 to 220 mgKOH / g, the crosslinking agent being a water-soluble compound having two or more epoxy groups, and the crosslinked polymer having a crosslinking rate of greater than 80%. Specifically, the method includes: Step 1 of mixing water, a pigment, and a dispersing resin having an anionic group to produce a dispersion in which the pigment is dispersed in the water; and Step 2 of reacting anionic groups, such as carboxyl groups, of the dispersing resin contained in the dispersion with functional groups, such as epoxy groups, of the crosslinking agent to form a crosslinked polymer, the dispersing resin having an anionic group being water-soluble and having an acid value of 181 to 220 mgKOH / g, the crosslinking agent being a water-soluble compound having two or more epoxy groups, and the crosslinked polymer having a crosslinking rate of greater than 80%.

[0053] The step 1 is, for example, a step of treating a mixture of a pigment, a dispersing resin, and water using a dispersing machine.

[0054] Examples of the dispersing machine that can be used include kneading dispersers with high-speed stirring blades, such as an Intensive Mixer (manufactured by Nippon Eirich Co., Ltd.), a Butterfly Mixer (Inoue Seisakusho Co., Ltd.), and a Planetary Mixer (Inoue Seisakusho Co., Ltd.); media-type wet dispersers, such as an SC Mill (Nippon Coke and Engineering Co., Ltd.) and a Nano Mill (Asada Iron Works Co., Ltd.); and media-less wet dispersers, such as a Starburst (Sugino Machine Co., Ltd.) and an ultrasonic processor (Hielscher Ultrasonics GmbH).

[0055] In particular, it is preferable to use a kneading disperser having the high-speed stirring blades as the disperser, in order to prevent a decrease in the ink jet ejection properties of the ink due to the influence of beads, etc., used in a media-type wet disperser. Furthermore, compared to a wet disperser, a kneading disperser having the high-speed stirring blades can raise the temperature of the contents of the disperser to nearly 100°C, thereby increasing the ease with which the dispersing resin is adsorbed to the pigment. If there is little dispersing resin not adsorbed to the pigment, aggregates of the crosslinked polymer are less likely to occur during crosslinking treatment, and good printer ejection properties are maintained.

[0056] On the other hand, when the media-type wet disperser or media-less type wet disperser is used, the step 1 may include a step 1-1 of mixing the pigment, dispersing resin, and water and pre-dispersing the mixture using a stirrer or the like to produce a mixture containing the pigment and water, and a step 1-2 of treating the mixture obtained in the step 1-1 with the media-type wet disperser or media-less type wet disperser. This step allows the dispersibility of the pigment and the like contained in the aqueous pigment dispersion to be confirmed during the process.

[0057] The neutralization of the dispersed resin is preferably carried out during or after the completion of step 1. Specifically, the neutralization can be carried out by supplying the neutralizing agent to the mixture during step 1 or to the dispersion obtained after the completion of step 1, and mixing the neutralizing agent with the mixture.

[0058] Furthermore, the dispersion obtained in step 1 may be subjected to centrifugation, pH adjustment, or metal ion removal, if necessary, before step 2 is carried out.

[0059] Next, step 2 will be described. Step 2 is a step in which an anionic group, such as a carboxyl group, of the dispersing resin is reacted with a functional group, such as an epoxy group, of the crosslinking agent to form a dispersing resin having an anionic group that coats or adsorbs on the surface of the pigment. The reaction is preferably carried out within a temperature range of 60 to 70°C in order to obtain an aqueous pigment dispersion with even better storage stability.

[0060] As described above, the crosslinking agent is preferably supplied to the dispersion obtained after completion of step 1, but may also be supplied to the mixture of the pigment, the dispersing resin, and the water during step 1.

[0061] The aqueous pigment dispersion obtained through steps 1 and 2 is preferably subjected to centrifugation or filtration as necessary in order to remove coarse particles and reduce the amount of sediment contained in the dispersion obtained in step 1, the aqueous pigment dispersion, and the ink.

[0062] The aqueous pigment dispersion obtained by the above method can be used to produce inks such as inkjet inks, as described below. However, because the aqueous pigment dispersion obtained by the above method tends to have a slightly high pH, ​​if there is a discrepancy between the pH and the pH expected for the ink, it is preferable to adjust the pH of the aqueous pigment dispersion to a lower value in advance, in order to increase the flexibility of ink design. One method for adjusting the pH of the aqueous pigment dispersion is to treat the aqueous pigment dispersion with an ion exchange resin. Specifically, one example is to mix the aqueous pigment dispersion with a weakly acidic cation exchange resin such as Amberlite IRC76 manufactured by Organo Corporation, and then remove the cation exchange resin.

[0063] (Inkjet Ink) The aqueous pigment dispersion of the present invention obtained by the above method can be used, for example, to produce ink. In particular, the aqueous pigment dispersion can be used to produce inkjet ink. The inkjet ink can be produced, for example, by supplying an aqueous medium, a binder, a surfactant, etc. to the aqueous pigment dispersion as needed and mixing them. When mixing the aqueous pigment dispersion with an aqueous medium, a binder, a surfactant, etc. as needed, a dispersing machine or various mixers such as a bead mill, ultrasonic homogenizer, high-pressure homogenizer, paint shaker, ball mill, roll mill, sand mill, sand grinder, Dyno Mill, Dispermat, SC Mill, or Nanomizer can be used.

[0064] The inkjet ink may contain other additives such as a binder, a surfactant, a wax, a wetting agent (a drying inhibitor), a penetrating agent, a preservative, a viscosity adjuster, a pH adjuster, a chelating agent, a plasticizer, an antioxidant, and an ultraviolet absorber, as required.

[0065] Examples of the binder that can be used include poly(meth)acrylic resin, polyurethane resin, polyester resin, and acid-modified polypropylene resin. The acid-modified polypropylene resin can be a resin obtained by modifying polypropylene with one or more acidic compounds, and it is preferable to use one having a polypropylene-derived skeleton (polypropylene skeleton) and a functional group derived from the acidic compound. An inkjet ink containing the acid-modified polypropylene resin can prevent mottling and streak-like printing defects during one-pass printing from occurring on the printed matter, even when printed on a recording medium that does not or poorly absorbs the solvent in the ink.

[0066] Commercially available products can also be used as the acid-modified polypropylene resin. Preferred commercially available products include Auroren (registered trademark) AE-301 and AE-502 manufactured by Nippon Paper Industries Co., Ltd. Furthermore, as the oxidized polyethylene wax, for example, a polyethylene wax that has been subjected to an oxidation treatment can be used, and specifically, a wax having a skeleton derived from polyethylene (polyethylene skeleton) can be used.

[0067] As the surfactant, for example, anionic surfactants, nonionic surfactants, cationic surfactants, amphoteric surfactants, etc. can be used.

[0068] As the surfactant, it is preferable to use one or more surfactants selected from the group consisting of anionic surfactants and nonionic surfactants, from the viewpoint of easily suppressing the occurrence of streak-like printing defects.

[0069] Examples of anionic surfactants include alkylbenzenesulfonates, alkylphenylsulfonates, alkylnaphthalenesulfonates, higher fatty acid salts, sulfate ester salts of higher fatty acid esters, sulfonates of higher fatty acid esters, sulfate ester salts and sulfonates of higher alcohol ethers, higher alkyl sulfosuccinates, polyoxyethylene alkyl ether carboxylates, polyoxyethylene alkyl ether sulfates, alkyl phosphates, and polyoxyethylene alkyl ether phosphates. Specific examples of these include dodecylbenzenesulfonate, isopropylnaphthalenesulfonate, monobutylphenylphenol monosulfonate, monobutylbiphenylsulfonate, and dibutylphenylphenol disulfonate.

[0070] Examples of nonionic surfactants include polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitol fatty acid esters, glycerin fatty acid esters, polyoxyethylene glycerin fatty acid esters, polyglycerin fatty acid esters, sucrose fatty acid esters, polyoxyethylene alkylamines, polyoxyethylene fatty acid amides, fatty acid alkylolamides, alkylalkanolamides, acetylene glycol, oxyethylene adducts of acetylene glycol, and polyethylene glycol polypropylene glycol block copolymers. Of these, preferred is one or more selected from the group consisting of polyoxyethylene nonylphenyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene dodecylphenyl ether, polyoxyethylene alkyl ethers, polyoxyethylene fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, fatty acid alkylolamides, acetylene glycol, oxyethylene adducts of acetylene glycol, and polyethylene glycol polypropylene glycol block copolymers.

[0071] As the nonionic surfactant, the inkjet ink preferably contains an acetylene-based surfactant, from the viewpoint of easily suppressing the occurrence of streak-like printing defects. The acetylene-based surfactant is a surfactant having an acetylene structure in the molecule. From the viewpoint of easily suppressing the occurrence of streak-like printing defects, the acetylene-based surfactant preferably contains one or more surfactants selected from the group consisting of acetylene glycol and oxyethylene adducts of acetylene glycol.

[0072] From the viewpoint of easily suppressing the occurrence of streak-like printing defects, the content of the acetylene-based surfactant is preferably 80 to 100 mass %, more preferably 85 to 99.9 mass %, and even more preferably 90 to 99.5 mass %, relative to the total amount of surfactants.

[0073] Other surfactants that can be used include silicone surfactants such as polysiloxane oxyethylene adducts; fluorine-based surfactants such as perfluoroalkyl carboxylates, perfluoroalkyl sulfonates, and oxyethylene perfluoroalkyl ethers; and biosurfactants such as spiculisporic acid, rhamnolipid, and lysolecithin.

[0074] The content of the surfactant is preferably 0.1 to 2% by mass, more preferably 0.5 to 2% by mass, and even more preferably 0.8 to 1.6% by mass, based on the total amount of the inkjet ink. An inkjet ink containing a surfactant at such a content exhibits good wettability of the ejected droplets on the surface of a substrate, tends to have sufficient wetting and spreading on the substrate, and is likely to be effective in preventing the occurrence of streak-like printing defects. Furthermore, if the amount of surfactant in the ink is within this range, the surfactant is less likely to concentrate when the ink is repeatedly heated and cooled, thereby maintaining good storage stability.

[0075] The use of a surfactant makes it easier for the inkjet ink ejected from the ejection openings of the inkjet head to wet and spread well on the surface of the substrate after landing on it, which makes it easier to prevent streak-like printing defects. Furthermore, the use of a surfactant makes it easier to improve the leveling properties of the inkjet ink by, for example, reducing the surface tension of the inkjet ink.

[0076] As the wax, for example, oxidized polyethylene wax can be used.

[0077] When an inkjet ink contains the oxidized polyethylene wax, it is possible to obtain a printed matter having excellent image fastness.

[0078] As the oxidized polyethylene wax, it is preferable to use an oxidized polyethylene wax in a state of being dissolved or dispersed in a solvent in order to obtain a printed matter having excellent image fastness.

[0079] As the oxidized polyethylene wax, commercially available products can also be used. Preferred commercially available products include AQUACER 515 and AQUACER 1547 manufactured by BYK Corporation.

[0080] The humectant can be used for the purpose of preventing drying of the inkjet ink in the ejection nozzles of the inkjet head. As the humectant, it is preferable to use one that is miscible with water and has the effect of preventing clogging of the ejection orifices of the inkjet head, and examples thereof include ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycols having a molecular weight of 2000 or less, propylene glycol, dipropylene glycol, tripropylene glycol, isopropylene glycol, isobutylene glycol, 1,4-butanediol, 1,3-butanediol, 1,5-pentanediol, 1,6-hexanediol, mesoerythritol, pentaerythritol, and glycerin.

[0081] A solid wetting agent can also be used as the wetting agent. Examples of such wetting agents include urea and urea derivatives. Examples of urea derivatives include ethylene urea, propylene urea, diethyl urea, thiourea, N,N-dimethyl urea, hydroxyethyl urea, hydroxybutyl urea, ethylene thiourea, and diethyl thiourea. These can be used alone or in combination of two or more. From the viewpoint of easily obtaining printed matter with excellent setting properties, it is preferable to use at least one selected from the group consisting of urea, ethylene urea, and 2-hydroxyethyl urea.

[0082] The content of the humectant is 3 to 50% by mass relative to the total amount of the inkjet ink, which makes it possible to achieve both ease of drying on the recording medium and prevention of the inkjet ink from sticking inside the inkjet head.

[0083] Examples of the penetrating agent include lower alcohols such as ethanol and isopropyl alcohol; and glycol monoethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl butyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, triethylene glycol monopropyl ether, triethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monobutyl ether, tripropylene glycol monomethyl ether, tripropylene glycol monoethyl ether, tripropylene glycol monopropyl ether, and tripropylene glycol monobutyl ether.

[0084] When the ink is repeatedly heated and cooled, the wetting agent and penetrant may promote concentration of the surfactant at low temperatures, and the concentrated components may adversely affect the dispersion of the pigment at high temperatures. However, by using the aqueous pigment dispersion of the present invention, this adverse effect can be reduced, and good storage stability can be obtained even when the ink is repeatedly heated and cooled.

[0085] In the inkjet ink obtained by the above method, the pigment is preferably used in a range of 1% by mass to 15% by mass relative to the total amount of printing ink, and a range of 2% by mass to 10% by mass is preferred in order to obtain printed matter that has high print density, is less likely to produce streaks, has excellent image fastness, and is excellent in dispersion stability.

[0086] The pH of the inkjet ink is preferably 7.0 or higher, more preferably 7.5 or higher, and even more preferably 8.0 or higher, in order to improve the storage stability and ejection stability of the ink, and to improve the wetting and spreading, print density, and abrasion resistance when printed on a recording medium that is poorly or non-absorbent of ink. The upper limit of the pH of the aqueous ink composition is preferably 11.0 or lower, more preferably 10.5 or lower, and even more preferably 10.0 or lower, in order to suppress deterioration of components constituting the ink application or ejection device (e.g., ink ejection orifices, ink flow paths, etc.) and to reduce the effects of ink adhesion to skin. From these viewpoints, the pH of the inkjet ink is preferably 7.0 to 11.0. Note that the above pH is measured at 25°C.

[0087] The viscosity of the inkjet ink is preferably 2 mPa·s or more and less than 10 mPa·s at 32°C. When the viscosity of the inkjet ink is in this range, when used in an inkjet recording method, the apparent deviation of the landing position on the recording medium caused by deflection of the ink droplet tends to be reduced, and the occurrence of streaks in the printed matter tends to be effectively prevented. Furthermore, an inkjet ink having a viscosity in this range tends to have excellent storage stability and ejection stability in an inkjet recording method. The viscosity of the inkjet ink at 32°C is preferably 3 mPa·s or more, more preferably 4 mPa·s or more. The viscosity of the aqueous ink composition at 32°C is preferably 8 mPa·s or less, more preferably 7 mPa·s or less. The above viscosity is a value measured, for example, using a cone-plate rotational viscometer equivalent to an E-type viscometer under the following conditions.

[0088] Measurement device: TVE-25 type viscometer (Toki Sangyo Co., Ltd., TVE-25 L) Calibration standard solution: JS20 Measurement temperature: 32°C Rotation speed: 10 to 100 rpm Injection amount: 1200 μL

[0089] The surface tension of the inkjet ink is preferably, for example, 20 to 40 mN / m at 25°C. If the surface tension of the aqueous ink composition is within this range, when used in an inkjet recording method, the wettability of the ejected droplets on the surface of the recording medium tends to be good, and they tend to spread sufficiently after landing. The surface tension of the inkjet ink at 25°C is preferably 25 mN / m or more, more preferably 27 mN / m or more. The surface tension of the aqueous ink composition at 25°C is preferably 35 mN / m or less, more preferably 32 mN / m or less.

[0090] The inkjet ink containing the aqueous pigment dispersion of the present invention has a high crosslinking rate, which allows the dispersing resin to more firmly adsorb to the pigment surface, resulting in good storage stability. Here, good storage stability means that the rate of change in volume average particle size measured by the method described below is less than 10% after 2 weeks of testing, less than 15% after 4 weeks, and less than 20% after 8 weeks. Furthermore, the storage method described below is an accelerated test, and storage at 60°C for 8 weeks yields results equivalent to those obtained after approximately 2 years of storage at room temperature (25°C), making it possible to predict deterioration due to long-term storage.

[0091] (Method for evaluating storage stability) The volume average particle diameter D0 of the inkjet ink immediately after production was measured using the particle diameter measurement method described below. Next, 30 mL of the inkjet ink was filled into a 30 mL polypropylene bottle and stored in a thermostatic chamber at 60° C. After a certain period of storage, the volume average particle diameter D1 of the inkjet ink was measured using the particle diameter measurement method described below.

[0092] The rate of change in particle size of the inkjet ink after storage for a certain period of time from the start of storage was calculated based on the volume average particle sizes D0 and D1 and the following formula, and the storage stability of the inkjet ink was evaluated based on the rate of change: Particle size change rate = [(D1 - D0) / (D0)] x 100

[0093] The particle size of the inkjet ink was measured under the following conditions: Measuring device: Particle size analyzer NANOTRAC WAVE 2 (manufactured by Microtrac Bell Co., Ltd.) Measurement temperature: 25°C Number of measurements: 1 Measurement time: 180 seconds Particle transmittance: Transmitted Particle refractive index: 1.51 Particle shape: Aspherical Density: 1.00 Solvent refractive index: 1.333 Filter: Stand: Norm

[0094] Furthermore, inkjet inks containing the aqueous pigment dispersions of the present invention can maintain a stable state even when the storage temperature is changed from low to high due to shipping, etc. The stability under such storage conditions can be evaluated by repeatedly raising and lowering the storage temperature. Higher storage temperatures increase molecular motion, which facilitates the separation of the adsorption between the pigment and the dispersion resin, making the pigment more susceptible to aggregation. On the other hand, lower storage temperatures (e.g., −40°C) cause some of the components in the inkjet ink (particularly surfactants) to precipitate or concentrate. Subsequently, when the ink temperature rises, the highly concentrated ink components may interact with the dispersion, potentially causing pigment aggregation. Due to this particle size increase mechanism, there may be no correlation between the storage stability at a constant temperature and the storage stability after repeated temperature increases and decreases. An inkjet ink containing the aqueous pigment dispersions of the present invention can maintain good storage stability after repeated temperature increases and decreases. Here, good storage stability after repeated temperature increases and decreases refers to a change in volume average particle size of less than 10% as measured by the following method.

[0095] (Evaluation Method for Heating and Cooling Cycle Test) The volume average particle diameter D0 of the inkjet ink immediately after production was measured using the particle diameter measurement method described below. Next, 30 mL of the inkjet ink was filled into a 30 mL volumetric polypropylene plastic bottle and left to stand in a thermostatic chamber at room temperature. The temperature inside the chamber was cooled to -40°C, maintained at -40°C for 4 hours, then increased to 70°C and maintained at 70°C for 4 hours. This temperature cycle was repeated four times, and the volume average particle diameter D2 of the inkjet ink after the cycle was completed was measured, and the rate of change from MV0 was calculated. Rate of change in particle diameter = [(D2 - D0) / (D0)] x 100

[0096] A printed matter obtained using the inkjet ink of the present invention comprises, for example, a recording medium and a coating film of the inkjet ink printed on the surface of the recording medium. The ink coating film formed on the surface of the recording medium is, for example, a dried product of the inkjet ink and contains the solid components of the inkjet ink (for example, the pigment and the pigment dispersant (B)).

[0097] The recording medium is, for example, plain paper, inkjet paper, glossy paper, poorly ink-absorbent recording medium, non-ink-absorbent recording medium, etc. This printed matter has sufficient image fastness even if the recording medium is the poorly ink-absorbent or non-ink-absorbent recording medium described above.

[0098] The printed matter can be obtained, for example, by printing the inkjet ink onto the surface of a recording medium using an inkjet recording method. Specifically, the printed matter can be obtained by ejecting the inkjet ink onto a recording medium using an inkjet recording method in which the distance from a plane (x) having ink ejection ports of an inkjet head to a position (y) where a perpendicular line to the plane (x) intersects with the recording medium is 1 mm or more.

[0099] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0100] (Dispersion Resin A) Dispersion Resin A, a radical polymer, is in the form of powder (diameter 1 mm or less) produced by solution polymerization, and has a monomer composition ratio of styrene / acrylic acid / methacrylic acid / butyl acrylate = 72.00 / 12.13 / 15.77 / 0.10 (mass ratio), a weight average molecular weight of 16,000, an acid value of 185 mgKOH / g, and a glass transition temperature of 139°C. Furthermore, Dispersion Resin A was found to be water-soluble in the water solubility test described below.

[0101] (Dispersion Resin B) Dispersion Resin B, a radical polymer, is a powder (diameter 1 mm or less) produced by solution polymerization, with a monomer composition ratio of styrene / acrylic acid / methacrylic acid / butyl acrylate = 69.06 / 13.41 / 17.43 / 0.10 (mass ratio), a weight average molecular weight of 14,000, an acid value of 202 mgKOH / g, and a glass transition temperature of 139°C. Furthermore, the result of the water solubility test described below showed that Dispersion Resin B was water soluble.

[0102] (Dispersion Resin C) Dispersion Resin C, a radical polymer, is a powder (diameter 1 mm or less) produced by solution polymerization, and has a monomer composition ratio of styrene / acrylic acid / methacrylic acid / butyl acrylate = 74.00 / 11.26 / 14.64 / 0.10 (mass ratio), a weight average molecular weight of 11,000, an acid value of 173 mg KOH / g, and a glass transition temperature of 115° C. Furthermore, Dispersion Resin C was found to be water-soluble in the water solubility test described below.

[0103] The weight average molecular weight in the present invention is a value measured by GPC (gel permeation chromatography) and converted into the molecular weight of polystyrene used as a standard substance. The measurement was carried out using the following equipment and conditions.

[0104] Pump: LC-9A, System Controller: SLC-6B, Auto-injector: S1L-6B, Detector: RID-6A, all manufactured by Shimadzu Corporation. Data processing software: Sic480II Data Station (manufactured by System Instruments). Column: GL-R400 (guard column) + GL-R440 + GL-R450 + GL-R 400M (manufactured by Hitachi Chemical Co., Ltd.). Elution solvent: tetrahydrofuran (THF). Elution flow rate: 2 ml / min. Column temperature: 35°C.

[0105] The water solubility of the dispersion resin was determined by the following procedure. (1) 10 g of dispersion resin was placed in a beaker. (2) To (1), an aqueous NaOH solution was added so as to achieve 100% neutralization, depending on the acid value of the dispersion resin. (3) Water was added to (2) so that the total amount, including the amount of water in the aqueous NaOH solution, was 100 g, and the mixture was stirred well while heating to 50-60°C as necessary. (4) The aqueous solution was brought to a liquid temperature of 25°C and allowed to stand, and after 24 hours or more, it was visually inspected for the presence of sediment. Presence of sediment: Water insoluble No sediment: Water soluble

[0106] (Production Example 1) Dispersion resin A and FASTOGEN SUPER MAGENTA RY (manufactured by DIC) as a magenta pigment were charged in the amounts shown in Table 1 into a planetary mixer (trade name: Chemical Mixer ACM04LVTJ-B, manufactured by Aikosha Seisakusho Co., Ltd.) with a jacket heated to 80°C, and the mixture was stirred at a rotation speed of 80 rpm and a revolution speed of 25 rpm. After 10 minutes, triethylene glycol as a solvent and a 34% by mass aqueous potassium hydroxide solution as a neutralizer were added, and the mixture was stirred again. Kneading was continued until 60 minutes had elapsed since the current value of the planetary mixer reached its maximum current value, thereby obtaining a kneaded product.

[0107] The obtained kneaded product was gradually mixed with ion-exchanged water to dilute it, and finally triethylene glycol was added as a diluent to obtain an aqueous pigment dispersion 1 having a pigment concentration of 15.4% by mass.

[0108] (Production Examples 2 and 3) Aqueous pigment dispersions 2 and 3 were obtained in the same manner as in Production Example 1, except that the raw materials used and their amounts were changed as shown in Table 1.

[0109]

[0110] (Example 1) Aqueous pigment dispersion 1 obtained in Production Example 1, a crosslinking agent, and ion-exchanged water in the amounts shown in Table 2 were placed in a lidded plastic container and stirred for 5 hours at 70°C. After stirring, the mixture was cooled to obtain crosslinked dispersion 1 having a pigment concentration of 15% by mass. The crosslinking rate of the crosslinked polymer in this crosslinked dispersion was 82%.

[0111] Examples 2 to 4, Comparative Examples 1 to 6 Crosslinked dispersions 2 to 10 were obtained in the same manner as in Example 1, except that the raw materials used and their amounts were changed as shown in Table 2.

[0112] The crosslinking ratio of the crosslinked polymers of crosslinked dispersions 1 to 10 in Examples 1 to 4 and Comparative Examples 1 to 6 was calculated as follows: Crosslinking ratio (mol %) = 100 × [number of moles of reactive groups in crosslinking agent] / [number of moles of carboxyl groups in the dispersion resin] Equation (2) In Equation (2), the "number of moles of reactive groups in the crosslinking agent" is the value obtained by dividing the weight of the crosslinking agent used by the equivalent weight of the reactive groups. In other words, it is the number of moles of the crosslinking agent used multiplied by the number of reactive groups in one molecule of the crosslinking agent.

[0113]

[0114] Denacol EX313: epoxy equivalent 141, solubility of 10 g of crosslinking agent in 90 g of ion-exchanged water (water solubility rate) 99% by mass (25°C), manufactured by Nagase ChemteX Corporation. Denacol EX810: epoxy equivalent 113, solubility of 10 g of crosslinking agent in 90 g of ion-exchanged water (water solubility rate) 100% by mass (25°C), manufactured by Nagase ChemteX Corporation. Denacol EX830: epoxy equivalent 268, solubility of 10 g of crosslinking agent in 90 g of ion-exchanged water (water solubility rate) 100% by mass (25°C), manufactured by Nagase ChemteX Corporation.

[0115] (Preparation Example 1) A plastic container was charged with ion-exchanged water, propylene glycol, glycerin, triethanolamine, TegoWET 280 (manufactured by Evonik, silicone-based surfactant), ACTICIDE B20 (manufactured by Thor Japan Co., Ltd., preservative), and ethylene urea in the amounts listed in Table 3. After the ethylene urea was dissolved, propylene glycol and SURFYNOL 420 (manufactured by Evonik, acetylene-based surfactant) were added and stirred to obtain Mixture A. Next, Auroren (registered trademark) AE-301 (manufactured by Nippon Paper Industries Co., Ltd., acid-modified polypropylene), ion-exchanged water, AQUACER 515 (manufactured by BYK, high-density oxidized polyethylene wax emulsion), and ion-exchanged water were mixed in the order listed to obtain Mixture B. The crosslinked dispersion 1 obtained in Example 1 was mixed with Mixture B in the amounts listed in Table 3, and then Mixture A was further mixed. The container was washed with ion-exchanged water as washing water, and then stirred to obtain Ink 1.

[0116] Preparation Examples 2 to 10 Inks 2 to 10 were obtained by preparing inks under the same conditions as in Preparation Example 1, except that crosslinked dispersion 1 was replaced with crosslinked dispersions 2 to 10.

[0117] <Evaluation of Properties> The properties of the ink were evaluated by the methods described below.

[0118] [Evaluation of storage stability] Immediately after production, the volume average particle diameter D0 of Inks 1 to 10 was measured using the particle diameter measurement method described below. Next, 30 mL of Inks 1 to 10 was filled into a 30 mL polypropylene bottle and stored in a thermostatic chamber at 60°C. After a certain period of time from the start of storage, the volume average particle diameter D1 of each ink after storage was measured using the particle diameter measurement method described below.

[0119] The rate of change in particle size of each ink after storage for a certain period from the start of storage was calculated based on the volume average particle sizes D0 and D1 and the following formula, and the storage stability of inks 1 to 10 was evaluated based on this rate of change: Rate of change in particle size = [(D1 - D0) / (D0)] x 100 The storage stability of inks 1 to 10 was evaluated as good if the rate of change in volume average particle size was less than 10% after 2 weeks of testing, less than 15% after 4 weeks, and less than 20% after 8 weeks.

[0120] [Heating / Cooling Cycle] The volume average particle diameter D0 of inks 1 to 10 immediately after production was measured using the particle diameter measurement method described below. Next, 30 mL of inkjet ink was filled into a 30 mL polypropylene plastic bottle and placed in a thermostatic chamber at room temperature. The temperature inside the chamber was cooled to -40°C, maintained at -40°C for 4 hours, then raised to 70°C and maintained at 70°C for 4 hours. This temperature cycle was repeated four times, and the volume average particle diameter D2 of each ink after the cycle was completed was measured using the following method, and the rate of change from D0 was calculated. Rate of particle diameter change = [(D2 - D0) / (D0)] x 100. For inks 1 to 10, the heating / cooling cycle was evaluated as "good" if the rate of change in volume average particle diameter was less than 10%.

[0121] The particle size of inks 1 to 10 in the storage stability and heating / cooling cycle evaluations was the MV (volume mean diameter) value measured under the following conditions: Measuring device: particle size analyzer NANOTRAC WAVE 2 (manufactured by Microtrac Bell Co., Ltd.) Measurement temperature: 25°C Number of measurements: 1 Measurement time: 180 seconds Particle transmittance: Transmitted Particle refractive index: 1.51 Particle shape: Aspherical Density: 1.00 Solvent refractive index: 1.333 Filter: Stand: Norm

[0122] [Printing Suitability Test] 50 mL of ink was filtered through a 0.45 μm membrane filter and filled into the black ink cartridge of a Hewlett-Packard ENVY4500 printer. The printing properties were set to grayscale printing: black ink only, and print quality: draft, and a solid print was made on HAMMER MILL printing paper manufactured by Sylvamo. The printed area was measured for color saturation using an X-Rite eXact colorimeter. A saturation value of 45 or higher was determined to indicate good printability.

[0123] The evaluation results are shown in Table 3.

[0124]

[0125] As shown in Table 3, inks 1 to 4, which are inks using the aqueous pigment dispersions of the present invention, not only exhibited good storage stability but also good results in the heating / cooling cycle evaluation. Furthermore, they also had excellent printability. On the other hand, inks 5 and 7 to 9 used aqueous pigment dispersions with a low crosslinking rate of the crosslinked polymer, and therefore exhibited poor storage stability and poor results in the heating / cooling cycle evaluation. Furthermore, aqueous pigment dispersions 5 and 6 used dispersion resins with low acid values, and therefore exhibited poor printability, resulting in low saturation of the resulting prints.

[0126] (Production Example 4) Dispersion resin B and 995B (manufactured by Mitsubishi Chemical Corporation) as a black pigment were charged in the amounts shown in Table 4 into a planetary mixer (trade name: Chemical Mixer ACM04LVTJ-B, manufactured by Aikosha Seisakusho Co., Ltd.) with a jacket heated to 80°C, and stirred at a rotation speed of 80 rpm and a revolution speed of 25 rpm. After 10 minutes, triethylene glycol as a solvent and a 34% by mass aqueous potassium hydroxide solution as a neutralizer were added, and the mixture was stirred again. Kneading was continued until 60 minutes had elapsed since the current value of the planetary mixer reached its maximum current value, thereby obtaining a kneaded product.

[0127] The obtained kneaded product was gradually mixed with ion-exchanged water to dilute it, and finally triethylene glycol was added as a diluent to obtain aqueous pigment dispersion 4 having a pigment concentration of 13.0% by mass.

[0128] (Production Example 5) Aqueous pigment dispersion 5 was obtained in the same manner as in Production Example 4, except that, among the raw materials used, the pigment was changed to a cyan pigment SBG-SD (manufactured by DIC Corporation) and the amounts of the other raw materials added were changed as shown in Table 4.

[0129]

[0130] (Example 5) Aqueous pigment dispersion 4 obtained in Production Example 4, a crosslinking agent, and ion-exchanged water in the amounts shown in Table 5 were placed in a lidded plastic container and stirred at 70°C for 5 hours. After stirring, the mixture was cooled to obtain crosslinked dispersion 11 having a pigment concentration of 12.5% ​​by mass. The crosslinking rate of the crosslinked polymer in this crosslinked dispersion was 82%.

[0131] Example 6 A crosslinked dispersion 12 was obtained in the same manner as in Example 5, except that the raw materials used and their amounts were changed as shown in Table 5.

[0132]

[0133] (Preparation Example 11) A plastic container was charged with ion-exchanged water, propylene glycol, glycerin, triethanolamine, TegoWET 280 (manufactured by Evonik, silicone-based surfactant), ACTICIDE B20 (manufactured by Thor Japan Co., Ltd., preservative), and ethylene urea in the amounts listed in Table 6. After the ethylene urea was dissolved, propylene glycol and SURFYNOL 420 (manufactured by Evonik, acetylene-based surfactant) were added and stirred to obtain Mixture A. Next, Auroren (registered trademark) AE-301 (manufactured by Nippon Paper Industries Co., Ltd., acid-modified polypropylene), ion-exchanged water, AQUACER 515 (manufactured by BYK, high-density oxidized polyethylene wax emulsion), and ion-exchanged water were mixed in the order listed to obtain Mixture B. The crosslinked dispersion 11 obtained in Example 5 was mixed with Mixture B in the amounts listed in Table 6, and then Mixture A was further mixed. The container was washed with ion-exchanged water as washing water, and then stirred to obtain Ink 11.

[0134] Preparation Example 12 Ink 12 was obtained by preparing under the same conditions as in Preparation Example 11, except that Crosslinked Dispersion 11 was changed to Crosslinked Dispersion 12 and the amounts in parts by mass were as shown.

[0135]

[0136] [Printability Test] 50 mL of ink was filtered through a 0.45 μm membrane filter and filled into the black ink cartridge of a Hewlett-Packard ENVY4500 printer. The printing properties were set to grayscale printing: black ink only, and print quality: draft, and a solid print was performed on HAMMER MILL printing paper manufactured by Sylvamo. The printed area was measured using an X-Rite eXact colorimeter to obtain the saturation. For inks using black pigments, a saturation value of 5 or less was determined to have good printability. On the other hand, for inks using cyan pigments, a saturation value of 40 or more was determined to have good printability.

[0137] As shown in Table 6, when the black pigment or cyan pigment was used, similar to the magenta pigment, good storage stability and heating / cooling cycle evaluation results were obtained. Furthermore, the printability was also excellent.

Claims

1. An aqueous pigment dispersion comprising water, a pigment, and a crosslinked polymer, wherein the crosslinked polymer is a reaction product of a dispersing resin having an anionic group and a crosslinking agent, the dispersing resin having an anionic group is water-soluble and has an acid value of 181 to 220 mgKOH / g, the crosslinking agent is a water-soluble compound having two or more epoxy groups, and the crosslinking rate of the crosslinked polymer exceeds 80%.

2. The aqueous pigment dispersion according to claim 1, wherein the ratio of the pigment to the dispersing resin having an anionic group (dispersing resin having an anionic group / pigment) is 0.10 to 0.

40.

3. The aqueous pigment dispersion according to claim 1, wherein the pigment is a quinacridone pigment.

4. An ink-jet ink comprising the aqueous pigment dispersion according to any one of claims 1 to 3.

5. A printed matter comprising the ink-jet ink according to claim 4 and a recording medium.

Citation Information

Patent Citations

  • Ink and ink set

    WO2018190139A1

  • Aqueous ink for inkjet recording

    JP2009046595A

  • Aqueous pigment dispersion for ink-jet recording

    JP2018109095A

  • Water-based pigment dispersion

    JP2022070102A

  • Method for producing water-based pigment dispersion

    JP2022070106A

Cited By

  • Water-based inkjet inks and printed materials

    JP7889687B1