Method for producing continuous cellulose fiber having improved thermal stability

By immersing cellulose fibers in an aqueous medium with glycosylating and esterifying agents and drying them continuously, the method addresses the inefficiencies of existing thermal stability enhancements, achieving stable cellulose fibers for industrial applications.

WO2024247869A1PCT designated stage expired Publication Date: 2024-12-05DAICEL CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018973
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing methods for improving thermal stability of cellulose fibers are not suitable for continuous production and require high-temperature drying, making them inefficient and costly for industrial applications.

Method used

Immersion of continuous cellulose fibers in an aqueous medium containing compounds like glycosylating agents and esterifying agents, such as glycerin and boric acid, followed by continuous drying, to enhance thermal stability without the need for prolonged high-temperature drying processes.

Benefits of technology

This method produces cellulose fibers with improved thermal stability, preventing color change and performance deterioration upon heating, suitable for industrial use in resin modifiers and reinforcing materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

The present invention addresses the problem of providing a method for producing a continuous cellulose fiber having improved thermal stability by an industrially feasible method. The present invention is a method for producing a continuous cellulose fiber having improved thermal stability, the method comprising: immersing a continuous cellulose fiber in an aqueous medium containing a compound (A) capable of reacting with a reducing terminal or a hydroxyl group of cellulose; causing the continuous cellulose fiber to absorb the aqueous medium; and then drying the continuous cellulose fiber. The series of steps are successively performed while the continuous cellulose fiber is wound or taken up.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing continuous cellulose fibers with improved thermal stability

[0001] The present invention relates to a method for producing continuous cellulose fibers with improved thermal stability.

[0002] Cellulose fibers are fibers containing cellulose, the main component of wood, and are classified into plant fibers, regenerated fibers (regenerated cellulose fibers), semi-synthetic fibers, cellulose nanofibers, etc. Such cellulose fibers are not limited to applications such as clothing, but are also widely used as industrial raw materials for food, cosmetics, functional paper, etc.

[0003] In recent years, in response to growing environmental awareness, cellulose fibers, a biomass-derived material, have been adopted as resin modifiers and reinforcing materials (see, for example, Patent Document 1). When using cellulose fibers as a resin reinforcing material, a common method involves producing continuous cellulose fibers, cutting the continuous fibers to a desired length, and incorporating them into a resin to obtain a fiber-reinforced resin composition, or impregnating the continuous cellulose fibers with a resin and then cutting them to a desired length to obtain a cellulose fiber-reinforced resin material (resin-impregnated long fiber bundle). On the other hand, cellulose has low thermal stability, and heating can cause deformation and discoloration of the appearance, resulting in performance degradation. Therefore, for example, in resin compositions containing cellulose fibers, the cellulose fibers can become discolored during heat treatment when preparing the resin composition or when obtaining a molded article from the resin composition, resulting in poor appearance.

[0004] As a method for improving the thermal stability of cellulose, for example, Patent Document 2 proposes a method in which an aqueous solution of a polyhydric alcohol is dropped onto cellulose filter paper, and then the aqueous solution is dried for 24 hours in an oven at 105° C. Furthermore, Patent Document 3 proposes a method for producing cellulose in which boric acid water is added to a fine cellulose powder, and then the cellulose powder containing the boric acid water is heat-treated at 105° C. for 24 hours or more, thereby suppressing yellowing and blackening at temperatures of 300° C. or less.

[0005] JP 2018-024967 A JP 2010-159364 A JP 2008-163053 A

[0006] The methods described in Patent Documents 2 and 3 are batch processes, making their application to continuous fibers difficult. Furthermore, these methods require a drying treatment at a temperature of 100°C or higher for 24 hours to obtain cellulose with improved thermal stability. Therefore, there is a need for an industrially feasible method for producing continuous cellulose fibers with improved thermal stability. Therefore, an object of the present invention is to provide an industrially feasible method for producing continuous cellulose fibers with improved thermal stability.

[0007] As a result of extensive research, the present inventors have found that continuous cellulose fibers with improved thermal stability can be produced by an industrially feasible method by immersing continuous cellulose fibers in an aqueous medium containing a compound capable of improving the thermal stability of cellulose by reacting with the reducing end or hydroxyl groups of cellulose, followed by drying, and performing a series of steps while winding or taking up the continuous fibers. That is, the present invention has the following aspects: [1] A method for producing continuous cellulose fibers with improved thermal stability, comprising immersing continuous cellulose fibers in an aqueous medium containing a compound (A) capable of reacting with the reducing end or hydroxyl groups of cellulose, allowing the continuous cellulose fibers to absorb the aqueous medium, and then drying, wherein the series of steps are continuously performed while winding or taking up the continuous cellulose fibers. [2] A method for producing continuous cellulose fibers according to [1], wherein the compound (A) comprises at least one compound selected from a glycosylating agent (a1) for the reducing end of cellulose and an esterifying agent (a2) for the hydroxyl groups of cellulose. [3] The method for producing continuous cellulose fibers according to [2], wherein the glycosylating agent (a1) contains a monohydric or higher alcohol and the esterifying agent (a2) contains boric acid. [4] The method for producing continuous cellulose fibers according to any of [1] to [3], wherein the immersion length of the continuous cellulose fibers is 1 to 1,000 cm, and the winding speed or take-up speed of the continuous cellulose fibers is 10 to 1,000 m / min. [5] The method for producing continuous cellulose fibers according to any of [1] to [4], wherein the concentration of the compound (A) in the aqueous medium is 0.1 to 50 mass%. [6] The method for producing continuous cellulose fibers according to any of [1] to [5], wherein the drying temperature of the continuous cellulose fibers is 10 to 300°C. [7] The method for producing continuous cellulose fibers according to any of [1] to [6], wherein the drying step comprises drying the continuous cellulose fibers with hot air and then further drying the continuous cellulose fibers while contacting them with a heated cylinder.[8] The method for producing continuous cellulose fibers according to any one of [1] to [7], wherein the continuous cellulose fibers include continuous regenerated cellulose fibers, spun fibers of short-fiber regenerated cellulose, or spun fibers of natural cellulose.

[0008] According to the present invention, it is possible to provide a method for producing continuous cellulose fibers with improved thermal stability in an industrially feasible manner.

[0009] An embodiment of the present disclosure will be described in detail below. However, the scope of the present disclosure is not limited to the embodiment described herein, and various modifications can be made without departing from the spirit of the present disclosure. Each aspect disclosed in this specification can be combined with any other feature disclosed in this specification. Furthermore, when multiple upper and lower limit values ​​are described for a specific parameter, any of these upper and lower limit values ​​can be combined to form a suitable numerical range. Furthermore, the lower and / or upper limit values ​​of a numerical range described in this disclosure are numerical values ​​within that range and may be replaced with numerical values ​​shown in the examples. The expression "X to Y" indicating a numerical range means "X or greater and Y or less." If a specific description described for one embodiment also applies to other embodiments, that description may be omitted in other embodiments. Each configuration and combination thereof in each embodiment is merely an example, and additions, omissions, substitutions, and other modifications of configurations are possible as appropriate within the spirit of the present disclosure. The present disclosure is not limited by the embodiments. Each feature disclosed herein may be combined with any other feature disclosed herein.

[0010] [Method for Producing Continuous Cellulose Fiber] This embodiment relates to a method for producing continuous cellulose fiber with improved thermal stability, which comprises immersing continuous cellulose fiber in an aqueous medium containing a compound (A) capable of reacting with the reducing end or hydroxyl group of cellulose, allowing the continuous cellulose fiber to absorb the aqueous medium (step (I)), and then drying (step (II)), and the series of steps is carried out continuously while the continuous cellulose fiber is being wound or taken up. In this production method, "continuously carrying out while winding or taking up the continuous cellulose fiber" means that the continuous cellulose fiber as a raw material is wound or taken up in one direction so that the continuous cellulose fiber is continuously processed in the order of steps (I) and (II). Furthermore, "winding the continuous cellulose fiber" refers to winding the continuous cellulose fiber obtained by the production method according to this embodiment onto a core or reel and recovering it as a final product. Furthermore, "taking up the continuous cellulose fiber" includes winding the continuous cellulose fiber obtained by the production method according to this embodiment on a winder or the like, and may also include unwinding the continuous cellulose fiber for another process.

[0011] <Step (I)> The production method according to this embodiment comprises immersing continuous cellulose fibers in an aqueous medium containing a compound (A) capable of reacting with the reducing ends or hydroxyl groups of cellulose, thereby causing the aqueous medium to be absorbed into the continuous cellulose fibers. The production method according to this embodiment comprises causing the continuous cellulose fibers to absorb the aqueous medium containing the compound (A), thereby causing the reducing ends or hydroxyl groups of cellulose to react with the compound (A). Note that "causing the continuous cellulose fibers to absorb the aqueous medium" includes not only taking in the aqueous medium into voids (pores) within the continuous cellulose fibers (water absorption), but also the continuous cellulose fibers absorbing the aqueous medium and swelling, the aqueous medium adhering to the surface of the continuous cellulose fibers, and the aqueous medium being incorporated between the fibers. Furthermore, in the final continuous cellulose fibers with improved thermal stability, the compound (A) may be immobilized in a state where it has reacted with the reducing ends or hydroxyl groups of cellulose, or may be immobilized (adhered) to the fiber surface.

[0012] (Continuous Cellulose Fibers) Cellulose is a plant-derived polysaccharide found in, for example, wood, cotton, ramie, linen, hemp, jute, Manila hemp, sisal, etc. The raw material continuous cellulose fibers (hereinafter sometimes referred to as "raw material fibers") used in the manufacturing method according to this embodiment may be, for example, natural cellulose fibers (short fibers) extracted from plants such as cotton, ramie, linen, hemp, jute, Manila hemp, and sisal, twisted together to form a long thread (continuous natural cellulose fibers (spun fibers)), or continuous regenerated cellulose fibers. They may also be monofilaments or multifilaments. Natural continuous cellulose fibers may contain lignin, hemicellulose, etc., but the cellulose content is preferably 60% or more, more preferably 60-80%. When the raw material fibers are continuous regenerated cellulose fibers, the manufacturing method thereof is not particularly limited, and may be, for example, continuous fibers obtained from solvent-process regenerated cellulose such as viscose rayon, lyocell, cupra, or ionic liquid. Alternatively, spun fibers made by twisting regenerated cellulose short fibers into long threads may also be used.

[0013] The average fiber diameter of the raw fiber may be 5 to 50 μm or 7 to 30 μm, from the viewpoint that the raw fiber easily absorbs the aqueous medium containing compound (A) in a short time when the raw fiber is immersed in the aqueous medium (hereinafter sometimes simply referred to as "aqueous medium"). The average fiber diameter of the raw fiber can be measured using a microscope. That is, the cross section of the raw fiber is observed under a microscope, and the length of the major axis of the cross section is measured. The average value of the lengths of the major axes measured for approximately 200 raw fibers is taken as the average fiber diameter. When the fiber cross section has an elliptical diameter, the length of the major axis is taken as the major diameter, and when the fiber cross section has an irregular shape, the longest part is taken as the major diameter.

[0014] (Aqueous medium containing compound (A)) Step (I) involves immersing raw fiber in an aqueous medium containing compound (A). The aqueous medium may be an aqueous solution of compound (A) or an emulsion (dispersion) in which compound (A) is dispersed. The water component contained in the aqueous medium may be pure water, ion-exchanged water, tap water, industrial water, or a mixture thereof. From the viewpoint of cost, the water component is preferably tap water or industrial water. The aqueous medium may also contain optional components other than the above-mentioned water component and compound (A).

[0015] (Compound (A) capable of reacting with the reducing end or hydroxyl group of cellulose) The aqueous medium contains a compound (A) capable of reacting with the reducing end or hydroxyl group of cellulose. The compound (A) may have a structure capable of chemically reacting with the reducing end or hydroxyl group of cellulose, or may be a compound having a structure capable of physically reacting with the reducing end or hydroxyl group of cellulose. The position of the reducing end or hydroxyl group of cellulose capable of reacting with the compound (A) is not particularly limited. Among these, it is preferable to contain at least one compound selected from a glycosylating agent (a1) for the reducing end of cellulose and an esterifying agent (a2) for the hydroxyl group of cellulose.

[0016] Glycosylating Agent (a1) In one embodiment, compound (A) can contain a glycosylating agent (a1) for the reducing end of cellulose. The term "glycosylating agent" refers to any compound capable of glycosylating the reducing end of cellulose. The glycosylating agent (a1) is not particularly limited as long as it is a compound capable of glycosylating the reducing end of cellulose. However, from the viewpoint of facilitating glycosylation of the reducing end, it is preferable that the glycosylating agent (a1) contains a monohydric or higher alcohol.

[0017] Examples of the monohydric or higher alcohol include, for example, alcohols having 1 to 20 carbon atoms. Specific examples include monohydric alcohols such as methanol, ethanol, propanol, isopropanol, butanol, ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, benzyl alcohol, and phenethyl alcohol; linear polyhydric alcohols such as mannitol, glycerin, erythritol, pentaerythritol, xylitol, glucitol, and ethylene glycol; and phenols such as phenol, para-cresol, meta-cresol, ortho-cresol, ethylphenol, guaiacol, and catechol. These may be used alone or in combination of two or more. Among these, from the viewpoint of more effectively glycosylating the reducing end, it is preferable to include glycerin, mannitol, pentaerythritol, methanol, or ethylene glycol, and it is more preferable to include glycerin, mannitol, or pentaerythritol.

[0018] When a glycosylating agent (a1) is used as compound (A), the ratio of the glycosylating agent (a1) to the total mass of the aqueous medium (the concentration of the glycosylating agent (a1)) is preferably 0.1 to 50% by mass, more preferably 0.5 to 20% by mass, and particularly preferably 1 to 15% by mass. By allowing the raw fiber to absorb an aqueous medium having a glycosylating agent (a1) concentration within the above range, continuous cellulose fibers with improved thermal stability can be more easily obtained.

[0019] Esterifying Agent (a2) In one embodiment, the compound (A) can contain an esterifying agent (a2) for the hydroxyl groups of cellulose. The term "esterifying agent" refers to any compound capable of esterifying the hydroxyl groups of cellulose. The esterifying agent (a2) is not particularly limited as long as it is a compound capable of esterifying the hydroxyl groups of cellulose. However, from the viewpoint of avoiding destruction of the internal structure of cellulose by the esterifying agent (a2), it is preferable for the esterifying agent (a2) to contain a weak acid such as acetic acid, boric acid, or a boric acid compound, more preferably boric acid or a boric acid compound, and even more preferably boric acid.

[0020] Examples of the boric acid compound include borate salts such as alkali metal salts, alkaline earth metal salts, and metal salts; metaboric acid and its salts; polyboric acid and its salts; etc. These boric acid compounds may be used alone or in combination of two or more.

[0021] When an esterifying agent (a2) is used as compound (A), the proportion of the esterifying agent (a2) relative to the total mass of the aqueous medium (the concentration of the esterifying agent (a2)) is preferably 0.1 to 50 mass%, more preferably 0.5 to 20 mass%, and particularly preferably 1 to 15 mass%. By having the aqueous medium having the esterifying agent (a2) at a concentration within the above range absorbed into the raw material fiber, continuous cellulose fibers with improved thermal stability are more likely to be obtained.

[0022] In one embodiment, from the viewpoint of improving thermal stability, the compound (A) preferably contains an esterifying agent (a2), and more preferably contains boric acid.

[0023] The compound (A) may contain other compounds in addition to the glycosylation agent (a1) and the esterification agent (a2). Examples of the other compounds include aluminum hydroxide, calcium hydroxide, dolomite, hydrotalcite, calcium hydroxide, barium hydroxide, basic magnesium carbonate, zirconium hydroxide, and metal hydrates such as tin oxide hydrate. The other compounds may be used alone or in combination of two or more.

[0024] In step (I), the raw fiber is immersed in an aqueous medium to allow the raw fiber to absorb the aqueous medium. Step (I) is preferably carried out under conditions where the immersion length of the raw fiber is 1 to 20 cm and the winding or take-up speed of the raw fiber is 10 to 1,000 m / min. The immersion length can be adjusted arbitrarily within a range of 1 to 20 cm. Similarly, the winding or take-up speed can also be adjusted arbitrarily within a range of 10 to 1,000 m / min. The "immersion length of the raw fiber" refers to the length of the portion of the raw fiber immersed in the aqueous medium. In one embodiment, step (I) may be carried out under conditions where the immersion length of the raw fiber is 1 to 1,000 cm and the winding or take-up speed of the raw fiber is 10 to 1,000 m / min. In this case, the immersion length can be adjusted arbitrarily within the range of 1 to 1,000 cm, and similarly, the winding speed or take-up speed can be adjusted arbitrarily within the range of 10 to 1,000 m / min.

[0025] The temperature of the aqueous medium can be set depending on the solubility of compound (A) in the water component. For example, in the case of boric acid, the saturated aqueous solution concentration at 20°C is less than 5% by mass. Therefore, for example, to prepare a 9% by mass aqueous solution, it is preferable to set the temperature of the aqueous medium to 50°C or higher.

[0026] In a preferred embodiment, step (I) may include adhering compound (A) to the raw fibers by immersing the raw fibers in an aqueous medium and allowing the raw fibers to absorb the aqueous medium. The concentration of compound (A) in the aqueous medium, the immersion length, and / or the winding or take-up speed may be adjusted so that the amount of compound (A) attached is 0.1 to 20% by mass, more preferably 0.3 to 15% by mass, relative to the total mass of the raw fibers. By adhering compound (A) to the raw fibers, preferably to at least a portion of the surface of the raw fibers, the thermal stability improving effect tends to be uniform. In a preferred embodiment, the amount of compound (A) attached may be 0.01 to 20 parts by mass, 0.01 to 10 parts by mass, or 0.03 to 5 parts by mass, relative to 100 parts by mass of the raw fibers. This embodiment is preferably carried out when the compound (A) contains boric acid or contains a glycosylating agent (a1) (preferably containing glycerin, pentaerythritol, or mannitol), which makes it easier to obtain cellulose fibers with a lower rate of weight loss on heating.

[0027] <Step (I')> The manufacturing method according to this embodiment preferably includes adjusting the amount of aqueous medium absorbed by the raw fiber after step (I) (step (I')). Specifically, it is more preferable to adjust the "ratio of the amount of aqueous medium absorbed by the raw fiber to the total mass of the raw fiber before absorbing the aqueous medium" (hereinafter referred to as the "aqueous medium ratio") to 200 mass% or less. Here, the "aqueous medium ratio" represents the sum of the amount of aqueous medium absorbed by the raw fiber and the amount of aqueous medium present in contact with and around the raw fiber. Furthermore, the aqueous medium ratio can be calculated by the formula "aqueous medium ratio (%) = (W2 - W1) / W1 × 100", where W1 is the weight of the raw fiber before absorbing the aqueous medium and W2 is the weight of the raw fiber after absorbing the aqueous medium. If an excessive amount of aqueous medium is absorbed into the raw fiber in step (I) or if the amount of aqueous medium coexisting around the raw fiber is too large, the drying time in step (II) described below may be too long, resulting in a decrease in production efficiency and / or an uneven improvement in thermal stability of the resulting continuous fiber. Therefore, it is preferable to carry out step (I') after step (I) and before step (II). It is particularly preferable to carry out step (I') from the viewpoint of controlling the amount of compound (A) attached to the fiber.

[0028] A preferred method for adjusting the aqueous medium ratio is to compress the raw fiber to remove the aqueous medium coexisting in and / or around the raw fiber, thereby adjusting the aqueous medium ratio to a range of 200% by mass or less. In one embodiment, the aqueous medium ratio may be 150% by mass or less, or may be 100% by mass or less. From the viewpoint of balancing the thermal stability improvement effect with the drying efficiency in step (II), the lower limit of the aqueous medium ratio is preferably 10% by mass or more.

[0029] A preferred method for compressing the raw fibers is to press the raw fibers against a roller or the like. Specifically, it is more preferred to wind or take up the raw fibers that have absorbed the aqueous medium toward a pressure roller or the like, and then bring the raw fibers into contact with the pressure roller so that a certain pressure is applied to the raw fibers, thereby removing the aqueous medium from the raw fibers and adjusting the aqueous medium ratio. In this method, one pressure roller may be used, or two or more pressure rollers may be installed. It is preferable to determine the aqueous medium ratio under specific conditions of immersion length, winding speed, or take-up speed through a preliminary test before carrying out step (I), and set the roller pressure based on this value.

[0030] <Step (II)> The production method according to this embodiment includes further drying the raw fiber after step (I) (or after steps (I) and (I')). The drying temperature for the raw fiber is preferably 10 to 300°C, more preferably 100 to 280°C. As a method for drying the raw fiber, a method combining non-contact drying and contact drying is preferred, from the viewpoint that this method is industrially feasible and also facilitates improving production efficiency. In one embodiment, a drying method combining hot air drying and cylinder drying is more preferred, and it is particularly preferred to carry out cylinder drying after hot air drying. Cylinder drying is a method in which the raw fiber is dried while being in contact with a heated cylinder. That is, it is particularly preferred that step (II) includes drying the raw fiber with hot air, and then further drying the raw fiber while being in contact with a heated cylinder.

[0031] From the viewpoint of drying efficiency, the temperature of the hot air used to dry the raw fiber with hot air is preferably 50 to 260°C, more preferably 80 to 200°C, and even more preferably 100 to 200°C. The air volume is preferably air, and more preferably nitrogen. The time for which hot air drying is carried out (non-contact drying time) can be adjusted as desired by the winding speed, etc. From the viewpoint of drying efficiency and reducing the thermal history of the fiber, the time is preferably 0.01 to 10 minutes, and more preferably 0.1 to 5 minutes.

[0032] It is more preferable to further perform cylinder drying (contact drying) after hot air drying (non-contact drying). From the viewpoints of drying efficiency and reducing the thermal history of the fibers, the cylinder temperature is preferably 50 to 260°C, more preferably 80 to 200°C, and even more preferably 100 to 200°C. Furthermore, from the viewpoint of thermal efficiency, the number of cylinders with which the raw material fibers are brought into contact is preferably 3 to 50, more preferably 5 to 30.

[0033] The production method according to the present embodiment, which includes the above-described steps (I) and (II) (preferably steps (I), (I'), and (II)), is preferably carried out using an apparatus comprising: a storage section for storing raw fiber; an immersion section including a container for immersing the raw fiber; a drying section for drying the raw fiber; and a recovery section for recovering the continuous cellulose fiber with improved thermal stability while winding it, or a take-up section for taking up the continuous cellulose fiber with improved thermal stability and unwinding it for other production steps. By winding the continuous cellulose fiber in the recovery section or taking up the continuous cellulose fiber in the take-up section, the raw fiber can be unwound from the storage section toward the immersion section and the drying section. Below, an example of the production method according to the present embodiment carried out using an apparatus comprising a storage section, an immersion section, a drying section, and a recovery section will be described.

[0034] The raw fiber is wound on a bobbin or the like and stored in the storage unit. The storage unit is large enough to store the bobbin and has a payout mechanism for paying out the raw fiber. It may also have a tensioning device for applying a certain tension to the raw fiber.

[0035] The raw fiber is first unwound from the storage section toward the soaking section. The soaking section is equipped with a container that contains an aqueous medium. A pressure roller is placed above the container on the outlet (drying section) side of the soaking section. After entering the inlet (storage section) side of the soaking section, the raw fiber is immersed in the aqueous medium in the container and wound up at a constant winding speed while absorbing the aqueous medium in the container. The raw fiber is then wound up toward the pressure roller placed on the outlet side of the soaking section to adjust the aqueous medium ratio.

[0036] The raw fiber leaving the immersion section is then wound towards the drying section, which is equipped with a non-contact drying device and a contact drying device. The raw fiber first enters the non-contact drying device and then the contact drying device. The raw fiber that has been heat-treated in the drying section is then wound towards the recovery section.

[0037] As described above, the production method according to this embodiment allows for the industrial production of continuous cellulose fibers with improved thermal stability. When continuous cellulose fibers with improved thermal stability are produced using an apparatus including a storage section, a soaking section, a drying section, and a take-up section, the regenerated cellulose fibers taken up in the take-up section may be fed to another production process, for example, an impregnation die for producing a fiber-reinforced resin.

[0038] Patent Documents 2 and 3 describe the improvement of cellulose thermal stability using compounds such as boric acid and glycerin. Conventional methods involve adding cellulose to an aqueous solution or dispersion containing compounds such as boric acid and glycerin, and then drying the resulting solution or dispersion at high temperatures to react the boric acid or glycerin with the reducing ends or hydroxyl groups of cellulose, thereby improving thermal stability. However, while this method is suitable for batch production, it is unsuitable for producing continuous fibers. Furthermore, the large amount of thermal energy consumed makes it cost-prohibitive for industrial production. The present inventors have discovered that continuous cellulose fibers with improved thermal stability can be produced by immersing continuous cellulose fibers in an aqueous medium containing compounds such as boric acid and glycerin that can react with the reducing ends or hydroxyl groups of cellulose, allowing the fibers to absorb the aqueous medium, and then recovering and drying the continuous cellulose fibers from the aqueous medium. This method not only eliminates the need for prolonged drying, but also surprisingly improves the thermal stability of cellulose to the same extent as when the fibers are dried together with a large amount of aqueous medium.

[0039] The cellulose continuous fiber with improved thermal stability obtained by the production method according to this embodiment is less susceptible to discoloration and performance degradation due to heat treatment, and is therefore suitable for use in fields such as resin modifiers and reinforcing materials, where discoloration and performance degradation due to heat are likely to be problems.

[0040] The present disclosure will be explained in more detail below by showing examples, but interpretation of the present disclosure is not limited to these examples.

[0041] The following materials were used as raw fiber and compound (A). <Raw fiber> Regenerated cellulose fiber: regenerated cellulose fiber (lyocell) obtained by a solvent method. Average fiber diameter: 11 μm, 552 tex, 2700 filaments. <Compound (A)> Glycosylating agent (a1): glycerin. Esterifying agent (a2): boric acid.

[0042] [Examples 1 and 2] Using an apparatus (Minisizer, manufactured by Kaji Seisakusho Co., Ltd., product name "DCC001P") equipped with a storage section, a dipping section, a drying section, and a recovery section, continuous cellulose fibers with improved thermal stability were produced under the conditions shown in Table 1. The thermal stability of the continuous cellulose fibers obtained by the production method of each example was evaluated under the following conditions.

[0043] <Evaluation of Thermal Stability> The continuous cellulose fiber of Example 1 obtained by glycerin treatment was heated in an oven at 260°C for 10 minutes. The continuous cellulose fiber of Example 2 obtained by boric acid treatment was heated in an oven at 240°C for 10 minutes. The color level of the continuous cellulose fiber of each example after heating was evaluated according to the following criteria. The color level of Blank 1 (raw material fiber that was not subjected to the thermal stability improvement treatment and heating test) was assigned Level 1, and the color of Reference Example 1 (raw material fiber that was subjected to the heating test without the thermal stability improvement treatment) was assigned Level 4, and the degree of coloration was compared. (Coloration Level) Level 1: Color tone similar to that of Blank 1. Level 2: Slightly more colored than Blank 1. Level 3: Slightly more colored than Level 2. Level 4: The entire fiber was colored similar to that of Reference Example 1.

[0044]

[0045] As shown in Table 1, it was found that the production method according to this embodiment can produce continuous cellulose fibers with improved thermal stability. The production method according to this embodiment can also be carried out industrially by using, for example, the apparatus used in the examples.

[0046] The production method according to this embodiment can produce continuous cellulose fibers with improved thermal stability in an industrially feasible manner. The continuous cellulose fibers produced by this embodiment are resistant to discoloration and performance degradation due to heating, and are therefore suitable for use in fields such as resin modifiers and reinforcing materials.

Claims

1. A method for producing continuous cellulose fibers having improved thermal stability, comprising: immersing continuous cellulose fibers in an aqueous medium containing a compound (A) capable of reacting with a reducing end or a hydroxyl group of cellulose, allowing the continuous cellulose fibers to absorb the aqueous medium, and then drying the fibers; and the above series of steps are continuously carried out while the continuous cellulose fibers are being wound or taken up.

2. The method for producing continuous cellulose fiber according to claim 1, wherein the compound (A) comprises at least one compound selected from a glycosylating agent (a1) for the reducing end of the cellulose and an esterifying agent (a2) for the hydroxyl group of the cellulose.

3. The method for producing continuous cellulose fibers according to claim 2, wherein the glycosylating agent (a1) contains a monohydric or higher alcohol, and the esterifying agent (a2) contains boric acid.

4. The method for producing continuous cellulose fibers according to any one of claims 1 to 3, wherein the immersion length of the continuous cellulose fibers is 1 to 1,000 cm, and the winding or take-up speed of the continuous cellulose fibers is 10 to 1,000 m / min.

5. A method for producing continuous cellulose fibers according to any one of claims 1 to 3, wherein the concentration of the compound (A) in the aqueous medium is 0.1 to 50 mass%.

6. A method for producing continuous cellulose fibers according to any one of claims 1 to 3, wherein the drying temperature for the continuous cellulose fibers is 10 to 300°C.

7. A method for producing continuous cellulose fibers according to any one of claims 1 to 3, wherein the drying step comprises drying the continuous cellulose fibers with hot air and then further drying the continuous cellulose fibers while contacting them with a heated cylinder.

8. The method for producing continuous cellulose fibers according to any one of claims 1 to 3, wherein the continuous cellulose fibers comprise continuous regenerated cellulose fibers, spun fibers of staple regenerated cellulose, or spun fibers of natural cellulose.

Citation Information

Patent Citations

  • Fine cellulose fiber complex

    JP2018024967A

  • Device for sizing spun yarn and method for sizing the same

    JP1996013320A

  • Method for controlling depolymerization of polysaccharides

    JP2008163053A

  • Method for suppressing discoloration of cellulose at high temperature

    JP2010159364A