Reinforcing film, device having reinforcing film, and method for producing same

The reinforcing film with a photocurable adhesive layer and antistatic properties addresses the challenges of adhesion, peeling, and charging in foldable devices, ensuring reliable adhesion and reduced charging and contamination.

WO2024247886A1PCT designated stage expired Publication Date: 2024-12-05NITTO DENKO CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/019040
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2024-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing reinforcing films for foldable devices face challenges in achieving a balance between low storage elasticity to prevent peeling, high strain recovery properties to maintain shape integrity, and low surface resistance to prevent charging, while also ensuring strong adhesion and preventing wrinkles and contamination.

Method used

A reinforcing film with a photocurable adhesive layer composed of an acrylic base polymer, a photocuring agent, a photopolymerization initiator, and an antistatic agent, featuring a specific monomer unit structure and composition that allows for easy peeling before curing, strong adhesion after curing, and low surface resistance, which is applied to a flexible film base material.

Benefits of technology

The solution provides a reinforcing film that can be easily applied and removed during device assembly, maintains adhesion reliability, suppresses peeling and wrinkles, and effectively reduces charging and contamination, ensuring the integrity and functionality of foldable devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024019040_05122024_PF_FP_ABST
    Figure JP2024019040_05122024_PF_FP_ABST
Patent Text Reader

Abstract

A reinforcing film (10) has an adhesive layer (2) layered and fixed on one main surface of a film substrate (1). The adhesive layer comprises a photocurable composition containing an acrylic base polymer having a crosslinked structure, a photo-curing agent, a photopolymerization initiator and an anti-static agent. The acrylic base polymer includes, as monomer units, an alkyl (meth)acrylate ester; a (meth)acrylic acid ester having an alkylene oxide chain; and one or more selected from the group consisting of a hydroxyl group-containing monomer and a carboxyl group-containing monomer.
Need to check novelty before this filing date? Find Prior Art

Description

Reinforcement film, device with reinforcement film, and method for manufacturing the same

[0001] The present invention relates to a reinforcing film to be attached to the surface of a device, and further to a device including the reinforcing film and a method for manufacturing the same.

[0002] An adhesive film may be attached to the surface of an optical device such as a display or an electronic device for the purpose of surface protection, imparting impact resistance, etc. Such an adhesive film usually has an adhesive layer fixedly laminated on the main surface of a film substrate, and is attached to the device surface via this adhesive layer.

[0003] By temporarily attaching an adhesive film to the surface of a device or a device component before use, such as during device assembly, processing, transportation, etc., it is possible to prevent the adherend from being scratched or damaged. Patent Documents 1 and 2 disclose reinforcing films that have an adhesive layer made of a photocurable adhesive composition on a film substrate.

[0004] This reinforcing film has a high gel fraction and low adhesiveness immediately after application to the adherend, making it easy to remove from the adherend. This allows for reworking from the adherend, and also allows for selective peeling and removal of the reinforcing film from areas of the adherend that do not require reinforcement. The reinforcing film's adhesive firmly bonds to the adherend upon photocuring, permanently bonding the film substrate to the adherend's surface, making it usable as a reinforcing material for protecting the surface of devices, etc.

[0005] In recent years, organic EL panels using bendable substrates (flexible substrates) such as resin films have been put to practical use, and foldable devices (foldable devices) have also been put to practical use. Patent Document 4 proposes using a photocurable adhesive containing an acrylic-based polymer with a low glass transition temperature as an adhesive for the reinforcing film of the foldable device, thereby suppressing peeling of the adhesive layer at the bending points of the foldable device.

[0006] JP 2020-41113 A JP 2020-134540 A JP 2019-20726 A International Publication No. 2022 / 050009

[0007] Foldable devices are repeatedly bent at the same location. At the bent point, compressive stress is applied to the inside and tensile stress to the outside, causing distortion at the bent point and its surrounding area. By designing the adhesive layer of the reinforcing film to have a low storage modulus and a soft texture, distortion at the bent point is alleviated, preventing peeling of the reinforcing film around the bent point and reducing damage to the display element due to stress.

[0008] On the other hand, if the adhesive is soft and has little elasticity, when the foldable device is held in a folded state and then returned to an open state (extended state), the deformation of the adhesive layer does not return to its original state, causing wrinkles and distorting the shape of the device. In order to suppress deformation such as wrinkles at the bending points, the adhesive of the reinforcing film of the foldable device is required to have high adhesive strength to the adherend as well as high shape recovery.

[0009] As described in Patent Document 3, in foldable devices, resin films such as polyimide are used as substrate materials for display elements, which are prone to charging and can cause problems with electrostatic breakdown of the device due to charging (static electricity). In order to suppress charging of a device to which a reinforcing film is attached, it is effective to incorporate an antistatic agent into the adhesive layer provided in contact with the device, thereby reducing the resistance of the adhesive layer and providing antistatic properties. However, even when an antistatic agent is added to the adhesive of the reinforcing film described in Patent Document 4, the adhesive does not sufficiently reduce its resistance. Increasing the amount of antistatic agent added causes the antistatic agent to bleed out, resulting in a decrease in the adhesive strength between the adhesive layer and the device and contamination of the device surface.

[0010] In order to reduce the resistance of the adhesive layer, it is conceivable to blend a polar group-containing compound such as polyol into the adhesive in addition to an antistatic agent. However, since additives such as polyol are low molecular weight components, if the blending amount of the additive is increased to reduce the resistance, the strain recovery of the adhesive will decrease, and deformation such as wrinkles will easily occur at the bending points of the foldable device.

[0011] As described above, it is not easy to achieve all of low storage elasticity (stress relaxation property), strain recovery property, and low resistance for a pressure-sensitive adhesive layer used in a foldable device.

[0012] The present invention aims to provide a reinforcing film that is easy to peel off immediately after being attached to an adherend, can be firmly adhered to the adherend by photocuring the adhesive after being attached to the adherend, is resistant to peeling from the adherend in a bent state, has high strain recovery in the adhesive layer, and can contribute to preventing static electricity in devices.

[0013] The reinforcing film of the present invention includes a pressure-sensitive adhesive layer bonded to one main surface of a film substrate, the pressure-sensitive adhesive layer comprising a photocurable composition containing an acrylic-based polymer, a photocuring agent, a photopolymerization initiator, and an antistatic agent.

[0014] The acrylic base polymer contains, as monomer units, a (meth)acrylic acid alkyl ester; a (meth)acrylic acid ester having an alkylene oxide chain, and a monomer having a crosslinkable functional group. Examples of the monomer having a crosslinkable functional group include a hydroxyl group-containing monomer and a carboxyl group-containing monomer. The weight average molecular weight of the acrylic base polymer before the introduction of a crosslinked structure is preferably 100,000 or more.

[0015] The amount of the (meth)acrylic acid alkyl ester is preferably 40 to 94 parts by weight, and the amount of the (meth)acrylic acid ester having an alkylene oxide chain is preferably 5 to 55 parts by weight, relative to 100 parts by weight of the total of the monomer units of the acrylic base polymer.

[0016] The (meth)acrylic acid ester having an alkylene oxide chain as a monomer unit of the acrylic base polymer is a compound represented by the general formula (1): CH 2 =CR 1 -COO-(R 2 -O) m -R 3 (1)

[0017] R 1 is a hydrogen atom or a methyl group. 2 is an alkylene group having 2 to 4 carbon atoms which may be branched. m is an integer of 1 to 5. R 3 is a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or an aryl group having 6 to 20 carbon atoms.

[0018] The (meth)acrylic acid alkyl ester as a monomer unit of the acrylic base polymer preferably has an alkyl group having 6 or more carbon atoms.

[0019] The content of the photocuring agent in the photocurable composition constituting the pressure-sensitive adhesive layer is preferably 3 to 25 parts by weight per 100 parts by weight of the acrylic base polymer.

[0020] The photocuring agent is preferably a polyfunctional (meth)acrylate. The polyfunctional (meth)acrylate may contain an alkylene oxide chain. In addition to the polyfunctional (meth)acrylate containing an alkylene oxide chain, a urethane (meth)acrylate may also be used as the photocuring agent.

[0021] The surface resistance of the adhesive layer is 5×10 11 The pressure-sensitive adhesive layer preferably has a shear storage modulus of 1.0×10 Ω or less at −20° C. after photocuring. 4 ~5.0 x 10 5 Pa is preferred.

[0022] The adhesive layer preferably has an adhesive strength to the polyimide film of 1 N / 25 mm or less before photocuring, and an adhesive strength to the polyimide film of 5 N / 25 mm or more after photocuring.

[0023] The reinforcing film is attached to the surface of the device, and the pressure-sensitive adhesive layer is photocured to obtain a device with the reinforcing film. The device may be a flexible device that can be bent.

[0024] The reinforcing film of the present invention has a pressure-sensitive adhesive layer made of a photocurable composition, and the adhesive strength to the adherend is increased by photocuring the pressure-sensitive adhesive layer after adhesion to the adherend. Because the adhesive strength to the adherend is low before photocuring, the reinforcing film can be easily peeled off from the adherend.

[0025] The adhesive layer of the reinforcing film contains an antistatic agent, and the acrylic base polymer contains a (meth)acrylic acid ester having an alkylene oxide chain as a monomer unit, resulting in low resistance, which suppresses static buildup in the adhesive layer itself and contributes to anti-static properties of the adherend. Furthermore, the adhesive layer has a low shear storage modulus at low temperatures and excellent stress relaxation, so even when repeatedly bent at the same location, peeling of the adhesive layer at the bent location is suppressed, resulting in excellent adhesion reliability.

[0026] Furthermore, since the pressure-sensitive adhesive layer has a high strain recovery rate, when the adherend is held in a folded state and then returned to an extended state, the shape of the pressure-sensitive adhesive layer is easily restored, and deformation such as wrinkles is unlikely to occur. Therefore, the reinforced film of the present invention can also be suitably used in foldable devices using a resin film substrate.

[0027] 1A and 1B are cross-sectional views showing the layered structure of a reinforcing film, and FIG. 1C are cross-sectional views showing the layered structure of a reinforcing film, and FIG. 1D are cross-sectional views showing a device to which a reinforcing film is attached.

[0028] 1 is a cross-sectional view showing one embodiment of a reinforced film. The reinforced film 10 includes a pressure-sensitive adhesive layer 2 on one main surface of a film substrate 1. The pressure-sensitive adhesive layer 2 is fixedly laminated on one main surface of the film substrate 1. The pressure-sensitive adhesive layer 2 is a photocurable pressure-sensitive adhesive made of a photocurable composition, and is cured by irradiation with actinic rays such as ultraviolet light, thereby increasing the adhesive strength with the adherend.

[0029] Fig. 2 is a cross-sectional view of a reinforced film having a release liner 5 temporarily attached to the main surface of a pressure-sensitive adhesive layer 2. Fig. 3 is a cross-sectional view showing a state in which a reinforced film 10 is attached to the surface of a device 20.

[0030] The release liner 5 is peeled off and removed from the surface of the adhesive layer 2, and the exposed surface of the adhesive layer 2 is attached to the surface of the device 20, thereby attaching the reinforcement film 10 to the surface of the device 20. In this state, the adhesive layer 2 has not yet been photocured, and the reinforcement film 10 (adhesive layer 2) is temporarily attached to the device 20. By photocuring the adhesive layer 2, the adhesive strength at the interface between the device 20 and the adhesive layer 2 increases, and the device 20 and the reinforcement film 10 are fixed together.

[0031] "Fixed" means that the two laminated layers are firmly bonded together, making it difficult or impossible to separate them at their interface. "Temporary adhesion" means that the adhesive strength between the two laminated layers is weak, making them easy to separate at their interface.

[0032] In the reinforced film shown in Figure 2, a film substrate 1 and a pressure-sensitive adhesive layer 2 are bonded together, and a release liner 5 is temporarily attached to the pressure-sensitive adhesive layer 2. When the film substrate 1 and the release liner 5 are peeled apart, peeling occurs at the interface between the pressure-sensitive adhesive layer 2 and the release liner 5, and the pressure-sensitive adhesive layer 2 remains bonded to the film substrate 1. No pressure-sensitive adhesive remains on the release liner 5 after peeling.

[0033] In the device with the reinforced film shown in Figure 3, before the photo-curing of the adhesive layer 2, the device 20 and the adhesive layer 2 are in a temporarily bonded state. When the film substrate 1 and the device 20 are peeled apart, the peeling occurs at the interface between the adhesive layer 2 and the device 20, so the adhesive layer 2 remains fixed to the film substrate 1. Because no adhesive remains on the device 20, peeling operations such as rework and cutting are easy. After the photo-curing of the adhesive layer 2, the adhesive strength between the adhesive layer 2 and the device 20 increases, resulting in a fixed state, making it difficult to peel the reinforced film 10 from the device 20.

[0034] [Film substrate] A flexible plastic film is used as the film substrate 1 of the reinforcing film 10. In order to bond the film substrate 1 and the pressure-sensitive adhesive layer 2 together, it is preferable that the surface of the film substrate 1 to which the pressure-sensitive adhesive layer 2 is to be attached is not subjected to a release treatment.

[0035] The thickness of the film substrate is, for example, about 4 to 150 μm. From the viewpoint of reinforcing the device by imparting rigidity and cushioning impact, the thickness of the film substrate 1 is preferably 5 μm or more, more preferably 12 μm or more, even more preferably 20 μm or more, and particularly preferably 25 μm or more. From the viewpoint of imparting flexibility to the reinforcing film so that it can be folded, the thickness of the film substrate 1 is preferably 125 μm or less, more preferably 100 μm or less. From the viewpoint of achieving both mechanical strength and flexibility, the compressive strength of the film substrate 1 is 100 to 3000 kg / cm 2 is preferred, and 200 to 2900 kg / cm 2 More preferably, 300 to 2800 kg / cm 2 is more preferably 400 to 2700 kg / cm 2 is particularly preferred.

[0036] Examples of plastic materials constituting the film substrate 1 include polyester-based resins, polyolefin-based resins, cyclic polyolefin-based resins, polyamide-based resins, polyimide-based resins, polyether ether ketone, polyethersulfone, polyarylate-based resins, and aramid-based resins. In a reinforcing film for an optical device such as a display, the film substrate 1 is preferably a transparent film. Furthermore, when photocuring of the pressure-sensitive adhesive layer 2 is performed by irradiating actinic rays from the film substrate 1 side, the film substrate 1 is preferably transparent to the actinic rays used to cure the pressure-sensitive adhesive layer. Polyester-based resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate, transparent polyimides, and transparent aramids are preferably used because they combine mechanical strength and transparency. When irradiating actinic rays from the adherend side, the adherend only needs to be transparent to actinic rays, and the film substrate 1 does not need to be transparent to actinic rays.

[0037] A functional coating such as an easy-adhesion layer, an easy-slip layer, a release layer, an antistatic layer, a hard coat layer, or an antireflection layer may be provided on the surface of the film substrate 1. As described above, in order to bond the film substrate 1 and the pressure-sensitive adhesive layer 2 together, it is preferable that no release layer is provided on the surface of the film substrate 1 to which the pressure-sensitive adhesive layer 2 is to be attached.

[0038] [Adhesive Layer] The adhesive layer 2, which is fixedly laminated on the film substrate 1, is made of a photocurable composition. The photocurable composition constituting the adhesive layer 2 contains an acrylic-based polymer, a photocuring agent, and a photopolymerization initiator, and further contains an antistatic agent.

[0039] The pressure-sensitive adhesive layer 2 has low adhesive strength to adherends such as devices and device components before photocuring, and is therefore easy to peel off. The adhesive strength of the pressure-sensitive adhesive layer 2 to adherends is improved by photocuring, so the reinforcing film is less likely to peel off from the device surface even when the device is in use, and adhesion reliability is excellent.

[0040] Photocurable pressure-sensitive adhesives hardly cure under normal storage conditions, but cure when exposed to actinic rays such as ultraviolet rays. Therefore, the reinforcing film of the present invention has the advantage that the timing of curing of the pressure-sensitive adhesive layer 2 can be set as desired, allowing for flexible adaptation to process lead times, etc.

[0041] <Base Polymer> The base polymer is the main component of the pressure-sensitive adhesive composition and is a key element that determines various properties of the pressure-sensitive adhesive layer, such as adhesive strength and storage modulus. In the present invention, an acrylic polymer is used as the base polymer of the pressure-sensitive adhesive. Acrylic polymers have excellent optical transparency and adhesive properties, and their adhesive strength, storage modulus, etc. can be easily controlled.

[0042] The acrylic base polymer contains a (meth)acrylic acid alkyl ester as a monomer component. The acrylic base polymer used in the present invention is a copolymer containing, as monomer components, a (meth)acrylic acid ester having an alkylene oxide chain and a monomer having a crosslinkable functional group in addition to the (meth)acrylic acid alkyl ester.

[0043] ((Meth)acrylic acid alkyl ester) As the (meth)acrylic acid alkyl ester, a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 20 carbon atoms is suitably used. From the viewpoint of lowering the glass transition temperature of the acrylic base polymer and reducing the storage modulus, thereby suppressing peeling of the pressure-sensitive adhesive layer when repeatedly flexed, it is preferred that the alkyl group of the (meth)acrylic acid alkyl ester be a chain alkyl group. The chain alkyl group may be linear or branched.

[0044] Examples of (meth)acrylic acid alkyl esters having a chain alkyl group include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, and methyl (meth)acrylate. Examples of the acrylate include nonyl acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, isotridecyl (meth)acrylate, tetradecyl (meth)acrylate, isotetradecyl (meth)acrylate, pentadecyl (meth)acrylate, cetyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, isooctadecyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate.

[0045] Among the exemplified (meth)acrylic acid alkyl esters, from the viewpoint of lowering the glass transition temperature of the acrylic base polymer, (meth)acrylic acid alkyl esters having a glass transition temperature of the homopolymer of −56° C. or less are preferred. In order to lower the glass transition temperature of the homopolymer, the number of carbon atoms in the alkyl group of the (meth)acrylic acid alkyl ester is preferably 6 or more. The number of carbon atoms in the alkyl group of the (meth)acrylic acid alkyl ester may be 20 or less, 12 or less, 10 or less, or 9 or less.

[0046] Specific examples of (meth)acrylic acid alkyl esters having a homopolymer glass transition temperature (Tg) of −56° C. or lower include 2-ethylhexyl acrylate (Tg: −70° C.), n-hexyl acrylate (Tg: −65° C.), n-heptyl acrylate, n-octyl acrylate (Tg: −65° C.), isononyl acrylate (Tg: −60° C.), n-nonyl acrylate (Tg: −58° C.), isooctyl acrylate (Tg: −58° C.), etc. Among these, 2-ethylhexyl acrylate, n-heptyl acrylate, and n-octyl acrylate are preferred, with n-octyl acrylate being particularly preferred, because they can reduce the storage modulus at around −20° C.

[0047] As the (meth)acrylic acid alkyl ester, (meth)acrylic acid C having an alkyl group with 6 to 9 carbon atoms 6-9 an alkyl ester and a (meth)acrylic acid C having an alkyl group with 10 to 20 carbon atoms; 10-20 Alkyl esters may be used in combination. (Meth)acrylic acid C 10-20 The alkyl ester is (meth)acrylic acid C 6-9 Although the Tg of the homopolymer is higher than that of the alkyl ester, there is a temperature region (plateau region) in the vicinity of the Tg where the temperature dependence of the viscoelasticity is small. Therefore, the acrylic base polymer is preferably a polymer containing (meth)acrylic acid C as a monomer component. 6-9 In addition to alkyl esters, (meth)acrylic acid C 10-20 By including an alkyl ester, the temperature dependency of the storage modulus in the low temperature range is reduced, which may prevent warping of the adherend due to temperature changes and peeling of the reinforcing film from the adherend.

[0048] Since the temperature range of the plateau region is wide and the storage modulus in the plateau region is small, (meth)acrylic acid C 10-20 Among the chain alkyl esters, (meth)acrylic acid C 12-18Among them, dodecyl (meth)acrylate and isostearyl (meth)acrylate are preferred, and dodecyl acrylate (also known as lauryl acrylate) is particularly preferred. As the (meth)acrylic acid alkyl ester, (meth)acrylic acid C 6-9 alkyl ester and (meth)acrylic acid C 10-20 When alkyl esters are used in combination, a combination of 2-ethylhexyl acrylate or n-octyl acrylate with dodecyl acrylate is particularly preferred.

[0049] ((Meth)acrylic acid ester having an alkylene oxide chain) The (meth)acrylic acid ester having an alkylene oxide chain is an ester of (meth)acrylic acid and an alcohol having an alkylene oxide chain, and is a compound represented by the following general formula (1): CH 2 =CR 1 -COO-(R 2 -O) m -R 3 (1)

[0050] R in general formula (1) 1 is a hydrogen atom or a methyl group, and R 1 is a hydrogen atom, the compound of formula (1) is an acrylate, 1 The compound of formula (1) in which R is a methyl group is a methacrylate. 1 is preferably a hydrogen atom.

[0051] R in general formula (1) 2 is an alkylene group having 2 to 4 carbon atoms which may be branched, and —R 2 -O- is an alkylene oxide chain. 2 By making the carbon number of R be 2 to 4, the resistance of the adhesive can be reduced and the compatibility between the acrylic base polymer and the photocuring agent can be improved. 2 Alkylene oxide-R having 2 to 4 carbon atoms 2 Specific examples of —O— include ethylene oxide (—CH 2 CH 2 -O-), propylene oxide (-CH(CH 3) CH 2 —O—), butylene oxide (—CH 2 CH 2 CH 2 CH 2 -O-).

[0052] In general formula (1), m is the number of repeating alkylene oxide units and is an integer from 1 to 5. When the number of repeating alkylene oxide units, m, is 5 or less, an acrylic base polymer with a high molecular weight (for example, a weight average molecular weight of 100,000 or more) can be easily obtained. When m is excessively large, the (meth)acrylate compound represented by general formula (1) tends to act as a chain transfer agent, and the molecular weight of the acrylic base polymer as a polymer does not become sufficiently large, which may result in insufficient adhesive strength of the pressure-sensitive adhesive.

[0053] R 3 is a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or an aryl group having 6 to 20 carbon atoms. From the viewpoint of lowering the Tg of the acrylic base polymer and improving the compatibility with the photocuring agent, R 3 is preferably an alkyl group having 1 to 3 carbon atoms, and is particularly preferably a methyl group or an ethyl group.

[0054] In the general formula (1), m=1, R 3 In the general formula (1), a compound in which m≧2, R 3 The compound in which is an alkyl group is a (meth)acrylic acid polyalkylene glycol ester.

[0055] Specific examples of the compound represented by general formula (1) include methoxyethyl (meth)acrylate, phenoxyethyl (meth)acrylate, ethoxyethoxyethyl (meth)acrylate, methoxydipropylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, etc. Among these, from the viewpoint of lowering the Tg of the acrylic base polymer and reducing the storage modulus of the pressure-sensitive adhesive layer at low temperatures, methoxyethyl acrylate (glass transition temperature of homopolymer: −50° C.) is particularly preferred.

[0056] (Monomer Having a Crosslinkable Functional Group) The monomer having a crosslinkable functional group is specifically a hydroxy group-containing monomer and a carboxy group-containing monomer. The acrylic base polymer may have both a hydroxy group-containing monomer and a carboxy group-containing monomer as monomer components, or may have only one of them. The introduction of a crosslinked structure into the acrylic base polymer tends to improve the cohesive strength and improve the releasability of the pressure-sensitive adhesive layer 2 from the adherend before photocuring.

[0057] Examples of hydroxy group-containing monomers include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, 4-(hydroxymethyl)cyclohexylmethyl (meth)acrylate, etc. Among these, 2-hydroxyethyl acrylate and 4-hydroxybutyl acrylate are preferred because they contribute significantly to improving the adhesive strength of the pressure-sensitive adhesive after photocuring.

[0058] Examples of the carboxy group-containing monomer include (meth)acrylic acid, 2-carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, etc. Among these, acrylic acid is particularly preferred because it contributes greatly to improving adhesive strength.

[0059] (Monomer Ratio) It is preferable that the amount of the (meth)acrylic acid alkyl ester is 40 to 94 parts by weight and the amount of the (meth)acrylic acid ester having an alkylene oxide chain is 5 to 55 parts by weight relative to 100 parts by weight of the total of the constituent monomer components of the acrylic base polymer.

[0060] The (meth)acrylic acid ester having an alkylene oxide chain is a component that contributes to improving the compatibility between the base polymer and the photocuring agent and reducing the resistance of the adhesive, and the higher the ratio in the acrylic base polymer, the lower the resistance of the adhesive layer tends to be. The amount of the (meth)acrylic acid ester having an alkylene oxide chain is preferably 5 parts by weight or more, more preferably 8 parts by weight or more, even more preferably 10 parts by weight or more, and may be 15 parts by weight or more or 20 parts by weight or more, relative to 100 parts by weight of the total of the constituent monomer components of the acrylic base polymer.

[0061] The higher the ratio of (meth)acrylic acid ester having an alkylene oxide chain, the lower the pressure-sensitive adhesive resistance tends to be. However, if the ratio of (meth)acrylic acid ester having an alkylene oxide chain is too high, the compatibility with the photocuring agent becomes excessive, resulting in a high adhesive strength (initial adhesive strength) between the pressure-sensitive adhesive layer and the adherend before photocuring, which may make peeling difficult. Furthermore, as the ratio of (meth)acrylic acid ester having an alkylene oxide chain increases, the ratio of (meth)acrylic acid alkyl ester decreases relatively, which may increase the glass transition temperature of the acrylic base polymer and reduce adhesion at low temperatures. Therefore, the amount of (meth)acrylic acid ester having an alkylene oxide chain is preferably 55 parts by weight or less, more preferably 50 parts by weight or less, even more preferably 45 parts by weight or less, and may be 40 parts by weight or less, 35 parts by weight or less, 30 parts by weight or less, or 25 parts by weight or less, relative to 100 parts by weight of the total monomer components constituting the acrylic base polymer.

[0062] From the viewpoint of lowering the glass transition temperature of the acrylic base polymer, the amount of the (meth)acrylic acid alkyl ester is preferably 40 parts by weight or more, more preferably 50 parts by weight or more, even more preferably 60 parts by weight or more, and may be 65 parts by weight or more, 70 parts by weight or more, 75 parts by weight or more, or 80 parts by weight or more, relative to 100 parts by weight of the total of the constituent monomer components of the acrylic base polymer.

[0063] On the other hand, as the ratio of the (meth)acrylic acid alkyl ester increases, the ratio of the (meth)acrylic acid ester having an alkylene oxide chain relatively decreases, and the compatibility between the acrylic base polymer and the photocuring agent may decrease. The amount of the (meth)acrylic acid alkyl ester is preferably 94 parts by weight or less, more preferably 90 parts by weight or less, and even more preferably 87 parts by weight or less, and may be 85 parts by weight or less, 83 parts by weight or less, 80 parts by weight or less, or 77 parts by weight or less, relative to 100 parts by weight of the total of the constituent monomer components of the acrylic base polymer.

[0064] The acrylic base polymer may contain two or more types of (meth)acrylic acid alkyl esters as monomer components. The two or more types of (meth)acrylic acid alkyl esters may include those having a homopolymer glass transition temperature of −56° C. or lower and those having a homopolymer glass transition temperature higher than −56° C., and may include those having an alkyl group with 6 or more carbon atoms and those having an alkyl group with 5 or less carbon atoms. As mentioned above, they may include those having an alkyl group with 6 to 9 carbon atoms and those having an alkyl group with 10 to 20 carbon atoms.

[0065] From the viewpoint of lowering the glass transition temperature of the acrylic base polymer, it is preferable that the amount of the (meth)acrylic acid alkyl ester having an alkyl group with 6 or more carbon atoms is within the above range. 6-9 The amount of alkyl ester may be within the above range, the total of 2-ethylhexyl acrylate, n-heptyl acrylate, and n-octyl acrylate may be within the above range, or the amount of n-octyl acrylate may be within the above range.

[0066] As the (meth)acrylic acid alkyl ester, (meth)acrylic acid C 6-9 alkyl ester and (meth)acrylic acid C 10-20 When alkyl ester is contained, (meth)acrylic acid C is preferably used relative to 100 parts by weight of the total amount of the constituent monomer components of the acrylic polymer. 6-9 The amount of alkyl ester is preferably 15 to 84 parts by weight, and (meth)acrylic acid C 10-20The amount of alkyl ester is preferably 10 to 79 parts by weight. 6-9 The amount of alkyl ester may be 20 to 70 parts by weight, 30 to 60 parts by weight, 35 to 55 parts by weight, or 40 to 50 parts by weight, and (meth)acrylic acid C 10-20 The amount of alkyl ester may be 15 to 60 parts by weight, 20 to 50 parts by weight, 25 to 45 parts by weight, or 30 to 40 parts by weight.

[0067] The amount of the monomer having a crosslinkable functional group (total amount of hydroxy group-containing monomer and carboxy group-containing monomer) relative to 100 parts by weight of the total of the constituent monomer components of the acrylic base polymer is preferably 0.5 to 15 parts by weight, more preferably 1 to 10 parts by weight, and even more preferably 1.5 to 7 parts by weight. When the acrylic base polymer contains a hydroxy group, the pressure-sensitive adhesive layer tends to have a high strain recovery rate and high shape restoring property, so the acrylic base polymer preferably contains a hydroxy group-containing monomer as a constituent monomer component, and the content of the hydroxy group-containing monomer is preferably within the above range.

[0068] The total amount of the (meth)acrylic acid alkyl ester and the (meth)acrylic acid ester having an alkylene oxide chain relative to a total of 100 parts by weight of the constituent monomer components of the acrylic base polymer is preferably 60 parts by weight or more, more preferably 70 parts by weight or more, even more preferably 80 parts by weight or more, and may be 85 parts by weight or more, 90 parts by weight or more, 93 parts by weight or more, or 95 parts by weight or more.

[0069] The total amount of the (meth)acrylic acid alkyl ester and the monomer having a functional group crosslinkable with the (meth)acrylic acid ester having an alkylene oxide chain relative to a total of 100 parts by weight of the constituent monomer components of the acrylic base polymer is preferably 65 parts by weight or more, more preferably 75 parts by weight or more, even more preferably 85 parts by weight or more, and may be 90 parts by weight or more, 95 parts by weight or more, 98 parts by weight or more, 99 parts by weight or more, or 100 parts by weight.

[0070] (Other Monomers) The acrylic base polymer may contain a monomer other than those described above as a constituent monomer component. Examples of the other monomers include nitrogen-containing monomers such as N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, N-acryloylmorpholine, N-vinylcarboxylic acid amides, and N-vinylcaprolactam. Examples of the other monomers include vinyl ester monomers, aromatic vinyl monomers, epoxy group-containing monomers, vinyl ether monomers, sulfo group-containing monomers, phosphate group-containing monomers, and acid anhydride group-containing monomers.

[0071] (Glass transition temperature) The glass transition temperature of the acrylic base polymer is preferably −40° C. or lower, more preferably −45° C. or lower, and may be −50° C. or lower or −55° C. or lower. When the glass transition temperature is sufficiently lower than the ambient temperature of the device, the storage modulus of the pressure-sensitive adhesive layer in the ambient temperature range of the device tends to be small, and peeling during repeated bending tends to be suppressed. The lower limit of the glass transition temperature of the acrylic base polymer is not particularly limited, but is generally −80° C. or higher, and may be −75° C. or higher or −70° C. or higher.

[0072] The glass transition temperature is the temperature (peak top temperature) at which the loss tangent tanδ in viscoelasticity measurement is maximized. Instead of the glass transition temperature determined by viscoelasticity measurement, the theoretical Tg calculated by Fox's formula may be used. The theoretical Tg is the glass transition temperature Tg of a homopolymer of the constituent monomer components of the acrylic base polymer. i and the weight fraction W of each monomer component i It is calculated by the following Fox formula: 1 / Tg=Σ(W i / Tg i )

[0073] Tg is the glass transition temperature of the polymer chain (unit: K), W i is the weight fraction of the monomer component i constituting the segment (copolymerization ratio based on weight), Tg iis the glass transition temperature (unit: K) of a homopolymer of monomer component i. The glass transition temperature of a homopolymer can be determined from the values ​​listed in Polymer Handbook, 3rd Edition (John Wiley & Sons, Inc., 1989). The Tg of a homopolymer of a monomer not listed in the above publication can be determined from the peak top temperature of tan δ measured by dynamic viscoelasticity measurement.

[0074] (Polymerization of Acrylic Polymer) The above monomer components are polymerized by various known methods such as solution polymerization, emulsion polymerization, and bulk polymerization to obtain an acrylic polymer as a base polymer. Solution polymerization is preferred from the viewpoint of cost and the balance of properties such as adhesive strength and holding power of the pressure-sensitive adhesive. Ethyl acetate, toluene, etc. are used as the solvent for solution polymerization. The solution concentration is usually about 20 to 80% by weight. Various known polymerization initiators such as azo-based and peroxide-based initiators can be used. A chain transfer agent may be used to adjust the molecular weight. The reaction temperature is usually about 50 to 80°C, and the reaction time is usually about 1 to 8 hours.

[0075] From the viewpoint of increasing the adhesive strength of the pressure-sensitive adhesive layer after photocuring, the weight-average molecular weight of the acrylic base polymer is preferably 100,000 or more, more preferably 150,000 or more, even more preferably 200,000 or more, and may be 300,000 or more, 400,000 or more, or 500,000 or more. As described above, when the number of repeating units of alkylene oxide in the (meth)acrylic acid ester having an alkylene oxide chain (m in general formula (1)) is small, the action of the monomer as a chain transfer agent is small, and therefore a high-molecular-weight acrylic polymer can be easily obtained.

[0076] From the viewpoints of handleability of the pressure-sensitive adhesive composition, compatibility with the photocuring agent, etc., the weight-average molecular weight of the acrylic base polymer is preferably 2,000,000 or less, more preferably 1,500,000 or less, even more preferably 1,200,000 or less, and may be 1,000,000 or less or 900,000 or less. As described below, a crosslinked structure is introduced into the acrylic base polymer, and the molecular weight of the acrylic base polymer refers to the molecular weight before the crosslinked structure is introduced.

[0077] <Crosslinking Agent> From the viewpoint of imparting an appropriate cohesive strength to the pressure-sensitive adhesive, thereby enabling the pressure-sensitive adhesive layer to exhibit adhesive strength, and ensuring the peelability of the pressure-sensitive adhesive layer from the adherend before photocuring, it is preferable that a crosslinked structure be introduced into the base polymer. For example, the crosslinked structure is introduced by adding a crosslinking agent to a solution obtained by polymerizing an acrylic base polymer, and then heating the solution as necessary.

[0078] Examples of crosslinking agents include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, carbodiimide-based crosslinking agents, and metal chelate-based crosslinking agents. These crosslinking agents react with functional groups such as hydroxy groups and carboxy groups introduced into the acrylic base polymer to form a crosslinked structure. Isocyanate-based crosslinking agents and epoxy-based crosslinking agents are preferred because they are highly reactive with the hydroxy groups and carboxy groups of the acrylic base polymer and facilitate the introduction of crosslinked structures. When the acrylic base polymer has hydroxy groups as crosslinkable functional groups, isocyanate-based crosslinking agents are preferred, and when the acrylic base polymer has carboxy groups as crosslinkable functional groups, epoxy-based crosslinking agents are preferred.

[0079] As the isocyanate-based crosslinking agent, a polyisocyanate having two or more isocyanate groups per molecule is used. The isocyanate-based crosslinking agent may be one having three or more isocyanate groups per molecule. Examples of the isocyanate-based crosslinking agent include lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate; alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate and isophorone diisocyanate; aromatic isocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate and xylylene diisocyanate; trimethylolpropane / trilene diisocyanate; Examples of the isocyanate adduct include a diisocyanate trimer adduct (e.g., "Takenate D101E" manufactured by Mitsui Chemicals), a trimethylolpropane / hexamethylene diisocyanate trimer adduct (e.g., "Coronate HL" manufactured by Tosoh), a trimethylolpropane adduct of xylylene diisocyanate (e.g., "Takenate D110N" manufactured by Mitsui Chemicals), and an isocyanurate of hexamethylene diisocyanate (e.g., "Coronate HX" manufactured by Tosoh).

[0080] The epoxy crosslinking agent is a polyfunctional epoxy compound having two or more epoxy groups in one molecule. The epoxy crosslinking agent may have three or more or four or more epoxy groups in one molecule. The epoxy group of the epoxy crosslinking agent may be a glycidyl group. Examples of epoxy crosslinking agents include N,N,N',N'-tetraglycidyl-m-xylylenediamine, diglycidylaniline, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, sorbitol polyglycidyl ether, glycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, polyglycerol polyglycidyl ether, sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, adipic acid diglycidyl ester, o-phthalic acid diglycidyl ester, triglycidyl tris(2-hydroxyethyl)isocyanurate, resorcinol diglycidyl ether, and bisphenol-S-diglycidyl ether. As the epoxy-based crosslinking agent, commercially available products such as "Denacol" manufactured by Nagase ChemteX, and "Tetrad X" and "Tetrad C" manufactured by Mitsubishi Gas Chemical Company, may be used.

[0081] The amount of crosslinking agent used may be adjusted appropriately depending on the composition, molecular weight, etc. of the acrylic base polymer. The amount of crosslinking agent used is about 0.01 to 5 parts by weight, preferably 0.03 to 3 parts by weight, more preferably 0.05 to 1 part by weight, and may be 0.08 to 0.8 parts by weight, or 0.1 to 0.5 parts by weight, relative to 100 parts by weight of the acrylic base polymer.

[0082] A crosslinking catalyst may be used to promote the formation of a crosslinked structure. Examples of the crosslinking catalyst include organometallic compounds such as organometallic complexes (chelates), compounds of metals and alkoxy groups, and compounds of metals and acyloxy groups; as well as tertiary amines. In particular, organometallic compounds are preferred from the viewpoint of suppressing the progress of the crosslinking reaction in a solution state at room temperature and ensuring the pot life of the pressure-sensitive adhesive composition. Examples of metals in organometallic compounds include iron, tin, aluminum, zirconium, zinc, titanium, lead, and cobalt. The amount of the crosslinking catalyst used is generally 0.5 parts by weight or less per 100 parts by weight of the acrylic base polymer.

[0083] <Photocuring agent> The pressure-sensitive adhesive composition constituting the pressure-sensitive adhesive layer 2 contains, in addition to the base polymer, a compound having two or more photopolymerizable functional groups per molecule as a photocuring agent. Pressure-sensitive adhesive compositions containing a photocuring agent have photocurability, and when photocuring is performed after lamination with an adherend, the adhesive strength to the adherend is improved.

[0084] The photopolymerizable functional group is preferably one that is polymerizable by a photoradical reaction, and the photocuring agent is preferably a compound having two or more ethylenically unsaturated bonds in one molecule, and polyfunctional (meth)acrylates are preferred because of their high compatibility with acrylic base polymers.

[0085] It is preferable to use a polyfunctional (meth)acrylate as the photocuring agent because it has high compatibility with the acrylic base polymer. The polyfunctional (meth)acrylate is typically an ester of a polyol and (meth)acrylic acid. Specific examples of the polyfunctional (meth)acrylate include polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, alkanediol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, isocyanuric acid di(meth)acrylate, isocyanuric acid tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol di(meth)acrylate, and trimethylolpropane di(meth)acrylate. Examples of the acrylate include ethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol poly(meth)acrylate, dipentaerythritol hexa(meth)acrylate, neopentyl glycol di(meth)acrylate, glycerin di(meth)acrylate, urethane (meth)acrylate, epoxy (meth)acrylate, butadiene (meth)acrylate, and isoprene (meth)acrylate.

[0086] The polyfunctional (meth)acrylate may be an ester of an alkylene oxide-modified polyol and (meth)acrylic acid. Examples of the alkylene oxide include ethylene oxide (EO) and propylene oxide (PO). The alkylene oxide may be a polyalkylene oxide such as polyethylene glycol or polypropylene glycol.

[0087] Specific examples of alkylene oxide-modified polyfunctional (meth)acrylates include bisphenol A ethylene oxide-modified di(meth)acrylate, bisphenol A propylene oxide-modified di(meth)acrylate, trimethylolpropane ethylene oxide-modified tri(meth)acrylate, trimethylolpropane propylene oxide-modified tri(meth)acrylate, isocyanuric acid ethylene oxide-modified di(meth)acrylate, isocyanuric acid propylene oxide-modified di(meth)acrylate, isocyanuric acid ethylene oxide-modified tri(meth)acrylate, isocyanuric acid propylene oxide-modified tri(meth)acrylate, pentaerythritol ethylene oxide-modified tetra(meth)acrylate, and pentaerythritol propylene oxide-modified tetra(meth)acrylate.

[0088] In polyfunctional (meth)acrylates containing alkylene oxide chains, such as polyalkylene glycol di(meth)acrylates and alkylene oxide-modified polyfunctional (meth)acrylates, the alkylene oxide is preferably (poly)ethylene oxide or (poly)propylene oxide, with (poly)ethylene oxide being particularly preferred. The chain length (number of repeating units of alkylene oxide) n of the alkylene oxide is approximately 1 to 15. When multiple alkylene oxide chains are contained in one molecule, the average chain length n is preferably 1 to 15. The (average) chain length n of the alkylene oxide chain may be 12 or less, 10 or less, 8 or less, 6 or less, 5 or less, 4 or less, or 3 or less. By adjusting the type and chain length of the alkylene oxide, compatibility with the acrylic base polymer can be adjusted to an appropriate range.

[0089] From the viewpoint of compatibility with the acrylic base polymer, the molecular weight of the polyfunctional (meth)acrylate as the photocuring agent is preferably 1500 or less, more preferably 1000 or less, and may be 800 or less, 500 or less, or 400 or less. From the viewpoint of achieving both compatibility with the base polymer and improved adhesive strength after photocuring, the functional group equivalent (g / eq) of the polyfunctional (meth)acrylate is preferably 500 or less, more preferably 400 or less, and may be 300 or less, 250 or less, 200 or less, 180 or less, or 160 or less. On the other hand, if the functional group equivalent of the polyfunctional (meth)acrylate is excessively small, the crosslinking point density of the pressure-sensitive adhesive layer after photocuring increases, resulting in an increased storage modulus and reduced adhesiveness at low temperatures. Therefore, the functional group equivalent of the photocuring agent is preferably 80 or more, more preferably 100 or more, and may be 120 or more or 130 or more.

[0090] As described above, polyfunctional (meth)acrylates have excellent compatibility with acrylic base polymers. However, polyfunctional (meth)acrylates having alkylene oxide chains have higher polarity than polyfunctional (meth)acrylates not having alkylene oxide chains, and therefore have lower compatibility with acrylic polymers, particularly with acrylic polymers having a small amount of polar functional groups.

[0091] A (meth)acrylic acid alkyl ester having an alkyl group with 6 or more carbon atoms has a relatively small volume ratio of alkylene oxide chains and therefore has low polarity compared to a (meth)acrylic acid alkyl ester having a small alkyl group with a small number of carbon atoms (for example, butyl acrylate having an alkyl group with 4 carbon atoms).

[0092] Acrylic polymers with a high ratio of (meth)acrylic acid alkyl esters in which the alkyl group has 6 or more carbon atoms have low polarity and therefore low compatibility with polyfunctional (meth)acrylates having alkylene oxide chains. Therefore, when an acrylic polymer with a high ratio of (meth)acrylic acid alkyl esters in which the alkyl group has 6 or more carbon atoms is blended with a polyfunctional (meth)acrylate having an alkylene oxide chain as a photocuring agent, problems such as bleeding of the photocuring agent may occur.

[0093] As mentioned above, the acrylic base polymer contains, as a monomer component, a (meth)acrylic acid ester having an alkylene oxide chain in addition to a (meth)acrylic acid alkyl ester having an alkyl group with 6 or more carbon atoms, which increases polarity and therefore exhibits compatibility with polyfunctional (meth)acrylates having alkylene oxide chains. Furthermore, the pressure-sensitive adhesive tends to have low resistance when both the acrylic base polymer and the photocuring agent contain alkylene oxide chains.

[0094] By adjusting the ratio of (meth)acrylic acid ester having an alkylene oxide chain in the constituent monomer components of the acrylic base polymer, it is possible to adjust the compatibility with the photocuring agent having an alkylene oxide chain. As mentioned above, if the (meth)acrylic acid ester having an alkylene oxide chain is not contained or if the ratio of the (meth)acrylic acid ester having an alkylene oxide chain is low, the compatibility with the photocuring agent is low, which can cause the photocuring agent to bleed out, etc.

[0095] On the other hand, if the acrylic base polymer has a polarity that makes it incompatible with the photocuring agent (a (meth)acrylic acid ester having an alkylene oxide chain), the photocuring agent tends to be unevenly distributed on the surface of the pressure-sensitive adhesive layer (near the adhesive interface with the adherend), and even if the amount of photocuring agent blended is small, the photocuring agent unevenly distributed at the adhesive interface with the adherend tends to form an adhesion-inhibiting layer (Weak Boundary Layer; WBL).

[0096] When a WBL is formed, the adhesive layer retains its bulk properties, such as its storage modulus, while the liquid properties of the surface (adhesive interface) become stronger, tending to reduce the adhesive strength with the adherend. Therefore, the adhesive layer before photocuring is easy to peel from the adherend. When a WBL is formed on an adhesive layer in which the photocuring agent is unevenly distributed near the adhesive interface with the adherend, the curing reaction of the photocuring agent is likely to proceed near the adhesive interface where the photocuring agent is present at a high density, leading to improved adhesive strength. Furthermore, when a WBL is formed, the increase in the storage modulus, which is a bulk property, due to photocuring tends to be suppressed, making the adhesive highly applicable to foldable devices.

[0097] The smaller the functional group equivalent weight of the photocuring agent and the higher the content of the photocuring agent, the higher the crosslink density upon photocuring, and therefore the higher the storage modulus of the pressure-sensitive adhesive layer after photocuring tends to be. From the viewpoint of increasing the adhesive strength of the pressure-sensitive adhesive after photocuring while suppressing an excessive increase in the storage modulus, the content of the photocuring agent in the pressure-sensitive adhesive composition is preferably 3 to 25 parts by weight, more preferably 5 to 20 parts by weight, or even 8 to 17 parts by weight or 10 to 15 parts by weight, per 100 parts by weight of the acrylic base polymer. As described above, if a WBL is formed on the surface (adhesion interface) of the pressure-sensitive adhesive layer by adjusting the compatibility between the acrylic base polymer and the photocuring agent, the adhesive strength is likely to increase upon photocuring even with a small amount of photocuring agent, and high adhesive strength can be achieved.

[0098] Two or more types of photocuring agents may be used in combination. For example, two or more types of polyfunctional (meth)acrylates having an alkylene oxide chain may be used as the photocuring agent, or a polyfunctional (meth)acrylate having an alkylene oxide chain and a polyfunctional (meth)acrylate having no alkylene oxide chain may be used. Furthermore, polyfunctional (meth)acrylates having different numbers of functional groups (the number of (meth)acryloyl groups in one molecule) may be used as the photocuring agent. For example, a bifunctional (meth)acrylate and a trifunctional or higher polyfunctional (meth)acrylate may be used in combination as the photocuring agent for the purpose of adjusting the adhesive strength and storage modulus of the pressure-sensitive adhesive layer after photocuring.

[0099] As the photocuring agent, a polyfunctional (meth)acrylate having an alkylene oxide chain and a urethane (meth)acrylate may be used. The urethane (meth)acrylate is a compound having one or more urethane bonds and two or more (meth)acryloyl groups in one molecule, preferably two or more urethane bonds in one molecule. A urethane (meth)acrylate having two or more urethane bonds can be obtained, for example, by reacting a polyisocyanate with a (meth)acrylic compound having a hydroxy group, and the isocyanate group of the polyisocyanate and the hydroxy group of the (meth)acrylic compound bond to form a urethane bond. A urethane (meth)acrylate having two or more urethane bonds can also be obtained by reacting a polyisocyanate with a polyol to prepare a prepolymer having an isocyanate group at its terminal, and then bonding a (meth)acrylic compound having a hydroxy group to the isocyanate group at the terminal of the prepolymer. Alternatively, a urethane (meth)acrylate having two or more urethane bonds can be obtained by reacting a polyisocyanate with a (meth)acrylic compound having a hydroxy group, and then reacting the reaction product with a polyol.

[0100] The polyisocyanate may be any of aromatic polyisocyanate, alicyclic polyisocyanate, and alicyclic polyisocyanate. As the aromatic polyisocyanate, tolylene diisocyanate (TDI) is particularly preferred. The tolylene diisocyanate may be either 2,4-tolylene diisocyanate or 2,6-tolylene diisocyanate, or a mixture of both. As the aliphatic polyisocyanate, hexamethylene diisocyanate (HDI) is particularly preferred. As the alicyclic polyisocyanate, isophorone diisocyanate (IPDI) is particularly preferred.

[0101] Examples of the (meth)acrylic compound having a hydroxy group include compounds having one hydroxy group and one (meth)acryloyl group, such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, hydroxyhexyl (meth)acrylate, hydroxymethyl acrylamide, and hydroxyethyl acrylamide; and compounds having one hydroxy group and two or more (meth)acryloyl groups, such as pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, trimethylolpropane di(meth)acrylate, and isocyanuric acid di(meth)acrylate.

[0102] A urethane (meth)acrylate obtained by reacting a diisocyanate with a (meth)acrylic compound having one hydroxy group and two or more (meth)acryloyl groups in one molecule has two urethane bonds and four or more (meth)acryloyl groups in one molecule. The number of (meth)acryloyl groups in the urethane (meth)acrylate may be six or more, eight or more, or 12 or less, or 10 or less.

[0103] The urethane (meth)acrylate may be commercially available from Kyoeisha Chemical, Shin-Nakamura Chemical, Negami Chemical Industries, Mitsubishi Chemical, Daicel Allnex, Resonac, or the like.

[0104] By including a urethane (meth)acrylate as a photocuring agent in addition to a polyfunctional (meth)acrylate having no urethane bond, the adhesive strength of the pressure-sensitive adhesive layer before photocuring may be small and the adhesive strength of the pressure-sensitive adhesive layer after photocuring may be large. One possible reason for this is that the urethane (meth)acrylate promotes the formation of WBL by the polyfunctional (meth)acrylate having no urethane bond, particularly the polyfunctional (meth)acrylate having an alkylene oxide chain.

[0105] When the photocurable composition constituting the pressure-sensitive adhesive layer contains, as a photocuring agent, a urethane (meth)acrylate in addition to a polyfunctional (meth)acrylate having no urethane bond, the content of the urethane (meth)acrylate is preferably 0.01 parts by weight or more, more preferably 0.05 parts by weight or more, and may be 0.08 parts by weight or more, or 0.1 parts by weight or more, relative to 100 parts by weight of the acrylic base polymer.

[0106] <Photopolymerization initiator> The photopolymerization initiator generates active species upon irradiation with actinic rays and promotes the curing reaction of the photocuring agent. As the photopolymerization initiator, a photocationic initiator (photoacid generator), a photoradical initiator, a photoanionic initiator (photobase generator), etc. are used depending on the type of photocuring agent, etc. When a polyfunctional acrylate is used as the photocuring agent, it is preferable to use a photoradical initiator. As the photoradical initiator, a photoradical generator that is cleaved by visible light or ultraviolet light having a wavelength shorter than 450 nm to generate a radical is preferred, and examples thereof include hydroxyketones, benzyl dimethyl ketals, aminoketones, acylphosphine oxides, benzophenones, and trichloromethyl group-containing triazine derivatives. The photoradical generators may be used alone or in combination of two or more.

[0107] The content of the photopolymerization initiator in the pressure-sensitive adhesive composition is preferably 0.001 to 5 parts by weight, more preferably 0.01 to 3 parts by weight, and even more preferably 0.03 to 1 part by weight, relative to 100 parts by weight of the acrylic base polymer. The content of the photopolymerization initiator in the pressure-sensitive adhesive composition is preferably 0.02 to 20 parts by weight, more preferably 0.05 to 10 parts by weight, and even more preferably 0.1 to 7 parts by weight, relative to 100 parts by weight of the photocuring agent.

[0108] <Antistatic Agent> The PSA composition contains an antistatic agent. When the PSA contains an antistatic agent, the PSA layer has a low resistance, reducing static electricity in the PSA layer and also providing the effect of suppressing static electricity on the adherend.

[0109] Examples of antistatic agents include ionic compounds containing organic cations, alkali metal salts, ion-conductive polymers, ion-conductive fillers, conductive polymers, etc. Among these, ionic compounds containing organic cations and alkali metal salts are preferred because of their excellent compatibility with acrylic-based polymers.

[0110] The ionic compound containing an organic cation may be an ionic liquid, which is a liquid at room temperature, or an ionic solid, which is a solid at room temperature. The ionic compound containing an organic cation is preferably composed of an organic anion or a fluoroinorganic anion and an onium cation. The organic anion may be a fluoroorganic anion containing a fluorine atom, or an organic anion not containing a fluorine atom.

[0111] Examples of the onium cation include nitrogen-containing onium cations, sulfur-containing onium cations (e.g., trialkylsulfonium cations), phosphorus-containing onium cations (e.g., tetraalkylphosphonium cations), etc. Among these, nitrogen-containing onium cations are preferred.

[0112] Examples of nitrogen-containing onium cations include pyridinium cations, pyrrolidinium cations, piperidinium cations, cations having a pyrroline skeleton, cations having a pyrrole skeleton, imidazolium cations, tetrahydropyrimidinium cations, dihydropyrimidinium cations, pyrazolium cations, pyrazolinium cations, and tetraalkylammonium cations.

[0113] The fluoroorganic anion constituting the ionic compound containing an organic cation may be completely fluorinated (perfluorinated) or partially fluorinated. Examples of fluoroorganic anions include perfluoroalkylsulfonates, bis(fluorosulfonyl)imides, and bis(perfluoroalkanesulfonyl)imides. More specifically, examples include trifluoromethanesulfonate, pentafluoroethanesulfonate, heptafluoropropanesulfonate, nonafluorobutanesulfonate, bis(fluorosulfonyl)imides, and bis(trifluoromethanesulfonyl)imides. Examples of organic anions that do not contain fluorine atoms include sulfonate anions such as p-toluenesulfonate, borate anions, and dicyanamide anions. Examples of fluoroinorganic anions include hexafluorophosphate and tetrafluoroboric acid.

[0114] The alkali metal salt preferably comprises the above organic anion or fluoroinorganic anion and an alkali metal cation. The alkali metal cation is preferably Li + , Na + or K + Among them, Li + is preferred.

[0115] The content of the antistatic agent in the PSA composition is approximately 0.01 to 3 parts by weight, preferably 0.03 to 2 parts by weight, more preferably 0.05 to 1 part by weight, and even more preferably 0.1 to 0.7 parts by weight, per 100 parts by weight of the acrylic base polymer. The content of the antistatic agent in the PSA layer 2 is approximately 0.01 to 2% by weight, preferably 0.03 to 1% by weight, more preferably 0.05 to 0.7% by weight, and even more preferably 0.1 to 0.5% by weight, and may be 0.15 to 0.4% by weight. If the amount of antistatic agent is too small, the PSA may not be able to sufficiently reduce its resistance. If the amount of antistatic agent is too large, bleed-out of the antistatic agent may cause contamination or corrosion of the adherend, or a decrease in adhesive strength.

[0116] As described above, since the acrylic base polymer of the pressure-sensitive adhesive composition contains a (meth)acrylic acid ester having an alkylene oxide chain as a monomer component, the resistance of the pressure-sensitive adhesive can be reduced even with a small amount of antistatic agent added, and therefore a pressure-sensitive adhesive layer having low surface resistance and excellent antistatic properties can be provided while suppressing problems such as bleed-out of the antistatic agent.

[0117] <Other Components> As described above, the photocurable pressure-sensitive adhesive composition constituting the pressure-sensitive adhesive layer 2 contains an acrylic base polymer, a photocuring agent, a photopolymerization initiator, and an antistatic agent. The pressure-sensitive adhesive composition may contain components other than these.

[0118] For example, the pressure-sensitive adhesive composition may contain an oligomer having a lower molecular weight than the base polymer. For example, the pressure-sensitive adhesive composition may contain, in addition to the acrylic base polymer, an acrylic oligomer having a weight-average molecular weight of approximately 1,000 to 30,000. The acrylic oligomer contains a (meth)acrylic acid alkyl ester as a main constituent monomer component. From the viewpoint of increasing the adhesive strength of the pressure-sensitive adhesive layer 2 after photocuring, the glass transition temperature of the acrylic oligomer is preferably 40°C or higher, more preferably 50°C or higher. The acrylic oligomer may contain a crosslinkable functional group, similar to the acrylic base polymer.

[0119] In addition to the above components, the pressure-sensitive adhesive composition may contain additives such as a silane coupling agent, a tackifier, a plasticizer, a softener, an anti-degradant, a filler, a colorant, an ultraviolet absorber, an antioxidant, and a surfactant, within a range that does not impair the properties of the present invention.

[0120] Additives may be used to reduce the resistance of the adhesive or to adjust the compatibility between the acrylic base polymer and the photocuring agent. For example, adding polyether polyols such as polyethylene glycol and polypropylene glycol tends to reduce the resistance of the adhesive. However, low-molecular-weight additives such as polyols do not contribute to the photocuring of the adhesive and remain as liquid components even after the adhesive is photocured. Therefore, if the amount of low-molecular-weight additives is large, the gel fraction of the adhesive after photocuring tends to be small, the adhesive layer tends to be prone to plastic deformation, and the strain recovery rate tends to be low. Therefore, the amount of additive is preferably 20 parts by weight or less, more preferably 10 parts by weight or less, even more preferably 5 parts by weight or less, and may be 3 parts by weight or less, 2 parts by weight or less, or 1 part by weight or less, per 100 parts by weight of the acrylic base polymer.

[0121] The total amount of the acrylic base polymer, crosslinking agent, and photocuring agent relative to the total solid content of the pressure-sensitive adhesive composition is preferably 80% by weight or more, more preferably 90% by weight or more, even more preferably 93% by weight or more, and may be 95% by weight or more, 97% by weight or more, or 98% by weight or more.

[0122] [Preparation of Reinforced Film] A reinforced film is obtained by laminating a photocurable pressure-sensitive adhesive layer 2 on a film substrate 1. The pressure-sensitive adhesive layer 2 may be formed directly on the film substrate 1, or a pressure-sensitive adhesive layer formed in a sheet form on another substrate may be transferred onto the film substrate 1.

[0123] The pressure-sensitive adhesive composition is applied to a substrate by roll coating, kiss roll coating, gravure coating, reverse coating, roll brush, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, die coating, or the like, and the solvent is dried and removed as needed to form a pressure-sensitive adhesive layer. A suitable drying method can be adopted as appropriate. The heating and drying temperature is preferably 40°C to 200°C, more preferably 50°C to 180°C, and even more preferably 70°C to 170°C. The drying time is preferably 5 seconds to 20 minutes, more preferably 5 seconds to 15 minutes, and even more preferably 10 seconds to 10 minutes.

[0124] When the pressure-sensitive adhesive composition contains a crosslinking agent, it is preferable to promote crosslinking by heating or aging simultaneously with or after drying of the solvent. The heating temperature and heating time are appropriately set depending on the type of crosslinking agent used, and crosslinking is usually achieved by heating in the range of 20°C to 160°C for about 1 minute to 7 days. The heating for drying and removing the solvent may also serve as the heating for crosslinking.

[0125] The introduction of a crosslinked structure into the acrylic-based polymer increases the gel fraction and tends to increase the storage modulus of the pressure-sensitive adhesive layer 2. The higher the gel fraction of the pressure-sensitive adhesive before photocuring, the harder the pressure-sensitive adhesive becomes, and the less adhesive residue tends to be left on the adherend when the reinforcing film is peeled from the adherend during rework or other processes. The gel fraction of the pressure-sensitive adhesive layer 2 before photocuring (i.e., the gel fraction of the photocurable composition constituting the pressure-sensitive adhesive layer) is preferably 25% or more, more preferably 30% or more, and may be 35% or more, 40% or more, or 45% or more. On the other hand, if the gel fraction is excessively high, the storage modulus of the pressure-sensitive adhesive after photocuring increases, resulting in poor stress-strain relaxation, which may cause the pressure-sensitive adhesive to peel off at bent portions when a flexible device is used. Therefore, the gel fraction of the pressure-sensitive adhesive layer 2 before photocuring is preferably 80% or less, and may be 75% or less, 70% or less, or 65% or less.

[0126] The gel fraction can be determined as the amount of insoluble matter in a solvent such as ethyl acetate, and specifically, it is determined as the weight fraction (unit: wt%) of the insoluble matter after immersing the pressure-sensitive adhesive layer in ethyl acetate for 7 days at 23° C. relative to the sample before immersion. Generally, the gel fraction of a polymer is equal to the degree of crosslinking, and the more crosslinked parts in the polymer, the higher the gel fraction.

[0127] Even after a crosslinked structure is introduced into the polymer by the crosslinking agent, the photocuring agent remains unreacted. Therefore, the pressure-sensitive adhesive layer 2 contains an acrylic base polymer with a crosslinked structure introduced therein, a photocuring agent, a photopolymerization initiator, and an antistatic agent. When the pressure-sensitive adhesive layer 2 is formed on the film substrate 1, it is preferable to provide a release liner 5 on the pressure-sensitive adhesive layer 2 for the purpose of protecting the pressure-sensitive adhesive layer 2, etc. Crosslinking may be performed after providing the release liner 5 on the pressure-sensitive adhesive layer 2.

[0128] When the pressure-sensitive adhesive layer 2 is formed on another substrate, the reinforcing film is obtained by transferring the pressure-sensitive adhesive layer 2 onto the film substrate 1 after drying the solvent. The substrate used to form the pressure-sensitive adhesive layer may be used as the release liner 5 as it is.

[0129] As the release liner 5, a plastic film such as polyethylene, polypropylene, polyethylene terephthalate, or polyester film is preferably used. The thickness of the release liner is typically 3 to 200 μm, preferably approximately 10 to 100 μm. The surface of the release liner 5 that comes into contact with the pressure-sensitive adhesive layer 2 is preferably treated with a release agent such as a silicone-based, fluorine-based, long-chain alkyl-based, or fatty acid amide-based release agent, or with silica powder. By treating the surface of the release liner 5 with a release treatment, when the release liner 5 is peeled from the film substrate 1, peeling occurs at the interface between the pressure-sensitive adhesive layer 2 and the release liner 5, maintaining the pressure-sensitive adhesive layer 2 adhered to the film substrate 1. The release liner 5 may be antistatically treated on either or both of the release-treated and untreated surfaces. By treating the release liner 5 with an antistatic treatment, charging when the release liner is peeled from the pressure-sensitive adhesive layer can be suppressed.

[0130] [Physical Properties of Pressure-Sensitive Adhesive Layer] The thickness of the pressure-sensitive adhesive layer 2 is, for example, about 1 to 300 μm. The thicker the pressure-sensitive adhesive layer 2, the more likely it is to have improved adhesion to an adherend. On the other hand, if the pressure-sensitive adhesive layer 2 is excessively thick, the fluidity before photocuring may be high, making handling difficult. Therefore, the thickness of the pressure-sensitive adhesive layer 2 is preferably 3 to 100 μm, more preferably 5 to 50 μm, even more preferably 6 to 40 μm, and particularly preferably 8 to 30 μm. From the viewpoint of reducing the thickness, the thickness of the pressure-sensitive adhesive layer 2 may be 25 μm or less, 20 μm or less, or 18 μm or less.

[0131] When the reinforcing film is used in an optical device such as a display, the total light transmittance of the pressure-sensitive adhesive layer 2 is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more. The haze of the pressure-sensitive adhesive layer 2 is preferably 2% or less, more preferably 1% or less, even more preferably 0.7% or less, and particularly preferably 0.5% or less.

[0132] The surface resistance of the adhesive layer 2 is 5.0×10 11 Ω or less is preferable, and 1.0 × 10 11 Ω or less is more preferable, and 7.0 × 10 10 Ω or less, 5.0×10 10 Ω or less or 3.0 x 10 10 As described above, the pressure-sensitive adhesive composition contains an antistatic agent, and the acrylic base polymer further contains a (meth)acrylic acid ester having an alkylene oxide chain as a monomer component, thereby making it possible to reduce the resistance of the pressure-sensitive adhesive layer 2.

[0133] The low resistance of the pressure-sensitive adhesive layer 2 can suppress electrical damage to the adherend due to static electricity, etc., when the reinforcing film is peeled off from the adherend. The pressure-sensitive adhesive layer 2 preferably has a surface resistance within the above range even after photocuring. In general, the surface resistance of the pressure-sensitive adhesive layer changes very little before and after photocuring. When the pressure-sensitive adhesive layer after photocuring has the above surface resistance, static electricity on the adherend to which the pressure-sensitive adhesive layer 2 is attached is removed via the pressure-sensitive adhesive layer 2, thereby suppressing charging of the adherend. Therefore, defects caused by static electricity, such as electrostatic breakdown, in devices to which the reinforcing film is attached can be suppressed.

[0134] The shear storage modulus of the pressure-sensitive adhesive layer 2 at 25°C before photocuring is 5.0 x 10 3 ~1.0 x 10 5 The shear storage modulus of the pressure-sensitive adhesive layer (hereinafter simply referred to as "storage modulus") is determined in accordance with the method described in JIS K7244-1 "Plastics - Test methods for dynamic mechanical properties" by reading the value at a predetermined temperature when measured at a frequency of 1 Hz in the range of -50 to 150°C at a heating rate of 5°C / min.

[0135] From the viewpoints of improving the processability of the pressure-sensitive adhesive layer, suppressing the pressure-sensitive adhesive from protruding from the edge face of the reinforcing film, and preventing contamination due to adhesive residue on the adherend when the reinforcing film is peeled from the adherend, the storage modulus of the pressure-sensitive adhesive layer 2 at 25°C before photocuring is 7.0 × 10 3 Pa or more is preferable, and 9.0 × 10 3Pa or more is more preferable, and 1.0 × 10 4 Pa or more or 1.5 x 10 4 From the viewpoint of providing flexibility to the pressure-sensitive adhesive layer, the storage modulus of the pressure-sensitive adhesive layer 2 at 25°C before photocuring may be 7.0 × 10 Pa or more. 4 Pa or less, and 5.0 × 10 4 Pa or less is more preferable, and 4.0 × 10 4 Pa or less or 3.0 x 10 4 Pa or less.

[0136] The storage modulus of the pressure-sensitive adhesive layer 2 at −20° C. before photocuring is 1.0×10 4 ~2.0 x 10 5 Pa is preferred, 1.5 × 10 4 ~1.0 x 10 5 Pa is more preferable, and 2.0 × 10 4 ~7.0 x 10 4 Pa or 3.0 x 10 4 ~7.0 x 10 4 When the storage modulus at low temperature of the pressure-sensitive adhesive layer before photocuring is within the above range, the storage modulus of the pressure-sensitive adhesive layer tends to be maintained low even after photocuring.

[0137] When the pressure-sensitive adhesive layer 2 is photocured, the photocuring agent undergoes a curing reaction, increasing the storage modulus and the adhesive strength to the adherend. It is preferable that the pressure-sensitive adhesive layer 2 has a small storage modulus at low temperatures even after photocuring.

[0138] The storage modulus of the adhesive layer after photocuring at −20° C. was 5.0×10 5 Pa or less, and 3.0 × 10 5 Pa or less is more preferable, and 2.0 × 10 5 Pa or less is more preferable, and 1.5×10 5 Pa or less or 1.0 x 10 5 The storage modulus at low temperatures of the pressure-sensitive adhesive layer 2 after photocuring is small, and therefore the pressure-sensitive adhesive layer exhibits strain relaxation properties in a low-temperature environment, and therefore peeling of the pressure-sensitive adhesive layer at the bending portion can be suppressed even when the device to which the reinforcing film is bonded is repeatedly bent or when the bent state is maintained for a long period of time.

[0139] As described above, the lower the glass transition temperature of the acrylic base polymer constituting the pressure-sensitive adhesive layer and the smaller the amount of photocuring agent used, the smaller the storage modulus of the photocured pressure-sensitive adhesive layer tends to be. In particular, when the acrylic base polymer contains n-octyl acrylate as a monomer component, a flat region of the storage modulus (a region in which the temperature dependence of the storage modulus is small) exists in the low temperature region around −20° C., making it easier to obtain a pressure-sensitive adhesive with a small storage modulus at −20° C.

[0140] If the storage modulus of the pressure-sensitive adhesive layer after photocuring is excessively small, the pressure-sensitive adhesive layer may peel off from the adherend due to insufficient adhesive holding power. Therefore, the storage modulus of the pressure-sensitive adhesive layer after photocuring at −20° C. should be 1.0×10 4 Pa or more is preferable, and 3.0 × 10 4 Pa or more is more preferable, and 5.0 × 10 4 Pa or more or 7.0 x 10 4 It may be Pa or more.

[0141] The strain recovery rate of the pressure-sensitive adhesive layer at a temperature of 60°C is preferably 85% or more, more preferably 90% or more, even more preferably 91% or more, and may be 92% or more. The strain recovery rate is measured by applying a shear stress of 2 kPa to the pressure-sensitive adhesive layer using a rotational rheometer for 10 minutes, then releasing the stress and allowing it to stand for 10 minutes to recover the strain, and measuring the maximum strain S 1 and the minimum strain S when stress is released 2 The strain recovery rate (%) is calculated by the following formula: 1 -S 2 ) / S 1

[0142] The strain recovery rate is an index showing the degree to which the adhesive layer is restored to its original shape when stress is applied to deform it (strained state) and the stress is released, and the closer it is to 100%, the higher the shape recovery ability. If the strain recovery rate is within the above range, when the foldable device is held in a folded state (a state in which an elongation strain is applied to the adhesive layer) and then returned to an extended state to release the stress on the adhesive layer, the adhesive layer easily restores its shape, making it less likely to develop deformation such as wrinkles.

[0143] As described above, by introducing an alkylene oxide structure into the acrylic base polymer to reduce resistance without using additives such as polyols (or using only small amounts), the amount of low molecular weight liquid components contained in the adhesive after photocuring is small and the gel fraction of the adhesive is large, making it possible to increase the strain recovery rate.

[0144] From the viewpoint of facilitating peeling from the adherend and preventing adhesive residue on the adherend after peeling of the reinforcing film, the adhesive strength between the pressure-sensitive adhesive layer 2 and the adherend before photocuring is preferably 1 N / 25 mm or less, more preferably 0.7 N / 25 mm or less, even more preferably 0.5 N / 25 mm or less, and may be 0.4 N / 25 mm or less, or 0.3 N / 25 mm or less. From the viewpoint of preventing peeling of the reinforcing film during storage or handling, the adhesive strength between the pressure-sensitive adhesive layer 2 and the adherend before photocuring is preferably 0.01 N / 25 mm or more, more preferably 0.02 N / 25 mm or more, and may be 0.03 N / 25 mm or more, 0.04 N / 25 mm or more, or 0.05 N / 25 mm or more.

[0145] The adhesive strength is determined by a peel test using a polyimide film as the adherend at a tensile speed of 300 mm / min and a peel angle of 180°. Unless otherwise specified, the adhesive strength is measured at 25°C.

[0146] From the viewpoint of adhesive reliability during practical use of the device, the adhesive strength between the adhesive layer and the adherend after photocuring is preferably 5 N / 25 mm or more, more preferably 7 N / 25 mm or more, even more preferably 8 N / 25 mm or more, and may be 9 N / 25 mm or more or 10 N / 25 mm or more.

[0147] The adhesive strength between the pressure-sensitive adhesive layer and the adherend after photocuring is preferably 5 times or more, more preferably 10 times or more, even more preferably 15 times or more, and may be 20 times or more, 30 times or more, or 50 times or more, of the adhesive strength between the pressure-sensitive adhesive layer and the adherend before photocuring. As described above, by adjusting the compatibility between the two based on the composition of the acrylic base polymer and the type of photocuring agent, it is possible to keep the adhesive strength before photocuring (initial adhesive strength) low and increase the adhesive strength of the pressure-sensitive adhesive after photocuring.

[0148] [Use of Reinforced Film] The reinforced film of the present invention is used by being attached to a device or a device component. The reinforced film 10 has the pressure-sensitive adhesive layer 2 fixed to the film substrate 1, and has low adhesive strength to the adherend after being attached to the adherend and before being photocured. Therefore, the reinforced film can be easily peeled from the adherend before being photocured.

[0149] The adherend to which the reinforced film is attached is not particularly limited, and examples thereof include various electronic devices, optical devices, and their components. In one embodiment, the reinforced film is attached to the surface of a foldable flexible device. The foldable device has a hinge portion and can be folded around this hinge portion. The folding angle can be set arbitrarily, and the device may be bent (folded) 180°. When the device is a display device, the reinforced film may be attached to the surface on the screen side, or to the back side (housing). In a flexible device that is configured to be bendable at a predetermined location such as a hinge portion, bending and extension are repeatedly performed at the same location during use.

[0150] The reinforcing film may be attached to the entire surface of the adherend, or may be selectively attached only to the area requiring reinforcement (reinforcement target area). Alternatively, the reinforcing film may be attached to the entire area requiring reinforcement (reinforcement target area) and the area not requiring reinforcement (non-reinforcement target area), and then the reinforcing film attached to the non-reinforcement target area may be cut and removed. Before the adhesive is photocured, the reinforcing film is temporarily attached to the surface of the adherend, so the reinforcing film can be easily peeled and removed from the surface of the adherend. The reinforcing film may be attached to the area requiring reinforcement and the area not requiring reinforcement, and the adhesive may be photocured by selectively irradiating the area requiring reinforcement with light. Then, the reinforcing film may be selectively peeled and removed from the non-reinforcement target area where the adhesive is not cured.

[0151] By laminating a reinforcing film, appropriate rigidity is imparted, which is expected to improve the handleability and prevent breakage of thin members such as flexible devices. When a reinforcing film is laminated to a work-in-progress in the device manufacturing process, the reinforcing film may be laminated to a large-sized work-in-progress before it is cut to the product size. The reinforcing film may also be laminated roll-to-roll to a mother roll of a device manufactured by a roll-to-roll process.

[0152] After laminating the reinforcing film to the adherend, the pressure-sensitive adhesive layer 2 is irradiated with actinic rays to photocure the pressure-sensitive adhesive layer. Examples of actinic rays include ultraviolet light, visible light, infrared light, X-rays, α-rays, β-rays, and γ-rays. Ultraviolet light is preferred as the actinic rays because it can inhibit curing of the pressure-sensitive adhesive layer during storage and facilitates curing. The irradiation intensity and irradiation time of the actinic rays may be appropriately set depending on the composition, thickness, etc. of the pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer 2 may be irradiated with actinic rays from either the film substrate 1 side or the adherend side, or may be irradiated with actinic rays from both sides.

[0153] As described above, by bonding the reinforced film of the present invention, appropriate rigidity is imparted to the adherend and stress is alleviated and dispersed, thereby suppressing various defects that may occur in the manufacturing process, improving production efficiency, and improving yield. The reinforced film is easily peeled from the adherend before photocuring the pressure-sensitive adhesive layer, so rework is easy even if lamination or bonding defects occur. Furthermore, processing such as selectively removing the reinforced film from areas other than the area to be reinforced is also easy.

[0154] When the completed device is in use, the reinforcing film prevents damage to the device even if an external force is suddenly applied due to the device being dropped, a heavy object being placed on the device, the device being hit by a flying object, etc. Furthermore, because the reinforcing film is firmly adhered to the device after the adhesive is photocured, the reinforcing film is unlikely to peel off even during long-term use, providing excellent reliability.

[0155] In a device with a reinforced film in which the reinforced film of the present invention is bonded to a flexible device using a resin substrate, peeling of the reinforced film at the bent portion is unlikely to occur even when the device is repeatedly bent or maintained in a bent state for a long period of time. Furthermore, even when the device is extended after maintaining a bent state for a long period of time, the pressure-sensitive adhesive layer has a high strain recovery rate and high shape restoring ability, so deformation such as wrinkles is unlikely to occur. Furthermore, since the pressure-sensitive adhesive layer has low resistance and can remove static electricity from the resin substrate of the device through the pressure-sensitive adhesive layer, problems such as electrostatic breakdown of the device caused by charging (static electricity) can be suppressed.

[0156] The present invention will be further explained below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0157] [Polymerization of Acrylic Polymer] <Polymer A> A reaction vessel equipped with a thermometer, a stirrer, a reflux condenser, and a nitrogen gas inlet tube was charged with 76 parts by weight of 2-ethylhexyl acrylate (2EHA), 4 parts by weight of 4-hydroxybutyl acrylate (4HBA), and 20 parts by weight of methoxyethyl acrylate (MEA) as monomers, 0.2 parts by weight of azobisisobutyronitrile (AIBN) as a polymerization initiator, and 233 parts by weight of ethyl acetate as a solvent, and nitrogen gas was introduced and purged with nitrogen for about 1 hour while stirring. The mixture was then heated to 60°C and reacted for 7 hours to obtain a solution of acrylic polymer A having a weight average molecular weight (Mw) of 700,000.

[0158] <Polymers B to Q> The amounts of monomers charged were changed as shown in Table 1. Solutions of polymers B to Q were obtained in the same manner as in the polymerization of polymer A except for the above.

[0159] [Preparation of Reinforced Film] <Example 1> (Preparation of Pressure-Sensitive Adhesive Composition) To a solution of acrylic polymer A (100 weight percent of the polymer solids), 0.1 parts by weight of a trifunctional isocyanate-based crosslinking agent ("Coronate HX" manufactured by Tosoh Corporation) as a crosslinking agent, 0.02 parts by weight of iron acetylacetonate ("Nacem Ferric" manufactured by Nippon Chemical Industry Co., Ltd.) as a crosslinking catalyst, a polyfunctional acrylate and a urethane acrylate shown in Table 1 as photocuring agents, 0.3 parts by weight of "Omnirad 651" manufactured by IGM Resins as a photopolymerization initiator, and 0.2 parts by weight of 1-butyl-3-methylpyridinium bistrifluoromethanesulfonylimide ("CIL-312" manufactured by Nippon Carlit Co., Ltd.) as antistatic agent A were added and mixed uniformly to prepare a pressure-sensitive adhesive composition shown in Table 1.

[0160] (Application of adhesive solution and crosslinking) The above-mentioned adhesive composition was applied to a 50 μm thick polyethylene terephthalate film using a fountain roll so that the thickness after drying was 25 μm. After drying at 130 ° C for 1 minute to remove the solvent, the release-treated surface of a release liner (a 25 μm thick polyethylene terephthalate film with both sides antistatically treated and one side silicone release-treated) was attached to the adhesive-coated surface. Thereafter, aging treatment was performed for 4 days in an atmosphere of 25 ° C to promote crosslinking, and a reinforced film was obtained in which a photocurable adhesive sheet was fixedly laminated on a polyethylene terephthalate film substrate and a release liner was temporarily attached thereto.

[0161] Examples 2, 4 to 11, Comparative Examples 1 to 5 Pressure-sensitive adhesive compositions were prepared and reinforcing films were produced in the same manner as in Example 1, except that the type of acrylic polymer and the type and amount of photocuring agent added were changed as shown in Table 1.

[0162] Example 3 A pressure-sensitive adhesive composition was prepared in the same manner as in Example 2, except that 0.2 parts by weight of antistatic agent B was used instead of antistatic agent A, and a reinforcing film was produced.

[0163] Example 12 (Preparation of Pressure-Sensitive Adhesive Composition) To a solution of acrylic polymer H (100 weight parts as polymer solids), 0.5 parts by weight of a tetrafunctional epoxy crosslinking agent ("Tetrad C" manufactured by Mitsubishi Gas Chemical Company, Ltd.) as a crosslinking agent, 0.2 parts by weight of zirconium tetraacetylacetonate ("ZC-150" manufactured by Matsumoto Fine Chemical Co., Ltd.) as a crosslinking catalyst, a polyfunctional acrylate and a urethane acrylate shown in Table 1 as photocuring agents, 0.3 parts by weight of "Omnirad 651" manufactured by IGM Resins as a photopolymerization initiator, and 0.2 parts by weight of "CIL-312" manufactured by Nippon Carlit Co., Ltd. as an antistatic agent were added and mixed uniformly to prepare a pressure-sensitive adhesive composition.

[0164] (Coating and Crosslinking of Pressure-Sensitive Adhesive Solution) Using the pressure-sensitive adhesive composition described above, coating and crosslinking were carried out in the same manner as in Example 1 to prepare a reinforcing film.

[0165] Examples 13 to 16 Pressure-sensitive adhesive compositions were prepared and reinforcing films were produced in the same manner as in Example 12, except that the type of acrylic polymer, the amount of crosslinking agent added, the type and amount of photocuring agent added, and the type of antistatic agent were changed as shown in Table 1.

[0166] <Comparative Example 6> A pressure-sensitive adhesive composition was prepared and a reinforcing film was produced in the same manner as in Example 12, except that the type of acrylic polymer, the type and amount of photocuring agent, and the amount of crosslinking agent added were changed as shown in Table 1.

[0167] Comparative Example 7 A pressure-sensitive adhesive composition was prepared and a reinforcing film was produced in the same manner as in Example 12, except that the type of acrylic polymer and the type and added amount of photocuring agent were changed as shown in Table 1 and 30 parts by weight of triol-type polypropylene glycol ("Preminol S-3011" manufactured by AGC, Mn = 10000, hereinafter referred to as "PPG") was added as an additive.

[0168] Comparative Example 8 A pressure-sensitive adhesive composition was prepared in the same manner as in Comparative Example 1, except that 10 parts by weight of PPG was added as an additive, and a reinforcing film was produced from the prepared composition.

[0169] [Evaluation] The pressure-sensitive adhesive layers of the reinforcing films obtained in the above Examples and Comparative Examples were evaluated as follows. Note that in Comparative Examples 1 and 2, the liquid photocuring agent oozed onto the surface of the pressure-sensitive adhesive layer, and the layer did not function as a pressure-sensitive adhesive, so evaluation was not performed.

[0170] <Weight-average molecular weight> The weight-average molecular weight (polystyrene equivalent) of the polymer was measured using GPC ("HLC-8220GPC" manufactured by Tosoh Corporation) under the following conditions: Sample concentration: 0.2 wt% (tetrahydrofuran solution) Sample injection amount: 10 μL Eluent: THF Flow rate: 0.6 mL / min Measurement temperature: 40°C Sample column: TSKguardcolumn SuperHZ-H (1 column) + TSKgel SuperHZM-H (2 columns) Reference column: TSKgel SuperH-RC (1 column) Detector: RI

[0171] <Surface Resistance> The release liner was peeled off from the reinforcing film to expose the pressure-sensitive adhesive layer (before photocuring). A probe (Model 152P-2P, manufactured by TREK) was brought into contact with the surface of the pressure-sensitive adhesive layer in an environment of a temperature of 25°C and a relative humidity of 50%, and the surface resistance was measured using a resistivity meter (Model 152-1, manufactured by TREK) under conditions of an applied voltage of 10 V and a voltage application time of 10 seconds.

[0172] <Storage modulus> A pressure-sensitive adhesive composition was applied to a release liner and crosslinked in the same manner as in each of the above-mentioned Examples and Comparative Examples to prepare a pressure-sensitive adhesive sheet (before photocuring). A release liner was attached to the surface of the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet before photocuring to shield it from oxygen, and the sheet was exposed to 1000 mJ / cm irradiated with a 365 nm LED lamp. 2 The adhesive sheets were then laminated to prepare a measurement sample having a thickness of approximately 0.8 mm, and a dynamic viscoelasticity measurement was carried out under the following conditions using a rotational rheometer (TA Instruments' "Discovery-HR2"), and the shear storage modulus G' at -20°C was read. (Measurement conditions) Deformation mode: Torsion Measurement frequency: 1 Hz Heating rate: 5°C / min Measurement temperature: -50 to 150°C Shape: Parallel plate 8.0 mmφ

[0173] <Strain recovery rate> A measurement sample was prepared in the same manner as described above. Using a rotational rheometer, a stress of 2 kPa was applied to the measurement sample for 10 minutes, and then the stress was released (stress: 0 kPa) and the sample was allowed to stand for 10 minutes to recover from the strain. The maximum strain S 1 and the minimum strain S when stress is released 2 Therefore, strain recovery rate (%) = 100 × (S 1 -S 2 ) / S 1 (Measurement conditions) Deformation mode: torsion Measurement temperature: 60°C Shape: parallel plate 8.0 mmφ

[0174] <Adhesion Strength> A 25 μm thick polyimide film (UBE's "Upilex 25S") was attached to a glass plate via double-sided adhesive tape (Nitto Denko's "No. 531") to obtain a polyimide film substrate for measurement. The release liner was peeled off and removed from the surface of a reinforced film cut into a 25 mm wide x 100 mm long piece, and the piece was then attached to the polyimide film substrate for measurement using a hand roller to obtain a test sample before photocuring. The reinforced film side (PET film substrate side) of the test sample before photocuring was irradiated with ultraviolet light to photocure the pressure-sensitive adhesive layer, thereby obtaining a test sample after photocuring. Using these test samples, the edge of the film substrate of the reinforced film was held with a chuck, and the reinforced film was peeled 180° at a pulling rate of 300 mm / min, to measure peel strength.

[0175] <Adherend Contamination> The release liner was peeled off from the surface of the reinforced film, and a polyimide film ("Upilex 25S" manufactured by UBE) was attached to the surface of the pressure-sensitive adhesive layer using a hand roller. After leaving to stand at 25°C for 30 minutes, the reinforced film was peeled off from the polyimide film, and the surface of the polyimide film was visually inspected under a fluorescent lamp to check for the presence or absence of contamination. Cases where contamination by attached matter was observed were rated x, and cases where no contamination was observed were rated ◯.

[0176] The compositions of the pressure-sensitive adhesives of the reinforcing films of the Examples and Comparative Examples (composition and weight-average molecular weight Mw of the acrylic polymer, and amounts of photocuring agent, crosslinking agent, antistatic agent, and PPG added) and the evaluation results of adhesive strength are shown in Tables 1 and 2. In Tables 1 and 2, the amount of each component is the amount added per 100 parts by weight of the solid content of the acrylic polymer, and in all examples, the amount of antistatic agent is 0.2 parts by weight. Details of the constituent monomers of the acrylic polymer, the crosslinking agent, and the photocuring agent are as follows:

[0177] (Monomers) 2EHA: 2-ethylhexyl acrylate BA: Butyl acrylate NOAA: n-octyl acrylate LA: Lauryl acrylate (dodecyl acrylate) 4HBA: 4-hydroxybutyl acrylate AA: Acrylic acid MEA: Methoxyethyl acrylate ("Acrix C-1" manufactured by Toagosei Co., Ltd.) EEEA: Ethoxyethoxyethyl acrylate ("Viscoat #180" manufactured by Osaka Organic Chemical Industry Co., Ltd.) AM90G: Methoxypolyethylene glycol #400 acrylate ("NK Ester AM90-G" manufactured by Shin-Nakamura Chemical Co., Ltd.)

[0178] (Crosslinking agent) TC: 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane (tetrafunctional epoxy compound, "Tetrad C" manufactured by Mitsubishi Gas Chemical Company) C / HX: isocyanurate of hexamethylene diisocyanate ("Coronate HX" manufactured by Tosoh Corporation)

[0179] (Photocuring agents) A200: polyethylene glycol #200 (n=4) diacrylate ("NK Ester A-200" manufactured by Shin-Nakamura Chemical Co., Ltd., functional group equivalent: 151 g / eq) A400: polyethylene glycol #400 (n=9) diacrylate ("NK Ester A-400" manufactured by Shin-Nakamura Chemical Co., Ltd., functional group equivalent: 263 g / eq) A600: polyethylene glycol #600 (n=14) diacrylate ("NK Ester A600" manufactured by Shin-Nakamura Chemical Co., Ltd., functional group equivalent: 371 g / eq) M350: trimethylolpropane EO-modified (n=1) triacrylate ("Aronix M-350" manufactured by Toagosei Co., Ltd., functional group equivalent: 143 g / eq) UA: Polycarbonate skeleton-containing urethane acrylate (Kyoeisha Chemical Company, "UF-X9-83", functional groups 2-3, weight average molecular weight 8400)

[0180] (Antistatic Agents) Antistatic Agent A: 1-butyl-3-methylpyridinium bistrifluoromethanesulfonylimide ("CIL-312" manufactured by Nippon Carlit) Antistatic Agent B: 1-ethyl-3-methylimidazolium bis(fluorosulfonyl)imide (abbreviation: EMI-FSI) Antistatic Agent C: 1-ethyl-3-methylimidazolium dicyanamide (abbreviation: EMI-N(CN) 2 )

[0181]

[0182]

[0183] Comparative Example 6, which used a pressure-sensitive adhesive containing polymer O, whose main monomer component was butyl acrylate (BA), and 30 parts by weight of a photocuring agent (A200), had a large storage modulus G' at -20°C after photocuring, and was poor in flexibility. Comparative Example 7, which blended 10 parts by weight of a long-chain photocuring agent (A600) and 30 parts by weight of PPG to reduce resistance, had a pressure-sensitive adhesive layer that achieved both a low storage modulus and low resistance, but had a reduced strain recovery rate.

[0184] In Comparative Example 1, which used Polymer J, whose main monomer component was 2-ethylhexyl acrylate (2EHA), which has a lower glass transition temperature than butyl acrylate, in order to achieve a low storage modulus, the compatibility between the polymer and the photocuring agent was low, resulting in the liquid photocuring agent seeping out. The same was true for Comparative Example 2, which used Polymer K, whose main monomer component was n-octyl acrylate (NOAA). 2EHA and NOAA have lower polarity than BA, and therefore the low compatibility between the acrylic polymer and the photocuring agent containing an alkylene oxide chain is thought to be the cause of the seeping out.

[0185] In Comparative Example 8, which used an adhesive in which 10 parts by weight of PPG was added to the composition of Comparative Example 1, no exudation of the photocuring agent was observed as in Comparative Example 1, but the surface of the polyimide film was contaminated after the reinforcing film was peeled off. In Comparative Example 8, the PPG acted as a compatibilizer, thereby suppressing the exudation of the photocuring agent, but it is believed that the photocuring agent and / or PPG were not sufficiently compatible in the composition, and the bled-out components were the cause of contamination of the adherend.

[0186] In Example 1, in which Polymer A containing methoxyethyl acrylate (MEA) as a monomer component was used instead of Polymer J in Comparative Example 1, G' was as small as in Comparative Example 8, and no contamination of the adherend due to seepage or bleed-out of the photocuring agent was observed. The pressure-sensitive adhesive layer of Example 1 had a high strain recovery rate of 93%, and combined low G', low resistance, and high recovery properties.

[0187] Examples 2, 4 to 10, which used polymers B to G containing methoxyethyl acrylate (MEA) as a monomer component instead of polymer K in Comparative Example 2, also had low G', low resistance, and high recovery properties, similar to Example 1, as did Example 3, which used a different type of antistatic agent. Example 3 had a lower surface resistance than Example 2, and it can be seen that antistatic agent B (EMI-FSI) exhibited better antistatic properties.

[0188] In Examples 1 to 10, the acrylic polymer contained MEA, an acrylic acid ester containing an alkylene oxide chain, as a constituent monomer, which is thought to have increased the polarity of the polymer, improved the compatibility between the acrylic polymer and the photocuring agent, and suppressed the seepage of the photocuring agent.In addition, it is thought that Examples 1 to 10 showed a high strain recovery rate because the pressure-sensitive adhesive layer after photocuring did not contain low-molecular-weight components such as PPG.

[0189] Example 11, which used Polymer H containing ethoxyethoxyethyl acrylate (EEEA) as a monomer component, also exhibited excellent properties similar to Examples 1 to 10. Example 12, which used Polymer I containing acrylic acid as a monomer component, exhibited excellent properties, but the strain recovery rate was smaller than those of Examples 1 to 11.

[0190] As the (meth)acrylic acid alkyl ester of the monomer component, C 8 The alkyl ester 2-ethylhexyl acrylate (2EHA) and C 12 Examples 13 to 16, which used the alkyl ester lauryl acrylate (LA), showed higher adhesive strength after photocuring and lower surface resistance than Example 12, demonstrating superior properties. Comparisons between Examples 13 and 14, and between Examples 15 and 16, reveal that the antistatic agent C (EMI-N(CN)) containing no fluorine atoms was effective. 2 ) exhibits antistatic properties equal to or greater than those of antistatic agent B (EMI-FSI).

[0191] Comparative Example 3, which used Polymer L having a weight-average molecular weight of 60,000, had low surface resistance and excellent antistatic properties, but photocuring did not sufficiently increase adhesive strength, and the adhesive strength of the pressure-sensitive adhesive layer after photocuring was insufficient. Methoxypolyethylene glycol acrylate (AM90G) used as a monomer component of Polymer L has a long polyethylene glycol chain length, so it is excellent at reducing resistance, but it acts as a chain transfer agent during polymer polymerization, which is thought to have prevented the molecular weight of the polymer from increasing sufficiently.

[0192] Comparative Example 4, which used Polymer M in which the proportion of MEA in the constituent monomer components of the acrylic polymer was 4%, had a small G' and a large strain recovery rate, but had a large surface resistance and insufficient antistatic properties.

[0193] Comparing Examples 2, 5, and 8 with Comparative Example 4, there is a tendency for the surface resistance of the pressure-sensitive adhesive layer to decrease as the proportion of MEA in the constituent monomer components of the acrylic polymer increases. These results show that copolymerizing an acrylic acid ester containing an alkylene oxide chain as a monomer component not only improves the compatibility between the acrylic polymer and the photocuring agent, but also reduces the resistance of the pressure-sensitive adhesive layer.

[0194] A comparison of Examples 5, 6, and 7 reveals that the surface resistance of the adhesive layer tends to decrease as the amount of photocuring agent increases, suggesting that the photocuring agent containing an alkylene oxide chain also contributes to the reduction in resistance. A comparison of Examples 2 and 4 also reveals that the resistance of the adhesive layer tends to decrease as the amount of the monomer component containing an alkylene oxide chain and the photocuring agent containing an alkylene oxide chain increases.

[0195] In Comparative Example 5, which used Polymer N, in which the proportion of MEA in the constituent monomer components of the acrylic polymer was 60%, the adhesive strength of the pressure-sensitive adhesive layer before photocuring was high and the easy peelability was poor. Furthermore, in Comparative Example 5, the adhesive strength did not increase sufficiently even after photocuring, and the adhesive strength of the pressure-sensitive adhesive layer after photocuring was insufficient. In Comparative Example 5, the proportion of acrylic acid ester containing an alkylene oxide chain in the monomer components constituting the acrylic polymer was high, which excessively increased the compatibility between the acrylic polymer and the photocuring agent, making it difficult for the photocuring agent to function as a WBL, and it is thought that this resulted in a large initial adhesive strength.

[0196] From the above results, it can be seen that a photocurable adhesive composition containing an acrylic-based polymer having a predetermined composition has low resistance and antistatic properties, low initial adhesive strength, and exhibits excellent adhesive properties after photocuring. Furthermore, it has a low storage modulus in the low temperature range and a high strain recovery rate, making it suitable as a reinforcing film for foldable devices.

[0197] REFERENCE SIGNS LIST 1 film substrate 2 pressure-sensitive adhesive layer 10 reinforcing film 5 release liner 20 adherend

Claims

1. A film substrate and an adhesive layer fixedly laminated on one main surface of the film substrate, the adhesive layer being made of a photocurable composition containing an acrylic base polymer, a photocuring agent, a photopolymerization initiator, and an antistatic agent, the acrylic base polymer containing, as monomer units, one or more selected from the group consisting of (meth)acrylic acid alkyl esters; (meth)acrylic acid esters represented by the following general formula (1); and hydroxyl group-containing monomers and carboxyl group-containing monomers, the amount of (meth)acrylic acid alkyl esters being 40 to 94 parts by weight and the amount of (meth)acrylic acid esters represented by the following general formula (1) being 5 to 55 parts by weight relative to a total of 100 parts by weight of the monomer units, the acrylic base polymer having a crosslinked structure introduced therein, Reinforcing film: CH 2 =CR 1 -COO-(R 2 -O) m -R 3 (1) In the general formula (1), R 1 is a hydrogen atom or a methyl group; R 2 is an optionally branched alkylene group having 2 to 4 carbon atoms, m is an integer of 1 to 5, R 3 is a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or an aryl group having 6 to 20 carbon atoms.

2. The reinforcing film according to claim 1, wherein the alkyl group of the (meth)acrylic acid alkyl ester has 6 or more carbon atoms.

3. The reinforced film according to claim 1 or 2, wherein the acrylic base polymer has a weight average molecular weight of 100,000 or more before the introduction of a crosslinked structure.

4. The reinforcing film according to claim 1 or 2, wherein the photocurable composition contains 3 to 25 parts by weight of the photocuring agent per 100 parts by weight of the acrylic base polymer.

5. The reinforcing film according to claim 1 or 2, wherein the photocuring agent is a polyfunctional (meth)acrylate.

6. The reinforcing film according to claim 5, wherein the light curing agent comprises a polyfunctional (meth)acrylate containing an alkylene oxide chain.

7. The reinforced film according to claim 6, wherein the light hardener further comprises a urethane (meth)acrylate.

8. The reinforcing film according to claim 1 or 2, wherein the adhesive layer has an adhesive strength to a polyimide film of 1 N / 25 mm or less before photocuring.

9. The reinforcing film according to claim 1 or 2, wherein the adhesive layer has an adhesive strength to a polyimide film of 5 N / 25 mm or more after photocuring.

10. The pressure-sensitive adhesive layer has a shear storage modulus of 1.0×10 at −20° C. after photocuring. 4 ~5.0 x 10 5 The reinforced film according to claim 1 or 2, wherein the elastic modulus is 1.0 Pa.

11. The surface resistance of the pressure-sensitive adhesive layer is 5×10 11 The reinforced film according to claim 1 or 2, having a stiffness of Ω or less.

12. A method for manufacturing a device with a reinforced film, in which a reinforced film is attached to the surface of a foldable device, comprising: bonding the adhesive layer of the reinforced film described in claim 1 or 2 to the surface of the foldable device; and photo-curing the adhesive layer.

13. A device with a reinforced film, in which a reinforced film is attached to a surface of a foldable device, the reinforced film comprises a film substrate and an adhesive layer fixedly laminated on one main surface of the film substrate, the adhesive layer being attached to the device surface, the adhesive layer being a photocured product obtained by photocuring a photocurable adhesive composition containing an acrylic base polymer and a photocuring agent, and containing an antistatic agent, the acrylic base polymer containing, as monomer units, one or more selected from the group consisting of an alkyl (meth)acrylate ester; a (meth)acrylate ester represented by the following general formula (1); and a hydroxyl group-containing monomer and a carboxyl group-containing monomer, the amount of the alkyl (meth)acrylate ester being 40 to 94 parts by weight and the amount of the (meth)acrylate ester represented by the following general formula (1) being 5 to 50 parts by weight, relative to 100 parts by weight of the total of the monomer units, the acrylic base polymer having a crosslinked structure introduced therein, the adhesive layer having a shear storage modulus at -20°C of 1.0 x 10 4 ~5.0 x 10 5 Device with reinforcing film: CH 2 =CR 1 -COO-(R 2 -O) m -R 3 (1) In the general formula (1), R 1 is a hydrogen atom or a methyl group; R 2 is an optionally branched alkylene group having 2 to 4 carbon atoms, m is an integer of 1 to 5, R 3 is a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or an aryl group having 6 to 20 carbon atoms.

14. The surface resistance of the pressure-sensitive adhesive layer is 5×10 11 The device with the reinforced film according to claim 13, having a resistance of Ω or less.

Citation Information

Patent Citations

  • Adhesive composition with variable adhesive force for display and adhesive sheet for display

    CN113004809A

  • Adhesive agent composition, adhesive agent layer, and adhesive sheet

    JP2012172045A

  • polarizing plate

    JP2015529344A

  • Driving apparatus of image sensor and camera module including the same

    KR1020220145220A

  • Pressure-sensitive adhesive composition, pressure-sensitive adhesive, pressure-sensitive adhesive for optical member, and optical member with pressure-sensitive adhesive layer obtained using same