Laminate, bonded article, image display system, and method for producing bonded article
The laminate with a hard coat, resin base, and heat seal layers addresses the issue of wrinkles and mold dependency in bonding to curved surfaces by using a high bending stiffness and thermal shrinkage, allowing for efficient, wrinkle-free lamination on curved surfaces like windshield glass.
Patent Information
- Application Number
- PCT/JP2024/019165
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-10-24
- Filing Date
- 2024-05-24
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional methods for bonding laminates with heat seal layers to curved surfaces, such as windshield glass, often result in wrinkles and require the use of molds, which are time-consuming to remove and limit the flexibility of the lamination process.
A laminate comprising a hard coat layer, a resin base material, and a heat seal layer, with a bending stiffness coefficient of 5 × 10^6 [GPa·μm^3] or more and an average thermal shrinkage rate of 0.3% or more at 140°C, allowing for effective bonding to curved surfaces without molds by using a bag and heat pressure, while minimizing wrinkles.
The laminate achieves good followability to curved surfaces and suppresses wrinkle formation, enabling efficient and mold-free lamination with improved surface conformity and reduced processing time.
Smart Images

Figure JP2024019165_05122024_PF_FP_ABST
Abstract
Description
Laminate, bonded body, image display system, and method for manufacturing bonded body
[0001] The present invention relates to a laminate having a hard coat layer, a resin substrate, and a heat seal layer, a bonded body obtained by bonding this laminate to an object to be bonded, an image display system using this laminate, and a method for manufacturing a bonded body in which this laminate is bonded to an object to be bonded.
[0002] Currently, there is known a head-up display or head-up display system that projects an image onto the windshield of a vehicle or the like to provide the driver with various information such as a map, driving speed, and vehicle status.
[0003] In a head-up display system, a virtual image containing the above-mentioned various pieces of information is projected onto the windshield glass and observed by the driver or the like. The position of the virtual image is located outside the vehicle and forward of the windshield glass. The position of the virtual image is usually 1000 mm or more forward of the windshield glass, and closer to the outside world than the windshield glass. This allows the driver to obtain the above-mentioned various pieces of information while looking at the outside world ahead, without having to move their line of sight significantly. Therefore, when using a head-up display system, it is expected that the driver will be able to drive more safely while obtaining various pieces of information.
[0004] A head-up display system is configured, for example, by attaching a light-transmitting reflective film, such as a half-mirror film, to a windshield glass to form a projection image display unit. Various types of such reflective films have been proposed.
[0005] For example, Patent Document 1 proposes an optical film that can be used as a display medium in a head-up display system, which has an optical functional layer and a block layer, and the block layer has a cured product of a resin composition containing a thermoplastic resin and an ultraviolet-curable resin. In this optical film, examples of the optical functional layer include a half-wave plate, a quarter-wave plate, a laminate of a half-wave plate and a circularly polarized light reflective layer, and a laminate of a quarter-wave plate and a circularly polarized light reflective layer. Furthermore, an example of the circularly polarized light reflective layer is a light reflective layer using a cholesteric liquid crystal.
[0006] International Publication No. 2021 / 009394
[0007] As disclosed in Patent Document 1, a reflective film used in a head-up display system is used by being attached to glass such as a windshield glass. Windshield glass usually has a curved surface. As a method for attaching a sheet-like material such as a reflective film to an object having such a curved surface, a method conceptually shown in FIG. 6 is known, which utilizes thermocompression bonding using a heat seal layer.
[0008] In this method, first, as shown in the upper part of Fig. 6, a laminate 100 such as a reflective film laminated with a heat seal layer (not shown) is placed between a substrate 102 having a curved surface such as a windshield glass and a mold 104 having a surface corresponding to the curved surface of the substrate 102, and then housed in a bag 106 such as a rubber bag as shown in the second part of Fig. 6. Next, the pressure inside this bag 106 is reduced and heated to form a sandwiched body in which the laminate 100 is sandwiched between the substrate 102 and the mold 104, and the laminate 100 (heat seal layer) is vacuum-heat-pressed to the substrate 102. After the pressure-pressing using the bag is completed, the sandwiched body is removed from the bag, and as shown in the third part of Fig. 6, the sandwiched body is heat-pressed using an autoclave, and the laminate 100 is further heat-pressed to the substrate 102. After the heat-pressing using the autoclave is completed, the laminate is removed from the autoclave as shown in the lower part of Figure 6, and finally the mold 104 is removed from the laminate, thereby obtaining a laminate in which the laminate 100 is bonded to the object to be bonded 102.
[0009] According to this method for producing a bonded body, a laminate such as a reflective film having a heat seal layer can be bonded along the curved surface of a substrate such as a curved glass plate while suppressing the occurrence of wrinkles. On the other hand, this method for producing a bonded body requires a mold having a surface corresponding to the curved surface of the substrate. Furthermore, after the bonding is completed, it is necessary to remove the mold from the clamping body that holds the laminate between the substrate and the mold, which is a time-consuming process. Therefore, there is a need for a method for bonding a laminate having a heat seal layer to a substrate having a curved surface without using a mold.
[0010] However, according to the investigations of the present inventors, when a laminate having a conventional heat seal layer is attached to an object having a curved surface without using a mold, problems such as the occurrence of wrinkles in the attached laminate and insufficient ability to conform to the curved surface of the object often occur.
[0011] The object of the present invention is to solve the problems of the conventional technology and to provide a laminate that, when attached to a curved object, easily follows the curved surface of the object to be attached and can also suppress the occurrence of wrinkles after attachment, a bonded body using this laminate, an image display system using this laminate, and a method for manufacturing a bonded body that bonds this laminate to an object to be attached.
[0012] In order to achieve the above object, the present invention has the following configuration: [1] A laminate having a hard coat layer, a resin substrate, and a heat seal layer in this order, wherein the heat seal layer is disposed on the outermost side of the laminate, and a bending stiffness coefficient S represented by the following formula 1 is 5×10 6 [GPa·μm 3 ] or more, and the average heat shrinkage at 140°C is 0.3% or more. Formula 1: Flexural rigidity coefficient S = Average tensile modulus of laminate [GPa] × (Thickness of laminate [µm]) 3[2] The laminate according to [1], wherein the heat seal layer has a storage modulus of 300 MPa or less at 90°C. [3] The laminate according to [1] or [2], wherein the heat seal layer has a storage modulus of 50 MPa or more at 25°C. [4] The laminate according to any one of [1] to [3], further comprising a reflective layer. [5] The laminate according to any one of [1] to [4], further comprising a retardation layer. [6] The laminate according to any one of [1] to [5], further comprising a polarization conversion layer. [7] The laminate according to any one of [1] to [6], further comprising a hard coat layer, a resin substrate, a retardation layer, a reflective layer, a polarization conversion layer, and a heat seal layer, in this order. [8] The laminate according to [7], wherein the heat seal layer has a storage modulus of 150 MPa or less at 90°C and a storage modulus of 100 MPa or more at 25°C. [9] The laminate according to any one of [1] to [7], further comprising a protective film on the side of the hard coat layer opposite to the resin substrate.
[10] The laminate according to [8], further comprising a protective film on the side of the hard coat layer opposite to the resin substrate side.
[11] A bonded body comprising glass having a curved surface and the laminate according to any one of [1] to
[10] bonded to the glass.
[12] A bonded body comprising windshield glass and the laminate according to any one of [1] to
[10] bonded to the windshield glass.
[13] An image display system comprising the laminate according to any one of [1] to
[10] and an image display device that projects an image onto the laminate.
[14] A method for producing a bonded body, comprising: Step 1 of laminating an object to be bonded having a curved surface and the laminate according to any one of [1] to
[10] so that the heat seal layer faces the object to be bonded, and placing the laminate in a bag, and heating the inside of the bag under reduced pressure without using a mold having a surface corresponding to the curved shape of the object to be bonded, thereby conforming the laminate to the curved shape to obtain a bonded body; and Step 2 of heat-pressing the bonded body obtained in Step 1.
[15] The method for producing a laminate according to
[14] , wherein a sheet-like member is sandwiched between the laminate and the bag and heated under reduced pressure.
[0013] According to the present invention, it is possible to provide a laminate that can be bonded to an object having a curved surface, with good curve-following properties, while suppressing the occurrence of wrinkles after bonding.
[0014] Fig. 4 is a diagram conceptually showing an example of a laminate of the present invention. Fig. 5 is a conceptual diagram for explaining a manufacturing method of a bonded body of the present invention. Fig. 6 is a conceptual diagram for explaining a manufacturing method of a bonded body of the present invention. Fig. 7 is a diagram conceptually showing an example of an image display system of the present invention. Fig. 8 is a partially enlarged view of Fig. 4. Fig. 9 is a conceptual diagram for explaining a conventional manufacturing method of a bonded body.
[0015] The laminate, bonded body, image display system, and manufacturing method of the bonded body of the present invention will be described in detail below based on preferred embodiments shown in the accompanying drawings. Note that the drawings described below are conceptual for explaining the present invention, and the present invention is not limited to the drawings shown below. Therefore, the size, shape, and positional relationship of each member, as well as the thickness of each layer in the laminate and the thickness relationship between each layer, etc., differ from the actual ones. Furthermore, in the following description, "to" indicating a numerical range includes the values written on both sides. For example, ε 1 is the number α 1 ~Number β 1 That is, ε 1 The range of α 1 and the number β 1 The range includes α 1 ≦ε 1 ≦β 1 is.
[0016] The laminate of the present invention has a hard coat layer, a resin substrate, and a heat seal layer in this order, with the heat seal layer being located on the outermost side. FIG. 1 conceptually shows an example of the laminate of the present invention. The illustrated laminate 10 has, from the bottom in the figure, a protective film 12, a hard coat layer 14, a resin substrate 16, a retardation layer 18, a reflective layer 20, a polarization conversion layer 24, and a heat seal layer 26. In the present invention, the protective film 12, the retardation layer 18, the reflective layer 20, and the polarization conversion layer 24 in the illustrated laminate 10 are provided as preferred embodiments but are not essential components. For example, the laminate of the present invention may not have the protective film 12, or may not have one or more of the retardation layer 18, the reflective layer 20, and the polarization conversion layer 24.
[0017] That is, the laminate of the present invention can have various layer configurations as long as it has the hard coat layer 14, the resin substrate 16, and the heat seal layer 26 in this order, with the heat seal layer being positioned on the outermost side. In addition to the layers shown in the figure, various layers such as a linear polarizer and a filter can also be used.
[0018] Here, the laminate 10 of the present invention has a bending stiffness coefficient S that satisfies the following formula 1: 'Bending stiffness coefficient S = average tensile modulus of laminate [GPa] × (thickness of laminate [μm])' 3 The bending stiffness coefficient S expressed as ' is 5 x 10 6 [GPa·μm 3 ] or more, and the average heat shrinkage rate at 140° C. is 0.3% or more. By having such a configuration, the laminate 10 of the present invention can easily follow the curved surface of the object to be laminated when laminated to the object to be laminated having a curved surface, and further can suppress the occurrence of wrinkles after lamination.
[0019] As described above with reference to Figure 6, when laminating a laminate such as a reflective film having a heat seal layer to a curved substrate such as a windshield glass, the laminate (heat seal layer) is laminated to the substrate by using a mold that sandwiches the laminate together with the substrate, and performing vacuum heat compression bonding using a bag such as a rubber bag, or heat compression bonding in an autoclave. This method of manufacturing a laminated body can bond the laminate to the substrate without causing wrinkles or the like in the laminate, and can suitably follow the curved surface of the substrate. On the other hand, this method of manufacturing a laminated body requires a mold that corresponds to the curved surface of the substrate, and further requires the work of removing the mold after laminating the laminate to the substrate, which is time-consuming.
[0020] Therefore, it is desired to bond a laminate having a heat seal layer to a curved substrate without using a mold. However, conventional laminates (films) have low rigidity and are slippery. Therefore, when a laminate is bonded to a substrate by vacuum thermocompression bonding or autoclave thermocompression bonding without using a mold, wrinkles that occur in the laminate when it contacts the substrate become locally large, and these wrinkles remain in the laminate even after bonding.
[0021] In contrast, the laminate of the present invention has a bending stiffness coefficient S of 5×10 6 [GPa·μm 3 ] or more, and has good rigidity. Therefore, when the laminate of the present invention contacts an object to be laminated, wrinkles that occur do not become locally large, and the laminate is pressed by a bag with uniform, small wrinkles overall. Furthermore, the laminate of the present invention has an average heat shrinkage rate of 0.3% or more at 140°C. Therefore, wrinkles are eliminated by heat shrinkage when heated and pressed in an autoclave. Therefore, the laminate of the present invention can be laminated to an object to be laminated having a curved surface without using a mold, with good conformability to curved surfaces and suppressing the occurrence of wrinkles after lamination. This point will be further explained later with reference to Figures 2 and 3.
[0022] In the present invention, the bending stiffness coefficient S is 15×10 6 [GPa·μm 3 ] or more is preferable, and 25 × 10 6 [GPa·μm 3 In the present invention, there is no upper limit to the bending stiffness coefficient S, but it is preferable that it is 3000×10 6 [GPa·μm 3 ] or less, and 300 × 10 6 [GPa·μm 3 ] or less is more preferable, and 100 × 10 6 [GPa·μm 3 Flexural rigidity coefficient S is more preferably 3000×10 6 [GPa·μm 3 ] or less is preferable in that it is possible to prevent the laminate from becoming unnecessarily thick and it is easy to handle when the laminate is rolled up.
[0023] In the present invention, from the viewpoint of improving conformability to the curved surface of the object to be laminated, the average heat shrinkage at 140°C is preferably 0.4% or more, more preferably 0.6% or more. In the present invention, there is no upper limit to the average heat shrinkage at 140°C, but 5.0% or less is preferred. By setting the average heat shrinkage at 140°C to 5.0% or less, dimensional changes can be suppressed when conducting a heat resistance test of the laminate, which is preferable. As will be described later, in order to obtain a laminate exhibiting the above average heat shrinkage, a method of using a resin substrate with large residual stress can be mentioned.
[0024] In the present invention, the average tensile modulus and average thermal shrinkage for calculating the bending stiffness coefficient S may be measured by the method described in the Examples below. Specific methods will be described in detail in the Examples. When measuring the average tensile modulus, first, using one in-plane direction of the laminate as a reference, sample pieces of a predetermined size are cut out along the length direction in each direction rotated 45° clockwise from that direction. Next, the cut sample pieces are placed in a tensile tester so that the chuck spacing in the measurement direction is 100 mm, and stretched at a measurement temperature of 25°C and a stretching rate of 300 mm / min so that the chuck spacing increases, to obtain a stress-strain curve. The tensile modulus is calculated by linear regression of the obtained curve. The in-plane direction of the laminate corresponding to the length direction of the test piece showing the maximum tensile modulus of the above sample pieces is defined as the first direction, and the direction perpendicular to the first direction is defined as the second direction. The average value of the tensile modulus in the first direction and the tensile modulus in the second direction is defined as the average tensile modulus of the laminate. The specific method will be described in detail in the Examples. When measuring the average thermal shrinkage, first, using one in-plane direction of the laminate as a reference, a sample piece of a predetermined size is cut out, with its length aligned in each direction rotated 45° clockwise from that direction. Next, two reference lines are marked in the width direction of the cut sample piece at intervals of 100 mm. The sample piece is then placed in a heating oven at 140°C for 45 minutes under no tension, and then cooled to room temperature, and the distance between the two reference lines is measured. The thermal shrinkage of the sample piece is measured from the distance before and after the treatment. The in-plane direction of the laminate corresponding to the length direction of the test piece showing the largest thermal shrinkage among the thermal shrinkages of each sample piece is defined as the first direction, and the direction perpendicular to the first direction is defined as the second direction. The average value of the thermal shrinkage in the first direction and the thermal shrinkage in the second direction is defined as the average thermal shrinkage of the laminate.
[0025] The lower limit of the average tensile elastic modulus is not particularly limited, but is preferably 0.01 GPa or more, more preferably 0.1 GPa or more. The upper limit of the average tensile elastic modulus is not particularly limited, but is preferably 10.0 GPa or less, more preferably 8.0 GPa or less.
[0026] The lower limit of the thickness of the laminate is not particularly limited, but is preferably 100 μm or more, more preferably 150 μm or more. The upper limit of the thickness of the laminate is not particularly limited, but is preferably 1000 μm or less, more preferably 400 μm or less. The thickness of the laminate may be measured by the method described in the Examples below.
[0027] As described above, the laminate 10 shown in FIG. 1 has, from the bottom in the drawing, the protective film 12, the hard coat layer 14, the resin substrate 16, the retardation layer 18, the reflective layer 20, the polarization conversion layer 24, and the heat seal layer 26.
[0028] In the laminate 10 of the present invention, a protective film 12 can be used to suppress transfer of bag irregularities when the laminate is placed in a bag such as a rubber bag and subjected to thermocompression bonding, to prevent blocking during winding, and to stabilize transport. As mentioned above, the protective film 12 is not an essential component of the laminate of the present invention. The protective film 12 is preferably applied to the surface of the hard coat layer 14 as shown in FIG. 1 . More specifically, the protective film 12 is disposed on the side of the hard coat layer 14 opposite the resin substrate 16. The protective film 12 may be provided on the hard coat layer 14 after formation of the hard coat layer 14 and before curved surface molding, or may be laminated on the hard coat layer 14 during curved surface molding. The protective film 12 may be peeled off, for example, when it is no longer needed during windshield processing. Examples of materials for the protect film 12 include resins such as polyethylene resins, polypropylene resins, polystyrene resins, and polyethylene terephthalate resins, nitrile rubbers such as acrylonitrile-butadiene rubbers, butyl rubber, acrylic rubbers, thermoplastic elastomers such as thermoplastic polyolefin elastomers (TPO), thermoplastic polyurethane elastomers (TPU), thermoplastic polyester elastomers (TPEE), thermoplastic polyamide elastomers (TPAE), and diene elastomers (1,2-polybutadiene, etc.), and elastomers such as silicone elastomers and fluorine-based elastomers. A film formed from one or more of these materials in a single layer or multilayer configuration can be used as the protect film 12.
[0029] The thickness of the protective film 12 is not particularly limited as long as the laminate satisfies the above-mentioned flexural modulus of elasticity, but is preferably 20 μm or more, more preferably 100 μm or more, and even more preferably 200 μm or more. There is no particular upper limit, but it is often 5000 μm or less.
[0030] The tensile modulus of elasticity of the protective film 12 is not particularly limited as long as the laminate satisfies the above-mentioned flexural modulus of elasticity, but is preferably 0.001 GPa or more, more preferably 0.01 GPa or more, even more preferably 0.1 GPa or more, and particularly preferably 1.0 GPa or more. There is no particular upper limit, but it is often 12.0 GPa or less.
[0031] The tensile modulus of the protective film 12 can be varied, for example, depending on the material constituting the protective film 12. In general, the tensile modulus tends to increase by increasing the molecular weight and / or crystallinity of the resin or elastomer. Furthermore, the tensile modulus of the protective film 12 in the stretching direction can be increased by stretching the protective film 12. Even when the protective film 12 is made up of multiple layers, the tensile modulus refers to the tensile modulus of the protective film as a whole.
[0032] It is desirable for the protective film 12 to shrink when heated. Generally, the protective film 12 is also stretched during its manufacturing process, and residual stress resulting from the stretching remains. Therefore, this residual stress can be utilized to cause thermal shrinkage by heating during curved surface conforming. The temperature at which the protective film 12 thermally shrinks varies depending on the material of the protective film 12, but shrinkage is preferably in the range of 80 to 200°C, and more preferably in the range of 90 to 140°C, which is the heating temperature used in typical curved surface conforming processes. Heating to shrink the protective film 12 may be applied to the entire curved glass, or may be applied locally to areas with high curvature where insufficient conforming is likely to occur.
[0033] The heat shrinkage rate of the protective film 12 is not particularly limited as long as the laminate satisfies the above heat shrinkage rate, but at 140° C., the average heat shrinkage rate in the direction in which the heat shrinkage rate is greatest and in the direction perpendicular to that direction is preferably 0.3 to 10.0%, and more preferably 0.3 to 5.0%. The heat shrinkage rate can be adjusted as appropriate by the stretching conditions when producing the protective film 12.
[0034] The protective film 12 may have an adhesive layer on at least one side, or may be a self-adhesive protective film having adhesive properties.
[0035] The laminate 10 of the present invention has a hard coat layer (HC layer) 14. The presence of the HC layer 14 provides abrasion resistance that makes it difficult to scratch even when rubbed with a hard substance, scratch resistance that makes it difficult to scratch even when pressed with a hard substance, and stain resistance that allows stains to be easily wiped off even when stains adhere.
[0036] The HC layer 14 is preferably formed by polymerizing and curing at least one compound selected from the group consisting of polysiloxane-containing compounds having polymerizable groups in their molecules and fluorine-containing compounds having polymerizable groups in their molecules, and a polymerizable compound other than these compounds having polymerizable groups in their molecules, as described below. It is more preferable that these polymerizable groups are radically polymerizable groups. This allows the compound selected from the group consisting of polysiloxane-containing compounds and fluorine-containing compounds to exist in a bonded state with the polymerizable compound forming the HC layer 14, thereby providing better antifouling properties. When the compound selected from the group consisting of polysiloxane-containing compounds and fluorine-containing compounds has a polymerizable group, the polymerizable group in the compound selected from the group consisting of polysiloxane-containing compounds and fluorine-containing compounds described below reacts to form a bond and is present in the HC layer 14.
[0037] In addition, when the HC layer 14 has a laminate structure of two or more layers described below, it is preferable that the compound selected from the group consisting of polysiloxane-containing compounds and fluorine-containing compounds is contained in at least the HC layer farthest from the resin substrate 16, and more preferably, only the HC layer farthest from the resin substrate 16 contains the compound. When using at least one compound selected from the group consisting of polysiloxane-containing compounds having a polymerizable group in the molecule and fluorine-containing compounds having a polymerizable group in the molecule, it is preferable that the HC layer 14 farthest from the resin substrate is at least a cured film of the compound, and more preferably, only the HC layer 14 farthest from the resin substrate is a cured film of the compound. Specific embodiments of the HC layer 14 will be described below, but the present invention is not limited to the following embodiments.
[0038] The fluorine-containing compound is not particularly limited, and any compound having a fluorine atom in the molecule can be used as long as it can impart abrasion resistance and antifouling properties to the HC layer 14. As the fluorine-containing compound, a fluorine-containing antifouling agent that exhibits the properties of an antifouling agent is preferably used.
[0039] The fluorine-containing compound may be any of a monomer, an oligomer, and a polymer. The fluorine-containing compound preferably has a substituent that contributes to bond formation or compatibility with other components in the HC layer 14 (for example, a polysiloxane-containing compound, a polymerizable monomer that is a component of the resin, or a resin). The substituents may be the same or different, and it is preferable that there are multiple substituents. The substituent is preferably a polymerizable group, and may be any polymerizable reactive group that exhibits any of radical polymerization, cationic polymerization, anionic polymerization, condensation polymerization, and addition polymerization. Preferred examples of the substituent include an acryloyl group, a methacryloyl group, a vinyl group, an allyl group, a cinnamoyl group, an epoxy group, an oxetanyl group, a hydroxyl group, a polyoxyalkylene group, a carboxyl group, and an amino group. Among them, a radical polymerizable group is preferred, and an acryloyl group or a methacryloyl group is more preferred. The fluorine-containing compound may be a polymer or an oligomer with a compound that does not contain a fluorine atom.
[0040] The polysiloxane-containing compound in the present invention is not particularly limited, and examples thereof include compounds having a polysiloxane structure in the molecule. The polysiloxane structure of the polysiloxane-containing compound may be any of linear, branched, and cyclic. As the polysiloxane-containing compound, a polysiloxane antifouling agent exhibiting the properties of an antifouling agent is preferably used.
[0041] The content of the polysiloxane-containing compound in the HC layer-forming curable composition is preferably 0.01 to 5 mass%, more preferably 0.1 to 5 mass%, still more preferably 0.5 to 5 mass%, and particularly preferably 0.5 to 2 mass%, relative to the total solid content in the HC layer-forming curable composition. When the HC layer 14 has a laminate structure of two or more layers, as described below, the content of the polysiloxane-containing compound in the HC layer-forming curable composition means the amount added in the HC layer-forming curable composition that forms the HC layer 14 containing the polysiloxane compound.
[0042] The HC layer 14 can be obtained by irradiating an HC layer-forming curable composition with active energy rays to cure it. In this specification, the term "active energy rays" refers to ionizing radiation, and includes X-rays, ultraviolet rays, visible light, infrared rays, electron beams, α rays, β rays, γ rays, etc.
[0043] The curable composition for forming the HC layer 14 contains at least one component that has the property of being cured by irradiation with active energy rays (hereinafter also referred to as the "active energy ray-curable component"). The active energy ray-curable component is preferably at least one polymerizable compound selected from the group consisting of radically polymerizable compounds and cationically polymerizable compounds. In this specification, the term "polymerizable compound" refers to a compound having a polymerizable group in its molecule, and there may be at least one polymerizable group per molecule. The polymerizable group is a group that can participate in a polymerization reaction, and specific examples include groups contained in the various polymerizable compounds described below. Examples of polymerization reactions include various polymerization reactions such as radical polymerization, cationic polymerization, and anionic polymerization. The HC layer 14 is preferably obtained by irradiating a curable composition for forming the HC layer, which contains at least one compound selected from the group consisting of polysiloxane-containing compounds having a polymerizable group in their molecules and fluorine-containing compounds having a polymerizable group in their molecules, and a polymerizable compound other than these compounds having a polymerizable group in their molecules, with active energy rays to polymerize and cure the composition. In this case, the polymerizable groups of the polysiloxane-containing compound, the fluorine-containing compound, and the polymerizable compound are preferably radically polymerizable groups. The HC layer 14 may have a single-layer structure or a laminated structure of two or more layers, and an HC layer having a single-layer structure or a laminated structure of two or more layers, which will be described in detail below, is preferred.
[0044] As a preferred embodiment of the curable composition for forming a single-layer HC layer, a first embodiment includes a curable composition for forming a HC layer containing at least one polymerizable compound having two or more ethylenically unsaturated groups in one molecule. The ethylenically unsaturated group refers to a functional group containing an ethylenically unsaturated double bond. A second embodiment includes a curable composition for forming a HC layer containing at least one radically polymerizable compound and at least one cationically polymerizable compound.
[0045] The curable composition for forming an HC layer preferably contains a polymerization initiator, and more preferably contains a photopolymerization initiator. The curable composition for forming an HC layer containing a radical polymerizable compound preferably contains a radical photopolymerization initiator, and the curable composition for forming an HC layer containing a cationic polymerizable compound preferably contains a cationic photopolymerization initiator. Only one type of radical photopolymerization initiator may be used, or two or more types with different structures may be used in combination. This also applies to cationic photopolymerization initiators. Each photopolymerization initiator will be explained in turn below.
[0046] The radical photopolymerization initiator may be any one that can generate radicals as active species upon irradiation with light, and known radical photopolymerization initiators can be used without any limitations. The radical photopolymerization initiator and auxiliary agent can be synthesized by known methods and are also available as commercially available products. Preferred examples of commercially available radical photopolymerization initiators include Irgacure (127, 651, 184, 819, 907, 1870 (CGI-403 / Irg184=7 / 3 mixed initiator, 500, 369, 1173, 2959, 4265, 4263, etc.), OXE01) manufactured by BASF, KAYACURE (DETX-S, BP-100, BDMK, CTX, BMS, 2-EAQ, ABQ, CPTX, EPD, ITX, QTX, BTC, MCA, etc.) manufactured by Nippon Kayaku, and Esacure (KIP100F, KB1, EB3, BP, X33, KT046, KT37, KIP150, TZT) manufactured by Sartomer.
[0047] The content of the radical photopolymerization initiator in the curable composition for forming an HC layer is not particularly limited, and may be appropriately adjusted within a range in which the polymerization reaction (radical polymerization) of the radical polymerizable compound proceeds satisfactorily. The content is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 1 to 10 parts by mass, relative to 100 parts by mass of the radical polymerizable compound contained in the curable composition for forming an HC layer.
[0048] The cationic photopolymerization initiator may be any one that can generate cations as active species upon irradiation with light, and known cationic photopolymerization initiators can be used without any restrictions.
[0049] As the cationic photopolymerization initiator, a diazonium salt, an iodonium salt, a sulfonium salt, or an iminium salt is preferred from the viewpoint of the sensitivity of the photopolymerization initiator to light, the stability of the compound, etc. Furthermore, an iodonium salt is preferred from the viewpoint of weather resistance.
[0050] Specific commercially available examples of iodonium salt-based cationic photopolymerization initiators include B2380 manufactured by Tokyo Chemical Industry Co., Ltd., BBI-102 manufactured by Midori Chemical Industry Co., Ltd., WPI-113 manufactured by Wako Pure Chemical Industries, Ltd., WPI-124 manufactured by Wako Pure Chemical Industries, Ltd., WPI-169 manufactured by Wako Pure Chemical Industries, Ltd., WPI-170 manufactured by Wako Pure Chemical Industries, Ltd., and DTBPI-PFBS manufactured by Toyo Synthetic Chemical Industry Co., Ltd.
[0051] Specific examples of iodonium salt compounds that can be used as cationic photopolymerization initiators include the following compounds PAG-1 and PAG-2.
[0052]
[0053]
[0054] The content of the cationic photopolymerization initiator in the curable composition for forming the HC layer is not particularly limited, and may be appropriately adjusted within a range in which the polymerization reaction (cationic polymerization) of the cationic polymerizable compound proceeds satisfactorily. The content is preferably 0.1 to 200 parts by mass, more preferably 1 to 150 parts by mass, and even more preferably 2 to 100 parts by mass, relative to 100 parts by mass of the cationic polymerizable compound.
[0055] Other photopolymerization initiators include those described in paragraphs 0052 to 0055 of JP-A-2009-204725, the contents of which are incorporated herein by reference.
[0056] -Components that can be optionally contained in the curable composition for forming an HC layer- The curable composition for forming an HC layer contains at least one component that has the property of being cured by irradiation with active energy rays and a compound selected from the group consisting of polysiloxane-containing compounds and fluorine-containing compounds, and can optionally contain, and preferably contains, at least one polymerization initiator. The details of these are as described above.
[0057] The curable composition for forming an HC layer preferably contains a solvent. The solvent is preferably an organic solvent, and one or more organic solvents can be mixed in any desired ratio. Specific examples of organic solvents include alcohols such as methanol, ethanol, propanol, n-butanol, and i-butanol; ketones such as acetone, methyl isobutyl ketone, methyl ethyl ketone, and cyclohexanone; cellosolves such as ethyl cellosolve; aromatics such as toluene and xylene; glycol ethers such as propylene glycol monomethyl ether; acetate esters such as methyl acetate, ethyl acetate, and butyl acetate; and diacetone alcohol. Among these, it is preferable to use a mixture of cyclohexanone, methyl ethyl ketone, methyl isobutyl ketone, butyl acetate, isopropyl acetate, and methyl acetate in any desired ratio.
[0058] The amount of solvent in the HC layer-forming curable composition can be adjusted as appropriate within a range that ensures the coating suitability of the composition. The solvent content is preferably 50 to 500 parts by mass, more preferably 80 to 200 parts by mass, relative to 100 parts by mass of the total amount of the polymerizable compound and the photopolymerization initiator. The solid content of the HC-forming curable composition is preferably 10 to 90% by mass, more preferably 50 to 80% by mass, and even more preferably 65 to 75% by mass, relative to the total mass of the HC-forming curable composition.
[0059] In addition to the above components, the curable composition for forming an HC layer can contain any amount of one or more known additives. Examples of additives include surface conditioners, polymerization inhibitors, polyrotaxanes, etc. For details, see, for example, paragraphs 0032 to 0034 of JP 2012-229412 A. However, the additives are not limited to these, and various additives that can generally be added to curable compositions for forming an HC layer can be used.
[0060] The curable composition for forming the HC layer can be prepared by mixing the above-described various components simultaneously or sequentially in any order. The preparation method is not particularly limited, and a known mixer or the like can be used for preparation.
[0061] The thickness of the HC layer 14 is preferably 1 μm or more, more preferably 1 to 100 μm, even more preferably 1 to 20 μm, particularly preferably 3 to 20 μm, and most preferably 5 to 20 μm. The thickness of the HC layer 14 is measured by cutting the HC layer 14 with a microtome to cut out a cross section, staining it overnight with an approximately 3% by mass aqueous solution of osmium tetroxide, cutting out the surface again, and observing the cross section using a scanning electron microscope (SEM).
[0062] An HC layer can be formed by applying a curable composition for forming an HC layer and irradiating it with active energy rays. Coating can be performed by known coating methods such as dip coating, air knife coating, curtain coating, roller coating, die coating, wire bar coating, and gravure coating. The HC layer can also be formed as an HC layer having a laminate structure of two or more layers (e.g., about two to five layers) by simultaneously or sequentially applying two or more compositions having different compositions.
[0063] The HC layer can be formed by irradiating the applied HC layer-forming curable composition with active energy rays. For example, when the HC layer-forming curable composition contains a radical polymerizable compound, a cationic polymerizable compound, a radical photopolymerization initiator, and a cationic photopolymerization initiator, the polymerization reactions of the radical polymerizable compound and the cationic polymerizable compound can be initiated and progressed by the action of the radical photopolymerization initiator and the cationic photopolymerization initiator, respectively. The wavelength of the irradiated light may be determined depending on the type of polymerizable compound and polymerization initiator used. Examples of light sources for light irradiation include high-pressure mercury lamps, ultra-high-pressure mercury lamps, carbon arc lamps, metal halide lamps, xenon lamps, chemical lamps, electrodeless discharge lamps, and LEDs (light-emitting diodes) that emit light in the 150 to 450 nm wavelength band. The light irradiation dose is 30 to 3,000 mJ / cm. 2 is preferred, and 100 to 1500 mJ / cm 2is more preferable. A drying treatment may be carried out as necessary either before or after light irradiation, or both. The drying treatment can be carried out by blowing hot air, placing the composition in a heating furnace, transporting the composition in the heating furnace, or the like. When the curable composition for forming an HC layer contains a solvent, the heating temperature is not particularly limited as long as it is set to a temperature at which the solvent can be dried and removed. Here, the heating temperature refers to the temperature of the hot air or the atmospheric temperature in the heating furnace.
[0064] The laminate 10 includes a resin substrate 16. The material of the resin substrate 16 is not particularly limited as long as the laminate 10 satisfies the above-mentioned requirements for the flexural modulus and thermal shrinkage rate. The resin substrate 16 is preferably transparent in the visible light region.
[0065] There are no particular limitations on the material of the resin substrate 16. Examples of the resin substrate 16 include plastic films such as polyesters such as polyethylene terephthalate (PET), polycarbonates, acrylic resins, epoxy resins, polyurethanes, polyamides, polyimides, polyolefins, cellulose derivatives, and silicones. A cellulose acylate film is preferred as the resin substrate 16.
[0066] The thickness of the resin substrate 16 is not particularly limited as long as the laminate satisfies the above-mentioned flexural modulus of elasticity, but is preferably 10 μm or more, more preferably 25 μm or more, and even more preferably 40 μm or more. There is no particular upper limit, but it is often 500 μm or less.
[0067] The tensile modulus of elasticity of the resin substrate 16 is not particularly limited as long as the laminate satisfies the above-mentioned flexural modulus of elasticity, but is preferably 1.0 GPa or more, more preferably 2.5 GPa or more, even more preferably 3.0 GPa or more, particularly preferably 3.5 GPa or more, and most preferably 4.0 GPa or more. There is no particular upper limit, but it is often 12.0 GPa or less.
[0068] The tensile modulus of the resin substrate 16 can vary depending on, for example, the type of resin that constitutes the resin substrate 16. In general, the tensile modulus tends to increase by increasing the molecular weight and / or crystallinity of the resin. Furthermore, the tensile modulus of the resin substrate 16 in the stretching direction can be increased by stretching. Even when the resin substrate 16 is made up of multiple layers, the tensile modulus refers to the tensile modulus of the resin substrate 16 as a whole.
[0069] The resin substrate 16 may be formed into a film by any method, for example, a melt film-forming method or a solution film-forming method.
[0070] (Melt film-forming method, smoothing) When the resin substrate 16 is formed into a film by the melt film-forming method, the melt film-forming method preferably includes a melting step of melting the resin in an extruder, a step of extruding the molten resin into a sheet form from a die, and a step of forming it into a film. Depending on the material of the resin, a filtering step of the molten resin may be provided after the melting step, or the molten resin may be cooled when extruded into a sheet form. Specific melt film-forming methods will be described below, but the present invention is not limited thereto.
[0071] The method for producing the resin substrate preferably includes a melting step in which the resin is melted in an extruder, a filtering step in which the molten resin is filtered through a filtering device equipped with a filter, a film forming step in which the filtered resin is extruded into a sheet form from a die and brought into close contact with a cooling drum to be cooled and solidified to form an unstretched resin substrate, and a stretching step in which the unstretched resin substrate is stretched uniaxially or biaxially. This configuration allows the production of a resin substrate. If the pore size of the filter used in the filtering step of the molten resin is 1 μm or less, foreign matter can be sufficiently removed. As a result, the surface roughness of the resulting resin substrate in the film width direction can be controlled. Specifically, the method for forming a resin substrate can include the following steps.
[0072] [Melting Process] The method for producing the resin substrate includes a melting process in which the resin is melted in an extruder. It is preferable to dry the resin or a mixture of the resin and additives to a moisture content of 200 ppm or less, and then introduce it into a single-screw (single-screw) or twin-screw extruder and melt it. To suppress decomposition of the resin, it is also preferable to melt it in nitrogen or vacuum. Detailed conditions can be determined by citing paragraphs 0051-0052 of Japanese Patent No. 4962661 (paragraphs 0085-0086 of US 2013 / 0100378), and the contents of these publications are incorporated herein by reference. The extruder is preferably a single-screw kneading extruder. Furthermore, it is also preferable to use a gear pump to increase the delivery accuracy of the molten resin (melt).
[0073] [Filtration step] The method for producing the resin substrate includes a filtration step of passing the molten resin through a filtration device equipped with a filter, and the pore size of the filter used in the filtration step is preferably 1 μm or less. Only one set of filtration devices having filters with such pore sizes may be installed in the filtration step, or two or more sets may be installed.
[0074] [Film Forming Step] The method for producing the resin substrate includes a film forming step in which the filtered resin is extruded through a die into a sheet, and the sheet is brought into close contact with a cooling drum to be cooled and solidified to form an unstretched resin substrate.
[0075] When the melted (and kneaded) and filtered resin (melt containing the resin) is extruded into a sheet form through a die, it may be extruded as a single layer or as a multilayer. When extruding a multilayer, for example, a layer containing an ultraviolet absorber and a layer not containing an ultraviolet absorber may be laminated, and a three-layer structure with an ultraviolet absorber-containing layer as the inner layer is more preferable in terms of suppressing deterioration of the polarizer due to ultraviolet rays and suppressing bleed-out of the ultraviolet absorber. When a resin substrate is produced by extruding a multilayer, the thickness of the inner layer of the resulting resin substrate relative to the thickness of all layers is preferably 50 to 99%, more preferably 60 to 99%, and even more preferably 70 to 99%. Such lamination can be performed using a feedblock die and a multi-manifold die.
[0076] According to paragraph 0059 of JP 2009-269301 A, it is preferable to extrude a resin (a melt containing a resin) extruded into a sheet form from a die onto a cooling drum (a casting drum), cool and solidify it, and obtain an unstretched resin substrate (raw sheet).
[0077] In the above-mentioned method for producing a resin substrate, the temperature of the resin extruded from the die is preferably 280 to 320°C, more preferably 285 to 310°C. It is preferable that the temperature of the resin extruded from the die in the melting step is 280°C or higher, since this reduces the amount of unmelted raw resin and suppresses the generation of foreign matter. It is preferable that the temperature of the resin extruded from the die in the melting step is 320°C or lower, since this reduces the decomposition of the resin and suppresses the generation of foreign matter. The temperature of the resin extruded from the die can be measured non-contact on the surface of the resin using a radiation thermometer (manufactured by Hayashi Denko, model number: RT61-2, emissivity 0.95).
[0078] In the method for producing the resin substrate, it is preferable to use an electrostatically applied electrode when the resin is brought into close contact with the cooling drum in the film forming step, which allows the resin to be tightly contacted with the cooling drum without roughening the film surface.
[0079] In the method for producing the resin substrate, the temperature of the resin when it is brought into close contact with the cooling drum (the point where the molten resin extruded from the die first comes into contact with the cooling drum) is preferably 280°C or higher. This increases the electrical conductivity of the resin, allowing it to be tightly adhered to the cooling drum by applying static electricity, and suppressing roughness of the film surface. The temperature of the resin when it is brought into close contact with the cooling drum can be measured non-contact with the surface of the resin using a radiation thermometer (manufactured by Hayashi Denko, model number: RT61-2, emissivity 0.95).
[0080] [Stretching Step] The method for producing the resin substrate includes a stretching step in which an unstretched resin substrate is uniaxially or biaxially stretched. In the longitudinal stretching step (a step of stretching in the same direction as the film transport direction), the resin substrate is preheated and then stretched in the transport direction with a group of rollers having different peripheral speeds (i.e., different transport speeds) while the resin substrate is still heated.
[0081] The preheating temperature in the longitudinal stretching step is preferably Tg-40°C or higher and Tg+60°C or lower, more preferably Tg-20°C or higher and Tg+40°C or lower, and even more preferably Tg or higher and Tg+30°C or lower, relative to the glass transition temperature (Tg) of the resin substrate. The stretching temperature in the longitudinal stretching step is preferably Tg or higher and Tg+60°C or lower, more preferably Tg+2°C or higher and Tg+40°C or lower, and even more preferably Tg+5°C or higher and Tg+30°C or lower. The stretching ratio in the longitudinal direction is preferably 1.0 to 2.5 times, and more preferably 1.1 to 2 times.
[0082] In addition to or instead of the longitudinal stretching step, the resin substrate is stretched transversely in the width direction by a transverse stretching step (a step of stretching the film in a direction perpendicular to the film conveying direction). In the transverse stretching step, for example, a tenter can be suitably used, and the resin substrate is stretched transversely by this tenter while holding both widthwise ends with clips. This transverse stretching can increase the tensile modulus of the resin substrate.
[0083] The transverse stretching is preferably carried out using a tenter, and the stretching temperature is preferably from Tg to Tg + 60°C, more preferably from Tg + 2°C to Tg + 40°C, and even more preferably from Tg + 4°C to Tg + 30°C, relative to the glass transition temperature (Tg) of the resin substrate. The stretching ratio is preferably 1.0 to 5.0 times, more preferably 1.1 to 4.0 times. It is also preferable to relax the resin substrate in either the longitudinal direction or the transverse direction, or both, after the transverse stretching.
[0084] Furthermore, it is preferable that the variation in thickness in both the width direction and the length direction depending on the location be 10% or less, more preferably 8% or less, even more preferably 6% or less, particularly preferably 4% or less, and most preferably 2% or less.
[0085] The thickness variation can be calculated as follows.
[0086] A 10 m (meter) sample of the stretched resin substrate is taken, and 20% of each end in the width direction of the film is removed. 50 samples are taken at equal intervals in both the width direction and the length direction from the center of the film, and the thickness is measured.
[0087] Average thickness in the width direction Th TD-av , maximum value Th TD-max , and the minimum value Th TD-min , (Th TD-max -Th TD-min ) ÷ Th TD-av ×100 [%] is the thickness variation in the width direction.
[0088] In addition, the average thickness in the longitudinal direction Th MD-av , maximum value Th MD-max , and the minimum value Th MD-min , (Th MD-max -Th MD-min ) ÷ Th MD-av ×100 [%] is the thickness variation in the longitudinal direction.
[0089] The stretching step can improve the thickness accuracy of the resin substrate.
[0090] The stretched resin substrate can be wound into a roll in a winding process. At this time, the winding tension of the resin substrate is 0.02 kg / mm 2 It is preferable to do the following:
[0091] Regarding other detailed conditions, the contents described in paragraphs 0134 to 0148 of JP 2015-224267 A regarding the melt film-forming process and the contents described in JP 2007-137028 A regarding the stretching process can be incorporated into this specification in accordance with the present invention.
[0092] (Solution Casting Method, Smoothing) When a resin substrate is formed into a film by a solution casting method, it is preferable to include the steps of casting a dope solution on a casting band to form a cast film, drying the cast film, and stretching the cast film. Specifically, it is preferable to form the film by the method described in Japanese Patent No. 4,889,335. In the present invention, it is preferable to adopt the following method. For example, there is a method described in Japanese Patent Laid-Open No. 11-123732, in which the drying speed of the cast film is set to 300% by mass / min (=5% by mass / s) or less in terms of the solvent content on a dry basis, and gentle drying is performed. Furthermore, there is a method described in Japanese Patent Laid-Open No. 2003-276037, in which, in a co-casting method for a multilayered cast film having a core layer as an intermediate layer and skin layers (outer layers) on both surfaces thereof, the viscosity of the dope forming the core layer is increased to ensure the strength of the cast film and the viscosity of the dope forming the outer layer is decreased. Furthermore, there are also preferred methods such as a method in which the casting film is rapidly dried to form a film on the surface of the casting film, and the surface condition is smoothed by the leveling effect of the formed film, and a method in which the casting film is stretched.
[0093] It is desirable for the resin base material 16 to shrink due to heat. When the laminate is made to conform to a curved glass surface, excess portions of the flat laminate are generated relative to the curved glass, which presumably makes it difficult to conform to the curved surface. However, it is preferable for the resin base material 16 to thermally shrink, which allows the excess portions of the laminate to shrink and enable it to conform to the curved surface.
[0094] Generally, resin substrates are stretched during their manufacturing process, and residual stress resulting from the stretching remains. Therefore, this residual stress can be utilized to cause thermal shrinkage during heating during curved surface conforming. It is presumed that this thermal shrinkage allows the substrate to conform to the curved glass. Furthermore, insufficient conforming is likely to occur in areas of significant curvature near the periphery of the curved glass, but is unlikely to occur in areas of small curvature. In contrast, laminates using thermally shrinkable resin substrates effectively suppress insufficient conforming in areas of significant glass curvature. In areas of significant glass curvature, the laminate has the freedom to expand in the thickness direction, resulting in in-plane shrinkage. In areas of small glass curvature, the laminate has the freedom to expand in the thickness direction, resulting in almost no in-plane shrinkage. The temperature at which the resin substrate 16 thermally shrinks varies depending on the material from which the resin substrate 16 is formed, but shrinkage is preferably in the range of 80 to 200°C, and more preferably in the range of 90 to 140°C, which is the heating temperature used in typical curved surface conforming processes. Heating to shrink the resin base material 16 may be applied to the entire curved glass, or may be applied locally to a portion where the curvature is high and insufficient conformance is likely to occur.
[0095] The amount of shrinkage of the resin substrate 16 required to prevent insufficient conformance varies depending on the curvature and dimensions of the glass. The thermal shrinkage of the resin substrate 16 is not particularly limited as long as it satisfies the above-mentioned thermal shrinkage when formed into a laminate, but at 140°C, the average thermal shrinkage in the direction in which the thermal shrinkage is greatest and in the direction perpendicular to that direction is preferably 0.3 to 5.0%, more preferably 0.3 to 3.0%, and even more preferably 0.3 to 2.0%. The thermal shrinkage can be adjusted as appropriate by adjusting the stretching conditions when producing the resin substrate.
[0096] The laminate 10 has a retardation layer 18. As mentioned above, the retardation layer 18 is not an essential component of the laminate of the present invention. The retardation layer 18 imparts a phase difference (optical path difference) to two orthogonal polarized light components, thereby changing the state of incident polarized light.
[0097] When the retardation layer 18 is disposed on the glass plate side facing the vehicle interior and provides optical compensation, the front retardation of the retardation layer may be a retardation that can provide optical compensation. In this case, the front retardation of the retardation layer 18 at a wavelength of 550 nm is preferably 50 to 160 nm. Furthermore, when the direction corresponding to the vertically upward direction of the surface of the glass plate when the windshield glass having the laminate is mounted on a vehicle is defined as 0°, the angle of the slow axis is preferably 10 to 50° or −50 to −10°.
[0098] In addition, when the retardation layer 18 converts linearly polarized light into circularly polarized light, the retardation layer 18 is preferably configured to give a front retardation of λ / 4, or may be configured to give a front retardation of 3λ / 4. The angle of the slow axis may be set so as to be oriented in a direction that converts incident linearly polarized light into circularly polarized light.
[0099] In this case, the retardation layer 18 preferably has a front retardation at a wavelength of 550 nm in the range of 100 to 450 nm, more preferably in the range of 120 to 200 nm or 300 to 400 nm, for example. In addition, the direction of the slow axis of the retardation layer 18 is preferably determined depending on the incident direction of projection light for projecting an image when the laminate is used in a head-up display system and the sense of the helix of the cholesteric liquid crystal layer constituting the reflective layer.
[0100] The retardation layer 18 is not particularly limited and can be appropriately selected depending on the purpose. Examples of the retardation layer 18 include a stretched polycarbonate film, a stretched norbornene-based polymer film, a transparent film containing and oriented inorganic particles having birefringence such as strontium carbonate, a thin film obtained by obliquely depositing an inorganic dielectric on a support, a film in which a polymerizable liquid crystal compound is uniaxially oriented and fixed in orientation, and a film in which a liquid crystal compound is uniaxially oriented and fixed in orientation.
[0101] Among these, a film in which a polymerizable liquid crystal compound is uniaxially aligned and fixed is a suitable example of the retardation layer 18. As an example, such a retardation layer 18 can be formed by applying a liquid crystal composition containing a polymerizable liquid crystal compound to a transparent substrate, a temporary support, or the surface of an alignment layer, forming the polymerizable liquid crystal compound in the liquid crystal composition into a nematic alignment in a liquid crystal state, and then fixing the alignment by curing.
[0102] The retardation layer 18 may be a layer obtained by applying a composition containing a polymer liquid crystal compound to the surface of a transparent substrate, a temporary support, an alignment layer, or the like, forming a nematic alignment in a liquid crystal state, and then fixing the alignment by cooling.
[0103] The thickness of the retardation layer 18 is not particularly limited, but is preferably 0.2 to 300 μm, more preferably 0.5 to 150 μm, and even more preferably 1.0 to 80 μm. The thickness of the retardation layer 18 formed from a liquid crystal composition is not particularly limited, but is preferably 0.2 to 10 μm, more preferably 0.5 to 5.0 μm, and even more preferably 0.7 to 2.0 μm.
[0104] The laminate 10 has a reflective layer 20. As mentioned above, the reflective layer 20 is not an essential component of the laminate of the present invention. The reflective layer 20 reflects part or all of visible light and is not particularly limited. Examples include a layer containing a metal, a layer in which a dielectric is laminated, and a layer containing a liquid crystal. The reflective layer 20 preferably has a cholesteric liquid crystal layer having a selective reflection center wavelength in the red wavelength region, a cholesteric liquid crystal layer having a selective reflection center wavelength in the green wavelength region, and a cholesteric liquid crystal layer having a selective reflection center wavelength in the blue wavelength region. The three cholesteric liquid crystal layers have mutually different selective reflection center wavelengths. Each cholesteric liquid crystal layer may be in direct contact with any of the other cholesteric liquid crystal layers.
[0105] As is well known, a cholesteric liquid crystal layer is a layer in which liquid crystal compounds are fixed in a helical oriented state of a cholesteric liquid crystal phase, and reflects light with a selective reflection center wavelength corresponding to the pitch of the helical structure and transmits light in other wavelength ranges. Furthermore, a cholesteric liquid crystal layer exhibits selective reflection for either left- or right-handed circularly polarized light at a specific wavelength.
[0106] Here, from the viewpoint of visibility, it is preferable that the reflective layer 20 satisfy the following requirements (i) to (iii): (i) in the wavelength range of 400 nm or more and less than 500 nm, the maximum value of natural light reflectance is more than 7% (preferably more than 20%), the difference between the maximum and minimum values of natural light reflectance is 3% or more, and the total value of the wavelength bandwidth of the region higher than the average value of the maximum and minimum values of natural light reflectance is 20 to 80 nm; (ii) in the wavelength range of 500 nm or more and less than 600 nm, the maximum value of natural light reflectance is more than 7% (preferably more than 20%), the difference between the maximum and minimum values of natural light reflectance is 3% or more, and the total value of the wavelength bandwidth of the region higher than the average value of the maximum and minimum values of natural light reflectance is 20 to 80 nm. (iii) In the wavelength range of 600 to 800 nm, the maximum value of the natural light reflectance is more than 7% (preferably, 20% or more), and the total value of the wavelength bandwidth of the region higher than the average value of the maximum and minimum values of the natural light reflectance is 120 nm or more.
[0107] In a reflective layer having a cholesteric liquid crystal layer, the reflected wavelength and reflectance can be adjusted by the selective reflection center wavelength and thickness (helical pitch number) of the cholesteric liquid crystal layer, etc. A reflection that satisfies requirement (i) can be realized mainly by a cholesteric liquid crystal layer that reflects light in the blue wavelength region, a reflection that satisfies requirement (ii) can be realized by a cholesteric liquid crystal layer that reflects light in the green wavelength region, and a reflection that satisfies requirement (iii) can be realized by a cholesteric liquid crystal layer that reflects light in the red wavelength region.
[0108] From the viewpoint of being able to increase transmittance while improving reflected color, the maximum natural light reflectance at 400 nm or more and less than 500 nm is preferably more than 7%, more preferably 20% or more. The upper limit is not particularly limited, but is often, for example, 35% or less. Similarly, from the viewpoint of being able to increase transmittance while improving reflected color, the maximum natural light reflectance at 500 nm or more and less than 600 nm is preferably more than 7%, more preferably 20% or more. The upper limit is not particularly limited, but is often, for example, 35% or less. From the viewpoint of being able to increase the brightness of a displayed image while improving reflected color, the maximum natural light reflectance at 600 to 800 nm is preferably more than 7%, more preferably 20% or more. The upper limit is not particularly limited, but is often, for example, 35% or less.
[0109] From the viewpoint of being able to increase transmittance while improving reflected color, the difference between the maximum and minimum natural light reflectance values at wavelengths of 400 nm or more and less than 500 nm is preferably 4 to 20%, more preferably 4 to 12%. Similarly, from the viewpoint of being able to increase transmittance while improving reflected color, the difference between the maximum and minimum natural light reflectance values at wavelengths of 500 nm or more and less than 600 nm is preferably 4 to 20%, more preferably 4 to 12%.
[0110] From the viewpoint of improving the reflected color and increasing the transmittance, the wavelength bandwidth of the region where the reflectance is higher than the average of the maximum and minimum values of the reflectance between 400 nm and less than 500 nm is preferably 30 to 78 nm, more preferably 35 to 75 nm. Similarly, from the viewpoint of improving the reflected color and increasing the transmittance, the wavelength bandwidth of the region where the reflectance is higher than the average of the maximum and minimum values of the reflectance between 500 nm and less than 600 nm is preferably 30 to 78 nm, more preferably 35 to 75 nm. The narrower the wavelength bandwidth between 400 nm and less than 500 nm and the narrower the wavelength bandwidth between 500 nm and less than 600 nm, the more advantageous the transmittance is. However, since the wavelength bandwidth between 600 and 800 nm is wide, if the wavelength bandwidth between 400 nm and less than 500 nm and / or the wavelength bandwidth between 500 nm and less than 600 nm is too narrow, the reflected color may deteriorate. From this point of view, it is preferable that the wavelength bandwidth from 400 nm to less than 500 nm and the wavelength bandwidth from 500 nm to less than 600 nm are within the above ranges. Furthermore, the wavelength bandwidth from 500 nm to less than 600 nm has a greater effect on the transmittance.
[0111] From the viewpoint of improving the reflected color and the front brightness of the displayed image, the wavelength bandwidth of the region where the reflectance is higher than the average value of the maximum and minimum reflectance values from 600 to 800 nm is preferably 120 to 200 nm.
[0112] The reflective layer 20 preferably has two or more cholesteric liquid crystal layers with different selective reflection center wavelengths, and each cholesteric liquid crystal layer is preferably in direct contact with any other cholesteric liquid crystal layer.
[0113] If the cholesteric liquid crystal layers are spaced apart, the thickness between the layers becomes thicker, making it difficult to obtain the effect of interference of light reflected by each cholesteric liquid crystal layer. In contrast, a configuration in which the cholesteric liquid crystal layers are in contact with each other is preferable because the wavelength band width can be narrowed by the effect of interference of light reflected by each cholesteric liquid crystal layer. In particular, if the thickness of each cholesteric liquid crystal layer is thinner than the wavelength of light (visible light 380 to 780 nm), the effect of interference becomes more pronounced, which is preferable.
[0114] When the reflective layer 20 has two or more cholesteric liquid crystal layers, the cholesteric liquid crystal layers are not limited to being in direct contact with each other, but may be stacked via an adhesive layer or the like.
[0115] Here, each cholesteric liquid crystal layer may have at least one selective reflection center wavelength, but at least one of the cholesteric liquid crystal layers may have two or more selective reflection center wavelengths. A cholesteric liquid crystal layer having two or more selective reflection center wavelengths is achieved by a helical structure in which the helical pitch changes in the thickness direction.
[0116] The total thickness of the reflective layer 20 is preferably 0.4 to 2.0 μm, more preferably 0.6 to 1.8 μm, and even more preferably 0.8 to 1.4 μm.
[0117] The laminate 10 has a polarization conversion layer 24. As mentioned above, the polarization conversion layer 24 is not an essential component of the laminate of the present invention. The polarization conversion layer 24 is a layer in which the helical orientation structure of the liquid crystal compound is fixed, and it is preferable that the pitch number x of the helical orientation structure and the film thickness y (unit: μm) of the polarization conversion layer satisfy all of the following relational expressions (a) to (c): 0.1≦x≦1.0 (formula (a)) 0.5≦y≦3.0 (formula (b)) 3000≦(1560×y) / x≦50000 (formula (c)) Note that one pitch of the helical structure of the liquid crystal compound corresponds to one turn of the helix of the liquid crystal compound. In other words, a pitch number of 1 is defined as a state in which the director of the helically oriented liquid crystal compound (the long axis direction in the case of rod-shaped liquid crystal) rotates 360°.
[0118] When the polarization conversion layer 24 has a helical structure of a liquid crystal compound, it exhibits optical rotation and birefringence for visible light, which has a wavelength shorter than the reflection peak wavelength in the infrared range. Therefore, it is possible to control polarization in the visible range. By setting the pitch number x of the helical orientation structure of the polarization conversion layer 24 and the thickness y of the polarization conversion layer within the above-mentioned ranges, it is possible to provide the polarization conversion layer with the function of optically compensating for visible light, or the function of converting linearly polarized light (p-polarized light) incident on the laminate to circularly polarized light.
[0119] The polarization conversion layer 24 exhibits optical rotation and birefringence for visible light because the liquid crystal compound has a helical structure that satisfies the relational expressions (a) to (c). In particular, by setting the pitch P of the helical structure of the polarization conversion layer 24 to a length that corresponds to the pitch P of the cholesteric liquid crystal layer whose selective reflection center wavelength is in the long-wavelength infrared region, the polarization conversion layer 24 exhibits high optical rotation and birefringence for short-wavelength visible light.
[0120] The relational expression (a) satisfies "0.1≦x≦1.0." When the pitch number x of the helical structure is 0.1 or more, sufficient optical rotation and birefringence are obtained, which is preferable. When the pitch number x of the helical structure is 1.0 or less, sufficient optical rotation and birefringence are obtained, making it easy to obtain the desired elliptically polarized light.
[0121] The relational expression (b) is "0.5≦y≦3.0". When the thickness y of the polarization conversion layer is 0.5 μm or more, sufficient optical rotation and birefringence are obtained. When the thickness y of the polarization conversion layer is 3.0 μm or less, the optical rotation and birefringence are sufficient, making it easy to obtain the desired circularly polarized light.
[0122] The relational expression (c) is "3000≦(1560×y) / x≦50000". When "(1560×y) / x" is 3000 or more, the desired polarization is easily obtained. When "(1560×y) / x" is 50000 or less, the desired polarization is easily obtained.
[0123] In the present invention, the pitch number x of the helical structure of the polarization conversion layer 24 is more preferably 0.1 to 0.8, and the film thickness y is more preferably 0.6 to 2.6 μm. Also, "(1560×y) / x" is more preferably 5000 to 13000.
[0124] That is, it is preferable that the polarization conversion layer 24 has a long helical pitch P and a small pitch number x. Specifically, it is preferable that the polarization conversion layer 24 has a helical pitch P equivalent to the pitch P of a cholesteric liquid crystal layer having a selective reflection center wavelength in the long-wavelength infrared region and a small pitch number x. More specifically, it is preferable that the polarization conversion layer 24 has a helical pitch P equivalent to the pitch P of a cholesteric liquid crystal layer having a selective reflection center wavelength of 3,000 to 10,000 nm and a small pitch number x. Since the selective reflection center wavelength corresponding to the pitch P is much longer than that of visible light, such a polarization conversion layer 24 more suitably exhibits the optical rotation and birefringence for visible light described above.
[0125] Such a polarization conversion layer 24 can be formed basically in the same way as a known cholesteric liquid crystal layer. However, when forming the polarization conversion layer 24, it is preferable to adjust the liquid crystal compound to be used, the chiral agent to be used, the amount of chiral agent added, the film thickness, etc. so that the pitch number x of the helical structure and the film thickness y [μm] of the polarization conversion layer 24 satisfy all of the relational expressions (a) to (c).
[0126] The laminate 10 has a heat seal layer 26. The heat seal layer 26 is a layer for physically joining the laminate and an object to be pasted.
[0127] The heat seal layer 26 preferably contains a thermoplastic resin or elastomer. Thermoplastic resins with good affinity and adhesion to the substrate (e.g., a glass substrate) are preferred. Examples of suitable thermoplastic resins include 1,2-polybutadiene resin, ethylene-vinyl acetate copolymer (abbreviated as "EVA," which typically contains 3% or more by weight of vinyl acetate structural units), and polyolefin resins such as polyethylene, polyvinyl chloride resin, polystyrene resin, vinyl ester resin (excluding EVA), saturated polyester resin, polyamide resin, fluororesin (e.g., polyvinylidene fluoride), polycarbonate resin, polyacetal resin, urethane resin, epoxy resin, (meth)acrylate resin (also referred to as (meth)acrylic resin, meaning (meth)acrylic acid ester resin, etc.), unsaturated polyester resin, silicone resin, and modified versions of these resins. Urethane resins include urethane-modified polyester resins and urethane resins. Preferred thermoplastic resins include polyvinyl butyral or ethylene-vinyl acetate copolymer.
[0128] Polyvinyl butyral can be obtained by acetalizing polyvinyl alcohol with butyraldehyde. The degree of acetalization of polyvinyl butyral is not particularly limited, but is preferably 40% or more, more preferably 60% or more. The upper limit is not particularly limited, but is preferably 85% or less, more preferably 75% or less. Polyvinyl alcohol used in the synthesis of polyvinyl butyral is usually obtained by saponifying polyvinyl acetate, and polyvinyl alcohol with a saponification degree of 80 to 99.8 mol% is generally used. The degree of polymerization of the polyvinyl alcohol is preferably 200 to 3000.
[0129] Examples of the elastomer include block (co)polymers of conjugated dienes, acrylic block (co)polymers, styrene block (co)polymers, block copolymers of aromatic vinyl compounds and conjugated dienes, hydrogenated products of block (co)polymers of conjugated dienes, hydrogenated products of block copolymers of aromatic vinyl compounds and conjugated dienes, ethylene-α-olefin copolymers, polar group-modified olefin copolymers, elastomers composed of polar group-modified olefin copolymers and metal ions and / or metal compounds, nitrile rubbers such as acrylonitrile-butadiene rubbers, butyl rubber, acrylic rubbers, thermoplastic elastomers such as thermoplastic polyolefin elastomers (TPO), thermoplastic polyurethane elastomers (TPU), thermoplastic polyester elastomers (TPEE), thermoplastic polyamide elastomers (TPAE), diene elastomers (1,2-polybutadiene, etc.), silicone elastomers, and fluorine-based elastomers.
[0130] The thermoplastic resin or elastomer may be synthesized by a known method, or a commercially available product may be used. Examples of commercially available elastomers include Kuralyte LA1114, Kuralyte LA2140, Kuralyte LA2250, Kuralyte LA2330, Kuralyte LA4285, Hybrar 5127, Hybrar 7311F, Septon 2104, and Septon 2063 (trade names, manufactured by Kuraray Co., Ltd.). The elastomer is preferably an acrylic block (co)polymer or a styrene block (co)polymer.
[0131] The weight average molecular weight of the thermoplastic resin and elastomer is preferably 10,000 to 1,000,000, more preferably 50,000 to 500,000, from the viewpoint of the balance between solubility in a solvent and storage modulus.
[0132] The heat seal layer 26 may contain a plasticizer. When the heat seal layer contains a plasticizer, the storage modulus of the heat seal layer changes, improving the slipperiness and adhesion to glass.
[0133] The plasticizer is not particularly limited, and examples thereof include phosphate esters, carboxylic acid esters, carbohydrate derivatives, barbituric acid derivatives, rosin ester resins, rosin resins, hydrogenated rosin ester resins, petrochemical resins, hydrogenated petrochemical resins, terpene resins, terpene phenol resins, aromatic modified terpene resins, hydrogenated terpene resins, and alkylphenol resins, and these can be used alone or in combination of two or more.
[0134] Examples of the phosphate esters include triphenyl phosphate (TPP) and tricresyl phosphate (TCP). Typical examples of carboxylic acid esters include phthalates and citrates. Examples of phthalates include dimethyl phthalate (DMP), diethyl phthalate (DEP), dibutyl phthalate (DBP), dioctyl phthalate (DOP), diphenyl phthalate (DPP), and diethylhexyl phthalate (DEHP). Examples of citrate esters include triethyl O-acetylcitrate (OACTE) and tributyl O-acetylcitrate (OACTB). Other examples of carboxylic acid esters include butyl oleate, methylacetyl ricinoleate, dibutyl sebacate, and various trimellitic esters. Phthalate ester plasticizers (DMP, DEP, DBP, DOP, DPP, DEHP) are commonly used.
[0135] Examples of the carboxylic acid esters include triethylene glycol di-2-ethylbutyrate, triethylene glycol di-2-ethylhexanoate, triethylene glycol dicaprylate, triethylene glycol di-n-octanoate, triethylene glycol di-n-heptanoate, tetraethylene glycol di-n-heptanoate, dibutyl sebacate, dioctyl azelate, dibutyl carbitol adipate, ethylene glycol di-2-ethylbutyrate, 1,3-propylene glycol di-2-ethylbutyrate, 1,4-butylene glycol di-2-ethylbutyrate, diethylene glycol di-2-ethylbutyrate, diethylene glycol di-2-ethylhexanoate, and dipropylene glycol di-2 n-ethyl butyrate, triethylene glycol di-2-ethylpentanoate, tetraethylene glycol di-2-ethylbutyrate, diethylene glycol dicaprylate, triethylene glycol di-n-heptanoate, tetraethylene glycol di-n-heptanoate, triethylene glycol di-2-ethylbutyrate, triethylene glycol bis(2-ethylbutyrate), triethylene glycol di(2-ethylhexanoate), triethylene glycol diheptanoate, tetraethylene glycol diheptanoate, dihexyl adipate, dioctyl adipate, hexylcyclohexyl adipate, diisononyl adipate, heptylnonyl adipate, and dibutyl sebacate.
[0136] The carbohydrate derivative is preferably a monosaccharide or a carbohydrate derivative containing 2 to 10 monosaccharide units (hereinafter also referred to as a carbohydrate derivative plasticizer). Examples of the carbohydrate derivative plasticizer include maltose octaacetate, cellobiose octaacetate, sucrose octaacetate, sucrose acetate isobutyrate, xylose tetrapropionate, glucose pentapropionate, fructose pentapropionate, mannose pentapropionate, galactose pentapropionate, maltose octapropionate, cellobiose octapropionate, sucrose octapropionate, xylose tetrabenzoate, glucose pentabenzoate, fructose pentabenzoate, mannose pentabenzoate, galactose pentabenzoate, maltose octabenzoate, cellobiose octabenzoate, sucrose octabenzoate, xylitol pentabenzoate, and sorbitol hexabenzoate.
[0137] The barbituric acid derivatives can be synthesized, for example, by a method for synthesizing barbituric acid, in which a urea derivative and a malonic acid derivative are condensed. Barbituric acids having two substituents on the nitrogen atom can be obtained by heating N,N'-disubstituted urea and malonic acid chloride, or by mixing malonic acid with an activator such as acetic anhydride and heating the mixture. Preferred synthesis methods include those described in, for example, Journal of the American Chemical Society, Vol. 61, p. 1015 (1939), Journal of Medicinal Chemistry, Vol. 54, p. 2409 (2011), Tetrahedron Letters, Vol. 40, p. 8029 (1999), and WO 2007 / 150011.
[0138] The plasticizer may be synthesized by a known method, or a commercially available product may be used. Commercially available plasticizers include Super Ester A75, A115, and A125 (all manufactured by Arakawa Chemical Industries, Ltd., rosin ester resins), Pine Crystal KR-85, KE-311, and PE-590 (all manufactured by Arakawa Chemical Industries, Ltd., rosin resins), Petrotack 60, 70, 90, 100, 100V, and 90HM (all manufactured by Tosoh Corporation, petrochemical resins), YS Polystar T30, T80, T100, T115, T130, T145, and T160 (all manufactured by Yasuhara Chemical Co., Ltd., terpene phenol resins), and YS Resin PX800, PX1000, PX1150, and PX1250 (all manufactured by Yasuhara Chemical Co., Ltd., terpene resins). Examples of suitable oils include MORESCO White P-40, P-55, P-60, P-70, P-80, P-100, P-120, P-150, P-200, P-260, and P-350P (all manufactured by MORESCO Corporation, paraffinic oils), Diana Process Oil NS-24, NS-100, NM-26, NM-68, NM-150, NM-280, NP-24, NU-80, and NF-90 (all manufactured by Idemitsu Kosan Co., Ltd., naphthenic oils), and Diana Process Oil AC-12, AC-460, AE-24, AE-50, AE-200, AH-16, and AH-58 (all manufactured by Idemitsu Kosan Co., Ltd., aromatic oils).
[0139] The content of the plasticizer is preferably 1 to 80% by mass, more preferably 5 to 70% by mass, of the solid content of the heat seal layer, taking into consideration the balance of the storage moduli of the heat seal layer at 25°C and 95°C.
[0140] The heat seal layer 26 is preferably formed using a composition (heat seal layer-forming composition) containing a polymerizable compound for chemically bonding to the reflective layer or the polarization conversion layer. The polymerizable compound is preferably one that can chemically bond to the polymerizable liquid crystal compound used to form the reflective layer or the polarization conversion layer. For example, when the polymerizable liquid crystal compound has an ethylenically unsaturated polymerizable group, the polymerizable compound also preferably has an ethylenically unsaturated polymerizable group.
[0141] Examples of the ethylenically unsaturated polymerizable group-containing compound include the following. However, the present invention is not limited to the following exemplified compounds. For example, polyethylene glycol 200 di(meth)acrylate, polyethylene glycol 300 di(meth)acrylate, polyethylene glycol 400 di(meth)acrylate, polyethylene glycol 600 di(meth)acrylate, triethylene glycol di(meth)acrylate, epichlorohydrin-modified ethylene glycol di(meth)acrylate (commercially available products include Denacol DA-811 manufactured by Nagase & Co., Ltd.), polypropylene glycol 200 di(meth)acrylate, polypropylene glycol 400 di(meth)acrylate, polypropylene glycol 700 di(meth)acrylate, ethylene oxide (EO), propylene oxide (PO),propylene oxide) block polyether di(meth)acrylate (commercially available products, such as the Blemmer PET series manufactured by Nippon Oil & Fats Co., Ltd.), dipropylene glycol di(meth)acrylate, bisphenol A EO addition type di(meth)acrylate (commercially available products, such as M-210 manufactured by Toagosei Co., Ltd. and NK Ester A-BPE-20 manufactured by Shin-Nakamura Chemical Co., Ltd.), hydrogenated bisphenol A EO addition type di(meth)acrylate (NK Ester A-HPE-4 manufactured by Shin-Nakamura Chemical Co., Ltd.), bisphenol A PO addition type di(meth)acrylate (commercially available products, such as Light Acrylate BP-4PA manufactured by Kyoeisha Chemical Co., Ltd.), bisphenol A epichlorohydrin addition type di(meth)acrylate (commercially available products, such as Ebecryl 150 manufactured by Daicel UCB Co., Ltd.), bisphenol A EO·PO addition type di(meth)acrylate (commercially available products include BP-023-PE manufactured by Toho Chemical Industry Co., Ltd.), bisphenol F Examples of bifunctional (meth)acrylate compounds include EO-added di(meth)acrylate (commercially available products include Aronix M-208 manufactured by Toagosei Co., Ltd.), 1,6-hexanediol di(meth)acrylate and its epichlorohydrin-modified products, neopentyl glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate and its caprolactone-modified products, 1,4-butanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, trimethylolpropane di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, pentaerythritol di(meth)acrylate monostearate, trimethylolpropane acrylic acid benzoate, and isocyanuric acid EO-modified di(meth)acrylate (commercially available products include Aronix M-215 manufactured by Toagosei Co., Ltd.);
[0142] Further, trifunctional (meth)acrylate compounds such as trimethylolpropane tri(meth)acrylate (commercially available products include, for example, TPMTA manufactured by Nippon Kayaku Co., Ltd.) and its EO, PO, or epichlorohydrin-modified products, pentaerythritol tri(meth)acrylate, glycerol tri(meth)acrylate and its EO, PO, or epichlorohydrin-modified products, isocyanuric acid EO-modified tri(meth)acrylate (commercially available products include, for example, Aronix M-315 manufactured by Toagosei Co., Ltd.), tris(meth)acryloyloxyethyl phosphate, hydrogen phthalate-(2,2,2-tri-(meth)acryloyloxymethyl)ethyl, glycerol tri(meth)acrylate and its EO, PO, or epichlorohydrin-modified products; Examples of such compounds include tetrafunctional (meth)acrylate compounds such as tetraerythritol tetra(meth)acrylate (commercially available products include TPMTA manufactured by Shin-Nakamura Chemical Co., Ltd.), EO, PO, and epichlorohydrin-modified products thereof, and ditrimethylolpropane tetra(meth)acrylate; pentafunctional (meth)acrylate compounds such as dipentaerythritol penta(meth)acrylate and EO, PO, epichlorohydrin, fatty acid, and alkyl-modified products thereof; and hexafunctional (meth)acrylate compounds such as dipentaerythritol hexa(meth)acrylate and EO, PO, epichlorohydrin, fatty acid, and alkyl-modified products thereof, and sorbitol hexa(meth)acrylate and EO, PO, epichlorohydrin, fatty acid, and alkyl-modified products thereof. Two or more ethylenically unsaturated polymerizable group-containing compounds may be used in combination. In this case, a mixture of dipentaerythritol pentaacrylate and dipentaerythritol hexaacrylate, "DPHA" (manufactured by Nippon Kayaku Co., Ltd.), or the like can be preferably used.
[0143] Also preferred as the ethylenically unsaturated polymerizable group-containing compound are polyester(meth)acrylates and epoxy(meth)acrylates having a weight-average molecular weight of 200 or more and less than 1,000. Commercially available polyester(meth)acrylates include those manufactured by Arakawa Chemical Industries Co., Ltd. under the trade name of the Beamset 700 series, such as Beamset 700 (hexafunctional), Beamset 710 (tetrafunctional), and Beamset 720 (trifunctional). Epoxy(meth)acrylates include those manufactured by Showa Polymer Co., Ltd. under the trade name of the SP series, such as SP-1506, 500, SP-1507, and 480, and those manufactured by VR series, such as VR-77, and those manufactured by Shin-Nakamura Chemical Co., Ltd. under the trade names of EA-1010 / ECA, EA-11020, EA-1025, and EA-6310 / ECA.
[0144] The I / O ratio (ratio of inorganic value (I value) to organic value (O value)) of the polymerizable compound (particularly, an ethylenically unsaturated polymerizable group-containing compound) is preferably 0.40 or more, more preferably 0.60 or more, and even more preferably 1.2 or more, from the viewpoint of adhesion to a glass substrate. There is no particular upper limit to the I / O ratio, but it is preferably less than 3.0 from the viewpoint of compatibility with a thermoplastic resin.
[0145] The I / O ratio is calculated using the calculation method in the organic conceptual diagram. The organic conceptual diagram was proposed by Fujita et al. and is an effective method for predicting various physicochemical properties from the chemical structure of an organic compound (see Koda Yoshio, Organic Conceptual Diagram - Fundamentals and Applications, Sankyo Publishing (1984)). Since the polarity of an organic compound depends on the number of carbon atoms and substituents, the inorganic and organic values of other substituents are determined based on the organic value of the methylene group being 20 and the inorganic value of the hydroxyl group being 100, and the inorganic and organic values of the organic compound are then calculated. Organic compounds with a high inorganic value have high polarity, and organic compounds with a high organic value have low polarity.
[0146] Specific methods for calculating the I value, O value, and I / O ratio have been published as an organic conceptual diagram calculation sheet for Excel by Homma et al., co-authors of "New Edition Organic Conceptual Diagram: Fundamentals and Applications" (http: / / www.ecosci.jp / sheet / orgs_help.html), and these calculations can be performed using this.
[0147] When the composition used to form the heat seal layer 26 contains a polymerizable compound, the content of the polymerizable compound is preferably 5 to 80 mass %, more preferably 10 to 60 mass %, and even more preferably 15 to 50 mass %, based on the solid content of the composition. The solid content of the composition means the other components in the composition excluding the solvent. Even if the other components are in a liquid state, they are counted as the solid content.
[0148] The composition used to form the heat seal layer 26 (heat seal layer-forming composition) preferably contains a polymerization initiator from the viewpoint of adhesion to glass. Examples of the polymerization initiator include a photopolymerization initiator. The photopolymerization initiator may be any one that can generate radicals as active species upon light irradiation, and known photopolymerization initiators can be used without any restrictions. Specific examples include diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, benzyl dimethyl ketal, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-2-morpholino(4-thiomethylphenyl)propan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone oligomer, and 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one and other acetophenones; 1,2-octanedione, 1-[4-(phenylthio)-, 2-(O-benzoyloxime)], and Oxime esters such as ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(0-acetyloxime); benzoins such as benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether; benzophenones such as benzophenone, methyl ortho-benzoylbenzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyl-diphenyl sulfide, 3,3',4,4'-tetra(t-butylperoxycarbonyl)benzophenone, 2,4,6-trimethylbenzophenone, 4-benzoyl-N,N-dimethyl-N-[2-(1-oxo-2-propenyloxy)ethyl]benzenemethanaminium bromide, and (4-benzoylbenzyl)trimethylammonium chloride;Thioxanthones such as 2-isopropylthioxanthone, 4-isopropylthioxanthone, 2,4-diethylthioxanthone, 2,4-dichlorothioxanthone, 1-chloro-4-propoxythioxanthone, and 2-(3-dimethylamino-2-hydroxy)-3,4-dimethyl-9H-thioxanthone-9-one mesochloride; and acylphosphine oxides such as 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide. Furthermore, as an auxiliary agent for the polymerization initiator, triethanolamine, triisopropanolamine, 4,4'-dimethylaminobenzophenone (Michler's ketone), 4,4'-diethylaminobenzophenone, 2-dimethylaminoethylbenzoic acid, ethyl 4-dimethylaminobenzoate, (n-butoxy)ethyl 4-dimethylaminobenzoate, isoamyl 4-dimethylaminobenzoate, 2-ethylhexyl 4-dimethylaminobenzoate, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone, etc. may be used in combination. The above polymerization initiators and auxiliary agents can be synthesized by known methods or are commercially available. Commercially available radical photopolymerization initiators include Irgacure (127, 651, 184, 819, 907, 1870 (CGI-403 / Irg184=7 / 3 mixed initiator, 500, 369, 1173, 2959, 4265, 4263, etc.), OXE01) manufactured by BASF, KAYACURE (DETX-S, BP-100, BDMK, CTX, BMS, 2-EAQ, ABQ, CPTX, EPD, ITX, QTX, BTC, MCA, etc.) manufactured by Nippon Kayaku, and Esacure (KIP100F, KB1, EB3, BP, X33, KT046, KT37, KIP150, TZT) manufactured by Sartomer, and the like;
[0149] The content of the polymerization initiator contained in the composition used to form the heat seal layer 26 is not particularly limited, and may be appropriately adjusted within a range that allows the polymerization reaction of the polymerizable compound to proceed smoothly. When the composition used to form the heat seal layer contains a polymerization initiator, the content of the polymerization initiator is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 1 to 10 parts by mass, relative to 100 parts by mass of the polymerizable compound contained in the composition.
[0150] The heat seal layer 26 may contain inorganic particles. When the heat seal layer 26 contains inorganic particles, unevenness is formed on the surface of the heat seal layer 26, and when the heat seal layer 26 is rolled up in a state where the heat seal layer 26 and the HC layer 14 are in direct contact with each other, friction between the heat seal layer 26 and the HC layer 14 can be reduced, allowing the heat seal layer 26 to be rolled up without wrinkles, which is preferable. The inorganic particles contained in the heat seal layer 26 are preferably inorganic oxide particles, more preferably silica (silicon dioxide) particles, aluminum oxide particles, titanium dioxide particles, or zirconium oxide particles, and even more preferably silica particles.
[0151] The inorganic particles preferably consist of primary particles, with secondary particles formed by aggregation of the primary particles. The average primary particle size of the inorganic particles is not particularly limited, but is preferably 5 to 50 nm, more preferably 5 to 15 nm. The average secondary particle size of the inorganic particles is not particularly limited, but is preferably 100 to 500 nm.
[0152] The content of the inorganic particles in the heat seal layer 26 is not particularly limited, but is preferably 1% by mass or more, and more preferably 9% by mass or more, relative to the total mass of the heat seal layer 26. The upper limit is not particularly limited, but is preferably 40% by mass or less, and more preferably 30% by mass or less.
[0153] The average primary particle diameter of inorganic particles is measured by observation with a transmission electron microscope. Specifically, the diameter of the circle circumscribing the primary particles is determined for 50 randomly selected primary particles, and the arithmetic mean is taken as the average primary particle diameter. The magnification of the transmission electron microscope is set to any magnification between 500,000 and 5,000,000 that allows the primary particle diameter to be determined. The average secondary particle diameter is a value measured by performing spherical fitting (refractive index 1.46) using a laser diffraction / scattering particle size distribution analyzer. For example, a MicroTrac MT3000 manufactured by Microtrac-Bell Corporation can be used as the measuring device.
[0154] The heat seal layer 26 may contain a leveling agent. Known leveling agents can be used as the leveling agent, and examples thereof include surfactants. Of these, fluorine-based surfactants or silicone surfactants are preferred. The fluorine content of the fluorine-based surfactant is preferably 3 to 40% by mass, more preferably 5 to 30% by mass, and even more preferably 7 to 25% by mass. Fluorine-based surfactants with a fluorine content within this range are effective in terms of the uniformity of the thickness of the coating film and the liquid saving.
[0155] The content of the leveling agent in the heat seal layer 26 is not particularly limited, but is preferably 0.005 to 0.5% by mass, more preferably 0.01 to 0.1% by mass, based on the total mass of the heat seal layer 26.
[0156] The heat seal layer 26 is preferably formed by applying a heat seal layer-forming composition. The heat seal layer-forming composition contains the above-mentioned components and is used to form the heat seal layer 26. From the viewpoint of coatability, the heat seal layer-forming composition preferably contains a solvent. The type of solvent is not particularly limited, and examples include water and organic solvents, with organic solvents being preferred. Examples of organic solvents include ketones, alkyl halides, amides, sulfoxides, heterocyclic compounds, hydrocarbons, esters, and ethers.
[0157] The method for applying the composition for forming a heat seal layer is not particularly limited, and examples thereof include wire bar coating, curtain coating, extrusion coating, direct gravure coating, reverse gravure coating, die coating, spin coating, dip coating, spray coating, and slide coating.
[0158] The coating film obtained by coating may be subjected to a drying treatment, if necessary. Examples of the drying treatment include a heat treatment. The heating temperature in the heat treatment is not particularly limited, but is preferably 50 to 150°C, and more preferably 60 to 140°C. The heating time is not particularly limited, but is preferably 0.5 to 20 minutes, and more preferably 0.5 to 10 minutes.
[0159] The surface of the formed heat seal layer 26 (the surface opposite the reflective layer or polarization conversion layer) may be subjected to a surface treatment as needed. For example, in order to reduce the water contact angle of the surface of the heat seal layer 26, the surface of the heat seal layer 26 may be subjected to a hydrophilization treatment. Examples of hydrophilization treatments include plasma treatment, ultraviolet irradiation treatment, corona treatment, and electron beam irradiation treatment, with corona treatment being preferred. The conditions for the hydrophilization treatment are appropriately selected depending on the type of treatment to be performed, and are preferably adjusted so that the water contact angle of the surface of the heat seal layer 26 falls within the range described above.
[0160] The average thickness of the heat seal layer 26 is preferably 0.2 μm or more, more preferably 0.4 μm or more, and even more preferably 0.8 μm or more, from the viewpoint of adhesion to the glass substrate, reflective layer, or polarization conversion layer. There is no particular upper limit, but from the viewpoint of thinning, it is preferably 20 μm or less, more preferably 10 μm or less. The average thickness is measured by cutting the heat seal layer 26 with a microtome to extract a cross section, observing the cross section with a scanning electron microscope (SEM), measuring the thickness at three different positions on the heat seal layer 26, and calculating the average (arithmetic mean) of the measured values.
[0161] The heat seal layer 26 may have a single layer structure or a multi-layer structure of two or more layers. When the heat seal layer 26 has a multi-layer structure, the average value of the total thickness of the heat seal layer 26 may be within the above range.
[0162] In the present invention, the storage modulus of the heat seal layer at 25° C. and 90° C. is determined as follows.
[0163] (Sample Preparation Method) A coating liquid obtained by dissolving the heat seal layer in a solvent or melting the heat seal layer is applied to the release-treated surface of a release-treated release PET (polyethylene terephthalate) sheet so that the thickness after drying is 40 μm, and then dried. The heat seal layer is then peeled off from the release PET sheet to prepare a test piece of the heat seal layer. (Measurement Method) Using a dynamic viscoelasticity measuring device (DVA-225 manufactured by ITS Japan Co., Ltd.), the storage modulus at 25°C and 90°C was measured under the following conditions for the test piece, which had been previously conditioned at a temperature of 25°C and a relative humidity of 60% for 2 hours or more. Sample: 5 mm x 20 mm Grip distance: 20 mm Set strain: 0.10% Measurement temperature: -40 to 140°C Heating condition: 5°C / min
[0164] The storage modulus of the heat seal layer at 25° C. is preferably 50 MPa or more, more preferably 100 MPa or more, and even more preferably 200 MPa or more, from the viewpoint of sliding property with glass. The upper limit of the storage modulus of the heat seal layer at 25° C. is not particularly limited, but is often 6 GPa or less.
[0165] The storage modulus of the heat seal layer at 90° C. is preferably 300 MPa or less, more preferably 150 MPa or less, even more preferably 100 MPa or less, and even more preferably 50 MPa or less, from the viewpoint of adhesion to glass during thermocompression bonding at 90° C. There is no particular lower limit for the storage modulus of the heat seal layer at 90° C., but it is often 0.01 MPa or more.
[0166] The laminate of the present invention comprises glass having a curved surface and the laminate of the present invention bonded to the glass having a curved surface. There are no limitations on the glass having a curved surface, and various known glass can be used. Examples include curved window glass, curved glass used for the interior and exterior of buildings, and curved glass used for lenses.
[0167] Another embodiment of the laminate of the present invention comprises a windshield glass and the laminate of the present invention bonded to the windshield glass. There are no limitations on the type of windshield glass, and various types of windshield glass (windshield glass) used in vehicles such as automobiles, ships, aircraft, trains, and motorcycles can be used. Therefore, the windshield glass may be a single sheet of glass or a laminated glass in which multiple sheets of glass are laminated. Furthermore, the laminated glass may have an interlayer film such as polyvinyl butyral between the sheets, or may not have an interlayer film.
[0168] Such a bonded body of the present invention is preferably manufactured by the manufacturing method of the bonded body of the present invention shown below. Figures 2 and 3 conceptually show an example of a manufacturing method of the bonded body of the present invention. The following explanation will be given by taking as an example a case where the laminate of the present invention is bonded to a windshield glass. However, the present invention is not limited thereto, and various known objects to be bonded can be used as long as they have a curved surface. Examples of objects to be bonded other than windshield glass include glass having the various curved surfaces described above.
[0169] In the manufacturing method of the bonded body of the present invention, first, as shown in the upper part of Fig. 2, a windshield glass 28 and the laminate 10 of the present invention are laminated. At this time, lamination is performed so that the heat seal layer 26 of the laminate 10 faces the windshield glass 28. During this lamination, the laminate 10 is made to follow the curved shape of the windshield glass 28, thereby causing wrinkles to form in the laminate 10, as shown in the upper part of Fig. 3. Next, as shown in the second part of Fig. 2, the laminate is placed in a bag 106 such as a rubber bag similar to the example shown in Fig. 6. Here, the manufacturing method of the bonded body of the present invention does not use the mold 104 used in the conventional manufacturing method shown in Fig. 6.
[0170] Further, vacuum thermocompression bonding is performed in the same manner as above. That is, by heating while reducing the pressure inside the bag 106, the laminate 10 is pressed by the bag 106, and as a result, the laminate 10 is pressed against the windshield glass 28 and thermocompression bonded. Here, the laminate 10 of the present invention has a bending stiffness coefficient S of 5×10 6 [GPa·μm 3 ] or more, and has sufficient rigidity. Therefore, large local wrinkles are not generated in the laminate 10 when pressed by the bag 106, and the laminate 10 is pressed by the bag 106 in a state in which small wrinkles are generated all over the laminate, as shown in the middle part of FIG.
[0171] A sheet (sheet-like member) such as a film, rubber, or cloth may be sandwiched between the laminate 10 and the bag 106 and then vacuum-heat-compressed. By sandwiching the sheet and then vacuum-heat-compressing, it is possible to suppress indentations caused by dust that has become mixed in between the laminate 10 and the bag 106 being pressed against the laminate 10. Furthermore, if the slipperiness between the laminate 10 and the bag 106 is poor, uneven deaeration can be reduced by sandwiching a sheet with good slipperiness between both the laminate 10 and the bag 106.
[0172] The material of the film is not particularly limited, but examples thereof include acrylic resin films, polycarbonate (PC) resin films, cellulose ester resin films such as triacetyl cellulose (TAC) resin films, polyethylene terephthalate (PET) resin films, polyolefin resin films, polyester resin films, and acrylonitrile-butadiene-styrene copolymer films, and from the viewpoint of heat resistance, polycarbonate resin films, cellulose ester resin films, and polyethylene terephthalate resin films are preferred.
[0173] The film may have a surface irregularity to improve the slipperiness. The surface irregularity can be imparted by a known method such as adding a matting agent to the film or embossing the film.
[0174] The surface of the film is preferably subjected to an antistatic treatment in order to reduce adhesion of foreign matter during vacuum thermocompression bonding. The antistatic treatment can be carried out by a known method such as adding an antistatic agent.
[0175] The rubber is not particularly limited in terms of material, but examples thereof include butadiene rubber (BR), styrene-butadiene rubber (SBR), chloroprene rubber (CR), isoprene rubber (IR), acrylonitrile-butadiene rubber (NBR), ethylene-propylene-diene rubber (EPDM), butyl rubber (IIR), chloroprene rubber (CR), silicone rubber, and fluororubber, with EPDM rubber, silicone rubber, and fluororubber being preferred from the viewpoint of heat resistance. These may be used alone or in combination of two or more.
[0176] The rubber may have an uneven surface from the viewpoint of improving the slipperiness. The uneven surface can be imparted by a known method such as adding a matting agent to the rubber or embossing the rubber.
[0177] The rubber is preferably subjected to an antistatic treatment on its surface in order to reduce adhesion of foreign matter during vacuum heat and pressure bonding. The antistatic treatment can be performed by a known method such as adding an antistatic agent.
[0178] The rubber may be formed into a film by a known method, or a commercially available product may be used. Examples of commercially available rubbers include EB240N, EB250N, EB260N, EB270N, EB280W, EB265N, EB565N, and EB360E2 (EPDM rubbers, manufactured by Maxell Kureha Co., Ltd.), SW940D, SW950D, SW960D, SW970D, SR950D, SR930T, SR940T, SH950T, and SW955T (silicone rubbers, manufactured by Maxell Kureha Co., Ltd.), and FB750N, FB760N, FB770N, FB780N, FB880N, and FB970N (fluororubbers, manufactured by Maxell Kureha Co., Ltd.).
[0179] The cloth is preferably made of a dust-free material in order to reduce the generation and adhesion of foreign matter during vacuum heat pressing, and is preferably sewn with conductive carbon yarn in order to prevent static electricity.
[0180] The fabric may be prepared by a known method, or a commercially available product such as HM-CLC (manufactured by Tanimura Co., Ltd.) may be used.
[0181] The above-mentioned film, rubber, cloth or other sheet-like member is preferably the same size as or larger than the laminate 10 so that the pressure from the bag 106 can be transmitted to the laminate 10 evenly.
[0182] The above-mentioned film, rubber, cloth or other sheet-like member may be the same size as the windshield glass 28 or may be larger in size.
[0183] The conditions for vacuum heat pressing, such as the degree of vacuum and heating temperature, may be set appropriately depending on the material forming the heat seal layer 26, the heat resistance of the other materials forming the laminate 10, and the thickness of the laminate 10, etc.
[0184] After the vacuum thermocompression bonding is completed, the laminated body of the laminate 10 and the windshield glass 28 is removed from the bag, and the laminated body of the laminate 10 and the windshield glass 28 is further thermocompression bonded in an autoclave in the same manner as before, as shown in the third row of Fig. 2. After the thermocompression bonding in the autoclave is completed, the laminated body is removed from the autoclave and cooled, as shown in the lower row of Fig. 2.
[0185] As described above, the laminate 10 of the present invention has an average heat shrinkage rate of 0.3% or more at 140°C. Therefore, as shown in the lower part of Figure 3, fine wrinkles are eliminated by the thermal shrinkage of the laminate 10 due to heating in an autoclave. That is, the laminate 10 of the present invention can be attached to a curved windshield glass with good conformability and sufficient suppression of wrinkles after attachment, even without using a mold 104 as shown in Figure 6.
[0186] The conditions such as pressure and heating temperature in the autoclave may be set appropriately depending on the heat resistance of the material forming the heat seal layer 26 and the other materials forming the laminate 10, the thickness of the laminate 10, etc.
[0187] The image display system of the present invention includes the laminate of the present invention and an image display device that projects an image onto the laminate of the present invention. Figure 4 conceptually shows an example in which the image display system of the present invention is used in a head-up display system. In the following description, the head-up display system is also referred to as HUD.
[0188] The HUD 30 shown in Fig. 4 includes a laminate 10A of the present invention and a projector 32. As conceptually shown in Fig. 5, the laminate 10A is attached to a windshield glass 28 with the heat seal layer 26 facing the windshield glass 28. The laminate 10A is obtained by attaching the laminate 10 shown in Fig. 1 to the windshield glass 28 and then peeling off the protective film 12.
[0189] The projector 32 shown in FIG. 4 includes an image forming section 34 , an intermediate image screen 36 , a mirror 38 , and a concave mirror 40 .
[0190] 4, the projection light projected by the projector 32 passes through a transparent window 46 provided on a dashboard 42 of a vehicle equipped with the HUD 30, as indicated by the dashed-dotted line, enters the laminate 10A bonded to the windshield glass 28, is reflected by the reflective layer 20, and is observed by the driver D (also indicated by the dashed-dotted line). As with known HUDs, in the illustrated HUD 30, the driver D observes a virtual image of the image projected on the windshield glass 28.
[0191] The image forming unit 34 has an LCD (Liquid Crystal Display) 50 and a projection lens 52. Both the LCD 50 and the projection lens 52 are well-known devices used in HUD projectors. The image forming unit 34 projects the image displayed by the LCD 50 onto the intermediate image screen 36 using the projection lens 52. In the projector 32, the intermediate image screen 36 converts the projected image into a real image, which is then reflected along a predetermined optical path by the mirror 38 and the concave mirror 40. As described above, this reflected light passes through the transmission window 46 provided in the dashboard 42, enters the laminate 10A, and is reflected, allowing the projected image to be observed by the driver D.
[0192] In a preferred embodiment, the LCD 50 displays a p-polarized image (projected image). That is, in a preferred embodiment of the HUD 30 of the present invention, the projector 32 emits p-polarized projection light. Therefore, if the LCD 50 does not display p-polarized projection light, it is preferable to provide a polarizer that converts the projection light from the LCD 50 to p-polarized light, for example, somewhere along the optical path of the projection light from the LCD 50 to the concave mirror 40. Any known polarizer can be used. Alternatively, a polarizer that converts the projection light from the LCD 50 to p-polarized light may be provided outside the projector 32, i.e., somewhere along the optical path of the projection light from the concave mirror 40 to the windshield glass 28.
[0193] The illustrated laminate 10A uses a cholesteric liquid crystal layer as the reflective layer 20, for example. In the illustrated laminate 10A, the retardation layer 18 is a quarter-wave plate, for example. This quarter-wave plate converts incident p-polarized light into circularly polarized light with a rotational direction that is selectively reflected by the reflective layer 20, i.e., the cholesteric liquid crystal layer. Therefore, the laminate 10A converts p-polarized light into circularly polarized light using the retardation layer 18, reflects this circularly polarized light using the reflective layer 20, and converts the circularly polarized light back to p-polarized light using the retardation layer 18. This allows the laminate 10A to selectively reflect p-polarized light. As is well known, polarized sunglasses selectively block S-polarized light. Therefore, by emitting p-polarized projection light from the projector 32, a p-polarized image can be projected, allowing the driver D to view the image projected by the HUD 30 even when wearing polarized sunglasses.
[0194] In the projector constituting the HUD of the present invention, the image forming unit 34 is not limited to one using the LCD 50, and various known image forming means used in HUD projectors can be used. Examples of such known image forming means used in HUD projectors (imagers) include a fluorescent display tube, a liquid crystal on silicon (LCOS) display using liquid crystal, an organic electroluminescence (organic EL) display, and a digital light processing (DLP) display using a digital micromirror device (DMD). In these image forming means, similar to the LCD 50, a projection lens projects a projected image onto the intermediate image screen 36. Furthermore, the image forming means of the image forming unit 34 can also be an image forming means using light beam scanning.
[0195] The projection light emitted from the image forming unit 34 is then converted into a real image (visible image) by the intermediate image screen 36. There are no limitations on the intermediate image screen 36, and various known intermediate image screens that convert the projected image into a real image in the HUD projector can be used. Specific examples of the intermediate image screen 36 include a scattering film, a microlens array, and a screen for rear projection.
[0196] As described above, the projected light that has been formed into a real image on the intermediate image screen 36 is reflected along a predetermined optical path by the mirror 38 and the concave mirror 40, passes through the transparent window 46 provided in the dashboard 42, and is projected onto the laminate 10A bonded to the windshield glass 28, where it is observed by the driver D (see the dotted line).
[0197] The mirror 38 is a known mirror used in a projector to adjust the optical path of the projection light. The mirror 38 may also be a so-called cold mirror that reflects visible light and transmits infrared light, thereby preventing heating of the components of the projector 32 due to sunlight entering through the windshield glass. On the other hand, the concave mirror 40 is a known concave mirror that enlarges and projects the projection light and is used in a HUD projector.
[0198] Although the projector 32 in the illustrated example uses a mirror 38 and a concave mirror 40 as components that change the optical path of the projected light, the present invention is not limited to this. For example, the projector 32 may have only one of the mirror 38 and the concave mirror 40, or may have one or more other light-reflecting elements, such as a free-form mirror, in addition to or instead of the mirror 38 and / or the concave mirror 40. In other words, the projector that constitutes the HUD of the present invention can be configured using various light-reflecting elements.
[0199] As described above, the projector 32 emits p-polarized projection light. The p-polarized projection light projected by the projector 32 and transmitted through the transmission window 46 then passes through the hard coat layer 14 and the resin substrate 16 and enters the retardation layer 18. As described above, the retardation layer 18 is a quarter-wave plate that converts the incident p-polarized projection light into circularly polarized light with a rotation direction that is selectively reflected by the reflective layer 20 (cholesteric liquid crystal layer). The circularly polarized projection light converted by the retardation layer 18 is reflected by the reflective layer 20 and re-enters the retardation layer 18, where it is converted back to p-polarized light by the retardation layer 18. The projection light converted to p-polarized light by the polarization conversion layer 24 is irradiated onto the viewing position of the driver D. Here, because the projected image is p-polarized, the driver D can properly view the projected image even when wearing polarized sunglasses, as described above. Furthermore, as described above, the laminate of the present invention can be attached to a curved substrate such as windshield glass 28 without causing wrinkles, etc. Therefore, HUD 30, which reflects projected light from projector 32 using laminate 10A, which is the laminate of the present invention, can project high-quality images without image distortion caused by wrinkles, etc. in laminate 10A, regardless of whether polarized sunglasses are worn or not.
[0200] On the other hand, when glare-causing s-polarized light, such as light reflected from a puddle or the hood, enters from outside the vehicle, this s-polarized light passes through the windshield glass 28 and enters the laminate 10A, and then passes through the heat seal layer 26 and enters the polarization conversion layer 24. The s-polarized light that enters the polarization conversion layer 24 is converted into elliptically polarized light with a rotation direction corresponding to the s-polarized light, for example, by the helical structure of the liquid crystal compound in the polarization conversion layer 24.
[0201] The elliptically polarized light that has passed through the polarization conversion layer 24 then enters the reflective layer 20. As described above, the reflective layer 20 is a cholesteric liquid crystal layer that selectively reflects circularly polarized light converted from p-polarized light by the retardation layer 18. Therefore, elliptically polarized light with a rotation direction corresponding to s-polarized light passes through the reflective layer 20. Furthermore, by passing through the reflective layer 20 (cholesteric liquid crystal layer), the elliptically polarized light with a rotation direction corresponding to s-polarized light is converted to circularly polarized light with a rotation direction corresponding to s-polarized light. The circularly polarized light that has passed through the reflective layer 20 enters the retardation layer 18. As described above, the retardation layer 18 is a quarter-wave plate that converts p-polarized light into circularly polarized light that is selectively reflected by the cholesteric liquid crystal layer that constitutes the reflective layer 20. Therefore, the circularly polarized light with a rotation direction corresponding to s-polarized light that has entered the retardation layer 18 passes through the retardation layer 18 and is converted to s-polarized light. In this way, s-polarized light that causes glare and enters from outside the vehicle passes through the laminate 10A as s-polarized light. Therefore, this s-polarized light is blocked by polarized sunglasses even when it reaches the driver D. That is, when the laminate of the present invention is used in a HUD, it has a polarization conversion layer, and thus compensates for the change in polarization of external light caused by the retardation layer and the reflective layer, and s-polarized light that enters from outside the vehicle and causes glare can be transmitted as s-polarized light, making it possible to block the light with polarized sunglasses.
[0202] The image display system of the present invention is not limited to the HUD shown in the figure, and can be used in various known image display systems as long as it includes the laminate of the present invention and an image display device that projects an image onto the laminate of the present invention.
[0203] The laminate, the bonded body, the image display system, and the method for manufacturing the bonded body of the present invention have been described in detail above, but the present invention is not limited to the above-mentioned embodiments, and various improvements or modifications may be made within the scope of the present invention.
[0204] The features of the present invention will be explained in more detail below with reference to examples. The materials, reagents, amounts and proportions of substances, and procedures shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the following examples.
[0205] <Preparation of curable composition for forming hard coat layer (HC layer)> The components were mixed according to the formulation shown in Table 1 below, and the mixture was filtered through a polypropylene filter having a pore size of 10 μm to prepare curable composition HC-1 for forming a hard coat layer. The blending amount of each component shown in Table 1 is expressed in parts by mass.
[0206]
[0207] PAG-1 is the following compound:
[0208]
[0209] <Preparation of Compositions for Forming Heat-Seal Layer> The components shown in the table below were mixed and filtered through a polypropylene filter with a pore size of 10 μm to prepare compositions for forming heat-seal layers HS-1 to HS-11. The blending amount of each component shown in Table 2 is expressed in parts by mass.
[0210]
[0211] <Preparation of reflective layer-forming composition, retardation layer-forming composition, and polarization conversion layer-forming composition> The components were mixed according to the formulations shown in Table 3 below and filtered through a polypropylene filter with a pore size of 10 μm to prepare reflective layer-forming compositions BG1, R1, and IR1, retardation layer-forming composition A1, and polarization conversion layer-forming composition TW-1. The blending amount of each component shown in Table 3 is expressed in parts by mass. Note that mixture 1, alignment control agent 1, and alignment control agent 2 are the following compounds.
[0212]
[0213]
[0214]
[0215]
[0216] <Saponification of Cellulose Acylate Film> A 100 μm-thick cellulose acylate film was prepared by the same preparation method as in Example 20 of WO 2014 / 112575. UV-531 manufactured by Teisei Kako Co., Ltd. was added to this cellulose acylate film as an ultraviolet absorber. The amount added was 3 phr (per hundred resin). The prepared cellulose acylate film was passed through a dielectric heating roll at a temperature of 60° C. to raise the surface temperature of the film to 40° C., and then an alkaline solution having the composition shown below was applied to one side of the film using a bar coater in an amount of 14 mL / m. 2 The coating was then allowed to stand for 10 seconds under a steam-type far-infrared heater (manufactured by Noritake Co., Ltd.) heated to 110°C. Next, pure water was applied at a rate of 3 mL / m using the same bar coater. 2 The resulting film was then washed with water using a fountain coater and drained with an air knife three times, and then allowed to dry in a drying zone at 70°C for 5 seconds to produce saponified cellulose acylate film 1. Cellulose acylate films 2 and 3 were prepared according to the same preparation procedure as for cellulose acylate film 1, except that the film thickness was adjusted to 140 μm and 180 μm, respectively. Cellulose acylate film 4 was prepared according to the same preparation procedure as for cellulose acylate film 1, except that the film thickness was adjusted to 180 μm and the stretching conditions were adjusted so that the residual stress was increased. Cellulose acylate film 5 was prepared according to the same preparation procedure as for cellulose acylate film 1, except that the film thickness was adjusted to 180 μm and the stretching conditions were adjusted so that the residual stress was increased even more. Cellulose acylate film 6 was prepared according to the same preparation procedure as for cellulose acylate film 5, except that the film thickness was adjusted to 40 μm. Cellulose acylate film 7 was prepared according to the same preparation procedure as for cellulose acylate film 1, except that the film thickness was adjusted to 80 μm. Cellulose acylate film 8 was prepared according to the same preparation procedure as for cellulose acylate film 1, except that the stretching conditions were adjusted so as to reduce residual stress.
[0217] --------------------------------------------------- Composition of alkaline solution --------------------------------------------------- Potassium hydroxide 4.7 parts by mass Water 15.7 parts by mass Isopropanol 64.8 parts by mass Surfactant (C 16 H 33 O(CHCHO) 10 H) 1.0 part by mass Propylene glycol 14.9 parts by mass
[0218] <Formation of Hard Coat Layer> An HC layer-forming curable composition HC-1 was applied to the surface of the cellulose acylate film 1 prepared above opposite to the saponification treatment surface, and cured to form an HC1 layer with a thickness of 6 μm. Specifically, the application and curing methods were as follows. The HC layer-forming curable composition HC-1 was applied at a conveying speed of 30 m / min by the die coating method using a slot die described in Example 1 of JP-A-2006-122889, and dried at an atmospheric temperature of 60°C for 60 seconds to obtain a coating film. Thereafter, under a nitrogen purge, an air-cooled metal halide lamp (manufactured by Eye Graphics Co., Ltd.) with an oxygen concentration of about 0.1% by volume and an illuminance of 150 mW / cm was applied to the coating film. 2 , irradiation amount 600mJ / cm 2 The coating film was cured by irradiating it with ultraviolet light of 1000 kJ / cm 2 to form an HC layer, thereby obtaining a film HC1 having a resin substrate and an HC layer.
[0219] <Formation of Heat Seal Layer> Composition HS-1 for forming a heat seal layer was applied to the surface of the film HC1 opposite to the hard coat layer using a wire bar so that the film would have a dry thickness of 0.8 μm, and then dried at 120° C. for 1 minute to form a coating film. Thereafter, under a nitrogen purge, an air-cooled metal halide lamp (manufactured by Eye Graphics Co., Ltd.) with an oxygen concentration of about 0.1% by volume and an illuminance of 150 mW / cm was applied to the coating film. 2, irradiation amount 300mJ / cm 2 The coating was cured by irradiating it with ultraviolet light of 1000 kJ / cm 2 , thereby preparing a laminate of Example 1 having a structure of HC layer / resin substrate / heat seal layer.
[0220] Examples 2 to 5, Comparative Examples 1 to 3 Laminates of Examples 2 to 5 and Comparative Examples 1 and 2 were produced in the same manner as in Example 1, except that cellulose acylate films 2 to 5 and 7 to 8 were used as the resin substrates. In addition, a laminate of Comparative Example 3 was produced in the same manner as in Comparative Example 2, except that a hard coat layer was not formed.
[0221] Example 6 Formation of Alignment Film A coating solution for forming an alignment film having the following composition was applied to the saponified surface of the saponified cellulose acylate film 5 (resin substrate) obtained above at a rate of 24 mL / m using a wire bar coater. 2 The coating was dried with hot air at 100° C. for 120 seconds to obtain an alignment film having a thickness of 0.5 μm.
[0222] -------------------------------------------------- Composition of coating liquid for forming alignment film -------------------------------------------------- Modified polyvinyl alcohol shown below: 28 parts by mass Citrate ester (AS3, manufactured by Sankyo Chemical Co., Ltd.) 1.2 parts by mass Photoinitiator (Irgacure 2959, manufactured by BASF) 0.84 parts by mass Glutaraldehyde 2.8 parts by mass Water 699 parts by mass Methanol 226 parts by mass --------------------------------------------------
[0223] (Modified polyvinyl alcohol)
[0224]
[0225] <Preparation of Reflective Film> The alignment film prepared above was subjected to a rubbing treatment (rayon cloth, pressure: 0.1 kgf (0.98 N), rotation speed: 1000 rpm (revolutions per minute), conveying speed: 10 m / min, number of strokes: 1 round trip) in a direction rotated 45° clockwise with respect to the long side direction of the resin substrate.
[0226] The reflective layer-forming composition IR1 was applied to the rubbed alignment film surface at room temperature using a wire bar to obtain a coating film with a dry film thickness of 0.4 μm. The coating film was dried at room temperature for 30 seconds and then heated in an 85°C atmosphere for 2 minutes. The coating film was then irradiated with ultraviolet light at 60% output for 6 to 12 seconds using a Fusion D-bulb (90 mW / cm lamp) at 60°C in an environment with an oxygen concentration of 1000 ppm or less, thereby fixing the cholesteric liquid crystal phase and obtaining a 0.4 μm-thick cholesteric liquid crystal layer IR1. Next, the same process was repeated using the reflective layer-forming composition BG1 on the surface of the obtained cholesteric liquid crystal layer IR1, resulting in a 0.84 μm-thick cholesteric liquid crystal layer BG1. Next, the same process was repeated using the reflective layer-forming composition R1 on the surface of the obtained cholesteric liquid crystal layer BG1, resulting in a 0.36 μm-thick cholesteric liquid crystal layer R1. In this way, a film A1 having a reflective layer composed of three cholesteric liquid crystal layers was obtained. The transmission spectrum of the film A1 was measured using a spectrophotometer (V-670, manufactured by JASCO Corporation), and the transmission spectrum had selective reflection center wavelengths of 515 nm, 685 nm, and 775 nm.
[0227] Composition HS-1 for forming a heat seal layer was applied to the reflective layer side of cellulose acylate film 1 of film A1 prepared above using a wire bar so that the film thickness after drying would be 0.8 μm, and then the coating was dried at 120° C. for 1 minute to form a coating film. Thereafter, under a nitrogen purge, an air-cooled metal halide lamp (manufactured by Eye Graphics Co., Ltd.) of 160 W / cm and an oxygen concentration of about 0.1% by volume was used to illuminate the coating film at an illuminance of 150 mW / cm. 2 , irradiation amount 300mJ / cm 2The coating was cured by irradiating it with ultraviolet light of 1000 kJ / cm 2 , thereby obtaining a film HS1 having a structure of resin substrate / reflective layer / heat seal layer.
[0228] <Formation of Hard Coat Layer> An HC layer-forming curable composition HC-1 was applied to the surface of the film HS1 prepared above opposite the HS layer, and cured to form an HC1 layer with a film thickness of 6 μm. Specifically, the application and curing methods were as follows. The HC layer-forming curable composition was applied at a conveying speed of 30 m / min using the die coating method using a slot die described in Example 1 of JP 2006-122889 A, and dried at an atmospheric temperature of 60°C for 60 seconds to obtain a coating film. Thereafter, under a nitrogen purge, an air-cooled metal halide lamp (manufactured by Eye Graphics Co., Ltd.) with an oxygen concentration of about 0.1% by volume and an illuminance of 150 mW / cm was used to illuminate the coating film. 2 , irradiation amount 600mJ / cm 2 The coating film was cured by irradiating it with ultraviolet light of 1000 kJ / cm 2 to form an HC layer, thereby obtaining a laminate of Example 6 having a structure of HC layer / resin substrate / reflective layer / heat seal layer.
[0229] Example 7 A laminate of Example 7 having a structure of HC layer / resin substrate / retardation layer / reflective layer / heat seal layer was produced in the same manner as in Example 6, except that a composition A1 for forming a retardation layer was applied to a rubbed alignment film surface using a wire bar, dried, and then cured under the following conditions, and a composition IR1 for forming a reflective layer was applied onto the cured retardation layer A1.
[0230] <Curing Conditions for Composition A1 for Forming Retardation Layer> After the composition A1 for forming a retardation layer was applied and dried to obtain a coating film, the coating film was placed on a hot plate at 50°C and heated with an electrodeless lamp "D bulb" (60 mW / cm) manufactured by Fusion UV Systems in an environment with an oxygen concentration of 1000 ppm or less. 2 The coating film was irradiated with ultraviolet light for 6 seconds using a UV ray irradiator (UV irradiator) to form a retardation layer. This resulted in a retardation layer having a thickness adjusted to achieve a desired front retardation, i.e., a desired retardation. The retardation of the prepared retardation layer at 550 nm was measured using an AxoScan manufactured by Axometrics, and was found to be 126 nm.
[0231] Example 8 A laminate of Example 8 having a structure of HC layer / resin substrate / retardation layer / reflective layer / polarization conversion layer / heat seal layer was prepared in the same manner as in Example 7, except that a polarization conversion layer TW1 was applied to the cholesteric liquid crystal layer R1 to a thickness of 1.5 μm. The polarization conversion layer TW1 was prepared by applying the polarization conversion layer-forming composition TW1 to the cholesteric liquid crystal layer R1 at room temperature using a wire bar, drying the coating at room temperature for 30 seconds, and heating it in an 85 ° C. atmosphere for 2 minutes. Then, in an environment with an oxygen concentration of 1000 ppm or less, the coating was irradiated with ultraviolet light at 60% output for 6 to 12 seconds using a Fusion D bulb (90 mW / cm lamp) at 60 ° C. to form a polarization conversion layer.
[0232] Example 9 A laminate having a structure of HC layer / resin substrate / retardation layer / reflective layer / polarization conversion layer / heat seal layer was produced in the same manner as in Example 8, except that cellulose acylate film 6 was used as the resin substrate.
[0233] (Preparation of Protective Film 1) Novatec HF560 (manufactured by Japan Polyethylene Corporation) was prepared as the resin constituting the substrate layer. Ultrathene (registered trademark) 750 (manufactured by Tosoh Corporation) was prepared as the ethylene-vinyl acetate copolymer constituting the adhesive layer. Novatec (registered trademark) LC522 (manufactured by Japan Polyethylene Corporation) was also used as the polyethylene resin constituting the adhesive layer. Next, a resin mixture for the adhesive layer was prepared by blending the ethylene-vinyl acetate copolymer and the polyethylene resin at a mass ratio of 50:50. Next, using a T-die composite film-forming machine having two extruders, the resin constituting the substrate layer and the resin mixture for the adhesive layer were charged into each extruder, and the discharge rate of each extruder was adjusted (220°C) so that the substrate layer thickness ratio was 96% and the adhesive layer thickness ratio was 4%, resulting in a film thickness of 200 μm. Protective Film 1, a two-layer laminate film, was prepared. The protective film 1 was attached to the HC layer side of the above laminate so that the adhesive layer and the HC layer of the laminate were in contact with each other, thereby producing a laminate of Example 9 having a configuration of protective film 1 / HC layer / resin substrate / retardation layer / reflective layer / polarization conversion layer / heat seal layer.
[0234] Example 10 (Preparation of Protective Film 2) Protective film 2 was prepared in the same manner as in the preparation of protective film 1, except that the discharge rate of each extruder was adjusted so that the base layer thickness ratio was 97% and the pressure-sensitive adhesive layer thickness ratio was 3%, and the film thickness was set to 250 μm. A laminate of Example 10 having a configuration of protective film 2 / HC layer / resin substrate / retardation layer / reflective layer / polarization conversion layer / heat seal layer was prepared in the same manner as in Example 9, except that protective film 2 was used.
[0235] <Measurement of Tensile Modulus> The tensile modulus was measured and calculated according to the method described in JIS K7127. For the laminates of the Examples and Comparative Examples, a width of 10 mm and a length of 150 mm were cut out, with the length aligned in each direction rotated 45° clockwise from one in-plane direction as a reference. The cut-out sample pieces were placed in a tensile tester (manufactured by Toyo Seiki Seisakusho, trade name "Strograph-R2") so that the chuck spacing in the measurement direction was 100 mm, and stretched at a stretching rate of 300 mm / min at a measurement temperature of 25°C so that the chuck spacing increased, to obtain a stress-strain curve. The tensile modulus was calculated by linear regression of the curve between the two specified strains ε1 = 0.0005 and ε2 = 0.0025. The in-plane direction of the laminate corresponding to the length direction of the test piece showing the maximum tensile modulus of elasticity among the tensile moduli of the above sample pieces was defined as the first direction, and the direction perpendicular to the first direction was defined as the second direction.The average value of the tensile modulus of elasticity in the first direction and the tensile modulus of elasticity in the second direction was defined as the average tensile modulus of elasticity of the laminate.
[0236] <Film Thickness Measurement> The film thickness was measured by observation with a scanning electron microscope (SEM) using the following method. The cross sections of the laminates of the Examples and Comparative Examples were exposed by a standard method such as an ion beam or a microtome, and then the exposed cross sections were observed with an SEM. In the cross-sectional observation, the laminate was divided into four equal parts in the width direction, and the film thickness of the laminate was determined as the arithmetic mean of the film thicknesses at three equal division points excluding both ends.
[0237] <Measurement of Heat Shrinkage Ratio> The heat shrinkage ratio was measured as follows. Using one in-plane direction as a reference, the laminates of the Examples and Comparative Examples were cut out to widths of 30 mm and lengths of 120 mm, with the length direction aligned in each direction rotated 45° clockwise from that direction. Two reference lines were pre-marked in the width direction of the cut-out specimens at an interval of 100 mm. The specimens were left unloaded in a heating oven at 140°C for 45 minutes, and then cooled to room temperature, and the distance between the two reference lines was measured. The measured distance after treatment was designated A [mm]. The value [%] calculated from the distance of 100 mm before treatment and the distance A mm after treatment using the formula "100 × (100 - A) / 100" was taken as the heat shrinkage ratio of the specimen. The in-plane direction of the laminate corresponding to the length direction of the test piece showing the greatest thermal shrinkage rate among the thermal shrinkage rates of each sample piece was defined as the first direction, and the direction perpendicular to the first direction was defined as the second direction.The average value of the thermal shrinkage rates in the first direction and the second direction was defined as the average thermal shrinkage rate of the laminate.
[0238] <Wrinkle Evaluation> Wrinkle evaluation was performed as follows. A 260 mm long x 330 mm wide laminate of each of the Examples and Comparative Examples was placed on the concave side of a curved glass substrate with a curvature of 330 mm in the longitudinal direction (R1750 mm) and 260 mm in the transverse direction (R1250 mm). The laminate was placed at the center of the glass substrate, with the heat seal layer surface facing the contact surface. The laminate was placed in a rubber bag and the pressure was reduced to 10 kPa (0.1 atmospheres) using a vacuum pump. The temperature was then increased to 115°C under reduced pressure, maintained for 60 minutes, and then returned to room temperature and pressure. The laminate was then maintained in an autoclave (manufactured by Kurihara Seisakusho) at 140°C and 1.3 MPa (13 atmospheres) for 60 minutes to remove air bubbles, resulting in a glass sample in which the laminate and glass substrate were bonded together via a heat seal layer. Protective film 1 was then peeled off for Example 9, and protective film 2 was peeled off for Example 10. The glass samples were evaluated according to the following criteria. A to C are acceptable ranges. A: No wrinkles were present. B: Wrinkles were present, but not more than two. C: There were more than two wrinkles and not more than 10 wrinkles. D: There were more than 10 wrinkles.
[0239] <Evaluation of curved surface conformability> Evaluation of curved surface conformability is as follows. For the glass samples prepared above, the areas where no wrinkles occurred were evaluated according to the following criteria. A to C are acceptable ranges. A: No lifting occurred between the laminate and the glass substrate. B: Lifting occurred between the laminate and the glass substrate, accounting for 10% or less of the area. C: Lifting occurred between the laminate and the glass substrate, accounting for more than 10% and 30% or less of the area. D: Lifting occurred between the laminate and the glass substrate, accounting for more than 30% of the area.
[0240] <Evaluation of Projected Image Visibility> The glass sample prepared above was placed indoors with an imager (iPad (registered trademark) manufactured by Apple Inc.) fixed and installed on a horizontal floor surface by adjusting the image projection angle. The glass sample was positioned using a pedestal so that the distance between the center of the glass sample (image display unit) and the center of the imager was 1.0 m. At this time, the glass sample was tilted so that the angle between the floor surface and the surface of the glass sample was 30°. From a distance of 1.0 m from the glass sample, the laminate side of the glass sample was visually observed so that the gray background simulating a road and the HUD display image were superimposed. The luminance LB of the gray background and the luminance LI of the white display on the imager were measured using a spectroradiometer (SR-3AR manufactured by Topcon Technohouse Corporation). The LI / LB ratio was 3.0. The HUD display image used displayed white characters and was evaluated according to the following criteria: A: Characters were clearly readable. B: The letters were distorted but legible. C: The letters were faint and difficult to read. D: The letters were faint and severely distorted due to wrinkles and raised areas, making them unreadable.
[0241] <Evaluation of Abrasion Resistance> The laminates of the Examples and Comparative Examples were placed on a glass plate (manufactured by Corning, product name: Eagle XG, thickness 1 mm) in the center of the glass plate, with the surface on the heat seal layer side as the contact surface. After holding this at 115°C and 10 kPa (0.1 atmospheres) for 1 hour, it was heated in an autoclave (manufactured by Kurihara Seisakusho) at 140°C and 1.3 MPa (13 atmospheres) for 60 minutes to remove air bubbles, and a glass sample in which the laminate and the glass substrate were bonded with a heat seal layer was produced. Thereafter, Protect Film 1 was peeled off for Example 9, and Protect Film 2 was peeled off for Example 10. The glass samples were conditioned at a temperature of 25°C and a relative humidity of 60% for 2 hours, and then the haze (HA) before the abrasion test was measured using a haze meter (manufactured by Nippon Denshoku Co., Ltd., NDH2000N). Using a Taber abrasion tester (rotary abrasion tester manufactured by Toyo Seiki Co., Ltd.), the surface of the hard coat layer was subjected to 100 cycles of testing at a rotation speed of 72 rpm under a CS-10F abrasion wheel and a load of 500 gf. After the test, the haze (HB) of the test portion of the laminate was measured. The delta haze (HB - HA) before and after the test was calculated and evaluated according to the following criteria. <<Delta haze before and after abrasion resistance test>> A: Less than 4%. B: Greater than 4%.
[0242] In the following Table 4, the column "Resin substrate" indicates the type of cellulose acylate film used, and each numerical value indicates the number of the cellulose acylate film. For example, "1" in Example 1 indicates cellulose acylate film 1. In Table 4, "Flexural rigidity coefficient (×10 6 GPa·μm 3 ) column indicates the magnitude of the bending stiffness coefficient. For example, "6" in Example 1 corresponds to "6 x 10 6 [GPa·μm 3 ]".
[0243]
[0244] As shown in the above table, it was confirmed that the laminate of the present invention exhibited the desired effects. Furthermore, a comparison of Examples 1 to 3 revealed that the bending stiffness coefficient was 15×10 6 [GPa·μm 3 ] or more, the effect is better, and6 [GPa·μm 3 ] or more, it was confirmed that the effect is even better. Furthermore, a comparison of Examples 1, 4, and 5 confirmed that the effect is better when the thermal shrinkage rate is 0.4% or more, and even better when it is 0.6% or more. Furthermore, as shown in Examples 6 to 10, the presence of a reflective layer can improve the visibility of the projected image using the laminate. In particular, as shown in Examples 9 and 10, the presence of a protective film in the laminate suppresses the transfer of the unevenness of the rubber bag when the laminate is placed in the rubber bag and subjected to thermocompression bonding, thereby further improving the visibility of the projected image. Furthermore, the presence of a hard coat layer in the laminate of the present invention can also improve abrasion resistance. From the above results, the effects of the present invention are clear.
[0245] Example 101 (Preparation of Protective Film 3) Except for adjusting the discharge rate of each extruder so that the base layer thickness ratio was 97% and the pressure-sensitive adhesive layer thickness ratio was 3%, and for setting the film thickness to 230 μm, protective film 3 was prepared in the same manner as in the preparation of protective film 1. Except for using protective film 3, a laminate of Example 101 having a configuration of protective film 3 / HC layer / resin substrate / retardation layer / reflective layer / polarization conversion layer / heat seal layer was prepared in the same manner as in Example 9.
[0246] Examples 102 to 106 Laminates of Examples 102 to 106 having a structure of protect film 3 / HC layer / resin substrate / retardation layer / reflective layer / polarization conversion layer / heat seal layer were prepared in the same manner as in Example 101, except that HS-2 to HS-6 were used as the heat seal layer-forming compositions.
[0247] Example 107 A laminate of Example 107 having a structure of protect film 3 / HC layer / resin substrate / retardation layer / reflective layer / polarization conversion layer / heat seal layer was produced in the same manner as in Example 106, except that the coating was carried out so that the film thickness of the heat seal layer after drying would be 3.0 μm.
[0248] Example 108 A laminate of Example 108 having a structure of protect film 3 / HC layer / resin substrate / retardation layer / reflective layer / polarization conversion layer / heat seal layer was produced in the same manner as in Example 106, except that the coating was carried out so that the film thickness of the heat seal layer after drying would be 4.0 μm.
[0249] Example 109 A laminate of Example 109 having a structure of protect film 3 / HC layer / resin substrate / retardation layer / reflective layer / polarization conversion layer / heat seal layer was produced in the same manner as in Example 106, except that the coating was carried out so that the heat seal layer had a film thickness of 5.0 μm after drying.
[0250] Examples 1010 to 1014 Laminates of Examples 110 to 114 having a structure of protect film 3 / HC layer / resin substrate / retardation layer / reflective layer / polarization conversion layer / heat seal layer were prepared in the same manner as in Example 109, except that HS-7 to HS-11 were used as the heat seal layer-forming composition.
[0251] The laminates of Examples 101 to 114 were evaluated for wrinkles and curved surface conformability as described above, and also evaluated as follows.
[0252] <Evaluation of Wrinkles After Vacuum Thermocompression Bonding at 90°C> Evaluation of wrinkles after vacuum thermocompression bonding at 90°C is as follows. A 260mm long x 330mm wide laminate of Examples 101 to 114 was placed on the concave side of a curved glass substrate with a curvature of 330mm long x 1750mm R in the longitudinal direction and 260mm short x 1250mm R in the transverse direction, with the heat seal layer surface being the contact surface. This was placed in a rubber bag and the pressure was reduced to 10 kPa (0.1 atmospheres) using a vacuum pump. The bag was then heated to 90°C under reduced pressure, held for 60 minutes, and then returned to room temperature and pressure. The glass sample was evaluated according to the following criteria: A: No wrinkles were present; B: Wrinkles were present, but there were two or fewer wrinkles; C: There were more than two wrinkles and no more than 10 wrinkles; D: There were more than 10 wrinkles.
[0253] <Evaluation of Adhesion After Vacuum Thermocompression Bonding at 90°C> Evaluation of adhesion after vacuum thermocompression bonding at 90°C is as follows. For the glass samples prepared above, portions where no wrinkles occurred were evaluated according to the following criteria. A: No portion of the laminate was peeled off from the glass substrate. B: Some portion of the laminate was peeled off from the glass substrate, and the peeling accounted for 5% or less of the area. C: Some portion of the laminate was peeled off from the glass substrate, and the peeling accounted for more than 5% but not more than 10% of the area. D: Some portion of the laminate was peeled off from the glass substrate, and the peeling accounted for more than 10% of the area.
[0254] <Evaluation of Projected Image Visibility of 90°C Vacuum Heat-Compression Bonded Products> The glass samples prepared above were held in an autoclave (manufactured by Kurihara Seisakusho) at 140°C and 1.3 MPa (13 atmospheres) for 60 minutes to remove air bubbles, and glass samples were prepared in which the laminate and glass substrate were bonded with a heat-seal layer. The protective films were then peeled off. Indoors, an imager (Apple iPad (registered trademark)) was fixed and installed on a horizontal floor surface while adjusting the image projection angle. The glass sample was positioned using a pedestal so that the distance between the center of the glass sample (image display unit) and the center of the imager was 1.0 m. The glass sample was tilted so that the angle between the floor and the surface of the glass sample was 30°. The laminate side of the glass sample was visually observed from a distance of 1.0 m from the glass sample, so that a gray background simulating a road and the HUD display image were superimposed. The luminance LB of the gray background and the luminance LI of the white display on the imager were measured using a spectroradiometer (SR-3AR, manufactured by Topcon Technohouse Corporation), and the LI / LB ratio was found to be 3.0. The HUD display image used displayed characters in white and was evaluated according to the following criteria: A: The characters were clearly readable. B: The characters were distorted due to wrinkles or lifting, and some parts were unreadable. C: The characters were severely distorted due to wrinkles or lifting, and some parts were unreadable. D: The characters were very distorted due to wrinkles or lifting, and many parts were unreadable.
[0255] <Evaluation of Abrasion Resistance of 90°C Vacuum Heat-Compression Bonded Products> The laminates of Examples 101 to 113 were placed on a glass plate (manufactured by Corning, product name: Eagle XG, thickness 1 mm) with the surface of the heat seal layer facing the center of the glass plate. After holding this at 90°C and 10 kPa (0.1 atmospheres) for 1 hour, the laminate was heated in an autoclave (manufactured by Kurihara Seisakusho) at 140°C and 1.3 MPa (13 atmospheres) for 60 minutes to remove air bubbles, and a glass sample was prepared in which the laminate and the glass substrate were bonded with a heat seal layer. The protective film was then peeled off. The glass sample was conditioned at 25°C and 60% relative humidity for 2 hours, and then the haze (HA) before the abrasion test was measured using a haze meter (manufactured by Nippon Denshoku Co., Ltd., NDH2000N). Using a Taber abrasion tester (rotary abrasion tester manufactured by Toyo Seiki Co., Ltd.), the surface of the hard coat layer was subjected to 100 cycles of testing at a rotation speed of 72 rpm under a CS-10F abrasion wheel and a load of 500 gf. After the test, the haze (HB) of the test portion of the laminate was measured. The delta haze (HB - HA) before and after the test was calculated and evaluated according to the following criteria. <<Delta haze before and after abrasion resistance test>> A: Less than 4%. B: Greater than 4%.
[0256]
[0257] The laminate of Example 109 was evaluated by sandwiching a rubber sheet or film between the laminate and a rubber bag, and then vacuum-heat-pressing the laminate as described below.
[0258] <Evaluation of Wrinkles in Vacuum Heat-Compression Bonded Products with a Rubber Sheet Sandwiched> The laminate of Example 109, measuring 260 mm long x 330 mm wide, was placed on the concave side of a curved glass substrate with a curvature of 330 mm long x 1750 mm R in the longitudinal direction and 260 mm short x 1250 mm R in the transverse direction, with the heat-seal layer surface facing the center of the glass substrate. A rubber sheet EB360E2 (2 mm thick, EPDM rubber, manufactured by Maxell Kureha Co., Ltd.), measuring 260 mm long x 330 mm wide, was laminated on the protective film 3-layer side of the laminate of Example 109. This was placed in a rubber bag and the pressure was reduced to 10 kPa (0.1 atmospheres) using a vacuum pump. The rubber sheet was then removed, and the glass sample, in which the laminate and the glass substrate were bonded with the heat-seal layer, was heated to 115°C under reduced pressure, held for 60 minutes, and then returned to room temperature and pressure. The laminate was then placed in an autoclave (manufactured by Kurihara Manufacturing Co., Ltd.) at 140°C and 1.3 MPa (13 atmospheres) for 60 minutes to remove any air bubbles, producing a glass sample in which the laminate and glass substrate were bonded together with a heat seal layer. The protective film 3 was then peeled off. The glass samples were evaluated according to the following criteria. A to C are acceptable ranges. A: No wrinkles were present. B: Wrinkles were present, but there were two or fewer wrinkles. C: There were more than two wrinkles and no more than 10 wrinkles. D: There were more than 10 wrinkles.
[0259] <Evaluation of curved surface conformability of vacuum heat-bonded products sandwiching a rubber sheet> The glass samples prepared above were evaluated for wrinkle-free areas according to the following criteria. A to C are acceptable ranges. A: No lifting occurred between the laminate and the glass substrate. B: Lifting occurred between the laminate and the glass substrate, accounting for 10% or less of the area. C: Lifting occurred between the laminate and the glass substrate, accounting for more than 10% but not more than 30% of the area. D: Lifting occurred between the laminate and the glass substrate, accounting for more than 30% of the area.
[0260] <Evaluation of Wrinkles in Vacuum Heat-Compression Bonded Products with a Film Sandwiched Between Them> The laminate of Example 109, measuring 260 mm long x 330 mm wide, was placed on the concave side of a curved glass substrate with a curvature of 330 mm long x 1750 mm R in the longitudinal direction and 260 mm short x 1250 mm R in the transverse direction, with the heat-seal layer surface being the contact surface, at the center of the glass substrate. A 260 mm long x 330 mm wide PET film (60 μm thick, manufactured by Fujifilm Corporation) was laminated on the protective film 3 layer side of the laminate of Example 109. This was placed in a rubber bag and the pressure was reduced to 10 kPa (0.1 atmospheres) using a vacuum pump. The PET film was then removed, and the glass sample in which the laminate and the glass substrate were bonded by the heat-seal layer was heated to 115°C under reduced pressure, held for 60 minutes, and then returned to room temperature and pressure. The laminate was then placed in an autoclave (manufactured by Kurihara Manufacturing Co., Ltd.) at 140°C and 1.3 MPa (13 atmospheres) for 60 minutes to remove any air bubbles, producing a glass sample in which the laminate and glass substrate were bonded together with a heat seal layer. The protective film 3 was then peeled off. The glass samples were evaluated according to the following criteria. A to C are acceptable ranges. A: No wrinkles were present. B: Wrinkles were present, but there were two or fewer wrinkles. C: There were more than two wrinkles and no more than 10 wrinkles. D: There were more than 10 wrinkles.
[0261] <Evaluation of curved surface conformability of vacuum thermocompression bonded product sandwiching film> For the glass samples prepared above, the wrinkle-free portions were evaluated according to the following criteria. A to C are acceptable ranges. A: No lifting occurred between the laminate and the glass substrate. B: Lifting occurred between the laminate and the glass substrate, accounting for 10% or less of the area. C: Lifting occurred between the laminate and the glass substrate, accounting for more than 10% but not more than 30% of the area. D: Lifting occurred between the laminate and the glass substrate, accounting for more than 30% of the area.
[0262] <Evaluation of Wrinkles in Vacuum Heat-Compression Bonded Products Sandwiched Between a Film and a Rubber Sheet> The laminate of Example 109, measuring 260 mm long x 330 mm wide, was placed on the concave side of a curved glass substrate with a curvature of 330 mm long x 1750 mm R in the longitudinal direction and 260 mm short x 1250 mm R in the transverse direction, with the heat seal layer surface being the contact surface, at the center of the glass substrate. A 260 mm long x 330 mm wide PET film (60 μm thick, manufactured by Fujifilm Corporation) was laminated on the protective film 3 layer side of the laminate of Example 109. A 260 mm long x 330 mm wide rubber sheet EB360E2 (2 mm thick, EPDM rubber, manufactured by Maxell Kureha Co., Ltd.) was laminated on the PET film. This was placed in a rubber bag and the pressure was reduced to 10 kPa (0.1 atmospheres) using a vacuum pump. The rubber sheet and PET film were then removed, and the glass sample in which the laminate and glass substrate were bonded with a heat-seal layer was heated to 115°C under reduced pressure, held for 60 minutes, and then returned to room temperature and pressure. The sample was then held in an autoclave (manufactured by Kurihara Seisakusho) at 140°C and 1.3 MPa (13 atmospheres) for 60 minutes to remove air bubbles, producing a glass sample in which the laminate and glass substrate were bonded with a heat-seal layer. The protective film 3 was then peeled off. The glass sample was evaluated according to the following criteria. A to C are acceptable ranges. A: No wrinkles were present. B: Wrinkles were present, but there were two or fewer wrinkles. C: There were more than two wrinkles and no more than 10 wrinkles. D: There were more than 10 wrinkles.
[0263] <Evaluation of curved surface conformability of vacuum heat-press bonded product sandwiching film and rubber sheet> For the glass samples prepared above, the areas where no wrinkles occurred were evaluated according to the following criteria. A to C are acceptable ranges. A: No lifting occurred between the laminate and the glass substrate. B: Lifting occurred between the laminate and the glass substrate, accounting for 10% or less of the area. C: Lifting occurred between the laminate and the glass substrate, accounting for more than 10% but not more than 30% of the area. D: Lifting occurred between the laminate and the glass substrate, accounting for more than 30% of the area.
[0264]
[0265]
[0266] The present invention can be suitably used in head-up display systems and the like.
[0267] REFERENCE SIGNS LIST 10, 100 Laminate 12 Protective film 14 Hard coat layer 16 Resin substrate 18 Retardation layer 20 Reflective layer 24 Polarization conversion layer 26 Heat seal layer 28 Windshield glass 30 HUD (Head-up display system) 32 Projector 34 Image forming unit 36 Intermediate image screen 38 Mirror 40 Concave mirror 42 Dashboard 46 Transmitting window 50 LCD (Liquid crystal display) 52 Projection lens 102 Substrate to be attached 104 Mold 106 Bag D Driver
Claims
1. A laminate having a hard coat layer, a resin substrate, and a heat seal layer in this order, the heat seal layer being disposed on the outermost side of the laminate, and the bending stiffness coefficient S represented by the following formula 1 is 5×10 6 [GPa·μm 3 ] or more, and the average heat shrinkage rate at 140 ° C. is 0.3% or more. Formula 1 Bending stiffness coefficient S = average tensile modulus of the laminate [GPa] × (thickness [μm] of the laminate) 3 2. The laminate according to claim 1, wherein the heat seal layer has a storage modulus of 300 MPa or less at 90°C.
3. The laminate according to claim 1, wherein the heat seal layer has a storage modulus of 50 MPa or more at 25°C.
4. The laminate according to claim 1, further comprising a reflective layer.
5. The laminate according to claim 4, further comprising a retardation layer.
6. The laminate according to claim 4, further comprising a polarization conversion layer.
7. The laminate according to claim 1, comprising the hard coat layer, the resin substrate, a retardation layer, a reflective layer, a polarization conversion layer, and the heat seal layer in this order.
8. The laminate according to claim 7, wherein the heat seal layer has a storage modulus of 150 MPa or less at 90°C and a storage modulus of 100 MPa or more at 25°C.
9. The laminate according to claim 1, further comprising a protective film on the side of said hard coat layer opposite to said resin substrate.
10. The laminate according to claim 8, further comprising a protective film on the side of said hard coat layer opposite to said resin substrate.
11. A laminate comprising glass having a curved surface and the laminate according to any one of claims 1 to 10 laminated to the glass.
12. A laminate comprising a windshield glass and the laminate according to any one of claims 1 to 10 attached to the windshield glass.
13. An image display system comprising the laminate according to any one of claims 1 to 10 and an image display device that projects an image onto the laminate.
14. A method for producing a laminate comprising: step 1 of laminating a curved object to be laminated and the laminate according to any one of claims 1 to 10 in such a manner that the heat seal layer faces the object to be laminated, and housing the laminate in a bag; and step 2 of heat-pressing the laminate obtained in step 1 by aligning the laminate to the curved shape of the object to be laminated, while reducing the pressure inside the bag and heating it, without using a mold having a surface corresponding to the curved shape of the object to be laminated.
15. The method for producing a laminate according to claim 14, further comprising the steps of: sandwiching a sheet-like member between the laminate and the bag; and heating the sheet-like member under reduced pressure.
Citation Information
Patent Citations
Manufacture of cellulose triacetate film
JP1999123732A
Manufacturing method for cellulose ester laminated film
JP2003276037A
Production method of coating film, Anti-reflecting film and its production method, polarizing plate using the Anti-reflecting film, and image displaying device using these
JP2006122889A
Thermoplastic resin film and its manufacturing process
JP2007137028A
Hard coat film, polarizing plate and image display
JP2009204725A