Dispersant, dispersion, ink, ink set, and printed matter
The use of a block polymer with specific acid value ratios in water-based inkjet inks addresses the challenges of achieving high printing density and durability on various media, while improving redispersibility and storage stability, effectively solving the trade-off issues in conventional inkjet inks.
Patent Information
- Application Number
- PCT/JP2024/019408
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2024-05-27
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional water-based inkjet inks face challenges in achieving high printing density and durability on various recording media, such as coated and uncoated papers, and film substrates, while also experiencing issues with redispersibility and nozzle clogging due to the trade-off between these properties.
A block polymer with an A block containing styrene and maleic acid units and a B block with vinyl monomer units is used as a dispersant, where the acid value of the A block is greater than that of the B block, enhancing hydrophilicity and adsorption to colorants, thereby improving redispersibility and durability.
The solution enables water-based inkjet inks to achieve high print densities and durability on diverse recording media, reducing nozzle clogging by maintaining excellent redispersibility and storage stability.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Dispersants, dispersions, inks, ink sets, and prints
[0001] FIELD OF THE INVENTION Embodiments of the present invention relate to dispersants, dispersions, inks, ink sets, and printed matter.
[0002] Inkjet printing uses paper and film substrates as recording media. Paper substrates are broadly divided into coated paper, such as art paper and coated paper, and uncoated paper, such as foam paper and wood-free paper. While coated paper has a smooth recording surface due to its coating, uncoated paper's rough surface allows aqueous inkjet ink to easily absorb into the paper's interior and not remain on the surface. This has made it difficult to achieve print density equivalent to that of coated paper. Furthermore, film substrates tend to achieve high print density because aqueous inkjet ink remains on the surface without absorbing it, but the ink is slow to dry, resulting in poor ink layer durability (abrasion resistance, water resistance, and solvent resistance). Therefore, aqueous inkjet inks must be tailored to each recording medium. However, preparing multiple aqueous inkjet inks for inkjet printing poses problems of cost and complicated ink volume management. Therefore, there is a need for aqueous inkjet inks that offer high print density and durability regardless of the type of recording medium.
[0003] Furthermore, a common problem with aqueous inkjet inks is that the ink tends to solidify near the nozzles of the inkjet head, resulting in poor inkjet ejection. This problem can be solved by improving redispersibility. Even if the aqueous inkjet ink dries near the nozzles, the dried ink is redispersed by the aqueous inkjet ink itself that is newly supplied to the nozzles from the head, making it less likely to solidify. To improve redispersibility, it is effective to not only reduce the colorant components contained in the aqueous inkjet ink, but also to increase the hydrophilicity of the dispersion resin that disperses the colorant components. However, there are problems in that reducing the colorant components reduces print density, and increasing the hydrophilicity of the dispersion resin reduces durability.
[0004] As a method for improving print density and redispersibility, Patent Document 1 discloses a dispersion using a block polymer composed of benzyl methacrylate ester in the A block and methacrylic acid / butyl methacrylate ester in the B block as a dispersing resin. Patent Document 2 discloses a dispersion using a comb polymer in which styrene-maleic acid resin is modified with polyalkylene oxide monoamine as a dispersing resin as a method for improving wetting and dispersibility of a colorant and print density. Patent Document 3 discloses a dispersion containing an A block polymer without acid groups and a B block polymer with acid groups, in which the terminals of the A block and B block are modified, as a method for improving inkjet ejection defects.
[0005] International Publication No. 2013 / 115071 Patent Publication No. 2010-514862 Patent Publication No. 2021-127449
[0006] However, because there is a trade-off between redispersibility, durability, and print density, conventional aqueous inkjet inks have not been able to satisfy these requirements at a high level.
[0007] An object of one embodiment of the present invention is to provide a dispersant and dispersion that can be used to produce an aqueous inkjet ink that has good redispersibility and durability and can achieve high print density on coated paper, uncoated paper, and film recording media.Another object of the present invention is to provide an aqueous inkjet ink, ink set, and printed matter that has good redispersibility and durability and can achieve high print density on coated paper, uncoated paper, and film recording media.
[0008] One embodiment of the present invention relates to a dispersant comprising a block polymer having an A block and a B block, wherein the A block comprises styrene units and maleic acid units, and the B block comprises vinyl monomer units, and the acid value of the A block is greater than the acid value of the B block. Another embodiment of the present invention relates to a dispersion comprising the dispersant, a colorant, and water. Another embodiment of the present invention relates to an ink comprising the dispersion. Another embodiment of the present invention relates to an ink set comprising the ink. Yet another embodiment of the present invention relates to a printed matter comprising a substrate and a printed layer formed using the ink or the ink set.
[0009] According to an embodiment of the present invention, a dispersant and dispersion can be provided that can be used to produce an aqueous inkjet ink that has good redispersibility and durability and can achieve high print density on recording media such as coated paper, uncoated paper, and film. Also, according to an embodiment of the present invention, an aqueous inkjet ink, ink set, and printed matter can be provided that have good redispersibility and durability and can achieve high print density on recording media such as coated paper, uncoated paper, and film.
[0010] First, the terms used in this specification will be explained. "C.I." stands for Color Index (C.I.). A monomer (hereinafter also referred to as "monomer") is an ethylenically unsaturated group-containing monomer and is a compound before polymerization. A monomer is a compound before polymerization, and a monomer unit is a partial structure derived from the monomer contained in a polymer obtained by polymerizing the monomer. A dispersant according to an embodiment of the present invention includes a block polymer. In the dispersant, the block polymer functions as a dispersing resin. The dispersing resin is a resin used to disperse a colorant. The molecular weight dispersity is a value obtained by dividing the weight average molecular weight by the number average molecular weight. The weight average molecular weight (Mw) and number average molecular weight (Mn) can be measured by GPC (gel permeation chromatography) and calculated using polystyrene as a standard sample. The weight-average molecular weight (Mw) and number-average molecular weight (Mn) can be measured, for example, using a TSK-GELSUPERHZM-N column (manufactured by Tosoh Corporation) at a column temperature of 40° C. with a GPC (manufactured by Tosoh Corporation, HLC-8320GPC) equipped with an RI detector, using tetrahydrofuran as the developing solvent at a flow rate of 0.35 mL / min. PStQuick (manufactured by Tosoh Corporation) can also be used as a polystyrene standard sample.
[0011] The dispersant includes a block polymer having an A block and a B block. The A block includes styrene units and maleic acid units, and the B block includes vinyl monomer units. The acid value of the A block is greater than the acid value of the B block. The method for synthesizing the block polymer is not limited, and any known block polymerization technique may be used, with living polymerization being preferred. The block polymer is preferably linear.
[0012] The dispersant is preferably used in, for example, inkjet ink, flexographic ink, gravure ink, stationery ink, textile printing ink, and color filter ink, and among these, inkjet ink is more preferred.
[0013] The dispersant contains a block polymer having an A block and a B block, with the A block having a higher acid value than the B block. As a result, the A block functions as a hydrophilic segment that repels the colorant due to charge, and the B block functions as a hydrophobic segment that adsorbs to the colorant. The A block contains styrene units and maleic acid units, while the B block contains vinyl monomer units. The presence of maleic acid units, a dibasic acid, in the A block enhances charge repulsion with colorant particles and improves dispersion stability. Furthermore, some of the carboxyl groups in the maleic acid units crosslink with trace amounts of metal ions contained in the recording medium, making them more likely to remain on the recording medium surface. This allows for high print density and the formation of a durable print layer on uncoated paper. Furthermore, during inkjet printing, solidified matter may form near the nozzles due to the dried aqueous inkjet ink. When new aqueous inkjet ink is supplied from the inkjet head to the nozzles, the dibasic acid of the maleic acid units contained in the new aqueous inkjet ink dissolves and eliminates the solidified matter, resulting in redispersibility.
[0014] <Dispersant> The dispersant includes a block polymer having an A block and a B block. In the block polymer, the A block includes styrene units and maleic acid units, and the B block includes vinyl monomer units, and the acid value of the A block is greater than the acid value of the B block.
[0015] <Block Polymer> The A block may contain a vinyl monomer unit in addition to a styrene unit and a maleic acid unit. A "vinyl monomer unit" is a monomer unit other than a styrene unit or a maleic acid unit.
[0016] The B block may contain styrene units and maleic acid units in addition to vinyl monomer units, which can reduce the viscosity of the colorant dispersion containing the block polymer, thereby improving dispersibility and ejection properties when used in an inkjet ink.
[0017] The molecular weight dispersity of the block polymer is preferably 1.0 or more and 2.0 or less, more preferably 1.0 or more and 1.7 or less. Narrowing the molecular weight dispersity makes it possible to reduce the content of high molecular weight polymers that deteriorate redispersibility and low molecular weight polymers that reduce print density, thereby improving redispersibility and print density. The block polymer may be synthesized by any synthesis method as long as the block polymer can be synthesized, but living polymerization is preferred, and living radical polymerization is more preferred.
[0018] The block polymer according to an embodiment of the present invention functions as a dispersing resin as long as it coexists with a dispersed substance such as a colorant. On the other hand, the block polymer according to an embodiment of the present invention can also function as a binder resin. For example, an ink or the like can be prepared by adding a block polymer that also functions as a binder resin to a colorant dispersion containing the block polymer that functions as a dispersing resin.
[0019] <Styrene Unit> The styrene unit can be formed from the following monomers. Examples include styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o-ethylstyrene, m-ethylstyrene, p-ethylstyrene, o-n-propylstyrene, m-n-propylstyrene, p-n-propylstyrene, o-isopropylstyrene, m-isopropylstyrene, p-isopropylstyrene, m-n-butylstyrene, p-n-butylstyrene, p-t-butylstyrene, 4-butenylstyrene, 2,4-dimethylstyrene, 2,5-dimethylstyrene, 3,5-dimethylstyrene, mesitylstyrene; p-phenylstyrene; o-fluorostyrene, m-fluorostyrene, p-fluorostyrene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, o-bromostyrene, m-bromostyrene, p-bromostyrene, o-methyl-p-fluorostyrene; o-methoxystyrene, m-methoxystyrene, and p-methoxystyrene. Among these, styrene is preferred in terms of polymerizability with maleic anhydride.
[0020] The content of the styrene unit is preferably 1 to 60% by mass, more preferably 5 to 50% by mass, of all the monomer units in the A block. By including an appropriate amount, the adsorption to the colorant is further improved.
[0021] As described above, the B block can also contain styrene units. The content of styrene units in the B block is preferably 0.0 to 30% by mass, more preferably 0.2 to 25% by mass, and even more preferably 1 to 20% by mass, of the total amount of all monomer units in the B block. Inclusion of an appropriate amount improves durability. In this specification, "a content of 0.0% by mass" means that the target component is not contained.
[0022] The block polymer may contain a single styrene unit or a combination of two or more styrene units.
[0023] <Maleic Acid Unit> The maleic acid unit can be obtained by hydrolyzing the acid anhydride group of the maleic anhydride unit formed by copolymerizing maleic anhydride with water to generate a dibasic acid, for example, following the synthesis of a precursor of a block polymer described below or when producing a dispersion using the precursor of the block polymer.
[0024] The content of maleic acid units is preferably 1 to 50% by mass, more preferably 3 to 45% by mass, and even more preferably 5 to 40% by mass, of all monomer units in block A. When an appropriate amount is contained, it imparts excellent dispersibility to the colorant dispersion particles, crosslinks with trace amounts of metal ions contained in uncoated paper, and makes it easier for the ink to remain on the paper surface, thereby achieving high print density.
[0025] The content of maleic acid units in the B block is preferably 0.0 to 30% by mass, more preferably 0.1 to 20% by mass, and even more preferably 0.1 to 10% by mass, of all monomer units in the B block. By including an appropriate amount, water solubility is further improved and redispersibility is improved while maintaining adsorption to the colorant.
[0026] In particular, when the B block has styrene units and maleic acid units, the content (% by mass) of styrene units relative to the total amount of monomer units in the B block is preferably 1 to 80% by mass greater, and particularly preferably 4 to 70% by mass greater, than the content (% by mass) of maleic acid units relative to the total amount of monomer units in the B block. When the content of styrene units in the B block is greater than the content of maleic acid units in the B block, synthesis of the block polymer used as the dispersion resin, particularly synthesis by the RAFT method described below, becomes easier. As a result, the molecular weight dispersity of the block polymer is more likely to fall within the preferred range described above, improving redispersibility and print density.
[0027] Furthermore, the content (% by mass) of maleic acid units in the A block relative to the amount of all monomer units contained in the block polymer is preferably 1 to 25% by mass, and more preferably 2 to 20% by mass, greater than the content (% by mass) of maleic acid units in the B block relative to the amount of all monomer units contained in the block polymer. By including an appropriate amount, the functions of the A block and the B block are more clearly distinguished, resulting in excellent redispersibility and storage stability of the dispersion.
[0028] <Vinyl Monomer Units> Examples of vinyl monomer units include (meth)acrylic acid ester units, (meth)acrylamide units, α-olefin units, maleimide units, N-substituted maleimide units, (meth)allyl monomer units, heterocyclic ring-containing monomer units, reactive functional group-containing monomer units, and other vinyl monomer units. Note that the scope of vinyl monomer units having an allyl group excludes units corresponding to (meth)acrylic acid ester units or (meth)acrylamide units. Furthermore, the scope of (meth)acrylic acid ester units and (meth)acrylamide units excludes units corresponding to vinyl monomer units having a heterocyclic structure. Furthermore, the scope of (meth)acrylic acid ester units, (meth)acrylamide units, and N-substituted maleimide units excludes units corresponding to vinyl monomer units having a reactive functional group (specific examples will be described later).
[0029] <(Meth)acrylic acid ester unit> Examples of the (meth)acrylic acid ester unit include (meth)acrylic acid alkyl ester units such as methyl (meth)acrylic acid ester, ethyl (meth)acrylic acid ester, propyl (meth)acrylic acid ester, iso-propyl (meth)acrylic acid ester, butyl (meth)acrylic acid ester, i-butyl (meth)acrylic acid ester, t-butyl (meth)acrylic acid ester, amyl (meth)acrylic acid ester, i-amyl (meth)acrylic acid ester, 2-ethylhexyl (meth)acrylic acid ester, octyl (meth)acrylic acid ester, i-octyl (meth)acrylic acid ester, decyl (meth)acrylic acid ester, i-decyl (meth)acrylic acid ester, dodecyl (meth)acrylic acid ester, i-dodecyl (meth)acrylic acid ester, stearyl (meth)acrylic acid ester, i-stearyl (meth)acrylic acid ester, and behenyl (meth)acrylic acid ester; aromatic ring (meth)acrylate ester units such as benzyl (meth)acrylate, phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxyethylene glycol (meth)acrylate, phenoxyethylene glycol (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, 2-naphthyl (meth)acrylate, 9-anthracenyl (meth)acrylate, and 1-pyrenylmethyl (meth)acrylate; alicyclic (meth)acrylate units such as cyclopropyl (meth)acrylate, cyclobutyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, cycloheptyl (meth)acrylate, cyclooctyl (meth)acrylate, cyclononyl (meth)acrylate, cyclodecyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, norbornyl (meth)acrylate, and adamantyl (meth)acrylate;(meth)acrylic acid alkoxyalkyl ester units such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; (meth)acrylic acid polyoxyalkylene ester units such as methoxypolyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, ethoxypolyethylene glycol (meth)acrylate, ethoxypolypropylene glycol (meth)acrylate, butoxypolyethylene glycol (meth)acrylate, butoxypolypropylene glycol (meth)acrylate, 2-ethylhexylpolyethylene glycol (meth)acrylate, and 2-ethylhexylpolypropylene glycol (meth)acrylate. In this specification, (meth)acrylic acid aromatic ring ester units and (meth)acrylic acid alicyclic ester units are collectively referred to as "(meth)acrylic acid cyclic ester units.";
[0030] The block polymer may contain a single (meth)acrylic acid ester unit or a combination of two or more types of (meth)acrylic acid ester units.
[0031] From the viewpoints of reactivity with maleic anhydride units, styrene units, and living polymerization agents, and adsorption to colorants, the block polymer preferably contains at least one selected from the group consisting of (meth)acrylic acid alkyl ester units and (meth)acrylic acid cyclic ester units, and more preferably contains (meth)acrylic acid alkyl ester units and (meth)acrylic acid cyclic ester units. By containing (meth)acrylic acid alkyl ester units and (meth)acrylic acid cyclic ester units, adsorption to hydrophobic colorants can be further improved.
[0032] In one embodiment, when the B block contains (meth)acrylic acid alkyl ester units and (meth)acrylic acid cyclic ester units, the content (% by mass) of the (meth)acrylic acid cyclic ester units relative to the amount of all monomer units contained in the B block is preferably 0.5 to 2.5, and particularly preferably 0.8 to 1.5, when the content (% by mass) of the (meth)acrylic acid alkyl ester units relative to the amount of all monomer units contained in the B block is taken as 1. By ensuring that the content of the (meth)acrylic acid cyclic ester units relative to the content of the (meth)acrylic acid alkyl ester units falls within the above range, adsorption to colorants is enhanced, redispersibility is improved, and the durability of printed matter is also improved.
[0033] Furthermore, when the A block contains vinyl monomer units, it is preferable that the A block contains (meth)acrylic acid alkyl ester units and the B block contains (meth)acrylic acid cyclic ester units. A dispersion resin containing such a block polymer exhibits particularly enhanced adsorption to colorants, improving redispersibility and the storage stability of colorant dispersions, as well as excellent durability. Furthermore, it is possible to prepare an aqueous inkjet ink that can produce printed matter with high print density regardless of the recording medium. Furthermore, in this case, when the content (% by mass) of the (meth)acrylic acid alkyl ester units relative to the amount of all monomer units contained in the A block is taken as 1, the content (% by mass) of the (meth)acrylic acid cyclic ester units relative to the amount of all monomer units contained in the B block is preferably 0.5 to 2.5, and particularly preferably 0.7 to 2.0.
[0034] <α-Olefin Unit> The α-olefin unit can be formed from the following monomers. Examples include 1-hexene (6 carbon atoms), 1-heptene (7 carbon atoms), 1-octene (8 carbon atoms), 1-nonene (9 carbon atoms), 1-decene (10 carbon atoms), 1-dodecene (12 carbon atoms), 1-tetradecene (14 carbon atoms), 1-hexadecene (16 carbon atoms), 1-octadecene (18 carbon atoms), 1-eicosene (20 carbon atoms), 1-docosene (22 carbon atoms), 1-tetracosene (24 carbon atoms), 1-octacosene (28 carbon atoms), 1-triacontene (30 carbon atoms), 1-dotriacontene (32 carbon atoms), 1-tetratriacontene (34 carbon atoms), 1-hexatriacontene (36 carbon atoms), and 1-octatriacontene (38 carbon atoms). The α-olefin unit is preferably an α-olefin having 6 to 50 carbon atoms, more preferably 6 to 30 carbon atoms, and even more preferably 6 to 28 carbon atoms.
[0035] The block polymer may contain a single type of α-olefin unit or a combination of two or more types of α-olefin units.
[0036] <(Meth)allyl Monomer Unit> The (meth)allyl monomer unit can be formed from the following monomers. Examples include alkyl (meth)allyl ethers such as methyl (meth)allyl ether and ethyl (meth)allyl ether; ring-containing (meth)allyl ethers such as phenyl (meth)allyl ether and cyclohexyl (meth)allyl ether; and (meth)allyl esters such as (meth)allyl propionate, (meth)allyl hexanoate, and (meth)allyl cyclohexanepropionate. The (meth)allyl monomer preferably has a (poly)alkyleneoxy group. Examples include (poly)alkyleneoxy group-containing (meth)allyl ethers such as polyalkylene glycol (meth)allyl ether, alkyleneoxy glycol (meth)allyl ether, and alkoxypolyalkylene glycol (meth)allyl ether. Among these, from the viewpoint of compatibility with the binder resin, it is preferable to have a (poly)alkyleneoxy group, and alkoxypolyalkylene glycol (meth)allyl ether is more preferable.
[0037] Examples of alkoxy polyalkylene glycol (meth)allyl ethers include methoxyethylene glycol (meth)allyl ether, methoxypolyethylene glycol (meth)allyl ether, methoxypropylene glycol (meth)allyl ether, methoxypolypropylene glycol (meth)allyl ether, ethoxyethylene glycol (meth)allyl ether, ethoxypolyethylene glycol (meth)allyl ether, ethoxypropylene glycol (meth)allyl ether, ethoxypolypropylene glycol (meth)allyl ether, propoxyethylene glycol (meth)allyl ether, propoxypolyethylene glycol (meth)allyl ether, propoxypropylene glycol (meth)allyl ether, propoxypolypropylene glycol (meth)allyl ether, etc. From the viewpoint of compatibility with the binder resin, methoxypolyethylene glycol (meth)allyl ether and methoxypolypropylene glycol (meth)allyl ether are more preferred, and methoxypolypropylene glycol (meth)allyl ether is even more preferred.
[0038] The block polymer may contain a single (meth)allyl monomer unit or a combination of two or more types of (meth)allyl monomer units.
[0039] <Maleimide Unit, N-Substituted Maleimide Unit> By incorporating maleimide units and N-substituted maleimide units (preferably N-substituted maleimide units) into a block polymer, the print density on both uncoated and coated paper can be improved while maintaining the storage stability of the dispersion and the fine dispersibility that enables inkjet ejection. This effect is presumably enhanced by the inclusion of maleimide units and / or N-substituted maleimide units, due to the charge repulsion effect of the two carboxyl groups derived from the maleic acid units and their ability to crosslink with traces of metal ions present in the recording media. By including maleimide units and N-substituted maleimide units in a block polymer that have highly polar imide bonds and hydrophobic properties, the adsorption of various colorants can be significantly improved. This allows the block polymer to exhibit excellent dispersibility for various colorants while promoting the phenomenon of crosslinking with traces of metal ions present in the media and insolubilizing them, thereby allowing the colorant to remain on the media surface during printing, thereby achieving high print density. When an N-substituted maleimide unit is used, the compatibility and adsorption to the colorant can be adjusted by changing the substituent.
[0040] The N-substituted maleimide unit can be formed from the following monomers. Examples include N-methylmaleimide, N-ethylmaleimide, N-laurylmaleimide, N-stearylmaleimide, N-behenylmaleimide, N-cyclohexylmaleimide, N-phenylmaleimide, and N-benzylmaleimide. Among these, cyclohexylmaleimide or N-phenylmaleimide is preferred from the viewpoints of storage stability and compatibility with the binder resin.
[0041] Examples of methods for forming maleimide units include a method in which maleic anhydride units are modified with ammonia, and examples of methods for forming N-substituted maleimide units include the following methods: a method in which N-substituted maleimide monomers are copolymerized, or a method in which maleic anhydride units are modified with an amine compound.
[0042] The block polymer may contain a single N-substituted maleimide unit or a combination of two or more types of N-substituted maleimide units.
[0043] The N-substituted maleimide unit may undergo hydrolysis (ring-opening) to form an amide bond, for example, when a dispersion described below is prepared. In this specification, the structure obtained in this case, i.e., a structure in which a carboxy group and a group having an amide bond are adjacent to each other, formed by ring-opening of an N-substituted maleimide, is also included in the term "N-substituted maleimide unit."
[0044] In one embodiment, the B block preferably contains maleic acid units and N-substituted maleimide. This makes it possible to form an aqueous inkjet ink that is excellent in redispersibility and that can produce printed matter with excellent durability and high print density. In this case, when the content (mass %) of maleic acid units relative to the amount of all monomer units contained in the B block is taken as 1, the content (mass %) of N-substituted maleimide relative to the amount of all monomer units contained in the B block is preferably 5 to 50, and particularly preferably 8 to 35. By setting the content of N-substituted maleimide relative to the content of maleic acid within the above range, it is possible to prepare an aqueous inkjet ink that is excellent in durability and that can produce printed matter with high print density regardless of the recording medium.
[0045] <Heterocyclic Monomer-Containing Unit> The heterocyclic monomer-containing unit can be formed from the following monomers: For example, N-vinyl-2-pyrrolidone, N-vinylcaprolactam, N-vinylpyrimidine, N-vinylpiperidone, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-vinylpiperazine, and (meth)acryloylmorpholine.
[0046] The block polymer may contain a single heterocycle-containing unit or a combination of two or more types.
[0047] <(Meth)acrylamide Unit> The (meth)acrylamide unit can be formed from the following monomers. Examples include methyl(meth)acrylamide, ethyl(meth)acrylamide, propyl(meth)acrylamide, butyl(meth)acrylamide, t-butyl(meth)acrylamide, t-octyl(meth)acrylamide, cyclohexyl(meth)acrylamide, benzyl(meth)acrylamide, methoxymethyl(meth)acrylamide, butoxymethyl(meth)acrylamide, methoxyethyl(meth)acrylamide, phenyl(meth)acrylamide, dimethyl(meth)acrylamide, diethyl(meth)acrylamide, N-(2-acetoacetoxyethyl)(meth)acrylamide, N,N'-methylenebis((meth)acrylamide), and diacetone(meth)acrylamide. Preferred acrylamide units are methyl(meth)acrylamide, ethyl(meth)acrylamide, propyl(meth)acrylamide, butyl(meth)acrylamide, cyclohexyl(meth)acrylamide, benzyl(meth)acrylamide, and diacetone(meth)acrylamide.
[0048] The block polymer may contain a single type of (meth)acrylamide unit or a combination of two or more types of (meth)acrylamide units.
[0049] <Reactive Functional Group-Containing Monomer Unit> Examples of the reactive functional group of the reactive functional group-containing monomer unit include a carboxy group, a hydroxyl group, an amino group, a cyano group, and an epoxy group. The reactive functional group-containing monomer unit can be formed from the following monomers. Examples of the carboxy group-containing monomer include (meth)acrylic acid, crotonic acid, itaconic acid, fumaric acid, isocrotonic acid, salicylic acid, and 4-carboxylphenylmaleimide. The carboxy group-containing monomer unit has the effect of enhancing the charge repulsion effect of the block polymer. Examples of hydroxyl group-containing monomers include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2 (or 3)-hydroxypropyl (meth)acrylate, 2 (or 3 or 4)-hydroxybutyl (meth)acrylate, and cyclohexanedimethanol mono(meth)acrylate, ethyl-α-hydroxymethyl acrylate, hydroxymethyl (meth)acrylamide, 3-hydroxyphenylmaleimide, 4-hydroxyphenylmaleimide, and hydroxyalkyl (meth)allyl ethers such as 2-hydroxyethyl (meth)allyl ether and 4-hydroxybutyl (meth)allyl ether. The hydroxyl group-containing monomer has the effect of increasing the water solubility and redispersibility of the block polymer. Examples of amino group-containing monomers include dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, t-butylaminoethyl (meth)acrylate, methylethylaminoethyl (meth)acrylate, dimethylaminostyrene, diethylaminostyrene, pentamethylpiperidinyl (meth)acrylate, tetramethylpiperidinyl (meth)acrylate, etc. Amino group-containing monomers have the effect of improving the adsorption power to colorants. Examples of cyano group-containing monomers include, but are not limited to, (meth)acrylonitrile, chloro(meth)acrylonitrile, 2-cyanoethyl (meth)acrylic acid ester, and β-cyanoethyl (meth)acrylamide. Among these, acrylonitrile and methacrylonitrile are preferred.Examples of epoxy group-containing monomers include glycidyl (meth)acrylate and 3,4-epoxycyclohexyl (meth)acrylate.
[0050] The block polymer may contain a single reactive functional group-containing monomer unit or a combination of two or more types of reactive functional group-containing monomer units.
[0051] <Other Monomer Units> Examples of other monomers include macromonomers, vinyl acetate, and other monomers not exemplified above.
[0052] Among these, (meth)acrylic acid ester units and / or N-substituted maleimide units are preferred in terms of adsorption to colorants. As mentioned above, among the (meth)acrylic acid ester units, (meth)acrylic acid alkyl ester units and (meth)acrylic acid cyclic ester units are preferred.
[0053] The content of the vinyl monomer units in the A block is preferably 5 to 90% by mass, more preferably 20 to 85% by mass, of all monomer units in the A block. The content of the vinyl monomer units in the B block is preferably 30 to 100% by mass, more preferably 40 to 95% by mass, of all monomer units in the B block. By including an appropriate amount, the polymerization reaction of the block polymer can proceed smoothly. Furthermore, from the viewpoints of reactivity with maleic anhydride units, styrene units, and living polymerization agents, and adsorption to colorants, the block polymer preferably contains at least one unit selected from the group consisting of (meth)acrylic acid ester units and N-substituted maleimide units. Among the (meth)acrylic acid ester units, it is particularly preferred to contain at least one unit selected from the group consisting of (meth)acrylic acid alkyl ester units and (meth)acrylic acid cyclic ester units. Furthermore, it is more preferred to contain both a chain alkyl group-containing (meth)acrylic acid ester unit and a ring-containing (meth)acrylic acid ester unit.
[0054] The block polymer may contain a single vinyl monomer unit or a combination of two or more types of vinyl monomer units.
[0055] The block polymer has an A block having styrene units and maleic acid units and a B block having vinyl monomer units, and the acid value of the A block is greater than the acid value of the B block. The block polymer is preferably a living radical polymer. The block polymer may be a block polymer having two types of blocks, an A block and a B block, and needless to say, the structure may be, for example, AB, BAB, ABA, etc., as long as the problem can be solved.
[0056] The acid value of the A block is greater than that of the B block, so that the A block functions as a hydrophilic segment responsible for dispersibility, and the B block functions as a hydrophobic segment responsible for adsorption to the colorant. The mass ratio of the A block to the B block (A block:B block) is preferably 10:90 to 90:10, more preferably 20:80 to 80:20, and even more preferably 30:70 to 70:30. By achieving an appropriate ratio, excellent colorant adsorption ability and charge repulsion effect can be obtained, resulting in a dispersion with excellent balance of performance.
[0057] The acid value of the A block is preferably 10 to 300 mgKOH / g, more preferably 40 to 200 mgKOH / g, and even more preferably 60 to 150 mgKOH / g. The acid value of the B block is preferably 0 to 100 mgKOH / g, more preferably 1 to 50 mgKOH / g, and even more preferably 1 to 30 mgKOH / g. The acid value of the A block is preferably at least 10 mgKOH / g higher than the acid value of the B block, and more preferably at least 20 mgKOH / g.
[0058] In an embodiment of the present invention, the acid value of each block is calculated by proportionally dividing the acid value of the block polymer according to the number of moles of acid groups contained in each block. For example, in the case of a block polymer consisting of only one A block and one B block, each of which contains 5% by mass of maleic acid units relative to the total monomer units of the block polymer (assuming that no acid groups exist other than the carboxy groups present in the maleic acid units), the acid value of the block polymer is 58 mgKOH / g, so the acid value of the A block is 58 × 5 / (5 + 1) ≈ 48 mgKOH / g, and the acid value of the B block is 58 × 1 / (5 + 1) ≈ 10 mgKOH / g.
[0059] The block polymer is preferably a living radical polymer. Living radical polymers can synthesize polymers with narrower molecular weight distributions than non-living block polymers. In other words, they can suppress low-molecular-weight polymers that reduce the dispersion stability of the colorant while suppressing high-molecular-weight polymers that lead to the generation of coarse particles. The molecular weight dispersity of the block polymer is preferably 1.0 or more and 2.0 or less, more preferably 1.0 or more and 1.7 or less. The block polymer can be obtained, for example, by first synthesizing the A block and then polymerizing the monomers used to synthesize the B block. Furthermore, the monomers used to synthesize the A block may also be polymerized.
[0060] Living radical polymerization methods include, depending on the method for stabilizing the polymer growing end, a method using a sulfur-based reversible chain transfer method (RAFT method), a method using an organotellurium compound (TERP method), a method using a transition metal catalyst (ATRP method), a nitroxide-mediated radical polymerization method (NMP method), etc. Among these, the RAFT method is preferred because it can control the polymerization of not only conjugated monomers but also non-conjugated monomers.
[0061] <Living Polymerization Agent> A living polymerization agent is a compound used in living radical polymerization. Therefore, the living radical polymer may have a polymerization agent residue. Examples of the living polymerization agent include a thiocarbonyl compound, an organic tellurium compound, and an organic ditellurium compound.
[0062] <Reversible Addition-Fragmentation Chain Transfer Polymerization (RAFT)> The RAFT method is a method in which a reversible exchange chain transfer reaction occurs more rapidly than a propagation reaction, allowing all polymers to grow uniformly. A thiocarbonyl compound is an organic sulfur compound used to synthesize living polymers in the RAFT method. Examples of thiocarbonyl compounds include dithiobenzoate, trithiocarbonate, and dithiocarbamate types. Among these, trithiocarbonate types are preferred because styrene and / or methacrylic acid ester-based monomers are used.
[0063] Examples of the dithiobenzoate type include 2-cyanopropan-2-yl dithiobenzoate and 4-cyano-4-[(thiobenzoyl)sulfanyl]pentanoic acid.
[0064] The trithiocarbonate type includes 4-cyano-4-[(dodecylsulfanylthiocarbonyl)sulfanyl]pentanoic acid, 2-cyano-2-[(dodecylsulfanylthiocarbonyl)sulfanyl]propane, S,S-dibenzyltrithiocarbonate, methyl 4-cyano-4-[(dodecylsulfanylthiocarbonyl)sulfanyl]pentanoate, trithiocarbonate=bis[4-(allyloxycarbonyl)benzyl], trithiocarbonate=bis{4-[ethyl-(2-acetyloxy)ethoxy]ethoxy}ethoxy}ethoxy] ... trithiocarbonate=bis{4-[ethyl-(2-hydroxyethyl)carbamoyl]benzyl}, trithiocarbonate=bis{4-(2-hydroxyethoxycarbonyl)benzyl}, 2-{[(dodecylthio)carbonothioyl]thio}propanoic acid, 3-<{[(1-carboxyethyl)thio]carbonothioyl}thio>propanoic acid, 4-<{[(2-carboxyethyl)thio]carbonothioyl}thio>-4-cyanopentanoic acid, and the like.
[0065] Examples of the dithiocarbamate type include 2'-cyanobutan-2'-yl 4-chloro-3,5-dimethylpyrazole-1-carbodithioate, 2'-cyanobutan-2'-yl 3,5-dimethylpyrazole-1-carbodithioate, cyanomethyl 3,5-dimethylpyrazole-1-carbodithioate, and cyanomethyl N-methyl-N-phenyldithiocarbamate.
[0066] <Organotellurium Compound Polymerization (TERP)> The TERP method is a polymerization method in which polymerization is carried out in the presence of an organotellurium compound by thermal dissociation of a bond between a tellurium atom and carbon, followed by degenerative chain transfer. Examples of organotellurium compounds include (methyltellanylmethyl)benzene, (1-methyltellanylethyl)benzene, 1-chloro-4-(1-methyltellanylethyl)benzene, 1-trifluoromethyl-4-(1-methyltellanylethyl)benzene, 3,5-bis-trifluoromethyl-1-(1-methyltellanylethyl)benzene, 1,2,3,4,5-pentafluoro-6-(1-methyltellanylethyl)benzene, 2-methyltellanylpropionitrile, (2-methyltellanylpropyl)benzene, methyl 2-methyltellanyl-2-methylpropionate, ethyl 2-methyltellanyl-2-methylpropionate, and 2-methyltellanyl-2-methylpropionitrile.
[0067] In addition to the organotellurium compound used as the polymerization initiator, an organoditellurium compound may be further added.
[0068] Examples of the organic ditellurium compound include dimethyl ditelluride, diethyl ditelluride, di-n-propyl ditelluride, diisopropyl ditelluride, dicyclopropyl ditelluride, di-n-butyl ditelluride, di-sec-butyl ditelluride, di-tert-butyl telluride, dicyclobutyl telluride, diphenyl ditelluride, bis-(p-methoxyphenyl) ditelluride, bis-(p-aminophenyl) ditelluride, bis-(p-nitrophenyl) ditelluride, bis-(p-cyanophenyl) ditelluride, bis-(p-sulfonylphenyl) ditelluride, dinaphthyl ditelluride, and dipyridyl ditelluride.
[0069] Atom Transfer Radical Polymerization (ATRP) is carried out using a transition metal complex of copper, ruthenium, iron, nickel, or the like as a redox polymerization catalyst. Examples of the transition metal complex include low-valent transition metal halides such as copper(I) chloride and copper(I) bromide.
[0070] Organic ligands are used in transition metal complexes. These ligands are used to enable solubility in polymerization solvents and reversible change of the redox polymerization catalyst. Coordinating atoms of transition metals include nitrogen, oxygen, phosphorus, and sulfur atoms.
[0071] The initiators used in atomic radical polymerization methods are mainly organic halides and sulfonyl halide compounds having highly reactive carbon-halogen bonds. Examples include ethyl bromoisobutyrate, ethyl bromobutyrate, ethyl chloroisobutyrate, ethyl chlorobutyrate, p-toluenesulfonic acid chloride, 1-bromoethylbenzene, and chloroethylbenzene. These can be used alone or in combination.
[0072] <Nitroxide Method (NMP Method)> Nitroxide-mediated living radical polymerization is carried out using a stable nitroxy free radical (=N—O.) as a radical capping agent. Examples of stable nitroxy free radicals include, but are not limited to, 2,2,6,6-tetramethyl-1-piperidinyloxy radical (TEMPO), 2,2,6,6-tetraethyl-1-piperidinyloxy radical, 2,2,6,6-tetramethyl-4-oxo-1-piperidinyloxy radical, 2,2,5,5-tetramethyl-1-pyrrolidinyloxy radical, 1,1,3,3-tetramethyl-2-isoindolinyloxy radical, and N,N-di-t-butylamineoxy radical. Instead of the nitroxy free radical, a stable free radical such as a galvinoxyl free radical may also be used.
[0073] The radical capping agent is used in combination with a radical polymerization initiator. The ratio of the two is not particularly limited, but a suitable ratio is 0.1 to 10 moles of the radical initiator per mole of the radical capping agent.
[0074] Examples of the radical polymerization initiator include dialkyl peroxides such as di-t-butyl peroxide, dicumyl peroxide, t-butylcumyl peroxide, α,α'-bis(t-butylperoxy-m-isopropyl)benzene, and 2,5-di(tert-butylperoxy)hexyne-3; peroxy esters such as t-butyl peroxybenzoate, t-butyl peroxyacetate, and 2,5-dimethyl-2,5-di(benzoylperoxy)hexane; cyclohexanone peroxide, 3,3 ketone peroxides such as 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane, 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, n-butyl-4,4-bis(t-butylperoxy)valerate, and the like; peroxyketals such as cumene hydroperoxide, diisopropylbenzene hydroperoxide, hydroperoxides such as 2,5-dimethylcyclohexane-2,5-dihydroperoxide; diacyl peroxides such as benzoyl peroxide, decanoyl peroxide, lauroyl peroxide, 2,4-dichlorobenzoyl peroxide; peroxydicarbonates such as bis(t-butylcyclohexyl)peroxydicarbonate; and organic peroxide initiators such as 2,2'-azobisisobutyronitrile and 2,2'-azobis(2-methylbutyronitrile). azo initiators such as 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethyl-4-methoxyvaleronitrile), dimethyl 2,2'-azobis(2-methylpropionate), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-hydroxymethylpropionitrile), 2,2'-azobis[2-(2-imidazolin-2-yl)propane], or mixtures thereof.
[0075] The living radical polymer is preferably synthesized by the RAFT method.
[0076] <Method for Synthesizing Block Polymers> Block polymers can be synthesized, for example, by a method including solution polymerization of a monomer mixture. During polymerization, a radical polymerization initiator and a living polymerization agent are added. For example, a monomer mixture containing styrene and maleic anhydride is first polymerized to form a block containing styrene units and maleic anhydride units. Next, a vinyl monomer is polymerized to form a B block, thereby synthesizing a precursor of the block polymer. Thereafter, the maleic anhydride units contained in the precursor of the block polymer are converted to maleic acid units by hydrolyzing the acid anhydride groups, thereby obtaining a block polymer having an A block and a B block. It goes without saying that the structure of the block polymer is not limited to, for example, AB, BAB, ABA, ABAB, etc., and the polymerization order is also not limited, as long as the problem can be solved. The block polymer may have one or more blocks corresponding to the A block and one or more blocks corresponding to the B block. However, when the block polymer has a plurality of blocks corresponding to the A block, the type of monomer unit contained in each A block shall be the same, and the ratio of the content of each monomer unit shall be 0.75 to 1.00. The "ratio of the content of the monomer unit" refers to the ratio (Wa2 / Wa1) of the mass content of the target monomer unit in two A blocks to the total mass of the content of the monomer units (represented as Wa1 (mass%) and Wa2 (mass%), respectively, provided that Wa1 ≧ Wa2). Furthermore, the average degrees of polymerization (average number of monomer units contained in the polymer) of the A blocks may be different, but the ratio of the average degrees of polymerization shall be 0.5 to 1.0. The "ratio of the average degrees of polymerization" refers to the ratio (Da2 / Da1) of the average degrees of polymerization in two A blocks (represented as Da1 and Da2, respectively, provided that Da1 ≧ Da2). In addition, when the block polymer has a plurality of blocks corresponding to the B block, the same applies as in the case of the A block.
[0077] The acid value of a block polymer refers to a theoretical value calculated from the composition and content of the monomers contained in the block polymer (specifically, the molecular weight of each monomer and the number and valence of acid groups present in the structure). It is preferably 10 to 300 mgKOH / g, more preferably 50 to 200 mgKOH / g, and even more preferably 80 to 150 mgKOH / g. By setting the acid value of the block polymer within the above range, the inkjet ink exhibits excellent storage stability and redispersibility, and by more efficiently crosslinking with the small amount of metal ions contained in the recording medium, the printed layer is more likely to remain on the recording medium surface. This allows for high print density, regardless of whether the paper is coated or uncoated, and also allows for the formation of a printed layer with enhanced cohesion and durability. In one embodiment, a block polymer having an acid value of 10 to 100 mgKOH / g can function as a binder resin in addition to its function as a dispersing resin. From the viewpoint of enabling the block polymer to function as a binder resin and producing a printed matter having excellent durability and adhesion, the acid value of the block polymer is preferably 10 to 80 mgKOH / g, and particularly preferably 10 to 60 mgKOH / g.
[0078] Examples of the organic solvent used in the solution polymerization include ethyl acetate, n-butyl acetate, isobutyl acetate, toluene, xylene, acetone, hexane, methyl ethyl ketone, and cyclohexanone.
[0079] The organic solvents can be used alone or in combination of two or more kinds.
[0080] The weight-average molecular weight of the block polymer is preferably 5,000 to 50,000, and more preferably 1,000 to 30,000. Having a suitable weight-average molecular weight improves the adsorption to the colorant, thereby further improving storage stability and redispersibility. Furthermore, in addition to the block polymer's strong adsorption to the colorant, it also promotes binding with the binder resin in the aqueous inkjet ink and crosslinks with traces of metal ions contained in the recording medium, allowing for the formation of a printed layer with higher cohesion and excellent durability.
[0081] The block polymer is preferably used after the organic solvent has been removed after solution polymerization.
[0082] In addition to the block polymer, the dispersant may contain other dispersants such as surfactants and pigment dispersing resins, as necessary. The content of the block polymer in the dispersant may be 50% by mass or more, 80% by mass or more, 95% by mass or more, or 98% by mass or more, based on the amount of the dispersant. The content of the block polymer may be 100% by mass or less.
[0083] <Dispersion> In an embodiment of the present invention, the dispersion contains a dispersant containing a block polymer, a colorant, and water. The dispersion preferably further contains a resin modifier. The block polymer contained in the dispersion may be modified with the resin modifier. The dispersion may also contain a basic compound, a binder resin (excluding the above-mentioned block polymer), and a water-soluble solvent.
[0084] <Colorant> The colorant can be appropriately selected from organic pigments, inorganic pigments, and dyes.
[0085] Examples of organic pigments include azo pigments, diazo pigments, phthalocyanine pigments, quinacridone pigments, isoindolinone pigments, dioxazine pigments, perylene pigments, perinone pigments, thioindigo pigments, anthraquinone pigments, and quinophthalone pigments.
[0086] Red organic pigments include C.I. Pigment Red 1, 2, 3, 4, 5, 6, 7, 9, 10, 14, 17, 22, 23, 31, 32, 38, 41, 48: 1, 48: 2, 48: 3, 48: 4, 49, 49: 1, 49: 2, 52: 1, 52: 2, 53: 1, 57: 1, 60: 1, 63: 1, 66, 67, 81: 1, 81: 2, 81: 3, 83, 88, 90, 105, 112, 119, 122, 123, 144, 146, 147, 148, 149, 150, 155, 166, 168, 169, 170, 171, 172, 175, 176, 177, 178, 179, 184, 185, 187, 188, 190, 200, 202, 206, 207, 208, 209, 210, 216, 220, 224, 226, 242, 246, 254, 255, 264, 266, 269, 270, 272, 279, etc.
[0087] Examples of yellow organic pigments include C.I. Pigment Yellow 1, 2, 3, 4, 5, 6, 10, 11, 12, 13, 14, 15, 16, 17, 18, 20, 24, 31, 32, 34, 35, 35: 1, 36, 36: 1, 37, 37: 1, 40, 42, 43, 53, 55, 60, 61, 62, 63, 65, 73, 74, 77, 81, 83, 86, 93, 94, 95, 97, 98, 100, 101, 104, 106, 108, 109, 110, 113, 114, 115, 116, 11 7, 118, 119, 120, 123, 125, 126, 127, 128, 129, 137, 138, 139, 147, 148, 150, 151, 152, 153, 154, 155, 156, 161, 162, 164, 166, 167, 168, 169, 170, 171, 172, 173, 174, 175, 176, 177, 179, 180, 181, 182, 185, 187, 188, 193, 194, 199, 213, 214, etc.
[0088] Examples of blue organic pigments include C.I. Pigment Blue 1, 2, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 22, 60, 64, 66, 79, 79, and 80.
[0089] Organic pigments other than red, yellow, and blue include C.I. Pigment Orange 2, 5, 13, 16, 17: 1, 31, 34, 36, 38, 43, 46, 48, 49, 51, 52, 55, 59, 60, 61, 62, 64, 71, 73, C.I. Pigment Green 7, 10, 36, 37, 58, 59, 62, 63, C.I. Pigment Violet 1, 19, 23, 27, 32, 37, 42 C.I. Pigment Brown 25, 28 C.I. Pigment Black 1 C.I. Pigment White 1, 2, 4, 5, 7, 11, 12, 18, 19, 21, 22, 23, 26, 27, 28, etc.
[0090] Among these, C.I. Pigment Red 31, 48:1, 48:2, 48:3, 48:4, 57:1, 122, 146, 147, 148, 150, 170, 176, 177, 184, 185, 202, 242, 254, 255, 264, 266, 269, C.I. Pigment Yellow 12, 13, 14, 17, 74, 83, 108, 109, 120, 150, 151, 154, 155, 180, 185, 213 C.I. Pigment Orange 34, 36, 38, 43, 64, 73 C.I. C.I. Pigment Green 7, 36, 37, 58, 62, 63, C.I. Pigment Blue 15:1, 15:3, 15:6, 16, 22, 60, 66, C.I. Pigment Violet 19, 23, 32, C.I. Pigment Brown 25, and C.I. Pigment Black 1 are preferred.
[0091] Other inorganic pigments include carbon black, carbon nanotubes, metal oxides, metal complexes, and other inorganic pigments. Examples of carbon black include furnace black, thermal lamp black, acetylene black, and channel black. Examples of metal oxides include titanium oxide, iron oxide, iron hydroxide, zirconia, and alumina. Examples of other inorganic pigments include ultramarine, yellow lead, zinc sulfide, and cobalt blue.
[0092] Carbon black has an average primary particle diameter of 11 to 50 nm and a specific surface area of 50 to 400 m2 by the BET method. 2It is preferable that the carbon black has properties such as a saturation of 10000 / g and a pH of 2 to 10. The above properties improve the adsorption of the block polymer, enabling finer dispersion and producing a dispersion with high print density. Commercially available carbon black products include Nos. 25, 30, 33, 40, 44, 45, 52, 850, 900, 950, 960, 970, 980, 1000, 2200B, 2300, 2350, 2600; MA7, MA8, MA77, MA100, MA230 (manufactured by Mitsubishi Chemical Corporation); RAVEN 760UP, 780UP, 860UP, 900P, 1000P, 1060UP, 1080UP, 1255 (manufactured by Birla Carbon Corporation); Examples of suitable carbon black include EGAL 330R, 400R, 660R, and MOGULL (manufactured by Cabot Corporation), Nipex 160IQ, 170IQ, 35, and 75; PrinteX 30, 35, 40, 45, 55, 75, 80, 85, 90, 95, and 300; Special Black 350 and 550; and Nerox 305, 500, 505, 600, and 605 (manufactured by Orion Engineered Carbons).
[0093] Titanium oxide may have an anatase or rutile crystal structure. Among these, the rutile type is preferred in terms of improving the hiding power of printed matter. Titanium oxide can be synthesized by the chlorine method, sulfuric acid method, etc., but the chlorine method is preferred in terms of improving whiteness.
[0094] It is preferable to suppress the activity of titanium oxide by treating the surface with an inorganic compound. After the inorganic compound treatment, it is preferable to further treat the surface with an organic compound. This improves the dispersion stability of titanium oxide. Examples of inorganic compounds include compounds of silicon, aluminum, zirconium, tin, antimony, and titanium, as well as hydrated oxides thereof. Examples of organic compounds include polyhydric alcohols, alkanolamines and derivatives thereof, higher fatty acids and metal salts thereof, and organometallic compounds.
[0095] The dye is preferably a disperse dye. The disperse dye is a dye that has the property of sublimating when heated. Examples of disperse dyes include C.I. Disperse Yellow 3, 7, 8, 23, 39, 51, 54, 60, 71, 86; C.I. Disperse Orange 1, 1:1, 5, 20, 25, 25:1, 33, 56, 76; C.I. Disperse Brown 2; C.I. Disperse Red 11, 50, 53, 55, 55:1, 59, 60, 65, 70, 75, 93, 146, 158, 190, 190:1, 207, 239, 240, 343; C.I. Vat Red 41; C.I. Disperse Violet 8, 17, 23, 27, 28, 29, 36, 57; C.I. Disperse Blue 19, 26, 26:1, 35, 55, 56, 58, 60, 64, 64:1, 72, 72:1, 81, 81:1, 91, 95, 108, 131, 141, 145, 165, 359, 360, and the like.
[0096] The colorants can be used alone or in combination of two or more.
[0097] The average primary particle diameter of the colorant is preferably 5 to 300 nm. The average primary particle diameter is the arithmetic mean value of approximately 20 particles randomly selected from an image magnified by a transmission electron microscope at a magnification of 2,000 to 100,000 times. When the particles are elliptical, the length of the longitudinal axis is used.
[0098] The content of the colorant in the dispersion is preferably 1 to 50% by mass, more preferably 5 to 30% by mass. By keeping the content of the colorant within the above range, storage stability is improved and vivid colors can be obtained.
[0099] <Resin Modifier> The block polymer may be modified with a resin modifier. In this case, the dispersant includes a polymer obtained by modifying the block polymer with the resin modifier. When the resin modifier is a crosslinking agent described below, the polymer obtained by modification has a structure derived from the block polymer and a partial structure derived from the crosslinking agent. The polymer obtained by modification using a crosslinking agent may have a network structure. The block polymer can be modified with a resin modifier before mixing the block polymer with a colorant. Alternatively, the block polymer can be modified with a resin modifier by adding the resin modifier to a dispersion containing the block polymer and the colorant after obtaining the dispersion. In particular, from the viewpoint of enhancing the redispersibility of the colorant, a method of modifying the block polymer by adding the resin modifier to the dispersion after obtaining the dispersion containing the block polymer and the colorant is preferably selected. The resin modifier is a compound having a functional group (reactive functional group) capable of reacting with the functional group of the block polymer before modification. The polarity of the block polymer can be changed by modifying the block polymer with a resin modifier. The block polymer modified with a resin modifier preferably has a bonding site formed by the reaction of the resin modifier with a maleic acid unit. The bonding site may be a bond formed by the reaction of a carboxy group of the block polymer before modification with a reactive functional group of the resin modifier. Examples of bonding sites include a hydroxyethoxycarbonyl structure formed by the reaction of a carboxy group with an epoxy group, a (hydroxymethyl)ethoxycarbonyl structure formed by the reaction of a carboxy group with an oxetanyl group, and an amide structure (amide bond) formed by the reaction of a carboxy group with an amino group.
[0100] Examples of the resin modifier include compounds having an epoxy group, an oxetanyl group, an isocyanate group, ammonia, an amino group, a quaternary ammonium salt, a thiol group, an aziridinyl group, a carbodiimide group, or an oxazoline group, etc. Among these, epoxy group-containing compounds are preferred.
[0101] The number of reactive functional groups contained in the resin modifier molecule is preferably one or more, and more preferably two or more. When the resin modifier has one reactive functional group, this compound functions as an end-capping agent. For example, by reacting the carboxyl group of the block polymer before modification with an end-capping agent having a hydrophobic group such as an alkyl group or an aromatic group and one epoxy group, the number of moles of carboxyl groups decreases while simultaneously introducing a hydrophobic group such as an alkyl group or an aromatic group, thereby modifying the block polymer to be hydrophobic. Similarly, by reacting a hydrophilic group with an end-capping agent having one epoxy group, the block polymer can be modified to be hydrophilic. When the resin modifier has two or more reactive functional groups, it functions as a cross-linking agent. For example, the carboxyl group of the block polymer reacts with the cross-linking agent to form a strong three-dimensional structure. A cross-linking agent is preferred as the resin modifier. The block polymer is strongly adsorbed to the colorant by cross-linking, improving storage stability. The weight average molecular weight or formula weight of the resin modifier is preferably 100 to 2,000, more preferably 120 to 1,500, and even more preferably 150 to 1,000.
[0102] The crosslinking agent preferably has a suitable water solubility so that it can react efficiently with the carboxyl groups of the block polymer in water, and the amount of the crosslinking agent dissolved in 100 g of water at 25°C is preferably 0.1 to 50 g, more preferably 0.2 to 40 g, and even more preferably 0.5 to 30 g.
[0103] The amount of resin modifier added is preferably 0.1 to 3.0 equivalents, more preferably 0.4 to 1.5 equivalents, of the functional groups in the resin modifier relative to the number of moles of carboxyl groups in the block polymer before modification. By setting the amount of resin modifier added within this range, the block polymer can have an appropriate number of bonding sites, which can improve redispersibility and durability.
[0104] Examples of resin modifiers having one reactive functional group include compounds having an epoxy group such as trimethylolpropane monoglycidyl ether, 2-ethylhexyl glycidyl ether, p-tert-butylphenyl glycidyl ether, lauryl alcohol (EO) 15 glycidyl ether, phenyl glycidyl ether, phenol (EO) 5 glycidyl ether, dibromophenyl glycidyl ether, C12-C13 mixed alcohol glycidyl ether, and N-glycidylphthalimide; compounds having an oxetanyl group such as 4,4'-(3-ethyloxetan-3-ylmethyloxymethyl)biphenyl (abbreviated as OXBP, hereinafter the same) and 3-ethyl-3-hydroxymethyloxetane (EHO); compounds having an amino group or a quaternary ammonium salt such as butane-1,4-bisammonium chloride; and compounds having a thiol group such as methanethiol, ethanethiol, and thiophenol. Examples of resin modifiers having two or more reactive functional groups include compounds having an epoxy group, such as polyglycidyl ethers such as ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, glycerin triglycidyl ether, glycerol polyglycidyl ether, polyglycerol polyglycidyl ether, trimethylolpropane diglycidyl ether, trimethylolpropane triglycidyl ether, trimethylolpropane polyglycidyl ether, sorbitol polyglycidyl ether, pentaerythritol polyglycidyl ether, resorcinol diglycidyl ether, neopentyl glycol diglycidyl ether, diglycidyl orthophthalate, and hydrogenated bisphenol A diglycidyl ether; 1,4-bis[{(3-ethyl-3-oxetanyl)methoxy}methyl]benzene (XDO), di[1-ethyl(3-oxetanyl)]methyl ether (DOX), di[1-ethyl(3-oxetanyl)]methyl ether (DOE), 1,6-bis[(3-ethyl-3-oxetanyl)methoxy]hexane (HDB), 9,9-bis[2-methyl-4-{2-(3-oxetanyl)}butoxyphenyl]fluorene, 9,compounds having an oxetanyl group, such as 9-bis[4-[2-{2-(3-oxetanyl)}butoxy]ethoxyphenyl]fluorene; organic polyisocyanates or isocyanate group-terminated prepolymers, including compounds having a (blocked) isocyanate group, such as aliphatic diisocyanates, such as hexamethylene diisocyanate and 2,2,4-trimethylhexamethylene diisocyanate; aromatic diisocyanates, such as tolylene-2,4-diisocyanate and phenylene diisocyanate; alicyclic diisocyanates; and aromatic triisocyanates, or urethane-modified products thereof; diamines, such as hydrazides, carbodihydrazides, thiocarbohydrazides, and oxalyl dihydrazides; Ethylenediamine, 1,3-propanediamine, 1,2-propanediamine, 1,4-butanediamine, 1,6-hexamethylenediamine, 1,8-octamethylenediamine, 1,11-diaminoundecane, 1,12-diaminododecane, 2-butyl-2-ethyl-1,5-pentanediamine, 1,5-diamino-2-methylpentane, 2,2-dimethyl-1,3-propanediamine, 2,4,4-trimethyl-1,6-diaminohexane, laurylpropylenediamine, ethylene glycol bis(2-aminoethyl)ether, 1,4-butanediol bis(3-aminopropyl)ether, 1,13-diamino-4,7,10-trioxatridecane, polyoxypropylenediamine, methane triamine, 1,2,3-propanetriamine, 1,8-diamino-4-aminomethyloctane, 3-(2-aminoethyl)pentane-1,5-diamine, 1,4,7-triaminocyclononane-1,4,7-triide, butane-1,1,4,4-tetraamine, 2,4-dimethyl-4-ethylamino-2,3,5-triaminohexane, 2,3-bis(diaminomethyl)butane-1,1,4,4-tetraamine, 1,2-bis(methylamino)ethane, 2,5-diamino-2,5-dimethylhexane, butane-1,1,4-trimethylamine, butane-1,1,4,4-tetramethylamine, 1,2-bis(dimethylamino)ethane, butane-1,1,4-tridimethylamine, butane-1,1,4,alkylenediamines such as 4-tetradimethylamine, hexamethylenetetramine, diethylenetriamine, dipropylenetriamine, bishexamethylenetriamine, triethylenetetraamine, adipic acid dihydrazide, succinic acid dihydrazide, sebacic acid dihydrazide, eicosanedioic acid dihydrazide, valine dihydrazide, tetraethylenepentamine, 3,3'-diamino-N-methyldipropylamine, tris(2-aminoethyl)amine, tris(4-aminoethyl)amine, 3,3'-diamino-N-methyldipropylamine, tris(2-aminoethyl)amine, tris(4-aminoethyl)amine, 1-methylamino-2-dimethylaminoethane, linear polyethyleneimine, and branched polyethyleneimine; alicyclic diamines such as 1,2-cyclohexanediamine, 1,4-cyclohexanediamine, isophoronediamine, 1,3-bis(aminomethyl)cyclohexane, 3(4),8(9)-bis(aminomethyl)tricyclo[5.2.1.02,6]decane (TCD diamine), isopropyl-2,4-diaminocyclohexane, isopropyl-2,6-diaminocyclohexane, 4,4'-methylenebis(cyclohexylamine), 4,4'-methylenebis(2-methylcyclohexylamine), adamantane-1,3-diamine, cyclohexane-1,3,5-triamine, 2,3,5-triaminobicyclo[2.2.1]heptane, piperazine, 2,5-dimethylpiperazine, and N-cyclohexyl-1,3-propanediamine; Aromatic ring diamines such as o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 2,4-toluenediamine, 2,6-toluenediamine, 2,2'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylether, 3,3'-diaminodiphenylsulfone, xylylenediamine, tris(4-aminophenyl)methane, 1,2,4-benzenetriamine, melamine, benzene-1,2,4,5-tetraamine, pyrimidine-2,4,5,6-tetraamine, 3,3'-diaminobenzidine, tetraaminophthalocyanine, and isophthalic acid dihydrazide;Compounds having an aziridinyl group, such as 4-bis(1-aziridinecarboxite), bisisophthaloyl-1-(2-methylaziridine), tri-1-aziridinylphosphine oxide, N,N'-hexamethylene-1,6-bis(1-aziridinecarboxite), 2,2'-bishydroxymethylbutanol-tris[3-(1-aziridinyl)propionate], trimethylolpropane tri-β-aziridinylpropionate, tetramethylolmethane tri-β-aziridinylpropionate, tris-2,4,6-(1-aziridinyl)-1,3,5-triazine, and 4,4'-bis(ethyleneiminocarbonylamino)diphenylmethane; compounds having a carbodiimide group, such as high molecular weight polycarbodiimides produced by decarboxylation condensation reaction of diisocyanate compounds in the presence of a carbodiimidization catalyst; Examples of such compounds include compounds in which two or more, preferably two to three, oxazoline groups are bonded to an aliphatic or aromatic group; bisoxazoline compounds such as 2,2-bis(2-oxazoline), 1,3-phenylenebisoxazoline, and 1,3-benzobisoxazoline; and compounds having an oxazoline group, such as terminal oxazoline group-containing compounds obtained by reacting such compounds with polybasic carboxylic acids.
[0105] Among these, compounds having an epoxy group are preferred, and examples thereof include trimethylolpropane monoglycidyl ether, 2-ethylhexyl glycidyl ether, p-tert-butylphenyl glycidyl ether, lauryl alcohol (EO)15 glycidyl ether, phenyl glycidyl ether, phenol (EO)5 glycidyl ether, dibromophenyl glycidyl ether, C12-C13 mixed alcohol glycidyl ether, N-glycidyl phthalimide, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, trimethylolpropane diglycidyl ether, trimethylolpropane triglycidyl ether, trimethylolpropane polyglycidyl ether, glycerol polyglycidyl ether, and the like. Preferred are trimethylolpropane monoglycidyl ether, trimethylolpropane diglycidyl ether, trimethylolpropane triglycidyl ether, ethylene glycol diglycidyl ether, and polyethylene glycol diglycidyl ether, and even more preferred are trimethylolpropane monoglycidyl ether, trimethylolpropane diglycidyl ether, and trimethylolpropane triglycidyl ether. From the viewpoint of treatment efficiency, it is preferable that the resin modifier is moderately soluble in water. Commercially available products include Denacol EX321, EX321L, EX810, EX811, EX850, and EX850L manufactured by Nagase ChemteX Corporation, and Adeka Glysilol ED-505 manufactured by ADEKA Corporation.
[0106] The resin modifiers can be used alone or in combination of two or more.
[0107] <Basic Compound> The basic compound neutralizes the carboxyl group of the maleic acid unit, thereby contributing to the dispersion stability of the colorant particles. Examples of the basic compound include organic amines such as ammonia, dimethylaminoethanol, diethanolamine, and triethanolamine; inorganic alkalis such as alkali metal hydroxides such as sodium hydroxide, lithium hydroxide, and potassium hydroxide; organic acids; and mineral acids.
[0108] From the viewpoint of dispersion stability of the dispersion, the basic compound used for neutralizing the block polymer is preferably used in an amount of 10 to 200 mol %, more preferably 40 to 160 mol %, and still more preferably 70 to 130 mol %, relative to 100 mol % of carboxy groups contained in the block polymer.
[0109] The basic compounds can be used alone or in combination of two or more.
[0110] <Binder Resin> The addition of a binder resin can improve adhesion to recording media, as well as durability and color development, such as abrasion resistance, water resistance, and solvent resistance, of printed matter. Examples of binder resins include (meth)acrylic resins, styrene-(meth)acrylic resins, polyurethane resins, styrene-butadiene resins, vinyl chloride resins, polyolefin resins, polyester resins, polyurethane resins, alkyd resins, fluororesins, and silicone-containing resins. Block polymers can also be used as binder resins, and the use of block polymers having the above-mentioned acid values in particular makes it easy to obtain printed matter with excellent adhesion, durability, and color development, without adding binder resins other than the block polymer.
[0111] <Water-Soluble Solvent> The water-soluble solvent wets the colorant and the water-soluble inorganic salt. The water-soluble solvent is a compound that dissolves (is miscible) in water but does not dissolve the water-soluble inorganic salt. Examples of the water-soluble solvent include glycols such as ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, polyethylene glycol, and polypropylene glycol; diols such as butanediol, pentanediol, and hexanediol; glycol esters such as propylene glycol laurate; ethers such as diethylene glycol monoethyl, diethylene glycol monobutyl, and diethylene glycol monohexyl; glycol ethers such as cellosolves containing propylene glycol ether, dipropylene glycol ether, and triethylene glycol ether; alcohols such as methanol, ethanol, isopropyl alcohol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, butyl alcohol, and pentyl alcohol; sulfolane; lactones such as γ-butyrolactone; lactams such as N-(2-hydroxyethyl)pyrrolidone; and glycerin. Among these, glycols such as diethylene glycol and triethylene glycol are preferred.
[0112] The water-soluble solvents may be used alone or in combination of two or more kinds.
[0113] The nonvolatile content of the dispersion is preferably adjusted with water to about 5 to 80% by mass.
[0114] The D50 average particle size (median diameter) of the colorant is preferably 20 to 200 nm, more preferably 25 to 150 nm, even more preferably 30 to 130 nm, and particularly preferably 35 to 90 nm. For example, when used in inkjet inks, a colorant with an appropriate particle size improves ejection stability from a nozzle and further improves the storage stability of the dispersion. The D50 average particle size is measured using a dynamic light scattering method (e.g., Microtrac UPAEX-150 manufactured by Microtrac Bell).
[0115] <Method for Producing Dispersion> The method for producing the dispersion is, for example, to first add a colorant to a mixture obtained by stirring and mixing a block polymer, an optional basic compound, and water, and then mix and stir the mixture, followed by a dispersion treatment. Next, a centrifugation treatment is performed as necessary to obtain a dispersion. The timing for blending each material is arbitrary, and it goes without saying that the dispersion treatment can be performed multiple times.
[0116] The following dispersing devices can be used for the dispersion treatment. Examples of dispersing devices include high-speed mixers, homogenizers, high-pressure homogenizers, Silverson mixers, planetary mixers, trimixes, kneaders, extruders, horizontal sand mills, vertical sand mills, ball mills, two-roll mills, three-roll mills, bead mills, Nanomizers, dispersers equipped with ultrasonic oscillators, high-pressure dispersers, counter-impingement type dispersers, oblique collision type dispersers, batch type rotor stators, and in-line type rotor stators. Among these, bead mills are preferred. Examples of commercially available bead mills include super mills, sand grinders, agitator mills, grain mills, Dyno Mills, pearl mills, and Cobol Mills.
[0117] The colorant is preferably subjected to a micronization treatment before being dispersed. This allows the primary particle size of the colorant to be further refined, resulting in a dispersion with a finer volume average particle size D50 (median diameter) of colorant particles. The micronization treatment is preferably a method in which the colorant is coated with a block polymer by a salt milling method to refine the colorant. The salt milling method involves, for example, kneading a water-soluble solvent, a water-soluble inorganic salt (e.g., sodium chloride), a colorant, and a block polymer to coat the surface of the colorant with the block polymer, followed by removing the water-soluble inorganic salt and the water-soluble solvent. Examples of kneading devices used in the salt milling method include a kneader, a two-roll mill, a three-roll mill, a ball mill, an attritor, a horizontal sand mill, a vertical sand mill, and / or an annular bead mill. Among these, a kneader is preferred in terms of its ability to efficiently coat the surface of the colorant. The kneading conditions can be adjusted appropriately depending on the type of colorant, the degree of micronization, and the like. Heating or cooling can also be performed as needed.
[0118] <Ink> In an embodiment of the present invention, the ink contains a dispersion. Uses of the ink include relief printing ink used in letterpress printing, flexographic printing, etc., intaglio printing ink used in gravure printing, etc., lithographic printing ink used in offset printing, etc., stencil printing ink used in screen printing, textile printing, etc., inkjet printing, and on-demand printing ink used in electrostatic charge developing toner printing. Among these, inkjet ink used in inkjet printing is preferred. Note that uses of the dispersion other than ink include, for example, paints for building materials and automobiles, color filters, solid-state imaging devices, sensors such as LiDAR, etc.
[0119] <Ink Manufacturing Method> A method for manufacturing an ink according to an embodiment of the present invention will be described. Note that the manufacturing method is not limited to the following. The ink is manufactured by adding a dispersion, and, if necessary, a water-soluble organic solvent, water, a binder resin, a surfactant, and other additives, followed by stirring and mixing. During manufacturing, the ink may be stirred and mixed while being heated to a temperature of 40 to 100°C, if necessary.
[0120] (Removal of Coarse Particles) Coarse particles contained in the ink are preferably removed by means of filtration, centrifugation, or the like. The filtration method preferably involves suction filtering the ink using a membrane filter to separate the coarse particles. The filter pore size is not particularly limited as long as it can remove coarse particles and dust, but in the case of inkjet ink, it is preferably 0.3 to 5 μm, and more preferably 0.5 to 3 μm.
[0121] Inkjet ink In an embodiment of the present invention, the inkjet ink preferably contains a water-soluble solvent (other than water) in addition to the dispersion. The inkjet ink uses water as a solvent (medium), but it is preferable to use a water-soluble solvent in combination to prevent the ink from drying. The water-soluble solvent has a lower surface tension than water, and therefore improves the penetration and wetting / spreading properties of the ink into the substrate after printing.
[0122] Examples of the water-soluble solvent include polyhydric alcohols, polyhydric alcohol alkyl ethers, polyhydric alcohol aryl ethers, nitrogen-containing heterocyclic compounds, amides, amines, sulfur-containing compounds, propylene carbonate, ethylene carbonate, and other water-soluble solvents.
[0123] Examples of polyhydric alcohols include glycerin, ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, 1,2-propanediol, 1,3-propanediol, dipropylene glycol, tripropylene glycol, polypropylene glycol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,2-pentanediol, 1,3-pentanediol, 1,4-pentanediol, 1,5-pentanediol, 1,2-hexanediol, 1,3-hexanediol, 1,4-hexanediol, 1,5-hexanediol, and 1,6 -hexanediol, 3-methyl-1,3-butanediol, trimethylolethane, trimethylolpropane, 1,2,6-hexanetriol, 1,2,4-butanetriol, 1,2,3-butanetriol, petriol, 2-ethyl-2-methyl-1,3-propanediol, 3,3-dimethyl-1,2-butanediol, 2,2-diethyl-1,3-propanediol, 2-methyl-2-propyl-1,3-propanediol, 2,4-dimethyl-2,4-pentanediol, 2,5-dimethyl-2,5-hexanediol, 5-hexene-1,2-diol, 2-ethyl-1,3-hexanediol, and the like. Among these, 2-ethyl-1,3-hexanediol, 2,2,4-trimethyl-1,3-pentanediol, 1,2-propanediol, 1,2-butanediol, 1,3-butanediol, 1,2-pentanediol, 1,5-pentanediol, 1,2-hexanediol, 1,6-hexanediol, and 1,2-heptanediol are preferred.
[0124] Examples of polyhydric alcohol alkyl ethers include ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, tetraethylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monobutyl ether, etc. Examples of polyhydric alcohol aryl ethers include ethylene glycol monophenyl ether, diethylene glycol monophenyl ether, tetraethylene glycol chlorophenyl ether, ethylene glycol monobenzyl ether, ethylene glycol monoallyl ether, etc.
[0125] Examples of nitrogen-containing heterocyclic compounds include 2-pyrrolidone, N-methyl-2-pyrrolidone, N-hydroxyethyl-2-pyrrolidone, 1,3-dimethylimidazolidinone, ε-caprolactam, γ-butyrolactone, etc. Examples of amides include formamide, N-methylformamide, N,N-dimethylformamide, etc. Examples of amines include monoethanolamine, diethanolamine, triethanolamine, monoethylamine, diethylamine, triethylamine, etc. Examples of sulfur-containing compounds include dimethyl sulfoxide, sulfolane, thiodiethanol, etc.
[0126] The water-soluble solvents may be used alone or in combination of two or more kinds.
[0127] The content of the water-soluble solvent in the inkjet ink is preferably 3 to 60% by mass, more preferably 3 to 50% by mass. The content of water in the inkjet ink is preferably 10 to 90% by mass, more preferably 30 to 80% by mass. The inclusion of an appropriate amount of water-soluble solvent improves the ink ejection stability from the head.
[0128] The inkjet ink preferably contains a binder resin. This improves the water resistance, solvent resistance, abrasion resistance, gloss, etc. of the printed layer. Examples of binder resins include (meth)acrylic resins, styrene-(meth)acrylic resins, polyurethane resins, styrene-butadiene resins, vinyl chloride resins, polyolefin resins, polyester resins, polyurethane resins, alkyd resins, fluororesins, and silicone-containing resins. Block polymers can also be used as binder resins.
[0129] The content of the binder resin is preferably from 1 to 30% by mass, and more preferably from 2 to 20% by mass, of the non-volatile content of the inkjet ink.
[0130] The binder resins can be used alone or in combination of two or more.
[0131] The inkjet ink may contain additives as needed. Examples of additives include surfactants, antifoaming agents, waxes, moisturizing agents, and preservatives. The total content of the additives in the inkjet ink is preferably 0.05 to 10% by mass, and more preferably 0.2 to 5% by mass.
[0132] In particular, when the inkjet ink contains a surfactant, it is preferable that the inkjet ink contains a surfactant having an HLB (Hydrophile-Lipophile Balance) value calculated by the Griffin method of 2 to 8.5, because using the surfactant in combination with a dispersion containing a block polymer can provide printed matter with excellent print density, durability, print quality, etc. Furthermore, it is preferable to use an acetylene diol surfactant as the surfactant having an HLB value calculated by the Griffin method of 2 to 8.5, because these effects are particularly well exhibited.
[0133] Furthermore, in terms of obtaining a printed matter with excellent redispersibility and high print density, when the content (% by mass) of the block polymer in the total amount of the inkjet ink is taken as 1, the content (% by mass) of the surfactant having an HLB value of 2 to 8.5, as calculated by the Griffin method, in the total amount of the inkjet ink is preferably 0.02 to 0.9, and particularly preferably 0.05 to 0.75.
[0134] Wax is a resin that is solid at room temperature (25° C.) and melts (i.e., has a melting point) at a temperature between 40 and 200° C. In an embodiment of the present invention, wax is not included in the binder resin.
[0135] Generally, wax has low affinity for water and tends to be concentrated at the gas-liquid interface, so even after the print is made, it remains in a form that covers the surface, thereby significantly improving the blocking suppression of the print.
[0136] The melting point of the wax is preferably from 80 to 180°C, more preferably from 100 to 160°C, in order not to adversely affect the storage stability of the inkjet ink and to ensure good redispersibility.
[0137] The wax exists in the inkjet ink in a dissolved state (water-soluble resin) or a dispersed state (resin microparticles). The latter is particularly preferred because it is easy to prevent blocking of printed matter, is less likely to interact with the block polymer, and is less likely to deteriorate the storage stability of the inkjet ink. Furthermore, it is capable of sealing voids on the paper surface, thereby significantly improving print density in printed matter on uncoated paper. In the embodiments of the present invention, the term "water-soluble resin" refers to a resin in which a 1% by weight aqueous solution of the target resin is transparent to the naked eye at 25°C. Furthermore, the term "resin microparticles" refers to a resin other than a water-soluble resin, having a D50 average particle size of 5 to 1,000 nm, as measured using the same apparatus and method as for the colorant described above.
[0138] When resin fine particles are used as the wax, the D50 average particle size is preferably 10 to 200 nm, more preferably 20 to 150 nm, and even more preferably 30 to 100 nm, from the viewpoints of ensuring the storage stability of the inkjet ink, improving the print density of the printed matter, and preventing blocking.
[0139] The wax is preferably paraffin wax, microcrystalline wax, carnauba wax, polyethylene wax, or polypropylene wax. Among these, paraffin wax, polyethylene wax, and polypropylene wax are more preferred because they have a relatively high melting point, do not deteriorate the storage stability of the inkjet ink, do not inhibit the dispersibility described above, and improve the printing density and dry fluidity.
[0140] The moisturizing agent is preferably a sugar. Examples of the sugar include monosaccharides, disaccharides, oligosaccharides (including trisaccharides and tetrasaccharides), polysaccharides, etc. Examples of the monosaccharide include glucose, mannose, fructose, ribose, xylose, arabinose, galactose, etc. Examples of the disaccharide include maltose, cellobiose, lactose, sucrose, trehalose, etc. Examples of the oligosaccharide include maltotriose, etc. Examples of the polysaccharide include α-cyclodextrin, cellulose, etc. Derivatives of these sugars, for example, reducing sugars of sugars (for example, sugar alcohols [general formula: HOCH 2 (CHOH) n CH 2 OH (where n is an integer of 2 to 5)), sugar oxides (for example, aldonic acid, uronic acid, etc.), amino acids, thioacids, etc. Among these, sugar alcohols are preferred, and maltitol and sorbitol are more preferred.
[0141] Inkjet inks can be used in various inkjet printers, including, for example, charge-controlled, continuous-jet, such as spray, and on-demand, such as piezo, thermal, and electrostatic suction.
[0142] <Flexographic Printing Ink> In an embodiment of the present invention, the flexographic printing ink preferably contains a binder resin in addition to the dispersion. Examples of the binder resin include acrylic resin and urethane resin. The flexographic printing ink may also contain additives, solvents, and crosslinking agents.
[0143] (Acrylic Resin) Examples of the acrylic resin include an acrylic copolymer, an acrylic acid-styrene copolymer resin, an acrylic acid-maleic acid resin, an acrylic acid-styrene-maleic acid resin, etc. The acrylic copolymer is a copolymer of (meth)acrylic acid and a (meth)acrylic acid ester.
[0144] (Urethane Resin) In addition to polyurethane resin, examples of urethane resins include polyurethane-urea resins. From the viewpoint of film-forming properties, it is preferable that the urethane resin has an acid value. The weight-average molecular weight of the urethane resin is preferably 10,000 to 100,000. When the urethane resin has an appropriate molecular weight, adhesion to the substrate, water friction resistance, scratch resistance, and blocking resistance are further improved.
[0145] The acid value of the binder resin is preferably 20 to 180 mgKOH / g, more preferably 40 to 150 mgKOH / g. A suitable acid value improves resolubility during printing, adhesion to substrates, water abrasion resistance, and blocking resistance.
[0146] The content of the binder resin is preferably 1 to 50% by mass relative to 100% by mass of the flexographic printing ink. When the content is moderate, the strength of the printed layer is improved, and adhesion to the substrate and water abrasion resistance are further improved.
[0147] Flexographic printing inks may contain additives as needed, such as leveling agents, wetting agents, water repellents, antifoaming agents, waxes, and crosslinking agents.
[0148] The solvent used in the flexographic printing ink may be water or the water-soluble solvents described above. The solvents may be used alone or in combination of two or more.
[0149] Flexographic printing ink can be prepared by mixing and dispersing the aforementioned components. For example, an aqueous flexographic ink can be prepared by adding optional components such as wax and wetting agents to the dispersion described above and mixing and stirring them. Dispersion and stirring can be performed using, for example, a high-speed mixer, a homogenizer, a planetary mixer, a trimix, a kneader, an extruder, a horizontal sand mill, a vertical sand mill and / or an annular bead mill, a paint shaker, a ball mill, a disperser equipped with an ultrasonic oscillator, a two-roll mill, a three-roll mill, or the like.
[0150] <Ink Set> In an embodiment of the present invention, the ink set preferably includes two or more inks of different colors. Of the two or more inks (two or more colors), at least one ink contains the dispersion described above. The colors included in the ink set include two or more inks selected from cyan, magenta, yellow, black, and white. Alternatively, the ink set includes two or more inks selected from red, green, blue, and orange. The colorants used in the ink set are not particularly limited, but can be appropriately selected from the colorants described above. The applications are not particularly limited, but the ink set can be used in packaging applications such as cardboard, paper container packaging, and labels, in addition to existing printing market applications such as commercial printing. Needless to say, the ink set can also include inks of colors other than cyan, magenta, yellow, black, white, red, green, blue, and orange. Examples of ink sets include inkjet ink sets and flexographic printing ink sets.
[0151] <Method for Manufacturing Printed Matter> In an embodiment of the present invention, the printed matter preferably comprises a substrate and a printing layer formed from ink. Examples of substrates include paper substrates and plastic substrates. Paper substrates are broadly classified into coated paper, such as coated paper, art paper, cast paper, and lightly coated paper, and uncoated paper, such as fine paper and foam paper. Coated paper is coated with a coating agent and has a smooth printing surface, while uncoated paper has a rough surface without a coating agent, resulting in significant differences in ink absorption between the two. Examples of plastic substrates include polyvinyl chloride sheets, polyester films, polypropylene films, and polyethylene films. The substrate may also be a laminate of multiple materials. Other examples include resin-coated photographic paper and synthetic paper (e.g., Yupo: registered trademark). The thickness of the substrate is approximately 20 to 300 μm, and the basis weight of the substrate is 30 to 300 g / m. 2 The thickness of the printed layer is preferably 0.01 to 5 μm, more preferably 0.1 to 4 μm, and even more preferably 0.5 to 3 μm. By keeping the thickness of the printed layer within the above range, it is possible to obtain sufficient color development as a printed matter, while allowing the solvent to evaporate sufficiently in the drying process during production of the printed layer, thereby forming a strong film. The printed layer can be formed using a printing machine suitable for each ink, such as an inkjet printer, flexographic printer, gravure printer, or offset printer. After printing the ink, a drying process can be added as necessary. Examples of dryers used in the drying process include hot air dryers and infrared heaters.
[0152] <Paint> In an embodiment of the present invention, the paint preferably contains a dispersion and a binder resin, and more preferably contains a crosslinking agent. The paint is preferably an aqueous paint containing a dispersion and a binder resin. The ratio of the dispersion to the binder resin varies depending on the desired application and is not particularly limited.
[0153] (Binder Resin) Examples of binder resins include acrylic resins, polyester resins, alkyd resins, fluororesins, urethane resins, and silicone-containing resins containing crosslinkable functional groups. Examples of crosslinking agents include melamine resins, urea resins, polyisocyanate compounds, blocked polyisocyanate compounds, epoxy compounds, carboxy group-containing compounds, acid anhydrides, and alkoxysilane group-containing compounds. Among these, a combination of an acrylic resin and a melamine resin is preferred.
[0154] The coating material may further contain water, organic solvents, rheology control agents, pigment dispersing resins, anti-settling agents, curing catalysts, antifoaming agents, antioxidants, ultraviolet absorbers, surface conditioners, crosslinking agents, extender pigments, etc. as needed.
[0155] The paint can be made by mixing and dispersing the above materials.
[0156] The paint can be applied to a variety of substrates, including metal substrates such as iron, stainless steel, aluminum, and surface-treated aluminum; cement-based substrates such as cement, lime, and gypsum; and plastic substrates such as polyvinyl chlorides, polyesters, polycarbonates, and acrylics.
[0157] The paint can be applied by brushing, roller coating, spray coating, etc. After application, the coating is dried at room temperature or by heating to form a coating. The thickness of the coating is usually about 5 to 70 μm.
[0158] <Stationery Ink> In an embodiment of the present invention, the stationery ink contains the dispersion and can be used for applications such as writing instruments, recorders, and printers. The stationery ink preferably contains a binder resin. Depending on the application (e.g., ballpoint pen, marking pen, etc.), the stationery may optionally contain a water-soluble organic solvent, a thickener, a lubricant, an antiseptic, an antibacterial agent, etc. The ratio of colorant to binder resin varies depending on the desired application and is not particularly limited.
[0159] Stationery is preferably prepared by preparing a high-concentration dispersion, diluting it with water, and adding a binder resin and, if necessary, other additives. The dispersion may be dispersed by any of the known dispersion methods described above. More preferred applications for stationery include thixotropic inks (e.g., gel inks for water-based ballpoint pens) and Newtonian inks (e.g., low-viscosity water-based ballpoint pens). Furthermore, the pH (25°C) of the stationery is preferably adjusted to 5 to 10, more preferably 6 to 9.5, using a pH adjuster or the like, from the viewpoints of usability, safety, the stability of the ink itself, and compatibility with the ink container.
[0160] The content of the colorant can be adjusted appropriately depending on the density of the lines drawn on the stationery, and is preferably about 0.1 to 40% by mass of the total amount of the ink composition for stationery.
[0161] <Textile Printing Agent> In an embodiment of the present invention, the textile printing agent preferably contains a dispersion containing a colorant, water, and a binder resin. The textile printing agent can record images such as letters, pictures, and designs on fabrics such as woven fabrics, nonwoven fabrics, and knitted fabrics. The ratio of the colorant to the binder resin varies depending on the desired application and is not particularly limited.
[0162] The binder resin may be any of the above-mentioned binder resins. The binder resin may be in the form of water-dispersed particles, a water-soluble resin, etc. Examples of the binder resin include urethane resin and acrylic resin.
[0163] After preparing the dispersion, the printing agent can be prepared by further mixing it with water, a binder resin, and other additives as necessary, to prepare a printing agent suitable for a preferred processing method such as dip dyeing or printing depending on the fiber to be colored.
[0164] In an embodiment of the present invention, the printing agent can be used to print on fabrics, artificial leather, natural leather, etc. It is particularly excellent for printing on fabrics. The fabric is preferably a medium formed of fibers, and may be a woven fabric or a nonwoven fabric. Examples of materials include cotton, silk, wool, hemp, nylon, polyester, polyurethane, and rayon.
[0165] <Examples of Embodiments> (1) A dispersant comprising a block polymer having an A block and a B block, wherein the A block comprises styrene units and maleic acid units, and the B block comprises vinyl monomer units, and the acid value of the A block is greater than the acid value of the B block. (2) The dispersant according to (1) above, wherein the molecular weight dispersity of the block polymer is 1.0 or more and 2.0 or less. (3) The dispersant according to (1) or (2) above, wherein the A block further comprises vinyl monomer units, and the vinyl monomer units contain one or more units selected from the group consisting of N-substituted maleimide units and (meth)acrylic acid ester units. (4) The dispersant according to any one of (1) to (3) above, wherein in the B block, the vinyl monomer units contain one or more units selected from the group consisting of N-substituted maleimide units and (meth)acrylic acid ester units. (5) A dispersion comprising the dispersant according to any one of (1) to (4) above, a colorant, and water. (6) The dispersion according to (5) above, wherein the block polymer is modified with a resin modifier. (7) An ink comprising the dispersion according to (5) or (6) above. (8) An ink set comprising the ink according to (7) above. (9) A printed matter comprising a substrate and a printed layer formed using the ink according to (7) above or the ink set according to (8) above.
[0166] The present invention is related to the subject matter described in Japanese Patent Application No. 2023-087812, filed on May 29, 2023, the disclosure of which is incorporated herein by reference.
[0167] The present invention will be described in more detail below with reference to examples and comparative examples. However, it goes without saying that the present invention is not limited to the examples. Hereinafter, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass."
[0168] (Acid Value) Hereinafter, the acid value of the block polymer was calculated by the method described above, i.e., from the composition of the monomers contained in the block polymer. Specifically, the number of moles of acid groups contained in 1 g of the block polymer was calculated, and then the mass (mg) of potassium hydroxide (molecular weight 56.1) in an amount equimolar to the number of moles of the acid groups was used as the theoretical value of the acid value (mg KOH / g). The theoretical value of the acid value was calculated assuming that all maleic anhydride units introduced during the production of the block polymer were hydrolyzed to maleic acid in the final block polymer.
[0169] The living polymerization agents used in the synthesis of the block polymers are shown in Table 1.
[0170]
[0171] The amines used in the synthesis of the block polymers are shown in Table 2.
[0172]
[0173] Amine 3: JEFFAMINE M1000 (manufactured by HUNTSMAN), an amine having a copolymerization site of oxypropylene units (PO) and oxyethylene units (EO). Weight average molecular weight: 1000, PO / EO = 3 / 19 (molar ratio).
[0174] <Production of Block Polymer (Dispersed Resin)> (Production of Block Polymer (Dispersed Resin) 1) A reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer was charged with 10.0 parts (0.102 mol) of maleic anhydride, 10.0 parts (0.096 mol) of styrene, 2.0 parts (0.005 mol) of 4-cyano-4-[(dodecylsulfanylthiocarbonyl)sulfanyl]pentanoic acid as a living polymerization agent, and 100.0 parts of methyl ethyl ketone. After purging with nitrogen gas, the reaction vessel was heated to 80°C. While stirring, 0.5 parts (0.002 mol) of 2,2'-azobis(2,4-dimethylvaleronitrile) (manufactured by Tokyo Chemical Industry Co., Ltd.) was added dropwise over 6 hours. Thereafter, after confirming that the polymerization conversion rate had reached 95 to 100%, the reaction temperature was lowered to 60°C. Next, 80.0 parts (0.707 mol) of N-isopropylacrylamide was charged to the resulting reaction solution, and while heating and stirring at 80°C, 0.5 parts (0.002 mol) of 2,2'-azobis(2,4-dimethylvaleronitrile) (manufactured by Tokyo Chemical Industry Co., Ltd.) was added dropwise over 6 hours. After that, it was confirmed that the polymerization conversion rate had reached 95 to 100%, and the B block was synthesized. Through the above steps, a precursor of block polymer 1 was obtained, consisting of a block containing styrene units and maleic anhydride units and the B block. The temperature inside the reaction vessel was then lowered to 60°C. Next, 10 parts of water and 0.05 parts of diazabicycloundecene were added to the resulting reaction solution, and the mixture was heated to 80°C with stirring and maintained for 5 hours. The maleic anhydride units were hydrolyzed by the water to form maleic acid units (A block). The solvent was then completely removed by concentration under reduced pressure, yielding block polymer 1 consisting of an A block containing styrene units and maleic acid units and a B block. The resulting block polymer 1 had a number-average molecular weight of 10,000, a weight-average molecular weight of 17,000, an acid value of 112 mgKOH / g, and a molecular weight dispersity of 1.7. Potassium hydroxide was then added to the resulting block polymer 1 so that the degree of neutralization calculated from the acid value was 100%, and ion-exchanged water was added so that the nonvolatile content was 30%. The mixture was stirred at 50°C for 1 hour to obtain an aqueous solution of block polymer 1. The term "aqueous solution" refers to a liquid containing an aqueous solvent and components dispersed and / or dissolved in the aqueous solvent.Block polymer 1 is a polymer that functions as a dispersing resin, and will hereinafter also be referred to as "dispersing resin 1."
[0175] (Production of Block Polymers (Dispersion Resins) 2 to 54, 56 to 58, 60 to 62, 65, and 66) Block polymer precursors were produced in the same manner as Dispersion Resin 1, except that the raw materials and amounts charged were changed as shown in Tables 1, 3-1, and 3-7. Next, the maleic anhydride units present in the block polymer precursors were hydrolyzed using the compounds shown in Tables 3-1 to 3-7 (for Dispersion Resins 56 to 58, a portion of the maleic anhydride units was modified with an amine compound simultaneously with the hydrolysis), yielding block polymers Dispersion Resins 2 to 54, 56 to 58, 60 to 62, 65, and 66 (all of which were obtained in the form of aqueous solutions with a nonvolatile content of 30%). The molecular weight of the block polymers was adjusted by appropriately changing the amount of polymerization initiator used, etc.
[0176] (Production of Block Polymer (Dispersion Resin) 55) A block polymer precursor and then a block polymer were synthesized in the same manner as in Dispersion Resin 1, except that the raw materials and charged amounts were changed as shown in Tables 1 and 3-6 and the living polymerization agent was changed to 2.0 parts (0.009 mol) of 2-methyl-2-(methyltellanyl)propanenitrile (manufactured by Tokyo Chemical Industry Co., Ltd.) and 1.5 parts (0.005 mol) of dimethyl ditelluride (manufactured by Tokyo Chemical Industry Co., Ltd.), and an aqueous solution of Dispersion Resin 55 (non-volatile content 30%) was obtained.
[0177] (Production of Block Polymer (Dispersion Resin) 59) A reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer was charged with 4.8 parts (0.049 mol) of maleic anhydride, 5.0 parts (0.048 mol) of styrene, 12.5 parts (0.088 mol) of butyl methacrylate, 5.0 parts (0.029 mol) of phenylmaleimide, 2.0 parts (0.005 mol) of 4-cyano-4-[(dodecylsulfanylthiocarbonyl)sulfanyl]pentanoic acid as a living polymerization agent, and 100.0 parts of methyl ethyl ketone. The atmosphere in the reaction vessel was then purged with nitrogen gas, and the reaction vessel was heated to 80° C. While stirring, 0.5 parts (0.002 mol) of 2,2′-azobis(2,4-dimethylvaleronitrile) (manufactured by Tokyo Chemical Industry Co., Ltd.) was added dropwise over 6 hours. After confirming that the polymerization conversion rate had reached 95 to 100%, the reaction temperature was lowered to 60°C. Subsequently, 0.5 parts (0.005 mol) of maleic anhydride, 10.0 parts (0.096 mol) of styrene, and 35.0 parts (0.208 mol) of cyclohexyl methacrylate were added to the resulting reaction solution, and while heating and stirring at 80°C, 0.5 parts (0.002 mol) of 2,2'-azobis(2,4-dimethylvaleronitrile) (manufactured by Tokyo Chemical Industry Co., Ltd.) was added dropwise over 6 hours. After that, it was confirmed that the polymerization conversion rate had reached 95 to 100% (Block B). The temperature inside the reaction vessel was then lowered to 60°C. Next, 4.8 parts (0.049 mol) of maleic anhydride, 5.0 parts (0.048 mol) of styrene, 12.5 parts (0.088 mol) of butyl methacrylate, and 5.0 parts (0.029 mol) of phenylmaleimide were added to the resulting reaction solution, and while heating and stirring at 80°C, 0.5 parts (0.002 mol) of 2,2'-azobis(2,4-dimethylvaleronitrile) (manufactured by Tokyo Chemical Industry Co., Ltd.) was added dropwise over 6 hours. It was then confirmed that the polymerization conversion rate had reached 95 to 100%. Through the above steps, a precursor of block polymer 59 was obtained, consisting of two blocks containing styrene units and maleic anhydride units and one B block. The temperature inside the reaction vessel was then lowered to 60°C.Next, 10 parts of water and 0.05 parts (0.328 mmol) of diazabicycloundecene were added to the resulting reaction solution, and the mixture was heated to 80°C with stirring and maintained for 5 hours. The maleic anhydride units were hydrolyzed with water to form maleic acid units (A blocks). The solvent was then completely removed by vacuum concentration, yielding block polymer 59, which consisted of two A blocks each containing a styrene unit and a maleic acid unit and one B block. The resulting block polymer 59 had a number-average molecular weight of 13,000, a weight-average molecular weight of 18,000, an acid value of 113 mgKOH / g, and a molecular weight dispersity of 1.4. Potassium hydroxide was then added to the resulting block polymer so that the degree of neutralization reached 100% based on its acid value. Ion-exchanged water was then added to the mixture so that the nonvolatile content reached 30%. The mixture was stirred at 50°C for 1 hour, yielding an aqueous dispersion of dispersion resin 59.
[0178] (Production of Block Polymer (Dispersion Resin) 63) A block polymer was produced in the same manner as Dispersion Resin 1, except that the raw materials and amounts charged were changed as shown in Table 3-7, and this block polymer was used as is as Block Polymer 63. (However, Block Polymer 63 was obtained in the form of an aqueous liquid with a nonvolatile content of 30%.) The molecular weight of Block Polymer 63 was adjusted by appropriately changing the amount of polymerization initiator used, etc.
[0179] (Production of Block Polymer (Dispersion Resin) 64) The raw materials and amounts charged were changed as shown in Table 3-7, and a polymer was synthesized in the same manner as in Dispersion Resin 1, except that 2.5 parts (0.010 mol) of 2,2'-azobis(2,4-dimethylvaleronitrile) (manufactured by Tokyo Chemical Industry Co., Ltd.) was used, to obtain an aqueous solution of Dispersion Resin 64 having no blocks (non-volatile content 30%).
[0180] Tables 3-1 to 3-7 below show the structures (% by mass) of the monomers used in synthesizing the precursors of the block polymers, and Tables 4-1 to 4-7 below show the structures (% by mass) of the monomer units present in the produced block polymers, as well as the molecular weights of the block polymers.
[0181]
[0182]
[0183]
[0184]
[0185]
[0186]
[0187]
[0188] The abbreviations for the monomers listed in Tables 3-1 to 3-7 are as follows: Manh: maleic anhydride St: styrene CHMA: cyclohexyl methacrylate CHA: cyclohexyl acrylate IBMA: isobornyl methacrylate DCPMA: dicyclopentanyl methacrylate BzMA: benzyl methacrylate MMA: methyl methacrylate BMA: butyl methacrylate LMA: lauryl methacrylate StMA: stearyl methacrylate VA: behenyl acrylate PME-400: methoxypolyethylene glycol methacrylate (NOF Corporation, Blenmer PME-400) PMI: phenylmaleimide CHMI: cyclohexylmaleimide MAA: methacrylic acid IPAm: N-isopropylacrylamide
[0189]
[0190]
[0191]
[0192]
[0193]
[0194]
[0195]
[0196] The acid values of each block listed in Tables 4-1 to 4-7 are values calculated from the acid value of the block polymer using the method described above. In the tables, there are some areas where the total content of each monomer unit does not equal 100% by mass, and some areas where the total calculated from the acid values of each block does not match the acid value listed in the "Dispersed Resin" column. This is because the content values are rounded to one decimal place, and the acid values are rounded to one decimal place. There are also some areas where the difference calculated from the amount of maleic acid units in each block does not match the value listed in the "Difference in the amount of maleic acid units relative to the amount of total monomer units in the dispersed resin" column. These discrepancies are also due to rounding. Among the abbreviations for monomers listed in Tables 4-1 to 4-7, details of monomers not listed in Tables 3-1 to 3-7 are as follows: MleAcd: maleic acid MamAcd1: N-laurylmaleamic acid MamAcd2: N-cyclohexylmaleamic acid MamAcd3: N-methoxypolyalkylene glycol maleamic acid (wherein the ratio of the number of moles of oxypropylene units (PO) added to the number of moles of oxyethylene units (EO) added in the structure is PO / EO = 3 / 19 (molar ratio))
[0197] <Preparation of Dispersions> (Preparation of Dispersion Set 1) 20 parts of Printex 85 (carbon black, manufactured by Orion Engineered Carbons) as colorant K, 20 parts of an aqueous dispersion liquid (non-volatile content 30%) of dispersion resin 1 as a dispersant, 15 parts of methyl ethyl ketone, and 45 parts of water were mixed and premixed with a stirrer. After premixing with a 0.6 L Dyno Mill filled with 1,800 parts of zirconia beads with a diameter of 0.5 mm, this dispersion was carried out. 100 parts of water was then added, and 100 parts of the solution was distilled under reduced pressure using an evaporator to obtain a black dispersion. Next, dispersion set 1 (K, C, M, Y) was obtained using the same method, except that the pigments were changed as follows: Cyan as colorant C: LIONOGEN BLUE FG-7358G (C.I. Pigment Blue 15:3) manufactured by Toyocolor Co., Ltd. Magenta as colorant M: TOSHIKI RED 150TR (C.I. Pigment Red 150) manufactured by Tokyo Color Materials Co., Ltd. Yellow as colorant Y: LIONOL YELLOW TT1405G (C.I. Pigment Yellow 14) manufactured by Toyocolor Co., Ltd.
[0198] (Production Examples of Dispersion Sets 2 to 62, 64 to 67) Dispersion Sets 2 to 62, 64 to 67 were obtained in the same manner as Dispersion Set 1, except that the dispersing resin used as the dispersant was changed according to Table 5.
[0199] (Production Example of Dispersion Set 63) The dispersion resin used as the dispersant was changed according to Table 5, and the same method as for Dispersion Set 1 was used. Then, 2.45 parts of Denacol EX321 (epoxy crosslinking agent, manufactured by Nagase Chemitex, non-volatile content 100%, epoxy equivalent 140 g / eq) was added as a resin modifier (crosslinking agent) to 100 parts of the dispersion, and the mixture was stirred at 70°C for approximately 2 hours. Ion-exchanged water equivalent to the amount of water evaporated was added to adjust the concentration, and Dispersion Set 63 was obtained.
[0200]
[0201] <Production of Inkjet Ink Set> (Production of Inkjet Ink Set 1) 25.0 parts of the black dispersion from the obtained Dispersion Set 1, 20.0 parts of propylene glycol, 5.0 parts of 1,2-hexanediol, 10.0 parts of Joncryl 538 (manufactured by BASF Japan) as a binder resin, 35.95 parts of ion-exchanged water, and 32.0 parts of Surfynol DF110D (an acetylene diol surfactant manufactured by Air Products Japan, active ingredient 32%, calculated by the Griffin method) as a surfactant were mixed together to prepare an inkjet ink set. A black inkjet ink was obtained by mixing 0.1 parts and 0.5 parts of BYK-348 (a siloxane surfactant manufactured by BYK, HLB value calculated by the Griffin method = 2.7), 0.5 parts of triethanolamine as a pH adjuster, 2.9 parts of AQUACER 515 (manufactured by BYK) as a wax, and 0.05 parts of Proxel GXL(s) (manufactured by Arch Chemical Co.) as a preservative. Inkjet ink set 1 (K, C, M, Y) was obtained using the same method except for changing the dispersion used in dispersion set 1. AQUACER 515: polyethylene wax (resin fine particles) manufactured by BYK, melting point 135°C, non-volatile content 35%.
[0202] <Production of Inkjet Ink Sets 2 to 67> Inkjet ink sets 2 to 67 were obtained in the same manner as inkjet ink set 1, except that dispersion set 1 was changed to dispersion sets 2 to 67, respectively. In each of the inkjet inks constituting inkjet ink sets 1 to 67, the content by mass of the surfactant having an HLB value of 2 to 8.5 calculated by the Griffin method was 0.02 when the content by mass of the dispersion resin was taken as 1.
[0203] <Production of Inkjet Ink Sets 68 to 74> Inkjet ink sets 68 to 74 were obtained using the same method and materials as for Inkjet Ink Set 9, except that the type and amount of Surfynol DF110D added and the amount of ion-exchanged water added were changed as shown in Table 6 below.
[0204]
[0205] Table 6 also lists the mass contents of surfactants having an HLB value of 2 to 8.5 calculated by the Griffin method, when the mass content of the dispersion resin is taken as 1. Details of the trade names of the surfactants listed in Table 6 are as follows: Surfynol DF110D: acetylene diol-based surfactant manufactured by Air Products Japan, active ingredient 32%, HLB value calculated by the Griffin method = 2.7 Surfynol 104: acetylene diol-based surfactant manufactured by Air Products Japan, active ingredient 100%, HLB value calculated by the Griffin method = 3.0 Surfynol 440: acetylene diol-based surfactant manufactured by Air Products Japan, active ingredient 100%, HLB value calculated by the Griffin method = 8.1 Surfynol 465: acetylene diol-based surfactant manufactured by Air Products Japan, active ingredient 100%, HLB value calculated by the Griffin method = 13.2
[0206] <Production of Printed Material> (Production of Printed Material 1) The obtained inkjet ink set 1 was loaded into an inkjet printer (manufactured by Seiko Epson Corporation, model number: EM-930C, piezo system), and printed on high-quality paper (NPi Form NEXT-IJ, manufactured by Nippon Paper Industries Co., Ltd., 64 g / m 2 ), and coated paper (OK Top Coat, manufactured by Oji Paper Co., Ltd., 104.7 g / m 2 ) and a PET film (FE2001, manufactured by Tamura Chemical Co., Ltd., thickness 12 μm) were printed solid over the entire surface (fine mode) with black ink, cyan ink, magenta ink, and yellow ink. Immediately after printing, the printed matter was placed in an air oven at 70° C. and dried for 5 minutes, thereby obtaining printed matter 1.
[0207] <Production of Printed Matters 2 to 74> Printed Matters 2 to 74 were obtained in the same manner as for Printed Matter 1, except that inkjet inks 2 to 74 were used.
[0208] Examples 1 to 133, Comparative Examples 1 to 8 The dispersions, inkjet inks, and printed materials produced above were subjected to the following evaluations 1 to 6.
[0209] <Evaluation 1: Evaluation of Storage Stability> With regard to the obtained dispersion set, the storage stability was evaluated as follows using each of the black colored dispersion (hereinafter also referred to as K), cyan colored dispersion (hereinafter also referred to as C), magenta colored dispersion (hereinafter also referred to as M), and yellow colored dispersion (hereinafter also referred to as Y). The dispersions were stored in a thermostatic chamber at 70°C to accelerate aging, and then the change in viscosity of the dispersions before and after aging was evaluated. The viscosity was measured using an E-type viscometer (TVE-20L, standard cone, manufactured by Toki Sangyo Co., Ltd.) at 25°C and a rotation speed of 50 rpm, and the value after 1 minute was taken as the viscosity value. The evaluation criteria were as follows. A rating of 2 or higher was considered to be in the practical range. 5: For each of the K, C, M, and Y colors, the viscosity change rate after four weeks of storage is less than ±10%. 4: For each of the K, C, M, and Y colors, the viscosity change rate after two weeks of storage is less than ±10%. 3: For each of the K, C, M, and Y colors, the viscosity change rate after one week of storage is less than ±10%. 2: For each of the K, C, M, and Y colors, the viscosity change rate after one week of storage is between ±10% and 20%. 1: For each of the K, C, M, and Y colors, the viscosity change rate after one week of storage is more than ±20%.
[0210] <Evaluation 2: Evaluation of Coarse Particle Amount> The amount of coarse particles in the resulting dispersion set was evaluated using each of the black, cyan, magenta, and yellow colored dispersions as follows. Specifically, the amount of coarse particles in the dispersion was evaluated by the time it took for a fixed amount of dispersion to pass through a 25 mm diameter glass fiber filter (manufactured by GF / BGE Healthcare Life Sciences). When the amount of coarse particles was high, the filter clogged, resulting in a longer observed passing time. Furthermore, when the amount of coarse particles was even higher, the filter clogged, making it impossible to filter the entire amount of dispersion. Generally, filters used in the ink supply path to an inkjet head are larger than 1 μm, and inkjet recording inks generally have a lower colorant concentration than dispersions. Therefore, passing through the filter by this test method is sufficient; however, a faster filtration rate leads to higher resolubility and disintegration of colorant particles, resulting in superior productivity. The evaluation conditions are shown below. A 25 mm diameter filter holder (manufactured by ADVANTEC) with a 15 ml graduated funnel and a 25 mm diameter glass fiber filter (manufactured by GF / BGE Healthcare Life Sciences) is placed on a suction vessel equipped with a vacuum pump via a cock. The vacuum pump is operated using the cock so that the pressure inside the suction vessel is not reduced. 15 g of dispersion is weighed into the funnel. The pressure between the pump and the suction vessel is opened, and the time it takes for the entire amount of dispersion to pass through the filter is measured. The pressure inside the suction vessel at this time is 0.05 MPa to 0.07 MPa. Hereinafter, a rating of 2 or higher was considered to be within the practical range. 5: Filtering is possible in less than 20 seconds for each of K, C, M, and Y colors. 4: Filtering is possible in 20 seconds or more and less than 30 seconds for each of K, C, M, and Y colors. 3: Filtering is possible in 30 seconds or more and less than 45 seconds for each of K, C, M, and Y colors. 2: Filtering is possible in 45 seconds or more and less than 60 seconds for each of K, C, M, and Y colors. 1: Filtering is not possible in less than 60 seconds for each of K, C, M, and Y colors.
[0211] <Evaluation 3: Redispersibility Evaluation> The redispersibility of the obtained inkjet ink was evaluated as follows. 10 μL of inkjet ink was dropped onto an aluminum dish and left to stand in a thermostatic oven at 40°C for 2 hours to evaporate and solidify the aqueous ink. After a predetermined time had elapsed, 1 mL of redispersibility cleaner was dropped, and the solid matter was visually confirmed after 1 minute. Furthermore, evaluations were also conducted using the same procedure, with the remaining time in the thermostatic oven at 40°C being 4, 8, and 12 hours. Ink that can be redispersed even after standing for a long period of time means that even if it dries and solidifies on the inkjet head, it can be treated with a cleaner and used for printing as usual. The evaluation criteria are as follows. A rating of 2 or higher was considered to be in the practical range. 5: In each of the K, C, M, and Y colors, the solidified material was uniformly redispersed even after standing for 12 hours. 4: In each of the K, C, M, and Y colors, the solidified material was uniformly redispersed after standing for 8 hours, but was not redispersed after standing for 12 hours. 3: In each of the K, C, M, and Y colors, the solidified material was uniformly redispersed after standing for 4 hours, but was not redispersed after standing for 8 hours. 2: In each of the K, C, M, and Y colors, the solidified material was uniformly redispersed after standing for 2 hours, but was not redispersed after standing for 4 hours. 1: In each of the K, C, M, and Y colors, the solidified material was not redispersed regardless of the standing time.
[0212] <Evaluation 4: Evaluation of density on fine paper> The inkjet ink obtained was loaded into an inkjet printer (manufactured by Seiko Epson Corporation, model number: EM-930C, piezo system), and printed on fine paper (NPi Form NEXT-IJ, manufactured by Nippon Paper Industries Co., Ltd., 64 g / m²). 2) and a 100% solid image was printed using black ink, cyan ink, magenta ink, and yellow ink. The print was left to stand for 24 hours at 25°C and a relative humidity of 50%, and then the obtained test piece was measured using an eXactAdvance densitometer manufactured by X-rite. The color measurement conditions were ISO status T based on density, a viewing angle of 2°, and a light source D50. A larger numerical value for print density means a higher print density. The evaluation criteria are as follows. A rating of 2 or higher was considered to be in the practical range. 5: OD value for each of K, C, M, and Y colors is higher than the density of Comparative Example 1 by 0.3 or more. 4: OD value for each of K, C, M, and Y colors is higher than the density of Comparative Example 1 by 0.2 or more and less than 0.3. 3: OD value for each of K, C, M, and Y colors is higher than the density of Comparative Example 1 by 0.1 or more and less than 0.2. 2: OD value for each of K, C, M, and Y colors is higher than the density of Comparative Example 1 by less than 0.1. 1: OD value for each of K, C, M, and Y colors is equal to or lower than the density of Comparative Example 1.
[0213] <Evaluation 5: Evaluation of density on coated paper> The obtained inkjet ink was loaded into an inkjet printer (manufactured by Seiko Epson Corporation, model number: EM-930C, piezo system), and printed on coated paper (OK Topcoat manufactured by Oji Paper Co., Ltd., 104.7 g / m²) 2) and a 100% solid image was printed using black ink, cyan ink, magenta ink, and yellow ink. The print was left to stand for 24 hours at 25°C and a relative humidity of 50%, and then the obtained test piece was measured using an eXactAdvance densitometer manufactured by X-rite. The color measurement conditions were ISO status T based on density, a viewing angle of 2°, and a light source D50. A larger numerical value for print density means a higher print density. The evaluation criteria are as follows. A rating of 2 or higher was considered to be in the practical range. 5: OD value for each of K, C, M, and Y colors is higher than the density of Comparative Example 1 by 0.7 or more. 4: OD value for each of K, C, M, and Y colors is higher than the density of Comparative Example 1 by 0.5 or more and less than 0.7. 3: OD value for each of K, C, M, and Y colors is higher than the density of Comparative Example 1 by 0.2 or more and less than 0.5. 2: OD value for each of K, C, M, and Y colors is higher than the density of Comparative Example 1 by more than 0.0 and less than 0.2. 1: OD value for each of K, C, M, and Y colors is equal to or lower than the density of Comparative Example 1.
[0214] <Evaluation 6: Durability Evaluation of Printed Matter> The inkjet inks obtained in the examples and comparative examples were loaded into an inkjet printer (Seiko Epson Corporation, model number: EM-930C, piezo type), and 100% solid images were printed on PET film (Tamura Chemical Co., Ltd., FE2001, 12 μm thick) using black ink, cyan ink, magenta ink, and yellow ink. The resulting prints were evaluated using a Gakushin-type abrasion fastness tester AB-301 (Tester Sangyo Co., Ltd.) under conditions of a load of 500 g and 30 round trips of friction, using Kanakin No. 3 (abrasion resistance evaluation), Kanakin No. 3 soaked in water (water resistance evaluation), and Kanakin No. 3 soaked in ethanol (solvent resistance evaluation), and the surface condition of the image was visually observed. If the durability evaluation was excellent on a film substrate that does not soak into the recording medium, it is possible to exhibit sufficient durability on a paper substrate that does soak into the inkjet ink. The rating scale was as follows: A rating of 2 or higher was considered to be in the usable range. 5: In the rub resistance, water resistance, and solvent resistance evaluations for each of the K, C, M, and Y colors, there were no scratches on the printed surface and no ink peeling. 4: In the rub resistance, water resistance, and solvent resistance evaluations for each of the K, C, M, and Y colors, there were scratches on the printed surface or ink peeling of less than 5%. 3: In the rub resistance, water resistance, and solvent resistance evaluations for each of the K, C, M, and Y colors, there were scratches on the printed surface or ink peeling of 5% or more but less than 15%. 2: In the rub resistance, water resistance, and solvent resistance evaluations for each of the K, C, M, and Y colors, there were scratches on the printed surface or ink peeling of 15% or more but less than 30%. 1: In the rub resistance, water resistance, and solvent resistance evaluations for each of the K, C, M, and Y colors, there were scratches on the printed surface or ink peeling of 30% or more.
[0215] The evaluation results of the Examples and Comparative Examples are shown in Table 7 below. In Table 7, "inkjet ink sets 1 to 74" are abbreviated to "inks 1 to 74."
[0216]
[0217] The results in Tables 5 and 7 show that Examples 1 to 63 had good storage stability and good coarse particle content. Examples 64 to 133 exhibited excellent inkjet ink redispersibility and showed high print density without an ink-receiving layer when printed on coated and uncoated paper. It also demonstrates that a dispersion resin can be provided that can achieve excellent durability even when printed on a non-absorbent film substrate. Comparative Examples 1 and 5 did not contain maleic acid units, Comparative Examples 2 and 6 did not have an A block or B block, Comparative Examples 3 and 7 did not contain styrene units, and Comparative Examples 4 and 8 did not contain vinyl monomer units, and therefore, the problems of the present application could not be solved.
Claims
1. A dispersant comprising a block polymer having an A block and a B block, said A block comprising styrene units and maleic acid units, said B block comprising vinyl monomer units, and an acid number of said A block being greater than an acid number of said B block.
2. The dispersant according to claim 1, wherein the molecular weight dispersity of said block polymer is 1.0 or more and 2.0 or less.
3. The dispersant according to claim 1 or 2, wherein the A block further comprises a vinyl monomer unit, and the vinyl monomer unit contains one or more units selected from the group consisting of an N-substituted maleimide unit and a (meth)acrylic acid ester unit.
4. The dispersant according to any one of claims 1 to 3, wherein in the B block, the vinyl monomer unit contains one or more units selected from the group consisting of N-substituted maleimide units and (meth)acrylic acid ester units.
5. A dispersion comprising the dispersant according to any one of claims 1 to 4, a colorant, and water.
6. The dispersion of claim 5, wherein said block polymer is modified with a resin modifier.
7. An ink comprising the dispersion according to claim 5 or 6.
8. An ink set comprising the ink according to claim 7.
9. A printed matter comprising a substrate and a printing layer formed using the ink according to claim 7 or the ink set according to claim 8.
Citation Information
Patent Citations
Production method of low molecular weight sma
JP2002506895A
Water-based pigment formulations
JP2010528120A
Polymer dispersant for inorganic pigment
JP2016168584A
Coating colorant, coloring composition, and method for producing coating colorant
JP2020203965A
Dispersion liquid, ink composition for ink jet recording, and dispersing resin
JP2022081148A