Conductive film and electromagnetic wave shielding material using same

The conductive film, featuring a thermosetting resin layer and a metal complex conductive layer, addresses the lack of stretchability and conformability in conventional shielding materials by ensuring effective electromagnetic wave blocking and heat resistance, suitable for wearable devices.

WO2024247973A1PCT designated stage expired Publication Date: 2024-12-05PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/019452
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2024-05-27
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional electromagnetic shielding materials lack stretchability and conformability to irregular surfaces, leading to gaps and reduced effectiveness in blocking electromagnetic waves, especially when applied to wearable devices or curved surfaces.

Method used

A conductive film with a thermosetting resin layer and a conductive layer containing a metal complex, where the thermosetting resin layer has high elongation at break and tensile modulus, and the conductive layer has a specific thickness and surface resistivity, allowing for excellent flexibility and heat resistance while maintaining conductivity.

Benefits of technology

The conductive film effectively blocks electromagnetic waves without gaps on irregular surfaces, maintains conductivity through stretching, and provides excellent heat resistance, making it suitable for wearable devices and applications requiring conformability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024019452_05122024_PF_FP_ABST
    Figure JP2024019452_05122024_PF_FP_ABST
Patent Text Reader

Abstract

One aspect of the present invention relates to a conductive film which has a thermosetting resin layer and a conductive layer that is positioned on at least a part of at least one surface of the thermosetting resin layer, and which is characterized in that: the thermosetting resin layer has an elongation break at 20°C of 50% or more, a tensile elastic modulus at 20°C of 1.0 MPa to 200 MPa inclusive, and a storage elastic modulus at 250°C of 0.1 MPa to 200 MPa inclusive; the conductive layer has a film thickness of 0.1 μm to 3.0 μm inclusive; the conductive layer contains a metal complex; and the conductive layer has a surface resistivity of 1 × 10-2 Ω / □ to 10 Ω / □ inclusive.
Need to check novelty before this filing date? Find Prior Art

Description

Conductive film and electromagnetic wave shielding material using the same

[0001] The present invention relates to a conductive film and an electromagnetic wave shielding material using the same.

[0002] Electromagnetic wave shielding materials have been used for some time to prevent malfunction of electronic devices and electromagnetic interference caused by electromagnetic waves leaking from electric circuits, as well as information fluctuations due to interception of communication radio waves.

[0003] Electromagnetic wave shielding materials generally have a conductive layer laminated on a substrate. For example, Patent Document 1 discloses a flexible electromagnetic wave absorbing sheet formed by sequentially laminating a resistive film, a dielectric layer, and an electromagnetic wave shielding layer, and characterized in that the resistive film is formed from a conductive organic polymer.

[0004] Recently, there has been a demand for electromagnetic wave shielding materials that can be worn or used as a skin patch. For such applications, the shielding material must be stretchable, but the electromagnetic wave absorbing sheet described in Patent Document 1 is flexible but not stretchable, so when it is made to conform to minute irregularities or three-dimensional curved surfaces, gaps are created, making it impossible to effectively block electromagnetic waves.

[0005] Patent Document 2 discloses an electromagnetic wave shielding material having electromagnetic wave shielding properties, comprising a stretchable substrate and a conductive layer disposed on the surface of the substrate, the conductive layer having a thickness of 5 nm to 500 nm, wherein cracks occur in the conductive layer when a tensile force is applied to the electromagnetic wave shielding material so that the electromagnetic wave shielding material elongates by 2%, and when the tensile force on the electromagnetic wave shielding material is released after the tensile force is applied to the electromagnetic wave shielding material so that the electromagnetic wave shielding material elongates by 2%, the cracked portions of the conductive layer re-contact. In this technology, the conductive layer is formed on a stretchable substrate, but when the sheet material is folded or when it is attempted to conform to sharp irregularities, cracks occur in the conductive layer, degrading conductivity and potentially preventing sufficient blocking properties.

[0006] The present invention has been made in view of the above circumstances, and has an object to provide a conductive film that can be used as an electromagnetic wave shield and has excellent conformability and stretchability.

[0007] International Publication No. 2018 / 088492 Patent No. 6562834

[0008] As a result of extensive research, the present inventors have found that the above problems can be solved by a laminate having the following configuration, and have completed the present invention through further research based on this finding.

[0009] That is, a conductive film according to one aspect of the present invention is a conductive film having a thermosetting resin layer and a conductive layer on at least a part of at least one surface of the thermosetting resin layer, wherein the thermosetting resin layer has a breaking elongation rate of 50% or more at 20°C, a tensile modulus of elasticity at 20°C of 1.0 MPa or more and 200 MPa or less, and a storage modulus of elasticity at 250°C of 0.1 MPa or more and 200 MPa or less, the conductive layer has a film thickness of 0.1 μm or more and 3.0 μm or less, the conductive layer contains a metal complex, and the conductive layer has a surface resistivity of 1×10 -2 It is characterized in that the resistance is Ω / □ or more and 10Ω / □ or less.

[0010] Fig. 1 is a schematic cross-sectional view of a conductive film according to one embodiment of the present invention. Fig. 2 is a schematic cross-sectional view of a conductive film according to another embodiment of the present invention. Fig. 3 is a schematic cross-sectional view of a conductive film according to yet another embodiment of the present invention. Fig. 4 is a schematic cross-sectional view of a conductive film according to yet another embodiment of the present invention. Fig. 5 is a schematic cross-sectional view of a conductive film according to yet another embodiment of the present invention.

[0011] The conductive film of this embodiment includes a thermosetting resin layer and a conductive layer on at least a portion of at least one surface of the thermosetting resin layer. The thermosetting resin layer has a breaking elongation of 50% or more at 20°C and a tensile modulus of elasticity of 1.0 MPa or more and 200 MPa or less at 20°C. The thermosetting resin layer also has a storage modulus of elasticity of 0.1 MPa or more and 200 MPa or less at 250°C. The conductive layer has a film thickness of 0.1 μm or more and 3.0 μm or less, and contains a metal complex. The conductive layer also has a surface resistivity of 1×10 -2 It is Ω / □ or more and 10Ω / □ or less.

[0012] As described above, the conductive film of this embodiment has a thermosetting resin layer with a breaking elongation of 50% or more at 20°C, which allows the film to efficiently block electromagnetic waves without losing conductivity even in uneven areas with a small radius of curvature. Furthermore, the thermosetting resin layer has a tensile modulus of 1.0 MPa to 200 MPa at 20°C, which allows the film to be flexible and conform to uneven or curved surfaces without gaps. Furthermore, the thermosetting resin layer has a storage modulus of 0.1 MPa to 200 MPa at 250°C, which allows the film to have sufficient heat resistance. Furthermore, the conductive layer contains a metal complex and has a film thickness of 0.1 μm to 3.0 μm, which allows the film to have sufficient conductivity and electromagnetic wave blocking properties while suppressing breakage of the conductive layer due to elongation of the film.

[0013] Therefore, the conductive film of this embodiment is a conductive film with excellent conformability to irregularities and stretchability, which makes it suitable for use as an electromagnetic wave shield.

[0014] Specific embodiments of the present invention will be described below with reference to the drawings. Note that the embodiment described below is merely one of various embodiments of the present invention. The following embodiment can be modified in various ways depending on the design as long as the object of the present invention can be achieved. Furthermore, the reference numerals in the drawings indicate the following: 1 conductive film, 2 conductive layer, 3 resin layer, 4 adhesive layer.

[0015] As shown in Fig. 1 , the conductive film 1 of this embodiment includes a thermosetting resin layer 3 and a conductive layer 2 on at least a portion of at least one surface of the thermosetting resin layer 3. The conductive layer 2 may be provided on the entire surface of one surface of the thermosetting resin layer 3 as shown in Fig. 1 , or may be provided on only a portion of one surface of the thermosetting resin layer 3 as shown in Fig. 2 . Alternatively, as shown in Fig. 3 , the conductive layer 2 may be provided on both surfaces of the thermosetting resin layer 3. In the conductive film 1 shown in Fig. 3 , the conductive layer 2 is provided on the entire surface of one surface of the thermosetting resin layer 3 and on a portion of the other surface, but the present invention is not limited to this embodiment and may be provided on the entire surface of both surfaces or on a portion of both surfaces.

[0016] In another embodiment, the conductive film 1 of the present embodiment may also include a conductive layer 2 inside the thermosetting resin layer 3, as shown in Fig. 4. In the specific example shown in Fig. 4, the conductive layer 2 is provided on the surface of a through hole provided in the thermosetting resin layer 3. This configuration has the advantage that the conductive layers provided on both sides can be electrically connected and can be connected to an electrical ground in a small area.

[0017] Each component of the conductive film according to this embodiment will be described in more detail.

[0018] (Thermosetting resin layer) The thermosetting resin layer of this embodiment (hereinafter also simply referred to as "resin layer") has elasticity, and has a breaking elongation at 20°C of 50% or more and a tensile modulus at 20°C of 1.0 MPa or more and 200 MPa or less.

[0019] In this embodiment, the breaking elongation refers to the elongation rate until breaking, and together with the tensile modulus, is an index of the flexibility of the resin layer. A more preferable breaking elongation is 100% or more and 500% or less. In this embodiment, the upper limit of the breaking elongation is the higher the better, but 1000% is sufficient.

[0020] The thermosetting resin layer has a tensile modulus of elasticity at 20° C. of 1.0 MPa to 200 MPa, more preferably 1.0 MPa to 50 MPa, and even more preferably 1.5 MPa to 30 MPa.

[0021] A conductive film having a resin layer having a breaking elongation and tensile modulus within the above-mentioned ranges has high conformability when deformed into any shape, and therefore it is possible to obtain a conductive film and electromagnetic wave shielding material that has excellent conformability to, for example, clothing, is resistant to breakage, and has excellent stretchability.

[0022] The tensile modulus in this embodiment is a value measured by the following method: First, a cured resin composition constituting the resin layer is cut into a size of 50 mm x 5.5 mm and attached to a universal testing machine (AGS-X manufactured by Shimadzu Corporation). Then, a test is performed at room temperature (25°C) and a tensile speed of 500 mm / min, and the tensile modulus is calculated by determining the slope of r-σ (initial tensile modulus) using the least squares method from all stress (σ) data corresponding to strains (r) from 1.0% to 5.0% elongation. Strain (r) = x / x0 (x is the movement distance of the grips, x0 is the initial distance between the grips) Stress (σ) = F / (d·l) (F is the test force, d is the film thickness, and l is the width of the test piece)

[0023] Furthermore, the breaking elongation is measured by the tester at the time when the cured product breaks.

[0024] Furthermore, the thermosetting resin layer of this embodiment has a storage modulus of 0.1 MPa or more and 200 MPa or less at 250°C. This ensures that the resin layer of this embodiment has sufficient heat resistance, and can withstand the temperatures of the ink drying and curing processes, for example, when forming a conductive layer using ink. A more preferred range for the storage modulus is 1 MPa or more and 10 MPa or less. The storage modulus in this embodiment is a value that can be measured by the method described in the Examples section below.

[0025] The resin layer of this embodiment is not particularly limited as long as it is composed of a material (thermosetting resin composition) containing a thermosetting resin whose tensile modulus, elongation at break, and storage modulus fall within the above-mentioned ranges. However, for example, the resin layer is preferably formed from either a cured product, semi-cured product, or dried product of a resin composition containing a thermosetting resin. In this embodiment, a "semi-cured product" refers to a resin composition that has been partially cured to the extent that it can be further cured. That is, a semi-cured product refers to a resin composition that has been semi-cured (B-staged). For example, when a resin composition is heated, its viscosity initially gradually decreases, and then curing begins, and the viscosity gradually increases. In such a case, the semi-cured state can be described as the state between when the viscosity begins to increase and when it is completely cured. In this embodiment, a "dried product" refers to a resin composition (the resin composition in A-stage) before curing, after the solvent has been dried.

[0026] The thermosetting resin may be, for example, a thermosetting resin that is commonly used as an insulating layer for various film substrates or electronic substrates. Specific examples of the thermosetting resin include epoxy resins, polyrotaxane resins, acrylic resins, urethane resins, silicone resins, isocyanate resins, polyol resins, and hydrogenated styrene-based elastomer resins. Among these, the resin layer of this embodiment is preferably a cured product, semi-cured product, or dried product of a resin composition containing at least one thermosetting resin selected from the group consisting of epoxy resins, polyrotaxane resins, acrylic resins, and hydrogenated styrene-based elastomer resins.

[0027] As the thermosetting resin, particularly preferred is an epoxy resin. Specific examples of epoxy resins include bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol S epoxy resins, aralkyl epoxy resins, phenol novolac epoxy resins, alkylphenol novolac epoxy resins, biphenol epoxy resins, naphthalene epoxy resins, dicyclopentadiene epoxy resins, epoxidized products of condensation products of phenols and aromatic aldehydes having a phenolic hydroxyl group, triglycidyl isocyanurate, alicyclic epoxy resins, etc. Depending on the situation, these may be used alone or in combination of two or more.

[0028] More preferred examples of the epoxy resin include an epoxy resin containing two or more epoxy groups in one molecule and having a molecular weight of 500 or more, or an epoxy resin having an epoxy equivalent of 400 g / eq or more. Commercially available epoxy resins may be used, including, for example, JER1003 (manufactured by Mitsubishi Chemical, molecular weight 1300, bifunctional), EXA-4816 (manufactured by DIC, molecular weight 824, bifunctional), YP50 (manufactured by Nippon Steel Sumitomo Metal Chemicals, molecular weight 60,000 to 80,000, bifunctional), PMS-14-67 (manufactured by Nagase ChemteX Corporation, molecular weight 300,000, multifunctional), and PASR-001 (manufactured by Nagase ChemteX Corporation, molecular weight 500,000, multifunctional). The above-mentioned epoxy resins may be used alone or in combination of two or more.

[0029] The polyrotaxane resin that can be suitably used in this embodiment is a resin having a structure in which a linear axial molecule penetrates a cyclic molecule and the ends of the cyclic molecule are blocked to prevent the cyclic molecule from coming out. Specific examples include polyrotaxanes such as those described in Japanese Patent No. 4482633.

[0030] The above-mentioned thermosetting resins may be used singly or in combination of two or more.

[0031] In the thermosetting resin composition used in the resin layer of this embodiment, the amount of the thermosetting resin as described above is not particularly limited as long as it fulfills its role as a base resin, but is usually preferably about 30% by mass or more and 98% by mass or less, more preferably 50% by mass or more and 90% by mass or less, based on the total resin composition.

[0032] The thermosetting resin composition used in this embodiment may further contain a curing agent for the purpose of curing the thermosetting resin. Examples of the curing agent include phenol-based curing agents, amine-based curing agents, acid anhydride-based curing agents, ester-based curing agents, imidazole-based curing agents, dicyandiamide, cationic curing agents, and metal soaps. These may be used without any particular limitation, and one or more types may be used in combination.

[0033] In this embodiment, the amount of the curing agent is not particularly limited as long as it fulfills its role as a curing agent, but it is preferably about 0.1% by mass to 30% by mass, more preferably 0.1% by mass to 10% by mass, based on the total amount of the resin composition.

[0034] Furthermore, the resin composition of this embodiment may contain various additives as other components in addition to those described above. Examples of additives include curing accelerators, dispersants, fillers, antioxidants, leveling agents, pigments, dyes, etc. These may be used alone or in combination. The amount of these other components may be appropriately set depending on their role and is not particularly limited, but is preferably about 0.001 parts by mass or more and 50% by mass or less of the total resin composition.

[0035] The thickness of the resin layer of this embodiment is not particularly limited as long as it fulfills its role as a substrate (base layer) of the conductive film, but from the viewpoint of combining both properties of flexibility and strength as a support when used in an electromagnetic wave shielding material, the thickness is preferably about 10 μm to 500 μm, more preferably 25 μm to 200 μm, and even more preferably 50 μm to 100 μm.

[0036] The method for forming the resin layer of this embodiment is not particularly limited. To give one example, first, a thermosetting resin composition constituting the resin layer is dissolved in an appropriate organic solvent (e.g., methyl ethyl ketone, toluene, etc.) to prepare a resin varnish. The resin varnish is then applied to a support such as a PET film using a bar coater or the like to a desired thickness, and the coating is dried to remove the solvent, thereby forming a resin layer. Furthermore, the resin layer may be formed by curing the resin composition by heating and pressurizing under specified conditions.

[0037] (Conductive Layer) In the conductive film of the present embodiment, the conductive layer contains a metal complex, and the surface resistivity of the conductive layer is 1×10 -2 The surface resistivity is preferably in the range of 1×10 to 10 Ω / □. By providing such a conductive layer with a thickness of 0.1 μm to 3.0 μm, the conductive film of the present embodiment can efficiently block electromagnetic waves. A more preferred range of the surface resistivity is 1×10 -2 Ω / □ or more 1×10 -1 Ω / □ or less.

[0038] In this embodiment, the metal complex contained in the conductive layer is a compound formed by bonding a metal ion with one or more ligands. In this embodiment, the conductive layer can be formed using a metal complex by, for example, a reduction reaction, a substitution reaction, an oxidation-reduction reaction, or thermal decomposition. The reason why a conductive layer obtained from a metal complex is highly elastic is unclear, but it is thought to be due to the fact that the crystalline structure is not regular, but has an amorphous or fine crystalline structure. On the other hand, compared to conductive layers formed by other methods for obtaining metal thin films, such as vacuum deposition and sputtering, the conductive layer of this embodiment has slightly inferior conductivity, but still has sufficient conductivity for specific applications, such as electromagnetic wave shielding. Furthermore, because the conductive layer is highly elastic, the conductive film of this embodiment has sufficient conformability and stretchability, making it easy to apply to various products (including flexible fabric products). In addition, because the conductive layer of this embodiment contains a metal complex, cracks are less likely to occur in the conductive film even when it is repeatedly stretched and contracted, as is the case with conventional conductive layers, and it has the excellent advantage of maintaining conductivity even after stretching.

[0039] In this embodiment, the metal complex is obtained, for example, by reacting a metal salt with a catalyst. Examples of methods for producing the metal complex include a method in which the metal salt and the catalyst are added to a dissolving agent and stirred for a predetermined period of time. The stirring method is not particularly limited and can be appropriately selected from known methods, such as a method of stirring using a stirring bar, stirring blades, or mixer, or a method of applying ultrasound.

[0040] In this embodiment, examples of the metal constituting the metal complex include iron, cobalt, nickel, copper, zinc, ruthenium, rhodium, palladium, silver, platinum, osmium, and iridium. Among these, it is preferable to include silver because it has better electrical conductivity.

[0041] In the present embodiment, examples of metal salts for forming a metal complex include metal oxides, chlorides, sulfides, cyanides, carbonates, acetates, nitrates, salts of iron, sulfates, phosphates, and carboxylates. Among these, carboxylates are preferred because of their superior conductivity and storage stability.

[0042] In this embodiment, a metal complex can be obtained by reducing a silver salt to silver metal using a catalyst. Examples of catalysts include metal borohydrides, aluminum hydrides, amine compounds, alcohols, organic acids, reducing sugars, sugar alcohols, sodium sulfite, hydrazine compounds, dextrin, hydroquinone, hydroxylamine, ethylene glycol, glutathione, and oxime compounds. Among these, amine compounds are preferred because of their superior reaction rate and stability. Examples of amine compounds include primary amines, secondary amines, tertiary amines, and polyamines, such as methylamine, ethylamine, propylamine, butylamine, pentylamine, hexylamine, heptylamine, octylamine, nonylamine, decylamine, undecylamine, dodecylamine, tridecylamine, tetradecylamine, pentadecylamine, hexadecylamine, heptadecylamine, octadecylamine, allylamine, and n- Examples of the amine include propylamine, isopropylamine, n-butylamine, sec-butylamine, tert-butylamine, n-pentylamine, isopentylamine, 2-ethylhexylamine, tert-hexylamine, phenylamine, cyclopentylamine, tert-octylamine, tert-decylamine, tert-dodecylamine, tert-octadecylamine, dimethylamine, diethylamine, dipropylamine, dibutylamine, diphenylamine, dicyclopentylamine, methylbutylamine, trimethylamine, triethylamine, tripropylamine, triphenylamine, ethylenediamine, 1,3-diaminopropane, and hexamethylenediamine.

[0043] In this embodiment, the metal complex may contain a dissolving agent. The dissolving agent is selected from the group consisting of an organic solvent, a chelating agent, and a combination thereof. The organic solvent is selected from the group consisting of an alkane hydrocarbon, a carbamate, an alkene, a cyclic hydrocarbon, an aromatic hydrocarbon, an amine, a polyamine, an amide, an ether, an ester, an alcohol, a thiol, a thioether, a phosphine, and a combination thereof. Examples of the organic solvent include pentane, hexane, heptane, octane, nonane, decane, undecane, dodecane, tridecane, tetradecane, pentadecane, hexadecane, octadecane, nonadecane, icosane, cyclohexane, cycloheptane, cyclooctane, cyclononane, cyclodecane, decalin, benzene, toluene, xylene, tetralin, xylene, dimethyl ether, diethyl ether, dipropyl ether, dibutyl ether, methyl t-butyl ether, tetradecane, methyl t-butyl ether ... Examples of the alcohol include dihydrofuran, tetrahydropyran, dihydropyran, 1,4-dioxane, 1-propanol, 2-propanol, 1-methoxy-2-propanol, 1-butanol, 2-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 1-hexanol, 2-hexanol, 3-hexanol, 1-octanol, 2-octanol, 3-octanol, tetrahydrofurfuryl alcohol, cyclopentanol, terpineol, and the like. Examples of chelating agents include ethylenediaminetetraacetic acid, iminodiacetic acid, ethylenediamine-di(o-hydroxyphenylacetic acid), nitrilotriacetic acid, dihydroxyethylglycine, trans-1,2-cyclohexanediaminetetraacetic acid, diethylenetriamine-N,N,N',N",N"-pentaacetic acid, glycol ether diamine-N,N,N',N'-tetraacetic acid, dimethyl sulfoxide, diethylenetriamine, tert-octylamine, tert-butylamine, 2-ethylhexylamine, and ethylenediamine.

[0044] The conductive layer of this embodiment can be formed using a metal complex ink containing the metal complex described above. The metal complex ink preferably contains the metal complex in an amount of 0.1 wt % or more and 40 wt % or less.

[0045] The metal complex ink that can be used in this embodiment may be a commercially available product, and for example, silver complex ink "EI-1207" manufactured by Electroniks is preferably used.

[0046] The conductive layer of this embodiment may contain the metal complex at least in part, and such a conductive layer can be obtained, for example, by applying the metal complex ink described above onto the thermosetting resin layer by a spray method or the like so that the resulting film thickness is 0.1 μm to 3.0 μm, and then heating and sintering the applied layer at a predetermined temperature (depending on the type of metal).

[0047] (Adhesive Layer) The conductive film 1 of this embodiment may further include an adhesive layer 4 as shown in Fig. 5. The adhesive layer 4 can serve as an adhesive layer when attaching the conductive film 1 to an object, and can also serve as a protective layer for the conductive layer 2.

[0048] Such an adhesive layer 4 may be provided on the conductive layer 2 as shown in Fig. 5, or may be provided on the thermosetting resin layer 3. Alternatively, it may be provided on both the conductive layer 2 and the thermosetting resin layer 3. The provision of such an adhesive layer 4 has the advantage of making it possible to easily adhere the conductive film to the adherend. In particular, the provision of an adhesive layer 4 on the conductive layer 2 is preferable because it has the advantage of being able to effectively protect the conductive layer.

[0049] The adhesive layer 4 of this embodiment is not particularly limited as long as it is made of a material having adhesive properties.

[0050] Specifically, adhesives and pressure sensitive adhesives used in the field of electromagnetic wave shielding materials and the like can be used as the adhesive layer 4 of this embodiment without any particular limitations.

[0051] Examples of adhesives that can be used in this embodiment include thermoplastic adhesives and thermosetting adhesives. More specifically, examples of thermoplastic adhesives include adhesives whose main component is polyvinyl alcohol, acrylic resin, polyvinyl acetate, polyethylene, polyolefin, polyamide, polyester, various rubbers, or polyurethane. Examples of thermosetting adhesives that can be used include epoxy resin adhesives and phenol resin adhesives. The thermosetting adhesive may be composed of a semi-cured resin or the like.

[0052] Examples of the adhesive include rubber-based adhesives, acrylic-based adhesives, silicone-based adhesives, and urethane-based adhesives. From the viewpoint of adhesion, acrylic-based adhesives and urethane-based adhesives are preferred.

[0053] The thickness of the adhesive layer in this embodiment is not particularly limited, but from the viewpoint of achieving both adhesive strength and flexibility, it is preferably 0.1 μm or more and 200 μm or less, and more preferably 0.5 μm or more and 50 μm or less.

[0054] There are no particular limitations on the method for forming the adhesive layer 4. For example, when an adhesive or the like is used, the adhesive layer 4 can be formed by applying the adhesive to the conductive layer 2 and / or the thermosetting resin layer to the desired thickness, or by bonding a film-shaped adhesive film or pressure-sensitive adhesive film or the like.

[0055] (Uses of Conductive Film) The conductive film as described above can be used in a variety of applications, but can be particularly suitably used as an electromagnetic wave shielding material.

[0056] (Electromagnetic Wave Shielding Material) This embodiment also includes an electromagnetic wave shielding material made of the conductive film described above. The electromagnetic wave shielding material of this embodiment can be placed without gaps on a surface with minute irregularities or a three-dimensional curved surface, and can effectively block electromagnetic waves. In addition, it has the advantage of being able to be attached to objects of any shape and having excellent workability.

[0057] The electromagnetic wave shielding material of the present embodiment has the above-described properties and is therefore suitable for use in wearable computing devices. Specifically, it can also be used in situations and applications where bioelectric signals are detected, such as in electromyography sensors, electrocardiogram sensors, and electroencephalogram sensors.

[0058] As described above, this specification discloses various aspects of the technology, but the main technologies among them are summarized below.

[0059] A conductive film according to a first aspect of the present invention is a conductive film having a thermosetting resin layer and a conductive layer on at least a part of at least one surface of the thermosetting resin layer, wherein the thermosetting resin layer has a breaking elongation of 50% or more at 20°C, a tensile modulus of elasticity of 1.0 MPa or more and 200 MPa or less at 20°C, and a storage modulus of elasticity of 0.1 MPa or more and 200 MPa or less at 250°C, the conductive layer has a film thickness of 0.1 μm or more and 3.0 μm or less, the conductive layer contains a metal complex, and the conductive layer has a surface resistivity of 1×10 -2 It is characterized in that the resistance is Ω / □ or more and 10Ω / □ or less.

[0060] A conductive film according to a second aspect of the present invention is the conductive film of the first aspect, wherein the conductive layer is formed using a metal complex ink.

[0061] A conductive film according to a third aspect of the present invention is the conductive film according to the first or second aspect, wherein the metal complex contains silver.

[0062] A conductive film according to a fourth aspect of the present invention is the conductive film according to any one of the first to third aspects, which has a conductive layer also inside the thermosetting resin layer.

[0063] A conductive film according to a fifth aspect of the present invention is the conductive film according to any one of the first to fourth aspects, further comprising an adhesive layer.

[0064] A conductive film according to a sixth aspect of the present invention is the conductive film according to any one of the first to fifth aspects, wherein the thermosetting resin layer is any one of a cured product, a semi-cured product, and a dried product of a resin composition containing at least one thermosetting resin selected from an epoxy resin, a polyrotaxane resin, an acrylic resin, and a hydrogenated styrene-based elastomer resin.

[0065] An electromagnetic wave shielding material according to a seventh aspect of the present invention is an electromagnetic wave shielding material comprising the conductive film according to any one of the first to sixth aspects.

[0066] An electromagnetic wave shielding material according to an eighth aspect of the present invention is the electromagnetic wave shielding material according to the seventh aspect, which is used in a wearable computing device.

[0067] The present invention will be explained in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.

[0068] First, the various materials used in this example are as follows:

[0069] (Epoxy Resin) Epoxy Resin 1 Acrylonitrile as polymerization unit (a), isobornyl acrylate as polymerization unit (b), and polymerization unit (c) represented by the following formula (1) were polymerized so that the blending ratio (polymerization %) of (a):(b):(c) was 10:20:70, and glycidyl methacrylate was further added as polymerization unit (d) so that the epoxy equivalent relative to the total amount of acrylic resin was the value shown in Table 1. The mixture was then polymerized to obtain Epoxy Resin 1 (manufactured by Nagase ChemteX Corporation, "PMS-14-67EK40") containing methyl ethyl ketone as a solvent. The solids content was 40% by weight. (In the formula, R1 is hydrogen or a methyl group, R2 is hydrogen or an alkyl group, and X is an integer.)

[0070] Epoxy resin 2 (manufactured by Nagase ChemteX Corporation, "PMS-14-64EK40") was obtained in the same manner as in "PMS-14-67EK40" except that the amount of polymerization unit (d) was changed. The solid content was 40% by weight.

[0071] Epoxy resin 3 (manufactured by Nagase ChemteX Corporation, "PASR-001") was obtained in the same manner as in "PMS-14-67EK40" except that the ratio of the polymerization units (a) to (d) was changed. The solid content was 20%.

[0072] Bisphenol-type epoxy resin ("jER1003" manufactured by Mitsubishi Chemical Corporation) Bisphenol-type epoxy resin ("jER1006FS" manufactured by Mitsubishi Chemical Corporation)

[0073] (Polyrotaxane) Polyrotaxane: "SH3400P" manufactured by Advanced Soft Materials Co., Ltd.

[0074] (Hardening agent) Acid anhydride hardener ("Rikacid TBN-100" manufactured by New Japan Chemical Co., Ltd.) Amine-based hardener ("Porea SL-100A" manufactured by Kumiai Chemical Industry Co., Ltd.) Carboxylic acid-based hardener ("TN-1" manufactured by NOF Corporation) Phenol-based hardener ("KAYAHARD GPH-103" manufactured by Nippon Kayaku Co., Ltd.) Acid anhydride hardener ("YH-307" manufactured by Mitsubishi Chemical Corporation)

[0075] (Curing accelerator) Imidazole-based curing accelerator ("2PZ-CN" manufactured by Shikoku Kasei)

[0076] (Solvent) Methyl ethyl ketone

[0077] (Metallic ink) Silver complex ink: "EI-1207" manufactured by Electroniks Palladium particle-containing ink: "Metalloid ML-130" manufactured by Iox Corporation

[0078] <Preparation of Thermosetting Resin Layer (Cured Film)> Resin varnishes 1 to 9 were prepared using the blending compositions (parts by mass) of each component shown in Table 1. After leaving to degas, each of the resin varnishes 1 to 9 was applied to a PET film (SP-PET O1, manufactured by Mitsui Chemicals Tohcello Co., Ltd.) using a bar coater to a thickness (after curing) shown in Table 2 below. The film was then heated in an oven at 80°C for 60 minutes and then further heated at 180°C for 120 minutes to obtain cured resin films 1 to 11 that would become the thermosetting resin layer. The thickness of each cured resin film was measured using a micrometer (MDH-25MB, manufactured by Mitutoyo Corporation).

[0079]

[0080] <Characteristics of Thermosetting Resin Layer (Cured Film)> (Method for Measuring Tensile Modulus and Elongation at Break) A sample (cured resin film) was cut to a size of 90 mm x 5.5 mm, attached to a universal testing machine (AGS-X manufactured by Shimadzu Corporation), and tested at a tensile speed of 500 mm / min. The tensile modulus was calculated from the stress at elongations of 1.0% to 5.0%. The elongation at which the sample broke was also measured.

[0081] (Method for measuring storage modulus) Each cured resin film was cut into a 10 mm × 30 mm piece and attached to a dynamic viscoelasticity measuring device (DMS6100 manufactured by Seiko Instruments Inc.) A test was performed at a strain amplitude of 10 μm, a frequency of 10 Hz (sine wave), and a temperature rise rate of 5° C. / min, and the storage modulus at 250° C. was measured.

[0082] The results are shown in Table 2. It should be noted that the storage modulus of Cured Film 10 could not be measured because it melted upon heating.

[0083]

[0084] <Preparation of Conductive Films> (Examples 1 to 11 and Comparative Examples 1 to 4) Each cured film to be used as a thermosetting resin layer was placed on a platen heated to 200°C, and a silver complex ink was sprayed onto each film to form a conductive layer with a thickness shown in Table 3, ensuring a uniform film thickness, to obtain the conductive films of Examples 1 to 11.

[0085] Comparative Example 5 A palladium particle-containing ink was applied to a cured film 7 using a bar coater to a uniform thickness of 0.7 μm, and then heated in an oven at 80° C. for 30 minutes to dry the ink. A conductive layer was then formed by electroless copper plating, thereby obtaining a conductive film of Comparative Example 5.

[0086] Comparative Example 6 Cured Film 7 was placed in a vacuum deposition apparatus, and copper was deposited to a thickness of 0.1 μm to form a conductive layer, thereby obtaining a conductive film of Comparative Example 6.

[0087] Comparative Example 7 Cured Film 7 was placed in a sputtering device, and conductive layers were formed by sputtering titanium to a thickness of 0.005 μm and then copper to a thickness of 0.1 μm, thereby obtaining a conductive film of Comparative Example 7.

[0088] (Thickness of conductive layer) The thickness of the conductive layer in the conductive film was measured by cutting the conductive film of each example and comparative example into 3 mm squares, solidifying it with an embedding resin, polishing the cross section using an ion milling device, and observing the cross section with an optical microscope.

[0089] [Evaluation Test] <Method for Measuring Sheet Resistance> For each conductive film, the film thickness value was input into a resistivity meter (MCP-T370, manufactured by Mitsubishi Chemical Analytech), and the volume resistivity of the surface was measured using the four-terminal method. The average value of measurement results at five or more points was used as the volume resistivity value.

[0090] <Method for Evaluating Heat Resistance> The storage modulus of the conductive film at 250°C was measured in the same manner as in the method for measuring the storage modulus described above, and evaluated according to the following criteria: Pass: 1 MPa or more Fail: Less than 1 MPa or below the measurement limit

[0091] <Method for evaluating electromagnetic wave shielding property> Each conductive film was placed in the electromagnetic wave shielding property evaluation device described in Japanese Patent No. 5619265, and the electric field shielding effect was measured. The electric field shielding effect over the range of 1 GHz to 6 GHz was evaluated according to the following criteria: Excellent: 30 dB or more; Good: 20 dB or more but less than 30 dB; Passable: 10 dB or more but less than 20 dB; Poor: Less than 10 dB.

[0092] <Method for evaluating 10% repeated stretchability> Each conductive film was cut into a size of 10 mm x 40 mm and placed on a stretchability evaluation device (DMLHB, manufactured by Yuasa System Co., Ltd.) and a sheet-shaped tensile test jig (DLD-ST, manufactured by Yuasa System Co., Ltd.) with a fixed distance of 20 mm. Wiring connected to a resistance meter (RM3545-02, manufactured by Hioki Electric Co., Ltd.) was fixed to both ends of the test piece with alligator clips. The test piece was repeatedly stretched and contracted at a frequency of 0.19 Hz while measuring the resistance value at 10% stretch, and the number of stretches until the resistance value reached 1200 Ω was counted. Based on the number of stretches, evaluation was performed according to the following criteria. Excellent: 10,000 times or more Good: 5,000 times or more but less than 10,000 times Pass: 1,000 times or more but less than 5,000 times Poor: Less than 1,000 times

[0093] The above results are summarized in Tables 3 and 4.

[0094]

[0095]

[0096] (Discussion) As is clear from the results in Table 3, it was confirmed that all of the conductive films of this embodiment have low resistivity, excellent heat resistance, and excellent electromagnetic wave shielding. It was also found that even after repeated 10% expansion and contraction, an increase in resistivity can be suppressed and conductivity can be maintained. In other words, it was demonstrated that the conductive film of this embodiment is a conductive film with excellent conformability and elasticity that can be used as an electromagnetic wave shield.

[0097] On the other hand, as shown in Table 4, the conductive film of Comparative Example 1, in which the thermosetting resin layer did not have a sufficient storage modulus, did not achieve heat resistance, and the conductive film of Comparative Example 2, in which the thermosetting resin layer did not have a sufficient elongation at break, was unable to maintain conductivity after stretching. Furthermore, the conductive film of Comparative Example 3, in which the conductive layer was too thin, failed to achieve sufficient electromagnetic wave shielding properties and also exhibited poor conductivity after stretching. The conductive film of Comparative Example 4, in which the conductive layer was too thick, was unable to maintain conductivity after stretching. Furthermore, the conductive films of Comparative Examples 5 to 7, in which the conductive layer was formed using conventional methods for forming conductive layers (plating, vapor deposition, sputtering) without using a metal complex, developed cracks in the conductive layer when stretched, and were unable to maintain conductivity after stretching.

[0098] In order to express the present invention, the present invention has been properly and sufficiently described above through embodiments with reference to specific examples, drawings, etc., but it should be recognized that those skilled in the art can easily make changes and / or improvements to the above-described embodiments. Therefore, unless changes or improvements made by those skilled in the art deviate from the scope of the claims set forth in the claims, such changes or improvements are construed as being encompassed within the scope of the claims.

[0099] The present invention has wide industrial applicability in technical fields related to electromagnetic wave absorption, electromagnetic wave shielding, and the like.

Claims

1. A conductive film having a thermosetting resin layer and a conductive layer on at least a portion of at least one surface of the thermosetting resin layer, wherein the thermosetting resin layer has a breaking elongation of 50% or more at 20°C, a tensile modulus of elasticity of 1.0 MPa or more and 200 MPa or less at 20°C, and a storage modulus of elasticity of 0.1 MPa or more and 200 MPa or less at 250°C, the conductive layer has a film thickness of 0.1 μm or more and 3.0 μm or less, the conductive layer contains a metal complex, and the conductive layer has a surface resistivity of 1×10 -2 A conductive film having a resistivity of Ω / □ or more and 10 Ω / □ or less.

2. The conductive film according to claim 1, wherein the conductive layer is formed using a metal complex ink.

3. The conductive film of claim 1, wherein said metal complex comprises silver.

4. The conductive film according to claim 1, further comprising a conductive layer inside said thermosetting resin layer.

5. The conductive film according to claim 1, further comprising an adhesive layer.

6. The conductive film according to claim 1, wherein the thermosetting resin layer is either a cured product, a semi-cured product or a dried product of a resin composition containing at least one thermosetting resin selected from the group consisting of epoxy resins, polyrotaxane resins, acrylic resins and hydrogenated styrene-based elastomer resins.

7. An electromagnetic wave shielding material comprising the conductive film according to any one of claims 1 to 6.

8. The electromagnetic shielding material according to claim 7, which is used in a wearable computing device.

Citation Information

Patent Citations

  • Ink composition for absorbing electromagnetic wave and absorber for electromagnetic wave

    JP2002188031A

  • Impact absorbing material for flat display, optical filter for plasma display, plasma display panel, and method of manufacturing impact absorbing material for flat display

    JP2007094191A

  • Method of manufacturing light permeable electromagnetic shield material, and light permeable electromagnetic shield material

    JP2011035220A

  • Curable resin composition, electromagnetic wave shielding film, circuit board, and manufacturing method of circuit board

    JP2021048314A

  • Process for preparation of laminated metal film

    KR1020100109233A