Rubber composition for tire and tire using same
The rubber composition for tires, with specific blending ratios of silica and alkyl alkoxysilane, addresses the challenge of achieving both scorch resistance and wet grip performance by using a sulfur-containing silane coupling agent, enhancing tire durability and performance.
Patent Information
- Application Number
- PCT/JP2024/019885
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-01
- Filing Date
- 2024-05-30
- Publication Date
- 2024-12-05
AI Technical Summary
Existing tire rubber compositions face challenges in achieving both excellent scorch resistance and wet grip performance, as adding silica to improve wet grip can lead to shortened scorch time and processability issues due to the high reactivity of sulfur-containing silane coupling agents.
A rubber composition containing diene rubber, silica, a sulfur-containing silane coupling agent, and an alkyl alkoxysilane compound, with specific blending ratios of silica (80-300 parts by mass) and alkyl alkoxysilane (10-20 parts by mass), and sulfur-containing silane coupling agent (3.5-5.5% by mass), where the ratios satisfy 0.03<(b/a)<0.06 and c/b≧1.5, using alkyldiethoxysilane or alkyltriethoxysilane, to maintain wet grip performance while enhancing scorch resistance.
The composition achieves excellent scorch resistance without impairing wet grip performance, maintaining the dispersion effect of silica while suppressing its high reactivity, thus improving tire durability and performance.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Rubber composition for tires and tire using the same
[0001] The present invention relates to a rubber composition for tires and a tire using the same, and more particularly to a rubber composition for tires that has excellent scorch resistance without impairing wet grip performance, and a tire using the same.
[0002] Generally, racing pneumatic tires are available for both dry and wet roads, with the optimal tire selected depending on the weather and road conditions. For racing tires designed for wet roads, techniques such as incorporating a large amount of silica or silica with a high specific surface area have been used to improve wet grip performance. However, due to silica's low affinity with rubber components and its high cohesion, simply incorporating silica into the rubber component does not disperse the silica, resulting in insufficient wet grip performance improvement. To address this issue, a silane coupling agent capable of reacting with silica is typically incorporated into a rubber composition containing silica. However, incorporating a large amount of silane coupling agent in conjunction with the incorporation of a large amount of silica or high specific surface area silica shortens the scorch time, and vulcanization progresses during kneading and extrusion, resulting in poor processability, or so-called burnt formation.
[0003] Conventional techniques aimed at improving the wet grip performance of tires include, for example, Patent Documents 1 to 6 listed below.
[0004] International Publication WO2013 / 133432 Pamphlet Japanese Patent Application Laid-Open No. 2019-104484 Japanese Patent No. 6969243 Japanese Patent No. 5888361 Japanese Patent No. 5644838 Japanese Patent No. 7397272
[0005] However, the prior art does not disclose or suggest any technical idea of simultaneously improving wet grip performance and scorch resistance by appropriately combining a sulfur-containing silane coupling agent and an alkylalkoxysilane compound. For example, Patent Document 6 discloses a cap tread rubber in which silica, a terpene resin, a silane coupling agent, and an alkyltriethoxysilane are blended with a modified diene rubber, but does not disclose or suggest the ratios of silica, sulfur-containing silane coupling agent, and alkylalkoxysilane compound of the present invention described below, nor does it mention any improvement in scorch resistance. An object of the present invention is to provide a rubber composition for tires that has excellent scorch resistance without impairing wet grip performance, and a tire using the same.
[0006] As a result of extensive research, the present inventors have discovered that the above-mentioned problems can be solved by specifying the amount of silica and the type of alkylalkoxysilane compound in a rubber composition for tires containing a diene rubber, silica, a sulfur-containing silane coupling agent, and an alkylalkoxysilane compound, and by specifying the compounding ratio of the sulfur-containing silane coupling agent and the alkylalkoxysilane compound, and have thus completed the present invention.
[0007] That is, the present invention provides a rubber composition for a tire containing a diene rubber, silica, a sulfur-containing silane coupling agent, and an alkylalkoxysilane compound, wherein the amount of silica blended is 80 to 300 parts by mass per 100 parts by mass of the diene rubber, the alkylalkoxysilane compound is an alkyldiethoxysilane or an alkyltriethoxysilane, and the amounts of the sulfur-containing silane coupling agent and the alkylalkoxysilane compound blended satisfy the following formulas (1) and (2): 0.03<(b / a)<0.06 (1) c / b≧1.5 (2) In formulas (1) and (2), a is the amount (parts by mass) of the silica blended per 100 parts by mass of the diene rubber, b is the amount (parts by mass) of the sulfur-containing silane coupling agent blended per 100 parts by mass of the diene rubber, and c is the amount (parts by mass) of the alkylalkoxysilane compound blended per 100 parts by mass of the diene rubber. The present invention also provides a tire using the rubber composition for a tire.
[0008] According to the present invention, there is provided a rubber composition for tires containing a diene rubber, silica, a sulfur-containing silane coupling agent, and an alkylalkoxysilane compound, characterized in that the amount of silica blended is 80 to 300 parts by mass per 100 parts by mass of the diene rubber, the alkylalkoxysilane compound is an alkyldiethoxysilane or an alkyltriethoxysilane, and the amounts of the sulfur-containing silane coupling agent and the alkylalkoxysilane compound blended satisfy the formulas (1) and (2). Therefore, it is possible to provide a rubber composition for tires that has excellent scorch resistance without impairing wet grip performance, and a tire using the same.
[0009] As mentioned above, methods for improving the wet grip performance of tires have been used, such as incorporating a large amount of silica or incorporating silica with a high specific surface area. However, silica has low affinity with rubber components, which requires the incorporation of a large amount of silane coupling agent. However, this method has the problem of shortening the scorch time and deteriorating processability (deteriorating scorch resistance). This problem is particularly pronounced when using a sulfur-containing silane coupling agent that has excellent silica dispersibility but high reactivity. Therefore, the present invention uses a specific alkylalkoxysilane compound that is effective in improving silica dispersibility but does not contain sulfur, and specifies the ratio of the sulfur-containing silane coupling agent and alkylalkoxysilane compound. This method maintains the silica dispersibility inherent to the sulfur-containing silane coupling agent, suppresses its high reactivity, and improves scorch resistance, while also successfully maintaining wet grip performance.
[0010] The present invention will now be described in further detail.
[0011] (Diene Rubber) The diene rubber used in the rubber composition for tires of the present invention (hereinafter sometimes simply referred to as the rubber composition) preferably contains styrene-butadiene copolymer rubber (SBR) as an essential component. When the total diene rubber used in the present invention is taken as 100 parts by mass, the amount of SBR blended can be determined taking into account various conditions such as temperature and weather, for example, in the case of racing applications, but can be, for example, 70 parts by mass or more, preferably 85 parts by mass or more, and more preferably 100 parts by mass. In the present invention, any diene rubber that can be blended into a typical rubber composition can be used in addition to SBR. Examples include natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), acrylonitrile-butadiene copolymer rubber (NBR), and ethylene-propylene-diene terpolymer (EPDM). These may be used alone or in combination of two or more types. The molecular weight and microstructure of the SBR used in the present invention are not particularly limited, but terminal modification with amine, amide, silyl, alkoxysilyl, carboxyl, hydroxyl, or the like is also preferred. Furthermore, from the viewpoint of enhancing the effects of the present invention, the SBR used in the present invention preferably has a styrene content of 20 to 45% by mass and / or a glass transition temperature (Tg) of -60 to -10°C (note that, if the SBR is oil-extended, the Tg is the value measured excluding the oil used for oil extension). The glass transition temperature (Tg) referred to in the present invention refers to the midpoint temperature of the transition region when a thermogram is measured by differential scanning calorimetry (DSC) at a heating rate of 20°C / min.
[0012] (Silica) The silica used in the present invention can be a silica having a high specific surface area. Specifically, the silica used in the present invention has a nitrogen adsorption specific surface area N 2 SA is 100 to 300m 2 / g, and 130 to 270 m 2 / g is more preferable. 2 The SA is measured in accordance with JIS K6217-2. In the present invention, silica made from a biomass material such as rice husk may also be used.
[0013] (Sulfur-Containing Silane Coupling Agent) The sulfur-containing silane coupling agent used in the present invention may be any that can be used in a rubber composition containing silica, and examples thereof include bis-(3-triethoxysilylpropyl)tetrasulfide, bis(3-triethoxysilylpropyl)disulfide, 3-trimethoxysilylpropylbenzothiazole tetrasulfide, γ-mercaptopropyltriethoxysilane, and 3-octanoylthiopropyltriethoxysilane. Furthermore, sulfur-containing silane coupling agents represented by the following formula (2), which are disclosed in, for example, International Publication WO 2014 / 002750, can also be used. (A) a (B) b (C) c (D) d (R1) e SiO (4-2a-b-c-d-e) / 2 (2) (In formula (2), A represents a divalent organic group containing a sulfide group, B represents a monovalent hydrocarbon group having 5 to 10 carbon atoms, C represents a hydrolyzable group, D represents an organic group containing a mercapto group, and R1 represents a monovalent hydrocarbon group having 1 to 4 carbon atoms, and the relationships 0≦a<1, 0<b<1, 0<c<3, 0<d<1, 0≦e<2, and 0<2a+b+c+d+e<4 are satisfied.) In the present invention, scorch resistance can be improved even when a silane coupling agent having a highly reactive mercapto group is used.
[0014] (Alkylalkoxysilane Compound) The alkylalkoxysilane compound used in the present invention is an alkyldiethoxysilane or an alkyltriethoxysilane. The alkyldiethoxysilane can be represented by the following formula (3), and the alkyltriethoxysilane can be represented by the following formula (4).
[0015]
[0016] In formulas (3) and (4), R1, R2, and R3 each independently represent an alkyl group having 1 to 20 carbon atoms, and Et represents an ethyl group. Among the alkyl groups having 1 to 20 carbon atoms for R1 and R2, a methyl group is preferred. Among the alkyl groups having 1 to 20 carbon atoms for R3, an alkyl group having 7 to 20 carbon atoms is preferred, and specific examples include a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, and a dodecyl group. Of these, from the viewpoint of compatibility with diene rubbers, an alkyl group having 8 to 10 carbon atoms is more preferred, with an octyl group and a nonyl group being particularly preferred.
[0017] (Aluminum Hydroxide) In the present invention, aluminum hydroxide can be blended from the viewpoint of improving the effect. The conditions of the aluminum hydroxide, such as its particle size distribution, are not particularly limited, and it can be appropriately selected from known aluminum hydroxides. For example, a commercially available product such as BF013 manufactured by Nippon Light Metal Co., Ltd. can be mentioned.
[0018] (Carbon Black) In the present invention, carbon black can be blended. The carbon black is not particularly limited, and various grades of carbon black, such as SAF-HS, SAF, ISAF-HS, ISAF, ISAF-LS, IISAF-HS, HAF-HS, HAF, HAF-LS, and FEF, can be used. The nitrogen adsorption specific surface area N of the carbon black is 2 SA is 100 to 250m 2 / g is preferred.
[0019] (Tackifying Resin) The rubber composition of the present invention can be blended with a tackifying resin to further improve its effects. The tackifying resin used in the present invention is not particularly limited, and specific examples include phenolic resins (e.g., phenolic resins, phenol-acetylene resins, phenol-formaldehyde resins), coumarone resins (e.g., coumarone resins, coumarone-indene resins, coumarone-indene-styrene resins), terpene resins (e.g., terpene resins, modified terpene resins (aromatic modified terpene resins, etc.), terpene phenolic resins), styrene resins, acrylic resins, rosin resins (e.g., rosin, rosin esters, hydrogenated rosin derivatives), hydrogenated terpene resins), petroleum resins (e.g., C5 petroleum resins such as dicyclopentazine resins, C9 petroleum resins, alicyclic petroleum resins, C5 / C9 copolymer petroleum resins), xylene resins (e.g., xylene resins, xylene-acetylene resins, xylene-formaldehyde resins), α-pinene resins, and aliphatic saturated hydrocarbon resins. Among these, for reasons of superior effects of the present invention, one or more selected from C9 petroleum resins, phenolic resins, coumarone-indene resins, terpene resins, modified terpene resins, styrene resins, acrylic resins, rosin-based resins, and dicyclopentadiene resins are preferred. Examples of modified terpene resins include aromatic modified terpene resins, such as those obtained by polymerizing terpene resins such as α-pinene, β-pinene, dipentene, and limonene with aromatic compounds such as styrene, α-methylstyrene, vinyltoluene, and indene. Commercially available aromatic modified terpene resins can be used, such as YS Resin TO-125 (terpene styrene resin, Mw = 2000, softening point 120-130°C) manufactured by Yasuhara Chemical Co., Ltd.
[0020] (Rubber Composition Blending Ratio) In the rubber composition of the present invention, the blending amount of silica is 80 to 300 parts by mass, preferably 100 to 250 parts by mass, per 100 parts by mass of diene rubber. If the blending amount of silica is less than 80 parts by mass, tan δ0°C decreases, and if it exceeds 300 parts by mass, scorch resistance deteriorates. In the rubber composition of the present invention, the blending amount of the sulfur-containing silane coupling agent is preferably 3.5 to 5.5% by mass, more preferably 4 to 5% by mass, per 100 parts by mass of diene rubber. In the rubber composition of the present invention, the blending amount of the alkylalkoxysilane compound is preferably 10 to 20 parts by mass, more preferably 12 to 18 parts by mass, per 100 parts by mass of diene rubber.
[0021] In the rubber composition of the present invention, in order to achieve the effects of the present invention, it is necessary that the compounding amounts of the sulfur-containing silane coupling agent and the alkylalkoxysilane compound satisfy the following formulas (1) and (2), and it is more preferable that the compounding amounts satisfy the following formulas (11) and (21).
[0022] 0.03<(b / a)<0.06 (1) c / b≧1.5 (2)
[0023] 0.032<(b / a)<0.058 (11) 1.6<c / b<5.0 (21)
[0024] In the formulas (1) and (2), a is the amount (parts by mass) of the silica per 100 parts by mass of the diene rubber, b is the amount (parts by mass) of the sulfur-containing silane coupling agent per 100 parts by mass of the diene rubber, and c is the amount (parts by mass) of the alkylalkoxysilane compound per 100 parts by mass of the diene rubber.
[0025] In one embodiment of the present invention, when aluminum hydroxide is used, the amount thereof is preferably 15 parts by mass or more, more preferably 20 to 80 parts by mass, per 100 parts by mass of the diene rubber. When carbon black is used, the amount thereof is preferably 3 to 50 parts by mass, per 100 parts by mass of the diene rubber. When a tackifying resin is used, the amount thereof is preferably 10 to 100 parts by mass, per 100 parts by mass of the diene rubber.
[0026] (Other Components) In addition to the above-mentioned components, the rubber composition of the present invention may contain various additives commonly used in rubber compositions, such as vulcanizing or crosslinking agents; vulcanizing or crosslinking accelerators; various fillers such as clay, talc, and calcium carbonate; antioxidants; plasticizers; resins; and curing agents. These additives can be kneaded by a conventional method to form a composition, which can then be used for vulcanization or crosslinking. The amounts of these additives may be conventional amounts, as long as they do not conflict with the objectives of the present invention. The method for producing the rubber composition of the present invention is not particularly limited, and specific examples include methods in which the above-mentioned components are kneaded using known methods and devices (e.g., Banbury mixers, kneaders, rolls, etc.). When the composition of the present invention contains a vulcanizing agent (e.g., sulfur) and a vulcanization accelerator, it is preferable to first mix the components other than the vulcanizing agent and vulcanization accelerator at a high temperature (preferably 100 to 155°C), cool the mixture, and then mix the vulcanizing agent and vulcanization accelerator, in order to achieve better effects of the present invention in the resulting composition. The composition of the present invention can be vulcanized or crosslinked under conventionally known vulcanization or crosslinking conditions.
[0027] The rubber composition of the present invention can be suitably used for tire treads, particularly cap treads, preferably racing tire treads, particularly cap treads. The tire of the present invention is preferably a pneumatic tire, which can be filled with air, an inert gas such as nitrogen, or other gases.
[0028] The present invention will be further explained below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0029] Standard Example 1, Examples 1-6, Comparative Examples 1-6 In the formulation (parts by mass) shown in Table 1, the components excluding the vulcanization system (vulcanization accelerator, sulfur) were kneaded for 5 minutes in a 1.7-liter internal Banbury mixer, then discharged from the mixer and cooled to room temperature. The composition was then re-charged into the same Banbury mixer, and the vulcanization system was added and kneaded to obtain a rubber composition. The resulting rubber composition was then press-vulcanized in a specified mold at 150°C for 30 minutes to prepare vulcanized rubber test pieces. The physical properties of the resulting vulcanized rubber test pieces were measured using the test methods shown below.
[0030] Scorch time: Tested at 125°C in accordance with JIS K6300. The results are expressed as an index, with the value of Standard Example 1 being 100. A larger index indicates better scorch resistance. Wet grip performance: In accordance with JIS K6394:2007, tan δ (0°C) was measured using a viscoelasticity spectrometer (manufactured by Toyo Seiki Seisakusho) under conditions of an elongation deformation strain rate of 10±2%, a frequency of 20 Hz, and a temperature of 0°C. The results are expressed as an index, with Standard Example 1 being 100. A larger index indicates better wet grip performance.
[0031] The results are also shown in Table 1.
[0032] Standard Example 2, Examples 7-12, Comparative Examples 7-12 The above-mentioned "Standard Example 1, Examples 1-6, Comparative Examples 1-6" were repeated except that the blending amounts of each material were changed as shown in Table 2. The results are shown in Table 2. The results of Examples 7-12 and Comparative Examples 7-12 are the values relative to Standard Example 2 in Table 2.
[0033] Standard Example 3, Examples 13-18, Comparative Examples 13-18 The above-mentioned "Standard Example 1, Examples 1-6, Comparative Examples 1-6" were repeated except that the blending amounts of each material were changed as shown in Table 3. The results are shown in Table 3. The results of Examples 13-18 and Comparative Examples 13-18 are the values relative to Standard Example 3 in Table 3.
[0034]
[0035]
[0036]
[0037] * 1: SBR (Nipol NS522 manufactured by ZS Elastomers Co., Ltd., styrene content = 39 mass%, oil-extended product obtained by adding 37.5 mass parts of an oil component to 100 mass parts of SBR, Tg of SBR excluding the oil component = -25 ° C.) * 2: Silica (Ultrasil 7000GR manufactured by Evonik, nitrogen adsorption specific surface area N 2 SA=172m 2 / g) *3: Carbon black (SEAT 9 manufactured by Tokai Carbon Co., Ltd., nitrogen adsorption specific surface area N 2 SA=142m 2 / g) *4: Aluminum hydroxide (BF013 manufactured by Nippon Light Metal Co., Ltd.) *5: Resin 1 (Neopolymer 140S manufactured by ENEOS Corporation) *6: Silane coupling agent 1 (Si69 manufactured by Evonik) *7: Silane coupling agent 2 (Si363 manufactured by Evonik. Has a mercapto group at the end.) *8: Alkyltriethoxysilane (KBE-3083, octyltriethoxysilane manufactured by Shin-Etsu Chemical Co., Ltd.) *9: Alkyldiethoxysilane (KBE-22, dimethyldiethoxysilane manufactured by Shin-Etsu Chemical Co., Ltd.) *10: Oil (Extract No. 4S manufactured by Showa Shell Sekiyu K.K.) *11: Stearic acid (Beads Stearic Acid YR manufactured by NOF Corporation) *12: Zinc oxide (Zinc oxide 3 types manufactured by Seido Chemical Industry Co., Ltd.) *13: Antiaging agent (6PPD manufactured by Flexis) * 14: Vulcanization accelerator 1 (Sansera D-G manufactured by Sanshin Chemical Industry Co., Ltd.) * 15: Vulcanization accelerator 2 (Noccela CZ-G manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) * 16: Sulfur (Kinka-jirushi oil-filled fine sulfur manufactured by Tsurumi Chemical Industry Co., Ltd.) * 17: Terminally modified SBR (trade name TUFDENE E581 manufactured by Asahi Kasei Corporation, styrene amount = 36 mass%, oil-extended product in which 37.5 mass parts of oil component are added to 100 mass parts of SBR, the terminals are modified with hydroxyl groups. Tg of SBR excluding the oil component = -27 ° C.) * 18: Resin 2 (Yasuhara Chemical Co., Ltd. YS Resin TO125)
[0038] The results in Tables 1 to 3 show that the rubber compositions of each Example contain diene rubber, silica, a sulfur-containing silane coupling agent, and an alkylalkoxysilane compound, with the silica content being 80 to 300 parts by mass per 100 parts by mass of the diene rubber, the alkylalkoxysilane compound being an alkyldiethoxysilane or an alkyltriethoxysilane, and the amounts of the sulfur-containing silane coupling agent and the alkylalkoxysilane compound satisfying the formulas (1) and (2), and therefore exhibit excellent scorch resistance without impairing wet grip performance compared to Reference Examples 1, 2, and 3. In contrast, in Comparative Example 1, (b / a) and (b / a) in the formulas (1) and (2) were 0.10 and c / b was 0.5, respectively, and therefore the scorch time was poor. In Comparative Example 2, (b / a) in the formulas (1) and (2) was 0.06 and c / b was 0.8, respectively, and therefore the scorch time was poor. In Comparative Example 3, (b / a) was 0.10 and c / b was 1.0 in the formulas (1) and (2), resulting in a worsening scorch time. In Comparative Example 4, c / b was 1.3 in the formulas (1) and (2), resulting in a worsening wet grip performance. In Comparative Example 5, (b / a) was 0.02 in the formulas (1) and (2), resulting in a worsening wet grip performance. In Comparative Example 6, (b / a) was 0.10 in the formulas (1) and (2), resulting in a worsening scorch time. In Comparative Example 7, (b / a) was 0.10 and c / b was 0.3 in the formulas (1) and (2), resulting in a worsening scorch time. In Comparative Example 8, (b / a) was 0.06 and c / b was 0.4 in the formulas (1) and (2), resulting in a worsening scorch time. In Comparative Example 9, (b / a) was 0.10 and c / b was 0.5 in the formulas (1) and (2), so the scorch time was poor. In Comparative Example 10, c / b was 0.6 in the formulas (1) and (2), so the wet grip performance was poor. In Comparative Example 11, (b / a) was 0.02 in the formulas (1) and (2), so the wet grip performance was poor.In Comparative Example 12, the (b / a) ratio in the formulas (1) and (2) was 0.10, resulting in a worsening scorch time. In Comparative Example 13, the (b / a) ratio in the formulas (1) and (2) was 0.10 and the c / b ratio was 0.3, resulting in a worsening scorch time. In Comparative Example 14, the (b / a) ratio in the formulas (1) and (2) was 0.06 and the c / b ratio was 0.3, resulting in a worsening scorch time. In Comparative Example 15, the (b / a) ratio in the formulas (1) and (2) was 0.10 and the c / b ratio was 0.7, resulting in a worsening scorch time. In Comparative Example 16, the c / b ratio in the formulas (1) and (2) was 0.8, resulting in a worsening wet grip performance. In Comparative Example 17, the (b / a) ratio in the formulas (1) and (2) was 0.02, resulting in a worsening wet grip performance. In Comparative Example 18, the (b / a) ratio in the formulas (1) and (2) was 0.10, and the scorch time was therefore poor.
[0039] The present invention includes the following embodiments: Embodiment 1: A rubber composition for a tire containing a diene rubber, silica, a sulfur-containing silane coupling agent, and an alkylalkoxysilane compound, wherein the amount of silica blended is 80 to 300 parts by mass per 100 parts by mass of the diene rubber, the alkylalkoxysilane compound is an alkyldiethoxysilane or an alkyltriethoxysilane, and the blending amounts of the sulfur-containing silane coupling agent and the alkylalkoxysilane compound satisfy the following formulas (1) and (2): 0.03<(b / a)<0.06 (1) c / b≧1.5 (2) In the formulas (1) and (2), a is the amount (parts by mass) of the silica per 100 parts by mass of the diene rubber, b is the amount (parts by mass) of the sulfur-containing silane coupling agent per 100 parts by mass of the diene rubber, and c is the amount (parts by mass) of the alkylalkoxysilane compound per 100 parts by mass of the diene rubber. Embodiment 2: The rubber composition for a tire according to Embodiment 1, wherein the sulfur-containing silane coupling agent is a sulfur-containing silane coupling agent having a mercapto group. Embodiment 3: The rubber composition for a tire according to Embodiment 1 or 2, further comprising 15 parts by mass or more of aluminum hydroxide per 100 parts by mass of the diene rubber. Embodiment 4: The rubber composition for a tire according to any one of Embodiments 1 to 3, wherein 70 parts by mass or more of styrene-butadiene copolymer rubber is contained per 100 parts by mass of the diene rubber. Embodiment 5: The rubber composition for a tire according to embodiment 4, wherein the styrene content of the styrene-butadiene copolymer rubber is 20 to 45 mass % and / or the glass transition temperature (Tg) is −60 to −10° C. Embodiment 6: The nitrogen adsorption specific surface area N 2 SA is 100 to 300m 2 / g. Embodiment 7: The rubber composition for a tire according to any one of embodiments 1 to 5, wherein the alkyl group in the alkyldiethoxysilane is a methyl group. Embodiment 8: The rubber composition for a tire according to any one of embodiments 1 to 6, wherein the alkyl group in the alkyltriethoxysilane is an alkyl group having 7 to 20 carbon atoms. Embodiment 9: A tire using the rubber composition for a tire according to any one of embodiments 1 to 8.
Claims
1. A rubber composition for tires containing a diene rubber, silica, a sulfur-containing silane coupling agent, and an alkylalkoxysilane compound, wherein the amount of silica is 80 to 300 parts by mass per 100 parts by mass of the diene rubber, the alkylalkoxysilane compound is an alkyldiethoxysilane or an alkyltriethoxysilane, and the amounts of the sulfur-containing silane coupling agent and the alkylalkoxysilane compound satisfy the following formulas (1) and (2): 0.03<(b / a)<0.06 (1) c / b≧1.5 (2) In the formulas (1) and (2), a is the amount (parts by mass) of the silica per 100 parts by mass of the diene rubber, b is the amount (parts by mass) of the sulfur-containing silane coupling agent per 100 parts by mass of the diene rubber, and c is the amount (parts by mass) of the alkylalkoxysilane compound per 100 parts by mass of the diene rubber.
2. The rubber composition for tires according to claim 1, characterized in that the sulfur-containing silane coupling agent is a sulfur-containing silane coupling agent having a mercapto group.
3. The rubber composition for tires according to claim 1, further comprising 15 parts by mass or more of aluminum hydroxide per 100 parts by mass of the diene rubber.
4. The rubber composition for tires according to claim 1, wherein the styrene-butadiene copolymer rubber accounts for 70 parts by mass or more per 100 parts by mass of the diene rubber.
5. The rubber composition for tires according to claim 4, characterized in that the styrene amount of the styrene-butadiene copolymer rubber is 20 to 45 mass % and / or the glass transition temperature (Tg) is -60 to -10°C.
6. The nitrogen adsorption specific surface area N of the silica 2 SA is 100-300m 2 The rubber composition for tires according to claim 1, wherein the viscosity is 100 / g.
7. The rubber composition for tires according to claim 1, wherein the alkyl group in said alkyldiethoxysilane is a methyl group.
8. A rubber composition for tires according to claim 1, characterized in that the alkyl group in said alkyltriethoxysilane is an alkyl group having 7 to 20 carbon atoms.
9. A tire using the rubber composition for tires according to claim 1.
Citation Information
Patent Citations
Pneumatic tire
JP2019104484A
Rubber composition for tire treads
JP5644838B2
Rubber composition for tire tread
JP5888361B2
Rubber composition for tires and pneumatic tires
JP6969243B2
pneumatic tires
JP7397272B2