Highly conductive film and manufacturing method therefor

The highly conductive film, featuring a polymer matrix, in-situ etched nano-satellite particles, and a specific cross-linking agent, addresses the limitations of conductive composite materials by enhancing electron tunneling and mechanical strength, resulting in superior electrical conductivity and stability under deformation.

WO2024248266A1PCT designated stage expired Publication Date: 2024-12-05RES & BUSINESS FOUND SUNGKYUNKWAN UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/000488
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-01
Filing Date
2024-01-10
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conductive composite materials face limitations in simultaneously achieving high electrical conductivity and mechanical strength due to the increased distance between micro-sized conductive fillers in polymer matrices, which reduces the efficient conductive path and electron tunneling barrier height.

Method used

A highly conductive film comprising a polymer matrix, conductive fillers with in-situ etched nano-satellite particles, and a cross-linking agent such as 2,5-dimethyl-2,5-di(t-butyl peroxy), methyl tris(methylethyl ketoximo) silane, which forms a non-contact percolation network to enhance electron tunneling and mechanical properties.

Benefits of technology

The film achieves significantly improved electrical conductivity and mechanical strength, with 4,200 times higher conductivity compared to non-crosslinked films, maintaining stability under 40% strain without resistance change, and exhibits excellent viscoelastic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024000488_05122024_PF_FP_ABST
    Figure KR2024000488_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The highly conductive film according to one embodiment of the present invention has excellent strength and electrical conductivity, by comprising: a polymer matrix; a conductive filler supported in the polymer matrix; and a cross-linking agent, wherein the cross-linking agent comprises at least one selected from the group consisting of 2,5-dimethyl-2,5-di (t-butyl peroxy), methyl tris (methylethyl ketoxymo) silane, ViBis-(N-methylbenzamido) methylethoxysilanenyl tris (methylethyl ketoxymo) silane, and methyltriacetoxy silane.
Need to check novelty before this filing date? Find Prior Art

Description

High-conductivity film and method for producing the same

[0001] The present invention relates to a high-conductivity film and a method for producing the same.

[0002] As the application fields of electronic devices expand, interest in flexible electronic devices—devices that maintain stable electrical properties and fully demonstrate their performance even under various deformations—is growing. In electronic devices requiring flexibility and stretchability, such as flexible displays, a key technology is forming stretchable electrodes without compromising mechanical properties like strength or electrical conductivity.

[0003] Meanwhile, metal nanomaterials generally refer to nano-sized metals such as gold, silver, copper, and nickel formed through chemical synthesis from metal ions using a reducing agent. These metal nanomaterials are useful because their shape and size can be appropriately controlled by controlling process conditions such as reaction time and temperature during the synthesis process. Furthermore, metal nanomaterials have higher electrical conductivity than bulk metal materials, and are therefore utilized in the development of materials requiring enhanced elasticity and electrical conductivity.

[0004] Accordingly, conductive fillers, such as the aforementioned metal nanomaterials, are being used to develop conductive composite materials that can connect individual components with highly conductive channels as elements for implementing flexible electronic devices. However, adding more than a certain amount of conductive filler to enhance conductivity can degrade mechanical properties, such as strength, thus limiting the improvement in electrical conductivity achieved through such conductive fillers.

[0005] Recently, conductive composites have been constructed by filling conductive fillers into a polymer matrix to simultaneously implement electrical conductivity and mechanical properties of such conductive composites. However, there are limitations in forming efficient conductive paths as the distance between micro-sized conductive fillers in the polymer matrix increases, or there is a limit to the height of the electron tunneling barrier when using a non-contact percolation network based on electron tunneling between conductive fillers.

[0006] For example, Korean Patent No. 1496156 discloses a conductive composite including a reduced graphene oxide plate-like structure having a nematic structure and a polymer permeated into the pores of the reduced graphene oxide plate-like structure.

[0007] [Prior Art Literature]

[0008] [Patent Document]

[0009] (Patent Document 1) Japanese Patent Publication No. 2016-115659

[0010] The problem to be solved by the present invention is to provide a highly conductive film having excellent strength and electrical conductivity and a method for producing the same, comprising: a polymer matrix; a conductive filler supported in the polymer matrix; and a crosslinking agent, wherein the crosslinking agent includes at least one selected from the group consisting of 2,5-dimethyl-2,5-di(t-butyl peroxy), methyl tris(methylethyl ketoxymo) silane, ViBis-(N-methylbenzamido)methylethoxysilaneyl tris(methylethyl ketoxymo) silane, and methyltriacetoxy silane.

[0011] However, the problems to be solved by the present invention are not limited to those mentioned above, and other problems to be solved that are not mentioned can be clearly understood by a person having ordinary skill in the art to which the present invention pertains from the description below.

[0012] A highly conductive film according to one embodiment of the present invention comprises a polymer matrix; a conductive filler supported in the polymer matrix; and a crosslinking agent, wherein the crosslinking agent comprises at least one selected from the group consisting of 2,5-dimethyl-2,5-di(t-butyl peroxy), methyl tris(methylethyl ketoxymo) silane, ViBis-(N-methylbenzamido)methylethoxysilaneyl tris(methylethyl ketoxymo) silane, and methyltriacetoxy silane.

[0013] Here, the crosslinking agent may be included in an amount of 2 wt% to 7.5 wt% based on the total weight of the high-conductivity film.

[0014] Additionally, the conductive filler may include a nanofiller and nanosatellite particles etched in-situ from the nanofiller, and a volume ratio of the nanofiller and the nanosatellite particles may be 1:0.01 to 0.5.

[0015] Here, the nano satellite particles may be obtained by in-situ etching of the nano filler by a redox reaction of an organic solvent, and the organic solvent may be selected from the group consisting of tetrahydrofuran (THF), tetrahydrofuran peroxide (THF peroxide), hydrogen peroxide (H2O2), HCl:FeCl3, HCl:K3[Fe(CN)6], HCl:Fe(NO3)3, HCl:HNO3, H2O:HNO3, and combinations thereof.

[0016] Additionally, the conductive filler may include a metal selected from the group consisting of Ag, Cu, Al, Au, Pt, Sn, Ni, Pb, Hg, Co, Cd, Fe, Cr, Zn, and combinations thereof.

[0017] Here, the conductive filler may have a shape selected from the group consisting of flake, sphere-type, flower-type, plate-type, and combinations thereof.

[0018] Here, the average particle size of the conductive filler may be 1 nm to 500 nm.

[0019] Here, the conductive filler may be included in an amount of 10% to 50% by volume based on the total volume of the high-conductivity film.

[0020] Additionally, the polymer matrix may include a polymer selected from the group consisting of silicone rubber, polyurethane rubber, acrylic rubber, styrene-butadiene rubber, nitrile rubber, polybutadiene rubber, chloroprene rubber, styrene-butadiene-vinylpyridine rubber, isoprene rubber, butyl rubber, ethylene-propylene rubber, polysulfide rubber, acrylic-butadiene rubber, fluororubber, and combinations thereof.

[0021] Here, the polymer matrix may be included in an amount of 10 wt% to 60 wt% based on the total weight of the high-conductivity film.

[0022] In addition, the high-conductivity film has a density of 4.5 g / cm 2 10 g / cm 2 It can be , and the electrical conductivity can be 0.0005 S / cm to 80,000 S / cm.

[0023] A method for manufacturing a highly conductive film according to another embodiment of the present invention comprises the steps of (1) preparing a polymer solution by dissolving a polymer matrix in an organic solvent; (2) adding an organic solvent and a conductive filler to the polymer solution and performing a primary dispersion; (3) adding a crosslinking agent and performing a secondary dispersion; and (4) drying, pressing, and curing, wherein the crosslinking agent comprises at least one selected from the group consisting of 2,5-dimethyl-2,5-di(t-butyl peroxy), methyl tris(methylethyl ketoxymo) silane, ViBis-(N-methylbenzamido)methylethoxysilaneyl tris(methylethyl ketoxymo) silane, and methyltriacetoxy silane.

[0024] In addition, in the step (4), the pressing can be performed at a temperature of 150°C to 200°C and a pressure of 0.5 MPa to 5 MPa for 5 to 30 minutes, and the curing can be performed at 180°C to 230°C for 1 to 6 hours.

[0025] Here, the step (1) may be dissolving the polymer matrix in an organic solvent at a concentration of 1 wt% to 30 wt%.

[0026] Additionally, in the step (2), the amount of the organic solvent added may be 500% to 1,000% by volume based on the total volume of the polymer solution, and the amount of the conductive filler added may be 50% to 150% by weight based on the total weight of the polymer solution.

[0027] Here, the first dispersion of step (2) and the second dispersion of step (3) can be performed by a method selected from the group consisting of ultrasonic stirring, stirring, shear mixing, 3-roll milling, and combinations thereof.

[0028] According to an embodiment of the present invention, a highly conductive film can efficiently improve electrical conductivity by including a polymer matrix and a conductive filler supported in the polymer matrix, specifically, a conductive filler including a nano filler and nano satellite particles etched in-situ from the nano filler.

[0029] More specifically, the nano-satellite particles, in-situ etched by the redox reaction of the nano-filler and the organic solvent, can form an efficient network in the form of satellites around the nano-filler, thereby efficiently improving electrical conductivity compared to conventional micro-fillers or simply mixed micro / nano heterogeneous fillers.

[0030] In particular, the high-conductivity film can further improve strength and electrical conductivity by including a crosslinking agent including at least one selected from the group consisting of 2,5-dimethyl-2,5-di(t-butyl peroxy), methyl tris(methylethyl ketoxymo) silane, ViBis-(N-methylbenzamido)methylethoxysilaneyl tris(methylethyl ketoxymo) silane, and methyltriacetoxy silane.

[0031] Specifically, even if the nano-filler forms an efficient network of in-situ etched nano-satellite particles in the form of satellites around the nano-filler, there is a limit to improving mechanical properties such as strength due to the porous putty-like viscoelastic properties. However, the highly conductive film according to one embodiment of the present invention can maximize the non-contact percolation network based on electron tunneling by including a specific cross-linking agent, thereby efficiently controlling electron affinity and lowering the barrier height of electron tunneling, thereby securing excellent strength and electrical conductivity.

[0032] More specifically, a highly conductive film according to an embodiment of the present invention can secure excellent strength and electrical conductivity by narrowing the tunneling distance between conductive fillers by generating nano-satellite particles etched in-situ from nano-fillers, and improving the tunneling network by controlling the electron affinity through a cross-linking method using a specific cross-linking agent to make the electron tunneling barrier height negligible. In particular, compared to a non-cross-linked highly conductive film, the cross-linked highly conductive film is non-porous and has an electrical conductivity 4,200 times higher, and has almost no change in resistance even at a strain of 40%, so that high electrical conductivity can be stably maintained even after shape deformation.

[0033] Figure 1 shows a high-resolution transmission electron microscopy (HRTEM) image of the high-conductivity film of Example 1.

[0034] Figure 2 shows the electron affinity and work function of AgFL of the high-conductivity films of Examples 1 to 4.

[0035] Figure 3 shows the electrical conductivity of the high-conductivity films of Examples 1 and 5 to 7.

[0036] Figure 4 shows the electrical conductivity of the high-conductivity films of Example 1 and Comparative Example 1.

[0037] Figure 5 shows the high-conductivity films of Example 1 and Comparative Example 1.

[0038] The advantages and features of the present invention, and the methods for achieving them, will become clearer with reference to the embodiments described in detail below together with the accompanying drawings. However, the present invention is not limited to the embodiments disclosed below and may be implemented in various different forms. These embodiments are provided solely to ensure that the disclosure of the present invention is complete and to fully inform those skilled in the art of the scope of the invention, and the present invention is defined solely by the scope of the claims.

[0039] When describing embodiments of the present invention, detailed descriptions of known functions or configurations will be omitted if they are deemed to unnecessarily obscure the gist of the invention. Furthermore, the terms described below are defined in light of their functions in the embodiments of the present invention and may vary depending on the intent or custom of the user or operator. Therefore, their definitions should be based on the overall content of this specification.

[0040]

[0041] High-conductivity film

[0042] A highly conductive film according to one embodiment of the present invention comprises a polymer matrix; a conductive filler supported in the polymer matrix; and a crosslinking agent, wherein the crosslinking agent comprises at least one selected from the group consisting of 2,5-dimethyl-2,5-di(t-butyl peroxy), methyl tris(methylethyl ketoxymo) silane, ViBis-(N-methylbenzamido)methylethoxysilaneyl tris(methylethyl ketoxymo) silane, and methyltriacetoxy silane.

[0043] The high-conductivity film may contain the cross-linking agent in an amount of 2 wt% to 7.5 wt% based on the total weight of the high-conductivity film. For example, the content of the cross-linking agent may be 2.5 wt% to 7.5 wt%, 5 wt% to 7.5 wt%, or 6 wt% to 7 wt% based on the total weight of the high-conductivity film. By satisfying the content of the cross-linking agent within the above range, the work function and energy level of the conductive filler may be similar, thereby maximizing the improvement in electrical conductivity.

[0044] In addition, the conductive filler may include a nanofiller and nanosatellite particles etched in-situ from the nanofiller. At this time, the volume ratio of the nanofiller and the nanosatellite particles may be 1:0.01 to 0.5. For example, the volume ratio of the nanofiller and the nanosatellite particles may be 1:0.05 to 0.3, 1:0.07 to 0.2, or 1:0.09 to 0.16. When the content of the nanofiller and the nanosatellite particles etched in-situ from the nanofiller satisfies the above range, the improvement in electrical conductivity can be maximized.

[0045] The above nanosatellite particles may be formed by in-situ etching of the nanofiller through a redox reaction of an organic solvent. Specifically, the nanosatellite particles may be arranged in a satellite shape to form a network around the nanofiller, but the present invention is not limited thereto.

[0046] Specifically, through a redox reaction between a conductive filler and an organic solvent used for its dispersion, nano-satellite particles in situ formed from the surface of the nano-filler can form a satellite shape around the nano-filler and form a percolation network. That is, the highly conductive film according to an embodiment of the present invention can effectively and stably form a conductive network even in a room-temperature mixing process without additional heat treatment, thereby efficiently improving the electrical conductivity of the conductive composite compared to the conventional micro-filler or simply mixed micro / nano heterogeneous filler.

[0047] The organic solvent may be selected from the group consisting of tetrahydrofuran (THF), tetrahydrofuran peroxide (THF peroxide), hydrogen peroxide (H2O2), HCl:FeCl3, HCl:K3[Fe(CN)6], HCl:Fe(NO3)3, HCl:HNO3, H2O:HNO3, and combinations thereof. The organic solvent must include a solvent that is reactive with a metal and can etch the metal, and tetrahydrofuran (THF) or tetrahydrofuran peroxide (THF peroxide) may be preferable as the organic solvent, but is not limited thereto.

[0048] Additionally, the conductive filler may include a metal selected from the group consisting of Ag, Cu, Al, Au, Pt, Sn, Ni, Pb, Hg, Co, Cd, Fe, Cr, Zn, and combinations thereof. The conductive filler may preferably include Ag, but is not limited thereto.

[0049] The conductive filler may have a shape selected from the group consisting of flake, sphere-type, flower-type, plate-type, and combinations thereof. The conductive filler may preferably have a flake shape, but is not limited thereto.

[0050] The average particle size of the conductive filler may be 1 nm to 500 nm. For example, the average particle size of the conductive filler may be 1 nm to 400 nm, 1 nm to 300 nm, 1 nm to 200 nm, 5 nm to 500 nm, 5 nm to 350 nm, 5 nm to 150 nm, 10 nm to 500 nm, 15 nm to 500 nm, 20 nm to 450 nm, 25 nm to 450 nm, 30 nm to 400 nm, 35 nm to 400 nm, 40 nm to 350 nm, or 50 nm to 300 nm.

[0051] The high-conductivity film may contain the conductive filler in an amount of 10% to 50% by volume based on the total volume of the high-conductivity film. For example, the content of the conductive filler may be 15% to 50% by volume, 25% to 48% by volume, 30% to 46% by volume, or 35% to 45% by volume based on the total volume of the high-conductivity film.

[0052] Additionally, the polymer matrix may include a polymer selected from the group consisting of silicone rubber, polyurethane rubber, acrylic rubber, styrene-butadiene rubber, nitrile rubber, polybutadiene rubber, chloroprene rubber, styrene-butadiene-vinylpyridine rubber, isoprene rubber, butyl rubber, ethylene-propylene rubber, polysulfide rubber, acrylic-butadiene rubber, fluororubber, and combinations thereof. The polymer matrix may preferably include silicone rubber, but is not limited thereto, in that it is desirable to have a certain level of flexibility, such as viscoelasticity or elasticity.

[0053] The high-conductivity film may contain the polymer matrix in an amount of 10 wt% to 60 wt% based on the total weight of the high-conductivity film. For example, the content of the polymer matrix may be 15 wt% to 55 wt%, 25 wt% to 50 wt%, or 30 wt% to 45 wt% based on the total weight of the high-conductivity film.

[0054] In addition, the high-conductivity film has a density of 4.5 g / cm 2 10 g / cm 2 It can be. For example, the density of the high-conductivity film is 4.5 g / cm 2 9 g / cm 2 or 5 g / cm 2 8 g / cm 2 It could be.

[0055] The high-conductivity film may have an electrical conductivity of 0.0005 S / cm to 80,000 S / cm. For example, the high-conductivity film may have an electrical conductivity of 0.001 S / cm to 30,000 S / cm, 0.005 S / cm to 10,000 S / cm, 0.01 S / cm to 5,000 S / cm, 0.05 S / cm to 3,000 S / cm, 0.1 S / cm to 1,000 S / cm, 0.5 to 800 S / cm, 1 S / cm to 500 S / cm, 10 S / cm to 400 S / cm, or 10 S / cm to 300 S / cm.

[0056]

[0057] Method for manufacturing a high-conductivity film

[0058] A method for manufacturing a highly conductive film according to another embodiment of the present invention comprises the steps of (1) preparing a polymer solution by dissolving a polymer matrix in an organic solvent; (2) adding an organic solvent and a conductive filler to the polymer solution and performing a primary dispersion; (3) adding a crosslinking agent and performing a secondary dispersion; and (4) drying, pressing, and curing, wherein the crosslinking agent comprises at least one selected from the group consisting of 2,5-dimethyl-2,5-di(t-butyl peroxy), methyl tris(methylethyl ketoxymo) silane, ViBis-(N-methylbenzamido)methylethoxysilaneyl tris(methylethyl ketoxymo) silane, and methyltriacetoxysilane.

[0059] Step (1) of preparing a polymer solution by dissolving a polymer matrix in an organic solvent

[0060] A method for producing a high-conductivity film according to another embodiment of the present invention includes a step of preparing a polymer solution by dissolving a polymer matrix in an organic solvent.

[0061] The description of the polymer matrix and organic solvent is as described above.

[0062] In addition, the step (1) may be dissolving the polymer matrix in an organic solvent at a concentration of 1 wt% to 30 wt%. For example, the polymer solution may be prepared by dissolving the polymer matrix in the organic solvent at a concentration of 1 wt% to 25 wt%, 5 wt% to 20 wt%, or 10 wt% to 20 wt%.

[0063] Step (2) of adding an organic solvent and a conductive filler to the above polymer solution and performing primary dispersion

[0064] A method for manufacturing a highly conductive film according to another embodiment of the present invention includes a step of adding an organic solvent and a conductive filler to the polymer solution and performing a first dispersion.

[0065] The description of the above conductive filler is as described above.

[0066] The organic solvent used in the above step (2) may be a peroxide of the organic solvent used in the above step (1). For example, tetrahydrofuran may be used in the above step (1), and peroxidized tetrahydrofuran, i.e., tetrahydrofuran peroxide, may be used in the above step (2), but is not limited thereto.

[0067] In the above step (2), the amount of the organic solvent added may be 500% to 1,000% by volume based on the total volume of the polymer solution, and the amount of the conductive filler added may be 50% to 150% by weight based on the total weight of the polymer solution.

[0068] For example, in the step (2), the amount of the organic solvent added may be 600% to 850% by volume or 650% to 800% by volume based on the total volume of the polymer solution prepared in the step (1), and the amount of the conductive filler added may be 60% to 130% by weight, 70% to 120% by weight, or 80% to 110% by weight based on the total weight of the polymer solution prepared in the step (1).

[0069] The above primary dispersion may be performed by a method selected from the group consisting of ultrasonic stirring, stirring, shear mixing, 3-roll milling, and combinations thereof. For example, the above primary dispersion may be performed using a top sonicator, but is not limited thereto.

[0070] Step (3) of adding a cross-linking agent and performing secondary dispersion

[0071] A method for manufacturing a high-conductivity film according to another embodiment of the present invention includes a step of introducing a cross-linking agent and performing secondary dispersion.

[0072] The description of the above cross-linking agent is as described above.

[0073] The above secondary dispersion can be performed by a method selected from the group consisting of ultrasonic stirring, stirring, shear mixing, 3-roll milling, and combinations thereof.

[0074] Drying, pressing and curing steps (4)

[0075] A method for manufacturing a high-conductivity film according to another embodiment of the present invention includes the steps of drying, pressing and curing.

[0076] In the above step (4), the pressing can be performed at a temperature of 150°C to 200°C and a pressure of 0.5 MPa to 5 MPa for 1 to 15 minutes, and the curing can be performed at 180°C to 230°C for 1 to 6 hours.

[0077] For example, the pressing can be performed using a hot press at a temperature of 155°C to 185°C or 160°C to 180°C and a pressure of 0.5 MPa to 3.5 MPa or 1 MPa to 3 MPa for 3 to 12 minutes or 5 to 10 minutes, and the curing can be performed at 185°C to 220°C or 190°C to 210°C for 2 to 6 hours or 2.5 to 5 hours.

[0078] The above contents are explained in more detail with the following examples. However, the following examples are only intended to illustrate the present invention, and the scope of the examples is not limited to these examples.

[0079]

[0080] [Example]

[0081] Manufacturing of high-conductivity films

[0082] Example 1

[0083] A polymer solution was prepared by dissolving silicone rubber in tetrahydrofuran at a concentration of 15 wt%. Subsequently, 15 ml of peroxidized tetrahydrofuran and 2.1 g of silver nanoflakes (AgFL) were added to 2 g of the polymer solution, and primary dispersion was performed using a tip sonicator at 420 W for 10 minutes. Subsequently, 0.262 g of 2,5-dimethyl-2,5-di(t-butyl peroxy) (dissolved in hexane at a concentration of 8 wt%) as a crosslinking agent was added, and secondary dispersion was performed at 300 rpm for 60 minutes. Subsequently, drop casting was performed for drying for one day, and then compression was performed using a hot press at 170°C and 2 MPa of pressure for 10 minutes, followed by curing at 200°C for 4 hours to produce a highly conductive film. At this time, the high-conductivity film included silver nanoflakes (AgFL) and silver nanosatellite particles (AgNS) etched in-situ from the silver nanoflakes.

[0084]

[0085] Examples 2 to 4

[0086] A high-conductivity film was manufactured in the same manner as in Example 1, except that the content of the cross-linking agent was changed as shown in Table 1 below.

[0087]

[0088] Examples 5 to 7

[0089] A high-conductivity film was manufactured in the same manner as in Example 1, except that the total content and volume ratio of AgFL-AgNS were changed by changing the content of peroxidized tetrahydrofuran and silver nanoflake (AgFL), as shown in Table 1 below.

[0090]

[0091] Comparative Example 1

[0092] A high-conductivity film was manufactured in the same manner as in Example 1, except that no cross-linking agent was added.

[0093]

[0094] Content of cross-linking agent (weight%) AgFL-AgNS total content (volume%) Volume ratio of AgFL and AgNS Example 1740 35.75 : 4.25 Example 2240 35.75 : 4.25 Example 3640 35.75 : 4.25 Example 47.5 40 35.75 : 4.25 Example 5736 33.00 : 3.00 Example 6738 34.50 : 3.50 Example 7742 36.50 : 5.50 Comparative Example 1-40 35.75 : 4.25

[0095]

[0096] Experimental Example 1: HRTEM image

[0097] For the high-conductivity films of Examples 1 to 7 and Comparative Example 1, images were obtained using a high-resolution transmission electron microscope (HRTEM). At this time, images were obtained at 200 kV using a JEM ARM 200F device.

[0098] Figure 1 shows a high-resolution transmission electron microscopy (HRTEM) image of the highly conductive film of Example 1. As shown in Figure 1, it was confirmed that silver nanoflakes (AgFL) were in-situ etched by peroxidized tetrahydrofuran to produce silver nanosatellite particles (AgNS). Specifically, the silver nanosatellite particles (AgNS) had a bimodal size distribution, and the inter-particle distance was very short, less than 4 nm.

[0099]

[0100] Experimental Example 2: Electron Affinity and Work Function of AgFL

[0101] For the highly conductive films of Examples 1 to 7 and Comparative Example 1, the electron affinity and work function of AgFL were measured using Kelvin probe force microscopy (KPFM). At this time, a Nanonavi-E-sweep device was used.

[0102] Figure 2 shows the electron affinity and AgFL work function of the high-conductivity films of Examples 1 to 4. As can be seen in Figure 2, it can be confirmed that the electron affinity and AgFL work function of the high-conductivity films vary depending on the content of the cross-linking agent, and the high-conductivity film of Example 1 with a cross-linking agent content of 7 wt% was the best in terms of electron affinity and AgFL work function.

[0103] Specifically, the average work function of AgFL was measured to be 4.70 eV, the electron affinity of Example 1 with a cross-linking agent content of 7 wt% was measured to be 4.62 eV, and the electron affinity of Example 4 with a cross-linking agent content of 7.5 wt% was measured to be 4.73 eV, so it was confirmed that the tunneling barrier height can be ignored when the cross-linking agent content is 7 wt% or less.

[0104]

[0105] Experimental Example 3: Electrical Conductivity

[0106] For the high-conductivity films of Examples 1 to 7 and Comparative Example 1, electrical conductivity was measured using the Four points method using a Four points probe.

[0107] Figure 3 shows the electrical conductivity of the high-conductivity films of Examples 1 and 5 to 7. As can be seen in Figure 3, it can be confirmed that the electrical conductivity of the high-conductivity film varies depending on the total content and volume ratio of AgFL-AgNS in the high-conductivity film, and the higher the total content of AgFL-AgNS or the content ratio of AgNS, the better the electrical conductivity.

[0108] Figure 4 shows the electrical conductivity of the high-conductivity films of Example 1 and Comparative Example 1. As seen in Figure 4, the electrical conductivity (61,451 S / cm) of the high-conductivity film of Example 1 manufactured using a crosslinking agent was much superior to that of Comparative Example 1 (32,401 S / cm).

[0109]

[0110] Experimental Example 4: Flexibility

[0111] Figure 5 shows the high-conductivity films of Example 1 and Comparative Example 1. As seen in Figure 5, the high-conductivity film of Example 1 had superior flexibility compared to Comparative Example 1.

Claims

1. Polymer matrix; a conductive filler supported in the polymer matrix; and Contains a cross-linking agent, A highly conductive film, wherein the crosslinking agent comprises at least one selected from the group consisting of 2,5-dimethyl-2,5-di(t-butyl peroxy), methyl tris(methylethyl ketoxymo) silane, ViBis-(N-methylbenzamido)methylethoxysilaneyl tris(methylethyl ketoxymo) silane, and methyltriacetoxy silane.

2. In paragraph 1, A high-conductivity film comprising 2 to 7.5 wt% of the cross-linking agent based on the total weight of the high-conductivity film.

3. In paragraph 1, The conductive filler comprises a nano-filler and nano-satellite particles etched in-situ from the nano-filler, A highly conductive film, wherein the volume ratio of the nano filler and the nano satellite particles is 1:0.01 to 0.

5.

4. In paragraph 3, The above nano satellite particles are in-situ etched nano fillers by a redox reaction of an organic solvent, A highly conductive film, wherein the organic solvent is selected from the group consisting of tetrahydrofuran (THF), tetrahydrofuran peroxide (THF peroxide), hydrogen peroxide (H2O2), HCl:FeCl3, HCl:K3[Fe(CN)6], HCl:Fe(NO3)3, HCl:HNO3, H2O:HNO3, and combinations thereof.

5. In paragraph 1, A highly conductive film, wherein the conductive filler comprises a metal selected from the group consisting of Ag, Cu, Al, Au, Pt, Sn, Ni, Pb, Hg, Co, Cd, Fe, Cr, Zn and combinations thereof.

6. In paragraph 1, A highly conductive film, wherein the conductive filler has a shape selected from the group consisting of flake, sphere-type, flower-type, plate-type, and combinations thereof.

7. In paragraph 1, A highly conductive film, wherein the average particle size of the conductive filler is 1 nm to 500 nm.

8. In paragraph 1, A high-conductivity film comprising the conductive filler in an amount of 10% to 50% by volume based on the total volume of the high-conductivity film.

9. In paragraph 1, A highly conductive film, wherein the polymer matrix comprises a polymer selected from the group consisting of silicone rubber, polyurethane rubber, acrylic rubber, styrene-butadiene rubber, nitrile rubber, polybutadiene rubber, chloroprene rubber, styrene-butadiene-vinylpyridine rubber, isoprene rubber, butyl rubber, ethylene-propylene rubber, polysulfide rubber, acrylic-butadiene rubber, fluororubber, and combinations thereof.

10. In paragraph 1, A high-conductivity film comprising 10 to 60 wt% of the polymer matrix based on the total weight of the high-conductivity film.

11. In paragraph 1, The above high-conductivity film has a density of 4.5 g / cm 2 10 g / cm 2 A high-conductivity film having an electrical conductivity of 1 S / cm to 75,000 S / cm. 12.(1) A step of preparing a polymer solution by dissolving a polymer matrix in an organic solvent; (2) A step of adding an organic solvent and a conductive filler to the polymer solution and performing a primary dispersion; (3) Step of adding a cross-linking agent and performing secondary dispersion; and (4) Includes drying, pressing and curing steps, A method for producing a highly conductive film, wherein the crosslinking agent comprises at least one selected from the group consisting of 2,5-dimethyl-2,5-di(t-butyl peroxy), methyl tris(methylethyl ketoxymo) silane, ViBis-(N-methylbenzamido)methylethoxysilaneyl tris(methylethyl ketoxymo) silane, and methyltriacetoxy silane.

13. In paragraph 12, A method for producing a highly conductive film, wherein in the step (4), the pressing is performed at a temperature of 150°C to 200°C and a pressure of 0.5 MPa to 5 MPa for 1 to 15 minutes, and the curing is performed at 180°C to 230°C for 1 to 6 hours.

14. In paragraph 12, The above step (1) is a method for producing a highly conductive film, wherein the polymer matrix is ​​dissolved in an organic solvent at a concentration of 1 wt% to 30 wt%.

15. In paragraph 12, A method for producing a highly conductive film, wherein in the above step (2), the amount of the organic solvent added is 500% to 1,000% by volume based on the total volume of the polymer solution, and the amount of the conductive filler added is 50% to 150% by weight based on the total weight of the polymer solution.

16. In paragraph 12, A method for producing a highly conductive film, wherein the first dispersion of the above step (2) and the second dispersion of the above step (3) are each performed by a method selected from the group consisting of ultrasonic stirring, stirring, shear mixing, 3-roll milling, and combinations thereof.

Citation Information

Patent Citations

  • A rubber-based nonlinear conductive insulating material and its processing method

    CN108299741B

  • Hot-pressing buffer silicone rubber sheet and manufacturing method thereof

    CN112300577A

  • Conductive elastomer film, method for productionthereof, and conductive elastomer composition

    KR1020000076164A

  • Curable electroconductive adhesive composition, electromagnetic shielding film, electroconductive adhesive film, adhesion method, and circuit board

    KR1020150035604A

  • Conductive composites and electrionic device including the same

    KR102129415B1