Method for producing recycled EPS pellets having diameter of 1 mm or less and length of 1 mm or less from waste styrofoam by strand cutting
The method of adding SBS to waste EPS and using a cutting machine to produce 1 mm or less pellets addresses the challenge of recycling Styrofoam by maintaining physical properties, enabling efficient and sustainable reuse of recycled EPS pellets.
Patent Information
- Application Number
- PCT/KR2024/002086
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-02
- Filing Date
- 2024-02-14
- Publication Date
- 2024-12-05
AI Technical Summary
Existing methods for recycling waste Styrofoam struggle to produce pellets with a diameter and length of 1 mm or less, which are necessary for regenerating Styrofoam with similar physical properties to the original, due to difficulties in manufacturing and processing that result in reduced impact strength and elongation.
A method involving the addition of styrene-butadiene-styrene (SBS) to waste EPS, extrusion, and strand cutting using a specific cutting machine with rotating blades to achieve pellets of 1 mm or less in diameter and length, while maintaining the physical properties of the original Styrofoam.
The method effectively produces recycled EPS pellets with improved impact strength and elongation, suitable for reuse in various applications, enhancing both economic efficiency and environmental sustainability through resource recycling.
Smart Images

Figure KR2024002086_05122024_PF_FP_ABST
Abstract
Description
Method for manufacturing recycled EPS pellets with a diameter and length of 1 mm or less by strand cutting from waste Styrofoam
[0001] The present invention relates to a method for manufacturing recycled EPS pellets having a diameter and length of 1 mm or less by strand cutting from waste Styrofoam, wherein waste Styrofoam is formed into strands and then cut to manufacture pellets having a diameter and length of 1 mm or less, thereby enabling them to be reused as expanded styrene.
[0002] EPS (Expanded Polystyrene) is made by injecting hydrocarbon gases such as pentane and butane as a blowing agent into polystyrene resin and then expanding it with steam. It is commonly called styrofoam and is widely used in various fields such as cushioning materials, packaging materials, and building insulation materials.
[0003] Because Styrofoam is used in so many different ways, vast quantities are discarded. However, because it does not rot or decompose, it is either landfilled or incinerated. However, landfilling Styrofoam not only negatively impacts the ecosystem because it takes a long time to decompose, but also requires massive landfills. Furthermore, incineration of Styrofoam produces toxic gases and smoke, negatively impacting the environment.
[0004] Accordingly, various methods for recycling Styrofoam have been proposed. For example, Patent Document 0001 (Korean Patent Publication No. 10-0710044) relates to an insulating material using waste Styrofoam and a method for manufacturing the same. The patent document discloses a method of manufacturing an insulating material by crushing waste Styrofoam, mixing it with limestone powder, water, an organic solvent, silicone rubber, and an adhesive containing an emulsifying surfactant, and pressing and drying the mixture in a mold.
[0005] However, the recycling of waste Styrofoam according to the above patent document 0001 only involves crushing waste Styrofoam, adding functional materials, and then compressing the waste Styrofoam, so it cannot be a fundamental recycling method for waste Styrofoam and cannot be widely utilized in various fields.
[0006] Another method is EPS recycling through volume reduction. Volume reduction of EPS packaging material typically involves heating the EPS to remove the foaming gas, thereby recovering polystyrene with a reduced volume. This reduced volume makes it easier to transport overseas. However, since the physical properties of waste EPS packaging material deteriorate during the volume reduction process, recycled EPS through volume reduction is difficult to use for the same purpose as the EPS before disposal. Furthermore, a polymerization process is required to regenerate waste EPS into Styrofoam for the same purpose as before disposal. For polymerization, waste Styrofoam must be manufactured into pellets with a diameter and length of 1 mm or less, but manufacturing waste Styrofoam into pellets of 1 mm or less is quite difficult.
[0007] In this regard, Patent Document 0002 (Korean Patent Publication No. 10-1497017) relates to a process for manufacturing pellets from waste Styrofoam, which first reduces waste Styrofoam to obtain a polystyrene resin melt with a reduced volume, then adds a foaming agent, an antioxidant, and other additives to the molten polystyrene resin and extrusion-moldes it to manufacture an ingot cake, and then reprocesses the ingot cake into a polystyrene ingot pellet, thereby disclosing that waste Styrofoam can be regenerated into a standardized pellet shape suitable for transportation and handling without chemically changing the polystyrene, which is the material of the Styrofoam.
[0008] However, since the above patent document 0002 only improves the ease of transportation by continuously winding and rotating extruded polystyrene ingot pellets in a circular shape around a reference axis, even if polystyrene is manufactured as a strand, the technical features of patent document 0002 make it impossible to manufacture it with a diameter and length of 1 mm or less, and it is difficult to expect recovery of the reduced molecular weight and increase in physical properties, so it is difficult to regenerate the pellets into Styrofoam for the same purpose.
[0009] Patent Document 0003 (Japanese Patent Laid-Open No. 1999-226955) discloses that by pre-compressing shredded waste styrofoam, then melt-mixing it with an extruder, and then further degassing it, strands can be discharged without breaking, thereby improving the molding efficiency of pellets compared to the conventional process of directly feeding shredded expanded polystyrene into the extruder. However, Patent Document 003 only states that strands can be manufactured without breaking, and does not disclose the diameter of the strands or the diameter size of the pellets. Furthermore, even if the strands can be manufactured to have a diameter of 1 mm or less, cutting them to manufacture pellets with a length of 1 mm or less requires considerable technology, and thus remains a problem to be solved.
[0010] Therefore, there is a need to develop a new method for recycling waste EPS that can manufacture pellets of 1 mm or less in both diameter and length through strand cutting while preventing the phenomenon of reduction in impact strength and elongation in the recycling process (extrusion and melting process) so that waste Styrofoam can be recycled and applied to the same properties and fields as the Styrofoam before disposal.
[0011] [Prior Art Literature]
[0012] [Patent Document]
[0013] (Patent Document 1) Korean Patent No. 10-0710044 (Registration Date: April 16, 2007)
[0014] (Patent Document 2) Korean Patent No. 10-1497017 (Registration Date: February 23, 2015)
[0015] (Patent Document 3) Japanese Patent Publication No. 1999-226955 (Published: August 24, 1998)
[0016] In order to solve the above problems, the present invention provides a method for producing recycled EPS pellets having a diameter and length of 1 mm or less from waste Styrofoam, which produces recycled EPS pellets having a diameter and length of 1 mm or less through strand cutting from waste Styrofoam while preventing deterioration of physical properties such as elongation and impact strength, and recycled EPS pellets produced by the above production method.
[0017] In order to solve the above problem, the present invention provides, in one aspect, a method for manufacturing a strand having a diameter of 1 mm or less from waste Styrofoam and then cutting the strand to manufacture a recycled EPS pellet having a length of 1 mm or less, comprising the steps of: (a) crushing an ingot manufactured from waste EPS and mixing 1 to 5 parts by weight of styrene-butadiene-styrene (SBS) with respect to 100 parts by weight of the ingot; (b) introducing the mixture of step (a) into an extruder, melting and kneading the mixture, and extruding a strand having a diameter of 1 mm or less; (c) cooling the strand extruded in step (b) so that the surface temperature of the strand becomes 70 to 80°C when it is introduced into a roller of a cutting machine; And (d) a step of introducing the cooled strands in step (c) into a cutting machine and cutting them to a diameter and length of 1 mm or less; wherein the cutting machine in step (d) comprises a roller part including an upper roller and a lower roller; and a cutting part including a rotating body having a fixed blade and one or more rotating blades to cut the strands at the fixed blades by rotation of the rotating blades; and a distance from a point (A1) where the strands first come into contact with the lower roller to a blade edge (B1) of the rotating blade is 70 to 80 mm, and a point (C1) where the blade edge (B1) of the rotating blade comes into contact with the introduced strand is characterized in that the straight direction in which the strands move and the rear blade portion of the rotating blade have an angle of 5 to 10 degrees.
[0018] In one embodiment, the ingot may be manufactured by including the steps of (1) crushing waste EPS; and (2) reducing the crushed waste EPS, and then extruding and cooling the same to manufacture an ingot; wherein the reducing may be performed by thermal melting or solvent dissolution.
[0019] In one embodiment, the lower roller and the rotating body may be driven by two different axes, and the diameter of the lower roller may be 40 to 50 mm.
[0020] In one embodiment, the rotation speed of the lower roller in step (d) may be 300 to 600 rpm, and the surface linear speed of the rotating body may be 10 to 16 m / sec.
[0021] In addition, the present invention provides recycled EPS pellets having a diameter and length of 1 mm or less, manufactured from waste Styrofoam according to the above manufacturing method.
[0022] The present invention can prevent deterioration of physical properties caused by extrusion and melting processes when regenerating waste Styrofoam (waste EPS), thereby producing a regenerated EPS raw material having physical properties similar to or improved upon those of the EPS before disposal, and furthermore, can produce the regenerated EPS raw material into a pellet form having a diameter and length of 1 mm or less through strand cutting.
[0023] Therefore, the recycled EPS pellets having a diameter and length of 1 mm or less manufactured from waste EPS according to the present invention can be used as seeds in polymerization or composite manufacturing with various compounds such as polymers and foaming agents, and can be widely used in the same field as the waste EPS or in various fields, thereby improving both economic efficiency and environmental friendliness in terms of resource recycling.
[0024] Fig. 1 is a photograph showing a part of a cutting machine according to one embodiment of the present invention.
[0025] FIG. 2 is a diagram illustrating the angle formed when a rotating blade and a strand come into contact according to one embodiment of the present invention.
[0026] Hereinafter, the composition of the present invention, including preferred embodiments that can be easily implemented by those skilled in the art to which the present invention pertains, will be described in detail. In detailing the principles of the preferred embodiments of the present invention, if a detailed description of a related, known function or configuration is judged to unnecessarily obscure the gist of the present invention, such detailed description will be omitted.
[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. In general, the nomenclature used herein is well known and commonly used in the art.
[0028] Throughout this specification, whenever a part is said to "include" a component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise specifically stated.
[0029] In one aspect, the present invention provides a method for manufacturing a strand having a diameter of 1 mm or less from waste Styrofoam and then cutting the strand to manufacture a recycled EPS pellet having a length of 1 mm or less, comprising the steps of: (a) crushing an ingot manufactured from waste EPS and mixing 1 to 5 parts by weight of styrene-butadiene-styrene (SBS) with respect to 100 parts by weight of the ingot; (b) introducing the mixture of step (a) into an extruder, melting and kneading the mixture, and extruding a strand having a diameter of 1 mm or less; (c) cooling the strand extruded in step (b) so that the surface temperature of the strand becomes 70 to 80°C when it is introduced into a roller of a cutting machine; And (d) a step of introducing the cooled strands in step (c) into a cutting machine and cutting them to a diameter and length of 1 mm or less; wherein the cutting machine in step (d) includes a roller part including an upper roller and a lower roller; and a cutting part including a rotating body having a fixed blade and one or more rotating blades, and cutting the strands at the fixed blade by rotation of the rotating blade; and the distance from the point (A1) where the strand first comes into contact with the lower roller to the tip (B1) of the rotating blade is 70 to 80 mm, and the angle between the straight direction in which the strand moves and the rear blade portion of the rotating blade at the point (C1) where the tip (B1) of the rotating blade comes into contact with the introduced strand is 5 to 10°, and the present invention provides a method for manufacturing recycled EPS pellets having a diameter and length of 1 mm or less by strand cutting from waste Styrofoam.
[0030] In the present invention, step (a) is a step of crushing an ingot manufactured from waste EPS, and then mixing 1 to 5 parts by weight of styrene-butadiene-styrene (SBS) with respect to 100 parts by weight of the ingot, wherein the ingot is crushed so that it can be mixed and melted with other components, and then 1 to 5 parts by weight of SBS is mixed with respect to 100 parts by weight of the ingot, thereby preventing the waste EPS from being decomposed and its properties from being deteriorated during the extrusion and melting process for regenerating the waste EPS.
[0031] Specifically, the SBS is added to prevent or supplement the elongation and impact strength of the waste EPS from deteriorating during the extrusion and melting process for regenerating the waste EPS, and is included in an amount of 1 to 5 parts by weight per 100 parts by weight of the ingot, thereby improving the elongation and impact strength of the recycled EPS raw material to a level similar to or higher than that of the EPS before disposal, while maintaining the foaming effect and shape of the Styrofoam constant.
[0032] In the above step (a), additional additives may be mixed to add functionality. For example, for 100 parts by weight of the ingot, 0.1 to 0.5 parts by weight of an antioxidant may be further added to prevent the waste EPS from being oxidized or / and decomposed during the regeneration process. The antioxidant may be a phenol-based, amine-based, sulfur-based, phosphorus-based, etc., and any commonly used antioxidant may be applied, so the type is not limited.
[0033] As another example, for 100 parts by weight of the above ingot, 0.1 to 0.5 parts by weight of a heat stabilizer can be further mixed to prevent the physical properties from being deteriorated by shear stress during the extrusion process of the waste EPS. The heat stabilizer can be a commonly used material, and its type is not limited.
[0034] In addition, it may further include other additives such as antibacterial agents, flame retardants, coupling agents, light stabilizers, anti-slip agents, and colorants.
[0035] In the above step (a), the ingot can be manufactured by including (1) a step of crushing waste EPS; and (2) a step of reducing the crushed waste EPS, and then extruding and cooling it to manufacture an ingot.
[0036] Specifically, the step (1) above is a step of crushing waste EPS, a step of crushing the collected waste EPS into small particles of 50 to 100 mm in size or crystal particles of small grains forming waste EPS or finer particles of 1 mm or less, and may further include a step of removing foreign substances from the waste EPS before crushing, washing, drying and sorting.
[0037] The above step (2) is a step of reducing the pulverized waste EPS, then extruding and cooling to produce an ingot. The reduction can be achieved by thermal melting or solvent dissolution. For example, the pulverized waste EPS is fed into a reducing machine and melted at 120 to 160°C, thereby removing foaming gas and air from the waste EPS to obtain a polystyrene melt with reduced volume. Thereafter, the polystyrene melt is extruded at 120 to 160°C and cooled to form an ingot. At this time, the ingot can have various shapes depending on the shape of the molding machine during extrusion, and the shape is not limited, but for example, it can have a circular cross-section, a square cross-section, a triangular cross-section, etc.
[0038] In the present invention, step (b) is a step of feeding the mixture of step (a) into an extruder, melting and kneading, and extruding strands having a diameter of 1 mm or less. Specifically, the mixture is fed into the extruder, melted and kneaded in a temperature range of 170 to 185°C, sufficiently melting and kneading the mixture while preventing deterioration of physical properties due to deterioration and oxidation and breaking or breaking during strand ejection, and the melted and kneaded waste EPS melt is ejected from the extruder as strands through a nozzle.
[0039] The diameter of the above nozzle may be 1 to 3.2 mm, preferably 2.5 mm or less, and the arrangement, shape, and angle of the nozzle may be adjusted in consideration of the process speed, enlargement, etc., and are not limited thereto. For example, the arrangement of the nozzle may be in two rows vertically or in a circle, and the angle may be 45° downward or the strand may fall vertically.
[0040] In addition, before discharging the strand through the nozzle, a step of removing foreign substances may be further included, and the method of removing foreign substances may be performed by a conventional method, and the method is not limited thereto. However, as an example, foreign substances may be removed by passing the molten substance through a screen of 100 to 120 mesh.
[0041] Additionally, the temperature of the strand when discharged through the nozzle may be 180 to 240°C, preferably 190 to 230°C, and may vary depending on the diameter of the strand being discharged.
[0042] The strand discharged through the above nozzle is elongated during the drawing process, and the diameter of the strand is 1 mm or less, preferably 0.6 to 1 mm.
[0043] In the present invention, step (c) is a step of cooling the strand discharged in step (b) so that the surface temperature of the strand becomes 70 to 80°C when it is introduced into the roller of the cutting machine. Specifically, step (c) cools the strand discharged in step (b) so that the surface temperature of the strand becomes 70 to 80°C when it is introduced into the roller of the cutting machine, thereby preventing the strand from sticking to each equipment when passing through the cooling equipment and the cutting machine or from breaking during the movement due to overcooling.
[0044] The above cooling can be performed by immersion in water or by spraying water, and it is preferable to select a cooling method according to conditions to prevent rapid cooling or overcooling of the strand. For example, in the case of cooling by spraying water, the strand can be cooled by continuously spraying water on the upper part of the strand and minimizing contact between the strand and the water. In the case of immersion in water, the degree and speed of cooling of the strand can be controlled by controlling the temperature of the water and the speed at which it passes through the water.
[0045] In the present invention, step (d) is a step of introducing the strand cooled in step (c) into a cutting machine and cutting it to a diameter and length of 1 mm or less, which will be described in detail with reference to a photograph showing a part of a cutting machine according to a preferred embodiment of the present invention of FIG. 1.
[0046] Referring to FIG. 1, step (d) is performed by introducing the strand cooled in step (c) into a cutting machine to manufacture pellets having a diameter and length of 1 mm or less, wherein the cutting machine of step (d) includes a roller unit (10) including an upper roller (11) and a lower roller (12); and a cutting unit (20) including a rotating body (22) having a fixed blade (21) and one or more rotating blades (22a) and cutting the strand at the fixed blade (21) by rotation of the rotating blade (22a); and the lower roller (12) and the rotating body (22) are driven by two different axes, respectively.
[0047] Specifically, the upper roller (11) of the roller section (10) is a roller positioned relatively higher than the lower roller (12) to pressurize the strand introduced between the rollers so that the strand can be transmitted to the fixed blade (21) of the cutting machine at a certain angle, and the upper roller (11) has a diameter of 40 to 80 mm, which may be the same as or different from the diameter of the lower roller (12), and for example, may be 70 to 80 mm, but may be adjusted depending on manufacturing conditions. The lower roller (12) is a roller positioned relatively lower than the upper roller (11) to pull the strand so that the strand can be introduced into the cutting machine and moved to the fixed blade (21), and the diameter of the lower roller (12) is 40 to 50 mm. The lower roller (12) above has a diameter of 40 to 50 mm, so that the speed of drawing the strand does not slow down or speed up, so that the diameter of the strand can be drawn to 1 mm or less, and the speed at which the strand contacts the fixed blade (21) is also controlled so that the strand drawn to a diameter of 1 mm can be cut into pellets of 1 mm in length without breaking.
[0048] The above roller section (10) may include additional rollers in addition to the upper roller (11) and the lower roller (12) in some cases.
[0049] The above cutting section (20) cuts the strand at the fixed blade (21) by the rotation of the rotating blade (22a) when the rotating body (22) having the rotating blade (22a) is driven by another actuator different from the roller section (10), and the horizontal distance from the point (A1) where the strand first comes into contact with the lower roller (12) to the tip (B1) of the rotating blade is set to 70 to 80 mm, thereby controlling the pulling speed so that the pellet can have a diameter and length of 1 mm or less.
[0050] In addition, FIG. 2 is a diagram illustrating a preferred example of the present invention, which illustrates the angle formed when a rotary blade (22a) and a strand come into contact, wherein, at a point (C1) where the tip (B1) of the rotary blade comes into contact with the introduced strand (30), the straight direction in which the strand (30) moves and the rear blade (D) portion of the rotary blade (22a) have an angle (θ) of 5 to 10°, so that the strand is cut to 1 mm or less without causing a cutting defect such as the cutting surface of the strand becoming slanted or broken.
[0051] In addition, when the lower roller (12) and the rotating body (22) are driven by respective actuators provided on two different axes, the speed of the lower roller (12) can be 300 to 600 rpm, and the linear speed of the surface of the rotating body can be 10 to 16 m / sec.
[0052] In this way, in the step (d), the strand cooled in the step (c) passes through the roller section (10) of the cutting machine and moves to the fixed blade (21), where it is cut at the fixed blade (21) by the rotating blade (22a) to be manufactured into a pellet having a diameter and length of 1 mm or less.
[0053] Before the above step (d), a step of drying the cooled strand may be further included to remove moisture remaining in the strand. The drying method may be performed by a conventional method, and the method is not limited thereto. For example, an air wiper may be used. The air wiper may be in a plate shape, and when the strand passes through the upper part of the plate shape, moisture may be removed from the strand by a portion that sucks air and a portion that sucks moisture. The air suction portion and the moisture suction portion may be respectively arranged at the upper / lower part or the lower / upper part of the plate shape, and the plate shape may be inclined.
[0054] The pellets manufactured in the above step (d) have a diameter and length of 0.6 to 1 mm.
[0055] In addition, the present invention provides recycled EPS pellets having a diameter and length of 1 mm or less, manufactured from waste Styrofoam by the above manufacturing method.
[0056] In addition, the present invention provides that the manufactured recycled EPS pellets can be polymerized with a polymer, a foaming agent, etc. as a seed to form an EPS composite, which can be used in the same field as the EPS before disposal.
[0057] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited to the examples.
[0058] <Example>
[0059] 1. Manufacturing recycled EPS pellets from waste Styrofoam
[0060] After crushing waste Styrofoam into 50 to 100 mm pieces, it was placed in a reducing machine and heated to 120 to 160°C with an electric heater to melt it. Thereafter, the melt was placed in an extruder, melted and extruded at 120 to 160°C to remove foaming gas and air, and then the melt extrudate was cooled to form an ingot.
[0061] After the above ingot was prepared by crushing, it was put into a mixing facility and mixed together with 0 to 6 parts by weight of an impact modifier (polystyrene-butadiene-polystyrene copolymer, SBS), 0.1 to 0.5 parts by weight of an antioxidant, and 0.1 to 0.5 parts by weight of a heat stabilizer for 100 parts by weight of the above ingot.
[0062] The above mixture was fed into an extruder and melted at 170 to 185°C, then passed through a screen of 100 to 125 mesh to remove foreign substances, and then drawn into strands and discharged through a nozzle with a diameter of 2.5 mm.
[0063] After this, water was sprayed on the strand to cool it so that the surface temperature of the strand when introduced into the roller of the cutting machine was 65 to 85°C (described as the cooling temperature), and then the moisture remaining in the strand was removed using a multi-wiper.
[0064] The above-mentioned moisture-removed strand was introduced into a cutter having a body with a roller and a rotating blade driven by two axes, thereby manufacturing pellets.
[0065] At this time, in the roller section of the cutting machine, the upper roller had a diameter of 70 mm, the lower roller had a diameter of 35 to 55 mm, the speed of the lower roller was 330 rpm, and the horizontal distance from the point (A1) where the strand first comes into contact with the lower roller to the tip (B1) of the rotating blade was 65 to 85 mm.
[0066] In addition, at the point (C1) where the tip (B1) of the rotary blade contacts the introduced strand, the straight direction in which the strand (30) moves and the rear blade portion of the rotary blade (22a) exhibit an angle of 3 to 12°. This is described as the rotary blade-strand angle.
[0067] Additionally, the surface linear speed of the rotating body including the rotating blade was set to 15 m / sec.
[0068] Regenerated EPS pellets manufactured under different conditions in each of the above steps are described as Examples 1 to 11 and Comparative Examples 1 to 11, and the diameter and length of the pellets manufactured in each Example and Comparative Example are measured and shown in Table 1 below.
[0069] SBS(weight part)Rotating body surface linear speed(m / sec)Lower roller speed(rpm)Cooling temperature(℃)Lower roller diameter(mm)Spacing(mm)Rotating blade-strand angle(°)Pellet sizeDiameter(mm)Length(mm)Example 11153307545757≤1≤1Example 23153307545757≤1≤1Example 35153307545757≤1≤1Example 43153307045757≤1≤1Example 531533 08045757≤1≤1Example 63153307540757≤1≤1Example 73153307550757≤1≤1Example 83153307545707≤1≤1Example 93153307545807≤1≤1Example 103153307545755≤1≤1Example 11315330754575 10≤1≤1Comparative Example 10153307545757Strand Defect-Comparative Example 20.5153307545757>1>1Comparative Example 36153307545757≤1>1Comparative Example 43153306545757Strand Defect-Comparative Example 53153308545757Strand Defect-Comparative Example 631533075 35757 Strand Defect - Comparative Example 73153307555757 Strand Defect - Comparative Example 83153307545657 Strand Defect - Comparative Example 93153307545857 Strand Defect - Comparative Example 103153307545753 Strand Defect - Comparative Example 1131533075457512 Strand Defect -
[0070] Through the above Table 1, it can be seen that when producing recycled EPS pellets from waste Styrofoam by strand cutting, SBS is included in an amount of 1 to 5 parts by weight, the cooling temperature is 70 to 80°C, the lower roller diameter is 40 to 50 mm, the separation distance is 70 to 80 mm, and the rotating blade-strand angle is 5 to 10°, recycled EPS can be produced from waste Styrofoam into pellets of 1 mm or less in both diameter and length.
[0071] 2. Mechanical properties
[0072] (1) Impact strength
[0073] Each of the examples and comparative examples described in Table 1 above was produced as 1 / 4" and 1 / 8" test pieces, and the impact strength was measured according to ASTM D256 at 23°C.
[0074] As a result, the average impact strength of Examples 1 to 11 was 1.9 kgcm / cm, and the average impact strength of Comparative Examples 1 to 11 was 1.6 kgcm / cm, indicating that the impact strength of the Examples was higher than that of the Comparative Examples.
[0075] (2) Elongation
[0076] For each of the examples and comparative examples described in Table 1 above, elongation was measured according to ASTM D 790.
[0077] As a result, the average elongation of Examples 1 to 11 was 2.1%, which was higher than the average elongation of Comparative Examples 1 to 11, which was 1.2%.
[0078] From the above experimental results, it can be seen that the present invention can manufacture recycled EPS pellets having a diameter and length of 1 mm or less while preventing a decrease in impact strength and elongation of waste EPS.
[0079] While the present invention has been described above with reference to the embodiments described herein or illustrated in the accompanying drawings, these are merely exemplary, and those skilled in the art will understand that various modifications and equivalent embodiments are possible. Accordingly, the technical protection scope of the present invention should be defined by the following claims.
[0080]
[0081] [Explanation of symbols]
[0082] 10: Roller section, 11: Upper roller, 12: Lower roller
[0083] 20: cutting part, 21: fixed blade, 22: rotating body, 22a: rotating blade
[0084] 30: Strand
[0085] A1: The point where the strand first comes into contact with the lower roller.
[0086] B1: The tip of the rotating blade
[0087] C1: The point where the tip of the rotating blade contacts the introduced strand.
[0088] D: Rear blade part of the rotary blade
[0089] The present invention relates to a method for manufacturing recycled EPS pellets having a diameter and length of 1 mm or less by strand cutting from waste Styrofoam, and is recognized as having industrial applicability because it can be widely used in the same field as EPS before disposal or in various fields by being used as a seed in polymerization or composite material manufacturing with various compounds such as polymers and foaming agents.
Claims
1. A method for manufacturing a strand having a diameter of 1 mm or less from waste Styrofoam and then cutting the strand to manufacture a recycled EPS pellet having a length of 1 mm or less. (a) A step of crushing an ingot manufactured from waste EPS, and then mixing 1 to 5 parts by weight of styrene-butadiene-styrene (SBS) with respect to 100 parts by weight of the ingot; (b) a step of introducing the mixture of step (a) into an extruder, melting and kneading the mixture, and extruding strands having a diameter of 1 mm or less; (c) a step of cooling the strand discharged in step (b) so that the surface temperature of the strand becomes 70 to 80°C when it is introduced into the roller of the cutting machine; and (d) a step of introducing the cooled strand in step (c) into a cutting machine and cutting it to a diameter and length of 1 mm or less; including, The cutting machine of the above step (d) includes a roller part including an upper roller and a lower roller; and a cutting part including a rotating body having a fixed blade and one or more rotating blades, and cutting the strand at the fixed blade by rotation of the rotating blade; The distance from the point (A1) where the strand first comes into contact with the lower roller to the tip of the rotating blade (B1) is 70 to 80 mm. A method for manufacturing recycled EPS pellets having a diameter and length of 1 mm or less by strand cutting from waste Styrofoam, characterized in that the straight direction in which the strand moves and the rear blade portion of the rotary blade have an angle of 5 to 10° at a point (C1) where the blade tip (B1) of the rotary blade contacts the introduced strand.
2. In paragraph 1, A method for producing recycled EPS pellets having a diameter and length of 1 mm or less from waste Styrofoam by strand cutting, characterized in that the ingot is produced by including (1) a step of crushing waste EPS; and (2) a step of reducing the crushed waste EPS, and then extruding and cooling the same to produce an ingot.
3. In paragraph 2, A method for producing recycled EPS pellets having a diameter and length of 1 mm or less by strand cutting from waste Styrofoam, characterized in that the above reduction is performed by thermal melting or solvent dissolution.
4. In paragraph 1, A method for manufacturing recycled EPS pellets having a diameter and length of 1 mm or less by strand cutting from waste Styrofoam, characterized in that the lower roller and the rotating body are driven by two different axes.
5. In paragraph 1, A method for producing recycled EPS pellets having a diameter and length of 1 mm or less by strand cutting from waste Styrofoam, characterized in that the diameter of the lower roller is 40 to 50 mm.
6. In paragraph 1, A method for producing recycled EPS pellets having a diameter and length of 1 mm or less by strand cutting from waste Styrofoam, characterized in that the rotation speed of the lower roller in the above step (d) is 300 to 600 rpm and the surface linear speed of the rotating body is 10 to 16 m / sec.
7. Recycled EPS pellets having a diameter and length of 1 mm or less, manufactured from waste Styrofoam according to any one of clauses 1 to 6.
Citation Information
Patent Citations
Method for collecting and using polystyrene foam plastic waste
JP1997503235A
Pellet manufacturing apparatus using the waste styrofoam
KR101778536B1
Method and machine for cutting strand, and method of operating the machine
KR1019960700870A
Method and apparatus for reproducing used styro-foam which reproduce used styro-foam into polystyrene ingot pellet or foamed ingot pellet and same ingot pellet
KR1020140033936A
Extruder
KR1020180117502A