Resin composition
The resin composition combines recycled resin with a new graft copolymer and ungrafted copolymer to enhance mechanical properties, addressing the limitations of recycled resin compositions and achieving improved impact and tensile strength, suitable for eco-friendly products with enhanced performance.
Patent Information
- Application Number
- PCT/KR2024/007268
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-02
- Filing Date
- 2024-05-28
- Publication Date
- 2024-12-05
AI Technical Summary
Recycled resin compositions used in thermoplastic resin molded products exhibit lower impact resistance, tensile strength, and chemical resistance compared to new resin compositions, due to reduced shock absorption efficiency of rubber particles, making them unsuitable for high-performance applications.
A resin composition is developed that includes a mixture of recycled resin, a new graft copolymer composition with specific particle size ranges, and a new ungrafted copolymer, enhancing the mechanical properties by optimizing the ratio and particle sizes of conjugated diene-based polymers, aromatic vinyl monomers, and vinyl cyan monomers to improve impact resistance and processability.
The resulting resin composition achieves improved impact strength, tensile strength, and flow index, making it suitable for eco-friendly products with enhanced mechanical properties while maintaining a carbon reduction effect.
Smart Images

Figure KR2024007268_05122024_PF_FP_ABST
Abstract
Description
resin composition
[0001] [Cross-reference with related applications]
[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0071351, filed June 2, 2023, the entire contents of which are incorporated herein by reference.
[0003]
[0004] [Technical Field]
[0005] The present invention relates to a resin composition, and more particularly, to a resin composition comprising a graft copolymer composition containing a certain amount of a new resin in a regenerated resin.
[0006] A diene graft copolymer comprises a diene rubber polymer and a shell comprising vinyl aromatic monomer units and vinyl cyan monomer units grafted onto the diene rubber polymer. Compared to conventional high-impact polystyrene (HIPS), the diene graft copolymer exhibits superior impact resistance, chemical resistance, thermal stability, colorability, fatigue resistance, rigidity, and processability. Due to these properties, diene rubber-like thermoplastic resin molded products manufactured from the diene graft polymer are used as components for automobile interior and exterior materials, office equipment, and various electrical and electronic products.
[0007] Meanwhile, thermoplastic resin compositions must contain recycled resin to be certified as eco-friendly. However, because recycled resins have been used before, they have lower impact resistance, tensile strength, chemical resistance, and thermal stability compared to virgin resins. Furthermore, they can expose foreign matter on the surface of molded parts during processing. Consequently, recycled resins have been used as raw materials for low-quality materials. To overcome these issues with recycled resins, technologies are being developed to manufacture eco-friendly products by mixing them with virgin resins at specific ratios.
[0008] However, in the case of recycled resin, the impact absorption efficiency of the rubber particles is reduced, so the overall mechanical properties are lower than those of new resin, and therefore thermoplastic resin molded products using recycled resin have problems of reduced impact strength and rigidity.
[0009]
[0010] [Prior Art Literature]
[0011] [Patent Document]
[0012] (Patent Document 0001) KR 10-2016-0144185 A
[0013] The present invention has been devised to solve the problems of the above-mentioned prior art, and provides a recycled resin composition in which the mechanical properties are overcome by maximizing the shock absorption efficiency of rubber particles.
[0014] (1) The present invention provides a resin composition comprising a regenerated resin, a new graft copolymer composition, and a new non-graft copolymer, wherein the new graft copolymer composition comprises: a first graft copolymer comprising a first conjugated diene polymer having an average particle diameter of 75 nm or more and 220 nm or less; and a second graft copolymer comprising a second conjugated diene polymer having an average particle diameter of 250 nm or more and 400 nm or less, wherein the new graft copolymer composition comprises the first conjugated diene polymer in an amount of 8 wt% or more and 50 wt% or less based on the total content of the first conjugated diene polymer and the second conjugated diene polymer.
[0015] (2) The present invention provides a resin composition comprising, in the above (1), 70 parts by weight or more and 88 parts by weight or less of the regenerated resin, based on 100 parts by weight of the contents of the regenerated resin, the new graft copolymer composition, and the new non-graft copolymer.
[0016] (3) The present invention provides a resin composition comprising 75 parts by weight or more and 85 parts by weight or less of the regenerated resin, based on 100 parts by weight of the contents of the regenerated resin, the new graft copolymer composition, and the new non-graft copolymer in any one of the above (1) or (2).
[0017] (4) The present invention provides a resin composition comprising, based on 100 parts by weight of the contents of the regenerated resin, the new graft copolymer composition, and the new non-graft copolymer in any one of the above (1) to (3), the new graft copolymer in an amount of 10 parts by weight or more and 18 parts by weight or less, and the new non-graft copolymer in an amount of 1 part by weight or more and 15 parts by weight or less.
[0018] (5) The present invention provides a resin composition in which, in any one of the above (1) to (4), the new graft copolymer composition comprises the first conjugated diene polymer in an amount of 10 wt% or more and 43 wt% or less based on the total content of the first conjugated diene polymer and the second conjugated diene polymer.
[0019] (6) The present invention provides a resin composition in which the average particle diameter of the first conjugated diene polymer is 78 nm or more and 208 nm or less in any one of the above (1) to (5).
[0020] (7) The present invention provides a resin composition according to any one of the above (1) to (6), wherein the regenerated resin has an Izod impact strength measured according to ASTM D256 of 7 kg·cm / cm or more and 12 kg·cm / cm or less, and a flow index measured according to ASTM D1238 of 25 g / 10 min or more and 35 g / 10 min or less.
[0021] (8) The present invention is a resin composition according to any one of the above (1) to (7), wherein the Izod impact strength measured according to ASTM D256 is 17.0 kg·cm / cm or more, and the tensile strength measured according to ASTM D638 is 395 kg / cm 2 The present invention provides a resin composition having a flow index of 26.0 g / 10 min or more as measured under the conditions of 220°C and 10 kg according to ASTM D1238.
[0022] (9) The present invention provides a resin composition in which, in any one of the above (1) to (8), the non-graft copolymer comprises an aromatic vinyl monomer unit and a vinyl cyan monomer unit, and the first graft copolymer and the second graft copolymer each further comprise an aromatic vinyl monomer unit and a vinyl cyan monomer unit.
[0023] (10) The present invention provides a resin composition in which, when an impact specimen cross-section of the resin composition is observed using a TEM image in any one of the above (1) to (9), cavitation is observed inside the first graft copolymer and the second graft copolymer.
[0024] (11) The present invention provides a method for producing a resin composition, comprising: a step of producing a new graft copolymer composition by performing graft polymerization in the presence of a first conjugated diene polymer latex including a first conjugated diene polymer having an average particle diameter of 75 nm or more and 220 nm or less and a second conjugated diene polymer latex including a second conjugated diene polymer having an average particle diameter of 250 nm or more and 400 nm or less; and a step of mixing the produced new graft copolymer composition, a regenerated resin, and a new non-graft copolymer, wherein the new graft copolymer is produced by containing the first conjugated diene polymer in an amount of 8 wt% or more and 50 wt% or less based on the total content of the first conjugated diene polymer and the second conjugated diene polymer.
[0025] The resin composition according to the present invention has excellent impact strength, flow index, and tensile strength even if it contains a recycled resin.
[0026] Figure 1 is a TEM image of a cross-section of an impact specimen of a thermoplastic resin composition according to Reference Example 1.
[0027] Figure 2 is a TEM image of a cross-section of an impact specimen of a thermoplastic resin composition according to Reference Example 2.
[0028] Figure 3 is a TEM image of a cross-section of an impact specimen of a thermoplastic resin composition according to Comparative Example 1.
[0029] Hereinafter, the present invention will be described in more detail to facilitate understanding. The terms and words used in this specification and claims should not be interpreted based on their conventional or dictionary meanings. Based on the principle that the inventor can appropriately define the concepts of terms to best explain his or her invention, they should be interpreted in a way that aligns with the technical spirit of the present invention.
[0030] The terminology used herein is for the purpose of describing exemplary embodiments only and is not intended to limit the present invention. Singular expressions include plural expressions unless the context clearly dictates otherwise.
[0031] In the present invention, the term 'monomer unit' may indicate a component, structure, or substance itself derived from a monomer, and as a specific example, may mean a repeating unit formed within a polymer by a monomer introduced during polymerization of the polymer and participating in the polymerization reaction.
[0032] In the present invention, the 'weight average molecular weight' is generally measured by gel permeation chromatography (GPC). For example, after dissolving the sample to be measured in a THF (tetrahydrofuran) solution, the relative value to a standard sample (PS, standard polystyrene) can be measured through gel permeation chromatography (GPC).
[0033] The term 'composition' as used in the present invention includes a mixture of materials comprising the composition as well as reaction products and decomposition products formed from the materials of the composition.
[0034] In the present invention, the 'average particle diameter' may refer to the arithmetic mean particle diameter in the particle size distribution measured by dynamic light scattering, specifically, the scattering intensity average particle diameter. The average particle diameter of the conjugated diene polymer can be measured using the Nicomp 380 equipment (product name, manufacturer: PSS Nicomp).
[0035]
[0036] Resin composition
[0037] The present invention provides a resin composition.
[0038] According to one embodiment of the present invention, a resin composition includes a regenerated resin, a new graft copolymer composition, and a new non-graft copolymer, wherein the new graft copolymer composition includes a first graft copolymer including a first conjugated diene polymer having an average particle diameter of 75 nm or more and 220 nm or less; and a second graft copolymer including a second conjugated diene polymer having an average particle diameter of 250 nm or more and 400 nm or less, wherein the new graft copolymer composition includes the first conjugated diene polymer in an amount of 8 wt% or more and 50 wt% or less based on the total content of the first conjugated diene polymer and the second conjugated diene polymer.
[0039] The present inventors have discovered that the mechanical properties of a recycled resin composition can be improved by mixing a new resin containing a graft copolymer in the form of large-diameter rubber particles and small-diameter rubber particles in a specific ratio into a recycled resin, thereby completing the present invention.
[0040]
[0041] Hereinafter, each component of a resin composition according to one embodiment of the present invention will be described.
[0042]
[0043] 1. Regenerated resin
[0044] According to one embodiment of the present invention, recycled resin is a component included in a resin composition to obtain certification as an eco-friendly product. It is a recycled product obtained by processing and reusing used resin or resin waste. Specifically, the recycled resin may refer to resin waste collected, shredded, washed, separated, and sorted, then processed and reused for a specific purpose. The form of the recycled resin is not particularly limited.
[0045] According to one embodiment of the present invention, the recycled resin may be at least one selected from the group consisting of recycled polyethylene, recycled polypropylene, recycled polyester, recycled polystyrene, recycled polyamide, recycled polycarbonate, recycled diene-based graft polymer, and recycled vinyl-based non-graft polymer.
[0046] According to one embodiment of the present invention, the regenerated resin may include a conjugated diene monomer unit, a vinyl cyan monomer unit, and an aromatic vinyl monomer unit. The conjugated diene monomer unit may improve the impact resistance of the regenerated resin. The vinyl cyan monomer unit may improve the chemical resistance of the regenerated resin. In addition, the aromatic vinyl monomer unit may improve the processability of the regenerated resin.
[0047] According to one embodiment of the present invention, the conjugated diene monomer for forming the conjugated diene monomer unit included in the regenerated resin may be at least one selected from the group consisting of 1,3-butadiene, isoprene, chloroprene, and piperylene, and a specific example thereof may be 1,3-butadiene.
[0048] According to one embodiment of the present invention, the aromatic vinyl monomer for forming the aromatic vinyl monomer unit included in the regenerated resin may be at least one selected from the group consisting of α-methyl styrene, α-ethyl styrene, p-methyl styrene, 2,4-dimethyl styrene, styrene, p-fluoro styrene, p-chloro styrene, and p-bromo styrene, and a specific example thereof may be styrene.
[0049] According to one embodiment of the present invention, the vinyl cyan monomer for forming the vinyl cyan monomer unit included in the regenerated resin may be at least one selected from the group consisting of acrylonitrile, methacrylonitrile, (Z)-3-phenyl acrylonitrile, and α-chloro acrylonitrile, and a specific example thereof may be acrylonitrile.
[0050] According to one embodiment of the present invention, the regenerated resin may include a regenerated graft copolymer including a conjugated diene polymer, an aromatic vinyl monomer unit, and a vinyl cyan monomer unit. Specifically, the regenerated graft copolymer included in the regenerated resin may have a core-shell structure including a core including a conjugated diene polymer formed of the conjugated diene monomer unit, and a shell surrounding the core and formed of the aromatic vinyl monomer unit and the vinyl cyan monomer unit.
[0051] According to one embodiment of the present invention, the regenerated resin may have an Izod impact strength of 7 kg·cm / cm or more and 12 kg·cm / cm or less as measured according to ASTM D256, and a flow index of 25 g / 10 min or more and 35 g / 10 min or less as measured according to ASTM D1238. If the above conditions are satisfied, a resin composition having a carbon reduction effect and minimum mechanical properties can be realized.
[0052]
[0053] According to one embodiment of the present invention, the resin composition may contain the regenerated resin in an amount of 70 parts by weight or more and 88 parts by weight or less, based on 100 parts by weight of the contents of the regenerated resin, the new graft copolymer, and the new non-graft copolymer, and for specific examples, the resin composition may contain the regenerated resin in an amount of 71 parts by weight or more, 72 parts by weight or more, 73 parts by weight or more, 74 parts by weight or more, or 75 parts by weight or more, and further, the resin composition may contain the regenerated resin in an amount of 87 parts by weight or less, 86 parts by weight or less, or 85 parts by weight or less. When the above-described ranges are satisfied, the impact strength, tensile strength, and flow index of the resin composition may all be improved.
[0054]
[0055] 2. New graft copolymer composition
[0056] According to one embodiment of the present invention, the novel graft copolymer composition is a graft copolymer that has never been used before and is a component that improves the impact resistance of a thermoplastic resin composition.
[0057] According to one embodiment of the present invention, the new graft copolymer composition may be a graft polymer including a conjugated diene polymer including a conjugated diene monomer unit as a rubber polymer and a shell including an aromatic vinyl monomer unit and a vinyl cyan monomer unit grafted onto the conjugated diene polymer. The shell may include an aromatic vinyl monomer unit and a vinyl cyan monomer unit that are not grafted onto the conjugated diene polymer.
[0058]
[0059] According to one embodiment of the present invention, the conjugated diene monomer for forming the conjugated diene monomer unit included in the new graft copolymer composition may be at least one selected from the group consisting of 1,3-butadiene, isoprene, chloroprene, and piperylene, and a specific example thereof may be 1,3-butadiene.
[0060] According to one embodiment of the present invention, the aromatic vinyl monomer for forming the aromatic vinyl monomer unit included in the new graft copolymer composition may be at least one selected from the group consisting of α-methyl styrene, α-ethyl styrene, p-methyl styrene, 2,4-dimethyl styrene, styrene, p-fluoro styrene, p-chloro styrene, and p-bromo styrene, and a specific example thereof may be styrene.
[0061] According to one embodiment of the present invention, the vinyl cyan monomer for forming the vinyl cyan monomer unit included in the new graft copolymer composition may be at least one selected from the group consisting of acrylonitrile, methacrylonitrile, (Z)-3-phenyl acrylonitrile, and α-chloro acrylonitrile, and a specific example thereof may be acrylonitrile.
[0062]
[0063] According to one embodiment of the present invention, the content of the conjugated diene polymer included in the new graft copolymer composition may be 40 to 80 wt%, preferably 50 to 70 wt%. When the above-described conditions are satisfied, the impact resistance of the new graft polymer composition can be further improved.
[0064] According to one embodiment of the present invention, the content of the aromatic vinyl monomer unit included in the new graft copolymer composition may be 10 to 50 wt%, preferably 20 to 40 wt%. When the above-described conditions are satisfied, the processability of the new graft copolymer composition can be further improved.
[0065] According to one embodiment of the present invention, the content of the vinyl cyan monomer unit included in the new graft copolymer composition may be 1 to 30 wt%, preferably 5 to 25 wt%. When the above-described conditions are satisfied, the chemical resistance of the new graft polymer composition can be further improved.
[0066]
[0067] According to one embodiment of the present invention, the new graft copolymer composition may include two or more types of conjugated diene polymers having different average particle diameters. Specifically, the new graft copolymer composition may include a first conjugated diene polymer, which is a small-diameter rubber particle having a relatively small average particle diameter, a first graft copolymer including an aromatic vinyl monomer unit and a vinyl cyan monomer unit, and a second conjugated diene polymer, which is a large-diameter rubber particle having a relatively large average particle diameter, a second graft copolymer including an aromatic vinyl monomer unit and a vinyl cyan monomer unit.
[0068] According to one embodiment of the present invention, the first graft copolymer included in the new graft copolymer composition may have a core-shell structure including a core comprising a first conjugated diene polymer formed of the conjugated diene monomer unit, and a shell surrounding the core and formed of the aromatic vinyl monomer unit and the vinyl cyan monomer unit. In addition, the second graft copolymer included in the new graft copolymer composition may have a core-shell structure including a core comprising a second conjugated diene polymer formed of the conjugated diene monomer unit, and a shell surrounding the core and formed of the aromatic vinyl monomer unit and the vinyl cyan monomer unit.
[0069] In the past, a single type of conjugated diene polymer having a single average particle diameter was included in a resin composition containing a recycled resin. However, in the case of the present invention, in which two or more types of conjugated diene polymers having different average particle diameters are included in a resin composition containing a recycled resin, the number of rubber particles increases compared to the case in which a single type of conjugated diene polymer having a single average particle diameter is included, and thus the shock absorption efficiency increases.
[0070] According to one embodiment of the present invention, the first conjugated diene polymer may have an average particle diameter of 75 nm or more and 220 nm or less, and for specific examples, may be 76 nm or more, 77 nm or more, 78 nm or more, 79 nm or more, or 80 nm or more, and may also be 216 nm or less, 212 nm or less, 208 nm or less, 204 nm or less, or 200 nm or less. When the above-described conditions are satisfied, the impact resistance of the new graft copolymer composition can be improved. If the average particle diameter of the first conjugated diene polymer is less than 75 nm, the aromatic vinyl monomer unit and the vinyl cyan monomer unit are not grafted well, so the impact resistance is reduced, and if it exceeds 220 nm, there is no significant difference from the average particle diameter of the second conjugated diene polymer, so the effect of improving the impact absorption efficiency disappears.
[0071] According to one embodiment of the present invention, the second conjugated diene polymer may have an average particle diameter of 250 nm or more and 400 nm or less, and for specific examples, may be 260 nm or more, 270 nm or more, 280 nm or more, 290 nm or more, or 300 nm or more, and may also be 390 nm or less, 380 nm or less, 370 nm or less, 360 nm or less, or 350 nm or less. When the above-described conditions are satisfied, the impact resistance of the new graft copolymer composition may be improved.
[0072] According to one embodiment of the present invention, the new graft copolymer composition may contain the first conjugated diene polymer in an amount of 8 wt% or more and 50 wt% or less based on the total content of the first conjugated diene polymer and the second conjugated diene polymer, and as a specific example, the first conjugated diene polymer may contain the first conjugated diene polymer in an amount of 8.5 wt% or more, 9 wt% or more, 9.5 wt% or more, or 10 wt% or more based on the total content of the first conjugated diene polymer and the second conjugated diene polymer, and further may contain the first conjugated diene polymer in an amount of 48 wt% or less, 46 wt% or less, 44 wt% or less, or 43 wt% or less. When the above-described ranges are satisfied, the impact strength, tensile strength, and flow index of the resin composition may all be improved.
[0073] According to one embodiment of the present invention, when a cross-section of an impact specimen of a resin composition including the new graft copolymer composition and the regenerated resin is observed using a TEM image, cavitation is observed inside each of the first graft copolymer and the second graft copolymer derived from the new graft copolymer composition, but no cavity may be observed inside the graft copolymer derived from the regenerated resin. The impact specimen may refer to a specimen to which an impact has been applied to the resin composition.
[0074] Specifically, when stress is applied to the resin composition, the first graft copolymer and the second graft copolymer derived from the new graft copolymer composition may concentrate stress on each of the first graft copolymer and the second graft copolymer, and thus, the monomer chains (physical and chemical bonds) within them may be broken, thereby forming cavities. However, in the case of the graft copolymer derived from the regenerated resin, the monomer chains within the graft copolymer have already been decomposed by mechanical heat treatment during the regeneration process before the point at which the regenerated resin is included in the resin composition, and therefore, even if stress is applied to the resin composition, cavities may not be formed within the graft copolymer.
[0075] According to one embodiment of the present invention, when an impact is applied to a resin composition including the new graft copolymer composition, a cavity is formed inside each of the first graft copolymer and the second graft copolymer included in the resin composition, thereby relieving the surrounding stress, so that the impact strength of the resin composition can be improved.
[0076]
[0077] According to one embodiment of the present invention, the resin composition may contain 10 parts by weight or more and 18 parts by weight or less of the new graft copolymer composition, based on 100 parts by weight of the contents of the regenerated resin, the new graft copolymer composition, and the new non-graft copolymer, and for specific examples, it may contain 11 parts by weight or more, 12 parts by weight or more, or 13 parts by weight or more, and further, it may contain 17 parts by weight or less, 16 parts by weight or less, or 15 parts by weight or less. When the above-described range is satisfied, the impact strength, tensile strength, and flow index of the resin composition may all be improved.
[0078]
[0079] 3. Novel non-graft polymers
[0080] According to one embodiment of the present invention, the new non-graft copolymer is a non-graft copolymer that has never been used before and is a component that improves the tensile strength and processability of a resin composition.
[0081] According to one embodiment of the present invention, the new non-grafted copolymer is a non-grafted copolymer and may include an aromatic vinyl monomer unit and a vinyl cyan monomer unit.
[0082] According to one embodiment of the present invention, the aromatic vinyl monomer for forming the aromatic vinyl monomer unit included in the new non-graft copolymer may be at least one selected from the group consisting of α-methyl styrene, α-ethyl styrene, p-methyl styrene, 2,4-dimethyl styrene, styrene, p-fluoro styrene, p-chloro styrene, and p-bromo styrene, and a specific example thereof may be styrene.
[0083] According to one embodiment of the present invention, the vinyl cyan monomer for forming the vinyl cyan monomer unit included in the new non-graft copolymer may be at least one selected from the group consisting of acrylonitrile, methacrylonitrile, (Z)-3-phenyl acrylonitrile, and α-chloro acrylonitrile, and a specific example thereof may be acrylonitrile.
[0084]
[0085] According to one embodiment of the present invention, the content of the aromatic vinyl monomer unit included in the new graft copolymer may be 60 to 90 wt%, preferably 65 to 85 wt%. When the above-described conditions are satisfied, the processability of the new graft copolymer can be further improved.
[0086] According to one embodiment of the present invention, the content of vinyl cyanide monomer units included in the new non-graft copolymer may be 10 to 40 wt%, preferably 15 to 35 wt%. When the above-described conditions are satisfied, the chemical resistance of the diene-based graft polymer can be further improved.
[0087]
[0088] 4. Other additives
[0089] According to one embodiment of the present invention, the resin composition may further include other additives. The additives may be at least one selected from the group consisting of a lubricant, an antioxidant, a light stabilizer, a hydrolysis stabilizer, a release agent, a pigment, an antistatic agent, a conductive agent, an electromagnetic shielding agent, a magnetizing agent, a mineral filler, a crosslinking agent, an antibacterial agent, a processing aid, a metal deactivator, a flame retardant, an antifriction and wear-resistant agent, and a coupling agent.
[0090] The above additives can be used without limitation as long as they are used in the technical field of the present invention, and a person skilled in the art can select the additives included in the present invention according to the purpose.
[0091]
[0092] <Method for producing resin composition>
[0093] The present invention provides a method for producing a resin composition.
[0094] A method for preparing a resin composition according to one embodiment of the present invention comprises the steps of: preparing a new graft copolymer composition by performing graft polymerization in the presence of a first conjugated diene polymer latex including a first conjugated diene polymer having an average particle diameter of 75 nm to 220 nm and a second conjugated diene polymer latex including a second conjugated diene polymer having an average particle diameter of 250 nm to 400 nm; and mixing the prepared new graft copolymer composition, a regenerated resin, and a new non-graft copolymer, wherein the new graft copolymer is prepared by containing the first conjugated diene polymer in an amount of 8 wt% to 50 wt% based on the total content of the first conjugated diene polymer and the second conjugated diene polymer.
[0095]
[0096] Hereinafter, embodiments of the present invention will be described in detail so that those skilled in the art can easily implement them. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein.
[0097]
[0098] Example 1
[0099] <Preparation of a New Graft Copolymer Composition>
[0100] Into a nitrogen-purged polymerization reactor (autoclave), 55 parts by weight (based on solids) of polybutadiene rubber latex as a large-diameter rubber latex having an average rubber particle diameter of 320 nm and a gel content of 70%, 10 parts by weight (based on solids) of polybutadiene rubber latex as a small-diameter rubber latex having an average rubber particle diameter of 100 nm and a gel content of 90%, 90 parts by weight of ion-exchanged water, 7.0 parts by weight of styrene as a monomer, and 3.0 parts by weight of acrylonitrile were charged, and the reactor temperature was maintained at 50°C. Then, 0.05 parts by weight of cumene hydroperoxide, 0.09 parts by weight of sodium pyrophosphate, 0.12 parts by weight of dextrose, and 0.002 parts by weight of ferrous sulfide were charged in batches to initiate the reaction.
[0101] Simultaneously with the start of polymerization, a mixture of 17.5 parts by weight of styrene, 7.5 parts by weight of acrylonitrile, 0.2 parts by weight of tertiary dodecyl mercaptan, and 0.12 parts by weight of cumene hydroperoxide was continuously fed into the reactor for 2 hours while raising the temperature to 75°C. After the continuous feeding was completed, 0.06 parts by weight of cumene hydroperoxide, 0.04 parts by weight of sodium pyrophosphate, 0.06 parts by weight of dextrose, and 0.001 parts by weight of ferrous sulfide were added, stirred at 80°C for 30 minutes, maintained for 30 minutes, and the reaction was terminated.
[0102] After the above reaction was completed, 0.5 parts by weight of an antioxidant (winstay-L / IR1076=0.8 / 0.2) emulsion was added to the latex, and then an aqueous magnesium sulfate solution was added to coagulate the latex, followed by dehydration, washing, and drying to obtain a powder of a new graft copolymer composition.
[0103]
[0104] <Manufacture of resin composition>
[0105] A recycled resin (manufactured by Daiichi Industrial Resin Co., Ltd.) having an Izod impact strength (kg·cm / cm, 1 / 4``) of 9 kg·cm / cm and a melt flow index (g / 10 min) of 30 g / 10 min as a copolymer of a recycled vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound, and a new non-graft copolymer (manufactured by LG Chemical Co., Ltd., product name: 97HC) having a weight average molecular weight of 165,000 g / mol and manufactured by polymerizing 70 wt% of styrene and 30 wt% of acrylonitrile were prepared.
[0106] 75 parts by weight of a recycled resin, 13 parts by weight of a new graft polymer, 12 parts by weight of a new non-graft copolymer, and ethylene bissteamide (EBA) as an active agent and other additives (heat stabilizer, pigment) were added to a mixer and mixed, and then an extruder was used at 230°C to obtain a resin composition in the form of pellets.
[0107]
[0108] Example 2
[0109] A resin composition was obtained by performing the same method as in Example 1, except that 48 parts by weight of large-diameter rubber latex and 7 parts by weight of small-diameter rubber latex were used in the <Preparation of a New Graft Copolymer Composition> step of Example 1.
[0110]
[0111] Example 3
[0112] A resin composition was obtained by performing the same method as in Example 1, except that 40 parts by weight of large-diameter rubber latex and 30 parts by weight of small-diameter rubber latex were used in the <Preparation of a New Graft Copolymer Composition> step of Example 1.
[0113]
[0114] Example 4
[0115] In the <Preparation of a New Graft Copolymer Composition> step of Example 1, a small-diameter rubber latex was used, and instead of 10 parts by weight (based on solid content) of polybutadiene rubber latex having an average particle diameter of 100 nm and a gel content of 90%, 10 parts by weight (based on solid content) of polybutadiene rubber latex having an average particle diameter of 80 nm and a gel content of 90% was used, a resin composition was obtained in the same manner as in Example 1.
[0116]
[0117] Example 5
[0118] In the <Preparation of a New Graft Copolymer Composition> step of Example 1, a small-diameter rubber latex was used, and instead of 10 parts by weight (based on solid content) of polybutadiene rubber latex having an average particle diameter of 100 nm and a gel content of 90%, 10 parts by weight (based on solid content) of polybutadiene rubber latex having an average particle diameter of 200 nm and a gel content of 90% was used, a resin composition was obtained in the same manner as in Example 1.
[0119]
[0120] Example 6
[0121] In the <Preparation of New Graft Copolymer Composition> step of Example 1, 40 parts by weight of large-diameter rubber latex and 30 parts by weight of small-diameter rubber latex were used, and in the <Preparation of Resin Composition> step of Example 1, 85 parts by weight of recycled resin, 13 parts by weight of new graft polymer, 2 parts by weight of new vinyl-based non-graft copolymer, and other additives (heat stabilizer, pigment) as a lubricant were added to a mixer and mixed, and then an extruder was used at 230°C to obtain a resin composition in the form of pellets, in the same manner as in Example 1, a resin composition was obtained.
[0122]
[0123] Comparative Example 1
[0124] A resin composition was obtained by performing the same method as in Example 1, except that in the <Preparation of a New Graft Copolymer Composition> step of Example 1, 65 parts by weight of large-diameter rubber latex was used and small-diameter rubber latex was not used.
[0125]
[0126] Comparative Example 2
[0127] A resin composition was obtained by performing the same method as in Example 1, except that 60 parts by weight of large-diameter rubber latex and 5 parts by weight of small-diameter rubber latex were used in the <Preparation of a New Graft Copolymer Composition> step of Example 1.
[0128]
[0129] Comparative Example 3
[0130] A resin composition was obtained by performing the same method as in Example 1, except that 30 parts by weight of large-diameter rubber latex and 35 parts by weight of small-diameter rubber latex were used in the <Preparation of a New Graft Copolymer Composition> step of Example 1.
[0131]
[0132] Comparative Example 4
[0133] In the <Preparation of a New Graft Copolymer Composition> step of Example 1, a resin composition was obtained in the same manner as in Example 1, except that 10 parts by weight (based on solid content) of polybutadiene rubber latex having an average particle diameter of 100 nm and a gel content of 90% was used instead of 10 parts by weight of polybutadiene rubber latex having an average particle diameter of 70 nm and a gel content of 90% as a small-diameter rubber latex.
[0134]
[0135] Comparative Example 5
[0136] In the <Preparation of a New Graft Copolymer Composition> step of Example 1, the same method as Example 1 was performed except that 10 parts by weight (based on solid content) of polybutadiene rubber latex having an average particle diameter of 100 nm and a gel content of 90% was used instead of 10 parts by weight of polybutadiene rubber latex having an average particle diameter of 230 nm and a gel content of 90% as a small-diameter rubber latex.
[0137]
[0138] Comparative Example 6
[0139] In the <Preparation of New Graft Copolymer Composition> step of Example 1, 65 parts by weight of large-diameter rubber latex was used, and no small-diameter rubber latex was used; and in the <Preparation of Resin Composition> step of Example 1, 85 parts by weight of recycled resin, 13 parts by weight of new graft polymer, 2 parts by weight of new vinyl-based non-graft copolymer, and other additives (heat stabilizer, pigment) were added to a mixer and mixed, and then an extruder was used at 230°C to obtain a resin composition in the form of pellets, in the same manner as in Example 6, a resin composition was obtained.
[0140]
[0141] Comparative Example 7
[0142] In the <Preparation of New Graft Copolymer Composition> step of Example 1, 65 parts by weight of large-diameter rubber latex was used, and no small-diameter rubber latex was used; and in the <Preparation of Resin Composition> step of Example 1, 60 parts by weight of recycled resin, 13 parts by weight of graft polymer, 27 parts by weight of new vinyl-based non-graft copolymer, and ethylene bissteamide (EBA) as a lubricant and other additives (heat stabilizer, pigment) were added to a mixer and mixed, and then an extruder was used at 230°C to obtain a resin composition in the form of pellets, in the same manner as in Example 1, a resin composition was obtained.
[0143]
[0144] Comparative Example 8
[0145] In the <Preparation of New Graft Copolymer Composition> step of Example 1, 65 parts by weight of large-diameter rubber latex was used, and no small-diameter rubber latex was used; and in the <Preparation of Resin Composition> step of Example 1, 60 parts by weight of recycled resin, 20 parts by weight of graft polymer, 20 parts by weight of new vinyl-based non-graft copolymer, and other additives (heat stabilizer, pigment) were added to a mixer and mixed, and then an extruder was used at 230°C to obtain a resin composition in the form of pellets, in the same manner as in Example 1, a resin composition was obtained.
[0146]
[0147] Comparative Example 9
[0148] In the <Preparation of New Graft Copolymer Composition> step of Example 1, 65 parts by weight of large-diameter rubber latex was used, and no small-diameter rubber latex was used; in the <Preparation of Resin Composition> step of Example 1, no new vinyl-based non-graft copolymer was added, and 90 parts by weight of recycled resin, 10 parts by weight of graft polymer, and ethylene bissteamide (EBA) as a lubricant and other additives (heat stabilizer, pigment) were added to a mixer and mixed, and then an extruder was used at 230°C to obtain a resin composition in the form of pellets, in the same manner as in Example 1, to obtain a resin composition.
[0149]
[0150] Reference Example 1
[0151] A recycled resin (manufactured by Daiichi Industrial Resin Co., Ltd.) was prepared as a copolymer of a recycled vinyl cyanide compound, a conjugated diene compound, and an aromatic vinyl compound, having an Izod impact strength (kg·cm / cm, 1 / 4``) of 9 kg·cm / cm and a melt flow index (g / 10 min) of 30 g / 10 min.
[0152] 100 parts by weight of recycled resin, ethylene bissteamide (EBA) as an active agent, and other additives (heat stabilizer, pigment) were added to a mixer and mixed, and then an extruder was used at 230°C to obtain a resin composition in the form of pellets.
[0153]
[0154] Reference Example 2
[0155] A resin composition was obtained by performing the same method as in Example 1, except that in the <Preparation of a New Graft Copolymer Composition> step of Example 1, 65 parts by weight of a small-diameter rubber latex was used instead of a large-diameter rubber latex.
[0156]
[0157] Experimental Example 1
[0158] The thermoplastic resin compositions according to Examples 1 to 6 and Comparative Examples 1 to 9 were extruded and injected to manufacture specimens, and the physical properties of the specimens were measured by the methods described below, and the results are shown in Tables 1 to 3 below.
[0159]
[0160] * Izod impact strength (kg·cm / cm, 1 / 4``): Measured according to ASTM D256. In the present invention, when the Izod impact strength is 17.0 kg·cm / cm or more, the impact resistance is considered to be excellent.
[0161]
[0162] * Tensile strength (kg / cm) 2 ): It was measured according to ASTM D638. In the present invention, the tensile strength is 395 kg / cm 2In this case, the tensile strength was considered to be excellent.
[0163]
[0164] * Melt Flow Index (g / 10 min): Measured under the conditions of 220℃ and 10kg according to ASTM D1238. In the present invention, when the melt flow index is 26.0g / 10min or higher, the processability is considered excellent.
[0165]
[0166] Experimental Example 2
[0167] Each of the thermoplastic resin compositions according to Reference Example 1, Reference Example 2, and Comparative Example 1 was extruded and injected to manufacture specimens, a notch was formed in each specimen, and the specimen was cut in half through the notch to form an impact specimen. The impact specimen was cut into a 1 cm triangular block, and then the block was trimmed to a size of 100 ㎛ * 200 ㎛ using an ultra-microtome (Leica product name: FC7 / UC5) at room temperature, placed in a container containing OsO4 crystals, sealed well, and left at room temperature for about 2 days to perform dyeing. Thereafter, the dyed block was washed with distilled water, and the block was sectioned at a thickness of 80 nm and a speed of 1 mm / s using an ultra-microtome (Leica product name: FC7 / UC5) at room temperature to obtain thin sections. TEM images were observed for the above thin sections using a TEM analysis device (Jeol, product name JEM-1400) under 120 kV conditions. The observed TEM images are shown in Figs. 1 to 3.
[0168]
[0169] Example 123456 Regenerated resin (parts by weight) 757575757585 New graft copolymer Small-diameter rubber particle size 100 nm 100 nm 100 nm 80 nm 200 nm 100 nm Large-diameter rubber particle size 320 nm 320 nm 320 nm 320 nm 320 nm Small-diameter rubber particle ratio 15.38% 12.72% 42.86% 15.38% 15.38% 42.86% Content (parts by weight) 1313131313 New non-graft copolymer (parts by weight) 12121212122 Thermoplastic resin composition Impact strength (1 / 4``)17.817.120.318.51819Tensile strength402395420405400395Fluid index28.528.826.028.028.830.2
[0170] Comparative Example 123456 Regenerated resin (parts by weight) 757575757585 New graft copolymer Small-diameter rubber particle size -100 nm 100 nm 70 nm 230 nm - Large-diameter rubber particle size 320 nm 320 nm 320 nm 320 nm 320 nm 320 nm Small-diameter rubber particle ratio 0% 7.69% 53.85% 15.38% 15.38% 0% Content (parts by weight) 1313131313 New non-graft copolymer (parts by weight) 12121212122 Thermoplastic resin composition Impact strength (1 / 4``)15.816.020.114.313.215.0Tensile strength390390423405393365Fluid index29.128.524.227.029.030.9
[0171] Comparative Example 789 Regenerated resin (parts by weight) 606090 New graft copolymer Small-diameter rubber particle size---Large-diameter rubber particle size 320 nm 320 nm 320 nm Small-diameter rubber particle ratio 0% 0% 0% Content (parts by weight) 132010 New non-graft copolymer (parts by weight) 27200 Thermoplastic resin composition Impact strength (1 / 4``) 14.7 19.5 14.9 Tensile strength 454 370 374 Flow index 24.2 25.2 33.0
[0172] Referring to Tables 1 to 3, it was confirmed that the resin compositions of Examples 1 to 6, in which the particle size of the small-diameter conjugated diene polymer was 75 nm or more and 220 nm or less, the particle size of the large-diameter conjugated diene polymer was 250 nm or more and 400 nm or less, and the proportion of the small-diameter conjugated diene polymer was 8 wt% or more and 50 wt% or less with respect to the total content of the small-diameter conjugated diene polymer and the large-diameter conjugated diene polymer, had excellent impact strength, tensile strength, and flow index.
[0173] In addition, referring to FIGS. 1 to 3, in the case of Reference Example 1, which does not include a new graft copolymer composition, cavitation was not formed inside the graft copolymer in the resin composition, but in the cases of Reference Example 2 and Comparative Example 1, which include a new graft copolymer composition, it was confirmed that cavities were formed inside the new graft copolymer in each resin composition and observed as white.
[0174]
[0175] It was confirmed that the resin compositions of Comparative Examples 1 and 6, which did not contain a small-diameter conjugated diene polymer, had significantly lower impact strength than the resin compositions of Examples 1 to 6.
[0176]
[0177] It was confirmed that the resin composition of Comparative Example 2, in which the proportion of the small-diameter conjugated diene polymer was less than 8 wt% with respect to the total content of the small-diameter conjugated diene polymer and the large-diameter conjugated diene polymer, had a significantly lower impact strength than the resin compositions of Examples 1 to 6.
[0178]
[0179] It was confirmed that the resin composition of Comparative Example 3, in which the proportion of the small-diameter conjugated diene polymer exceeds 50 wt% with respect to the total content of the small-diameter conjugated diene polymer and the large-diameter conjugated diene polymer, had a significantly lower fluidity index compared to the resin compositions of Examples 1 to 6.
[0180]
[0181] It was confirmed that the resin composition of Comparative Example 4, in which the particle size of the small-diameter conjugated diene polymer was less than 75 nm, and the resin composition of Comparative Example 5, in which the particle size exceeded 220 nm, had significantly lower impact strength than the resin compositions of Examples 1 to 6.
[0182]
[0183] Meanwhile, the resin compositions of Comparative Examples 7 to 9 differ only in the contents of the recycled resin, the new graft copolymer, and the new non-graft copolymer, respectively, compared to the thermoplastic resin compositions of Comparative Examples 1 and 6. It was confirmed that the resin composition of Comparative Example 7, in which the recycled resin content was less than 70 parts by weight and the new non-graft copolymer content exceeded 15 parts by weight, had improved tensile strength, but significantly lowered impact strength and fluidity index, and the resin composition of Comparative Example 8, in which the recycled resin content was less than 70 parts by weight and the new graft copolymer content exceeded 18 parts by weight, secured impact strength, but significantly lowered fluidity index and tensile strength, and the resin composition of Comparative Example 9, in which the recycled resin content exceeded 88 parts by weight and did not include the new non-graft copolymer, had significantly lowered impact strength and tensile strength.
Claims
1. Comprising a regenerated resin, a new graft copolymer composition and a new non-graft copolymer, The above novel graft copolymer composition is, A first graft copolymer comprising a first conjugated diene polymer having an average particle diameter of 75 nm or more and 220 nm or less; and A second graft copolymer comprising a second conjugated diene polymer having an average particle diameter of 250 nm or more and 400 nm or less, A resin composition wherein the new graft copolymer composition comprises the first conjugated diene polymer in an amount of 8 wt% or more and 50 wt% or less based on the total content of the first conjugated diene polymer and the second conjugated diene polymer.
2. In paragraph 1, A resin composition comprising the regenerated resin in an amount of 70 parts by weight or more and 88 parts by weight or less, based on 100 parts by weight of the regenerated resin, the new graft copolymer composition, and the new non-graft copolymer.
3. In paragraph 1, A resin composition comprising the regenerated resin in an amount of 75 parts by weight or more and 85 parts by weight or less, based on 100 parts by weight of the regenerated resin, the new graft copolymer composition, and the new non-graft copolymer.
4. In paragraph 1, A resin composition comprising 10 to 18 parts by weight of the new graft copolymer and 1 to 15 parts by weight of the new non-graft copolymer, based on 100 parts by weight of the contents of the regenerated resin, the new graft copolymer composition, and the new non-graft copolymer.
5. In paragraph 1, A resin composition wherein the new graft copolymer composition comprises the first conjugated diene polymer in an amount of 10 wt% or more and 43 wt% or less based on the total content of the first conjugated diene polymer and the second conjugated diene polymer.
6. In paragraph 1, A resin composition wherein the average particle diameter of the first conjugated diene polymer is 78 nm or more and 208 nm or less.
7. In paragraph 1, The above-mentioned recycled resin has an Izod impact strength of 7 kg·cm / cm or more and 12 kg·cm / cm or less as measured according to ASTM D256, A resin composition having a flow index of 25 g / 10 min or more and 35 g / 10 min or less as measured according to ASTM D1238.
8. In paragraph 1, The above resin composition has an Izod impact strength of 17.0 kg·cm / cm or more as measured according to ASTM D256, Tensile strength measured according to ASTM D638 is 395 kg / cm 2 That's all, A resin composition having a flow index of 26.0 g / 10 min or more as measured under the conditions of 220°C and 10 kg according to ASTM D1238.
9. In paragraph 1, The above non-graft copolymer comprises an aromatic vinyl monomer unit and a vinyl cyan monomer unit, A resin composition wherein the first graft copolymer and the second graft copolymer each further comprise an aromatic vinyl monomer unit and a vinyl cyan monomer unit.
10. In paragraph 1, When the cross-section of the impact specimen of the above resin composition was observed using a TEM image, A resin composition in which cavitation is observed inside the first graft copolymer and the second graft copolymer.
11. A step of preparing a new graft copolymer composition by performing graft polymerization in the presence of a first conjugated diene polymer latex including a first conjugated diene polymer having an average particle diameter of 75 nm or more and 220 nm or less and a second conjugated diene polymer latex including a second conjugated diene polymer having an average particle diameter of 250 nm or more and 400 nm or less; and A step of mixing the newly produced graft copolymer composition, the regenerated resin, and the newly produced non-graft copolymer, A method for producing a resin composition, wherein the new graft copolymer is produced by including the first conjugated diene polymer in an amount of 8 wt% or more and 50 wt% or less based on the total content of the first conjugated diene polymer and the second conjugated diene polymer.
Citation Information
Patent Citations
ABS resin composition using recycled resin and method of manufacturing the same
KR1020160144185A
Thermoplastic resin composition and molded article using the same
JP2019119874A
Thermoplastic resin composition with good mechanicalproperties, weatherability and colorability
KR1020070073230A
Thermoplastic resin composition having improved impact resistance and gloss
KR1020110118022A
Thermoplastic resin composition having improved impact resistance, scratch resistance and gloss
KR1020110120146A