Method for manufacturing aluminum nitride

The method of synthesizing aluminum nitride by heating aluminum hydride powder below 1000°C in a controlled atmosphere addresses the high-temperature challenges of conventional methods, achieving high-purity AlN with reduced energy and carbon footprint.

WO2024248470A1PCT designated stage expired Publication Date: 2024-12-05ALINK CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/007293
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-01
Filing Date
2024-05-29
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional methods for producing aluminum nitride require high temperatures, making them energy-intensive, costly, and challenging to achieve high purity, while also generating excessive carbon emissions.

Method used

A method involving the preparation of aluminum hydride (AlH3) powder, which is heated below 1000°C in a controlled atmosphere with low moisture and oxygen levels, allowing for the synthesis of high-purity aluminum nitride (AlN) at lower temperatures, reducing energy consumption and carbon production.

Benefits of technology

This approach enables the production of high-purity AlN powder at lower temperatures, reducing energy usage and manufacturing costs, and minimizing carbon emissions, while maintaining excellent thermal and electrical insulation properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024007293_05122024_PF_FP_ABST
    Figure KR2024007293_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing aluminum nitride. The present invention provides a method capable of manufacturing aluminum nitride at a low process temperature. The method for manufacturing aluminum nitride, according to an embodiment of the present invention, comprises the steps of: preparing AlH3 powder; heating the AlH3 powder to less than 1000°C in an N2 atmosphere; and cooling the AlN powder formed by heating the AlH3 powder.
Need to check novelty before this filing date? Find Prior Art

Description

Aluminum nitride manufacturing method

[0001] The present invention relates to a method for producing aluminum nitride. The present invention provides a method capable of producing aluminum nitride at a low processing temperature.

[0002] Aluminum nitride (AlN) is a solid nitride of aluminum, with a thermal conductivity of up to 321 W / (m·K), which is more than 10 times that of alumina, and an electrical conductivity of 10 -11 10 inland -13 Ω -1 ·cm -1 As such, aluminum nitride has excellent thermal conductivity and electrical insulation properties, so it is widely used as an electronic device material and heat dissipation material.

[0003] There are several methods for manufacturing aluminum nitride, including carbothermal reduction, chemical vapor synthesis, and plasma synthesis. The carbothermal reduction method is a method that produces AlN and CO by reacting Al2O3, C(CH4), and N2. The chemical vapor synthesis method uses a chemical vapor method to react AlCl3 and NH3 to produce AlN and NH4Cl. The plasma synthesis method produces AlN by striking the target aluminum metal with plasma in an ammonia or nitrogen atmosphere. Conventional manufacturing methods all have the disadvantage of being difficult to meet process conditions and high manufacturing costs because they are performed at temperatures close to or higher than 1000℃. Japanese Patent Publication No. 6345533, a prior art document, discloses a method for producing aluminum nitride by reducing alumina granules using a reduction method, but it is not suitable for obtaining high-purity aluminum nitride and has the same problem as the prior art in that it reacts by heating at a high temperature of 1580 to 1900°C.

[0004] The purpose of the present invention is to provide a manufacturing method capable of manufacturing aluminum nitride at a low temperature.

[0005] In addition, the present invention can produce high-purity, fine powder-form aluminum nitride.

[0006] In addition, the present invention can reduce the amount of energy used and the amount of carbon generated when manufacturing aluminum nitride.

[0007] Additionally, the present invention can reduce manufacturing costs.

[0008] A method for manufacturing aluminum nitride according to an embodiment of the present invention comprises the steps of preparing AlH3 powder; heating the AlH3 powder to less than 1000°C in an N2 atmosphere; and cooling AlN powder formed by heating the AlH3 powder.

[0009] In the above heating step, the heating temperature may be 600 to 900°C.

[0010] The above heating step can be performed in an N2 atmosphere in which the concentration of moisture and oxygen is maintained at 100 ppm or less.

[0011] The step of preparing AlH3 powder may include a step of dissolving AlCl3 and LiAlH4 in a solvent and reacting them; a step of removing a precipitate produced by the reaction from the solution; and a step of producing AlH3 powder while supplying an inert gas to the solution from which the precipitate has been removed.

[0012] A method for producing aluminum nitride according to an embodiment of the present invention can produce aluminum nitride at a low temperature.

[0013] In addition, the present invention can produce high-purity, fine powder-form aluminum nitride.

[0014] In addition, the present invention can reduce the amount of energy used and the amount of carbon generated when manufacturing aluminum nitride.

[0015] Additionally, the present invention can reduce manufacturing costs.

[0016] Figure 1 shows the XRD analysis results of AlH3 powder manufactured according to an embodiment of the present invention.

[0017] Figures 2 to 4 are XRD analysis results of AlN powder manufactured according to an embodiment of the present invention.

[0018] Figure 5 is an SEM photograph of the AlN powder of Example 3.

[0019] Figure 6 is the XRD analysis result before heat treatment of Al powder, which is comparative example 1 of the present invention.

[0020] Figure 7 is the XRD analysis result after heat treatment of Al powder, which is comparative example 1 of the present invention.

[0021] Fig. 8(a) is a photograph of the AlN powder of Comparative Example 1 (after heat treatment), and Fig. 8(b) is a SEM photograph of Comparative Example 1 (after heat treatment).

[0022] Hereinafter, preferred embodiments of the present invention will be described with reference to the attached drawings. However, the embodiments of the present invention may be modified in various other forms, and the scope of the present invention is not limited to the embodiments described below. In addition, the embodiments of the present invention are provided so that a person having average knowledge in the art can more completely explain the present invention. Throughout the specification, the term "including" a certain component does not exclude other components, but rather means that other components may be included, unless specifically stated otherwise.

[0023]

[0024] A method for manufacturing aluminum nitride according to an embodiment of the present invention comprises the steps of preparing AlH3 powder; heating the AlH3 powder to less than 1000°C in an N2 atmosphere; and cooling AlN powder formed by heating the AlH3 powder.

[0025]

[0026] The AlH3 powder prepared in the step of preparing the above AlH3 powder may be fine and of high purity. In one embodiment, the AlH3 powder may be prepared by solution reaction of AlCl3 and LiAlH4. By using the AlH3 powder prepared in this manner, high-purity AlN powder can be prepared even at low temperatures. The AlH3 powder may have an average particle size of several to several hundred µm, preferably 1 to 10 µm.

[0027] The method for producing AlH3 powder in this step may include a step of dissolving AlCl3 and LiAlH4 in a solvent and reacting them; a step of removing a precipitate produced by the reaction from the solution; and a step of producing AlH3 powder while supplying an inert gas to the solution from which the precipitate has been removed.

[0028] In the step of dissolving AlCl3 and LiAlH4 in a solvent and reacting them, AlCl3 and LiAlH4 are in powder form and can be added in a molar ratio of 1:3, and preferably, LiAlH4 can be added so that the molar ratio to AlCl3 exceeds 1:3. The solvent can be used in an amount that AlCl3 and LiAlH4 can sufficiently dissolve. The solvent is not particularly limited as long as it can dissolve AlCl3 and LiAlH4, and preferably, it can be an organic solvent. In one embodiment, the solvent can be dibutyl ether. This step can be performed using various mixers, stirrers, etc., and can be performed at room temperature. In this step, AlCl3 and LiAlH4 react to produce AlH3 and LiCl, and LiCl can be precipitated as a solid.

[0029] The step of removing the precipitate generated by the reaction from the above solution is a step for removing LiCl and other byproducts. Filtering in this step can utilize various filtering or precipitation methods used in the relevant field and is not particularly limited. In one embodiment, this step can be performed by passing the solution through a paper or fiber filter.

[0030] The step of producing the above AlH3 powder can be performed by various processes, but can be performed while supplying an inert gas such as N2 or Ar in order to produce high-purity AlH3 powder. This is because AlH3 dissolved in a solvent can react rapidly with moisture and oxygen. The inert gas can be supplied heated to a temperature of 200°C or lower, preferably 30 to 50°C. If the temperature of the inert gas exceeds 200°C, some of the produced AlH3 powder is decomposed into Al and H2 again, which causes a problem in that the purity of the AlH3 powder is lowered. The produced AlH3 powder can be obtained through filtering.

[0031] In one embodiment, the step of producing the AlH3 powder may be performed by placing the solution in which AlH3 is produced into a reactor, and a condenser may be installed in the reactor to prevent the AlH3 in the solution from evaporating and disappearing or reacting by exposure to the external environment. In this case, the inert gas may be supplied in the form of bubbles to the solution in which AlH3 is produced, and the bubbles may be supplied in the form of microbubbles or nanobubbles having an average particle size of several tens of nanometers to several hundred micrometers. This allows the bubbles to be evenly distributed throughout the solution in which AlH3 is produced.

[0032]

[0033] Next, a step of heating the prepared AlH3 powder to less than 1000°C in a N2 atmosphere is performed. This step causes the Al nuclei produced during the decomposition of AlH3 to react with N2, and the H2 produced together during the decomposition process to react first with trace amounts of oxygen and moisture that may exist in the surroundings, thereby synthesizing high-purity AlN. The heating temperature in this step may preferably be 600 to 900°C, and more preferably 850 to 950°C.

[0034] Since Al has very good reactivity with oxygen (O2) and moisture (H2O), there is a problem that Al2O3 and Al(OH)3 compounds are formed even at room temperature when oxygen or moisture is present during the decomposition process of AlH3 in the solution. In this case, if an inert gas, particularly a nitrogen (N2) atmosphere, is formed, the Al nuclei formed during the decomposition process do not react with oxygen or moisture, so that they exist as Al nuclei and H2 in the solution. Here, H2 first reacts with a trace amount of oxygen or moisture contained in the supplied nitrogen (N2) gas, thereby preventing the Al nuclei from being oxidized or hydroxylated, and allowing the Al nuclei to react with nitrogen (N2) to synthesize high-purity AlN. Preferably, the oxygen and moisture concentrations of the N2 atmosphere in this step may be 100 ppm or less.

[0035] To explain the reaction in this step more specifically, AlH3 decomposes when heated to temperatures below 1000°C, producing Al nuclei and H2. These Al nuclei are extremely small and have a large surface area, enabling rapid reaction with the surrounding environment. This allows for increased reaction efficiency with N2 even at low temperatures, dramatically reducing the amount of energy used in the production of AlN.

[0036] At this stage, N2 gas can be supplied at a flow rate of 0.5 to 2 l / min, the heating rate can be 3 to 10 ℃ / min, and the heating temperature can be maintained for 1 to 3 hours after reaching the temperature.

[0037]

[0038] Next, the heated reactant can be cooled to obtain AlN. The cooling process can be performed by placing the heated reactant in a furnace and slowly cooling it, and is not particularly limited.

[0039]

[0040] The aluminum nitride manufactured through the above method is in powder form and may have an average particle diameter of several tens of nm to several µm, and preferably, the average particle diameter of the powder may be 1 µm or less.

[0041]

[0042] Manufacturing example: Manufacturing of AlH3 powder

[0043] 8 g each of AlCl3 and LiAlH4 were added to 300 ml of dibutyl ether and stirred at room temperature for 1 hour. After stirring, byproducts were removed by filtration and only the clear solution portion was collected. The solution was transferred to a three-necked flask, and a N2 gas inlet tube was connected to one inlet, a reflux condenser to induce solvent evaporation and condensation was connected to the other inlet, and the final inlet was closed with a rubber stopper. N2 gas heated to 40°C was injected into the three-necked flask at a rate of 100 ml / min, and the reaction was carried out for 4 hours. After completion of the reaction, the solution was poured onto a filter paper in a nitrogen chamber where the oxygen and moisture concentrations were maintained at 100 ppm or less to obtain the precipitated reactant. Isopropyl ether was poured onto the obtained precipitate to remove residual dibutyl ether, and the precipitate was washed and dried to obtain AlH3 powder.

[0044]

[0045] Experimental example: XRD analysis of AlH3 powder

[0046] The XRD of the AlH3 powder manufactured in the manufacturing example was measured using X'pert pro MPD, and the results are shown in Fig. 1. Referring to Fig. 1, it can be confirmed that high-purity AlH3 powder was manufactured.

[0047]

[0048] Manufacturing example: Manufacturing of AlN powder

[0049] Example 1: 1 g of the previously prepared AlH3 powder was placed in a ceramic container and placed in a heat treatment furnace with controlled atmosphere. N2 gas was supplied to the heat treatment furnace at a rate of 1.0 ml / min, and the internal temperature was increased to 700°C at a rate of 5°C / min. After maintaining the furnace in that state for 2 hours, the heat treatment furnace was allowed to cool gradually to cool the product, AlN.

[0050]

[0051] Example 2: AlN was manufactured in the same manner as in Example 1, except that the temperature of the heat treatment furnace was increased to 800°C.

[0052]

[0053] Example 3: AlN was manufactured in the same manner as in Example 1, except that the temperature of the heat treatment furnace was increased to 900°C.

[0054]

[0055] Comparative Example 1: AlN was manufactured in the same manner as in Example 3, except that Al powder with an average particle size of 5 µm was used instead of the previously manufactured AlH3 powder.

[0056]

[0057] Experimental example: SEM and visual observation of AlN

[0058] The AlN of Example 3 and Comparative Example 1 were observed using SEM and with the naked eye. Fig. 5 is an SEM photograph of Example 3, and Fig. 8 is a general photograph (a) and an SEM photograph (b) of Comparative Example 1. In the case of Example 3, it can be confirmed that it was manufactured as a powder with an average particle diameter of 100 nm or less, and no clumping was observed even when observed with the naked eye. In the case of Comparative Example 1, as shown in Fig. 8, it can be seen that clumps were formed rather than powder.

[0059]

[0060] Experimental Example: XRD Analysis of AlN

[0061] XRD analysis was performed on Examples 1 to 3 using X'pert pro MPD, and the results are shown in Figs. 2 to 4, respectively. In addition, XRD analysis was performed on the Al powder used in Comparative Example 1 before and after heat treatment, and the results are shown in Figs. 6 and 7, respectively.

[0062] In Example 1, Al was observed together with AlN, but in Example 2, the Al peak decreased, and in Example 3, the Al peak was not observed. This shows that although AlN is produced by heating at 700°C, higher purity AlN can be produced when the heating process is performed at a higher temperature. In particular, it can be seen that only AlN can be obtained when heating to 900°C. In the case of Comparative Example 1, it was confirmed that AlN, Al, and other substances were present after heat treatment.

[0063]

[0064] The present invention is not limited to the above-described embodiments and the attached drawings, but is intended to be defined by the appended claims. Therefore, those skilled in the art will appreciate that various substitutions, modifications, and alterations may be made without departing from the technical spirit of the present invention as defined in the claims, and such modifications are also within the scope of the present invention.

[0065]

Claims

1. Step of preparing AlH3 powder; A step of heating the above AlH3 powder to less than 1000 ℃ in an N2 atmosphere, and Comprising a step of cooling the AlN powder formed by heating the AlH3 powder, Method for manufacturing aluminum nitride.

2. In paragraph 1, In the above heating step, the heating temperature is 600 to 900 ℃. Method for manufacturing aluminum nitride.

3. In paragraph 1, The above heating step is performed in an N2 atmosphere in which the concentration of moisture and oxygen is maintained at 100 ppm or less. Method for manufacturing aluminum nitride.

4. In paragraph 1, The average particle size of the aluminum nitride powder manufactured by the present method is 1 µm or less. Method for manufacturing aluminum nitride.

5. In paragraph 1, The steps for preparing AlH3 powder are: A step of reacting AlCl3 and LiAlH4 by dissolving them in a solvent; A step of removing a precipitate produced by the reaction from the above solution; and A step of producing AlH3 powder while supplying an inert gas to a solution from which the above precipitate has been removed; Method for manufacturing aluminum nitride.

Citation Information

Patent Citations

  • Process for producing aluminium nitride

    EP1310455A1

  • Apparatus for measuring surface shape by optical heterodyne interference

    JP1992066807A

  • Method for producing aluminum nitride

    JP2755961B2

  • A manufacturing method of aluminum nitride and an aluminum nitride prepared by the same

    KR1020170105783A

  • Component analysis method for designing side sill of green car