Preparation method of isocyanate composition
The method of reacting an amine compound with phosgene and using secondary purification with phenol and p-toluenesulfonyl isocyanate addresses the discoloration issues in isocyanate compounds, achieving stable and transparent isocyanate compositions for optical products.
Patent Information
- Application Number
- PCT/KR2024/095854
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-05-29
- Filing Date
- 2024-05-30
- Publication Date
- 2024-12-05
AI Technical Summary
Isocyanate compounds used in polyurethane production are prone to discoloration and white cloudiness due to their high reactivity, leading to reduced transparency in optical products, as they can oxidize, form self-polymers, and react with other components during storage and processing.
A method involving the reaction of an amine compound with phosgene, followed by thin-film distillation and secondary purification using phenol and p-toluenesulfonyl isocyanate, to control acidity and reduce self-polymers and by-products, thereby enhancing storage stability and transparency.
The method significantly reduces discoloration and haze in isocyanate compositions, ensuring excellent long-term storage stability and transparency, particularly in optical applications like lenses.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
Method for preparing an isocyanate composition
[0001] Cross-citation with related application(s)
[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0069508, filed May 30, 2023, and Korean Patent Application No. 10-2024-0070341, filed May 29, 2024, the entire contents of which are incorporated herein by reference.
[0003] The present invention relates to a method for producing an isocyanate composition that can suppress discoloration and white clouding and improve transparency when applied to a product.
[0004]
[0005] Isocyanates are raw materials for polyurethane, widely used in coatings, adhesives, paints, foams, and optical materials. Polyurethanes used in fields requiring superior appearance properties, particularly optical applications requiring transparency, require minimal discoloration. To achieve this, it is crucial that not only does the polyurethane polymer resist discoloration during the polyurethane reaction, but also that the raw isocyanates themselves, particularly those with higher bifunctionality, remain discoloration-free.
[0006] However, because isocyanates are highly reactive, they are prone to oxidation by oxygen in the air during storage, or to deterioration or discoloration by forming self-polymers. This also causes discoloration or clouding in optical products such as urethane lenses using isocyanates. Furthermore, when producing polyisocyanates through the polymerization of diisocyanates, specifically polyurethane through the urethane conversion reaction of diisocyanates and polyhydric alcohols, the polymers are prone to discoloration due to the catalysts or solvents used in the polymerization reaction.
[0007] In this regard, various methods have been studied and proposed to suppress discoloration in isocyanates, polyisocyanates, and products manufactured using them, such as a method of manufacturing and storing them by sealing them with nitrogen gas to block them from air, or a method of storing them by adding additives such as ultraviolet absorbers.
[0008] Japanese Patent Application Laid-Open No. Hei 2-228317 discloses a method for producing a polyisocyanate for a light-colored polyurethane lacquer, which comprises modifying an isocyanate and then treating it with a peroxide. Japanese Patent Application Laid-Open No. Hei 8-291129 discloses a method for producing an isocyanate with reduced discoloration by contacting a discolored isocyanate with an ozone-containing gas. In addition, Japanese Patent Application Laid-Open No. 2012-506465 discloses a method for producing an isocyanate with reduced discoloration by irradiating the discolored isocyanate with light having a wavelength of 200 to 600 nm.
[0009] However, the above methods could not sufficiently achieve a reduced discoloration effect.
[0010] Another method was proposed, which involved mixing a compound that did not participate in the polymerization reaction with isocyanate and storing it, but there was a problem that the added compound caused discoloration during subsequent product manufacturing.
[0011] Accordingly, research is needed on polyisocyanate compositions that do not cause discoloration or deterioration during the isocyanate synthesis process, storage process, and further product processing process.
[0012]
[0013] The present invention provides a method for producing an isocyanate composition that effectively reduces self-polymers and by-products generated due to the high reactivity of isocyanate compounds during a long-term storage process.
[0014]
[0015] According to one embodiment of the present invention, a method for producing an isocyanate composition is provided, comprising the steps of: obtaining an isocyanate mixture by reacting an amine compound with phosgene in a solvent; performing a first purification by thin-film distillation of the mixture and adding phenol and paratoluenesulfonyl isocyanate; and performing a second purification of the first-purified mixture by thin-film distillation or reduced-pressure distillation.
[0016]
[0017] In addition, according to one embodiment of the present invention, an isocyanate composition manufactured according to the above-described manufacturing method and having excellent long-term storage stability is provided.
[0018]
[0019] In addition, according to one embodiment of the present invention, a polyisocyanate composition is provided, which comprises an isocyanate composition manufactured according to the above-described manufacturing method and a polyisocyanate formed by a polymerization reaction of a polyvalent thiol.
[0020]
[0021] In addition, according to one embodiment of the present invention, an optical article comprising the above-described polyisocyanate composition is provided.
[0022]
[0023] The method for producing an isocyanate composition according to the present invention can effectively reduce self-polymerization and by-products generated due to the high reactivity of the isocyanate compound during a long-term storage process through a secondary purification process using a specific additive.
[0024] Accordingly, the isocyanate composition manufactured according to the present invention exhibits excellent transparency when applied to a product, with significantly reduced discoloration and cloudiness, and can exhibit excellent quality, particularly when applied to an optical lens.
[0025]
[0026] The terminology used herein is for the purpose of describing exemplary embodiments only and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. In this specification, it should be understood that the terms "comprise," "include," or "have" indicate the presence of a feature, number, step, component, or combination thereof, but do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.
[0027] The present invention is susceptible to various modifications and takes various forms. Specific embodiments are illustrated and described in detail below. However, this is not intended to limit the present invention to specific disclosed forms, but rather to encompass all modifications, equivalents, and alternatives falling within the spirit and technical scope of the present invention.
[0028]
[0029] Isocyanate compounds have high reactivity, and are easily oxidized by oxygen in the air during the storage process, or form self-polymers (dimers, trimers, oligomers, etc.) and deteriorate or discolor. In addition, by-products are generated through reactions with other components in the composition, and there is a problem that the transparency of optical articles to which they are applied is reduced.
[0030] To address these issues, the inventors conducted extensive research on the manufacturing and storage processes of isocyanate compositions. They confirmed that even when manufacturing lenses using isocyanate compositions that exhibited yellowing, some products did not exhibit defects. They also discovered that the transparency of a product is affected by white turbidity in addition to yellowing, and that changes in the acidity of the composition during the purification process affect the formation of isocyanate self-polymerization and byproducts.
[0031] When a composition undergoes a secondary purification process using a specific additive, the acidity of the composition is controlled to an appropriate range during a long-term storage process, effectively reducing the production of self-polymers and by-products due to the high reactivity of isocyanate compounds, and accordingly, yellowing and whitening are controlled to an appropriate range, thereby improving the transparency of the final product, thereby completing the present invention.
[0032] In particular, it was confirmed that the reaction rate in the mixing stage prior to thermal polymerization of the lens polymerization solution can be reduced even during lens casting, thereby improving the thermal control efficiency of the polymerization solution and effectively reducing the filter time.
[0033]
[0034] <Method for producing an isocyanate composition>
[0035] A method for producing an isocyanate composition according to one embodiment of the invention comprises the steps of: reacting an amine compound with phosgene in a solvent to obtain an isocyanate mixture; performing a first purification step by thin-film distillation of the mixture and adding phenol and paratoluenesulfonyl isocyanate; and performing a second purification step by thin-film distillation or reduced-pressure distillation of the first-purified mixture.
[0036]
[0037] Here, the isocyanate mixture may include, in addition to the monomer of the isocyanate compound itself, a dimer having a repeating unit of 2 in which two isocyanate compounds are bonded, a trimer having a repeating unit of 3 in which three isocyanate compounds are bonded, and a copolymer having three or more isocyanate compounds bonded. In the present specification, the term 'oligomer' includes all of the dimers, trimers, and polymers of the isocyanate compounds in the isocyanate mixture, and is defined as an isocyanate oligomer having a repeating unit of 2 to 200.
[0038] The above isocyanate compounds are, for example, 1,4-tetramethylene diisocyanate, 1,5-pentamethylene diisocyanate, 1,6-hexamethylene diisocyanate, 1,3-cyclohexylene diisocyanate, 1,4-cyclohexylene diisocyanate, isophorone diisocyanate, norbornene diisocyanate, methylenediphenyl diisocyanate, methylenedicyclohexyl isocyanate, toluene diisocyanate, m-xylylene diisocyanate, p-xylylene diisocyanate, and o-xylylene diisocyanate.
[0039] The oligomer of the above isocyanate compound may be generated by a side reaction during the synthesis of the isocyanate compound from an amine compound, or may be a by-product formed by the highly reactive self-polymerization of the isocyanate compound after the synthesis is complete. The above-mentioned by-products may cause discoloration and clouding of the polyisocyanate composition in which the isocyanate composition is used, as well as the transparency and color of the isocyanate composition itself. Therefore, it is necessary to reduce the content of the above-mentioned by-products in the case of isocyanate compositions used in the optical field. However, in a commercial process, it is difficult to extremely control the content of by-products in terms of process efficiency and cost. Therefore, in the present invention, the self-polymerization and by-products generated due to the high reactivity of the isocyanate compound during a long-term storage process can be effectively reduced through a secondary purification process using a specific additive.
[0040] Hereinafter, the method for manufacturing the above isocyanate composition will be described step by step.
[0041]
[0042] (Synthesis steps of isocyanate compounds)
[0043] It includes a step of reacting an amine compound with phosgene in a solvent to obtain an isocyanate mixture.
[0044] The above isocyanate mixture may include an isocyanate compound (=monomer) and an isocyanate oligomer having a repeating unit of 2 to 200.
[0045] Solvents that can be used in the above phosgenation reaction include aromatic hydrocarbon solvents such as benzene, toluene, xylene, and ethylbenzene; chlorinated aromatic hydrocarbon solvents such as monochlorobenzene, 1,2-dichlorobenzene, and 1,4-dichlorobenzene; and chlorinated hydrocarbon solvents such as dichloromethane, chloroform, and carbon tetrachloride. Two or more of these can be used in combination.
[0046] The amine compound used in the above phosgenation reaction may be, for example, an amine compound obtained by hydrogenating a nitro compound or a chloride thereof. Specifically, the amine compound may be at least one selected from the group consisting of 1,4-tetramethylene diamine, 1,5-pentamethylene diamine, 1,6-hexamethylene diamine, 1,3-cyclohexylene diamine, 1,4-cyclohexylene diamine, isophorone diamine, diamine, methylenediphenyl diamine, methylenedicyclohexyl diamine, toluene diamine, m-xylylene diamine, p-xylylene diamine, and o-xylylene diamine, and salts thereof, and preferably, m-xylylene diamine, p-xylylene diamine, o-xylylene diamine, or a salt thereof.
[0047] The above amine compound may be included in an amount of 1 to 20 parts by weight per 100 parts by weight of the solvent. If the content of the amine compound exceeds 20 parts by weight, there is a risk of precipitation of a large amount of the amine compound. Preferably, the content may be included in an amount of 1 to 15 parts by weight or 3 to 10 parts by weight.
[0048]
[0049] Specifically, the phosgenation reaction can be carried out by a direct phosgenation method (Method 1) in which an amine compound is directly reacted with phosgene; a method in which an amine compound is reacted with anhydrous hydrochloric acid to form an amine-hydrochloride compound and then the formed salt is reacted with phosgene (Method 2); or a method in which an amine compound is reacted with carbonic acid to form an aliphatic amine-carbonate compound and then the formed salt is reacted with phosgene (Method 3).
[0050] The direct phosgenation method of the above method 1 can be performed by reacting an amine compound and phosgene in the above organic solvent. At this time, the phosgene can be introduced all at once at the beginning of the reaction, or can be introduced in part at the beginning of the reaction and the remainder can be introduced in installments during the reaction.
[0051] Meanwhile, the above method 1 can be performed by a first step of dissolving a portion of phosgene in the solvent and then adding the amine compound; and a second step of adding the remaining phosgene after the addition of the amine compound is complete and causing a reaction. At this time, the first step is preferably performed at a temperature of -15°C to -10°C to prevent leakage of highly toxic phosgene and also to prevent rapid heat generation when the amine compound is added, and the phosgenation reaction in the second step can be controlled to 120°C to 140°C so that the reaction can occur at an appropriate reaction rate without concern for decomposition of the amine compound.
[0052] In the case of the above method 2, it can be carried out by a step of reacting an amine compound with hydrochloric acid in an organic solvent to form an amine-hydrochloride compound, and then introducing phosgene to cause the reaction. The formation of the amine-hydrochloride compound can be carried out at a temperature of 30°C or lower, preferably at a temperature of about 23±5°C, and the reaction after the introduction of phosgene can be controlled to 120°C to 140°C. When carried out under such temperature conditions, the solubility of the amine-hydrochloride compound can be increased, and thermal decomposition of the isocyanate can be prevented, thereby producing a high-purity isocyanate compound in high yield.
[0053] In the case of the above method 3, it can be carried out by a step of reacting an amine compound with carbonic acid in a solvent to form an amine-carbonate compound, and then introducing phosgene to cause the reaction. At this time, the formation of the amine-carbonate compound can be carried out at a temperature of 30°C or lower, preferably about 23±5°C, and the reaction after the introduction of phosgene can be controlled to 80°C to 180°C. Preferably, it can be in the range of 100°C or higher, or 120°C or higher, and 150°C or lower, or 140°C or lower. When carried out under such temperature conditions, the solubility of the amine-carbonate compound is increased, and thermal decomposition of the isocyanate is prevented, thereby producing a high-purity isocyanate compound in a high yield.
[0054] It is preferable to perform the manufacturing reaction of an isocyanate compound according to the above method 2 because it is possible to control the formation of isocyanate oligomers and by-products manufactured by the phosgenation reaction within an appropriate range, and also to control the color of the composition within an appropriate range. Accordingly, the composition can satisfy mathematical equation 1.
[0055] After the reaction with phosgene is completed according to each method, a removal process such as nitrogen bubbling for unreacted phosgene and hydrogen chloride gas and a solvent removal process such as distillation may be optionally further performed, and these processes may be performed according to a conventional method.
[0056]
[0057] (1st purification stage)
[0058] Next, the mixture is subjected to thin film distillation, and a step of primary purification is included by adding phenol and paratoluenesulfonyl isocyanate.
[0059] The above first purification step reduces the oligomer content within the mixture through a thin-film distillation process and maintains the acidity of the composition within an appropriate range by adding phenol and paratoluenesulfonyl isocyanate. In particular, the second purification step described below enables the final composition to exhibit excellent storage stability and physical properties.
[0060] First, the thin film distillation process (TFE) is performed using a thin film distillation device. The mixture to be separated is introduced into the device, and as a rotating body such as a wiper rotates, heat is applied to the thin film, and the desired component is separated according to the boiling point.
[0061] In the above first purification step, thin film distillation can be performed at a temperature of 100°C to 170°C, a pressure of 0.001 to 10 kPa, and a rotation speed of 80 to 200 rpm, and thin film distillation is performed within the above range, so that the content of oligomers can be effectively reduced to about 0.3 to 3% (GPC Area%).
[0062] Preferably, the temperature of the thin film purification is 130°C or higher, 140°C or higher, 150°C or higher, 170°C or lower, 160°C or lower, or can be performed at 130°C to 155°C, and it is easy to control the oligomer content within an appropriate range under the above temperature conditions.
[0063] Preferably, the pressure of the thin film purification is 0.001 kPa or more, 0.003 kPa or more, 0.005 kPa or more, 10 kPa or less, 8 kPa or less, 5 kPa or less, or can be performed at 0.001 to 5.0 kPa, and it is easy to control the oligomer content within an appropriate range under the above pressure conditions.
[0064] Here, the rotation speed of the thin film purification means the rotation speed of a rotor (e.g., a wiper) within the device, and is preferably 90 rpm or more, 110 rpm or more, 130 rpm or more, 300 rpm or less, 200 rpm or less, or can be performed at 130 to 180 rpm, and it is easy to control the oligomer content within an appropriate range under the pressure conditions.
[0065]
[0066] Next, a first purification step is performed by adding phenol and paratoluenesulfonyl isocyanate after thin film distillation.
[0067] Here, paratoluenesulfonyl isocyanate refers to a component different from the above-mentioned isocyanate compound.
[0068] When the above phenol and paratoluenesulfonyl isocyanate are used in combination, it is easy to control the content range of oligomers among the components included in the phosgenation reaction mixture by maintaining the acidity of the composition within an appropriate range, and at the same time, it is easy to control the color of the composition.
[0069] The acidity of the above-mentioned primary purified mixture may be 100 to 300 ppm, preferably 100 to 250 ppm, or 110 to 180 ppm. When the above-mentioned acidity range is achieved, the oligomer content in the composition can be controlled after the secondary purification process described below, and the long-term storage stability of the composition can be further improved, which is preferable.
[0070] Here, acidity, specifically, was calculated according to the following mathematical formula 1 using the measured value obtained by performing potentiometric titration with a 0.01 N potassium hydroxide (KOH) methanol solution on the isocyanate composition. The conditions of the measurement method will be described in detail in the experimental examples below.
[0071] [Mathematical Formula 1]
[0072] Acidity (as HCl) (ppm) = [(AB) * N * f * 36.5 * 106] / (C * 103)
[0073] In the above mathematical formula 1,
[0074] A: Volume (ml) of KOH methanol solution consumed in titration of isocyanate composition sample
[0075] B: Volume (ml) of KOH methanol solution consumed in the blank titration
[0076] N: Normality of KOH methanol solution
[0077] f: When the normal concentration of the KOH methanol solution used for measurement changes, this is a correction factor to make it the same as the 0.01 N KOH methanol solution. It is measured according to ASTM D-1638 and TOLOCHIMIE 04-01-68. For a 0.01 N KOH methanol solution, the f value is 1.
[0078] C: Weight of isocyanate composition sample (g)
[0079] The above phenol is added in an amount of 50 to 1,500 ppm, preferably 100 to 1,300 ppm, or 200 to 800 ppm, based on the total weight of the isocyanate mixture. By using it in combination with paratoluenesulfonyl isocyanate in the above range, the content of oligomers in the mixture and the acidity of the composition are controlled within an appropriate range, thereby improving the long-term storage stability of the composition and simultaneously improving transparency and color characteristics when applied to a product.
[0080] The above paratoluenesulfonyl isocyanate is a different compound from the isocyanate compound synthesized in the step of obtaining the above-described isocyanate mixture. Here, the paratoluenesulfonyl isocyanate is added in an amount of 50 to 2,000 ppm based on the total weight of the isocyanate mixture, and preferably, 100 to 1,500 ppm, or 500 to 1,200 ppm. By using it in combination with phenol in the above range, the content of oligomers in the mixture and the acidity of the composition are controlled within an appropriate range, thereby improving the long-term storage stability of the composition and, at the same time, improving transparency and color characteristics when applied to a product.
[0081]
[0082] According to one embodiment of the invention, in addition to phenol and paratoluenesulfonyl isocyanate, triphenyl phosphate may be further included in the primary purification process. When this is used, the desired effect can be easily achieved due to the synergistic effect with phenyl and paratoluenesulfonyl isocyanate. The triphenyl phosphate may be included in an amount of 10 to 500 ppmw, preferably 50 to 400 ppmw, or 90 to 300 ppmw, based on the total content of the isocyanate mixture.
[0083] The addition steps of the above phenol, paratoluenesulfonyl isocyanate, and triphenyl phosphate can each be carried out under nitrogen charging.
[0084]
[0085] According to one embodiment of the invention, the first purification step may further include an additional reduced pressure distillation process for removing solvent and low-boiling point impurities prior to thin film distillation. The conditions for performing the reduced pressure distillation process are not particularly limited, but may be performed using a distillation tower such as a plate tower. More preferably, it may be performed as a reduced pressure distillation process for removing the solvent, followed by a reduced pressure distillation process for controlling low-boiling point impurities.
[0086]
[0087] (2nd purification stage)
[0088] Next, a step of secondary purification is included by thin film distillation or reduced pressure distillation of the above-mentioned primary purified mixture.
[0089] The above-mentioned secondary purification step is a process for further improving the storage stability of the composition controlled within the appropriate acidity range in the primary purification process, and further reduces the content of oligomers within the mixture through a thin film distillation or reduced pressure distillation process of the primary purified mixture, thereby maintaining the acidity of the composition within the appropriate range.
[0090]
[0091] First, the thin film distillation process (TFE, Thin Film Evaporation) is performed using a thin film distillation device of the same type as the primary purification process described above. After the mixture to be separated is introduced into the device, heat is applied to the thin film as a rotating body such as a wiper rotates, and the desired component is separated according to the boiling point.
[0092] In the above-mentioned second purification step, thin film distillation can be performed at a temperature of 100°C to 170°C, a pressure of 0.001 to 1.0 kPa, and a rotation speed of 300 to 500 rpm, and thin film distillation is performed within the above range, so that the content of oligomers can be effectively reduced to about 1.5% (GPC Area%) or less.
[0093] Preferably, the temperature of the thin film purification is 120°C or higher, 130°C or higher, 140°C or higher, 170°C or lower, or 160°C or lower, or can be performed at 110°C to 170°C or 130°C to 160°C, and it is easy to control the oligomer content within an appropriate range under the above temperature conditions.
[0094] Preferably, the pressure of the thin film purification can be 0.002 kPa or more, 0.005 kPa or more, 0.8 kPa or less, 0.3 kPa or less, or 0.003 to 0.4 kPa, 0.005 to 0.3 kPa, and it is easy to control the oligomer content within an appropriate range under the above pressure conditions.
[0095] Here, the rotation speed of the thin film purification means the rotation speed of a rotor (e.g., a wiper) within the device, and is preferably 200 rpm or more, 350 rpm or more, 450 rpm or less, or 430 rpm or less, or can be performed at 200 to 450 rpm, 350 to 450 rpm, and it is easy to control the oligomer content within an appropriate range under the rotation speed conditions.
[0096] The above-mentioned reduced pressure distillation process is a method of distilling by reducing pressure under a pressure lower than atmospheric pressure, and by distilling under reduced pressure, it can be performed at a lower temperature than atmospheric pressure distillation. The conditions for performing the reduced pressure distillation process include a temperature of 100°C to 170°C, a pressure of 0.001 to 1.0 kPa, and can be performed using a distillation tower such as a plate tower.
[0097] Preferably, the temperature of the above-described decompression purification is 120°C or higher, 130°C or higher, 140°C or higher, or 170°C or lower, or can be performed at 110°C to 170°C or 130°C to 170°C, and it is easy to control the oligomer content within an appropriate range under the above-described temperature conditions.
[0098] Preferably, the pressure of the above-described pressure purification can be performed at 0.002 kPa or more, 0.005 kPa or more, 0.8 kPa or less, 0.3 kPa or less, or 0.003 to 0.4 kPa, 0.005 to 0.4 kPa, or 0.01 to 0.4 kPa, and it is easy to control the oligomer content within an appropriate range under the above-described pressure conditions.
[0099] The acidity of the above-mentioned secondary purified mixture may be 100 to 250 ppm, preferably 100 to 250 ppm, or 110 to 150 ppm. When the above-mentioned acidity range is implemented, it is easy to ultimately control the oligomer content in the composition to about 1.0% or less, and the long-term storage stability of the composition can be further improved, which is preferable.
[0100]
[0101] Next, according to one embodiment of the invention, phenol may be further added in the second purification step.
[0102] When performing secondary purification using the above phenol, it is easy to control the content range of oligomers among the components included in the phosgenation reaction mixture by maintaining the acidity of the composition within the above-mentioned appropriate range, and at the same time, it is easy to adjust the color of the composition.
[0103] The above phenol is added in an amount of 50 to 1,500 ppm, preferably 100 to 1,300 ppm, or 500 to 800 ppm, based on the total weight of the isocyanate mixture. By using it in the above range, the content of the oligomer in the mixture and the acidity of the composition are controlled within an appropriate range, thereby improving the long-term storage stability of the composition and simultaneously improving transparency and color characteristics when applied to a product.
[0104] The above phenol addition step can be carried out under nitrogen charging.
[0105]
[0106] According to one embodiment of the invention, in the second purification step, paratoluenesulfonyl isocyanate, which is different from the isocyanate compound synthesized in the step of obtaining the isocyanate mixture in addition to phenol, may be further included, and it is easier to achieve the desired properties due to the synergistic effect with phenol.
[0107] Here, the paratoluenesulfonyl isocyanate is added in an amount of 50 to 1,500 ppm, preferably 100 to 1,300 ppm, or 500 to 900 ppm, based on the total weight of the isocyanate mixture. By using it in combination with phenol in the above range, the content of oligomers in the mixture and the acidity of the composition are controlled within an appropriate range, thereby improving the long-term storage stability of the composition and simultaneously improving transparency and color characteristics when applied to a product.
[0108] The step of adding the above paratoluenesulfonyl isocyanate can be carried out under nitrogen charging.
[0109]
[0110] According to one embodiment of the invention, when the secondary purification step is performed by thin film distillation, an additional reduced pressure distillation process for removing solvent and low boiling point impurities prior to the thin film distillation may be further included. The conditions for performing the reduced pressure distillation process are not particularly limited, but may be performed using a distillation tower such as a plate tower. More preferably, it may be performed by a reduced pressure distillation process for removing the solvent, followed by a reduced pressure distillation process for controlling low boiling point impurities.
[0111]
[0112] <Isocyanate composition>
[0113] According to another embodiment of the invention, an isocyanate composition manufactured according to the method for manufacturing the above isocyanate composition is provided. The composition is advantageous in that the content of impurities such as oligomers is remarkably low, and the acidity of the composition is controlled within an appropriate range, so that self-polymers or impurities are not easily formed even when stored for a long period of time.
[0114] The above isocyanate composition can be manufactured into a polyisocyanate as described below and applied to various products.
[0115]
[0116] The above isocyanate composition may have a haze of 0.1 to 0.38%, preferably 0.15 to 0.36%, as measured according to ASTM D1003 after 3 months at 5±0.5°C. This confirms that the composition has excellent long-term storage stability. The measurement of the haze was performed after 3 months at room temperature (24±1°C) and atmospheric pressure (1 atm), and more specific details will be described in the experimental examples section described below.
[0117] The above isocyanate composition may have an isocyanate oligomer content of 2 to 200 repeating units, measured according to GPC analysis after 3 months at 5±0.5℃, of 1.0%Area or less, preferably 0.3 to 1.0%Area, or 0.3 to 0.95%Area. Through this, it can be confirmed that the composition has excellent long-term storage stability. The measurement of the oligomer content was performed after 3 months at 5±0.5℃, and more specific details will be described in the experimental examples section described below.
[0118]
[0119] <Polyisocyanate composition>
[0120] According to another embodiment of the invention, a polyisocyanate composition is provided, which comprises an isocyanate composition manufactured according to the method for manufacturing the above isocyanate composition and a polyisocyanate formed by a polymerization reaction of a polyvalent thiol.
[0121]
[0122] The above polythiol is a compound containing two or more thiol groups (-SH) in one molecule, and specifically, it may be a compound having two or more, or three or more, and eight or fewer, or five or fewer thiol groups in the molecule.
[0123] The above polyvalent thiol compounds include, for example, 1,9-dimercapto-3,7-dithianonane, 1,13-dimercapto-3,7,11-trithiatridecane, glycol di(3-mercaptopropionate), 1,4-Dithiane-2,5-diyldimethanethiol, 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 2-mercaptomethyl-1,5-dimercapto-3-thiapentane, trimethylolpropane tri(3-mercaptopropionate), 4,8-di(mercaptomethyl)-1,11-dimercapto-3,6,9-trithiaundecane, 5,9-di(mercaptoethyl)-1,12-dimercapto-3,7,10-trithiadodecane, pentaerythritol Pentaerythritol tetra(3-mercaptopropionate), pentaerythritol tetra(mercaptoacetate), 3,6,9,12-Tetrathiatetradecane-1,14-dithiol, 3,6,10,13-Tetrathiapentadecane-1,8,15-trithiolIt may be at least one selected from the group consisting of 15-trithiol.
[0124]
[0125] The above polymerization reaction is a thiourethane reaction between an isocyanate compound in an isocyanate composition and a thiol group in a polyvalent thiol.
[0126] Specifically, the above polyvalent thiol may be added in an amount such that the molar ratio of the thiol group in the polyvalent thiol is 0.8 or more, or 0.9 or more, and 1.1 or less, or 1.0, per 1 mole of the isocyanate group of the isocyanate compound. If the molar ratio of the thiol group to the isocyanate group is less than 0.8 outside the above molar ratio range, the viscosity of the polymer produced may decrease due to the excess isocyanate group, and thus, the processability may decrease. In addition, if the molar ratio of the thiol group to the isocyanate group exceeds 1.1, the discoloration prevention effect may decrease due to the excess thiol group.
[0127] The above polymerization reaction can be carried out under atmospheric pressure and an inert gas atmosphere such as nitrogen or argon.
[0128] The above polymerization reaction is preferably performed at a temperature range of -15°C or higher, or 0°C or higher, and 20°C or lower, or 15°C or lower, so that the reaction rate can be easily controlled without concern for discoloration and the reaction efficiency can also be increased.
[0129] The above polymerization reaction may be carried out under non-catalytic conditions, or may be carried out in the presence of a catalyst that typically promotes urethane reactions, such as a tin-based or amine-based catalyst. When carried out in the presence of a catalyst, the catalyst may be added together with the isocyanate-based mixture at the step of adding the polythiol.
[0130] The progress of the above polymerization reaction can be estimated by measuring the concentration of isocyanate groups in the polymerization reactant using the n-dibutylamine method using a transfer titration device, or by measuring the refractive index. In the present invention, the polymerization reaction can be performed until the concentration of isocyanate groups in the polymerization reactant reaches the calculated value of the isocyanate groups remaining after reacting with the polyvalent thiol.
[0131] As a result of the polymerization reaction described above, polyisocyanate, specifically polythiourethane, is produced.
[0132] The above polyisocyanate composition may further include additives such as an internal release agent, an ultraviolet absorber, a polymerization initiator, a heat stabilizer, a color corrector, a chain extender, a crosslinking agent, a light stabilizer, a filler, and a photosensitizer, if necessary, and the content thereof may be appropriately determined within a range that does not impair the discoloration and discoloration inhibition properties of the composition.
[0133]
[0134] The above polyisocyanate composition can be used in a wide range of fields due to its excellent physical properties, and can also be used as an optical material requiring excellent appearance properties, particularly transparency, such as eyeglass lenses, camera lenses, plastic lenses, and prisms.
[0135]
[0136] According to another embodiment of the invention, an article comprising the composition or manufactured using the composition is provided.
[0137] At this time, the above-mentioned product may be an optical product such as a spectacle lens, a camera lens, a plastic lens, or a prism.
[0138]
[0139] Hereinafter, the functions and effects of the invention will be described in more detail through specific examples of the invention. However, these examples are provided merely as examples of the invention and do not define the scope of the invention.
[0140]
[0141] [Example 1 and Comparative Example 1: Preparation of isocyanate composition]
[0142] Example 1-1
[0143] (Preparation of isocyanate compound) 471 g of 1,2-dichlorobenzene and 32.5 g of m-XDA with a purity of 99.4% were placed in a flask and stirred while adding anhydrous hydrochloric acid at room temperature (23±5℃). The temperature rose to 50℃ while adding anhydrous hydrochloric acid. After adding a total of 80 g of anhydrous hydrochloric acid for 4 hours, the formed salt was cooled to room temperature and 43 ml of phosgene was added to the reactor, and the reactor temperature was heated to 130℃. From the time of adding phosgene until the end of the reaction, a dry ice-acetone cooler was used to prevent phosgene from leaking out. After the reactor temperature reached 130℃, the reactor temperature was maintained at 125-135℃ for 2 hours so that the reaction solution became transparent. After the solution became transparent, the inside of the reactor was cooled to 80℃ and nitrogen was blown in to cool it.
[0144] (1st purification) The solvent was removed from the reaction mixture by vacuum distillation using a 20-stage plate column under the conditions of a pressure of 10.0 kPa, a bottom temperature of 150°C, and a top temperature of 60°C, and then low-boiling-point impurities were removed by vacuum distillation under the conditions of a pressure of 0.2 kPa, a bottom temperature of 160°C, and a top temperature of 140°C.
[0145] Next, for thin film distillation, the mixture was placed in a thin film distillation device with a rotor rotating at 160 rpm at 150°C and 0.003 kPa, thereby reducing the content of oligomers in the mixture to approximately 3% (GPC Area%).
[0146] Next, nitrogen was charged into the mixture, and pTSI 900 ppmw, Phenol 500 ppmw, and TPP 100 ppmw were added to adjust the acidity of the mixture to 140 ppm (in HCl equivalent).
[0147] (Secondary purification) The first purified mixture was again placed in a thin film distillation device with a rotor rotating at 400 rpm at 150°C and 0.2 kPa for thin film distillation, thereby reducing the content of oligomers in the mixture to approximately 1.0% (GPC Area%).
[0148] Next, nitrogen was charged into the above mixture, and 500 ppm of phenol, which was partially removed during thin film distillation, was additionally added to obtain an XDI composition having a final acidity of 110 ppm (in terms of HCl). Next, nitrogen was charged into the XDI composition, and it was stored under refrigerated conditions at about 5°C for 3 months.
[0149]
[0150] Example 1-2
[0151] An isocyanate composition was manufactured and stored in the same manner as in Example 1-1, except that in the secondary purification process in Example 1-1, 900 ppmw of pTSI was additionally added in addition to phenol, thereby obtaining an XDI composition having a final acidity of 240 ppm (in terms of HCl).
[0152]
[0153] Example 1-3
[0154] An isocyanate composition was manufactured and stored in the same manner as in Example 1-1, except that in the secondary purification process in Example 1-1, the content of phenol was changed to 250 ppmw, thereby finally obtaining an XDI composition having an acidity of 105 ppm (in terms of HCl).
[0155]
[0156] Example 1-4
[0157] An isocyanate composition was manufactured and stored in the same manner as in Example 1-1, except that in the secondary purification process in Example 1-1, thin film distillation was performed at 135°C and 0.02 kPa to obtain an XDI composition having a final acidity of 105 ppm (in terms of HCl).
[0158]
[0159] Example 1-5
[0160] An isocyanate composition was manufactured and stored in the same manner as in Example 1-1, except that in the secondary purification process in Example 1-1, thin film distillation was performed at 135°C and 0.2 kPa to obtain an XDI composition having a final acidity of 105 ppm (in terms of HCl).
[0161]
[0162] Example 1-6
[0163] An isocyanate composition was manufactured and stored in the same manner as in Example 1-1, except that in the secondary purification process in Example 1-1, thin film distillation was performed at 140°C and 0.2 kPa to obtain an XDI composition having a final acidity of 105 ppm (in terms of HCl).
[0164]
[0165] Example 1-7
[0166] An isocyanate composition was manufactured and stored in the same manner as in Example 1-1, except that in the secondary purification process in Example 1-1, thin film distillation was performed at 150°C and 0.02 kPa to obtain an XDI composition having an acidity of 105 ppm (in terms of HCl).
[0167]
[0168] Example 1-8
[0169] An isocyanate composition was prepared and stored in the same manner as in Example 1-1, except that in the secondary purification process in Example 1-1, an XDI composition having a final acidity of 107 ppm (in terms of HCl) was obtained without the addition of phenol.
[0170]
[0171] Example 1-9
[0172] An isocyanate composition was manufactured and stored in the same manner as in Example 1-1, except that in the secondary purification process in Example 1-1, the content of phenol was changed to 1,000 ppmw and reduced pressure distillation was performed at 162°C and 0.25 kPa instead of thin film distillation, thereby finally obtaining an XDI composition having an acidity of 105 ppm (in terms of HCl).
[0173]
[0174] Comparative Example 1-1
[0175] (Preparation of isocyanate compound) 471 g of 1,2-dichlorobenzene and 32.5 g of m-XDA with a purity of 99.4% were placed in a flask and stirred while adding anhydrous hydrochloric acid at room temperature (23±5℃). The temperature rose to 50℃ while adding anhydrous hydrochloric acid. After adding a total of 80 g of anhydrous hydrochloric acid for 4 hours, the formed salt was cooled to room temperature and 43 ml of phosgene was added to the reactor, and the reactor temperature was heated to 130℃. From the time of adding phosgene until the end of the reaction, a dry ice-acetone cooler was used to prevent phosgene from leaking out. After the reactor temperature reached 130℃, the reactor temperature was maintained at 125-135℃ for 2 hours so that the reaction solution became transparent. After the solution became transparent, the inside of the reactor was cooled to 80℃ and nitrogen was blown in to cool it.
[0176] (1st purification) The solvent was removed from the reaction mixture by vacuum distillation using a 20-stage plate column under the conditions of a pressure of 10.0 kPa, a bottom temperature of 150°C, and a top temperature of 60°C, and then low-boiling-point impurities were removed by vacuum distillation under the conditions of a pressure of 0.2 kPa, a bottom temperature of 160°C, and a top temperature of 140°C.
[0177] Next, for thin film distillation, the mixture was introduced into a thin film distillation device with a rotor rotating at 160 rpm at 150°C and 1.5 kPa, thereby reducing the content of oligomers in the mixture to approximately 3% (GPC Area%).
[0178] Next, nitrogen was filled into the mixture, and 500 ppmw of phenol and 100 ppmw of TPP were added to adjust the acidity of the mixture to 12 ppm (in terms of HCl), thereby obtaining an XDI composition.
[0179] Next, the XDI composition was filled with nitrogen and stored under refrigerated conditions at about 5°C for 3 months.
[0180]
[0181] Comparative Example 1-2
[0182] An isocyanate composition was manufactured and stored in the same manner as in Comparative Example 1-1, except that in the first purification process in Comparative Example 1-1, 1000 ppmw of pTSI and 500 ppmw of phenol were added after thin film distillation to adjust the acidity of the mixture to 150 ppm (in terms of HCl) to obtain an XDI composition.
[0183]
[0184] Comparative Example 1-3
[0185] In Comparative Example 1-1, in the first purification process, after thin film distillation, 300 ppmw of EMP and 500 ppmw of Phenol were added to adjust the acidity of the mixture to 108 ppm (in terms of HCl), and then the first purified mixture was put into a thin film distillation device in which the rotor rotates at 400 rpm at 150°C and 0.2 kPa for thin film distillation again, and an XDI composition having an acidity of 103 ppm (in terms of HCl) was finally obtained. An isocyanate composition was manufactured and stored in the same manner as in Comparative Example 1-1, except that the second purification process was performed to obtain an XDI composition having an acidity of 103 ppm (in terms of HCl).
[0186]
[0187] Comparative Example 1-4
[0188] In Comparative Example 1-1, in the first purification process, a phosphonate-based additive (TNPP: Tris Nonylphenyl Phosphite) was added after thin-film distillation to adjust the acidity of the mixture to 140 ppm (in terms of HCl), and then the first-purified mixture was subjected to a second purification process in which the rotor was rotated at 400 rpm at 150°C and 0.2 kPa for thin-film distillation, thereby finally obtaining an XDI composition having an acidity of 120 ppm (in terms of HCl), and an isocyanate composition was manufactured and stored in the same manner as in Comparative Example 1-1.
[0189]
[0190] Comparative Example 1-5
[0191] In Comparative Example 1-1, in the first purification process, 500 ppmw of phenol was added after thin film distillation to adjust the acidity of the mixture to 12 ppm (in terms of HCl), and then the first purified mixture was subjected to reduced pressure distillation at 162°C and 0.25 kPa to obtain an XDI composition having an acidity of 10 ppm (in terms of HCl), except that an isocyanate composition was manufactured and stored in the same manner as in Comparative Example 1-1.
[0192]
[0193] [Experimental Example 1: Analysis of Isocyanate Composition]
[0194] Isocyanates of Example 1 and Comparative Example 1
[0195] (1) Measurement of the Hazen color number (APHA)
[0196] For the isocyanate compositions manufactured in the above examples and comparative examples after 3 months of storage, the Hazen color number (APHA) was measured according to the following method, and the results are shown in Table 1.
[0197] Specifically, APHA was measured using HunterLab's Ultrascan Pro according to the ASTM D1209 method under the following measurement conditions. A lower APHA value indicates better discoloration resistance.
[0198] <APHA 측정 조건>
[0199] Colorimeter: Ultrascan Pro
[0200] Light source: C / 2
[0201] Cell: 10mm quartz
[0202]
[0203] (2) Gel permeation chromatography (GPC) analysis
[0204] Gel permeation chromatography (GPC) analysis was performed on the isocyanate compositions manufactured in the above examples and comparative examples after 3 months of storage, and the resulting oligomer content is shown in Table 1.
[0205] <GPC 분석 조건>
[0206] Device used: Agilent
[0207] Columns: Agilent PL Mixed D, Agilent PLgel 100Å, Agilent PLgel 50Å
[0208]
[0209] Sample concentration: 1 wt / vol% in tetrahydrofuran (THF)
[0210] Carrier: THF
[0211] Detection method: RI
[0212] Flow rate: 1.0 ml / min
[0213] Column temperature: 25℃
[0214] Detector: Agilent RI detector
[0215] When preparing the calibration curve, polystyrene standard foams with molecular weights of 104 to 24,600 g / mol were used.
[0216]
[0217] (3) Purity evaluation
[0218] Purity of the isocyanate compositions manufactured in the above examples and comparative examples after 3 months of storage was measured under the following conditions, and the results are shown in Table 1.
[0219] <GC 분석 조건>
[0220] Device used: Agilent HP-6890
[0221] Column: Agilent HP-5 (30m * 0.320mm * 0.25㎛),
[0222] Sample concentration: 20 wt / vol% in methyl chloride (MC)
[0223] Carrier: Nitrogen (N2)
[0224] Flow rate: 1.0 ml / min
[0225] Oven temperature: 100℃-> 10℃ / min -> 165℃(3 min) -> 20℃ / min -> 300℃(15min
[0226] Detector: FID(Flame Ionization detector)detector
[0227] Injection volume: 1uL
[0228]
[0229] (4) Haze evaluation
[0230] For the isocyanate compositions manufactured in the above examples and comparative examples after 3 months of storage, the haze of the isocyanate compositions was measured according to ASTM D1003 under the following conditions.
[0231] <Haze 측정 조건>
[0232] Colorimeter: Ultrascan Pro
[0233] Light source: C / 2
[0234] Cell: 10 mm quartz
[0235] Classification Oligomer (3 months, GPC area%) APHA Purity (GC area%) Haze% Example 1-10.5 58.1 499.76 0.24 Example 1-20.9 49.3 99.74 0.22 Example 1-30.6 08.8 299.84 0.31 Example 1-40.5 96.8 799.77 0.21 Example 1-50.6 28.2 99.69 0.36 Example 1-60.5 19.2 099.78 0.19 Example 1-70.5 37.9 299.80 0.19 Example 1-80.6 67.5 499.83 0.28 Example 1-90.9 65.3 799.61 0.38 Comparative Example 1-11.03-99.73 Comparative example of white turbidity occurrence 1-22.209.8699.683.53 Comparative example of white turbidity occurrence 1-32.5213.1099.730.39 Comparative example 1-41.2015.1299.650.40 Comparative example 1-513.7-99.45 White turbidity occurrence
[0236] As can be confirmed from the experimental data in Table 1 above, the isocyanate composition according to the present invention significantly reduces the generation of oligomers, by-products, etc. even when stored for a long period of time, and accordingly, discoloration and cloudiness are significantly reduced and excellent transparency is achieved.
[0237]
[0238] [Example 2 and Comparative Example 2]
[0239] Example 2-1: Manufacturing of optical lenses
[0240] 20.8 g of the isocyanate composition manufactured in Example 1-1, 0.04 g of zelec UN (manufactured by Stepan), and 0.04 g of biosorb 583 (manufactured by Sakai Chemical industry Co., Ltd) were mixed in a flask at room temperature with stirring for about 20 minutes to manufacture a polyisocyanate.
[0241] After visually confirming that all components of the polyisocyanate were well mixed, 0.002 g of dibutyltin chloride was added and stirred for 10 minutes. 19.2 g of 2,3-bis(2-sulfanyl ethyl sulfanyl)propane-1-thiol was added to the mixture, and the mixture was degassed under 5 mbar conditions and stirred for 1 hour to prepare a polyisocyanate composition.
[0242] The above polyisocyanate composition was filtered through a 1 μm PTFE filter and then injected into a mold consisting of a glass mold and tape. This mold was placed in an oven and the temperature was gradually increased from 10°C to 120°C, and a polymerization reaction was performed for 20 hours. After polymerization was completed, the mold was removed from the oven and released to obtain a plastic lens. The obtained plastic lens was annealed at 120°C for 6 hours to produce a final optical lens sample.
[0243]
[0244] Examples 2-2 to 2-9 and Comparative Examples 2-1 to 2-5
[0245] In the above Example 2-1, an optical lens was manufactured in the same manner as in Example 1-1 except that the isocyanate compositions of Examples 1-2 to 1-9 and Comparative Examples 1-1 to 1-5 were used instead of the isocyanate composition of Example 1-1.
[0246]
[0247] [Experimental Example 2: Optical Lens Evaluation]
[0248] Classification L*a*b*YI Example 2-194.89-0.541.051.5 Example 2-294.90-0.571.101.6 Example 2-394.92-0.541.011.5 Example 2-494.91-0.491.121.6 Example 2-594.92-0.500.991.5 Example 2-694.86-0.481.051.6 Example 2-794.86-0.521.061.6 Example 2-894.93-0.571.081.6 Example 2-994.94-0.571.111.6 Comparative Example 2-1 Comparative Example of White Turbidity Occurrence 2-2 Comparative example of white turbidity occurrence 2-394.94-0.571.101.7 Comparative example 2-494.88-0.571.101.7 Comparative example 2-5 White turbidity occurrence
[0249] As can be seen from the experimental data in Table 2 above, the isocyanate composition according to the present invention exhibits significantly reduced discoloration and cloudiness, exhibits excellent transparency when applied to a product, and it was confirmed that the YI value of the optical lens was improved compared to the comparative example. For reference, when the YI value exceeds 1.6 and has a value of 1.7 or higher, it can be seen that the physical properties of the product are significantly deteriorated.
Claims
1. A step of reacting an amine compound with phosgene in a solvent to obtain an isocyanate mixture; A step of performing a first purification by thin-film distillation of the above mixture and adding phenol and paratoluenesulfonyl isocyanate; and It includes a step of secondarily purifying the above-mentioned first purified mixture by thin film distillation or reduced pressure distillation, Method for preparing an isocyanate composition.
2. In paragraph 1, In the above second purification step, phenol is further added, Method for preparing an isocyanate composition.
3. In paragraph 1, The acidity of the above first purified mixture is 100 to 300 ppm. Method for preparing an isocyanate composition.
4. In paragraph 1, In the above first purification step, Thin film distillation is performed at a temperature of 100 to 170°C, a pressure of 0.001 to 10 kPa, and a rotation speed of 80 to 200 rpm. Method for preparing an isocyanate composition.
5. In paragraph 1, In the above first purification step, The above phenol is included in an amount of 50 to 1,500 ppmw with respect to the total content of the isocyanate mixture. Method for preparing an isocyanate composition.
6. In paragraph 1, In the above first purification step, The above paratoluenesulfonyl isocyanate is included in an amount of 50 to 2,000 ppmw based on the total content of the isocyanate mixture. Method for preparing an isocyanate composition.
7. In paragraph 1, In the above first purification step, Further comprising 10 to 500 ppmw of triphenyl phosphate relative to the total content of the isocyanate mixture, Method for preparing an isocyanate composition.
8. In paragraph 1, The acidity of the above secondary purified mixture is 100 to 250 ppm. Method for preparing an isocyanate composition.
9. In paragraph 1, In the above second purification step, The above thin film distillation is performed at a temperature of 100 to 170°C, a pressure of 0.001 to 1.0 kPa, and a rotation speed of 300 to 500 rpm. Method for preparing an isocyanate composition.
10. In paragraph 1, In the above second purification step, The above reduced pressure distillation is performed at a temperature of 100 to 170°C, a pressure of 0.001 to 1.0 kPa, and a rotation speed of 300 to 500 rpm. Method for preparing an isocyanate composition.
11. In paragraph 2, In the above second purification step, The above phenol is further included in an amount of 50 to 1,500 ppmw based on the total content of the isocyanate mixture. Method for preparing an isocyanate composition.
12. In paragraph 1, In the above second purification step, Further comprising paratoluenesulfonyl isocyanate in an amount of 50 to 1,500 ppmw based on the total content of the isocyanate mixture. Method for preparing an isocyanate composition.
13. In paragraph 1, The above isocyanate mixture comprises at least one isocyanate compound selected from the group consisting of 1,4-tetramethylene diisocyanate, 1,5-pentamethylene diisocyanate, 1,6-hexamethylene diisocyanate, 1,3-cyclohexylene diisocyanate, 1,4-cyclohexylene diisocyanate, isophorone diisocyanate, norbornene diisocyanate, methylenediphenyl diisocyanate, methylenedicyclohexyl isocyanate, toluene diisocyanate, m-xylylene diisocyanate, p-xylylene diisocyanate, and o-xylylene diisocyanate. Method for preparing an isocyanate composition.
14. An isocyanate composition manufactured according to paragraph 1, A haze of 0.1 to 0.38% as measured according to ASTM D1003 after 3 months at 5±0.5℃, Isocyanate composition.
15. An isocyanate composition manufactured according to paragraph 1, An isocyanate oligomer content of 2 to 200 repeat units measured by GPC analysis after 3 months at 5±0.5℃ is 1.0%Area or less. Isocyanate composition.
16. A polyisocyanate composition comprising a polyisocyanate formed by a polymerization reaction of an isocyanate composition manufactured according to paragraph 1 and a polythiol.
17. An optical article comprising a polyisocyanate composition according to Article 16.
Citation Information
Patent Citations
An isocyanate stabilizer and its preparation method
CN108003072B
Method for stabilizing isocyanate compound and stabilized isocyanate composition
JP1993078304A
Reactive polyurethane compositions with low residualmonomer content
KR1020050033045A
Cultivation method of Cissus quadrangularis
KR102255693B1
Curable compositions containing isocyanate functional components having improved durability
US20140290855A1