Silica heat reflection plate and method for manufacturing same

The silica heat reflecting plate with adjusted OH group content and a laminated structure addresses heat resistance and contamination issues, ensuring high reflectance and longevity for efficient semiconductor processing.

WO2024252930A1PCT designated stage expired Publication Date: 2024-12-12FURUYA KINZOKU KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018844
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-06
Filing Date
2024-05-22
Publication Date
2024-12-12

AI Technical Summary

Technical Problem

Existing silica heat reflectors face issues with heat resistance, contamination, and reduced lifespan due to the melting of thin gold films and challenges in bonding silica plates at high temperatures, leading to poor adhesion and reflectivity in high-temperature semiconductor processing.

Method used

A silica heat reflecting plate with a thin film reflector made of Ir, Pt, Rh, Ru, or Mo, and a bonding method that adjusts the OH group content in silica plates to within 1000 ppm or less, ensuring better adhesion and longevity, along with a laminated structure and oxide layers for improved reflectance and thermal management.

Benefits of technology

The solution provides a silica heat reflecting plate with enhanced heat resistance, reduced contamination, and prolonged lifespan, maintaining high reflectance and adhesion up to 1000°C, optimizing energy efficiency and process yield in semiconductor manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018844_12122024_PF_FP_ABST
    Figure JP2024018844_12122024_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of the present disclosure is to provide: a silica heat reflection plate which withstands use at temperatures up to 1,000°C, and which, in comparison to conventional silica heat reflection plates, maintains better adhesion between a silica plate and a reflector, is better at suppressing deterioration of a metal component of the reflector, has better heat reflection characteristics, has better bondability between silica plates, and has a longer service life; and a method for manufacturing the same. With respect to a silica heat reflection plate according to the present disclosure, a reflector 3 reflects infrared rays L1 that are incident thereon from a first silica plate side, or reflects infrared rays L2 that are incident thereon from a second silica plate side. The first silica plate 1 and the second silica plate 2 have an OH group content of 1,000 ppm or less. The reflector 3 is a thin film. A surface layer including at least a reflection surface of the reflector is formed of one element that is selected from the group consisting of Ir, Pt, Rh, Ru, Re, and Mo, or is formed of an alloy that contains at least one element that is selected from the group consisting of Ir, Pt, Rh, Ru, Re, and Mo, and that has a melting point of 1,200°C or more.
Need to check novelty before this filing date? Find Prior Art

Description

Silica heat reflector and its manufacturing method

[0001] The present disclosure relates to a silica heat reflector that can be used as a heat reflector in various heat treatment devices that heat treat wafers, substrates, etc. at high temperatures, for example in the fields of semiconductors and electronic components, and that has high reflectivity, thereby enabling energy savings in the heat treatment device and suppressing contamination, and a method for manufacturing the same.

[0002] In the manufacturing or processing of semiconductor wafers, heat treatment is performed to impart various properties to the semiconductor wafers. For example, the semiconductor wafers are placed in a furnace core tube made of high-purity quartz, and the heat treatment is performed in a controlled atmosphere inside the furnace core tube. In the heat treatment equipment used in this heat treatment process, a heat retainer (lid) is installed between the furnace interior and the hearth to cover the furnace opening in order to maintain a high temperature inside the furnace and prevent heat dissipation to the hearth.

[0003] One such heat retainer is one that blocks the opening of the heat treatment chamber and has quartz plates stacked at a distance from each other and exposed to the heat treatment chamber. The quartz plates have smooth, bubble-free surfaces and a gold thin film formed inside the quartz plates by gold vapor deposition (see, for example, Patent Document 1).

[0004] A technology has been disclosed in which a thermal insulation structure of a vertical heat treatment furnace is composed of multiple support columns and multiple reflective heat shield plates arranged at predetermined intervals in the vertical direction on the support columns (see, for example, Patent Document 2). According to Patent Document 2, the heat shield plate is formed from a reflective film and a transparent quartz layer covering the surface of the reflective film. One method of forming this heat shield plate is to use a pair of circular transparent quartz plates that form the transparent quartz layer, provide a reflective film on one side of one of the transparent quartz plates, sandwich the reflective film between the other transparent quartz plate, and weld the peripheries of the two transparent quartz plates to seal and integrate them. Another method of forming a heat shield plate is to provide a reflective film on the top surface of the circular transparent quartz plate that forms one of the transparent quartz layers, pour transparent quartz onto the reflective film, and seal the reflective film to form the other transparent quartz layer.

[0005] Also disclosed is a silica heat reflector comprising a silica plate and a reflector disposed inside the silica plate, the outer periphery of which is completely covered by the silica plate, and which reflects infrared rays incident on one surface of the silica plate, wherein the reflector is a thin film, plate, or foil, and the surface layer of the reflector, including at least the reflective surface, is made of Ir, Pt, Rh, Ru, Re, Hf, or Mo, or an alloy containing at least one selected from Ir, Pt, Rh, Ru, Re, Hf, and Mo (see, for example, Patent Document 3). Patent Document 3 discloses a method for bonding the silica plate using surface activated bonding. According to Patent Document 3, a silica heat reflector can be provided that has a high reflectivity by ensuring a higher reflective area ratio than conventional methods, has a small heat capacity, allows for energy savings, suppresses contamination inside the furnace, and has a long life.

[0006] JP 2001-102319 A JP 11-97360 A JP 2022-105255 A

[0007] In Patent Document 1, a gold thin film with high infrared reflectivity is used as the metal reflective film that contributes to infrared reflection. However, the melting point of gold is 1064°C, and the heat treatment temperature during semiconductor wafer manufacturing or processing reaches nearly 90% of the gold melting point, causing problems such as melting, peeling, and shrinkage of the gold thin film, resulting in practical heat resistance issues. Furthermore, bonding of a silica plate is required to encapsulate the gold thin film that contributes to infrared reflection within the silica plate. However, since silica has a very high softening point of 1720°C and an annealing point of 1180°C, melting and bonding the silica plate requires a temperature of at least 1200°C, which precludes the use of materials with low melting points such as gold.

[0008] Patent Document 2 uses a method in which a reflective film is sandwiched between quartz plates and the periphery of the quartz plates is welded. However, the reflective film is susceptible to heat, which can lead to peeling. Furthermore, it is difficult to maintain a vacuum inside, and there is an unavoidable risk of the thin film being damaged by an increase in internal pressure during high-temperature use. Furthermore, other methods for forming heat shields involve pouring transparent quartz, which makes it impossible to avoid thermal and physical damage to the metal thin film.

[0009] In Patent Document 3, a reflector made of a high-melting-point metal material is subjected to surface activation bonding to suppress thermal and physical damage to the metal material. However, since metal silicon used in surface activation bonding and OH groups due to plasma treatment remain on the metal reflector during surface activation bonding, when the silica heat reflector of Patent Document 3 is used for heat treatment in the manufacturing or processing step of semiconductor wafers, if the heat treatment temperature exceeds 800°C, the bonding rate between the silica plates may decrease and the metal reflector may be deteriorated, which may result in a shortened lifespan of the silica heat reflector and a decrease in the yield of the silica heat reflector.

[0010] The present disclosure aims to provide a silica heat reflector that can withstand use up to 1000°C, maintains better adhesion between the silica plate and the reflector than conventional ones, suppresses deterioration of the metal components of the reflector, has good heat reflection properties, has good bonding between the silica plates, and has a long life, and a method for manufacturing the same.

[0011] The present inventors have found, after extensive research, that the above-mentioned problems can be solved by adjusting the content of OH groups in the silica plate to a predetermined range, and have thus completed the present invention. That is, the silica heat reflecting plate according to the present invention comprises a first silica plate, a second silica plate whose surface faces the first silica plate, a reflector provided on at least one of the surface of the second silica plate facing the first silica plate and the surface of the first silica plate facing the second silica plate, and a joining portion in which at least the peripheral portions of the joining surfaces of the first silica plate and the second silica plate are joined continuously in an annular shape along the peripheral edges, and has a structure of a joining plate of the first silica plate and the second silica plate. The reflector is a silica heat reflector that reflects infrared rays incident from the first silica plate side or the second silica plate side, the first silica plate and the second silica plate have an OH group content of 1000 ppm or less, the reflector is a thin film, and a surface layer including at least the reflective surface of the reflector is made of one element selected from the group consisting of Ir, Pt, Rh, Ru, Re and Mo, or an alloy containing at least one element selected from the group consisting of Ir, Pt, Rh, Ru, Re and Mo and having a melting point of 1200°C or higher.

[0012] In the silica heat reflector according to the present invention, it is preferable that the first silica plate and the second silica plate each have an elemental content of Li, Na, K, Ca, Mg, B, Fe, and Cu of 1 ppm or less, and an Al content of 10 ppm or less, thereby suppressing contamination inside a heat treatment furnace.

[0013] In the silica heat reflecting plate according to the present invention, it is preferable that the surface roughness of at least a part of the outer peripheral plane of at least one of the first silica plate and the second silica plate is 5 μm or less in arithmetic mean roughness Ra, which can be appropriately adjusted to increase the reflectivity and disperse the reflected heat.

[0014] In the silica heat reflector according to the present invention, it is preferable that the reflector has a reflectance of 75% or more in the infrared region of 1500 to 2400 nm incident from the first silica plate side or the second silica plate side. Considering the maximum wavelength of thermal radiation when the furnace body temperature is 950°C and the behavior of the reflectance of the metal reflector, it is important to ensure high reflectance in the infrared region of 1500 to 2400 nm.

[0015] In the silica heat reflector according to the present invention, the thickness of the first silica plate and the second silica plate is preferably 0.5 to 2.0 mm, which can suppress energy loss due to heat absorption by the silica heat reflector itself and improve thermal response during heating and cooling of the furnace body.

[0016] In the silica heat reflector according to the present invention, the thickness of the reflector is preferably 50 to 500 nm, which allows the reflector to maintain close contact with the silica plate and efficiently reflect heat.

[0017] In the silica heat reflector according to the present invention, an oxide layer containing one oxide selected from the group consisting of silicon oxide, aluminum oxide, sapphire, lithium tantalate, lithium niobate, magnesium oxide, titanium oxide, yttrium oxide, strontium titanate, germanium oxide, zinc oxide, indium oxide, indium tin oxide, tin oxide, tungsten-doped tin oxide, and tantalum oxide, or an oxide layer containing two or more oxides selected from the group consisting of silicon oxide, aluminum oxide, sapphire, lithium tantalate, lithium niobate, magnesium oxide, titanium oxide, yttrium oxide, strontium titanate, germanium oxide, zinc oxide, indium oxide, indium tin oxide, tin oxide, tungsten-doped tin oxide, and tantalum oxide, is provided at least in one of the positions between the first silica plate and the reflector and between the second silica plate and the reflector, and the thickness of the oxide layer is preferably 50 nm or less. The oxide layer promotes adhesion between the reflector and the silica plate, suppresses heat absorption by the oxide layer, and allows for efficient heat reflection.

[0018] The method for manufacturing a silica heat reflecting plate according to the present invention is characterized by comprising: a first step of preparing a first silica plate and a second silica plate; a second step of forming a reflector on at least one of the surfaces of the first silica plate and the second silica plate; a third step of joining the first silica plate and the second silica plate together with the surfaces of the reflector formed on at least one of the first silica plate and the second silica plate as opposing surfaces; and a fourth step of joining at least the peripheral portions of the opposing surfaces of the first silica plate and the second silica plate.

[0019] In the method for manufacturing a silica heat reflector according to the present invention, it is preferable to carry out a fifth step after the fourth step in which the outer peripheral surfaces of the first silica plate and the second silica plate are polished to adjust the final plate thickness, thereby enabling more accurate adjustment of the final plate thickness.

[0020] In the method for manufacturing a silica heat reflector according to the present invention, it is preferable that in the fourth step, the first silica plate and the second silica plate are bonded together in a vacuum atmosphere of 100 Pa or less, an argon atmosphere, or a nitrogen atmosphere, and then the first silica plate and the second silica plate are bonded together at a pressure of 3500 kPa or less and a temperature of 400 to 1000° C. This can suppress deterioration of the reflector due to oxygen or hydrogen, and deterioration of the reflector due to heat, and maintain the heat reflectance.

[0021] The method for manufacturing a silica thermal reflector according to the present invention preferably further comprises, between the third step and the fourth step, a step A of placing a pressing material made of carbon, oxide, nitride, or boride, or a pressing material containing at least one selected from the group consisting of carbon, oxide, nitride, and boride, at a location in contact with at least the outer circumferential plane of the first silica plate and the second silica plate, which allows the first silica plate and the second silica plate to be joined while suppressing contamination of the reflector by impurities.

[0022] The method for manufacturing a silica heat reflector according to the present invention preferably further comprises, between the third and fourth steps, a step B of preparing a plurality of stacks of first and second silica plates obtained in the third step and stacking 2 to 30 pairs of the stacks in the stacking direction with spacers interposed therebetween, the spacers being made of carbon, oxide, nitride, or boride, or containing at least one selected from the group consisting of carbon, oxide, nitride, and boride, and the fourth step being a step of simultaneously bonding 2 to 30 pairs of the stacked plates. This allows for simultaneous bonding of multiple pairs of first and second silica plates while suppressing bonding of different silica plates, such as a first silica plate and another second silica plate, or another first silica plate and a second silica plate.

[0023] In the method for manufacturing a silica heat reflector according to the present invention, it is preferable that the reflector is formed by any one of sputtering, chemical vapor deposition, and vapor deposition in the second step. This makes it possible to make the thickness of the reflector uniform, thereby making the heat reflectance uniform. Furthermore, the density of the film can be improved, thereby improving the heat reflectance.

[0024] The method for manufacturing a silica thermal reflector according to the present invention preferably further includes, between the first and second steps, a step C of reverse sputtering the surfaces where the first and second silica plates will face each other in the third step. Cleaning the surfaces where the first and second silica plates face each other to remove impurities improves adhesion between the first silica plate and the reflector, the first silica plate and the oxide layer, the second silica plate and the reflector, and the second silica plate and the oxide layer, as well as improving adhesion at the joint between the first and second silica plates at the peripheral portions. Removing the impurities prevents impurities on the surfaces of the first and second silica plates 1 and 2 from coming into contact with and reacting with the surface of the reflector 3, thereby preventing deterioration of the reflector 3.

[0025] The method for producing a silica heat reflector according to the present invention preferably further comprises at least one step selected from the group consisting of step D, in which heat treatment is performed at 1000° C. or less after step 2, and step E, in which heat treatment is performed at 1000° C. or less after step 4. This can improve the density of the reflector and the heat reflectance.

[0026] According to the present disclosure, it is possible to provide a silica heat reflector and a method for manufacturing the same that can withstand use up to 1000°C, maintain better adhesion between the silica plate and the reflector than conventional methods, suppress deterioration of the metal components of the reflector, have good heat reflection properties, good bonding between the silica plates, and have a long life.

[0027] Fig. 1 is a plan schematic diagram showing a silica heat reflector according to the present embodiment. Fig. 2 is a schematic diagram showing a first example of the A-A cross section of the silica heat reflector shown in Fig. 1. Fig. 3 is a schematic diagram showing a third example of the A-A cross section of the silica heat reflector shown in Fig. 1, which is a schematic diagram of a silica heat reflector having an oxide layer between the silica plate and the reflector. Fig. 4 is a schematic diagram showing a fourth example of the A-A cross section of the silica heat reflector shown in Fig. 1, which is a schematic diagram of a silica heat reflector having oxide layers between the first reflector and the first silica plate, and between the second reflector and the second silica plate. 2A is a schematic diagram showing a method for manufacturing a silica heat reflector of the first example shown in Figure 2, (a) shows a first step of preparing a first silica plate and a second silica plate, (b) shows a second step of forming a reflector on the surface of the first silica plate, (c) shows a third step of joining the first silica plate and the second silica plate with the surface of the reflector formed on the first silica plate as the opposing surface, and (d) shows a fourth step of bonding at least the peripheral portions of the opposing surfaces of the first silica plate and the second silica plate. 3A is a schematic diagram showing a method for manufacturing a silica heat reflector of the second example shown in Figure 3, (e) shows a first step of preparing a first silica plate and a second silica plate, (f) shows a second step of forming a reflector on both the surface of the first silica plate and the surface of the second silica plate, (g) shows a third step of joining the first silica plate and the second silica plate with the surface of the reflector formed on the first silica plate facing the surface of the reflector formed on the second silica plate, and (h) shows a fourth step of bonding at least the peripheral portions of the opposing surfaces of the first silica plate and the second silica plate. FIG. 7 is a schematic diagram showing another example of the steps performed following the first step (a), the second step (b), and the third step (c) shown in FIG. 6, in which (c-1) shows step B in which a plurality of stacks of the first silica plate and the second silica plate obtained in the third step are prepared and 2 to 30 sets of the stacks are stacked in the stacking direction with spacers in between, and (d-1) shows the fourth step in which each of the 2 to 30 sets of stacked stacks is simultaneously bonded.7 is a schematic diagram showing another example of steps performed subsequent to the first step (e), the second step (f), and the third step (g) shown in FIG. 7, where (g-1) shows step B in which a plurality of stacks of first silica plates and second silica plates obtained in step 3 are prepared and 2 to 30 sets of the stacks are stacked in the stacking direction with spacers interposed therebetween, and (h-1) shows step 4 in which each of the 2 to 30 stacked sets is simultaneously bonded.

[0023] FIG. 1 is a graph showing the results of measuring the reflectance of a silica heat reflector according to Example 1 using a spectrophotometer.

[0024] FIG. 2 is a graph showing the results of measuring the reflectance of a silica heat reflector according to Example 2 using a spectrophotometer.

[0025] FIG. 3 is a graph showing the results of measuring the reflectance of a silica heat reflector according to Comparative Example 1 using a spectrophotometer.

[0026] FIG. 4 is a graph showing the relationship between the arithmetic mean roughness Ra and reflectance in Example E.

[0028] Hereinafter, the present invention will be described in detail with reference to the embodiments, but the present invention is not limited to these descriptions. Various modifications may be made to the embodiments as long as the effects of the present invention are achieved.

[0029] (Mode in which a reflector is formed on a first silica plate) A silica heat reflector according to this embodiment will be described with reference to Figures 1 and 2. The silica heat reflector 100 according to this embodiment includes a first silica plate 1, a second silica plate 2 whose surface faces the first silica plate 1, a reflector 3 provided on the surface of the first silica plate 1 facing the second silica plate 2, and a joint 4 formed by continuously joining the first silica plate 1 and the second silica plate 2 in a ring shape along at least the peripheral edge of the joining surface. The silica heat reflector 100 has a structure in which the first silica plate 1 and the second silica plate 2 are joined together, and the reflector 3 is formed on the first silica plate 1. a heat reflector that reflects infrared rays incident from the first silica plate side or the second silica plate side, wherein the first silica plate (1) and the second silica plate (2) have an OH group content of 1000 ppm or less, the reflector (3) is a thin film, and the surface layer of the reflector (3) including at least the reflective surface is made of one element selected from the group consisting of Ir, Pt, Rh, Ru, Re, and Mo, or an alloy containing at least one element selected from the group consisting of Ir, Pt, Rh, Ru, Re, and Mo and having a melting point of 1200°C or higher.

[0030] (Mode in which reflectors are formed on first and second silica plates) As shown in FIGS. 1 and 3 , the reflector 3 is preferably provided on both the first silica plate 1 and the second silica plate 2. When a silica plate with a reflective film and a silica plate without a reflective film are combined, voids are likely to occur. Therefore, it is preferable to provide a reflective film on both silica plates and then bond them together. In the silica heat reflector 200, a first reflector 3a (hereinafter sometimes simply referred to as "reflector 3") is provided on the first silica plate 1, and a second reflector 3b (hereinafter sometimes simply referred to as "reflector 3") is provided on the second silica plate 2, and the first reflector 3a and the second reflector 3b are bonded together. This can further increase the reflectivity. Furthermore, peeling due to film stress is less likely to occur. Furthermore, it is more preferable that the first reflector 3a and the second reflector 3b are bonded together. Hereinafter, the first reflector 3a and the second reflector 3b will sometimes be referred to as "reflector 3" without distinguishing them from the reflector 3.

[0031] (Composition of Reflector) The surface layer of the reflector 3, including at least the reflective surface, is made of one element selected from the group consisting of Ir, Pt, Rh, Ru, Re, and Mo, or an alloy containing at least one element selected from the group consisting of Ir, Pt, Rh, Ru, Re, and Mo and having a melting point of 1200°C or higher. When a Si substrate on which a circuit or the like is formed is heat-treated in a semiconductor heat treatment furnace, a silica heat reflector is used at around 1000°C. If the reflector 3 is made of the above metal or alloy, dissolution or softening of the reflector 3 can be prevented. If dissolution or softening of the reflector 3 occurs, stains will occur due to reactions between the first silica plate 1 and the second silica plate 2 and the reflector 3, and a decrease in reflectivity will occur. The total content of Ir, Pt, Rh, Ru, Re, and Mo in the alloy is preferably 50% by mass or more, and more preferably 60% by mass or more.

[0032] (Thickness of Reflector) The reflector 3 is a thin film. The thickness of the reflector 3 is preferably 50 to 500 nm, more preferably 100 to 400 nm. If the thickness of the reflector 3 is less than 50 nm, heat is transmitted through the reflector 3 without being reflected, resulting in a decrease in heat reflectance, and if the thickness of the reflector 3 is greater than 500 nm, peeling may occur due to film stress. When the first reflector 3a and the second reflector 3b are provided, the total thickness is preferably 50 to 500 nm, more preferably 100 to 400 nm.

[0033] (Composition of the First Silica Plate and the Second Silica Plate) The first silica plate 1 and the second silica plate 2 may be crystalline silica plates or amorphous silica plates. They may also be synthetic quartz glass plates or fused quartz glass plates. Synthetic quartz glass plates are preferred. The first silica plate 1 and the second silica plate 2 preferably have a Li, Na, K, Ca, Mg, B, Fe, and Cu content of 1 ppm or less and an Al content of 10 ppm or less. Contamination inside a heat treatment furnace can be suppressed. If the Li, Na, K, Ca, Mg, B, Fe, and Cu content of the first silica plate 1 and the second silica plate 2 exceeds 1 ppm, or if the Al content of the first silica plate 1 and the second silica plate 2 exceeds 10 ppm, when a heat reflector is used in a semiconductor heat treatment furnace to heat-treat a Si substrate on which a circuit or the like is formed, the inside of the heat treatment furnace may be contaminated, potentially rendering the Si substrate on which a circuit or the like is formed unusable.

[0034] (Size and Thickness of the First and Second Silica Plates) The shape of the first and second silica plates 1 and 2, when viewed from the front of the reflector 3, is, for example, circular, elliptical, rectangular, or square, with circular being preferred. The diameter of the circle is, for example, 5 to 50 cm. The width of the annular shape of the joint 4 between the peripheral edges is, for example, 0.5 to 20 mm. The thickness of the first and second silica plates 1 and 2 is preferably 0.5 to 2.0 mm, more preferably 1.0 to 1.5 mm. This suppresses energy loss due to heat absorption by the silica heat reflector itself and improves thermal response during heating and cooling of the furnace body. The difference in thickness between the first and second silica plates 1 and 2 is preferably 0.1 mm or less, and more preferably they are the same thickness. If the thickness of the first and second silica plates 1 and 2 is thinner than 0.5 mm, there is a risk of damage or deformation due to a decrease in the strength of the heat reflector when using the heat reflector in a semiconductor heat treatment furnace to heat-treat a Si substrate on which a circuit or the like is formed. On the other hand, if the thickness of the first silica plate 1 and the second silica plate 2 exceeds 2.0 mm, when a heat reflector is used in a semiconductor heat treatment furnace to heat treat a Si substrate on which circuits or the like are formed, the heat reflector, particularly the silica plate, may absorb heat (thermal radiation, infrared rays), which may reduce the thermal efficiency within the semiconductor heat treatment furnace.

[0035] (Surface Roughness of the Outer Surface of the First Silica Plate and the Second Silica Plate) For at least one outer surface of the first silica plate 1 and the second silica plate 2, the surface roughness of at least a portion of the outer surface is preferably 5 μm or less in arithmetic mean roughness Ra. More preferably, it is 2 μm or less, even more preferably, 1 μm or less, and even more preferably, 0.5 μm or less. This allows for appropriate adjustments to enhance reflectivity and disperse reflected heat. The lower limit of the arithmetic mean roughness Ra is preferably, for example, 0.01 μm or more, and more preferably, 0.1 μm or more. Examples of surfaces with such surface roughness include blasted surfaces and etched surfaces. When the outer surface is a blasted surface, the arithmetic mean roughness Ra is preferably 2 μm or less, more preferably, 1 μm or less, and even more preferably, 0.5 μm or less. The blasting treatment can be wet blasting or dry blasting. The etching treatment can be wet etching or dry etching. The arithmetic mean roughness may be equal or different on the peripheral plane. For example, the arithmetic mean roughness Ra of the entire peripheral plane may be 5 μm or less, or the central portion of the peripheral plane may be smooth, and the arithmetic mean roughness Ra of the outer annular portion surrounding the central portion may be 5 μm or less. A "smooth surface" refers to a surface that has not undergone a roughening treatment such as blasting or etching during the manufacture of the silica heat reflector of this embodiment. Furthermore, the arithmetic mean roughness Ra of the central portion of the peripheral plane may be 2 μm or less, and the arithmetic mean roughness Ra of the outer annular portion surrounding the central portion may be 5 μm or less, or the entire peripheral plane may be smooth. Furthermore, the surface of the silica plate at the peripheral portion other than the portion where the metal film is formed may be rougher than the surface of the silica plate at the portion where the metal film is formed and surrounded by the peripheral portion. In this case, it is possible to suppress the transmission of heat incident on the peripheral portion. In this embodiment, the term "peripheral plane" is synonymous with "outer plane."

[0036] (OH Group Content of First Silica Plate and Second Silica Plate) The OH group content of each of the first silica plate 1 and the second silica plate 2 is 1000 ppm or less, preferably 900 ppm or less, and more preferably 800 ppm or less. Silica is a material with high infrared transmittance, but OH groups absorb infrared rays near 1400 nm, 2200 nm, and 2700 nm. Because the infrared transmittance of the silica plate decreases as the wavelength increases, wavelengths from 1500 nm to 2400 nm are particularly important. Furthermore, high reflectance can be achieved by suppressing absorption by OH groups near 2200 nm and improving reflectance. Furthermore, infrared absorption by OH groups near 2700 nm can be suppressed. If the OH group content of the first silica plate 1 and the second silica plate 2 exceeds 1000 ppm, deterioration due to reaction between the reflector 3 and the OH groups is accelerated, resulting in partial loss or deterioration of the metal film and resulting in stains. Furthermore, infrared rays passing through the silica plate are absorbed by OH groups, reducing the reflectivity of the silica heat reflector. The lower limits of the OH group content of the first silica plate 1 and the second silica plate 2 are preferably 1 ppm or more, and more preferably 20 ppm or more. If the OH group content is too low, the bonding strength between the silica plates may be reduced. The OH groups present in the silica plate are hardly unevenly distributed depending on the location.

[0037] The OH group content of the first silica plate 1 and the second silica plate 2 was determined as follows: First, the absorbance was measured using a Fourier transform infrared spectrophotometer (FT-IR), and then the absorbance value near 2720 nm was applied to the Beer-Lambert equation to calculate the absorbance, and the calculated value was divided by the density to determine the OH group concentration.

[0038] (Reflectance of Silica Heat Reflector) In the silica heat reflectors 100, 200, 300, and 400 according to this embodiment, it is preferable that the reflectance of the reflector 3 in the infrared region of 1500 to 2400 nm incident from the first silica plate side or the second silica plate side is 75% or more. In FIG. 2, the incident direction L1 from the first silica plate side and the incident direction L2 from the second silica plate side are shown as examples. The temperature of the semiconductor furnace body for which the heat reflector is provided is 1000°C or less, but there is an optimal wavelength for efficient heating. According to Planck's law, the radiation intensity emitted in all directions is expressed by the following equation (1): According to Equation 1, strong radiation can be seen in the infrared region, but as the temperature rises, the maximum wavelength of thermal radiation, where the radiation intensity is greatest, shifts to a smaller value. This suggests that when heating at a specified furnace body temperature, it is most efficient to reflect the thermal radiation containing the maximum wavelength toward the furnace interior. The maximum wavelength of thermal radiation is expressed by Wien's displacement law and can be calculated using Equation 2. Considering the behavior of the maximum wavelength of thermal radiation and the reflectivity of metal reflectors when the furnace body temperature is 950°C, it is preferable for silica heat reflectors to have high reflectivity in the infrared region of 1500 to 2400 nm. Specifically, this is as follows: silica plates absorb infrared radiation in the wavelength range of 3500 nm or longer, making it difficult to reflect it; the reflectivity of metal reflecting films increases as the wavelength increases; and the maximum wavelength of infrared radiation emitted from the furnace body depends on the furnace body temperature. Therefore, since the reflectivity of metal reflecting films is relatively lower at wavelengths shorter than the maximum wavelength than at wavelengths longer than the maximum wavelength, it is important for silica heat reflectors to efficiently reflect infrared radiation in the shorter wavelength region. For example, according to (Equation 2), when the furnace body temperature is 800°C, the maximum wavelength of thermal radiation is 2701 nm, and when the furnace body temperature is 1000°C, the maximum wavelength of thermal radiation is 2276 nm. Because the maximum wavelength of thermal radiation at a furnace body temperature of 950°C is just under 2400 nm, high reflectance is particularly required in the infrared region of 1500 to 2400 nm. If the reflectance of a silica heat reflector in the infrared region of 1500 to 2400 nm is less than 75%, when using the silica heat reflector in a semiconductor heat treatment furnace to heat treat a Si substrate with a circuit or the like formed thereon, the heat treatment efficiency may be reduced, requiring a higher heat treatment temperature. This increases the thermal damage suffered by the silica heat reflector. The reflectance is preferably an average reflectance of 75% or more, calculated from the integrated value of the reflectance in the infrared region of 1500 to 2400 nm. A more preferable reflectance is 75% or more across the entire infrared region of 1500 to 2400 nm.

[0039] (Oxide Layer) As shown in FIG. 4 , the silica heat reflector 300 has an oxide layer 5 between the first silica plate 1 and the reflector 3, the oxide layer 5 containing one oxide selected from the group consisting of silicon oxide, aluminum oxide, sapphire, lithium tantalate, lithium niobate, magnesium oxide, titanium oxide, yttrium oxide, strontium titanate, germanium oxide, zinc oxide, indium oxide, indium tin oxide, tin oxide, tungsten-doped tin oxide, and tantalum oxide, or two or more oxides selected from the group of oxides. The thickness of the oxide layer 5 is preferably 50 nm or less. More preferably, the thickness of the oxide layer 5 is 40 nm or less. The silica heat reflector may also have an oxide layer 5 between the second silica plate and the reflector (not shown). Also, as shown in FIG. 5 , the silica heat reflector 400 may have an oxide layer 5 a between the first silica plate 1 and the first reflector 3 a, and an oxide layer 5 b between the second silica plate 2 and the second reflector 3 b. The oxide layer 5 (5a, 5b) improves the adhesion between the reflector 3 (3a, 3b) and the silica plates 1, 2, and also suppresses heat absorption by the oxide layer 5 (5a, 5b), allowing for efficient heat reflection. The material for the oxide layer 5 (5a, 5b) is preferably a material that further improves the adhesion between the first silica plate 1 or the second silica plate 2 and the reflector 3, and that allows the reflector 3 to reflect heat without absorbing heat itself. Furthermore, if the thickness of the oxide layer 5 (5a, 5b) exceeds 50 nm, the oxide layer 5 (5a, 5b) may absorb heat (thermal radiation, infrared rays), potentially reducing the heat reflectance of the silica heat reflector. When the reflector 3 and oxide layer 5 are provided, incident infrared rays may be directed to the oxide layer 5 before the reflector 3, as shown in FIG. 4 , for example, as shown by L1.

[0040] (Manufacturing Method for Forming a Reflector on a First Silica Plate) A manufacturing method for a silica heat reflector 100 will be described with reference to FIG. 6 . The manufacturing method for the silica heat reflector 100 includes a first step of preparing a first silica plate 1 and a second silica plate 2, as shown in FIG. 6( a), a second step of forming a reflector 3 on the surface of the first silica plate 1, as shown in FIG. 6( b), a third step of joining the first silica plate 1 and the second silica plate 2 together, with the surfaces of the reflectors 3 formed on the first silica plate 1 facing each other, as shown in FIG. 6( c), and a fourth step of joining at least the peripheral portions of the facing surfaces of the first silica plate 1 and the second silica plate 2, as shown in FIG. 6( d). The peripheral portions are joined to form a joint 4. In FIG. 6( b), the reflector 3 is formed on the surface of the first silica plate 1, but the reflector 3 may also be formed on the surface of the second silica plate 2. Because the first silica plate 1 and the second silica plate 2 are not substantially distinguishable, the embodiment in which the reflector 3 is formed on the surface of the first silica plate 1 is illustrated here.

[0041] (Manufacturing Method in Which Reflectors are Formed on First and Second Silica Plates) A ​​manufacturing method of a silica heat reflector 200 will be described with reference to Fig. 7 . The manufacturing method of the silica heat reflector 200 includes a first step of preparing a first silica plate 1 and a second silica plate 2, as shown in Fig. 7(e) ; a second step of forming a reflector 3a on the surface of the first silica plate 1 and a reflector 3b on the surface of the second silica plate 2, as shown in Fig. 7(f) ; a third step of joining the first silica plate 1 and the second silica plate 2 together, with the surface of the reflector 3a formed on the first silica plate 1 and the surface of the reflector 3b formed on the second silica plate 2 as opposing surfaces, as shown in Fig. 7(g) ; and a fourth step of joining at least the peripheral portions of the opposing surfaces of the first silica plate 1 and the second silica plate 2, as shown in Fig. 7(h) . The peripheral portions are joined to form a joint 4.

[0042] In the manufacturing method of the silica heat reflectors 100, 200, it is preferable to carry out a fifth step after the fourth step, in which the outer peripheral surfaces of the first silica plate 1 and the second silica plate 2 are polished to adjust the final plate thickness. This allows for more accurate adjustment of the final plate thickness. The silica heat reflectors 100, 200 are adjusted to have a plate thickness of, for example, 1.0 to 4.0 mm. Furthermore, the plate thicknesses of the first silica plate 1 and the second silica plate 2 are each adjusted to be 0.5 to 2.0 mm.

[0043] In the manufacturing method of the silica heat reflector 100, 200, in the fourth step, it is preferable to create a vacuum atmosphere of 100 Pa or less, an argon atmosphere, or a nitrogen atmosphere, and then bond the materials at a pressure of 3500 kPa or less and a temperature of 400 to 1000°C. This prevents deterioration of the reflector due to oxygen or hydrogen, and heat, and maintains the heat reflectivity. Welding using an oxyhydrogen burner is also possible, but temperature control is difficult, and bonding requires high temperatures of 1000°C or higher, which can deteriorate the metal film and reduce the reflectivity. The argon or nitrogen atmosphere may be an argon atmosphere under reduced pressure lower than atmospheric pressure or a nitrogen atmosphere under reduced pressure, or atmospheric pressure. Furthermore, if the vacuum atmosphere exceeds 100 Pa, impurities remaining in the atmosphere will remain attached to the surfaces of the first silica plate 1, the second silica plate 2, and the reflector 3 during the subsequent bonding process. This could result in the impurities coming into contact with the surface of the reflector 3 during the manufacturing of the silica heat reflectors 100, 200, causing a reaction, resulting in deterioration of the reflector 3 and increased heat transmission. Furthermore, when the manufactured silica heat reflectors 100, 200 are used in a semiconductor heat treatment furnace or the like, the impurities could be dispersed inside the furnace or the like. When a vacuum atmosphere of 100 Pa or less is used, a vacuum atmosphere of 80 Pa or less is preferred. If the pressure at which the first silica plate 1 and the second silica plate 2 are pressed together exceeds 3500 kPa, excessive pressure may be applied, resulting in defects such as cracking of the first silica plate 1 and the second silica plate 2. It is more preferable that the pressure at which the first silica plate 1 and the second silica plate 2 are pressed together be 3000 kPa or less. The lower limit of this pressure is preferably 800 kPa, more preferably 1000 kPa, to ensure reliable bonding. Furthermore, if the temperature during bonding is lower than 400°C, the bonding strength between the first silica plate 1 and the second silica plate 2 will be insufficient, and there is a risk that the first silica plate 1 and the second silica plate 2 will peel off when the manufactured heat reflector 100, 200 is used in a semiconductor heat treatment furnace or the like. Furthermore, if the temperature during bonding is higher than 1000°C, there is a risk that the reflective surface of the reflector 3 will become cloudy, reducing the reflectance of the reflector 3.The temperature during bonding is preferably 500 to 900°C, and more preferably 600 to 850°C.

[0044] (Manufacturing Method for a Form Including an Oxide Layer) The manufacturing method for the silica heat reflector 300 will be described, highlighting the differences from the manufacturing method for the silica heat reflector 100. The manufacturing method for the heat reflector 300 further includes a step F (not shown) of forming an oxide layer on the surface of the first silica plate 1 after the first step of preparing the first silica plate 1 and the second silica plate 2 shown in FIG. 6(a). The oxide layer is preferably formed by sputtering, chemical vapor deposition, or vapor deposition. The manufacturing method further includes a step G (not shown) of forming a reflector on the oxide layer. The subsequent steps are the same as the third and fourth steps in the manufacturing method for the heat reflector 100.

[0045] The manufacturing method of the silica heat reflector 400 will be described below, highlighting the differences from the manufacturing method of the heat reflector 200. The manufacturing method of the silica heat reflector 400 includes a first step of preparing the first silica plate 1 and the second silica plate 2 shown in FIG. 7( e), followed by a step H (not shown) of forming an oxide layer on the surface of the first silica plate 1 and another oxide layer on the surface of the second silica plate 2. The oxide layer is preferably formed by sputtering, chemical vapor deposition, or vapor deposition. The manufacturing method further includes a step I (not shown) of forming a reflector on the oxide layer formed on the first silica plate 1 and another reflector on the oxide layer formed on the second silica plate 2. The subsequent steps are similar to the third and fourth steps in the manufacturing method of the heat reflector 200.

[0046] (Pressing Material) The manufacturing method for the silica heat reflectors 100, 200, 300, and 400 preferably further includes a step A between the third and fourth steps, as shown in FIG. 6(d) or 7(h), in which a pressing material 6 made of carbon, oxide, nitride, or boride, or a pressing material containing at least one selected from the group consisting of carbon, oxide, nitride, and boride, is placed at a location in contact with at least the outer peripheral surface of the first silica plate 1 and the second silica plate 2. This allows the first and second silica plates to be joined while suppressing contamination of the reflector by impurities. The pressing material 6 is, for example, a flat or curved plate. The shape and size of the pressing material 6 are preferably similar or congruent to those of the first and second silica plates, and if similar, may be increased by up to +10%. The thickness of the pressing material 6 is preferably 1 to 70 mm, more preferably 30 to 50 mm. When bonding, it is necessary for the components of the pressurizing machine to come into contact with the first silica plate 1 and the second silica plate 2. If a pressing material made of a material other than "a pressing material made of carbon, oxide, nitride or boride, or a pressing material containing at least one selected from the group consisting of carbon, oxide, nitride and boride" is used, there is a risk that it will react with the first silica plate and the second silica plate and be altered. Furthermore, there is a risk that the manufactured silica heat reflecting plates 100, 200, 300, 400 will have an adverse effect on the semiconductor substrate when used in a semiconductor heat treatment furnace or the like.

[0047] (Overlapping Pressing) As shown in FIG. 8, the manufacturing method of the silica heat reflector 100 according to this embodiment further includes, between the third and fourth steps, a step B (FIG. 8(c-1)) in which a plurality of stacks of the first silica plate and the second silica plate obtained in the third step are prepared, and 2 to 30 sets of the stacks are stacked in the stacking direction with spacers 7 sandwiched therebetween, and the spacers 7 are preferably made of carbon, oxide, nitride or boride, or contain at least one kind selected from the group consisting of carbon, oxide, nitride and boride, and the fourth step is preferably a step (FIG. 8(d-1)) in which the 2 to 30 sets of the stacked stacks are simultaneously joined. As shown in FIG. 9 , the method for manufacturing the silica heat reflector 200 according to this embodiment further includes a step B (FIG. 9( g-1 )) between the third and fourth steps, in which multiple stacks of the first and second silica plates obtained in the third step are prepared and 2 to 30 stacks of the stacks are stacked in the stacking direction with spacers 7 sandwiched therebetween. The spacers 7 are preferably made of carbon, oxide, nitride, or boride, or at least one selected from the group consisting of carbon, oxide, nitride, and boride. The fourth step is preferably a step (FIG. 9( h-1 )) in which 2 to 30 stacked stacks of the stacks are simultaneously bonded. Multiple pairs of first and second silica plates can be simultaneously bonded while suppressing bonding between different silica plates, such as a first silica plate and a different second silica plate, or another first silica plate and a second silica plate, using the spacers 7. If the number of stacked stacks exceeds 30, handling may be impaired. For the silica heat reflectors 300 and 400, step B is similarly performed, and multiple sets can be bonded simultaneously by simultaneously bonding the stacked bodies in step 4. The shape and size of the spacer 7 are preferably similar to or congruent with those of the first and second silica plates, and if similar, may be increased by up to +10%. The thickness of the spacer 7 is preferably 1 to 70 mm, and more preferably 30 to 50 mm.

[0048] In the manufacturing method of the silica heat reflectors 100, 200, 300, and 400 according to this embodiment, it is preferable to form the reflectors 3 (3a and 3b) by any of sputtering, chemical vapor deposition, and vapor deposition in the second step. This allows the thickness of the reflector to be uniform, thereby making the heat reflectance uniform. Furthermore, the density of the film can be improved, thereby improving the heat reflectance.

[0049] The manufacturing method for the silica heat reflector 100, 200, 300, and 400 according to this embodiment preferably further includes, between the first and second steps, a step C of reverse sputtering the surfaces where the first and second silica plates 1 and 2 will face each other in the third step. Cleaning the surfaces where the first and second silica plates face each other to remove impurities improves adhesion between the first silica plate and the reflector, the first silica plate and the oxide layer, the second silica plate and the reflector, and the second silica plate and the oxide layer, as well as improving the adhesiveness of the joint between the first and second silica plates at their peripheral edges. Removing impurities prevents impurities on the surfaces of the first and second silica plates 1 and 2 from coming into contact with and reacting with the surface of the reflector 3, which would otherwise cause deterioration of the reflector 3. Furthermore, the anchoring effect improves adhesion of the formed film.

[0050] In the manufacturing method of the silica heat reflector 100, 200, 300, 400 according to this embodiment, it is more preferable to include a step D after the second step, preferably after the second step and before the third step, in which heat treatment is performed at 1000°C or less. It is also more preferable to include a step E after the fourth step in which heat treatment is performed at 1000°C or less. The lower limit temperature for the heat treatment is, for example, 100°C or more, preferably 200°C or more. Both steps D and E may be included. Furthermore, in the fourth step, when heating is performed at 400 to 1000°C during bonding, bonding and heat treatment are performed simultaneously. The density of the reflector 3 can be improved, thereby improving the heat reflectance. Heat treatment improves the reflectance by about 4%. When the density of the reflective film during deposition is insufficient, sufficient reflectance cannot be obtained. However, by performing heat treatment, the reflective film becomes denser, thereby achieving the desired reflectance. If the heat treatment is performed at a temperature higher than 1000° C., there is a risk that the first silica plate 1, the second silica plate 2 and the reflector 3 (3a, 3b) may react with each other.

[0051] Example 1: The first silica plate 1 and the second silica plate 2 were silica plates (synthetic quartz plates) with a plate size of 300 mm in diameter and a thickness of 1.0 mm, containing 1 ppm or less of Li, Na, K, Ca, Mg, B, Fe, and Cu, 10 ppm or less of Al, and an OH group concentration of 1,000 ppm. Impurities were measured using an ICP mass analyzer, and the OH group concentration was quantified using a Fourier transform infrared spectrophotometer (manufactured by JASCO Corporation, PS-4000). After cleaning the surfaces of these silica plates, 100 nm-thick Mo films were formed on each of the first silica plate 1 and the second silica plate 2 by sputtering to serve as reflectors 3a and 3b. The plates were bonded together with the reflective film facing inward, and a carbon plate was placed as a pressing member in contact with the outer peripheral surfaces of the first silica plate 1 and the second silica plate 2, and then set in an atmospherically controlled pressurizer. The specimens were then evacuated and held for 1 hour under the following conditions: a vacuum atmosphere of 10 Pa, a temperature of 800°C, and a pressure of 1400 kPa, for bonding. After bonding, the reflectance was measured using a spectrophotometer (Shimadzu Corporation, UV-3100PC). The measurement results are shown in Figure 10. As a result, the average reflectance from 1500 to 2400 nm was 82.98%, with reflectances of 77.71% at 1500 nm, 77.60% at 2220 nm, and 86.94% at 2400 nm.

[0052] (Example 2) The silica heat reflector prepared in Example 1 was placed in a vacuum annealing furnace (manufactured by ULVAC Riko Co., Ltd.) and heated to a pressure of 1.0 × 10 ‐4 A heat treatment was performed in which the temperature was raised to 800°C in a vacuum atmosphere of 10 Pa and held at this temperature for 20 minutes, and the reflectance of the silica heat reflector after the heat treatment was measured with a spectrophotometer in the same manner as in Example 1. The measurement results are shown in Figure 11. As a result, the average reflectance from 1500 to 2400 nm was 87.97%, with reflectances of 82.22% at 1500 nm, 82.39% at 2220 nm, and 91.72% at 2400 nm, indicating an overall improvement in reflectance of about 4 to 5% compared to the reflectance of Example 1.

[0053] Comparative Example 1: The first silica plate 1 and the second silica plate 2 were silica plates (synthetic quartz plates) with a plate size of 300 mm in diameter and a thickness of 1.0 mm, containing 1 ppm or less of Li, Na, K, Ca, Mg, B, Fe, and Cu, 10 ppm or less of Al, and an OH group concentration of 1200 ppm. Impurities were measured using an ICP mass analyzer, and the OH group concentration was quantified using a Fourier transform infrared spectrophotometer. After cleaning the surfaces of these silica plates, 100 nm-thick Mo films were deposited on each of the first silica plate 1 and the second silica plate 2 by sputtering to serve as reflectors 3a and 3b. The plates were bonded together with the reflective film facing inward, and a carbon plate was placed in contact with the outer peripheral surfaces of the first silica plate 1 and the second silica plate 2 as a pressing member, and then set in an atmospheric pressure-controlled pressurizer. The specimen was then evacuated and held for 1 hour under the following conditions: vacuum atmosphere of 10 Pa, temperature of 800°C, and pressure of 1400 kPa, for bonding. After bonding, the reflectance was measured using a spectrophotometer. The measurement results are shown in Figure 12. As a result, the average reflectance from 1500 to 2400 nm was 72.20%, with reflectances of 65.46% at 1500 nm, 71.97% at 2220 nm, and 76.85% at 2400 nm.

[0054] (Example A) As the first silica plate 1, a silica plate (synthetic quartz plate) having a plate size of Φ300 mm and a thickness of 1.03 mm, an OH group concentration of 912.39 ppm, Li, Na, K, Ca, Mg, B, Fe, Cu of 1 ppm or less, and Al of 10 ppm or less was used. As the second silica plate 2, a silica plate (synthetic quartz plate) having a plate size of Φ300 mm and a thickness of 1.04 mm, an OH group concentration of 926.50 ppm, Li, Na, K, Ca, Mg, B, Fe, Cu of 1 ppm or less, and Al of 10 ppm or less was used. Otherwise, a silica heat reflector was prepared in the same manner as in Example 1.

[0055] (Example A-1) Heat Treatment Temperature: 850°C The same heat treatment as in Example 2 was carried out except that the silica heat reflector of Example A was held at 850°C for 1 hour, and the reflectance of the silica heat reflector after the heat treatment was measured with a spectrophotometer in the same manner as in Example 1. The measurement results are shown in Table A. As a result, the average reflectance from 1500 to 2400 nm was 86.41%, with reflectances of 80.46% at 1500 nm, 83.29% at 2220 nm, and 89.42% at 2400 nm.

[0056] (Example A-2) Heat Treatment Temperature: 900°C The silica heat reflector of Example A was subjected to heat treatment in the same manner as in Example A-1, except that the heat treatment temperature was 900°C, and the reflectance was measured. The measurement results are shown in Table A. As a result, the average reflectance from 1500 to 2400 nm was 86.58%, with reflectances of 80.64% at 1500 nm, 83.76% at 2220 nm, and 89.99% at 2400 nm.

[0057] (Example A-3) Heat Treatment Temperature: 950°C The silica heat reflector of Example A was subjected to heat treatment in the same manner as in Example A-1, except that the heat treatment temperature was 950°C, and the reflectance was measured. The measurement results are shown in Table A. As a result, the average reflectance from 1500 to 2400 nm was 82.26%, with reflectances of 74.73% at 1500 nm, 79.77% at 2220 nm, and 86.81% at 2400 nm.

[0058] (Example A-4) Heat Treatment Temperature 1000°C The silica heat reflector of Example A was subjected to heat treatment in the same manner as in Example A-1, except that the heat treatment temperature was 1000°C, and the reflectance was measured. The measurement results are shown in Table A. As a result, the average reflectance from 1500 to 2400 nm was 79.04%, with reflectances of 73.81% at 1500 nm, 78.12% at 2220 nm, and 84.50% at 2400 nm.

[0059] (Reference Example A) Heat Treatment Temperature 1050°C The silica heat reflector of Example A was subjected to heat treatment in the same manner as in Example A-1, except that the heat treatment temperature was 1050°C, and the reflectance was measured. The measurement results are shown in Table A. As a result, the average reflectance from 1500 to 2400 nm was 70.00%, with reflectances of 64.74% at 1500 nm, 67.49% at 2220 nm, and 75.57% at 2400 nm.

[0060]

[0061] In Examples A-1 and A-2, the reflectance at wavelengths of 1500 nm, 2200 nm, and 2400 nm is all 75% or more, and the average reflectance is also 75% or more, allowing for efficient heat reflection when used as a silica heat reflector. In Examples A-3 and A-4, the reflectance at wavelength of 1500 nm is less than 75%, but the average reflectance is 75% or more, allowing for efficient heat reflection when used as a silica heat reflector.

[0062] On the other hand, in Reference Example A, the reflectance at a wavelength of 2400 nm was barely above 75%, but the reflectance at each wavelength of 1500 nm and 2200 nm was less than 75%, and the average reflectance was also less than 75%. It is believed that the heat treatment of the silica thermal reflector at a temperature higher than 1000°C caused reactions between the first silica plate 1, the second silica plate 2, and the reflector 3 (3a, 3b). Therefore, it is preferable that no reactions occur between the first silica plate 1, the second silica plate 2, and the reflector 3 (3a, 3b).

[0063] (Example B) As the first silica plate 1, a silica plate (fused quartz plate) having a plate size of Φ324 mm and a thickness of 1.04 mm, an OH group concentration of 256.59 ppm, Li, Na, K, Ca, Mg, B, Fe, Cu of 1 ppm or less, and Al of 10 ppm or less was used. As the second silica plate 2, a silica plate (fused quartz plate) having a plate size of Φ324 mm and a thickness of 1.04 mm, an OH group concentration of 245.77 ppm, Li, Na, K, Ca, Mg, B, Fe, Cu of 1 ppm or less, and Al of 10 ppm or less was used. Otherwise, a silica heat reflector was produced in the same manner as in Example 1.

[0064] (Example B-1) Heat Treatment Temperature: 850°C The same heat treatment as in Example 2 was carried out except that the silica heat reflector of Example B was held at 850°C for 1 hour, and the reflectance of the silica heat reflector after the heat treatment was measured with a spectrophotometer in the same manner as in Example 1. The measurement results are shown in Table B. As a result, the average reflectance from 1500 to 2400 nm was 87.25%, with reflectances of 80.30% at 1500 nm, 89.27% ​​at 2220 nm, and 90.95% at 2400 nm.

[0065] (Example B-2) Heat Treatment Temperature: 900°C The silica heat reflector of Example B was subjected to heat treatment in the same manner as in Example B-1, except that the heat treatment temperature was 900°C, and the reflectance was measured. The measurement results are shown in Table B. As a result, the average reflectance from 1500 to 2400 nm was 86.97%, with reflectances of 76.98% at 1500 nm, 85.81% at 2220 nm, and 87.26% at 2400 nm.

[0066] (Example B-3) Heat Treatment Temperature: 950°C The silica heat reflector of Example B was subjected to heat treatment in the same manner as in Example B-1, except that the heat treatment temperature was 950°C, and the reflectance was measured. The measurement results are shown in Table B. As a result, the average reflectance from 1500 to 2400 nm was 88.78%, with reflectances of 82.14% at 1500 nm, 89.51% at 2220 nm, and 92.11% at 2400 nm.

[0067] (Example B-4) Heat Treatment Temperature 1000°C The silica heat reflector of Example B was subjected to heat treatment in the same manner as in Example B-1, except that the heat treatment temperature was 1000°C, and the reflectance was measured. The measurement results are shown in Table B. As a result, the average reflectance from 1500 to 2400 nm was 87.28%, with reflectances of 80.81% at 1500 nm, 88.98% at 2220 nm, and 89.59% at 2400 nm.

[0068]

[0069] In Examples B-1 to B-4, the reflectance at each wavelength of 1500 nm, 2200 nm, and 2400 nm is all 75% or more, and the average reflectance is also 75% or more, so that when used as a silica heat reflector, heat can be reflected efficiently.

[0070] (Example C) As the first silica plate 1, a silica plate (synthetic quartz plate) having a plate size of Φ300 mm and a thickness of 1.22 mm, an OH group concentration of 71.60 ppm, Li, Na, K, Ca, Mg, B, Fe, Cu of 1 ppm or less, and Al of 10 ppm or less was used. As the second silica plate 2, a silica plate (synthetic quartz plate) having a plate size of Φ300 mm and a thickness of 1.23 mm, an OH group concentration of 71.60 ppm, Li, Na, K, Ca, Mg, B, Fe, Cu of 1 ppm or less, and Al of 10 ppm or less was used. Otherwise, a silica heat reflector was produced in the same manner as in Example 1.

[0071] (Example C-1) Heat Treatment Temperature: 850°C The same heat treatment as in Example 2 was carried out except that the silica heat reflector of Example C was held at 850°C for 1 hour, and the reflectance of the silica heat reflector after the heat treatment was measured with a spectrophotometer in the same manner as in Example 1. The measurement results are shown in Table C. As a result, the average reflectance in the 1500 to 2400 nm range was 88.83%, with reflectances of 82.01% at 1500 nm, 91.15% at 2220 nm, and 91.42% at 2400 nm.

[0072] (Example C-2) Heat Treatment Temperature: 900°C The silica heat reflector of Example C was subjected to heat treatment in the same manner as in Example C-1, except that the heat treatment temperature was 900°C, and the reflectance was measured. The measurement results are shown in Table C. As a result, the average reflectance from 1500 to 2400 nm was 88.94%, with reflectances of 81.95% at 1500 nm, 91.25% at 2220 nm, and 92.66% at 2400 nm.

[0073] (Example C-3) Heat Treatment Temperature: 950°C The silica heat reflector of Example C was subjected to heat treatment in the same manner as in Example C-1, except that the heat treatment temperature was 950°C, and the reflectance was measured. The measurement results are shown in Table C. As a result, the average reflectance from 1500 to 2400 nm was 88.55%, with reflectances of 81.36% at 1500 nm, 91.11% at 2220 nm, and 92.03% at 2400 nm.

[0074] (Example C-4) Heat Treatment Temperature 1000°C The silica heat reflector of Example C was subjected to heat treatment in the same manner as in Example C-1, except that the heat treatment temperature was 1000°C, and the reflectance was measured. The measurement results are shown in Table C. As a result, the average reflectance from 1500 to 2400 nm was 88.13%, with reflectances of 81.42% at 1500 nm, 90.44% at 2220 nm, and 91.80% at 2400 nm.

[0075] (Reference Example C) Heat Treatment Temperature 1050°C The silica heat reflector of Example C was subjected to heat treatment in the same manner as in Example C-1, except that the heat treatment temperature was 1050°C, and the reflectance was measured. The measurement results are shown in Table C. As a result, the average reflectance from 1500 to 2400 nm was 73.01%, with reflectances of 65.70% at 1500 nm, 75.56% at 2220 nm, and 77.09% at 2400 nm.

[0076]

[0077] In Examples C-1 to C-4, the reflectance at each wavelength of 1500 nm, 2200 nm, and 2400 nm is all 75% or more, and the average reflectance is also 75% or more, so that when used as a silica heat reflector, heat can be reflected efficiently.

[0078] On the other hand, in Reference Example C, the reflectance at wavelengths of 2200 nm and 2400 nm was barely above 75%, but the reflectance at a wavelength of 1500 nm was less than 75%, and the average reflectance was also less than 75%. It is believed that the heat treatment of the silica thermal reflector at a temperature higher than 1000°C caused reactions between the first silica plate 1, the second silica plate 2, and the reflector 3 (3a, 3b). Therefore, it is preferable that no reactions occur between the first silica plate 1, the second silica plate 2, and the reflector 3 (3a, 3b).

[0079] Examples A-1 to A-4, Reference Example A, Examples B-1 to B-4, Examples C-1 to C-4, and Reference Example C are compared. It was confirmed that the reflectance was higher when the OH group concentration was lower.

[0080] (Example D-1) 100 nm Rh film As the first silica plate 1, a silica plate (synthetic quartz plate) having a plate size of 20 mm x 40 mm and a thickness of 1.02 mm, an OH group concentration of 888.48 ppm, Li, Na, K, Ca, Mg, B, Fe, Cu of 1 ppm or less, and Al of 10 ppm or less was used. As the second silica plate 2, a silica plate (synthetic quartz plate) having a plate size of 20 mm x 40 mm and a thickness of 1.03 mm, an OH group concentration of 956.99 ppm, Li, Na, K, Ca, Mg, B, Fe, Cu of 1 ppm or less, and Al of 10 ppm or less was used. A silica heat reflector was fabricated in the same manner as in Example 1, except that Rh films were formed as reflectors 3a and 3b to a thickness of 100 nm, and the conditions for the atmospheric control pressurizer were a vacuum of 10 Pa or less, a temperature of 900°C, and a pressure of 2000 kPa for 3 hours. After fabrication, the reflectance of the silica heat reflector was measured in the same manner as in Example 1. The measurement results are shown in Table D. As a result, the average reflectance from 1500 to 2400 nm was 87.91%, with reflectances of 84.14% at 1500 nm, 85.78% at 2220 nm, and 90.99% at 2400 nm.

[0081] (Example D-2) 10 nm TiO 2 In the silica heat reflector of Example D-1, a TiO layer / 50 nm Ir layer was laminated to a thickness of 10 nm on each of the first silica plate 1 and the second silica plate 2. 2After the layer was deposited, TiO 2 A silica heat reflector was prepared in the same manner as in Example D-1, except that an Ir layer was formed as a laminated film on the layer to a thickness of 50 nm as reflectors 3a and 3b by sputtering, and the reflectance was measured. The measurement results are shown in Table D. As a result, the average reflectance from 1500 to 2400 nm was 87.45%, with reflectances of 81.23% at 1500 nm, 87.60% at 2220 nm, and 92.26% at 2400 nm.

[0082] (Example D-3) 10 nm TiO 2 In the silica heat reflector of Example D-1, a TiO layer / 50 nm Ru layer was formed on each of the first silica plate 1 and the second silica plate 2 to a thickness of 10 nm. 2 After the layer was deposited, TiO 2 A silica heat reflector was fabricated in the same manner as in Example D-1, except that a Ru layer was formed on the layer as reflectors 3a and 3b by sputtering to a thickness of 50 nm, and the reflectance was measured. The measurement results are shown in Table D. As a result, the average reflectance from 1500 to 2400 nm was 84.13%, with reflectances of 74.40% at 1500 nm, 85.10% at 2220 nm, and 89.47% at 2400 nm.

[0083]

[0084] In Examples D-1 and D-2, the reflectance at each wavelength of 1500 nm, 2200 nm, and 2400 nm is all 75% or more, and the average reflectance is also 75% or more, so that when used as a silica heat reflector, heat can be reflected efficiently.

[0085] In Example D-3, although the reflectance at each wavelength at 1500 nm is less than 75%, the average reflectance is 75% or more, so heat can be reflected without any problems when used as a silica heat reflector.

[0086] Example E: Effect of arithmetic mean roughness Ra A silica plate (synthetic quartz plate) having a plate size of 20 mm x 40 mm and a thickness of 1.03 mm, an OH group concentration of 941.06 ppm, Li, Na, K, Ca, Mg, B, Fe, Cu, or less, and Al, or less than 10 ppm, was used as the first silica plate 1. A silica plate (synthetic quartz plate) having a plate size of 20 mm x 40 mm and a thickness of 1.03 mm, an OH group concentration of 981.08 ppm, Li, Na, K, Ca, Mg, B, Fe, Cu, or less, and Al, or less than 10 ppm, was used as the second silica plate 2. Silica heat reflectors were fabricated in the same manner as in Example 1, except that Mo films were formed to a thickness of 50 nm for each of the reflectors 3a and 3b, and the conditions for the atmospheric control pressurizer were a vacuum of 10 Pa or less, a temperature of 850°C, and a pressure of 3000 kPa for 3 hours. After fabrication, the arithmetic mean roughness Ra of the silica heat reflector was measured using a surface roughness measuring instrument (manufactured by Mitutoyo Corporation, model number 178-560-11). The reflectance of the silica heat reflector was also measured from the first silica plate side using a spectrophotometer (manufactured by Shimadzu Corporation, UV-3100PC). The silica heat reflector was then subjected to a blasting treatment, and the arithmetic mean roughness Ra and reflectance of the silica heat reflector whose surface had been roughened by the blasting treatment were repeatedly measured. A graph of the arithmetic mean roughness Ra and reflectance was then created. The graph is shown in FIG. 13. As can be seen from the graph in Figure 13, the average reflectance exceeded 75% when the arithmetic mean roughness Ra was 2 µm or less. Furthermore, when the OH group concentration was measured before and after blasting, no change in concentration was observed. Therefore, the reflectance at the location where the reflector is present improved as the arithmetic mean roughness Ra decreased. The reflectance exceeded 75% when the arithmetic mean roughness Ra of the surface of the silica plate was 2 µm or less. By setting the arithmetic mean roughness Ra of the surface of the silica plate at locations where there is no reflector to 5 µm or less, it is possible to suppress the transmission of infrared rays even at locations where there is no reflector.

[0087] (Example F-1) The thickness of each Mo film was 25 nm. As the first silica plate 1, a silica plate (synthetic quartz plate) with a plate size of 20 mm x 40 mm and a thickness of 1.04 mm, an OH group concentration of 962.35 ppm, Li, Na, K, Ca, Mg, B, Fe, Cu of 1 ppm or less, and Al of 10 ppm or less was used. As the second silica plate 2, a silica plate (synthetic quartz plate) with a plate size of 20 mm x 40 mm and a thickness of 1.02 mm, an OH group concentration of 904.67 ppm, Li, Na, K, Ca, Mg, B, Fe, Cu of 1 ppm or less, and Al of 10 ppm or less was used. A silica heat reflector was fabricated in the same manner as in Example 1, except that Mo films were formed as reflectors 3a and 3b to a thickness of 25 nm, and the conditions for the atmospheric control pressurizer were a vacuum of 10 Pa or less, a temperature of 850°C, and a pressure of 3000 kPa for 3 hours. After fabrication, the reflectance of the silica heat reflector was measured in the same manner as in Example 1. The measurement results are shown in Table F. As a result, the average reflectance from 1500 to 2400 nm was 84.41%, with reflectances of 77.16% at 1500 nm, 81.57% at 2220 nm, and 88.78% at 2400 nm.

[0088] (Example F-2) Mo film thickness: 35 nm A silica heat reflector was prepared in the same manner as in Example F-1, except that Mo films were formed on the reflectors 3a and 3b to a thickness of 35 nm, and the reflectance was measured. The measurement results are shown in Table F. As a result, the average reflectance from 1500 to 2400 nm was 86.26%, with reflectances of 79.98% at 1500 nm, 82.89% at 2220 nm, and 90.45% at 2400 nm.

[0089] (Example F-3) Mo film thickness: 40 nm A silica heat reflector was prepared in the same manner as in Example F-1, except that Mo films were formed on the reflectors 3a and 3b to a thickness of 40 nm, and the reflectance was measured. The measurement results are shown in Table F. As a result, the average reflectance from 1500 to 2400 nm was 87.02%, with reflectances of 81.02% at 1500 nm, 83.45% at 2220 nm, and 90.60% at 2400 nm.

[0090] (Example F-4) Mo film thickness: 45 nm A silica heat reflector was prepared in the same manner as in Example F-1, except that Mo films were formed on the reflectors 3a and 3b to a thickness of 45 nm, and the reflectance was measured. The measurement results are shown in Table F. As a result, the average reflectance from 1500 to 2400 nm was 87.65%, with reflectances of 81.67% at 1500 nm, 84.03% at 2220 nm, and 91.64% at 2400 nm.

[0091] (Example F-5) Mo film thickness: 50 nm A silica heat reflector was prepared in the same manner as in Example F-1, except that Mo films were formed on the reflectors 3a and 3b to a thickness of 50 nm, and the reflectance was measured. The measurement results are shown in Table F. As a result, the average reflectance from 1500 to 2400 nm was 88.09%, with reflectances of 82.32% at 1500 nm, 84.58% at 2220 nm, and 92.09% at 2400 nm.

[0092] (Example F-6) Mo film thickness of 60 nm A silica heat reflector was prepared in the same manner as in Example F-1, except that Mo films were formed on the reflectors 3a and 3b to a thickness of 60 nm, and the reflectance was measured. The measurement results are shown in Table F. As a result, the average reflectance from 1500 to 2400 nm was 88.55%, with reflectances of 82.14% at 1500 nm, 87.96% at 2220 nm, and 92.42% at 2400 nm.

[0093]

[0094] In Examples F-1 to F-6, the reflectance at each wavelength of 1500 nm, 2200 nm, and 2400 nm is all 75% or more, and the average reflectance is also 75% or more, so that when used as a silica heat reflector, heat can be reflected efficiently.

[0095] REFERENCE SIGNS LIST 1 First silica plate 2 Second silica plate 3 Reflector 3a First reflector 3b Second reflector 4 Joint 5, 5a, 5b Oxide layer 6 Pressing member 7 Spacer L1 Incident direction from the first silica plate side L2 Incident direction from the second silica plate side

Claims

1. A silica heat reflecting plate comprising: a first silica plate; a second silica plate whose surface faces the first silica plate; a reflector provided on at least one of the surface of the second silica plate facing the first silica plate and the surface of the first silica plate facing the second silica plate; and a joint portion in which at least the peripheral portion of the joint surface between the first silica plate and the second silica plate is continuously joined in an annular shape along the peripheral portion, and has a structure of a joint between the first silica plate and the second silica plate, and the reflector reflects infrared rays incident from the first silica plate side or the second silica plate side, wherein the first silica plate and the second silica plate have an OH group content of 1000 ppm or less, and the reflector is a thin film, A silica heat reflector, characterized in that a surface layer including at least the reflective surface of the reflector is made of one type selected from the group consisting of Ir, Pt, Rh, Ru, Re, and Mo, or is made of an alloy containing at least one type selected from the group consisting of Ir, Pt, Rh, Ru, Re, and Mo and having a melting point of 1200°C or higher.

2. A silica heat reflector as described in claim 1, characterized in that the first silica plate and the second silica plate have a content of each of the elements Li, Na, K, Ca, Mg, B, Fe, and Cu of 1 ppm or less, and an Al content of 10 ppm or less.

3. A silica heat reflector as described in claim 1, characterized in that, in at least one of the outer peripheral planes of the first silica plate and the second silica plate, the surface roughness of at least a portion of the outer peripheral plane is an arithmetic mean roughness Ra of 5 μm or less.

4. A silica heat reflector as described in claim 1, characterized in that the reflectance of the reflector in the infrared region of 1500 to 2400 nm incident from the first silica plate side or the second silica plate side is 75% or more.

5. A silica heat reflector according to claim 1, characterized in that the thickness of said first silica plate and said second silica plate is 0.5 to 2.0 mm.

6. The silica heat reflector according to claim 1, characterized in that the thickness of the reflector is 50 to 500 nm.

7. The silica heat reflector according to claim 1, characterized in that it has an oxide layer containing one type selected from the group of oxides consisting of silicon oxide, aluminum oxide, sapphire, lithium tantalate, lithium niobate, magnesium oxide, titanium oxide, yttrium oxide, strontium titanate, germanium oxide, zinc oxide, indium oxide, indium tin oxide, tin oxide, tungsten-doped tin oxide, and tantalum oxide, or an oxide layer containing two or more types selected from the group of oxides, at least one of between the first silica plate and the reflector and between the second silica plate and the reflector, and the thickness of the oxide layer is 50 nm or less.

8. A method for manufacturing a silica heat reflector according to claim 1, comprising: a first step of preparing a first silica plate and a second silica plate; a second step of forming a reflector on at least one of the surfaces of the first silica plate and the second silica plate; a third step of joining the first silica plate and the second silica plate with the surface of the reflector formed on at least one of the first silica plate and the second silica plate as opposing surfaces; and a fourth step of joining at least the peripheral portions of the opposing surfaces of the first silica plate and the second silica plate.

9. A method for manufacturing a silica heat reflector as described in claim 8, characterized in that after the fourth step, a fifth step is carried out in which the outer peripheral planes of the first silica plate and the second silica plate are polished to adjust the final plate thickness.

10. A method for manufacturing a silica heat reflector as described in claim 8, characterized in that in the fourth step, after creating a vacuum atmosphere of 100 Pa or less, an argon atmosphere, or a nitrogen atmosphere, the first silica plate and the second silica plate are bonded at a temperature of 400 to 1000°C under a pressure of 3500 kPa or less.

11. A method for manufacturing a silica heat reflector as described in claim 8, further comprising, between the third step and the fourth step, a step A of placing a pressing material made of carbon, oxide, nitride or boride, or a pressing material containing at least one selected from the group consisting of carbon, oxide, nitride and boride, at locations in contact with at least the outer circumferential planes of the first silica plate and the second silica plate.

12. A method for producing a silica heat reflector as described in claim 8, further comprising a step B between the third step and the fourth step, of preparing a plurality of stacks of the first silica plate and the second silica plate obtained in the third step, and stacking 2 to 30 pairs of the stacks in the stacking direction with spacers in between, wherein the spacers are made of carbon, oxide, nitride or boride, or contain at least one type selected from the group consisting of carbon, oxide, nitride and boride, and the fourth step is a step of simultaneously bonding the stacks of 2 to 30 pairs.

13. The method for producing a silica heat reflector according to claim 8, wherein in the second step, the reflector is formed by any one of a sputtering method, a chemical vapor deposition method, and a deposition method.

14. A method for manufacturing a silica heat reflector as described in claim 8, further comprising a step C between the first and second steps, of reverse sputtering the surfaces that are to face each other in the third step between the first and second silica plates.

15. A method for producing a silica heat reflector as described in claim 8, further comprising at least one step selected from the group consisting of step D, in which heat treatment is performed at 1000°C or less after the second step, and step E, in which heat treatment is performed at 1000°C or less after the fourth step.

Citation Information

Patent Citations

  • Heating method

    JP2001044130A

  • Quartz member for semiconductor manufacturing equipment, method for manufacturing quartz member for semiconductor manufacturing equipment, heat treatment device, method for analyzing metal in quartz member

    JP2003522708A

  • Silica thermal reflection plate

    JP2022104503A

  • Silica heat reflection plate

    JP2022105255A