Preparation method for and use of biomass material

By preparing biochar at high temperatures and using copper and iron catalysts, the metal smelting industry's demand for charcoal substitutes has been solved, efficient utilization of biomass charcoal and environmentally friendly reducing agent applications have been achieved, and sulfur has been reduced. Content and ash improve smelting efficiency.

WO2024259841A1PCT designated stage expired Publication Date: 2024-12-26ANHUI UNIV OF SCI & TECH +1

Patent Information

Application Number
PCT/CN2023/127449
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-21
Filing Date
2023-10-30
Publication Date
2024-12-26

AI Technical Summary

Technical Problem

The charcoal production used in the existing metal smelting industry has led to the reduction of forest resources and environmental damage. Its substitutes such as petroleum coke and anthracite have problems such as low volatility and poor chemical activity at high temperatures, which cannot effectively replace charcoal, resulting in the development of the metallurgical industry. limit.

Method used

Biochar is used as a reducing agent to prepare biomass carbon by thermally chemical reaction of waste biological materials at high temperatures, and low-temperature carbonization is used to use copper and iron catalysts to reduce sulfur content and ash content and improve activity.

Benefits of technology

It realizes efficient utilization of biomass carbon, reduces sulfur content and ash content, improves reduction efficiency, provides a clean and environmentally friendly renewable resource, reduces dependence on forest resources, and promotes the comprehensive utilization of industry and agriculture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023127449_26122024_PF_FP_ABST
    Figure CN2023127449_26122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of biomass reducing agents. Disclosed are a preparation method for and the use of a biomass material. The present invention comprises the following steps: 1) preparation of a preliminary carbide; 2) addition of a copper-iron catalyst; 3) low-temperature carbonization; and 4) high-temperature carbonization. The biomass material of the present invention reduces the sulfur content and the ash content and has a high activity and reduction efficiency on the premise of being green and environmentally friendly and a relatively low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Preparation method and application of biomass material Technical Field

[0001] The present invention relates to the technical field of biomass reducing agents, and more particularly to a preparation method and application of a biomass material. Background Art

[0002] The primary reducing agents used in my country's metallurgical industry are charcoal, wood blocks, petroleum coke, and low-ash bituminous coal. Charcoal, due to its maximum porosity and numerous straight pores, is suitable for gas circulation. Its graphitization and crystallization levels do not increase significantly at high temperatures, and it exhibits high specific resistivity and reactivity under reducing conditions. Charcoal is, by far, the best reducing agent in industrial metallurgy. For a long time, charcoal has been the primary reducing agent used in my country's industrial metal production. Petroleum coke and bituminous coal can only be added in small quantities, primarily due to its high degree of graphitization at high temperatures, resulting in low reducing activity. Although anthracite has a high fixed carbon content and low ash content, it suffers from low volatility, poor chemical activity, easy expansion, and thermal separation at high temperatures, making it unsuitable for direct use as a reducing agent in industrial metal production.

[0003] Charcoal production requires a vast amount of forest resources, leading to a decline in these resources and severe damage to the ecological environment. Forest cover in my country accounts for less than 10% of the country's land area, and forest formation requires a long growth cycle. Large-scale deforestation is inconsistent with the requirements of protecting the ecological environment, creating a low-carbon society, and developing a circular economy. The development of the metal smelting industry cannot come at the expense of relatively scarce forest resources. Due to resource constraints, charcoal prices have risen sharply, severely impacting the economic profitability of metal smelting companies. The development of the metal smelting industry is limited by the availability of reducing agents. Biomass is a typical renewable energy source, offering advantages such as a wide range of sources, abundant reserves, and a short growth cycle. The total amount of biomass produced annually on Earth is approximately 140-180 billion tons, and China wastes over 6 billion tons of straw annually, presenting enormous potential for resource utilization.

[0004] The treatment of waste biomaterials has always been a thorny issue because direct incineration produces large amounts of greenhouse gases and contributes to global climate change. Biochar is a carbon-rich substance produced by thermochemical reactions of organic solids at high temperatures (300-1000°C) and in the absence of oxygen. Due to its unique properties, biochar plays an important role in carbon sequestration, improving soil properties, purifying polluted wastewater, adsorbing greenhouse gases, and assisting in biogas production. In this project, we focus on using biochar as a reducing agent to replace the charcoal, coal, and coke widely used in the metallurgical industry, thereby helping the metallurgical industry achieve its carbon reduction goals.

[0005] Developing a biochar-based reducing agent for industrial metallurgy that is widely available, environmentally friendly, and cost-effective, replacing charcoal in industrial metal production, is crucial for reducing production costs, ensuring stable furnace operation, and minimizing damage to forest resources. Therefore, providing a clean, green, and environmentally friendly biomass material preparation method and application is a pressing need for those skilled in the art.

[0006] Summary of the Invention

[0007] In view of this, the present invention provides a preparation method and application of a biomass material.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] A method for preparing a biomass material comprises the following steps:

[0010] 1) crushing the waste biomaterial into particles of 2 to 3 cm, placing it in a carbonization device, heating it to 300 to 400° C. at a rate of 40 to 50° C. / min under atmospheric conditions and maintaining it for 10 to 20 minutes, then washing and drying it to obtain a preliminary carbonized product;

[0011] 2) adding a copper-iron catalyst to the prepared carbide at a mass ratio of 80 to 100:1 and mixing uniformly to obtain a mixed material;

[0012] 3) Under inert gas conditions, water vapor is introduced to carbonize the mixture obtained in step 2) at a low temperature of 500-800° C. for 2-4 hours; after naturally cooling to room temperature, the mixture is separated from the copper-iron catalyst to obtain biochar;

[0013] 4) Under inert gas conditions, ammonia is introduced to carbonize the biomass charcoal obtained in step 3) at a high temperature of 1100-1300° C. for 4-6 hours. After the carbonization is completed, the biomass charcoal is naturally cooled to room temperature, washed, and dried to obtain a biomass material.

[0014] Furthermore, the waste biomaterial in step 1) is one or a mixture of any proportion of dried and dehydrated peanut shells, sunflower seed shells, chestnut shells, pistachio shells, walnut shells, macadamia shells, pine nut shells, coconut shells, rice husks, corn cobs, sugarcane bagasse, and crop straw.

[0015] Furthermore, in step 2), the copper-iron catalyst is chalcopyrite and iron ore, and the mass ratio of chalcopyrite: iron ore is 1:3-5.

[0016] Furthermore, during the low-temperature carbonization process in step 3), the heating rate is 5 to 10°C / min;

[0017] In step 3), the water vapor is introduced at a rate of 1.5 to 2 mL / min per 100 g of the total mass of the biochar.

[0018] Furthermore, the cleaning in step 1) and step 4) is performed by rinsing with clean water for 10 to 15 minutes.

[0019] Furthermore, in the high-temperature carbonization process of step 4), the heating rate is 20-25°C / min;

[0020] In step 4), the ammonia gas is introduced at a rate of 2 to 4 mL / min per 100 g of the total mass of the biochar.

[0021] The invention discloses an application of biomass materials in a metal smelting reduction process.

[0022] It can be seen from the above technical solution that compared with the prior art, the beneficial effects of the present invention are:

[0023] Biomass is a clean, low-carbon fuel with low sulfur and nitrogen contents, and very little ash. Therefore, the emissions of SO2, NOx and dust after combustion are much smaller than those of fossil fuels. It is a clean fuel and a renewable resource that can be recycled. It can be regarded as an inexhaustible and permanent energy source. Its utilization process does not increase the CO2 content in the atmosphere, which is of special significance for alleviating the increasingly serious "greenhouse effect".

[0024] The use of biomass reducing agents in the metal smelting industry and the electrolytic smelting ironmaking industry will fundamentally solve the problem of comprehensive utilization of agricultural and forestry wastes that has existed for many years. Moreover, the production process of biomass reducing agents enables the efficient utilization of biomass resources, which is conducive to promoting the integration of industrial and agricultural, urban and rural industrial chains, stimulating domestic demand, and increasing farmers' income.

[0025] Although the raw materials undergo pretreatment to remove impurities before carbonization, they still contain a small amount of sulfur. Therefore, the present invention introduces ammonia gas to desulfurize them. At high temperatures, ammonia gas generates highly reducing hydrogen within the device, which reacts with the carbon-sulfur bonds in the carbon material, thereby removing the sulfur.

[0026] The biomass material of the present invention reduces the sulfur content and ash content under the premise of being green, environmentally friendly and low in cost, and has high activity and high reduction efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are merely embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying any creative work.

[0028] Figure 1 is a flow chart of the present invention. DETAILED DESCRIPTION

[0029] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of the present invention.

[0030] Example 1

[0031] A method for preparing a biomass material comprises the following steps:

[0032] 1) crushing the dried and dehydrated peanut shells to a particle size of 2-3 cm, placing them in a carbonization device, heating them to 350°C at a rate of 45°C / min under atmospheric conditions and maintaining the temperature for 15 minutes, then rinsing them with water for 12 minutes and drying them to obtain a preliminary carbide;

[0033] 2) adding a copper-iron catalyst (mass ratio of chalcopyrite: iron ore = 1:4) to the prepared carbide in a mass ratio of 90:1 and mixing uniformly to obtain a mixed material;

[0034] 3) Under inert gas (helium) conditions, 1.8 mL / min of water vapor was introduced per 100 g of the total mass of the biochar, and the mixture obtained in step 2) was carbonized at a low temperature of 700° C., a heating rate of 8° C. / min, and a carbonization time of 3 h; after naturally cooling to room temperature, the mixture was separated from the copper-iron catalyst to obtain biochar;

[0035] 4) Under inert gas (helium) conditions, 3 mL / min of ammonia was introduced for every 100 g of the total mass of the biochar, and the biochar obtained in step 3) was carbonized at a high temperature of 1200°C, a heating rate of 23°C / min, and a carbonization time of 5 h. The biochar was naturally cooled, rinsed with water for 12 min, and dried to obtain a biomass material.

[0036] Example 2

[0037] A method for preparing a biomass material comprises the following steps:

[0038] 1) crushing the dried and dehydrated walnut shells and pine nut shells to a particle size of 2 to 3 cm, placing them in a carbonization device, heating them to 300°C at a rate of 40°C / min under atmospheric conditions and maintaining the temperature for 20 minutes, then rinsing them with water for 15 minutes and drying them to obtain a preliminary carbonized product;

[0039] 2) adding a copper-iron catalyst (mass ratio of chalcopyrite: iron ore = 1:5) to the prepared carbide at a mass ratio of 80:1 and mixing uniformly to obtain a mixed material;

[0040] 3) Under inert gas (helium) conditions, 1.5 mL / min of water vapor was introduced per 100 g of the total mass of the biochar, and the mixture obtained in step 2) was carbonized at a low temperature of 500° C., a heating rate of 5° C. / min, and a carbonization time of 4 h; after naturally cooling to room temperature, the mixture was separated from the copper-iron catalyst to obtain biochar;

[0041] 4) Under inert gas (helium) conditions, 2 mL / min of ammonia was introduced for every 100 g of the total mass of the biochar, and the biochar obtained in step 3) was carbonized at a high temperature of 1100 ° C., a heating rate of 20 ° C / min, and a carbonization time of 6 h. The biochar was naturally cooled, rinsed with water for 15 min, and dried to obtain a biomass material.

[0042] Example 3

[0043] A method for preparing a biomass material comprises the following steps:

[0044] 1) crushing the dried and dehydrated corn cobs and wheat straw to a particle size of 2 to 3 cm, placing them in a carbonization device, heating them to 400°C at a rate of 50°C / min under atmospheric conditions and maintaining the temperature for 10 minutes, then rinsing them with water for 10 minutes and drying them to obtain a preliminary carbonized product;

[0045] 2) adding a copper-iron catalyst (mass ratio of chalcopyrite: iron ore = 1:3) to the prepared carbide in a mass ratio of 100:1 and mixing uniformly to obtain a mixed material;

[0046] 3) Under inert gas (helium) conditions, 2 mL / min of water vapor was introduced per 100 g of the total mass of the biochar, and the mixture obtained in step 2) was carbonized at a temperature of 800° C., a heating rate of 10° C. / min, and a carbonization time of 2 h; after naturally cooling to room temperature, the mixture was separated from the copper-iron catalyst to obtain biochar;

[0047] 4) Under inert gas (helium) conditions, 4 mL / min of ammonia was introduced for every 100 g of the total mass of the biochar, and the biochar obtained in step 3) was carbonized at a high temperature of 1300 ° C., a heating rate of 25 ° C / min, and a carbonization time of 4 h. The biochar was naturally cooled, rinsed with water for 10 min, and dried to obtain a biomass material.

[0048] Comparative Example 1

[0049] A method for preparing a biomass material comprises the following steps:

[0050] 1) crushing the dried and dehydrated peanut shells to a particle size of 2-3 cm, placing them in a carbonization device, heating them to 350°C at a rate of 45°C / min under atmospheric conditions and maintaining the temperature for 15 minutes, then rinsing them with water for 12 minutes and drying them to obtain a preliminary carbonized product;

[0051] 2) Under inert gas (helium) conditions, 1.8 mL / min of water vapor was introduced per 100 g of the total mass of the biochar to carbonize the prepared carbide obtained in step 1) at a low temperature of 700° C., a heating rate of 8° C. / min, and a carbonization time of 3 h; after naturally cooling to room temperature, biochar was obtained;

[0052] 3) Under inert gas (helium) conditions, 3 mL / min of ammonia was introduced for every 100 g of the total mass of the biochar, and the biochar obtained in step 3) was carbonized at a high temperature of 1200°C, a heating rate of 23°C / min, and a carbonization time of 5 h. The biochar was naturally cooled, rinsed with water for 12 min, and dried to obtain a biomass material.

[0053] Comparative Example 2

[0054] A method for preparing a biomass material comprises the following steps:

[0055] 1) crushing the dried and dehydrated peanut shells to a particle size of 2-3 cm, placing them in a carbonization device, heating them to 350°C at a rate of 45°C / min under atmospheric conditions and maintaining the temperature for 15 minutes, then rinsing them with water for 12 minutes and drying them to obtain a preliminary carbonized product;

[0056] 2) adding an iron catalyst (iron ore) to the prepared carbide at a mass ratio of 90:1 and mixing uniformly to obtain a mixed material;

[0057] 3) Under inert gas (helium) conditions, 1.8 mL / min of water vapor was introduced per 100 g of the total mass of the biochar, and the mixture obtained in step 2) was carbonized at a low temperature of 700° C., a heating rate of 8° C. / min, and a carbonization time of 3 h; after naturally cooling to room temperature, the mixture was separated from the copper-iron catalyst to obtain biochar;

[0058] 4) Under inert gas (helium) conditions, 3 mL / min of ammonia was introduced for every 100 g of the total mass of the biochar, and the biochar obtained in step 3) was carbonized at a high temperature of 1200°C, a heating rate of 23°C / min, and a carbonization time of 5 h. The biochar was naturally cooled, rinsed with water for 12 min, and dried to obtain a biomass material.

[0059] Comparative Example 3

[0060] A method for preparing a biomass material comprises the following steps:

[0061] 1) crushing the dried and dehydrated peanut shells to a particle size of 2-3 cm, placing them in a carbonization device, heating them to 350°C at a rate of 45°C / min under atmospheric conditions and maintaining the temperature for 15 minutes, then rinsing them with water for 12 minutes and drying them to obtain a preliminary carbonized product;

[0062] 2) adding a copper catalyst (chalcopyrite) to the prepared carbide at a mass ratio of 90:1 and mixing uniformly to obtain a mixed material;

[0063] 3) Under inert gas (helium) conditions, 1.8 mL / min of water vapor was introduced per 100 g of the total mass of the biochar, and the mixture obtained in step 2) was carbonized at a low temperature of 700° C., a heating rate of 8° C. / min, and a carbonization time of 3 h; after naturally cooling to room temperature, the mixture was separated from the copper-iron catalyst to obtain biochar;

[0064] 4) Under inert gas (helium) conditions, 3 mL / min of ammonia was introduced for every 100 g of the total mass of the biochar, and the biochar obtained in step 3) was carbonized at a high temperature of 1200°C, a heating rate of 23°C / min, and a carbonization time of 5 h. The biochar was naturally cooled, rinsed with water for 12 min, and dried to obtain a biomass material.

[0065] Comparative Example 4

[0066] A method for preparing a biomass material comprises the following steps:

[0067] 1) crushing the dried and dehydrated peanut shells to a particle size of 2-3 cm, placing them in a carbonization device, heating them to 350°C at a rate of 45°C / min under atmospheric conditions and maintaining the temperature for 15 minutes, then rinsing them with water for 12 minutes and drying them to obtain a preliminary carbonized product;

[0068] 2) adding a copper-iron catalyst (mass ratio of chalcopyrite: iron ore = 1:4) to the prepared carbide in a mass ratio of 90:1 and mixing uniformly to obtain a mixed material;

[0069] 3) Under inert gas (helium) conditions, the mixture obtained in step 2) is carbonized at a low temperature of 700° C., a heating rate of 8° C. / min, and a carbonization time of 3 hours; after naturally cooling to room temperature, it is separated from the copper-iron catalyst to obtain biochar;

[0070] 4) Under inert gas (helium) conditions, 3 mL / min of ammonia was introduced for every 100 g of the total mass of the biochar, and the biochar obtained in step 3) was carbonized at a high temperature of 1200°C, a heating rate of 23°C / min, and a carbonization time of 5 h. The biochar was naturally cooled, rinsed with water for 12 min, and dried to obtain a biomass material.

[0071] Comparative Example 5

[0072] A method for preparing a biomass material comprises the following steps:

[0073] 1) crushing the dried and dehydrated peanut shells to a particle size of 2-3 cm, placing them in a carbonization device, heating them to 350°C at a rate of 45°C / min under atmospheric conditions and maintaining the temperature for 15 minutes, then rinsing them with water for 12 minutes and drying them to obtain a preliminary carbide;

[0074] 2) adding a copper-iron catalyst (mass ratio of chalcopyrite: iron ore = 1:4) to the prepared carbide in a mass ratio of 90:1 and mixing uniformly to obtain a mixed material;

[0075] 3) Under inert gas (helium) conditions, 1.8 mL / min of water vapor was introduced per 100 g of the total mass of the biochar, and the mixture obtained in step 2) was carbonized at a low temperature of 700° C., a heating rate of 8° C. / min, and a carbonization time of 3 h; after naturally cooling to room temperature, the mixture was separated from the copper-iron catalyst to obtain biochar;

[0076] 4) Under inert gas (helium) conditions, the biomass char obtained in step 3) was carbonized at a high temperature of 1200° C., a heating rate of 23° C. / min, a carbonization time of 5 h, and naturally cooled. The biomass char was rinsed with water for 12 min and dried to obtain a biomass material.

[0077] The biomass carbon specific surface area, sulfur content, and ash content of the biomass materials prepared in Examples 1-3 and Comparative Examples 1-5 were measured. The results are shown in Table 1:

[0078] Table 1: Biomass material performance levels

[0079] The results show that compared with Example 1, Comparative Example 1 does not add a copper-iron catalyst, the specific surface area of ​​the biochar is reduced, and the ash content is increased, indicating that the ability of the activator water vapor to promote the volatilization of organic molecules in the pores of the prepared carbide in the low-temperature carbonization step is reduced. Similarly, Comparative Document 2 uses iron ore as a catalyst, and Comparative Document 3 uses chalcopyrite as a catalyst. The catalytic efficiency of iron ore is not as good as that of chalcopyrite, and the catalytic efficiency of chalcopyrite is even higher than that of the copper-iron catalyst of the present application. However, chalcopyrite itself contains a large amount of sulfur, which will increase the sulfur content in the final product. After orthogonal experiments by the inventors, it was found that the ratio of chalcopyrite to iron ore is between 1:3-5, and the catalytic efficiency and sulfur content reach the optimal range.

[0080] Comparative Example 4 does not introduce activator water vapor during the low-temperature carbonization step. This prevents the organic molecules in the prepared carbonized product from volatilizing, resulting in a decrease in the specific surface area of ​​the biochar and a significant increase in ash content. The increased sulfur content in Comparative Example 4 is due to the removal of some ash impurities during the final rinsing step of step 4). The decreased specific surface area of ​​the biochar in Comparative Example 4 leads to a corresponding decrease in cleaning efficiency.

[0081] Comparative Document 5 does not introduce ammonia in the high-temperature carbonization step, so the biochar cannot be desulfurized, and its sulfur content is significantly higher than that of other embodiments and comparative examples.

[0082] The above description of the disclosed embodiments is intended to enable one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be readily apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention is not limited to the embodiments shown herein but is intended to conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a biomass material, characterized in that: The following steps are involved: 1) crushing the waste biomaterial into a particle size of 2 to 3 cm, placing it in a carbonization device, heating it to 300 to 400° C. at a rate of 40 to 50° C. / min under atmospheric conditions and maintaining it for 10 to 20 minutes, washing it after completion, and drying it to obtain a preliminary carbonized product; 2) adding a copper-iron catalyst to the prepared carbide at a mass ratio of 80 to 100:1, and mixing them uniformly to obtain a mixed material; 3) Under inert gas conditions, water vapor is introduced to carbonize the mixture obtained in step 2) at a low temperature of 500-800° C. for 2-4 hours; after naturally cooling to room temperature, the mixture is separated from the copper-iron catalyst to obtain biomass charcoal; 4) Under inert gas conditions, ammonia is introduced to carbonize the biomass charcoal obtained in step 3) at a high temperature of 1100-1300° C. for 4-6 hours, and then naturally cooled to room temperature, washed, and dried to obtain a biomass material.

2. The method for preparing a biomass material according to claim 1, characterized in that: Step 1) The waste biomaterial is one or a mixture of any proportion of dried and dehydrated peanut shells, sunflower seed shells, chestnut shells, pistachio shells, walnut shells, macadamia shells, pine nut shells, coconut shells, rice husks, corn cobs, bagasse, and crop straw.

3. The method for preparing a biomass material according to claim 1, characterized in that: Step 2) The copper-iron catalyst is chalcopyrite and iron ore, and the mass ratio of chalcopyrite to iron ore is 1:3-5.

4. The method for preparing a biomass material according to claim 1, characterized in that: During the low-temperature carbonization process of step 3), the heating rate is 5 to 10°C / min; In step 3), the amount of water vapor introduced is 1.5 to 2 mL / min for every 100 g of the total mass of the biochar.

5. The method for preparing a biomass material according to claim 1, characterized in that: The cleaning in step 1) and step 4) is performed by rinsing with clean water for 10 to 15 minutes.

6. The method for preparing a biomass material according to claim 1, characterized in that: Step 4) During the high temperature carbonization process, the heating rate is 20-25°C / min; In step 4), the amount of ammonia introduced is 2 to 4 mL / min for every 100 g of the total mass of the biochar.

7. Use of the biomass material according to claim 1 in a metal smelting reduction process.

Citation Information

Patent Citations

  • Method for preparing high-content nitrogen-doped porous carbon materia

    CN103922306A

  • Method for increasing specific resistance of biomass charcoal reduction agent for industrial silicon smelting

    CN105253888A

  • Compound reducing agent for fire refining of copper

    CN105567995A

  • Compound reducing agent containing biomass charcoal for copper smelting

    CN105755294A

  • Method for preparing nitrogen-containing activated carbon by ammonia activation

    CN108064215A

Cited By

  • Biochar with functions of carbon immobilization, carbon capture and in-situ conversion as well as preparation method and application of biochar

    CN119954156A