AI Technical Summary
Existing electroplating processes for achieving black, powdery deposits, such as black gold powder, result in waste due to uncovering processes and require gold-based galvanic baths, which are costly and limit the creation of bicolor effects without using varnishes or interrupting the galvanic process.
An electroplated alloy composed of In, Te, and Ru, optionally with additional metals like Pt, Cu, Bi, Zr, Sn, Co, Ni, Ge, Ga, Se, Zn, Fe, or Pd, is used, with specific CIELAB color coordinates and a powdery consistency, allowing for a vintage aesthetic effect and transformation into a shiny white deposit without varnishes or process interruptions.
The alloy provides a cost-effective, removable, and versatile deposit suitable for vintage and bicolor effects, maintaining adhesion through mechanical and chemical treatments, and withstands cataphoretic painting, overcoming adhesion issues typically seen with indium.
Abstract
Description
[0001] INDUSTRIAL INVENTION PATENT APPLICATION TITLED:
[0002] BLACK COLORED, POWDERY, ELECTROPLATED TERNARY OR QUATERNARY ALLOY
[0003] FIELD OF THE INVENTION
[0004] The present invention refers to the field of electroplated alloys and related electroplating solutions and processes.
[0005] STATE OF THE ART
[0006] Metal alloys obtained by electroplating are widely used in various manufacturing fields, both for their physical features and their distinctive aesthetic appearance. To this latter aim, colored alloys, obtained through electroplating of both individual metals and alloys, are of interest; such alloys find practical applications in a variety of fields: furniture, clothing, jewelry, and generally in all sectors requiring objects with specific aesthetic characteristics. Among the deposits useful to characterize the aesthetics of the object to be electroplated, especially in the high fashion sector, dark-colored deposits have recently been successful, particularly powdery deposits that, after an uncovering process using an abrasive material, give the galvanized object a vintage effect. Well-adhered and cohesive dark-colored deposits are usually obtained from galvanic baths based on ruthenium (CN110965088A) or other precious metals such as gold (W02020025448A1 , JPS63250487A), and palladium (IT102017000084504), and rhodium.
[0007] A black colored powdery deposit (also known as black gold powder) consisting of a ternary or quaternary, gold-based alloy can currently be obtained from commercially available galvanic solutions (for example, Smoke by Valmet, Blackor™ by ITALFIMET, Antiqua by Legor, and Blackclad by the same Applicant). A powdery deposit, such as one of these, is then removed from the surface of the galvanized object using an abrasive material. The only areas where uncovering does not occur are cavities of the object, such as, but not limited to, the recess of an engraved inscription or the space between two links of a chain. Therefore, the black colored, powdery deposit is mostly removed from the item, resulting in a waste of gold. After this uncovering process, a layer of varnish can be applied either by cataphoresis orspraying, and therefore the properties of the deposit are such that it can also withstand this post-treatment.
[0008] After the uncovering process, the galvanized object can also undergo chemical and / or electrochemical treatments suitable to alter the appearance of the black deposit. Specifically, but not limited to this, it is possible to transform the dark colored deposit into a silvery one. This process is particularly interesting from an innovative perspective because to achieve the bicolor effect, usually white and gold, the objects undergo a first galvanization process, for example they are gilded. The galvanization process is interrupted, and the objects are then treated with special peelable varnishes. At this point, for example, the objects are rhodium-plated. The galvanization process is interrupted again and the peelable varnish is removed. To date, this type of deposit can only be achieved through galvanic baths for electroplating of gold-based ternary or quaternary alloys, i.e., galvanic baths in which the absence of gold results in a completely different and unusable product. The aim of the present invention is to provide a powdery galvanic deposit with chemical, physical, and aesthetic characteristics similar to those of black gold powder, but gold-free. A further aim of the present invention is to provide a galvanic process for achieving a bicolor effect without using varnishes and without interruptions of the galvanic process.
[0009] SUMMARY OF THE INVENTION
[0010] The present invention solves the aforementioned problems by means of an electroplated alloy consisting of In, Te, Ru, and optionally another metal selected from the group consisting of Pt, Cu, Bi, Zr, Sn, Co, Ni, Ge, Ga, Se, Zn, Fe, and Pd, and having CIELAB color coordinates within the range 2<L<40; -10<a*<+10; -20<b*<+20, and a powdery consistency (hereinafter also referred to as powder). Surprisingly, the galvanic deposit of the present invention resulted to be particularly suitable and cost-effective for imparting, through plating and uncovering, a vintage aesthetic effect to objects, particularly in the finishing of fashion accessories. The deposit subject matter of the invention has physical properties of cohesion and adhesion suitable for a post-treatment of mechanical uncovering, and a possible post-treatment of chemical or electrochemical uncovering and / or cataphoretic or spray painting. Advantageously, the deposit of the invention is completely or partiallyremovable using specific chemical and electrochemical solutions, with the aim of making the deposit versatile inside the galvanic industry production cycle. Surprisingly, the electroplated alloy can be modified with a specific electrochemical treatment, known as ruthenium stripping or degreasing, to alter its aesthetic appearance and transform it into an indium deposit with its typical blue-white color, ideal for achieving yellow gold and white bicolor effects, but without the use of peelable varnishes and without interrupting the galvanic process. Since indium deposits are notoriously prone to adhesion problems, which are particularly evident in sweat tests - conditions similar to those required for cataphoretic painting - it is surprising and advantageous that the powder subject matter of the invention, once subjected to uncovering and / or degreasing, withstands final cataphoretic painting. Subject matter of the present invention is also an aqueous solution for electroplating the above-described alloy, said solution having a pH of 0.5-7 and comprising a ruthenium (Ru) salt, a tellurium (Te) salt, an indium (In) salt, a conductive salt, and optionally a salt of another metal, selected from the group consisting of Pt, Cu, Bi, Zr, Sn, Co, Ni, Ge, Ga, Se, Zn, Fe, and Pd.
[0011] Subject matter of the invention is also a method for electroplating of an alloy as described above using the aforementioned solution.
[0012] Subject matter of the invention is also a method for obtaining a finished object with a vintage aesthetic effect, said method comprising electroplating of an alloy as described above and subsequent at least partial removal by mechanical removal. Subject matter of the invention is also a method for obtaining a finished object with a bicolor aesthetic effect, said method comprising the electrodeposition of a powder as described above, subsequent partial mechanical removal and subsequent transformation of the residual powder into a shiny white deposit having CIELAB color coordinates within the range 70<L<100; -10<a*<+10; -10<b*<+10 by means of an electrochemical treatment of ruthenium stripping or degreasing.
[0013] DETAILED DESCRIPTION OF THE INVENTION
[0014] Preferably, the alloy subject matter of the present invention has a composition of In 25-55% w / w
[0015] Te 15-50% w / w
[0016] Ru 5-12% w / w0-40% w / w of another metal selected from the group consisting of Pt, Cu, Bi, Zr, Sn, Co, Ni, Ge, Ga, Se, Zn, Fe, and Pd.
[0017] According to a preferred embodiment, the alloy subject matter of the invention is a ternary In-Te-Ru alloy; according to other embodiments of the present invention, the alloy subject matter of the invention is a quaternary In-Te-Ru-Cu, or In-Te-Ru-Pt, or In-Te-Ru-Bi alloy.
[0018] Preferably, the deposit subject matter of the invention consists of
[0019] In 45-55% w / w; more preferably 50-54% w / w
[0020] Te 35-45% w / w; more preferably 36-40 or 37-42% w / w
[0021] Ru 7-11 % w / w; more preferably 8-12% w / w
[0022] having CIELAB color coordinates within the range 2<L<40; -10; -2<a*<+10; -20<b*<+20; more preferably 5<L<20; -2<a*<+2; -2<b*<+2
[0023] According to a preferred embodiment of the invention, the electroplated alloy has a composition of 10% Ru, 52% In and 38% Te, or 9% Ru, 48% In and 42% Te, with a powdery consistency (hereinafter also referred to as powder). The color of the powder according to this preferred embodiment is L=13, a=0.8, b=0.9.
[0024] For the purposes of the present invention, an electroplating solution is a galvanic bath (hereinafter also referred to as bath for brevity), and the solvent used is water. The ruthenium salt in the solution is preferably selected from the group consisting of ruthenium chloride, ruthenium nitrate, ruthenium sulfamate, ruthenium oxalate, ruthenium phosphate, ruthenium sulfate, ruthenium oxide, ruthenium nitrite, or a combination thereof. Preferably, the concentration of ruthenium metal is 0.05-1 g / L, more preferably 0.1 -0.5 g / L. The solution preferably comprises ruthenium chloride with a concentration of ruthenium as a metal of 0.15-0.25 g / L.
[0025] The indium salt in the solution is preferably selected from the group consisting of indium sulfate, indium carbonate, indium phosphate, indium nitrate, indium chloride, and indium citrate. The concentration of indium as a metal is preferably of 0.05-1 g / L. The solution preferably comprises indium sulfate with a concentration of Indium as a metal of 0.40-0.50 g / L.
[0026] The tellurium salt in the solution is preferably selected from the group consisting of telluric acid, tellurous acid, tellurium oxide, and orthotelluric acid. Preferably, the concentration of tellurium as a metal is of 0.05-1 g / L. The solution preferablycomprises tellurium oxide with a concentration of tellurium as a metal of 0.15-0.25 g / L.
[0027] The metal salts of ruthenium, indium, and tellurium are selected based on their stability depending on the selected buffer system.
[0028] The concentration of the abovementioned metals in the solution is each time determined so as to achieve both the desired color coordinate triplet and the characteristic adhesion and cohesion properties that make the deposit partially removable by mechanical uncovering, and convertible into an indium deposit by a possible subsequent electrochemical treatment.
[0029] The conductive salt is preferably selected from the following sodium, potassium, and ammonium salts: chloride, bromide, iodide, sulfamate, sulfate, phosphate, carbonate, thiocyanate, tetrafluoroborate, phosphite, and sulfite, and is present in solution at a concentration range between 1 and 300 g / L, preferably between 50 and 200 g / L. The conductive salt is preferably ammonium sulfate, preferably at a concentration of 100-150 g / L.
[0030] The solution may also contain one or more complexing agents that, in addition to modulating the behavior of the alloyed metals, ensure their stability in solution. The complexing agent is preferably an organic compound selected from the group consisting of citric acid, malic acid, oxalic acid, maleic acid, gluconic acid, malonic acid, acetic acid, NTA, EDTA, NTP, HEDP, glycolic acid, and derived thiocompounds.
[0031] In order to modify the chemical and physical properties of the deposit, making its functioning more versatile in a galvanic production process, at least one organic or inorganic substance can also be introduced into the solution. Said organic substance is preferably selected from the group consisting of thiourea, urea, folic acid, sodium dodecyl sulfate, pyridine, nicotinic acid, nicotinamide, and amino acids, at concentrations of 0.001-10 g / L, preferably between 0.01 and 5 g / L. Said inorganic substance is preferably selected from the group consisting of oxalic acid and salts thereof, alkali metal and alkaline earth metal halides, alkali metal and alkaline earth metal chalcogenides, and alkali metal and alkaline earth metal oxides, at concentrations of 0.001-10 g / L, preferably between 0.01 and 5 g / L.The presence of additional metals in solution serves to adjust the colorimetric coordinate triplet, regulate the alloy deposition conditions, modulate the deposit hardness, and module the deposit cohesion and adhesion properties. Another metal selected from the group consisting of Pt, Cu, Bi, Zr, Sn, Co, Ni, Ge, Ga, Se, Zn, Fe, and Pd may also be present in the solution as a soluble salt. Said other metal is present as a soluble salt at concentrations comprised between 0.01 and 0.3 g of metal per liter of solution.
[0032] Platinum salts can impart a bluish color to the deposit, and Pt salts useful to this aim are preferably selected from the group consisting of chloroplatinic acid, potassium hexachloroplatinate, chloroplatinous acid, potassium tetrachloroplatinate, platinum diaminodinitrite, platinum tetranitrite, platinum tetraaminodinitrite, platinum dinitrosulfate, platinum dichloride, and platinum tetrachloride. Copper salts can impart an even blacker color to the deposit, similar to the black powders currently known; copper salts useful to this aim are preferably selected from the group consisting of copper sulfate, copper pyrophosphate, copper iodide, copper bromide, copper chloride, copper fluoride, copper hydroxide, copper oxide, copper methanesulfonate, copper acetate, copper gluconate, and copper citrate. Bismuth salts can impart a blueish color to the deposit, and Bi salts useful to this aim are preferably selected from the group consisting of bismuth sulfate, bismuth citrate, bismuth ammonium citrate, bismuth nitrate, bismuth gallate, bismuth oxide, and bismuth chloride. Nickel salts useful to this aim are preferably selected from the group consisting of nickel sulfate, nickel sulfamate, nickel chloride, nickel hydroxide, nickel carbonate, and hexamminenickel chloride. Zinc salts useful to this aim are preferably selected from the group consisting of zinc sulfate, zinc oxide, zinc acetate, zinc methanesulfonate, zinc chloride, and zinc hydroxide. Iron salts useful to this aim are for example, but not limited to, iron sulfate, iron citrate, iron formate, iron nitrate, iron oxide, and iron hydroxide. Zirconium salts useful to this aim are preferably selected from the group consisting of zirconyl nitrate, zirconium oxide, and zirconium sulfate. Tin salts useful to this aim are preferably selected from the group consisting of tin sulfate, tin methanesulfonate, sodium stannate, potassium stannate, tin oxide, tin chloride, and tin hydroxide. Cobalt salts useful to this aim are preferably selected from the group consisting of cobalt sulfate, cobalt sulfamate,cobalt chloride, cobalt carbonate, and cobalamins. Germanium salts useful to this aim are preferably selected from the group consisting of germanium oxide and sodium germanate. Gallium salts useful to this aim are preferably selected from the group consisting of gallium hydroxide, gallium nitrate, and gallium oxide. Selenium salts useful to this aim are preferably selected from the group consisting of selenium oxide, selenic acid, and selenious acid. Palladium salts useful to this aim are preferably selected from the group consisting of palladium sulfate, palladium tetraamine sulfate, palladium tetraamine dichloride, palladium chloride, and palladium diamine dinitrite.
[0033] It is important to point out that, unlike current black gold formulations, the addition of gold ions into the formulation subject matter of the present invention has a negative effect, making the deposit harder and therefore more difficult to be removed by mechanical abrasion.
[0034] Working conditions such as, but not limited to, current intensity, temperature, stirring, and pH, as well as the chemical composition of the galvanic bath in terms of conductive salts, buffer systems, complexing agents, and relative amounts of metal ions, influence the colorimetric coordinate triplet and the adhesion and cohesion chemical-physical properties of the deposit.
[0035] In particular, the concentration of the conductive salt influences the morphology of the deposit, favoring the formation of dark-colored powder.
[0036] Tellurium ions are responsible for the formation of a soft, poorly cohesive, powdery deposit. Their presence catalyzes the deposition of other metal ions and hinders the growth of dense layers. The higher its concentration, the greater the formation of dark-colored powder on the cathode surface during electroplating.
[0037] The working pH determines the stability of the bath, as insoluble Te species tend to form at pH values above 6. The selected working pH falls in the range between 0.5 and 7, preferably between 1 and 4. This operating range allows to work with a clear solution, without precipitate formation, in which the chemical species, remaining dissolved, maintain their action aimed at obtaining a powdery deposit. The solution preferably contains a suitable buffer system; the pH of the solution is preferably adjusted to 2-3 by addition of an acid, preferably sulfuric acid.The working temperature and the current density are sensitive parameters that influence the deposition rate.
[0038] In order to maintain the performances of the bath subject matter of the present invention comparable to that of the current systems for deposition of a powdery black gold-based deposit, which, as a metal, is known to be highly efficient, the electroplating method according to the present invention operates at a temperature of 20-80°C, preferably 40-70°C. The operating current is preferably 0.5-5 A / dm2, more preferably 1-3 A / dm2. The voltage is preferably 0.5-10 V, more preferably 2-5 V for static applications. For barrel applications, the voltage is preferably 0.5-10 V, more preferably 3-7 V.
[0039] The duration of the current application should be sufficient to homogeneously deposit the black powder over the entire cathode surface and should not be excessive to avoid high thicknesses that lead to premature loss of part of the deposit. Since this is a bath comparable to a color bath, deposition times are short, usually no more than two minutes.
[0040] The bath stirring is a parameter that influences the deposition of the alloy, and its homogeneity on the chemical-physical properties of the alloy.
[0041] The method according to the present invention to obtain a finished object with a bicolor effect preferably comprises treating the object with a vintage effect in a solution containing a basic solution of cyanide ions, preferably 15 g / L of KCN and 30 g / L of KOH, at room temperature, in a cathode current with a voltage of 3-7 V, preferably 6 V, for the time necessary to obtain complete dissolution of the powder. The present invention can be better understood in light of the following embodiments.
[0042] BRIEF DESCRIPTION OF THE FIGURES
[0043] Figure 1 - shows: A) a brass zipper pull, that was submitted to plating with the following galvanic cycle:
[0044] a. Acid copper plating for 10 minutes, approximately 8 pm thick
[0045] b. Acid nickel plating for 15 minutes, approximately 10 pm thick;
[0046] c. Deposition of a nickel-phosphorus alloy for 10 minutes, approximately 1 pm thick;d. Deposition of a palladium-nickel alloy for 5 minutes, approximately 1.0 pm thick.
[0047] e. Deposition of 24 kt gold for 5 minutes, approximately 0.5 pm thick.
[0048] B) The brass zipper pull shown in Fig. 1 A after deposition of the alloy of the present invention
[0049] C) The brass zipper pull of Fig. 1B after 40 minutes of uncovering in a combination of corn sawdust, wax, and abrasive powder, which removes the dark layer from the most exposed areas
[0050] D) The same zipper pull as in Fig. 1 C, after being submitted to cathodic current treatment to remove the dark, powdery part of the deposit. In this way, the so-called bicolor aesthetic effect is observed.
[0051] EXPERIMENTAL PART
[0052] The CIELAB colorimetric coordinates according to the present invention were measured with a D65 illuminant in reflection mode with specular component included (SCI) and an observation angle of 10°, specifically, they were performed with a Konica Minolta CM-17d colorimeter.
[0053] All measurements were acquired with the same parameters, unless otherwise indicated.
[0054] EXAMPLE 1
[0055] The following were dissolved in 1 L of demineralized water:
[0056] • 120 g of ammonium sulfate
[0057] • 0.45 g of In as sulfate
[0058] • 0.20 g of Ru as Ru chloride
[0059] • 0.20 g of Te as Tellurium oxide
[0060] The pH of the solution was adjusted with sulfuric acid to a value between 2.3 and 2.8. A 5 cm x 3.5 cm brass sheet, previously plated with a nickel layer and subsequently with gold, was treated with the above solution at a temperature of 60 °C, with a deposition time of 90 seconds at a current of 2.0 A / dm2A powdery, loosely cohesive deposit was formed with colorimetric coordinates (L=13, a*=0.8, b*=0.9). The overall composition of the deposit, analyzed by EDS, was:In 52.1% w / w
[0061] Te 37.6% w / w
[0062] Ru 10.3% w / w
[0063] The composition of the powdery component of the deposit only, mechanically removed with conductive adhesive tape, is:
[0064] In 48.4% w / w
[0065] Te 42.7% w / w
[0066] Ru 8.9% w / w
[0067] EXAMPLE 1.a
[0068] Using the bath from Example 1 , and under the same electroplating conditions, a brass zipper pull, which had previously undergone the following galvanic cycle, was coated:
[0069] a) Acid copper plating for 10 minutes, approximately 8 pm thick
[0070] b) Acid nickel plating for 15 minutes, approximately 10 pm thick;
[0071] c) Deposition of a nickel-phosphorus alloy for 10 minutes, approximately 1 pm thick;
[0072] d) Deposition of a palladium-nickel alloy for 5 minutes, approximately 1.0 pm thick.
[0073] The object is then uncovered using a combination of corn sawdust, wax, and abrasive powder, which in 40 minutes is able to remove the dark, powdery layer from the outermost areas, while the deposit remains intact and black in the hidden areas.
[0074] A representative sample of the galvanized items that passed the quality test was subjected to oxidation tests in accordance with international standards adopted by the major fashion houses for quality control of finished products. The results are summarized in the following table.
[0075] Test performed Result Rating No. of items tested Artificial sweat (UNI EN ISO 31600 / 2:2015) 5 / 5 positive 5 Synthetic sweat (NF S 80-772:2010) 5 / 5 positive 5
[0076]
[0077] Damp heat with skin (UNI EN ISO 4611:2011) 5 / 5 positive 5Salt mist (UNI EN ISO 9227:2012) 5 / 5 positive 5 Color fastness to dry cleaning with 5 / 5 positive 5 perchloroethylene (UNI EN ISO 105-D01:2010)
[0078] Color fastness to domestic and commercial 5 / 5 positive 5 laundering (UNI EN ISO 105-006:2010)
[0079] SO2 / NOx Oxidation (China Test) Internal Method 5 / 5 positive 5 BLU 004
[0080]
[0081] Sulfur dioxide SO2oxidation (UNI ISO 4524 / 2:2008) 5 / 5 positive 5 Result: 5 / 5 Rating: Positive = No change
[0082] Result: 4 / 5 Rating: Positive = A slight change is reported
[0083] Result: 3 / 5 Rating: Negative = A change is reported
[0084] Result: 2 / 5 Rating: Negative = A clear change is reported
[0085] Result: 1 / 5 Rating: Negative = A clear and significant change is reported
[0086] EXAMPLE 1.b
[0087] Using the bath from Example 1 , a brass zipper pull (as in Fig. 1A), which had previously undergone the following galvanic cycle, was coated (as in Fig. 1A): a) Acid copper plating for 10 minutes, approximately 8 pm thick
[0088] b) Acid nickel plating for 15 minutes, approximately 10 pm thick;
[0089] c) Deposition of a nickel-phosphorus alloy for 10 minutes, approximately 1 pm thick;
[0090] d) Deposition of a palladium-nickel alloy for 5 minutes, approximately 1.0 pm thick.
[0091] e) Deposition of 24 kt gold for 5 minutes, approximately 0.5 pm thick.
[0092] The object is then uncovered using a combination of corn sawdust, wax, and abrasive powder, which in 40 minutes is able to remove the dark, powdery layer from the outermost areas, while the deposit remains intact and black in the hidden areas (see Fig. 1C). Once uncovered, the object can be further treated to eliminate the dark, powdery component of the deposit, obtaining a silvery surface with blue reflection in hidden areas (see Fig. 1 D). To this aim, the object is treated in a solution containing 15 g / L of KCN and 30 g / L of KOH, at room temperature, with a cathode current at a voltage of 6 V for the time necessary to obtain complete dissolution of the powder. A representative sample of the galvanized items that passed the quality test was subjected to oxidation tests in accordance with international standardsadopted by the major fashion houses for quality control of finished products. The results are summarized in the following table.
[0093] Test performed Result Rating No. of items tested Artificial sweat (UNI EN ISO 31600 / 2:2015) 5 / 5 positive 5 Synthetic sweat (NF S 80-772:2010) 5 / 5 positive 5 Damp heat with skin (UNI EN ISO 4611:2011) 5 / 5 negative 5 Salt mist (UNI EN ISO 9227:2012) 5 / 5 positive 5 Color fastness to dry cleaning with 5 / 5 positive 5 perchloroethylene (UNI EN ISO 105-D01:2010)
[0094] Color fastness to domestic and commercial 5 / 5 positive 5 laundering (UNI EN ISO 105-006:2010)
[0095] SO2 / NOx Oxidation (China Test) Internal Method 5 / 5 positive 5 BLU 004
[0096]
[0097] Sulfur dioxide SO2oxidation (UNI ISO 4524 / 2:2008) 5 / 5 positive 5 Result: 5 / 5 Rating: Positive = No change
[0098] Result: 4 / 5 Rating: Positive = A slight change is reported
[0099] Result: 3 / 5 Rating: Negative = A change is reported
[0100] Result: 2 / 5 Rating: Negative = A clear change is reported
[0101] Result: 1 / 5 Rating: Negative = A clear and significant change is reported EXAMPLE 1.c
[0102] The procedure is as in Example 1 , but once the surface is uncovered, the sample is cataphoresis-coated.
[0103] A representative sample of the galvanized items that passed the quality test was subjected to oxidation tests in accordance with international standards adopted by the major fashion houses for quality control of finished products. The results are summarized in the following table.
[0104] Test performed Result Rating No. of items tested Artificial sweat (UNI EN ISO 31600 / 2:2015) 5 / 5 positive 5 Synthetic sweat (NF S 80-772:2010) 5 / 5 positive 5 Damp heat with skin (UNI EN ISO 4611:2011) 5 / 5 negative 5 Salt mist (UNI EN ISO 9227:2012) 5 / 5 positive 5 Color fastness to dry cleaning with 5 / 5 positive 5
[0105]
[0106] perchloroethylene (UNI EN ISO 105-D01:2010)Color fastness to domestic and commercial 5 / 5 positive 5 laundering (UNI EN ISO 105-C06:2010)
[0107] SO2 / NOx Oxidation (China Test) Internal Method 5 / 5 positive 5 BLU 004
[0108]
[0109] Sulfur dioxide SO2oxidation (UNI ISO 4524 / 2:2008) 5 / 5 positive 5 Result: 5 / 5 Rating: Positive = No change
[0110] Result: 4 / 5 Rating: Positive = A slight change is reported
[0111] Result: 3 / 5 Rating: Negative = A change is reported
[0112] Result: 2 / 5 Rating: Negative = A clear change is reported
[0113] Result: 1 / 5 Rating: Negative = A clear and significant change is reported
[0114] EXAMPLE 2
[0115] The following were dissolved in 1 L of demineralized water:
[0116] • 50 g / L of sodium gluconate
[0117] • 60 g / L of iminodiacetic acid
[0118] • 0.40 g / L of In as indium sulfate
[0119] • 0.40 g / L of Ru as ruthenium chloride
[0120] • 0.50 g / L of Te as tellurium oxide
[0121] The pH of the solution was adjusted with sulfuric acid to a value comprised between 4.5 and 5.0. No precipitation or turbidity was observed. A 5 cm x 3.5 cm brass sheet, previously plated with nickel and subsequently with a 23kt Au-Ni alloy, was treated with the above solution at a temperature of 60 °C for 90 seconds, at a current of 2.0 A / dm2. A cohesive, grey powder (L=28, a*=1.0, b*=3.0) is obtained. Uncovering, under the same conditions, carried out on a zipper pull with the same galvanic cycle described in Example 1a, occurs in 60 minutes.
[0122] EXAMPLE 3
[0123] To the solution described in Example 1, 0.25 g / L of Cu (in the form of copper (II) sulfate) are added. Under the same deposition conditions (temperature and current), a black powder (L=7; a*=0.6; b*=1.0) is obtained, which is not very cohesive and easily uncoverable in 30 minutes. The overall composition of the deposit is as follows:
[0124] In 35.2% w / w
[0125] Te 18.7% w / wRu 8.9% w / w
[0126] Cu 37.2% w / w
[0127] The composition of the powdery component of the deposit only, mechanically removed using conductive adhesive tape, is as follows:
[0128] In 39.0% w / w
[0129] Te 18.5% w / w
[0130] Ru 7.3% w / w
[0131] Cu 43.9% w / w
[0132] Once the dark, powdery layer is removed by simple rubbing, the deposit appears grey-blue in color.
[0133] A representative sample of the galvanized items that passed the quality test was subjected to oxidation tests in accordance with international standards adopted by the major fashion houses for quality control of finished products. The results are summarized in the following table.
[0134] Test performed Result Rating No. of items tested Artificial sweat (UNI EN ISO 31600 / 2:2015) 4 / 5 positive 5 Synthetic sweat (NF S 80-772:2010) 2 / 5 negative 5 Damp heat with skin (UNI EN ISO 4611:2011) 3 / 5 negative 5 Salt mist (UNI EN ISO 9227:2012) 5 / 5 positive 5 Color fastness to dry cleaning with 5 / 5 positive 5 perchloroethylene (UNI EN ISO 105-D01:2010)
[0135] Color fastness to domestic and commercial 5 / 5 positive 5 laundering (UNI EN ISO 105-006:2010)
[0136] SO2 / NOx Oxidation (China Test) Internal Method 3 / 5 negative 5 BLU 004
[0137] Sulfur dioxide SO2 oxidation (UNI ISO 3 / 5 negative 5
[0138]
[0139] 4524 / 2:2008)
[0140] Result: 5 / 5 Rating: Positive = No change
[0141] Result: 4 / 5 Rating: Positive = A slight change is reported
[0142] Result: 3 / 5 Rating: Negative = A change is reported
[0143] Result: 2 / 5 Rating: Negative = A clear change is reported
[0144] Result: 1 / 5 Rating: Negative = A clear and significant change is reportedEXAMPLE 4
[0145] To the solution described in Example 1, 0.050 g / L of Pt (in the form of platinum (II) dinitrosulfate) are added. Under the same deposition conditions (temperature, time, and current), a black powder with blue reflections (L = 23.03; a* = -1.05; b* = 1.75) is obtained, which is not very cohesive and can be uncovered in 45 minutes. The overall composition of the deposit is:
[0146] In 37.3% w / w
[0147] Te 38.3% w / w
[0148] Ru 11.6 % p / p
[0149] Pt 11.1 % w / w
[0150] Once the dark powdery layer is removed by simple rubbing, the deposit appears dark grey in color.
[0151] EXAMPLE 5
[0152] The following were dissolved in 1 L of demineralized water:
[0153] • 160 g of ammonium sulfate
[0154] • 10 g of potassium diphosphate
[0155] • 0.15 g of Ru as ruthenium chloride
[0156] • 0.20 g of Te as tellurium oxide
[0157] • 0.20 g / L of Pt as platinum dinitrosulfate
[0158] • 0.40 g / L of In as indium sulfate
[0159] The pH of the solution was adjusted with sulfuric acid to a value comprised between 2.4 and 2.8. A 5 cm x 3.5 cm brass sheet, previously plated with nickel and subsequently with gold, was treated with the above-described solution at a temperature of 60 °C, with a deposition time of 60 seconds and a current of 2.0 A / dm2. A powdery and loosely cohesive deposit is obtained with colorimetric coordinates L = 28; a* = 0.03; b* = -0.87. The overall composition of the deposited layer, obtained by EDS spectroscopy, is:
[0160] In 31.3% w / w
[0161] Te 38.9% w / w
[0162] Ru 3.25 p / p
[0163] Pt 26.6% w / wThen, the formulation is tested on a small-scale pilot plant. A galvanic rack containing 30 zipper pulls is prepared, onto which the following galvanic cycle is applied:
[0164] a) Acid copper plating for 10 minutes, approximately 8 pm thick
[0165] b) Acid nickel plating for 15 minutes, approximately 10 pm thick;
[0166] c) Deposition of a nickel-phosphorus alloy for 10 minutes, approximately 1 pm thick;
[0167] d) Deposition of a palladium-nickel alloy for 5 minutes, approximately 1.0 pm thick.
[0168] Then, treatment with the above-described solution is performed at a temperature of 60°C, with a deposition time of 50 seconds and a current of 2.0 A / dm2
[0169] The resulting powdery deposit is black in color but has evident blue reflections and areas, which do not meet current market requirements. Furthermore, color uniformity and appearance of the deposit is strongly influenced by the position of the zipper pull in the rack with respect to the current density and stirring of the solution; this is another aspect that makes this platinum-based formulation not particularly suitable or advantageous for obtaining a vintage effect reproducible on a large number of different geometries and items.
[0170] Test performed Result Rating No. of items tested Artificial sweat (UNI EN ISO 31600 / 2:2015) 5 / 5 positive 5 Synthetic sweat (NF S 80-772:2010) 5 / 5 positive 5 Damp heat with skin (UNI EN ISO 4611:2011) 5 / 5 negative 5 Salt mist (UNI EN ISO 9227:2012) 5 / 5 positive 5 Color fastness to dry cleaning with 5 / 5 positive 5 perchloroethylene (UNI EN ISO 105-D01:2010)
[0171] Color fastness to domestic and commercial 5 / 5 positive 5 laundering (UNI EN ISO 105-006:2010)
[0172] SO2 / NOx Oxidation (China Test) Internal Method 5 / 5 positive 5 BLU 004
[0173]
[0174] Sulfur dioxide SO2oxidation (UNI ISO 4524 / 2:2008) 5 / 5 positive 5 Result: 5 / 5 Rating: Positive = No change
[0175] Result: 4 / 5 Rating: Positive = A slight change is reported
[0176] Result: 3 / 5 Rating: Negative = A change is reportedResult: 2 / 5 Rating: Negative = A clear change is reported
[0177] Result: 1 / 5 Rating: Negative = A clear and significant change is reported EXAMPLE 6
[0178] To the solution described in Example 1, 0.030 g / L of Bi (in the form of bismuth citrate) is added. Under the same deposition conditions (temperature, time, and current), a dark powder with red reflections (L = 17.8; a* = 5.3; b* = 4.7) is obtained, which is loosely cohesive and can be uncovered in 45 minutes.
[0179] The overall composition of the deposit is:
[0180] In 34.9% w / w
[0181] Te 47.4% w / w
[0182] Ru 7.6 % p / p
[0183] Bi 10.1% w / w
[0184] EXAMPLE 7
[0185] The following were dissolved in 1 L of demineralized water:
[0186] • 160 g of ammonium sulfate
[0187] • 10 g of potassium diphosphate
[0188] • 0.2030 g of Ru as ruthenium chloride
[0189] • 0.20 g of Te as tellurium oxide
[0190] • 0.10 g / L of Bi as bismuth citrate
[0191] • 0.353 g / L of In as indium sulfate
[0192] The pH of the solution was adjusted with sulfuric acid to a value comprised between 2.4 and 2.8. A 5 cm x 3.5 cm brass sheet, previously plated with nickel and subsequently with gold, was treated with the above-described solution at a temperature of 60 °C, with a deposition time of 60 seconds and a current of 2.0 A / dm2. A dark brown, powdery, and loosely cohesive deposit is obtained with colorimetric coordinates L = 21 ; a* = 8.0; b* = 11.7. The overall composition of the deposited layer is:
[0193] In 29.9% w / w
[0194] Te 37.8% w / w
[0195] Ru 8.8 % p / p
[0196] Bi 23.4% w / wEXAMPLE 7. a
[0197] Using the bath from Example 7, and under the same electroplating conditions, a brass zipper pull, which had previously undergone the following galvanic cycle, was covered:
[0198] 1. Acid copper plating for 10 minutes, approximately 8 pm thick
[0199] 2. Acid nickel plating for 15 minutes, approximately 10 pm thick;
[0200] 3. Deposition of a nickel-phosphorus alloy for 10 minutes, approximately 1 pm thick;
[0201] 4. Deposition of a palladium-nickel alloy for 5 minutes, approximately 1.0 pm thick.
[0202] The object is then uncovered using a combination of com sawdust, wax, and abrasive powder, which in 50 minutes is able to remove the dark, powdery layer from the outermost areas, while the deposit remains intact and brown-colored in the hidden areas.
[0203] Test performed Result Rating No. of items tested Artificial sweat (UNI EN ISO 31600 / 2:2015) 5 / 5 positive 5 Synthetic sweat (NF S 80-772:2010) 5 / 5 positive 5 Damp heat with skin (UNI EN ISO 4611:2011) 5 / 5 negative 5 Salt mist (UNI EN ISO 9227:2012) 5 / 5 positive 5 Color fastness to dry cleaning with 5 / 5 positive 5 perchloroethylene (UNI EN ISO 105-D01:2010)
[0204] Color fastness to domestic and commercial 5 / 5 positive 5 laundering (UNI EN ISO 105-006:2010)
[0205] SO2 / NOx Oxidation (China Test) Internal Method 5 / 5 positive 5 BLU 004
[0206]
[0207] Sulfur dioxide SO2oxidation (UNI ISO 4524 / 2:2008) 5 / 5 positive 5
[0208] Result: 5 / 5 Rating: Positive = No change
[0209] Result: 4 / 5 Rating: Positive = A slight change is reported
[0210] Result: 3 / 5 Rating: Negative = A change is reported
[0211] Result: 2 / 5 Rating: Negative = A clear change is reported
[0212] Result: 1 / 5 Rating: Negative = A clear and significant change is reported
Claims
CLAIMS1. An electroplated alloy consisting of In, Te, Ru, and optionally another metal selected from the group consisting of Pt, Cu, Bi, Zr, Sn, Co, Ni, Ge, Ga, Se, Zn, Fe, and Pd, said alloy having a powdery consistency and CIELAB color coordinates, as measured with a D65 illuminant in reflection mode with Specular Component Included (SCI) and an observation angle of 10°, within the range 2<L<40; -10<a*<+10; -20<b*<+20.
2. The alloy according to claim 1 having composition:In 25-55% w / w;Te 15-50% w / w;Ru 5-12% w / w;0-40% w / w of another metal selected from the group consisting of Pt, Cu, Bi, Zr, Sn, Co, Ni, Ge, Ga, Se, Zn, Fe, and Pd.
3. The alloy according to claim 1 or 2 consisting of In, Te, and Ru.
4. The alloy according to claim 3 consisting of:In 45-55% w / w;Te 35-45% w / w;Ru 7-11 % w / w;having CIELAB color coordinates within the range 5<L<20; -2<a*<+2; -2<b*<+2.
5. An aqueous solution for electroplating of the alloy according to any one of claims 1-4, said solution having a pH of 0.5-7 and comprising a ruthenium (Ru) salt, a tellurium (Te) salt, an indium (In) salt, a conductive salt, and optionally a salt of another metal selected from the group consisting of Pt, Cu, Bi, Zr, Sn, Co, Ni, Ge, Fe, Ga, Se, Zn, and Pd.
6. The solution according to claim 5, wherein the pH is 1-4, the concentration of indium as a metal is 0.05-1 g / L, the concentration of tellurium as a metal is 0.05-1 g / L, the concentration of ruthenium as a metal is 0.05-1 g / L, the concentration of the conductive salt is 1-300 g / L, and the concentration of the optional salt of another metal is 0.01-0.30 g / L.
7. A method for electroplating of an alloy according to any one of claims 1 -4, said method comprising the use of a solution according to any one of claims 5-6.
8. The method according to claim 7, wherein the temperature is 20-80 °C, the working current is 0.5 - 5 A / dm2, and the voltage is 0.5-10 V.
9. A method for obtaining a finished object with a vintage aesthetic effect, said method comprising electroplating of an alloy according to any one of claims 7-8 onto said object, and subsequent at least partial removal of said alloy by mechanical removal.
10. A method for obtaining a finished object with a bicolor aesthetic effect, said method comprising the steps according to claim 9 and subsequent transformation of the residual powder alloy into a shiny white deposit having CIELAB color coordinates within the range 70<L<100; -10<a*<+10; -10<b*<+10 by an electrolytic treatment of ruthenium stripping or degreasing.