Insoluble calcium salts from calcium-containing material

The process recovers insoluble calcium salts from calcium-containing materials by leaching and purification, addressing the need for sustainable utilization of industrial side streams and producing valuable calcium salts with low solubility.

WO2026234328A1PCT designated stage Publication Date: 2026-11-12TAPOJÄRVI OY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/FI2026/050239
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-05-08
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

There is a need for novel methods to utilize industrial side streams, particularly slags, as raw materials for producing valuable products, as they are often treated as waste and have limited applications.

Method used

A process and system for recovering insoluble calcium salts from calcium-containing materials, such as slags, by leaching with acids to produce calcium-containing leachate and solid residue, followed by separation and purification steps to obtain insoluble calcium salts like calcium citrate and calcium stearate.

Benefits of technology

This process enables the efficient production of insoluble calcium salts with low water solubility, reducing waste and providing a sustainable use for industrial by-products, while maintaining high purity and minimizing impurity leaching.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FI2026050239_12112026_PF_FP_ABST
    Figure FI2026050239_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a process and a system for recovering an insoluble calcium salt from calcium-containing material. The process comprises leaching the calcium-containing material; separating a solid residue from calcium-containing leachate; recovering a solid calcium salt from the calcium-containing leachate; and separating a solid calcium salt from a residual stream.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Insoluble calcium salts from calcium-containing material

[0002] Technical field

[0003] The invention is related to processes and systems for recovering insoluble calcium salts from calcium-containing material, such as slag.

[0004]

[0005] Many industrial processes produce co-products and side products in addition to the main product of the process. Some side streams of these processes may have conventionally even been treated as waste.

[0006] With the increasing environmental concern, there is an increasing demand for sustainable products and circular economy processes. Industrial side streams previously considered as waste are continuously explored for novel uses.

[0007] Slags are an example of industrial process streams that show potential for novel uses. Slags are a class of materials obtained as by-products or coproducts in metallurgical processes. Composition of slags varies by the exact metallurgical process in question. Slags often comprise mixtures of metal oxides and silicon dioxide. Slags may also contain metal sulfides and elemental metals. The major components of slags include the oxides of calcium, magnesium, silicon, iron, and aluminium, with lesser amounts of manganese, phosphorus, and others depending on the specifics of the raw materials used.

[0008] Slags are conventionally used in construction industry (e.g., in concretes), landfilling applications and agriculture (e.g., as a liming material). Slags may also be used as a raw material for producing certain metal compounds. However, novel methods for utilizing slags are needed. Slags, being byproducts or co-products of metallurgical processes, serve as a promising raw material for various applications within the concept of circular economy.Summary

[0009] An object of the invention is to reduce or even eliminate the drawbacks found in the prior art.

[0010] Particularly, an object of the presented invention is to provide novel uses for industrial side streams.

[0011] A further object of the invention is to provide processes for producing calcium salts that utilize industrial side streams as a raw material.

[0012] The invention is defined by what is recited in the independent claims. Embodiments or examples of the invention are presented in the dependent claims.

[0013] Any embodiments or examples of the invention presented herein that are specified with the open term ‘comprise’ may be further limited with a closed term ‘consisting of’.

[0014] All embodiments or examples of the invention are mutually freely combinable, unless otherwise indicated. The presented embodiments and examples of the invention are applicable to all aspects of the invention, both the process and the system.

[0015] Particularly, a process for recovering an insoluble calcium salt from calcium-containing material is provided. Correspondingly, a system for recovering an insoluble calcium salt from calcium-containing material is provided.

[0016] The presented process and system both utilize calcium-containing material as a starting material. Calcium-containing material should be in the course of this specification understood as a material having a calcium content high enough to facilitate profitable calcium salt production. Suitable calcium-containing materials may have a calcium content as calcium oxide (CaO) in the range of 20-60 wt-%, preferably in the range of 25-60 wt-%, more preferably in the range of 30-60 wt-%, calculated as weight percentage of calcium oxide of the total weight of the material. The calcium content of 20-60 wt-% as CaOcorresponds to approx. 13-40 wt-% of the total weight of the calcium-containing material as pure calcium. Correspondingly, the 25-60 wt-% as CaO corresponds to approx. 17-40 wt-% as pure calcium, and the 30-60 wt-% as CaO corresponds to approx. 20-40 wt-% as pure calcium, of the total weight of the calcium-containing material.

[0017] The presented process and system are suitable for producing insoluble calcium salts from calcium-containing material. The term ‘insoluble’ should be understood as poor solubility in water. Solubility of the calcium salt in water should be 0.2 g / 100 ml at 20°C or less. In other words, the insoluble calcium salt is a calcium salt having a solubility in water of 0.2 g / 100 ml at 20°C or less, such as 0.0001-0.2 g / 100 ml or even 0.0001-0.1 g / 100 ml at 20°C.

[0018] Brief description of the drawings

[0019] Fig. 1 presents the process and system of the invention.

[0020] Fig. 2 presents processes and systems according to embodiments of the invention.

[0021] Fig. 3 presents processes and systems according to embodiments of the invention.

[0022] Detailed description

[0023] The following reference numberswill be used in the course of this specification.

[0024] 100 system

[0025] 101 leaching reactor

[0026] 102 means for separating solid residue from calcium-containing leachate 103 means for recovering a solid calcium salt from the calcium-containing leachate

[0027] 104 means for separating solid calcium salt from residual stream

[0028] 105 means for drying solid calcium salt

[0029] 106 means for post-treating residual stream

[0030] 107 means for returning treated residual stream to acid

[0031] 200 calcium-containing material

[0032] 201 acid202 calcium-containing leachate

[0033] 204 solid residue

[0034] 206 solid calcium salt

[0035] 208 residual stream

[0036] 210 dried calcium salt

[0037] 212 treated stream

[0038] An insoluble calcium salt may be produced by the presented process. Solubility of the calcium salt in water should be 0.2 g / 100 ml at 20°C or less. In other words, the insoluble calcium salt is a calcium salt having a solubility in water of 0.2 g / 100 ml at 20°C or less, such as 0.0001-0.2 g / 100 ml at 20°C, preferably 0.0001-0.1 g / 100 ml at 20°C.

[0039] A process for recovering an insoluble calcium salt from calcium-containing material is presented. The process may comprise or consist of

[0040] a. leaching the calcium-containing material using an acid in a leaching reactor to dissolve calcium from the calcium-containing material, thus producing a process stream comprising a calcium- containing leachate and a solid residue;

[0041] b. separating the solid residue from the calcium-containing leachate;

[0042] c. recovering a solid calcium salt from the calcium-containing leachate, thus providing the solid calcium salt and a residual stream; and

[0043] d. separating the solid calcium salt from the residual stream.

[0044] Unless otherwise indicated, the process steps a. to d. are performed in the order specified herein. In other words, the leaching at a. is the first step in the process, followed subsequently by separating the solid residue at b., recovering the solid calcium salt at c., and separating the solid calcium salt at d.

[0045] A system for recovering an insoluble calcium salt from calcium-containing material is further presented. The system is configured to recover an insoluble calcium salt according to the presented process. The system comprises or consists of- a leaching reactor configured to leach the calcium-containing material using an aqueous acid solution to dissolve calcium from the calcium- containing material, thus configured to produce a process stream comprising a calcium-containing leachate and a solid residue;

[0046] - a means for separating the solid residue from the calcium-containing leachate;

[0047] - a means for recovering a solid calcium salt from the calcium-containing leachate, thus configured to provide the solid calcium salt and a residual stream; and

[0048] - a means for separating the solid calcium salt from the residual stream.

[0049] The presented process may be a batch process or a continuous process.

[0050] Referring to Figures 1-3, the presented process may comprise leaching the calcium-containing material 200 using an acid 201 at a. in a leaching reactor 101. The calcium-containing material 200 is leached in order to dissolve calcium from the calcium-containing material 200. Thus, a process stream comprising a calcium-containing leachate 202 and residue 204 is produced. Correspondingly, the presented system 100 may comprise a leaching reactor 101 configured to leach the calcium-containing material 200 using an acid 201 to dissolve calcium from the calcium-containing material 200. The leaching reactor 101 is thus configured to produce a process stream comprising a calcium-containing leachate 202 and a solid residue 204.

[0051] The calcium-containing material 200 suitable for the present invention may originate from different sources, provided that the calcium content in the material is suitable for the presented method. For example, materials comprising calcium as silicates, hydroxides, carbonates, or combinations thereof may be suitable for the present invention. For example slags, particularly pyrometallurgical slags may be suitable materials for the invention. Examples of suitable slags include, but are not limited to: bauxite slag, copper slag, steel slag, stainless steel slag, carbon steel slag, and any combinations thereof. For clarity, slag should be understood as slag formed in the manufacturing process of a certain metal or metal alloy. For example, steel slag should be understood as slag formed in the manufacturing process of steel. Likewise, stainless steel slag and carbon steel slag refer to slags formedin the manufacturing process of stainless steel and carbon steel, respectively. The slag may originate from different kinds of metallurgical processes, or different process stages of metallurgical processes, e.g., basic oxygen furnace slag (BOF slag), oxygen decarburization slag (OD slag), or electric arc furnace slag (EAF slag).

[0052] The acid 201 may be selected from the group comprising inorganic acids, organic acids, and any combination thereof. The acid may comprise citric acid, malic acid, stearic acid, or any combination thereof. Preferably, the acid is citric acid or a combination of citric acid and malic acid. The acid 201 is preferably used as an acid solution using an aqueous solvent or an organic solvent. More preferably, the acid 201 is used as an aqueous acid solution comprising water as the aqueous solvent.

[0053] The acid 201 used for the leaching at a. provides the anion for the insoluble calcium salt produced by the presented method. Therefore, the produced calcium salt may be selected from the group comprising calcium citrate, calcium malate, calcium stearate, or any combination thereof. The solid calcium salt 206 may be calcium stearate. The solid calcium salt 206 may be a calcium citrate salt, such as calcium citrate, calcium citrate tetrahydrate, or calcium citrate malate. ‘Calcium citrate tetrahydrate’ should be understood as tricalcium dicitrate tetrahydrate. In other words, the calcium citrate salt may be anhydrous calcium citrate that does not comprise crystal water, or calcium citrate tetrahydrate that comprises crystal water.

[0054] The acid 201 may be added in stoichiometric excess compared to the amount of the calcium salt to be recovered from the calcium-containing material 200. The acid 201 may be added in a weight ratio in the range of 1:1 to 10:1 to the weight of calcium in the calcium-containing material, preferably in a weight ratio in the range of 2: 1 to 5: 1 to the weight of calcium in the calcium-containing material.

[0055] The amount of the acid 201 added may alternatively or in addition be determined in comparison to the weight of the calcium-containing material 200 to be leached. The acid 201 may be added in a weight ratio in the range of 1:1to 1 :5 to the weight of the calcium-containing material, preferably in a weight ratio of 1 :1 to 1 :4 to the weight of the calcium-containing material.

[0056] Referring to Figures 1-3, the leaching reactor 101 at a. may be a continuous reactor. A calculated dwell time of the calcium-containing material in the continuous reactor may be in the range of 0.5-30 min. Preferably, the dwell time is in the range of 1-10 min, more preferably in the range of 3-8 min, even more preferably in the range of 4-6 min. The selected dwell time may enable an efficient or even complete leaching of the slag in the leaching reactor without compromising process economy in terms of, e.g., energy usage.

[0057] Alternatively, the leaching reactor 101 may be a batch reactor. In alteration to a single batch reactor, the leaching reactor 101 may be arranged as a plurality of batch reactors connected in series, such as two, three, or four batch reactors connected in series. A reaction time in the batch reactor or the plurality of batch reactors may be in the range of 0.5-30 min. Preferably, the reaction time is in the range of 1-10 min, more preferably in the range of 3-8 min, even more preferably in the range of 4-6 min.

[0058] The dwell time (in a continuous reactor) or the reaction time (in the batch reactor or plurality of batch reactors) as specified herein may be selected to obtain optimal leaching. Dwell times or reaction times shorter than specified above may lead to incomplete or insufficient leaching of the calcium, thus leaving an unacceptably high calcium concentration in the solid residue 204. Dwell times or reaction times longer than specified above may, in the other hand, lead to warming of the leachate 202, which may in turn lead to leaching of impurities or undesired elements from the calcium-containing material. Thus, the dwell times or reaction times as specified above ensure an optimal and selective leaching of calcium from the calcium-containing material.

[0059] The presented process may comprise controlling the temperature of the calcium-containing leachate 202 exiting the leaching reactor 101 at a. such that the temperature of the calcium-containing leachate 202 exiting the leaching reactor 101 is in the range of 0-10°C, preferably in the range of 0-5°C. Efficient temperature control may enable efficient calcium salt recovery at c. (see below). Controlling the temperature of the calcium-containing leachate202 exiting the leaching reactor 101 may comprise cooling the calcium-containing leachate 202 exiting the leaching reactor 101, cooling the acid entering the leaching reactor 101, cooling the leaching reactor 101 during the leaching process, or any combination thereof.

[0060] Controlling the temperature of the calcium-containing leachate 202 exiting the leaching reactor 101 may comprise cooling the calcium-containing leachate 202 exiting the leaching reactor 101. With efficient cooling of the calcium-containing leachate 202 exiting the leaching reactor 101 , recovery of the solid calcium salt 206 may be efficient, meaning that essentially all calcium originally contained in the calcium-containing leachate 202 is recovered from the leachate 202. Allowing the temperature of the calcium-containing leachate 202 exiting the leaching reactor 101 to increase above the specified range might result in a poor recovery of the solid calcium salt 206. The system 100 may correspondingly comprise a means for controlling the temperature of the calcium-containing leachate 202 exiting the leaching reactor 101 at a.

[0061] Controlling the temperature of the calcium-containing leachate 202 exiting the leaching reactor 101 may comprise cooling the acid 201 entering the leaching reactor 101 such that the temperature of the acid 201 when entering the leaching reactor 101 is in the range of 0-5°C. Cooling the acid entering the leaching reactor 101 may have an indirect effect on the recovery of the solid calcium salt 206 at the precipitation phase at c. through optimization of energy streams in the process. Controlling the temperature of the acid 201 entering the leaching reactor 101 may assist in controlling the temperature of the calcium-containing leachate 202 exiting the leaching reactor 101. Since the leaching is an exothermic reaction, temperature of the slag will increase during leaching. When the temperature of the aqueous acid solution 201 entering the leaching reactor 101 is properly controlled, i.e., when the acid 201 is cooled within the specified temperature range, it will be easier to control the temperature of the leachate 202 exiting the leaching reactor. In other words, controlling the temperature of the acid 201 entering the leaching reactor 101 will make it easier to control the temperature of the leachate 202 exiting the reactor within its specified temperature range. Correspondingly, the system 100 may comprise a means for controlling the temperature of the acid 201 entering the leaching reactor 101 at a, such as a cooler.Controlling the temperature of the calcium-containing leachate 202 exiting the leaching reactor 101 may further comprise cooling the leaching reactor 101 during the leaching at a. Cooling the leaching reactor 101 may comprise, e.g., conducting heat away from the reactor via its outer housing. Correspondingly, the system 100 may comprise a means for cooling the leaching reactor 101 during the leaching at a.

[0062] In efficient leaching process, most or even essentially all calcium compounds originally contained in the calcium-containing material 200 are dissolved into the calcium-containing leachate 202. In materials suitable for the present invention, calcium may be present as, e.g., calcium silicates, calcium hydroxides, calcium oxides, and combinations thereof. The solid residue 204 comprises components of the calcium-containing material 200 that are not soluble in the used acid, e.g., metals originally present in the calcium-containing material 200.

[0063] Referring to Figures 1-3, the presented process comprises separating the solid residue 204 from the calcium-containing leachate 202 at b. The separating is preferably performed by filtering. More preferably, the filtering is performed using a continuous filter, such as a belt filter or a drum filter. Continuous filtering may provide efficient separation of the residue 204 from the calcium-containing leachate 202, which may in turn improve the processability of the calcium-containing leachate 202 later in the process. The system 100 may correspondingly comprise a means 102 for separating the residue 204 from the calcium-containing leachate 202 at b. Preferably, the means 102 for separating the residue 204 from the calcium-containing leachate 202 is a filter, more preferably a continuous filter. In particularly preferred systems, the means 102 for separating the residue 204 from the calcium-containing leachate 202 is a belt filter or a drum filter.

[0064] Referring to Figures 1-3, the presented process may comprise recovering a solid calcium salt 206 from the calcium-containing leachate 202. In other words, the solid calcium salt 206 and a residual stream 208 are produced. Correspondingly, the system 100 may comprise a means 103 for recovering the solid calcium salt 206 from the calcium-containing leachate 202. The means 103 for recovering the solid calcium salt 206 may thus be configured toprovide the solid calcium salt 206 and the residual stream 208. The solid calcium salt 206 and the residual stream 208 may be obtained as a mixture at the recovering at c. In other words, the solid calcium salt 206 may be dispersed in the residual stream 208 after the recovering at c.

[0065] Recovering the solid calcium salt 206 from the calcium-containing leachate 202 at c. may comprise precipitating the solid calcium salt 206 from the calcium-containing leachate 202. Precipitation, or in other words, sedimentation, of the solid calcium salt 206 from the calcium-containing leachate 202, may occur when the concentration of the calcium salt in the calcium-containing leachate exceeds its solubility, causing the calcium salt to solidify out of the leachate, thus leaving the residual stream 208. Precipitation may occur due to a change in temperature, a change in concentration of the salt in the leachate (e.g., by evaporation of water from the leachate), or due to a change in the solvation environment (e.g., due to change of solvent or addition of a second solvent). Precipitation may occur more rapidly from a supersaturated solution.

[0066] The recovering at c., such as the precipitation, may performed at a temperature in the range of 30-70°C. The recovering at c. may be carried out for 1-60 minutes, such as for 10-30 minutes. Solubility of calcium salts, particularly in water, may decrease upon an increase in temperature. In other words, the leachate 202 may be a supersaturated calcium salt solution. Thus, recovering the solid calcium salt 206 may be faster at these specified elevated temperatures. However, if the temperature is higher than specified here, precipitation of impurities may increase to an unacceptable level. In other words, selecting the recovering temperature within the specified range may facilitate obtaining the solid calcium salt in a high purity. Particularly in processes aiming to recover calcium citrate tetrahydrate, i.e. , crystal water -containing calcium citrate, the precipitation may be performed at a temperature in the range of 30-50°C. At temperatures higher than 50°C, the crystal water may evaporate from the structure, thus producing a product different from what was intended.

[0067] Leaching of calcium, as desired, but also leaching of impurities, may occur not only at the leaching at a., but also during the separation at b., the recovery atc. and / or even during the separation at d., until the solid calcium salt 206 is completely separated from the residual stream 208. Therefore, it is beneficial to keep the time used for the separation at b., for the recovery at c. and / or for the separation at d. as short as possible to minimize the amount of impurities leached from the calcium-containing material 200. The separation time at b., the recovery time at c., and / or the separation time at d. may individually for each step be in the range of 0.5-10 min, such as in the range of 0.5-3 min.

[0068] The process may comprise monitoring and / or controlling pH at the leaching at a., at the separation at b., at the recovering at c., and / or at the separation at d. In other words, pH of the calcium-containing leachate 202, the mixture of the solid calcium salt 206 and the residual stream 208, and / or the residual stream 208 may be monitored and / or controlled at exit from the leaching reactor 101 , at exit from the means 102 for separating solid residue from calcium-containing leachate, at enter to the means 103 for recovering the solid calcium salt 206, at the means 103 for recovering the solid calcium salt 206, at the means 104 for separating the solid calcium salt 206, and / or at the exit from the means 104 for separating the solid calcium salt 206. At any of these checkpoints, i.e. at exit from the leaching reactor 101, at exit from the means 102 for separating the residue 204, at enter to the means 103 for recovering the solid calcium salt 206, at the means 103 for recovering the solid calcium salt 206, at the means 104 for separating the solid calcium salt 206, and / or at the exit from the means 104 for separating the solid calcium salt 206, the pH of the calcium-containing leachate 202 may be in the range of 3-6, preferably in the range of 3-5, more preferably in the range of 4-4.9.

[0069] In preferred processes, the the leaching at a. may comprise controlling the temperature and pH of the calcium-containing leachate 202 exiting the leaching reactor 101 simultaneously, such that the temperature of the calcium-containing leachate 202 exiting the leaching reactor 101 may be in the range of 0-25°C, preferably in the range of 0-20°C, and that the pH of the calcium-containing leachate 202 exiting the leaching reactor 101 may be in the range of 2-7, preferably in the range of 4-5.

[0070] pH values within the range specified here may enable an efficient and selective leaching of calcium from the calcium-containing material. If the pH increasesabove the specified range, leaching of the calcium may become less efficient, meaning that the calcium does not as effectively dissolve from the calcium-containing material. Furthermore, at pH values higher than specified here, the amount of undesired elements or impurities dissolving or leaching out from the calcium-containing material may increase to an unacceptable level. In other words, pH values within the specified range may enable an efficient recovery of the solid calcium salt 206 at a high purity.

[0071] Duration of the separation at b. and / or the recovering at c. may be determined by monitoring the pH pf the process stream. The pH may be monitored at exit from the means 102 for separating the residue 204, at enter to the means 103 for recovering the solid calcium salt 206, at the means 103 for recovering the solid calcium salt 206, at the means 104 for separating the solid calcium salt 206, and / or at the exit from the means 104 for separating the solid calcium salt 206. To prevent or at least to reduce leaching of impurities or other undesired elements from the calcium-containing material during the separation at b. and / or during the recovering at c., the pH value of the calcium-containing leachate should not increase above the values specified earlier. In other words, particularly at the separation at b. and / or at the recovering at c., pH of the calcium-containing leachate may be in the range of 3-6, preferably in the range of 3-5, more preferably in the range of 4-4.9. The separation at b. and / or the recovering at c. may be ended when the pH reaches a predetermined pH value, the predetermined pH value being within the specified range. In other words, the separation at b. and / or the recovering at c. may be carried out as long as the pH of the calcium-containing leachate 202 and / or of the residual stream 208 stays below the predetermined pH value.

[0072] Referring to Figures 1-3, the process may comprise separating the solid calcium salt 206 from the residual stream 208 at d. As mentioned above, the solid calcium salt 206 and the residual stream 208 may be obtained as a mixture at the recovering at c. The separation at d. may simplify further utilization, e.g. packaging and transport, of the solid calcium salt. Correspondingly, the system 100 may comprise a means 104 for separating the solid calcium salt 206 from the residual stream 208.In preferred processes, the separation at d. may be performed by filtration. Preferably, the filtering is continuous filtering. In other words, the filtering may be performed using a continuous filter, such as a belt filter or a drum filter. Correspondingly, the means 104 for separating the solid calcium salt 206 from the residual stream 208 may be a filter, preferably a continuous filter, such as a belt filter or a drum filter. Continuous filtering may provide uninterrupted separation of the solid calcium salt 206 from the residual stream 208.

[0073] Referring to Figure 2, the process may comprise drying the solid calcium salt 206 at e. to produce a dried calcium salt 210. After the separation at d., there may be traces of solvent left in the solid calcium salt 206 that may hinder the utilization, such as packaging and transport, of the solid calcium salt 206. Thus, it is beneficial to the quality of the insoluble calcium salt product to dry the solid calcium salt 206 by removing the solvent traces. The drying at e. may be performed by thermal methods, such as by heating, thus evaporating any solvent traces from the solid calcium salt 206 to provide the dried calcium salt 210. Correspondingly, the system 100 may comprise a means 105 for drying the solid calcium salt 206. The means 105 for drying the calcium salt may thus be configured to produce the dried calcium salt 210. The means 105 for drying the solid calcium salt 206 may be, e.g., a thermal drier, such as a paddle drier or a spray drier. The spray drier may be particularly suitable for producing anhydrous calcium citrate.

[0074] The insoluble calcium salt obtained by the presented process may be the solid calcium salt 206 or the dried calcium salt 210.

[0075] Referring to Figure 3, the process may further comprise post-treating the residual stream 208 at g. to produce a treated stream 212. Correspondingly, the system 100 may comprise a means 106 for post-treating the residual stream 208. The residual stream 208 originates from the materials used for the leaching at a., after the solid residue 204 and the solid calcium salt 206 are removed from the process stream. Therefore, the residual stream 208 may comprise the acid 201 to an extent where not all the acid is consumed by the solid calcium salt recovery. In situations where the acid 201 is used as an acid solution for the leaching at a., the residual stream may comprise the solvent used in the acid solution. In situations where the acid solution is an aqueousacid solution, the residual stream 208 may comprise water. In other words, the residual stream 208 may be a residual aqueous stream.

[0076] The post-treatment at f. may comprise purifying the residual stream 208, preferably by one or more of adjusting pH, precipitating impurities, ultrafiltration, and reverse osmosis. In situations where the acid 201 is used as an acid solution, the treated stream 212 may be a purified solvent. In situations where the acid 201 is used as an aqueous acid solution, the treated stream 212 may be purified water.

[0077] The process may conveniently further comprise returning the treated stream 212 to the acid 201 at g. to be used for the leaching at a. Correspondingly, the system 100 may comprise a means 107 for returning the treated stream 212 to the acid 201 to be used for the leaching at a.

[0078] The acid solution may comprise the treated stream 212 as the solvent or as a part of the solvent. In situations where the acid 201 is used as an acid solution, the acid solution may comprise the purified solvent obtained by the purification chosen as the post-treatment at f. as the solvent or as a part of the solvent. The treated stream may be combined with a solvent from an external source. In other words, the acid solution may comprise the acid 201 dissolved in a solvent from an external source, recycled solvent, i.e. , the treated stream, or both. In situations where the acid 201 is used as an aqueous acid solution, the aqueous acid solution may comprise the purified water obtained by the purification chosen as the post-treatment at f. as the aqueous solvent or as a part of the aqueous solvent. The treated aqueous stream may be combined with water from an external source, i.e., excess water or fresh water. In other words, the aqueous acid solution may comprise the acid 201 dissolved in water from an external source, recycled water, i.e., the treated aqueous stream, or both.

[0079] The post-treatment at f. and the returning at g. may enable recycling of process streams in the presented process. The post-treatment may reduce the consumption of the solvent used to dissolve the acid 101 for the leaching at a. Particularly in aqueous processes, water consumption of the process is high. Thus, it is beneficial to be able to recycle process streams to reduce theconsumption of external water (or in other words, fresh water). This may reduce the need for external water purification, thereby reducing cost and decreasing the environmental impact of the process.

[0080]

[0081] Example 1

[0082] Calcium citrate tetrahydrate (Ca3(CeH5O7)2*4H2O) was prepared from a stainless steel slag in a following process:

[0083] a. Leaching

[0084] 7.5 g citric acid was added to 200 ml of water in a beaker under magnetic stirring, thus producing a citric acid solution. The beaker was placed in an ice / salt bath. The resulting citric acid solution was cooled to 5°C. 10 g of stainless steel slag was added. The mixture was stirred for 5 minutes while monitoring the pH and the temperature of the mixture. After the 5 minutes of stirring, the mixture had a pH of 4.8 and a temperature of 9°C.

[0085] b. Filtering solid residue

[0086] Residual slag was separated from leachate by vacuum filtering using a Buchner funnel and a Whatman 589 / 2 filter paper. The filtrate was recovered in a beaker. The filtration was continued for 1 minute. pH and temperature of the filtrate was monitored during the filtration. After the filtration, the filtrate had a pH of 4.9 and a temperature of 18°C.

[0087] c. Precipitating calcium citrate tetrahydrate

[0088] The beaker containing the filtrate was heated to 50°C for 20 minutes, whereby calcium citrate tetrahydrate precipitated from the leachate, thus giving solid calcium citrate tetrahydrate dispersed in residual stream. After the precipitation, pH of the mixture stream was 4.2.

[0089] d. Filtering calcium citrate tetrahydrate

[0090] The precipitated calcium citrate tetrahydrate was separated from the residual stream by vacuum filtering using a Buchner funnel and a Whatman 589 / 3 filter paper.e. Drying

[0091] The solid calcium citrate tetrahydrate recovered on the filter paper was dried at 50°C overnight. Mass of the dried calcium citrate tetrahydrate was 8.2 g. 5

[0092] The recovered calcium citrate tetrahydrate was chemically characterized using X-ray fluorescence (PANalytical Axios Max, 4 kW). The content of carbon (C) and sulphur (S) was determined using a LECO® CS-200 combustion analyzer. The chemical composition of the recovered calcium 10 citrate tetrahydrate is presented in Table 1. Content of each element is presented as weight percentage of the total mass of the recovered calcium citrate tetrahydrate.

[0093] Table 1. Elemental composition of calcium citrate tetrahydrate recovered in 15 Example 1.

[0094] Example 2

[0095] Element Al Ca Mg C S Cl Mn Fe Ti Si Sr Content, 0.0123 22.2 0.0847 25.6 0.04 0.0094 0.0344 0.0069 0.0062 0.198 0.0132 wt-%

[0096]

[0097] 20 a. Leaching

[0098] 7.5 g citric acid was added to 150 ml of water in a beaker under magnetic stirring, thus producing a citric acid solution. The beaker was placed in an ice / salt bath. The resulting citric acid solution was cooled to 5°C. 10 g of stainless steel slag was added. The mixture was stirred for 3.5 minutes while 25 monitoring the pH and the temperature of the mixture. After the 5 minutes of stirring, the mixture had a pH of 4.8 and a temperature of 11 °C.

[0099] b. Filtering solid residue

[0100] Residual slag was separated from leachate by vacuum filtering using a 30 Buchner funnel and a Whatman 589 / 2 filter paper. The filtrate was recovered in a beaker. The filtration was continued for 1 minute. pH and temperature ofthe filtrate was monitored during the filtration. After the filtration, the filtrate had a pH of 4.9 and a temperature of 18°C.

[0101] c. Precipitating calcium citrate tetrahydrate

[0102] The beaker containing the filtrate was heated to 50°C for 20 minutes, whereby calcium citrate tetrahydrate precipitated from the leachate, thus giving solid calcium citrate tetrahydrate dispersed in residual stream. After the precipitation, pH of the mixture stream was 4.2.

[0103] d. Filtering calcium citrate tetrahydrate

[0104] The precipitated calcium citrate tetrahydrate was separated from the residual stream by vacuum filtering using a Buchner funnel and a Whatman 589 / 3 filter paper.

[0105] e. Drying

[0106] The solid calcium citrate tetrahydrate recovered on the filter paper was dried at 50°C overnight. Mass of the dried calcium citrate tetrahydrate was 8.4 g.

[0107] The recovered calcium citrate tetrahydrate was chemically characterized using X-ray fluorescence (PANalytical Axios Max, 4 kW). The content of carbon (C) and sulphur (S) was determined using a LECO® CS-200 combustion analyzer. The chemical composition of the recovered calcium citrate tetrahydrate is presented in Table 2. Content of each element is presented as weight percentage of the total mass of the recovered calcium citrate tetrahydrate.

[0108] Table 2. Elemental composition of calcium citrate tetrahydrate recovered in Example 2.

[0109] Element Al Ca Mg C S Mn Fe Ti Si Sr Content, 0.0135 22.5 0.153 25.2 0.03 0.0584 0.0064 0.0087 0.170 0.0138 wt-%

[0110]

[0111] Claims:

[0112] 1. A process for recovering an insoluble calcium salt from calcium- containing material (200), comprising

[0113] a. leaching the calcium-containing material (200) using an acid (201) in a leaching reactor (101) to dissolve calcium from the calcium-containing material, thus producing a process stream comprising a calcium-containing leachate (202) and a solid residue (204);

[0114] b. separating the solid residue (204) from the calcium-containing leachate (202);

[0115] c. recovering a solid calcium salt (206) from the calcium-containing leachate (202), thus providing the solid calcium salt (206) and a residual stream (208); and

[0116] d. separating the solid calcium salt (206) from the residual stream (208).

[0117] 2. The process according to claim 1, wherein the acid (201) used for leaching at a. comprises an acid selected from inorganic acids, organic acids, and any combination thereof, such as citric acid, malic acid, stearic acid, or any combination thereof, preferably wherein the acid is citric acid or a combination of citric acid and malic acid; and / or wherein the acid (201) is used as an acid solution using an aqueous solvent or an organic solvent, preferably wherein the acid (201) is used as an aqueous acid solution.

[0118] 3. The process according to claim 1 or 2, wherein the leaching reactor (101 ) at a. is a continuous reactor; or wherein the leaching reactor (101 ) at a. is a batch reactor, or a plurality of batch reactors connected in series, such as two, three, or four batch reactors connected in series.

[0119] 4. The process according to claim 4, wherein a calculated dwell time of the calcium-containing material (200) in the continuous reactor or a reaction time in the batch reactor or the plurality of batch reactors is in

Claims

the range of 0.5-30 min, preferably in the range of 1-10 min, more preferably in the range of 3-8 min, even more preferably in the range of 4-6 min.

5. The process according to any of the preceding claims, wherein the leaching at a. further comprises controlling the temperature of the calcium-containing leachate (202) exiting the leaching reactor (101) such that the temperature of the calcium-containing leachate (202) exiting the leaching reactor (101) is in the range of 0-10°C, preferably in the range of 0-5°C; and / or controlling the temperature of the acid (201) entering the leaching reactor (101) such that the temperature of the acid (201) entering the leaching reactor (101) is in the range of 0- 5°C.

6. The process according to any of the preceding claims, wherein any of the separating at b. and the separating at d. is individually performed by filtering, preferably wherein the filtering is performed using a continuous filter, such as a belt filter or a drum filter.

7. The process according to any of the preceding claims, wherein the recovering at c. comprises precipitating the solid calcium salt (206) from the calcium-containing leachate (202).

8. The process according to any of the preceding claims, wherein the recovering at c. is performed at a temperature in the range of 30-70°C.

9. The process according to any of the preceding claims, comprising monitoring and / or controlling pH at the leaching at a., at the separation at b., at the recovering at c., and / or at the separation at d.

10. The process according to any of the preceding claims, wherein the solid calcium salt (206) is a calcium citrate salt, such as calcium citrate, calcium citrate tetrahydrate, or calcium citrate malate; or wherein the solid calcium (206) salt is calcium stearate.

11. The process according to any of the preceding claims, further comprisinge. drying the solid calcium salt (206) to produce a dried calcium salt (210).

12. The process according to any of the preceding claims, further comprising one or more off. post-treating the residual stream (208) to produce a treated stream (212); andg. returning the treated stream (212) to the acid (201) to be used for the leaching at a.

13. The process according to claim 11, wherein the post-treatment at f.comprises purifying the residual stream (212) by one or more of adjusting pH, precipitating impurities, ultrafiltration, and reverse osmosis, whereby the treated stream (212) comprises purified water.

14. A system (100) for recovering an insoluble calcium salt from calcium- containing material (200) according to the process of any of claims 1 to 13, the system (100) comprisinga leaching reactor (101) configured to leach the calcium-containing material (200) using an aqueous acid solution (201) to dissolve calcium from the calcium-containing material (200), thus configured to produce a process stream comprising a calcium-containing leachate (202) and a solid residue (204);a means (102) for separating the solid residue (204) from the calcium-containing leachate (202);a means (103) for recovering a solid calcium salt (206) from the calcium-containing leachate (202), thus configured to provide the solid calcium salt (206) and a residual stream (208); and a means (104) for separating the solid calcium salt (206) from the residual stream (208).

15. The system according to claim 14, further comprising one or more of - a means (105) for drying the solid calcium salt (206), thus configured to produce a dried calcium salt (210);- a means (106) for post-treating the residual stream; and- a means (107) for returning the treated stream (212) to the acid (201 ) to be used for the leaching at a.