Polycrystalline diamond, semiconductor material, tool material, and tool
By doping polycrystalline diamond with nitrogen, phosphorus, or aluminum, and adhering to specific Raman scattering spectrum parameters, the graphite content is minimized, improving carrier mobility and fatigue strength, suitable for semiconductor materials and tools.
Patent Information
- Application Number
- PCT/JP2026/017365
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-05-01
- Publication Date
- 2026-11-12
AI Technical Summary
Existing polycrystalline diamond semiconductor materials contain residual graphite, which affects their semiconductor performance and tool materials, necessitating a reduction in graphite content to enhance conductivity and mechanical properties.
The development of polycrystalline diamond with controlled doping of nitrogen, phosphorus, or aluminum, and specific Raman scattering spectrum parameters to minimize graphite content, ensuring improved carrier mobility and fatigue strength, while maintaining high hardness and isotropic properties.
The solution results in polycrystalline diamond with reduced graphite content, enhancing carrier mobility and fatigue strength, suitable for semiconductor materials and tools, with improved mechanical properties and resistance to electrostatic cracks.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure 00000038_0000
Abstract
Description
Polycrystalline Diamond, Semiconductor Material, Tool Material and Tool
[0001] The present disclosure relates to a polycrystalline diamond, a semiconductor material, a tool material and a tool. This application claims priority based on Japanese Patent Application No. 2025-078005 filed on May 8, 2025. The entire contents described in the Japanese patent application are incorporated herein by reference.
[0002] In recent years, techniques for using diamond as a semiconductor material for electronic devices have been studied. In order to apply diamond to semiconductor materials, it is necessary to dope diamond with boron or the like to control the conductivity of diamond.
[0003] Patent Document 1 discloses a technique for producing polycrystalline diamond in which a first element such as boron is dispersed by subjecting graphite containing the first element to high-temperature and high-pressure treatment to convert the graphite into diamond.
[0004] Japanese Unexamined Patent Publication No. 2013-28498
[0005] The polycrystalline diamond of the present disclosure is a polycrystalline diamond containing at least one first element selected from the group consisting of nitrogen, phosphorus, boron, and aluminum, and the content of each of the first elements in the polycrystalline diamond on an atomic number basis is 1.0×10 16 / cm 3 or more and 1.0×10 22 / cm 3 or less, and the full width at half maximum X1 cm of the maximum peak in the primary Raman scattering spectrum of the polycrystalline diamond -1 and the full width at half maximum X2 cm of the maximum peak in the primary Raman scattering spectrum of synthetic type IIa single crystal diamond having a nitrogen content of 1 ppm or less on an atomic number basis -1 satisfy the relationship of the following formula I: X1-X2≧0.1 Formula I In the primary Raman scattering spectrum of the polycrystalline diamond, the first range where the Raman shift is 1340 cm -1 or more and 1380 cm -1 or less, and the Raman shift is 1560 cm -1 or more and 1600 cm-1 In the second range below, no peaks are present, and the primary Raman scattering spectra of the polycrystalline diamond and the synthetic type IIa single crystal diamond are measured at a temperature between 20°C and 25°C using a laser with a wavelength of 532 nm as the excitation light, indicating polycrystalline diamond.
[0006] Figure 1 shows the first-order Raman scattering spectrum of synthetic type IIa single-crystal diamond. Figure 2 is a perspective view showing an example of a state in which graphite is formed on a substrate. Figure 3 is a perspective view showing an example of a state in which polycrystalline diamond is produced by directly converting graphite on the substrate.
[0007] In the polycrystalline diamond described in Patent Document 1, a minute amount of the raw material graphite remains on its surface. From the viewpoint of improving semiconductor performance, diamonds and semiconductor materials with reduced graphite content are desired.
[0008] Therefore, this disclosure aims to provide polycrystalline diamond and semiconductor materials with reduced graphite content. Furthermore, this disclosure aims to provide tool materials made of said polycrystalline diamond and tools equipped with said polycrystalline diamond.
[0009] According to this disclosure, it is possible to provide polycrystalline diamond and semiconductor materials with reduced graphite content. Furthermore, according to this disclosure, it is possible to provide tool materials made of the polycrystalline diamond and tools equipped with the polycrystalline diamond.
[0010] First, embodiments of the present disclosure will be listed and described. (1) The polycrystalline diamond of the present disclosure is a polycrystalline diamond comprising at least one first element selected from the group consisting of nitrogen, phosphorus, boron, and aluminum, wherein the atomic number content of each of the first elements in the polycrystalline diamond is 1.0 × 10 16 / cm 3 The above 1.0 x 10 22 / cm 3 The following is the maximum peak in the first-order Raman scattering spectrum of the polycrystalline diamond, with a full width at half maximum (FMAX) of 1 cm. -1And, the full width at half maximum (FMAX) x 2 cm of the maximum peak in the first-order Raman scattering spectrum of synthetic type IIa single crystal diamond with a nitrogen content of 1 ppm or less based on the number of atoms. -1 This shows the relationship in equation I below, where X1 - X2 ≥ 0.1 Equation I In the first-order Raman scattering spectrum of the polycrystalline diamond, Raman shift 1340 cm⁻¹ -1 1380cm or more -1 The following first range, and Raman shift 1560 cm -1 More than 1600cm -1 In the second range below, no peaks are present, and the primary Raman scattering spectra of the polycrystalline diamond and the synthetic type IIa single crystal diamond are measured at a temperature between 20°C and 25°C using a laser with a wavelength of 532 nm as the excitation light, indicating polycrystalline diamond.
[0011] According to this disclosure, it is possible to provide polycrystalline diamond and semiconductor materials with reduced graphite content. In this disclosure, polycrystalline diamond and semiconductor materials with reduced graphite content also include polycrystalline diamond and semiconductor materials that do not contain graphite.
[0012] (2) In (1) above, the Raman shift λ 1 cm of the maximum peak in the first-order Raman scattering spectrum of the polycrystalline diamond -1 The Raman shift λ2cm of the maximum peak in the first-order Raman scattering spectrum of the synthetic type IIa single crystal diamond. -1 This can also be expressed by showing the relationship in Equation II below: λ1 - λ2 < 0 Equation II
[0013] In polycrystalline diamond exhibiting the relationship in equation II, tensile stress exists within the diamond crystal. Therefore, in semiconductor materials made from this polycrystalline diamond, carrier mobility is improved.
[0014] (3) In (1) or (2) above, the relationship between λ1 and λ2 may be expressed by the following formula IIA: λ1 - λ2 ≤ -0.1 Formula IIA
[0015] According to this, the carrier mobility is further improved in the semiconductor material made of polycrystalline diamond.
[0016] (4) In any of (1) to (3) above, the relationship between λ1 and λ2 may be expressed by the following equation IIB: λ1 - λ2 ≤ -0.2 Equation IIB
[0017] According to this, the carrier mobility is further improved in the semiconductor material made of polycrystalline diamond.
[0018] (5) In (1) above, the Raman shift λ 1 cm of the maximum peak in the first-order Raman scattering spectrum of the polycrystalline diamond. -1 The Raman shift λ2cm of the maximum peak in the first-order Raman scattering spectrum of the synthetic type IIa single crystal diamond. -1 This can also be expressed by showing the relationship in Equation III below: λ1 - λ2 ≥ 0 Equation III
[0019] In polycrystalline diamond exhibiting the relationship shown in equation III above, there is either no stress within the diamond crystal, or compressive stress is present. Therefore, this polycrystalline diamond exhibits improved fatigue strength compared to polycrystalline diamond with tensile stress. This polycrystalline diamond is suitable as a semiconductor material for mobile devices and other applications subject to impact.
[0020] (6) In (1) or (5) above, the relationship between λ1 and λ2 may be expressed by the following formula IIIA: λ1 - λ2 ≥ 0.1 Formula IIIA
[0021] According to this, the fatigue strength of polycrystalline diamond will be further improved.
[0022] (7) In (1), (5), or (6) above, the relationship between λ1 and λ2 may be expressed by the following formula IIIB: λ1 - λ2 ≥ 0.2 Formula IIIB
[0023] According to this, the fatigue strength of polycrystalline diamond will be further improved.
[0024] (8) In any of (1) to (7) above, the polycrystalline diamond includes a plurality of diamond crystal grains, and the average particle size of the diamond crystal grains may be 10 nm or more and 50,000 nm or less. The lower limit of the average particle size of the diamond crystal grains may be 10 nm or more from a manufacturing standpoint. When the average particle size of the diamond crystal grains is 50,000 nm or less, the hardness of the polycrystalline diamond tends to be higher.
[0025] (9) In any of (1) to (8) above, the Knoop hardness of the polycrystalline diamond may be 50 GPa or higher. The Knoop hardness is measured in accordance with JIS Z 2251:2009 at a temperature of 20°C to 25°C and a test load of 0.5 N.
[0026] According to this, polycrystalline diamond can possess excellent hardness.
[0027] (10) In any of (1) to (9) above, the volume resistivity of the polycrystalline diamond may be 1 mΩ·cm or more and 1000 Ω·cm or less. The volume resistivity is measured at 20°C or more and 25°C or less in accordance with JIS C2141-1992. Here, 1 mΩ·cm is 1 × 10⁻⁶ -3 It is synonymous with Ω・cm.
[0028] If the volume resistivity between 20°C and 25°C falls within the above range, it is likely to exhibit good semiconductor properties, being neither a metal nor an insulator.
[0029] (11) In any of (1) to (10) above, the polycrystalline diamond may consist of diamond crystal grains, the first element, and unavoidable impurities. This further improves the performance of the semiconductor material made of the polycrystalline diamond.
[0030] (12) The semiconductor material of the present disclosure is a semiconductor material comprising polycrystalline diamond as described in any of (1) to (11) above. Because the graphite content is reduced in the semiconductor material, the semiconductor material can have excellent performance.
[0031] (13) The tool material of the present disclosure is a tool material made of polycrystalline diamond as described in any of (1) to (11) above. A tool equipped with this tool material can suppress electrostatic cracks.
[0032] (14) The tool of the present disclosure is a tool comprising polycrystalline diamond as described in any of (1) to (11) above. The tool can suppress electrostatic cracks. Furthermore, the tool can prevent cracks from occurring in the tool during the processing of insulators, thereby improving fracture resistance.
[0033] [Details of Embodiments of the Disclosure] Specific examples of polycrystalline diamond, semiconductor materials, tool materials, and tools of the Disclosure are described below with reference to the drawings. In the drawings of the Disclosure, the same reference numerals represent the same or corresponding parts. In addition, dimensional relationships such as length, width, thickness, and depth have been modified as appropriate for clarity and simplification of the drawings and do not necessarily represent actual dimensional relationships.
[0034] In this disclosure, the notation "A to B" means A or greater and B or less. If no unit is specified for A, and only a unit is specified for B, then the unit for A and the unit for B are the same.
[0035] In this disclosure, if one or more numerical values are listed as the lower and upper limits of a numerical range, any combination of any one numerical value listed as the lower limit and any one numerical value listed as the upper limit shall also be disclosed.
[0036] In this disclosure, “equipment,” “includes,” “possesses,” and variations thereof are open-ended terms. Open-ended terms may or may not include additional elements in addition to the essential elements. The statement “consists of” is a closed term. However, even a configuration expressed in closed terms may include additional elements that are usually incidental or irrelevant to the subject technology.
[0037] [Embodiment 1: Polycrystalline Diamond] The polycrystalline diamond according to one embodiment of the present disclosure (hereinafter also referred to as "Embodiment 1") is a polycrystalline diamond containing at least one first element selected from the group consisting of nitrogen, phosphorus, boron, and aluminum. The atomic number content of each first element in the polycrystalline diamond is 1.0 × 10⁻¹⁶ 16 / cm 3 The above 1.0 x 10 22 / cm 3 The following is the full width at half maximum (FMAX) x 1 cm in the first-order Raman scattering spectrum of polycrystalline diamond. -1 And, the full width at half maximum (FMAX) x 2 cm of the maximum peak in the first-order Raman scattering spectrum of synthetic type IIa single crystal diamond with a nitrogen content of 1 ppm or less based on the number of atoms. -1 This shows the relationship shown in equation I below: X1 - X2 ≥ 0.1 Equation I In the first-order Raman scattering spectrum of polycrystalline diamond, Raman shift of 1340 cm⁻¹ -1 1380cm or more -1 The following first range, and Raman shift 1560 cm -1 More than 1600cm -1 No peaks are present in the second range below. The primary Raman scattering spectra of polycrystalline diamond and synthetic type IIa single-crystal diamond are measured using a 532 nm wavelength laser as the excitation light at temperatures between 20°C and 25°C.
[0038] <Structure and Composition> The polycrystalline diamond of Embodiment 1 is a polycrystalline material composed of multiple diamond crystal grains. That is, the polycrystalline diamond has diamond crystal grains as its basic composition and does not contain a metallic bonding phase (binder). The polycrystalline diamond possesses extremely high hardness and strength. Furthermore, even under high-temperature conditions, the polycrystalline diamond does not experience deterioration of mechanical properties or grain shedding due to differences in thermal expansion coefficients with the binder or catalytic action of the binder.
[0039] The polycrystalline diamond of Embodiment 1 is a polycrystalline body composed of multiple diamond crystal grains. Therefore, the polycrystalline diamond does not have the directionality (anisotropy) and cleavage of a single crystal, and has isotropic hardness and wear resistance in all directions.
[0040] The polycrystalline diamond of Embodiment 1 contains at least one first element selected from the group consisting of nitrogen, phosphorus, boron, and aluminum. The first element may consist of one or both of nitrogen and boron.
[0041] The atomic-based content of each of the first elements in the polycrystalline diamond of Embodiment 1 is 1.0 × 10⁻¹⁶. 16 / cm 3 The above 1.0 x 10 22 / cm 3 The following is true: The atomic count of each of the first elements in polycrystalline diamond is 1.0 × 10⁻¹⁶. 17 / cm 3 The above 1.0 x 10 21 / cm 3 The following is also acceptable: 1.0 × 10 19 / cm 3 The above 8.0 x 10 20 / cm 3 The following is also acceptable, or 1.0 × 10 20 / cm 3 The above 6.0 x 10 20 / cm 3 The following is also acceptable. Here, the content of each primary element in polycrystalline diamond, based on the number of atoms, means the content of that primary element based on the number of atoms if the polycrystalline diamond contains one primary element, and the content of each primary element based on the number of atoms if the polycrystalline diamond contains two or more primary elements.
[0042] If the polycrystalline diamond of Embodiment 1 contains two or more primary elements, the total content of all primary elements contained in the polycrystalline diamond, based on the number of atoms, is 1.0 × 10⁻¹⁶. 17 / cm 3 The above 1.0 x 10 21 / cm 3 The following is also acceptable: 1.0 × 10 19 / cm 3 The above 8.0 x 1020 / cm 3 The following is also acceptable, or 1.0 × 10 20 / cm 3 The above 6.0 x 10 20 / cm 3 The following is also acceptable.
[0043] The polycrystalline diamond of Embodiment 1 may contain unavoidable impurities, as long as the effects of the present disclosure are not impaired. Examples of unavoidable impurities include hydrogen, oxygen, nitrogen, alkali metal elements (lithium (Li), sodium (Na), potassium (K), etc.) and alkaline earth metal elements (calcium (Ca), magnesium (Mg), etc.). In the polycrystalline diamond of Embodiment 1, the content of each element that is an unavoidable impurity may be 0% by mass or more and 0.01% by mass or less. In the polycrystalline diamond of Embodiment 1, the total content of unavoidable impurities may be 0.05% by mass or less.
[0044] The atomic number content of each primary element in polycrystalline diamond, as well as the content of unavoidable impurities in polycrystalline diamond, are measured by secondary ion mass spectrometry (SIMS). The SIMS conditions are, for example, using a "CAMECA IMS-7f" instrument (manufactured by AMETEK), and the primary ion species Cs + The primary acceleration voltage is 16.0 kV, and the detection area is φ30 μm.
[0045] In the polycrystalline diamond of Embodiment 1, at least a portion of the first element is doped within the crystalline structure composed of carbon. The polycrystalline diamond of Embodiment 1 may contain carbon and the first element doped within the crystalline structure composed of carbon. The polycrystalline diamond of Embodiment 1 may contain carbon, the first element doped within the crystalline structure composed of carbon, and unavoidable impurities. The polycrystalline diamond of Embodiment 1 may consist of carbon, the first element doped within the crystalline structure composed of carbon, and unavoidable impurities.
[0046] In this disclosure, "first element doped into the crystal structure" means a state in which the first element exists in a state in which it is substituted for some of the carbon in the crystal structure of diamond, which is composed of carbon atoms bonded together by covalent bonds, and is dispersed within the crystal structure.
[0047] The first element is at least one selected from the group consisting of nitrogen, phosphorus, boron, and aluminum. The carbon that makes up polycrystalline diamond is a group 14 element of the periodic table. Nitrogen and phosphorus are group 15 elements of the periodic table. Boron and aluminum are group 14 elements of the periodic table. Group 13 elements (boron and aluminum) with a similar number of valence electrons to carbon act as acceptor atoms in polycrystalline diamond and contribute to the formation of p-type semiconductors. Group 15 elements (nitrogen and phosphorus) with a similar number of valence electrons to carbon act as donor atoms in polycrystalline diamond and contribute to the formation of n-type semiconductors.
[0048] The polycrystalline diamond of Embodiment 1 may be in a form that includes first elements clustered within the crystal structure, as long as the effects of the present disclosure are not impaired.
[0049] "Clustered primary elements within the crystal structure" refers to a state in which multiple atoms of the primary element exist within the crystal structure in an aggregated form. When polycrystalline diamond contains clustered primary elements within the diamond crystal structure, the primary elements are unevenly distributed within the crystal structure, which reduces the homogeneity of the polycrystalline diamond and may degrade the performance of the semiconductor material made from the polycrystalline diamond. Furthermore, it can cause significant distortion in the crystal structure, potentially reducing the hardness of the polycrystalline diamond. Therefore, the less the amount of clustered primary elements within the crystal structure of the polycrystalline diamond, the better the performance of the semiconductor material made from the polycrystalline diamond. The polycrystalline diamond of Embodiment 1 does not necessarily have to contain clustered primary elements.
[0050] In the X-ray diffraction pattern of the polycrystalline diamond of Embodiment 1, the ratio of the peak intensity derived from other crystal structures to the peak intensity derived from the carbon crystal structure may be 0.0001 or less. In this case, the proportion of other crystalline phases other than diamond in the polycrystalline diamond, such as the crystalline phase of the first element, is sufficiently reduced, resulting in good performance of the semiconductor material made of the polycrystalline diamond.
[0051] In polycrystalline diamond, whether or not the first element is doped into the crystal structure can be confirmed, for example, by (1) observing whether or not a crystalline phase of the first element exists in the polycrystalline diamond, by (2) measuring the distribution of the first element's content on an atomic number basis in the polycrystalline diamond, or by appropriately combining (1) and (2) above.
[0052] Regarding (1) above, the first element doped within the crystal structure does not constitute a crystalline phase different from that of diamond. Therefore, if all of the first element in polycrystalline diamond is doped within the crystal structure, the crystalline phase of the first element will not be observed in the polycrystalline diamond. In contrast, clustered first elements constitute a crystalline phase different from that of diamond. Therefore, if polycrystalline diamond contains clustered first elements, the crystalline phase of the first element will be observed in the polycrystalline diamond. The presence or absence of the crystalline phase of the first element can be observed, for example, by X-ray diffraction. Depending on the size of the crystalline phase of the first element, it may also be observed visually.
[0053] Regarding (2) above, when the first element is dispersed within the crystal structure, the distribution of its content on an atomic number basis is more uniform compared to when it exists in a clustered state. The distribution of the first element's content on an atomic number basis can be measured, for example, by secondary ion mass spectrometry (SIMS). The distribution of the first element's content on an atomic number basis can be considered uniform when the difference in the content of the first element on an atomic number basis measured at any two points in the crystal structure is less than or equal to a predetermined value. In other words, the first element can be considered to be dispersed within the crystal structure and not in a clustered state.
[0054] The polycrystalline diamond of Embodiment 1 may consist of diamond crystal grains, a first element, and unavoidable impurities. The content of diamond crystal grains in the polycrystalline diamond of Embodiment 1 may be 98% by volume or more and 100% by volume or less.
[0055] The diamond grain content (volume %) in polycrystalline diamond can be measured by combining a method using an energy-dispersive X-ray analyzer (EDX) attached to a scanning electron microscope (SEM) (e.g., JEOL's "JSM-7800F" (product name)) (e.g., Oxford's X-MAX80 EDS system) (hereinafter also referred to as "SEM-EDX") and X-ray diffraction. The specific measurement method is as follows.
[0056] First, a sample containing the cross-section of the polycrystalline diamond is prepared by cutting the diamond at an arbitrary position. A focused ion beam apparatus, a cross-section polisher, etc., can be used to prepare the cross-section. Next, the cross-section is observed using a scanning electron microscope (SEM) to obtain a backscattered electron image. In the backscattered electron image, the regions containing diamond crystal grains and non-diamond-like carbon appear as black regions, while other regions (e.g., elements derived from the binder) appear as gray or white regions. The magnification when observing the cross-section with the SEM is adjusted appropriately so that the number of diamond crystal grains observed in the measurement field of view is 100 or more. For example, the magnification when observing the cross-section with the SEM may be 10,000x.
[0057] Next, the backscattered electron image is subjected to binarization using image analysis software (such as "Win ROOF ver. 7.4.5" or "WinROOF2018" from Mitani Corporation). The image analysis software automatically sets an appropriate binarization threshold based on the image information (the measurer does not arbitrarily set the threshold). The inventors have also confirmed that there is no significant change in the measurement results even when the brightness of the image is varied. From the image after binarization, the area ratio of pixels originating from the dark field (pixels originating from diamond crystal grains and non-diamond-like carbon) to the area of the measurement field of view is calculated. By considering the calculated area ratio as a volume percentage, the sum (volume percentage) of the content of diamond crystal grains and the content of non-diamond-like carbon can be determined.
[0058] By calculating the area ratio of pixels originating from the brightfield (pixels originating from other regions) to the area of the measurement field of view from the binarized image, the content (volume %) of other regions can be determined.
[0059] As long as the sum (by volume) of the diamond grain content and the non-diamond-like carbon content in polycrystalline diamond is measured in the same sample, it has been confirmed that there is almost no variation in the measurement results even when the measurement field is changed and calculations are performed multiple times.
[0060] Furthermore, the fact that pixels originating from dark-field imaging are derived from diamond crystal grains and non-diamond-like carbon can be confirmed by performing elemental analysis on polycrystalline diamond using SEM-EDX.
[0061] Next, an X-ray diffractometer (Rigaku's "MiniFlex 600" (product name)) is used to obtain the X-ray spectrum of the above cross-section of polycrystalline diamond. The conditions for the X-ray diffractometer at this time are as follows: Characteristic X-ray: Cu-Kα (wavelength 1.54 Å) Tube voltage: 45 kV Tube current: 40 mA Filter: Multilayer mirror Optical system: Focusing method X-ray diffraction method: θ-2θ method.
[0062] In the obtained X-ray spectrum, the following peak intensities A and B are measured.
[0063] Peak intensity A: Peak intensity of non-diamond-like carbon, obtained by removing background noise from peak intensity at diffraction angle 2θ = 27.5° to 29.5°. Peak intensity B: Peak intensity of diamond crystal grains, obtained by removing background noise from peak intensity at diffraction angle 2θ = 43.8° to 44.0°.
[0064] The diamond grain content (volume %) is obtained by calculating the value of {peak intensity B / (peak intensity A + peak intensity B)} × {the sum of the diamond grain content and non-diamond-like carbon content obtained in the above-mentioned SEM-EDX (volume %)}. Since non-diamond-like carbon and diamond grains all have roughly the same electronic weight, the above X-ray peak intensity ratio can be considered as the volume ratio in polycrystalline diamond.
[0065] <Primary Raman Scattering Spectrum> <X1-X2> Full width at half maximum (FMAX) of the maximum peak in the primary Raman scattering spectrum of polycrystalline diamond of Embodiment 1 (X1 cm) -1 And, the full width at half maximum (FMAX) x 2 cm of the maximum peak in the first-order Raman scattering spectrum of synthetic type IIa single crystal diamond with a nitrogen content of 1 ppm or less based on the number of atoms. -1 This shows the relationship shown in equation I below: X1 - X2 ≥ 0.1 Equation I
[0066] The synthetic type IIa single-crystal diamond used as a standard sample refers to a high-purity single-crystal diamond free from lattice defects and internal strain, synthesized by the temperature difference method under high temperature and pressure. In synthetic type IIa single-crystal diamond, the concentration of nitrogen atoms, based on the number of atoms, is between 0 ppm and 1 ppm. Furthermore, in synthetic type IIa single-crystal diamond, the concentrations of phosphorus, boron, aluminum, and other non-carbon atoms, based on the number of atoms, are also between 0 ppm and 1 ppm. In other words, synthetic type IIa single-crystal diamond contains almost no atoms other than carbon. For example, high-purity type IIa single-crystal diamond manufactured by Sumitomo Electric Industries, Ltd. may be used as the synthetic type IIa single-crystal diamond.
[0067] Figure 1 shows the first-order Raman scattering spectrum (hereinafter also referred to as "Raman spectrum") of synthetic type IIa single-crystal diamond. In the Raman spectrum of Figure 1, the X-axis represents the Raman shift (cm). -1 The vertical axis shows the intensity normalized with the maximum peak intensity set to 1. As shown in Figure 1, the primary Raman scattering spectrum of synthetic type IIa single crystal diamond has a Raman shift of 1332 cm⁻¹. -1 1333cm or more -1 A sharp, strong diamond phonon peak is present below. The corresponding Raman shift is 1332 cm⁻¹. -1 1333cm or more -1 The peaks shown below correspond to the maximum peaks in the first-order Raman scattering spectra of synthetic type IIa single-crystal diamond. The full width at half maximum (FWHM) x 2 of these maximum peaks is typically 2 cm. -1 5cm or more -1 The following applies: A smaller total width at half maximum indicates higher crystallinity of the diamond.
[0068] When a diamond contains the first element, the full width at half maximum of the maximum peak in the primary Raman scattering spectrum of the diamond is equal to the full width at half maximum of the maximum peak in the primary Raman scattering spectrum of synthetic type IIa single crystal diamond x 2 (cm). -1 ) becomes larger. The greater the amount of boron (first element) contained in polycrystalline diamond, the larger the full width at half maximum of the maximum peak in the Raman spectrum (see Fig. 9 in P. W. May, W. J. Ludlow, M. Hannaway, P. J. Heard, J. A. Smith and K. N. Rosser, Diamond and Related Materials 2008 Vol. 17 Issue 2 Pages 105-117). Therefore, the greater the amount of first element contained in polycrystalline diamond, the larger the value of X1 - X2 in the above equation I.
[0069] Furthermore, in polycrystalline diamond, the smaller the crystal grains, the greater the total width at half maximum of the maximum peak in the primary Raman scattering spectrum of the polycrystalline diamond, which is equal to the total width at half maximum of the maximum peak in the primary Raman scattering spectrum of the synthetic type IIa single crystal diamond multiplied by 2 cm.-1 It becomes larger. Therefore, the smaller the crystal grains of polycrystalline diamond, the larger the value of X1 - X2 in the above equation I.
[0070] Full width at half maximum (FMAX) x 1 cm in the first-order Raman scattering spectrum of polycrystalline diamond. -1 And, the full width at half maximum (FMAX) x 2 cm of the maximum peak in the first-order Raman scattering spectrum of synthetic type IIa single-crystal diamond. -1 The fact that and exhibit the relationship in equation I above indicates that polycrystalline diamond contains the first element. Furthermore, it also suggests that the crystal grains of polycrystalline diamond are small.
[0071] The maximum peak in the primary Raman scattering spectrum of the polycrystalline diamond of Embodiment 1 is at a Raman shift of 1322 cm⁻¹. -1 1332cm or more -1 It exists within the following range.
[0072] The relationship between X1 and X2 may be expressed by the following equations IA or IB: 20 ≥ X1 - X2 ≥ 0.1 (Equation IA) 15 ≥ X1 - X2 ≥ 3 (Equation IB)
[0073] The above X1 is 2.1 cm -1 25cm or more -1 The following is also acceptable, or 5 cm -1 20cm or more -1 The following is also acceptable.
[0074] In this disclosure, the full width at half maximum X1 (cm²) of the maximum peak in the first-order Raman scattering spectrum of polycrystalline diamond is defined as follows: -1 The Raman rays are measured using the following procedure. First, the surface of the polycrystalline diamond sample is polished with a diamond grinding wheel until the surface roughness Ra is 20 nm or less. The sample is preferably square or nearly octagonal in shape. The polished surface is irradiated with a laser under the following conditions and the scattered Raman rays are detected.
[0075] <Measurement Conditions> Measurement device: LabRAM HR-800 (manufactured by HORIBA JOBIN YVON) Laser wavelength: 532 nm Measurement temperature: Room temperature (20°C to 25°C) Wavenumber resolution: 1 cm -1Measurements are performed under the following conditions. The wavenumber resolution of the instrument is evaluated by the full width at half maximum of the peak of the Rayleigh scattered light. A commercially available instrument from the instrument manufacturer can be used. Examples of instrument manufacturers include HORIBA, RENISHAW, BRUKER, HITACHI, and OXFORD. Laser irradiation position (measurement area): The first-order Raman scattering spectrum (hereinafter also referred to as "Raman lines") of polycrystalline diamond is detected at the following five locations (i) to (v). (i) A Raman line is detected at the center of the polished surface of the measurement sample (the centroid position in the two-dimensional plane). (ii) A straight line is drawn from the center to the edge of the polished surface, and the position P where the length of the straight line is maximum is identified. If the distance from the center to P is D1, a Raman line is detected on the line segment from the center to P at a position where the distance from the center is (3 / 4)D1. (iii) Draw a straight line from the central part in the opposite direction to P, and identify the intersection point Q between this line and the edge of the polished surface. That is, P, the central part, and Q lie on the same straight line L1. If the distance from the central part to Q is D2, detect the Raman line on the line segment from the central part to Q at a distance of (3 / 4)D2 from the central part. (iv) Draw a straight line L2 that passes through the central part and is perpendicular to the straight line L1 that passes through P, the central part, and Q, and identify the intersection points R and S between this straight line L2 and the edge of the polished surface. If the distance from the central part to R is D3, detect the Raman line on the line segment from the central part to R at a distance of (3 / 4)D3 from the central part. (v) If the distance from the central part to S is D4, detect the Raman line on the line segment from the central part to S at a distance of (3 / 4)D4 from the central part.
[0076] Spectral analysis is performed on the Raman rays detected at each of the five locations mentioned above to identify the diamond phonon peak. A Lorentz function is fitted to the diamond phonon peak using the least squares method to determine the full width at half maximum (FMAX) of the peak at each of the five locations. The average of the FMAX of the five peaks is calculated. In this disclosure, this average value is the FMAX X1 (cm) of the largest peak in the first-order Raman scattering spectrum of polycrystalline diamond. -1 This falls under the category of ).
[0077] In the present disclosure, the full width at half maximum X2 cm of the maximum peak in the primary Raman scattering spectrum of synthetic type IIa single-crystal diamond having a nitrogen content of 1 ppm or less on an atomic number basis -1 is the full width at half maximum X1 cm of the maximum peak in the primary Raman scattering spectrum of the aforementioned polycrystalline diamond -1 measured by the same method.
[0078] For the same diamond, crystallinity such as strain of the sample can be uniquely evaluated and compared between samples by the aforementioned setting of five measurement regions and the average calculation method.
[0079] <<First Range and Second Range>> In the primary Raman scattering spectrum of the polycrystalline diamond according to Embodiment 1, the Raman shift is 1340 cm -1 to 1380 cm -1 in the first range, and the Raman shift is 1560 cm -1 to 1600 cm -1 in the second range, no peaks are present.
[0080] In the primary Raman scattering spectrum of diamond, the peak present in the first range where the Raman shift is 1340 cm -1 to 1380 cm -1 is a peak derived from the D band of graphite. In the primary Raman scattering spectrum of diamond, the peak present in the second range where the Raman shift is 1560 cm -1 to 1600 cm -1 is a peak derived from the G band of graphite. In the primary Raman scattering spectrum of the polycrystalline diamond according to Embodiment 1, no peaks are present in the first range and the second range, which suggests that the polycrystalline diamond according to Embodiment 1 does not contain graphite. That is, in the polycrystalline diamond according to Embodiment 1, the graphite content is reduced.
[0081] In the present disclosure, the method for confirming whether peaks are present in the first range and the second range in the primary Raman scattering spectrum of polycrystalline diamond is as follows. The aforementioned full width at half maximum X1 (cm -1Using the same method as the measurement method described above, the primary Raman scattering spectrum (hereinafter also referred to as "Raman lines") of polycrystalline diamond is detected at five locations. Spectral analysis is performed on the Raman lines detected at each of the five locations to confirm whether peaks exist in the first and second ranges. The Raman spectral analysis is performed according to the following procedure.
[0082] (1) First, remove cosmic ray noise. If this cannot be done using the software recommended by each instrument manufacturer, reacquire data that does not contain cosmic ray noise. (2) Baseline correction may be applied if clear noise is identified. (3) Use the Lorentz function as a model and perform peak fitting using the nonlinear least squares method. Unless there is a special reason, the fitting range should preferably include 80% or more of the wavenumber range from which the spectrum was acquired, and if multiple peaks exist, it is desirable to set the model function as the sum of the multiple peaks. (4) If the fitting does not converge, it is almost always the case that no peaks have been detected. However, if clearly different initial values are arbitrarily input even though no peaks exist, results that differ from general knowledge may be obtained. For example, if a value equivalent to or less than the full width at half maximum of the single crystal diamond mentioned above, or more than 10 times that value, it means that the peak intensity is about the same as the ambient noise.
[0083] In this disclosure, if there are no peaks in the first and second ranges for all five Raman lines, it is determined that there are no peaks in the first and second ranges in the primary Raman scattering spectrum of polycrystalline diamond.
[0084] ≪λ1-λ2≫ Raman shift λ1 cm of the maximum peak in the primary Raman scattering spectrum of polycrystalline diamond of Embodiment 1 -1 And the Raman shift λ2cm of the maximum peak in the first-order Raman scattering spectrum of synthetic type IIa single-crystal diamond. -1 This can also be expressed by showing the relationship in Equation II below: λ1 - λ2 < 0 Equation II
[0085] From the viewpoint of improving the carrier mobility of semiconductor materials made of polycrystalline diamond, the relationship between λ1 and λ2 may be given by the following equation IIA or equation IIB: λ1 - λ2 ≤ -0.1 Equation IIA λ1 - λ2 ≤ -0.2 Equation IIB
[0086] The lower limit of λ1-λ2 is not particularly restricted, but it may be greater than or equal to -10, or greater than or equal to -5. λ1-λ2 may satisfy one of the following relationships: -∞ ≤ λ1-λ2 < 0, -10 ≤ λ1-λ2 ≤ -0.1, or -5 ≤ λ1-λ2 ≤ -0.2
[0087] If the polycrystalline diamond of Embodiment 1 exhibits the relationship λ1 - λ2 < 0, then λ1 is 1322 cm². -1 Total length: 1332.9 cm -1 The following is also acceptable: 1322cm -1 1332cm or more -1 The following is also acceptable, or 1326 cm -1 1332cm or more -1 The following is also acceptable.
[0088] If the polycrystalline diamond of Embodiment 1 exhibits the relationship λ1 - λ2 < 0, then λ2 is 1332 cm². -1 1333cm or more -1 The following is also acceptable.
[0089] Raman shift λ 1 cm of the maximum peak in the first-order Raman scattering spectrum of polycrystalline diamond of Embodiment 1 -1 The Raman shift λ2cm of the maximum peak in the first-order Raman scattering spectrum of the synthetic type IIa single-crystal diamond. -1 This can also be expressed by showing the relationship in Equation III below: λ1 - λ2 ≥ 0 Equation III
[0090] From the viewpoint of improving the fatigue strength of polycrystalline diamond, the relationship between λ1 and λ2 may be given by the following equation IIIA or equation IIIB: λ1 - λ2 ≥ 0.1 (Equation IIIA) λ1 - λ2 ≥ 0.2 (Equation IIIB)
[0091] The upper limit of λ1 - λ2 is not particularly restricted, but it may be, for example, 10 or less, or 5 or less. λ1 - λ2 may express one of the following relationships: ∞ ≥ λ1 - λ2 ≥ 0, 10 ≥ λ1 - λ2 ≥ 0.1, 5 ≥ λ1 - λ2 ≥ 0.2
[0092] If the polycrystalline diamond of Embodiment 1 exhibits the relationship λ1 - λ2 ≥ 0, then λ1 is 1332 cm². -1 1340cm or more -1 The following is also acceptable, or 1332 cm -1 1335cm -1 The following is also acceptable.
[0093] If the polycrystalline diamond of Embodiment 1 exhibits the relationship λ1 - λ2 ≥ 0, then λ2 is 1330 cm². -1 1335cm -1 The following is also acceptable: 1331 cm -1 1334cm or more -1 The following is also acceptable, or 1332 cm -1 1333cm or more -1 The following is also acceptable.
[0094] In this disclosure, the Raman shift λ1 (cm) of the maximum peak in the first-order Raman scattering spectrum of polycrystalline diamond is defined as follows: -1 ), and the Raman shift λ² (cm) of the maximum peak in the first-order Raman scattering spectrum of synthetic type IIa single-crystal diamond. -1 The measurement method is as follows: The above half-width x 1 (cm -1 Using the same method as the measurement method described above, the primary Raman scattering spectrum (hereinafter also referred to as "Raman lines") of polycrystalline diamond is detected at five locations. Spectral analysis is performed on the Raman lines detected at each of the five locations, and the Raman shift of the maximum peak is measured for each Raman line. The average of the Raman shifts at the five locations is calculated. In this disclosure, the average value is the Raman shift λ1 (cm) of the maximum peak in the primary Raman scattering spectrum of polycrystalline diamond. -1 This falls under the category of ).
[0095] In this disclosure, the Raman shift λ² (cm²) of the maximum peak in the primary Raman scattering spectrum of synthetic type IIa single crystal diamond having a nitrogen content of 1 ppm or less on an atomic basis is defined. -1 ) is the Raman shift λ1 (cm) of the maximum peak in the first-order Raman scattering spectrum of the above polycrystalline diamond. -1 It is measured using the same method as ).
[0096] <Average grain size of diamond crystal grains> The polycrystalline diamond of Embodiment 1 contains a plurality of diamond crystal grains. The average grain size of the diamond crystal grains may be 10 nm to 50,000 nm, 50 nm to 1,000 nm, 50 nm to 500 nm, or 50 nm to 200 nm.
[0097] The average grain size of diamond crystals in polycrystalline diamond can be determined by a scanning electron microscope (SEM) sectioning method. Specifically, the polycrystalline diamond is first observed using a scanning electron microscope at a magnification of 1,000 to 100,000 times to obtain an SEM image.
[0098] Next, draw a circle on the SEM image, and draw eight straight lines radially from the center of the circle (so that the intersection angles between each line are approximately equal) to the outer circumference of the circle. In this case, it is preferable to set the observation magnification and the diameter of the circle so that the number of diamond crystal grains that lie on each of the straight lines is approximately 10 to 50.
[0099] Next, for each of the above lines, count the number of times the line crosses the grain boundaries of the diamond crystal grains, and calculate the average intercept length by dividing the length of the line by the number of crossings. Multiply this average intercept length by 1.128 to obtain the value obtained as the first average grain size. Calculate the average of the first average grain sizes for the eight lines (the second average grain size). Calculate the second average grain size for each of the five SEM images using the above procedure, and calculate the average of these second average grain sizes. This average value is the average grain size of the diamond crystal grains in the polycrystalline diamond.
[0100] Furthermore, it has been confirmed that, as long as the average grain size of diamond crystals is measured in the same sample, there is almost no variation in the measurement results even when the selection of the measurement field of view is changed and calculations are performed multiple times.
[0101] <Knoop Hardness> The Knoop hardness of the polycrystalline diamond of Embodiment 1 may be 50 GPa or higher. The Knoop hardness of the polycrystalline diamond may be 50 GPa or higher and 120 GPa or lower, 60 GPa or higher and 100 GPa or lower, or 60 GPa or higher and 90 GPa or lower.
[0102] Knoop hardness shall be measured using a method compliant with "JIS Z 2251:2009 Knoop hardness test - Measurement method". A general microhardness tester can be used to measure Knoop hardness. The measurement environment may be room temperature (for example, around 23°C ± 5°C). A Knoop-type indenter (an indenter with a rhombic pyramidal shape) shall be used. The material of the indenter shall be single-crystal diamond. The test force (load) shall be 4.9 N (0.5 kgf). The holding time of the test force shall be 10 seconds. The approach speed of the indenter shall be 60 μm / s.
[0103] The Knoop hardness is measured at five locations on the polycrystalline diamond to be measured. The average value of the three measurements obtained by excluding the minimum and maximum values from the five measurements is calculated. In this disclosure, this average value corresponds to the Knoop hardness of the polycrystalline diamond.
[0104] <Volume Resistivity> The volume resistivity of the polycrystalline diamond of Embodiment 1 may be 1 mΩ·cm or more and 1000 Ω·cm or less, 10 mΩ·cm or more and 1000 Ω·cm or less, 20 mΩ·cm or more and 100 Ω·cm or less, or 100 mΩ·cm or more and 10 Ω·cm or less.
[0105] In this disclosure, the volume resistivity of polycrystalline diamond is measured at a temperature of 20°C to 25°C in accordance with JIS C2141-1992.
[0106] <Method for Manufacturing Polycrystalline Diamond> The polycrystalline diamond of Embodiment 1 can be manufactured, for example, by the following method. The manufacturing method described below will be explained step by step with reference to Figures 2 and 3.
[0107] <<Preparation Process>> This process is for preparing graphite. As shown in Figure 2, in the preparation process, graphite 1 containing carbon and a first element doped into the crystalline structure composed of carbon is prepared on a substrate 2. The prepared graphite 1 is converted into polycrystalline diamond by a conversion process described later. The grain size of the single crystals in graphite 1 and the content of the first element on an atomic number basis in graphite 1 are related to polycrystalline diamond. The grain size of the single crystals constituting graphite 1 may be 100 μm or less. The content of each of the first elements on an atomic number basis in graphite 1 is 1 × 10 16 / cm 3 The above 1 x 10 22 / cm 3 The following applies. Graphite 1 that satisfies the above single crystal grain size and the content of each of the first elements based on the number of atoms can be formed on a substrate 2, for example, by the following chemical vapor deposition (CVD) method.
[0108] ≪CVD Method≫ A substrate 2 for vapor-phase growth of graphite is placed in a vacuum chamber on its main surface. Any metal, inorganic ceramic material, or carbon material can be used as the material for the substrate 2, as long as it can withstand temperatures of approximately 1500°C to 3000°C. However, from the viewpoint of reducing impurities mixed into the graphite that will become the raw material for polycrystalline diamond, at least the main surface of the substrate may be made of carbon material, or it may be diamond or graphite with very few impurities.
[0109] Next, the substrate 2 placed in the vacuum chamber is heated to a temperature of approximately 1500°C to 3000°C. Known heating methods can be employed, for example, by installing a heater capable of directly or indirectly heating the substrate 2 in the vacuum chamber.
[0110] Next, a hydrocarbon gas and a gas containing the first element (hereinafter also referred to as "first element-containing gas") are introduced into the vacuum chamber. At this time, the vacuum level (pressure) inside the vacuum chamber is set to below atmospheric pressure. This allows the hydrocarbon gas and the gas containing the first element to be uniformly mixed inside the vacuum chamber.
[0111] As hydrocarbon gases, ethane, butane, methane, etc., can be used. Furthermore, as gases containing the first element, gases consisting of hydrides of the first element, hydrocarbon gases containing the first element, and halogenated gases containing the first element may be used. When using gases consisting of hydrides of the first element, the gas can be easily decomposed at high temperatures, allowing for efficient supply of the first element onto the substrate. When using hydrocarbon gases containing the first element, the first element, already bonded to carbon, can be supplied onto the substrate, allowing for more efficient doping of the first element into graphite. When using halogenated gases containing the first element, graphite can be synthesized while removing unintended metal impurities through the action of halogens, thus more effectively reducing the concentration of metal impurities in the graphite. For example, when doping with boron (B) as the first element, boron fluoride (BF) can be used. 3 ) gas can be used. When doping with nitrogen (N) as the first element, ammonia (NH 3 ) gas can be used. When doping with phosphorus (P) as the first element, phosphine (PH) can be used. 3 ) gas can be used. When doping with aluminum (Al) as the first element, trimethylaluminum ((CH) can be used. 3 ) 3 Al gas can be used.
[0112] Then, by thermally decomposing the mixed gas at a temperature of 1500°C or higher, graphite containing carbon and primary elements doped within a crystalline structure composed of carbon is formed on the main surface of the substrate. Within the graphite, the primary elements are dispersed within the crystalline structure.
[0113] In the above CVD method, the temperature and pressure in the synthesis conditions may be set to 1600°C or higher and 13 Torr or higher, respectively, in order to reduce the grain size of the single crystals contained in graphite 1 to 100 μm or less. By reducing the grain size of the single crystals contained in graphite 1 to 100 μm or less, the grain size of the diamond crystals in polycrystalline diamond produced by direct conversion can be suppressed to 50,000 nm or less. Furthermore, by adjusting the grain size of the single crystals contained in graphite 1 to 100 μm, the grain size of the diamond crystals in polycrystalline diamond can be reduced to 10 nm or higher and 50,000 nm or less. Note that the composition of graphite 1 may include a portion of single crystals, with the rest being in the state of amorphous, amorphous carbon, carbon nanotubes, fullerenes, etc., or it may be a polycrystalline material composed of single crystals. To obtain polycrystalline diamond with more uniform grain size, it is preferable to form graphite 1 in which each graphite phase is formed by a single phase. Here, grain size refers to the average grain size as described above.
[0114] In the above CVD method, the content of each element in graphite 1 based on the number of atoms is 1.0 × 10 16 / cm 3 The above 1.0 x 10 22 / cm 3 To achieve the following, the mixing ratio of hydrocarbon gases and gases containing the first element is adjusted. Specifically, by increasing the mixing ratio of gases containing the first element to hydrocarbon gases, the atomic number-based content of the first element in graphite 1 can be increased. Furthermore, the atomic number-based content of the first element can also be adjusted by changing the type of gases containing the first element. The atomic number-based content of each of the first elements in graphite 1 is 1.0 × 10⁻¹⁰. 16 / cm 3 The above 1.0 x 10 22 / cm 3 By doing the following, the atomic number basis content of the first element in polycrystalline diamond is 1.0 × 10 16 / cm 3 The above 1.0 x 10 22 / cm 3 The following can be done:
[0115] In this process, by using the above CVD method, graphite 1 containing carbon and a first element doped into a crystalline structure composed of carbon is obtained on the substrate 2, wherein the content of the first element on an atomic basis is 1.0 × 10 16 / cm 3 The above 1.0 x 10 22 / cm 3 The following graphite 1 is formed. In other words, the first element is 1.0 × 10 16 / cm 3 The above 1.0 x 10 22 / cm 3 Graphite 1, which is dispersed within the crystalline structure in the following atomic number-based content, is grown on the substrate 2 using the vapor phase.
[0116] Furthermore, with respect to the graphite prepared in this process, it is preferable that the distribution of the first element's content, based on the number of atoms, is uniform in both the thickness direction and the in-plane direction. By uniformly doping the first element into the graphite, the distribution of the first element in the polycrystalline diamond produced by the conversion process described later can be made uniform.
[0117] To ensure a uniform distribution of the first element's content based on atomic number, it is preferable to simultaneously introduce the hydrocarbon gas and each gas containing the first element into the vacuum chamber. This allows for easy and uniform mixing of the gases, enabling the efficient formation of uniformly doped graphite on the substrate. The gases may be supplied from directly above the main surface of the substrate toward the main surface, or from an oblique or horizontal direction toward the main surface of the substrate. From the viewpoint of more efficient and uniform doping of the first element, it is preferable to supply the gases from directly above the main surface of the substrate toward the main surface of the substrate. Furthermore, to further efficiently and uniformly dope the first element, guide members may be provided in the vacuum chamber to guide the hydrocarbon gas and the gas containing the first element onto the main surface of the substrate.
[0118] Furthermore, the density of the graphite prepared in this process is 0.8 g / cm³. 3 2.2g / cm or more 3 The following is also acceptable, or 1.4 g / cm³. 3 2.1g / cm or more3 The following is also acceptable: Graphite density of 0.8 g / cm³ 3 In the above case, the volume change when graphite is directly converted to polycrystalline diamond in the conversion process described later can be sufficiently reduced, thereby suppressing the probability of cracks occurring in the manufactured polycrystalline diamond, and also suppressing changes in the environment inside the apparatus, which in turn can improve the manufacturing yield. 3 Under the following conditions, polycrystalline diamond can be synthesized with a high yield of over 80%.
[0119] The density of graphite can be adjusted, for example, by the temperature (°C) and the introduction rate (sccm) of each gas when growing graphite on the main surface of the substrate. Specifically, the density of graphite can be increased by raising the temperature and by increasing the introduction rate of hydrocarbons.
[0120] Furthermore, it is preferable that the graphite prepared in this process has a low content of unavoidable impurities. Specifically, the content of each element that is an unavoidable impurity in graphite may be 0.01 mass% or less. This is because the content of unavoidable impurities in the graphite is carried over to the polycrystalline diamond produced. In addition, by keeping the content of unavoidable impurities low, grain growth caused by the presence of unavoidable impurities can be suppressed, so that single crystals of a more uniform size can be contained in the graphite. Note that analytical instruments used for analysis that can measure the content of unavoidable impurities in graphite, such as SIMS analysis and ICP analysis, generally have a detection limit of 0.01 mass%, so elements with a content of 0.01 mass% or less will not be detected by the above analytical instruments.
[0121] The inclusion of unavoidable impurities in graphite can be suppressed by setting a relatively high vacuum level in the vacuum chamber during the thermal decomposition of the gas. Specifically, the inventors have found that by maintaining the pressure in the vacuum chamber between 20 Torr and 200 Torr, more preferably between 20 Torr and 120 Torr, the content of each element, which is an unavoidable impurity, can be controlled to 0.01 mass% or less.
[0122] In the CVD method described above, the substrate is heated before the mixed gas is introduced into the vacuum chamber. However, the substrate may also be heated after the mixed gas is introduced, or both methods may be performed simultaneously.
[0123] ≪Graphite Surface Removal Process≫ This process involves removing the outermost layer of graphite formed in the preparation process to a thickness of 1 μm or more. The outermost layer of graphite is removed, for example, with sandpaper. The grit of the sandpaper is 400. By removing the outermost layer of graphite to a thickness of 1 μm or more and preparing the surface, and then performing high-temperature and high-pressure treatment in the next conversion process, graphite will no longer be detectable on the outermost surface of the resulting polycrystalline diamond. The reason for this is presumed to be as follows: By removing the outermost layer of graphite to a thickness of 1 μm or more, graphite of different particle sizes that grew slightly during the cooling process after the growth was completed, which was present on the outermost surface, is removed, the particle size becomes uniform in the thickness direction, the gaps on the outermost surface of the graphite are filled, and the gaps become smaller. As a result, appropriate temperature and pressure are uniformly applied to the graphite, making it easier for the graphite to be converted into diamond. There is no particular upper limit to the thickness of the graphite to be removed, but for example, it may be 10 μm. The inventors have discovered that by removing the outermost surface layer of graphite to a thickness of 1 μm or more, and then subjecting it to high-temperature and high-pressure treatment, graphite can no longer be detected on the outermost surface of the resulting polycrystalline diamond.
[0124] In conventional manufacturing methods, the above-mentioned graphite surface removal step was not performed.
[0125] <<Conversion Process>> This process involves sintering the graphite whose outermost surface has been removed in the graphite surface removal process to directly convert it into polycrystalline diamond. As a result, polycrystalline diamond 3 is produced on the substrate 2, as shown in Figure 3.
[0126] Specifically, first, the graphite 1 on the substrate 2 shown in Figure 2 is placed in a high-temperature, high-pressure apparatus. The high-temperature, high-pressure apparatus can be any apparatus that can accommodate graphite and control the internal conditions as described above. For example, a vacuum chamber used in the CVD method can be used.
[0127] Graphite 1 is exposed to high-temperature and high-pressure conditions of 1700°C to 2500°C and 15 GPa to 25 GPa. As a result, graphite 1 is instantaneously sintered and converted into polycrystalline diamond 3, as shown in Figure 3. In this case, the shape of the polycrystalline diamond 3 will inherit the shape of graphite 1, except for a slight change in volume. Alternatively, graphite 1 may be exposed to high-temperature and high-pressure conditions after the substrate 2 has been removed from it, and in this case as well, the produced polycrystalline diamond will basically inherit the shape of graphite 1.
[0128] In this process, it is preferable not to use additives such as sintering aids, catalysts, and binders. According to this process, polycrystalline diamond in which single crystals are strongly bonded can be produced without the use of additives, and by not using additives, polycrystalline diamond with higher hardness can be produced compared to when additives are used.
[0129] According to the manufacturing method described in detail above, the polycrystalline diamond of Embodiment 1 can be manufactured.
[0130] Furthermore, according to the above manufacturing method, the first element is uniformly dispersed in the graphite, which effectively suppresses localized abnormal growth of diamond crystal grains during the direct conversion from graphite to diamond. This makes it possible to make the grain size of the single crystals constituting polycrystalline diamond more uniform, and as a result, homogeneous polycrystalline diamond can be produced.
[0131] [Embodiment 2: Semiconductor Material] The semiconductor material according to one embodiment of the present disclosure (hereinafter also referred to as "Embodiment 2") is a semiconductor material made of polycrystalline diamond as described in Embodiment 1. The semiconductor material of Embodiment 2 can be applied, for example, to a transistor substrate and a heat sink.
[0132] [Embodiment 3: Tool Material] The tool material according to one embodiment of the present disclosure (hereinafter also referred to as "Embodiment 3") is a tool material made of polycrystalline diamond as described in Embodiment 1. An example of a tool to which the tool material is applied is the tool described in Embodiment 4, which will be described later.
[0133] [Embodiment 4: Tools] A tool according to one embodiment of the present disclosure (hereinafter also referred to as "Embodiment 4") is a tool comprising the polycrystalline diamond described in Embodiment 1. Each tool may be composed entirely of polycrystalline diamond, or only a part thereof (for example, the cutting edge portion in the case of a cutting tool) may be composed of polycrystalline diamond. Furthermore, a coating film may be formed on the surface of each tool. Examples of tools include cutting tools, wear-resistant tools, wire drawing tools, and grinding tools.
[0134] Examples of cutting tools include drills, end mills, replaceable cutting tips for drills, replaceable cutting tips for end mills, replaceable cutting tips for milling machines, replaceable cutting tips for turning machines, metal saws, gear cutting tools, reamers, taps, and cutting tools.
[0135] Examples of wear-resistant tools include scribers, scribing wheels, dressers, water and other fluid jet nozzles, and stitchels. Examples of wire drawing tools include dies. Examples of grinding tools include grinding wheels.
[0136] This embodiment will be described in more detail by reference to examples. However, this embodiment is not limited by these examples.
[0137] [Preparation of Polycrystalline Diamonds] Polycrystalline diamonds were prepared from each sample using the following method.
[0138] <<Preparation Process>> Graphite containing the primary element was prepared on a substrate by the CVD method. The main surface of the substrate was diamond. After placing the substrate in a vacuum chamber, the substrate was heated to between 1500°C and 3000°C, and the vacuum (pressure) inside the vacuum chamber was reduced to below atmospheric pressure. Next, methane gas and a gas containing the primary element (primary element-containing gas) were introduced into the vacuum chamber for more than one hour. The type of primary element-containing gas used for each sample is as shown in the "Primary Element-Containing Gas" column of Table 1. For example, in Sample 1 and Sample 2, methane gas and a gas containing boron (boron fluoride gas) were introduced into the vacuum chamber for more than one hour. In Sample 3, methane gas and ammonia gas were introduced into the vacuum chamber for more than one hour.
[0139] In each sample, the mixing ratio of methane gas to the primary element-containing gas was adjusted so that the atomic-based content of the primary element in the graphite matched the "content" of the "primary element" in "polycrystalline diamond" in Table 1. For example, the mixing ratio of methane gas to boron-containing gas (boron fluoride gas) in Sample 1 and Sample 2, and the mixing ratio of methane gas to ammonia gas in Sample 3, were adjusted so that the atomic-based content of the primary element (boron or nitrogen) in the graphite matched the "content" of the "primary element" in "polycrystalline diamond" in Table 1. Through the above process, graphite with a thickness of more than 100 μm was produced on the main surface of the substrate by thermal decomposition of the mixed gas at a temperature of 1500°C or higher.
[0140] ≪Graphite Surface Removal Process≫ Next, for samples where "Yes" is indicated in the "Graphite Surface Removal Process" column of Table 1, the outermost layer of graphite formed in the preparation process was removed to a thickness of 1 μm or more. The outermost layer of graphite was removed using sandpaper (grit: 400). For samples where "No" is indicated in the "Graphite Surface Removal Process" column of Table 1, the graphite surface removal process was not performed.
[0141] <<Conversion Process>> Next, the graphite on the substrate was converted into polycrystalline diamond at 1750°C and 15 GPa under ultra-high pressure using a large press capable of generating high temperature and pressure, thereby producing polycrystalline diamond for each sample.
[0142] [Evaluation] For each sample of polycrystalline diamond, the type and atomic number content of the first element, the average grain size of the diamond crystals, the Knoop hardness of the polycrystalline diamond, and the volume resistivity of the polycrystalline diamond were measured using the method described in Embodiment 1. The results are shown in Table 1.
[0143] The primary Raman scattering spectrum of synthetic type IIa single crystal diamond with a nitrogen content of 1 ppm or less (based on the number of atoms) was measured using the method and conditions described in Embodiment 1. In the primary Raman scattering spectrum of synthetic type IIa single crystal diamond, the Raman shift λ 2 cm of the maximum peak was measured. -1 1332.6 cm -1 After calibrating the measuring device and measurement conditions accordingly, the primary Raman scattering spectrum of polycrystalline diamond of each sample was measured using the method and conditions described in Embodiment 1.
[0144] In the first-order Raman scattering spectrum of synthetic type IIa single-crystal diamond, the maximum peak is measured at full width at half maximum (FMAX) x 2 cm. -1 It is 2.6 cm -1 The results were as follows: The maximum peak in the first-order Raman scattering spectrum of polycrystalline diamond for each sample was measured with a full width at half maximum (FMAX) of 1 cm. -1 and the Raman shift λ1cm of the maximum peak -1 The results are shown in Table 1. From the obtained values, X1 - X2 and λ1 - λ2 were calculated. The results are shown in Table 2.
[0145] In the first-order Raman scattering spectra of the polycrystalline diamond of each sample, the Raman shift was 1340 cm⁻¹. -1 1380cm or more -1 The following first range, and Raman shift 1560 cm -1 More than 1600cm -1 Table 2 shows the presence or absence of peaks in each of the following second ranges.
[0146]
[0147]
[0148] [Discussion] The polycrystalline diamonds of Samples 1 to 7 correspond to the examples. In the first-order Raman scattering spectra of the polycrystalline diamonds of Samples 1 to 7, the Raman shift was 1340 cm⁻¹. -1 1380cm or more -1 The following first range, and Raman shift 1560 cm -1 More than 1600cm -1 No peaks were found in the second range below. Therefore, the graphite content was reduced in the polycrystalline diamonds of samples 1 to 7.
[0149] While embodiments and examples of this disclosure have been described above, it is intended from the outset that the configurations of each of the embodiments and examples described above may be combined or modified in various ways as appropriate. The embodiments and examples disclosed herein should be considered in all respects to be illustrative and not restrictive. The scope of the present invention is indicated by the claims rather than the embodiments and examples described above, and all modifications within the scope of the claims are intended to be included in the meaning of equivalences.
[0150] 1. Graphite, 2. Substrate, 3. Polycrystalline diamond.
Claims
1. A polycrystalline diamond comprising at least one first element selected from the group consisting of nitrogen, phosphorus, boron, and aluminum, wherein the content of each of said first elements in said polycrystalline diamond on an atomic number basis is 1.0×10 16 / cm 3 or more and 1.0×10 22 / cm 3 or less, the full width at half maximum X1 cm of the maximum peak in the primary Raman scattering spectrum of said polycrystalline diamond -1 and the full width at half maximum X2 cm of the maximum peak in the primary Raman scattering spectrum of a synthetic type IIa single-crystal diamond having a nitrogen content of 1 ppm or less on an atomic number basis -1 satisfy the relationship of the following formula I: X1-X2≧0.1 Formula I, in the primary Raman scattering spectrum of the polycrystalline diamond, no peak is present in a first range where the Raman shift is 1340 cm -1 or more and 1380 cm -1 or less, and a second range where the Raman shift is 1560 cm -1 or more and 1600 cm -1 or less, and the primary Raman scattering spectrum of the polycrystalline diamond and the primary Raman scattering spectrum of the synthetic type IIa single-crystal diamond are measured at 20°C or more and 25°C or less using a laser with a wavelength of 532 nm as excitation light.
2. The Raman shift λ1 cm of the maximum peak in the first-order Raman scattering spectrum of the polycrystalline diamond. -1 The Raman shift λ2cm of the maximum peak in the first-order Raman scattering spectrum of the synthetic type IIa single crystal diamond. -1 This refers to the relationship shown in Equation II below: λ1 - λ2 < 0 Equation II The polycrystalline diamond according to claim 1.
3. The relationship between λ1 and λ2 is given by the following equation IIA: λ1 - λ2 ≤ -0.1 Equation IIA The polycrystalline diamond according to claim 1 or claim 2.
4. The relationship between λ1 and λ2 is given by the following equation IIB: λ1 - λ2 ≤ -0.2 Equation IIB The polycrystalline diamond according to any one of claims 1 to 3.
5. The Raman shift λ1 cm of the maximum peak in the first-order Raman scattering spectrum of the polycrystalline diamond. -1 The Raman shift λ2cm of the maximum peak in the first-order Raman scattering spectrum of the synthetic type IIa single crystal diamond. -1 This refers to the relationship shown in Equation III below: λ1 - λ2 ≥ 0 Equation III The polycrystalline diamond according to claim 1.
6. The relationship between λ1 and λ2 is given by the following formula IIIA: λ1 - λ2 ≥ 0.1 Formula IIIA Polycrystalline diamond according to claim 1 or claim 5.
7. The relationship between λ1 and λ2 is given by the following formula IIIB: λ1 - λ2 ≥ 0.2 Formula IIIB The polycrystalline diamond according to claim 1, claim 5, or claim 6.
8. The polycrystalline diamond according to any one of claims 1 to 7, wherein the polycrystalline diamond comprises a plurality of diamond crystal grains, and the average particle size of the diamond crystal grains is 10 nm or more and 50,000 nm or less.
9. The polycrystalline diamond according to any one of claims 1 to 8, wherein the Knoop hardness of the polycrystalline diamond is 50 GPa or higher, and the Knoop hardness is measured in accordance with JIS Z 2251:2009 at a temperature of 20°C or higher and a test load of 0.5 N.
10. The polycrystalline diamond according to any one of claims 1 to 9, wherein the volume resistivity of the polycrystalline diamond is 1 mΩ·cm or more and 1000 Ω·cm or less, and the volume resistivity is measured at 20°C or more and 25°C or less in accordance with JIS C2141-1992.
11. The polycrystalline diamond according to any one of claims 1 to 10, wherein the polycrystalline diamond comprises diamond crystal grains, the first element, and unavoidable impurities.
12. A semiconductor material comprising polycrystalline diamond according to any one of claims 1 to 11.
13. A tool material comprising polycrystalline diamond according to any one of claims 1 to 11.
14. A tool comprising polycrystalline diamond as described in any one of claims 1 to 11.