Semiconductor wafer dicing method
The combination of laser and plasma processes with a water-soluble polymer coating and selective etching addresses the inefficiencies of existing dicing methods, achieving efficient and precise wafer dicing for advanced packaging.
Patent Information
- Application Number
- PCT/KR2026/095119
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-03-17
- Publication Date
- 2026-11-12
AI Technical Summary
Existing wafer dicing methods, such as laser and plasma etching, face issues with complex processes, increased manufacturing costs, and difficulty in achieving clean cuts due to isotropic etching, leading to prolonged process times and reduced productivity.
A combination of laser and plasma processes is used to form groove and trench lines on semiconductor wafers, employing a water-soluble polymer coating, mixed wavelength laser beams, and selective plasma etching to achieve efficient and precise dicing.
The method shortens process time, effectively removes by-products, and enhances productivity by ensuring clean cuts and stable implementation for advanced packaging, particularly in HBM applications.
Smart Images

Figure KR2026095119_12112026_PF_FP_ABST
Abstract
Description
Semiconductor wafer dicing method
[0001] The present invention relates to a method for dicing a semiconductor wafer.
[0002] The dicing process is a process of cutting multiple semiconductor chips on a wafer using a blade or a laser, and various methods such as saw dicing, laser dicing, and stealth dicing have been used.
[0003] Meanwhile, in the wafer dicing process using blades, chipping defects and crack defects frequently occurred, and to solve these problems, a dicing process using laser or plasma etching has been applied instead of saw dicing.
[0004] However, the laser-based dicing process had the disadvantage of requiring a separate protective layer to prevent cut silicon particles from fusing to the surface of the semiconductor chip when forming grooves in the wafer's scribe lines or completely cutting the scribe lines. Additionally, the plasma-based dicing process required an etching mask to prevent the semiconductor chip surface from being etched when cutting the scribe lines, and required a separate protective layer coating process similar to the laser-based dicing process, which made the dicing process complex and increased manufacturing costs.
[0005] Specifically, the plasma-based dicing process generally utilizes the "Bosch process," which is a method for forming a structure of a desired depth by repeating the steps of depositing a protective film using a fluorocarbon-based gas and etching silicon using a plasma such as SF6. However, this process has the problem that it is difficult to secure a clean cut surface in the vertical direction because the etching tends to proceed isotropically. Additionally, since the etching and deposition steps must be repeated, the overall process time is prolonged and productivity is reduced.
[0006] Accordingly, the present invention aims to overcome the problems of the aforementioned prior art and provides a wafer dicing method capable of shortening process time and effectively removing by-products generated during the process by applying a combination of laser and plasma for the stable implementation of advanced packaging, particularly HBM.
[0007] A semiconductor wafer dicing method according to one embodiment of the present invention is proposed to solve the above-mentioned problems, and by applying a combination of a laser and plasma, the process time can be shortened and by-products generated during the process can be efficiently removed.
[0008] According to one embodiment, a semiconductor wafer dicing method for separating a wafer comprising a street layer, an integrated circuit layer, and a substrate layer into a plurality of semiconductor dies may be provided, comprising: an LP coating step of forming an LP coating layer on the street layer; a laser grooving step of forming a groove line along a wafer scribe line by irradiating a groove laser beam onto the wafer on which the LP coating layer is formed; a laser erosion step of forming a trench line on the wafer in which the groove line is extended downward by irradiating a erosion laser beam onto the formed groove line; and a plasma etching step of etching the trench line by performing either a first plasma process or a second plasma process according to the position of the lowest region of the trench line on the wafer on which the trench line is formed.
[0009] Additionally, a semiconductor wafer dicing method may be provided in which, in the above LP coating step, the LP coating layer is a water-soluble polymer, and the water-soluble polymer comprises at least one material selected from Polyvinyl Alcohol (PVA), Polyethylene Glycol (PEG), Hydroxypropyl Methylcellulose (HPMC), Gelatin, Polyacrylamide (PAM), Sodium Alginate, and Carboxymethyl Cellulose (CMC).
[0010] In addition, a semiconductor wafer dicing method may be provided in which, in the laser grooving step, the wavelength of the groove laser satisfies a wavelength range of 300 to 500 nm.
[0011] Additionally, a semiconductor wafer dicing method may be provided, wherein in the laser pulverizing step, the pulverizing laser beam is a mixed pulverizing laser beam comprising a first pulverizing laser beam and a second pulverizing laser beam, and the mixed pulverizing laser beam has a pulse width selected from a nanosecond range, a picosecond range, and a femtosecond range.
[0012] In addition, a semiconductor wafer dicing method may be provided in which the first fusion laser beam satisfies a wavelength range of 500 to 1500 nm and the second fusion laser beam satisfies a wavelength range of 100 to 400 nm.
[0013] Additionally, a semiconductor wafer dicing method may be provided in which, in the laser pulverizing step, the first pulverizing laser beam and the second pulverizing laser beam are sequentially irradiated, the first pulverizing laser beam induces the formation of a metal oxide layer on the inner periphery of the trench line, and the second pulverizing laser beam induces the removal of the metal oxide layer formed in the lower region of the inner periphery of the trench line.
[0014] Additionally, a semiconductor wafer dicing method may be provided in which the laser fusion step involves irradiating the first fusion laser beam to form the trench line on the wafer such that the lowest region of the trench line is located in the lowest region of the substrate layer, or forming the trench line such that the lowest region of the trench line is located within the integrated circuit layer.
[0015] In addition, a semiconductor wafer dicing method may be provided, wherein in the plasma etching step, if the lowest region of the trench line is located at the lowest region of the substrate layer, the first plasma process is performed, and the first plasma process is a plasma treatment process that utilizes CF4 plasma to etch a metal oxide layer formed in the entire inner periphery region of the trench line.
[0016] Additionally, a semiconductor wafer dicing method may be provided, wherein in the plasma etching step, if the lowest region of the trench line is located within the integrated circuit layer, a second plasma process is performed, and the second plasma process includes a plasma etching process that etches the lower region of the inner periphery of the trench line using SF6 plasma and a plasma treatment process that etches the metal oxide layer formed in the entire inner periphery of the trench line using CF4 plasma.
[0017] In addition, a semiconductor wafer dicing method may be provided, wherein in the plasma etching step, when the first plasma process is performed, the trench line has an anisotropic etching structure, and when the second plasma process is performed, the trench line has an isotropic etching structure.
[0018] A semiconductor wafer dicing method according to one embodiment of the present invention has the effect of shortening process time and efficiently removing by-products generated during the process by applying a combination of a laser and plasma.
[0019] FIG. 1 is a flowchart illustrating a dicing method for a semiconductor wafer according to one embodiment of the present invention.
[0020] FIG. 2 is a schematic diagram of a process for explaining a dicing method of a semiconductor wafer according to one embodiment of the present invention.
[0021] FIG. 3 is a first process schematic diagram for explaining the laser fusion step of the present invention.
[0022] FIG. 4 is a schematic diagram of a second process to explain the laser fusion step of the present invention.
[0023] FIG. 5 is a schematic diagram of a process for explaining the plasma etching step of the present invention.
[0024] Figure 6 is a diagram showing the microstructure of the wafer dicing area according to laser fusion conditions.
[0025] FIGS. 7 to 9 are drawings showing the microstructure of the wafer dicing region after the plasma process according to the examples and comparative examples.
[0026] Figure 10 shows the results of analyzing the oxide layer in the trench region.
[0027] In order to fully understand the structure and effects of the present invention, preferred embodiments of the present invention will be described in detail with reference to the attached drawings.
[0028] The present invention is not limited to the embodiments disclosed below, but can be implemented in various forms and subject to various modifications and changes. The description of the embodiments is provided merely to ensure that the disclosure of the present invention is complete and to fully inform those skilled in the art of the scope of the invention. In the attached drawings, the components are depicted enlarged from their actual size for convenience of explanation, and the proportions of each component may be exaggerated or reduced.
[0029] The terms used in this specification are for describing embodiments and are not intended to limit the invention. Furthermore, unless otherwise defined, the terms used in this specification may be interpreted in the sense commonly known to those skilled in the art. In this specification, the singular form includes the plural form unless specifically stated otherwise in the text. As used in this specification, 'comprises' and / or 'comprising' do not exclude the presence or addition of one or more other components, steps, actions, and / or elements to the mentioned components, steps, actions, and / or elements.
[0030] Where in this specification a layer is referred to as being 'on' another layer, it may be formed directly on the upper surface of the other layer, or a third layer may be interposed between them. Although terms such as first, second, etc., have been used in this specification to describe various regions, layers, etc., these regions and layers should not be limited by such terms. These terms are used merely to distinguish one specific region or layer from another region or layer. Accordingly, a part referred to as the first part in one embodiment may be referred to as the second part in another embodiment. The embodiments described and illustrated herein also include their complementary embodiments. Throughout the specification, parts indicated by the same reference numeral represent the same components.
[0031] The present invention provides a method for dicing a semiconductor wafer for the stable implementation of advanced packaging, particularly HBM.
[0032] More specifically, the semiconductor wafer dicing method is designed to efficiently remove formed by-products and protrusions by utilizing a combination of lasers and plasma, and to enable flexible responses such as full dicing and selective dicing depending on changes in semiconductor wafer thickness through equipment configuration and laser conditions.
[0033] <Semiconductor Wafer Dicing Method>
[0034] FIG. 1 is a flowchart for explaining a semiconductor wafer dicing method according to an embodiment of the present invention, FIG. 2 is a process schematic diagram for explaining a semiconductor wafer dicing method according to an embodiment of the present invention, FIG. 3 is a first process schematic diagram for explaining a laser fusion process of the present invention, FIG. 4 is a second process schematic diagram for explaining a laser fusion process of the present invention, and FIG. 5 is a process schematic diagram for explaining a plasma process of the present invention.
[0035] FIG. 5a) is a schematic diagram of a process to explain a first plasma process, and FIG. 5b) is a schematic diagram of a process to explain a second plasma process.
[0036] Referring to FIGS. 1 to 5, a semiconductor wafer dicing method (S10) according to one embodiment of the present invention relates to a semiconductor wafer dicing method for separating a wafer including a street layer, an integrated circuit layer, and a substrate layer into a plurality of semiconductor dies, and comprises an LP coating step (S100) for forming an LP coating layer on the street layer, a laser grooving step (S200) for forming a groove line along a wafer scribe line by irradiating a groove laser beam on the wafer having the LP coating layer formed thereon, a laser erosion step (S300) for forming a trench line on the wafer in which the groove line extends downward by irradiating a erosion laser beam on the formed groove line, and a plasma etching step (S400) for etching the trench line region by performing either a first plasma process or a second plasma process according to the position of the lowest region of the trench line on the wafer having the trench line formed thereon.
[0037] A semiconductor wafer dicing method according to one embodiment of the present invention may proceed in the following steps: a wafer mounting process in which the wafer is fixed to a dicing tab or support ring to protect the die from damage during dicing; a grooving process in which a fine groove line is formed on the wafer surface; a dicing process in which the wafer is transferred to individual chips; and a die separation process in which the cut die is picked up.
[0038] In a dicing method for a semiconductor wafer according to one embodiment of the present invention, the wafer may include a street layer, an integrated circuit layer, and a substrate layer.
[0039] The above-mentioned street layer refers to a layer that can distinguish one die and a die adjacent to the above-mentioned die in a dicing process and provide a cutting path, the above-mentioned integrated circuit layer refers to a layer containing semiconductor devices such as transistors, wiring and capacitors, and the above-mentioned substrate layer refers to a base layer that supports the overall structure of the wafer.
[0040] First, referring to FIG. 2, the LP coating step (S100) is a step of forming an LP coating layer by applying a water-soluble polymer (water-soluble resin) onto a wafer.
[0041] Here, the water-soluble polymer may include at least one material selected from Polyvinyl Alcohol (PVA), Polyethylene Glycol (PEG), Hydroxypropyl Methylcellulose (HPMC), Gelatin, Polyacrylamide (PAM), Sodium Alginate, and Carboxymethyl Cellulose (CMC).
[0042] The LP coating layer is uniformly formed on the wafer's surface layer and can serve to protect the wafer during the dicing process. Specifically, it can protect the die from by-products that may occur during subsequent processes or serve as a mask layer during the plasma process.
[0043] In the LP coating step (S100), the process of forming the LP coating layer can sequentially proceed with a resin coating process in which a water-soluble polymer is introduced onto a wafer, a rotation process in which a water-soluble polymer film having a uniform thickness is formed by rotating the wafer, and a curing process in which the water-soluble polymer film is cured through physical drying or UV irradiation.
[0044] Next, the laser grooving step (S200) is a step of forming groove lines, which are shallow and narrow grooves, on the wafer surface using a groove laser beam.
[0045] In the laser grooving step (S200), the wavelength of the groove laser beam may satisfy a wavelength range of 300 to 500 nm. The groove laser beam is irradiated along the scribe line, and a groove line may be formed on the surface of the wafer in a grid pattern. Additionally, the lowest region of the groove line may be located at the lowest region of the scribe layer, that is, the lowest region of the groove line may be in contact with the uppermost region of the substrate layer.
[0046] The groove line described above forms a path for wafer dicing, thereby enabling the dicing process to be performed precisely. In addition, the groove line can prevent chipping or cracking that may occur during the dicing process and minimize wafer breakage.
[0047] Next, referring to FIG. 3, the laser fusion step (S300) is a step of forming a trench line, which is a deep and narrow groove, on the wafer surface using a fusion laser beam. Here, the trench line may be a line including a groove line and an extension line.
[0048] In the laser fusion step (S300), the fusion laser beam may be a mixed fusion laser beam comprising a first fusion laser beam and a second fusion laser beam. That is, the fusion laser beam is a mixed beam rather than a single beam, and the first laser beam and the second laser beam may be irradiated sequentially.
[0049] In addition, the above-mentioned mixed ablation laser beam may have a pulse width selected from the nanosecond range, picosecond range, and femtosecond range.
[0050] Here, the first ablation laser beam is a laser beam for ablation, which vaporizes the integrated circuit layer or substrate layer to extend the groove line downward, thereby forming a trench line.
[0051] In addition, the second fusion laser beam is a laser beam for removing a metal oxide layer generated during the fusion process using the first fusion laser beam, specifically, removing a metal oxide layer located in the lower region of the formed trench line.
[0052] In the laser fusion step (S300), it is desirable to proceed under conditions of low frequency, low repetition processing, and mixed beam.
[0053] Specifically, the first abrasive laser beam satisfies a frequency range of 10 to 60 kHz and a number of irradiations of 1 to 3 cycles, and in a preferred embodiment of the present invention, the first abrasive laser beam satisfies a frequency range of 10 kHz and a number of irradiations of 1 cycle.
[0054] In addition, the first abrasive laser beam satisfies a wavelength range of 500 to 1500 nm, and the second abrasive laser beam satisfies a wavelength range of 100 to 400 nm.
[0055] In the laser fusion step (S300), the first fusion laser beam and the second fusion laser beam may be irradiated sequentially.
[0056] The first abrasive laser beam can induce the formation of a metal oxide layer on the inner periphery of the trench line, and the second abrasive laser beam can induce the removal of the metal oxide layer formed in the lower region of the inner periphery of the trench line.
[0057] Here, the metal oxide layer is formed by a chemical reaction between a metal element contained within the wafer and oxygen, and can be a silicon oxide layer.
[0058] That is, the first fusion laser beam can induce the formation of a silicon oxide layer on the inner periphery of the trench line while simultaneously forming a trench line, and the silicon oxide layer can protect the structure of the trench line by suppressing anisotropic etching in a subsequent process (plasma etching).
[0059] The second fusion laser beam can induce the removal of a metal oxide layer formed in the lower region of the trench line, and the region where the metal oxide layer is removed can become the region where etching begins in a subsequent process (plasma etching).
[0060] Referring to FIG. 4, in the laser fusion step (S300), the depth of the trench line can be controlled to a preset depth, and accordingly, full cutting fusion and selective cutting fusion are possible.
[0061] Full cutting fusion means forming a trench line that extends the groove line to the lowest region of the substrate layer, and selective cutting fusion may mean forming a trench line that extends the groove line so as not to go beyond the integrated circuit layer.
[0062] Specifically, the laser fusion step (S300) may form the trench line on the wafer such that the lowest region of the trench line is located in the lowest region of the substrate layer by irradiating the first fusion laser beam, or form the trench line such that the lowest region of the trench line is located in the integrated circuit layer.
[0063] In the laser fusion step (S300), if full cutting fusion is performed, a separate plasma etching process may not be performed in the subsequent process, and only a plasma treatment process may be performed; if selective cutting fusion is performed, a plasma etching process and a plasma treatment process may be performed sequentially in the subsequent process.
[0064] Referring to FIG. 5, the plasma etching step (S400) is a step of etching trench lines using plasma.
[0065] In one embodiment of the present invention, in the plasma etching step (S400), if the lowest region of the trench line is located at the lowest region of the substrate layer, the first plasma process can be performed, and the first plasma process may be a plasma treatment process that etches a metal oxide layer formed in the entire inner periphery region of the trench line using CF4 plasma.
[0066] In other words, if full cutting fusion is performed in the laser fusion step (S300), only the plasma treatment process for etching the metal oxide layer in the plasma etching step (S400) can be performed.
[0067] In the first plasma process, the CF4 plasma can uniformly decompose and remove the metal oxide layer formed on the inner periphery of the trench line, thereby allowing the wafer to be separated into a plurality of semiconductor dies.
[0068] In addition, in one embodiment of the present invention, in the plasma etching step (S400), if the lowest region of the trench line is located within the integrated circuit layer, the second plasma process can be performed, and the second plasma process may include a plasma etching process that etches the lower region of the inner periphery of the trench line using SF6 plasma and a plasma treatment process that etches the metal oxide layer formed in the entire inner periphery of the trench line using CF4 plasma.
[0069] In other words, if selective cutting fusion is performed in the laser fusion step (S300), a plasma etching process for plasma etching an integrated circuit layer adjacent to the lower region of the trench line and a plasma treatment process for etching a metal oxide layer can be performed sequentially in the plasma etching step (S400).
[0070] In the second plasma process, the SF6 plasma can etch the lower region of the trench line to extend the trench line, and the CF4 plasma can uniformly decompose and remove the metal oxide layer formed on the inner periphery of the trench line, thereby allowing the wafer to be separated into a plurality of semiconductor dies.
[0071] Meanwhile, in the plasma etching step (S400), when the first plasma process is performed, the trench line may have an anisotropic etching structure, and when the second plasma process is performed, the trench line may have an isotropic etching structure.
[0072] Specifically, when the first plasma process is performed in the plasma etching step (S400), the trench line may have a groove shape that narrows as it goes downward, and when the second plasma process is performed, the trench line may have a spherical groove shape.
[0073] <Example 1: Fusion of a Semiconductor Wafer>
[0074] A wafer including a street layer, an integrated circuit layer, and a substrate layer was prepared, and an LP coating step, a laser grooving step, and a laser fusion step were sequentially performed on the prepared wafer.
[0075] In the laser fusion step, a first fusion laser beam and a second fusion laser beam were sequentially irradiated, wherein the first fusion laser beam satisfied a frequency range of 10KHz, 30KHz, and 60KHz, and the number of irradiations was performed as one cycle. In addition, a trench line was formed by irradiating the first fusion laser beam such that the lowest region of the trench line was located at the lowest region of the substrate layer.
[0076] Here, the sample that underwent the full cutting and fusion process under the conditions of a mixed beam, a frequency of 10KHz, and 1 cycle is Sample A of Example 1, the sample that underwent the full cutting and fusion process under the conditions of a mixed beam, a frequency of 30KHz, and 1 cycle is Sample B of Example 1, and the sample that underwent the full cutting and fusion process under the conditions of a mixed beam, a frequency of 60KHz, and 1 cycle is Sample C of Example 1.
[0077] In the laser fusion step, a first fusion laser beam and a second fusion laser beam were sequentially irradiated, wherein the first fusion laser beam satisfied a frequency range of 10KHz, and the number of irradiations proceeded as 1 cycle, 2 cycles, and 3 cycles. In addition, a trench line was formed by irradiating the first fusion laser beam so that the lowest region of the trench line was located within the integrated circuit layer.
[0078] Here, the sample that underwent the selective cutting and fusion process under the conditions of a mixed beam, a frequency of 10KHz, and 1 cycle is Sample D of Example 1, the sample that underwent the selective cutting and fusion process under the conditions of a mixed beam, a frequency of 10KHz, and 2 cycles is Sample E of Example 1, and the sample that underwent the selective cutting and fusion process under the conditions of a mixed beam, a frequency of 10KHz, and 3 cycles is Sample F of Example 1.
[0079]
[0080] <Comparative Example 1: Fusion of a Semiconductor Wafer>
[0081] A wafer including a street layer, an integrated circuit layer, and a substrate layer was prepared, and an LP coating step, a laser grooving step, and a laser fusion step were sequentially performed on the prepared wafer.
[0082] In the laser fusion step, a first fusion laser beam was irradiated, wherein the first fusion laser beam satisfied a frequency range of 10KHz, and the number of irradiations was performed as one cycle. In addition, a trench line was formed by irradiating the first fusion laser beam such that the lowest region of the trench line was located within the integrated circuit layer.
[0083] Here, the sample that underwent the selective cutting and fusion process under the conditions of a single beam, a frequency of 10KHz, and 1 cycle is Sample A of Comparative Example 1.
[0084] <Example 2: Etching of a Semiconductor Wafer>
[0085] A wafer including a circuit layer, an integrated circuit layer, and a substrate layer was prepared, and an LP coating step, a laser grooving step, a laser fusion step, and a plasma etching step were sequentially performed on the prepared wafer.
[0086] Sample C of Example 1 was prepared, and a plasma treatment process using CF4 plasma was performed on the prepared Sample C of Example 1 to etch the silicon oxide layer formed in the entire inner perimeter area of the trench line.
[0087] Here, the sample that underwent the plasma treatment process on the sample that underwent the full cutting fusion process is Sample A of Example 2.
[0088] Sample D of Example 1 was prepared, and a plasma etching process using SF6 plasma and a plasma treatment process using CF4 plasma were sequentially performed on the prepared Sample D of Example 1 to etch the lower region of the inner perimeter of the trench line and simultaneously etch the silicon oxide layer formed on the entire inner perimeter of the trench line.
[0089] Here, the sample that underwent the plasma etching process and plasma treatment process on the sample that underwent the selective cutting fusion process is Sample B of Example 2.
[0090] <Comparative Example 2: Etching of a Semiconductor Wafer>
[0091] A wafer including a street layer, an integrated circuit layer, and a substrate layer was prepared, and the Bosch process, which forms deep vertical trenches by repeating two processes of deposition and etching on the prepared wafer, was performed.
[0092] Here, the deposition process is a process of forming a protective layer using a fluorocarbon-based gas, and the etching process is a process of plasma etching the wafer surface using SF6 gas.
[0093] Here, the sample that underwent the Bosch process is Sample A of Comparative Example 2.
[0094] <Experimental Example 1: Evaluation of Wafer Microstructure According to Laser Fracturing Conditions>
[0095] Samples A to F of Example 1 and Sample A of Comparative Example 1 were prepared, the trench lines of the prepared samples were observed, and the results are shown in FIG. 6.
[0096] Figure 6 is a diagram showing the microstructure of the wafer dicing area according to laser fusion conditions.
[0097] FIG. 6a) is an SEM image of samples A to C according to Example 1, FIG. 6b) is an SEM image of samples D to F according to Example 1, and FIG. 6c) is an SEM image of sample D according to Example 1 and sample A according to Comparative Example 1.
[0098] As shown in Fig. 6a), it can be seen that samples A to C according to Example 1 are formed such that the lowest region of the trench line is located at the lowest region of the substrate layer as the full cutting fusion process proceeds, and it can be seen that the silicon oxide layer is removed from the lower region of the inner perimeter of the trench line.
[0099] As shown in FIG. 6b), it was confirmed that samples D to F according to Example 1 were formed such that the lowest region of the trench line was located within the integrated circuit layer as the selective cutting fusion process proceeded. Similarly, it was confirmed that the silicon oxide layer was removed from the lower region of the inner perimeter of the trench line.
[0100] As shown in Fig. 6c), it was confirmed that silicon oxide formed over the entire inner perimeter of the trench line in Sample A according to Comparative Example 1 as a single beam was irradiated.
[0101] <Experimental Example 2: Evaluation of Wafer Microstructure>
[0102] Sample A of Example 2, Sample B of Example 2, and Sample A of Comparative Example 2 were prepared, the trench lines of the prepared samples were observed, and the results are shown in FIGS. 7 to 9.
[0103] FIGS. 7 to 9 are drawings showing the microstructure of the wafer dicing region after the plasma process according to the examples and comparative examples.
[0104] Figure 7 is an SEM image of sample A of Example 2, Figure 8 is an SEM image of sample B of Example 2, and Figure 9 is an SEM image of sample A of Comparative Example 2.
[0105] As shown in FIGS. 7 to 9, it was confirmed that the trench line of Sample A of Example 2 has an anisotropic etching structure, and that the silicon oxide layer formed over the entire inner periphery of the trench line was completely etched.
[0106] In addition, it was confirmed that the trench line of Sample B in Example 2 has an isotropic etching structure, and that the silicon oxide layer formed over the entire inner periphery of the trench line was completely etched.
[0107] In addition, it was confirmed that the trench line of Sample A of Comparative Example 2 had an anisotropic etching structure, but it was confirmed that surrounding by-products and defective protrusions were not completely removed in the inner periphery area of the trench line.
[0108] <Experimental Example 3: Evaluation of Wafer Microstructure>
[0109] Sample C of Example 1 and Sample A of Example 2 were prepared, and the inner perimeter of the trench line according to the prepared samples was analyzed by SEM and EDS, and the results are shown in FIG. 10.
[0110] Figure 10 shows the results of analyzing the oxide layer in the trench region.
[0111] FIG. 10a) is an SEM image and an EDS image observing the trench line of sample C according to Example 1, and FIG. 10b) is an SEM image and an EDS image observing the trench line of sample A of Example 2.
[0112] As shown in Fig. 10, it was confirmed that a silicon oxide layer was formed in the inner perimeter region of the trench line of Sample C according to Example 1. On the other hand, it was confirmed that the silicon oxide layer formed by the plasma treatment process was completely removed in the inner perimeter region of the trench line of Sample A of Example 2.
[0113] Although a method for dicing a semiconductor wafer according to an embodiment of the present invention has been described above as a specific embodiment, this is merely illustrative and the present invention is not limited thereto, and should be interpreted as having the broadest scope in accordance with the basic concept disclosed in this specification. Those skilled in the art may implement unspecified embodiments by combining or substituting the disclosed embodiments, and this also does not deviate from the scope of the rights of the present invention. Furthermore, those skilled in the art may easily change or modify the embodiments disclosed based on this specification, and it is evident that such changes or modifications also fall within the scope of the rights of the present invention.
Claims
1. A semiconductor wafer dicing method for separating a wafer comprising a circuit layer, an integrated circuit layer, and a substrate layer into a plurality of semiconductor dies, wherein LP coating step of forming an LP coating layer on the above street layer; A laser grooving step of forming groove lines along wafer scribe lines by irradiating a groove laser beam onto a wafer having an LP coating layer formed thereon; A laser fusion step of irradiating a fusion laser beam onto a formed groove line to form a trench line on the wafer in which the groove line extends downward; and Plasma etching step comprising etching the trench line by performing either a first plasma process or a second plasma process according to the position of the lowest region of the trench line on a wafer having the trench line formed thereon. Semiconductor wafer dicing method.
2. In Paragraph 1, In the above LP coating step, the LP coating layer is a water-soluble polymer, and The above water-soluble polymer comprises at least one material selected from Polyvinyl Alcohol (PVA), Polyethylene Glycol (PEG), Hydroxypropyl Methylcellulose (HPMC), Gelatin, Polyacrylamide (PAM), Sodium Alginate, and Carboxymethyl Cellulose (CMC). Semiconductor wafer dicing method.
3. In Paragraph 2, In the above laser grooving step, the wavelength of the groove laser satisfies a wavelength range of 300 to 500 nm, Semiconductor wafer dicing method.
4. In Paragraph 3, In the above laser fusion step, the fusion laser beam is a mixed fusion laser beam comprising a first fusion laser beam and a second fusion laser beam, and The above-mentioned hybrid ablation laser beam has a pulse width selected from the nanosecond range, the picosecond range, and the femtosecond range, Semiconductor wafer dicing method.
5. In Paragraph 4, The above-mentioned first ablation laser beam satisfies a wavelength range of 500 to 1500 nm, and The above second ablation laser beam satisfies a wavelength range of 100 to 400 nm, Semiconductor wafer dicing method.
6. In Paragraph 5, In the above laser fusion step, the first fusion laser beam and the second fusion laser beam are irradiated sequentially, and The first abrasion laser beam induces the formation of a metal oxide layer on the inner periphery of the trench line, and The second abrasion laser beam above induces the removal of a metal oxide layer formed in the lower region of the inner perimeter of the trench line, Semiconductor wafer dicing method.
7. In Paragraph 6, The above laser fusion step is, By irradiating the first abrasive laser beam, the trench line is formed on the wafer such that the lowest region of the trench line is located in the lowest region of the substrate layer, or the trench line is formed such that the lowest region of the trench line is located within the integrated circuit layer. Semiconductor wafer dicing method.
8. In Paragraph 7, In the above plasma etching step, If the lowest region of the above trench line is located in the lowest region of the above substrate layer, the first plasma process is performed, and The above first plasma process is a plasma treatment process that utilizes CF4 plasma to etch a metal oxide layer formed over the entire inner perimeter area of the trench line, Semiconductor wafer dicing method.
9. In Paragraph 8, In the above plasma etching step, If the lowest region of the above trench line is located within the integrated circuit layer, the second plasma process is performed, and The second plasma process described above includes a plasma etching process that etches the lower region of the inner perimeter of the trench line using SF6 plasma, and a plasma treatment process that etches the metal oxide layer formed over the entire inner perimeter of the trench line using CF4 plasma. Semiconductor wafer dicing method.