Composite material

A composite material combining paper pulp, waste plant material, and plant-derived cellulose particulates addresses sustainability issues by enhancing strength and water resistance, making it suitable for various applications.

WO2026238912A1PCT designated stage Publication Date: 2026-11-19SELLYUKOMP LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/064129
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2026-05-13
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing paper and composite materials rely heavily on wood fibers, leading to sustainability issues and inefficient use of resources, while waste plant materials like draff and barley straw have poor physical properties and high water absorption, limiting their applicability in structural and packaging materials.

Method used

A composite material is developed comprising 20-80 wt% paper pulp, 20-80 wt% waste plant material, and 0.1-10 wt% plant-derived cellulose particulate material, which enhances strength and water resistance by increasing hydrogen bonding and reducing porosity.

Benefits of technology

The composite material achieves improved mechanical properties and water resistance, reducing reliance on wood fibers and expanding usability in diverse applications, while being biodegradable and cost-effective.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2026064129_19112026_PF_FP_ABST
    Figure EP2026064129_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The invention provides a novel composite material that effectively addresses the material strength and water absorption challenges of waste plant material based composites by integrating plant-derived cellulose-containing particulate materials. This innovation extends the potential applications of waste plant materials beyond traditional uses, contributing to sustainable material development.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Composite Material

[0002] Field of the Invention

[0003] The present invention relates to composite materials, specifically those incorporating waste plant matter as a primary component in combination with paper pulp and an additive to enhance water resistance and mechanical properties.

[0004] Background of the Invention

[0005] Paper, card, and related composite materials are primarily formed from wood fibres, mainly cellulose fibres. The wood fibres are well known to have desirable strength properties and can be formed into products with excellent surface properties. Accordingly, the paper industry is a large consumer of wood from forests and plantations, which presents sustainability and ecological issues. Furthermore, many paper, card and composite materials are used in single use packaging which is then discarded, leading to inefficient use of the wood fibre materials. One goal of the present invention is to provide an alternative product which can mitigate use of wood fibre starting materials.

[0006] A wide variety of waste materials are derived from plant sources and generated through a range of agricultural and industrial processes, which then require disposal. As waste materials, their low value makes them attractive starting materials, but their physical properties are often poor and result in low grade products. As such, use of such waste plant material is limited. Even with recycled wood fibre materials, it is common to incorporate various non-biodegradable polymers and resins in order to achieve a viable composite material e.g. having sufficient strength, water resistance, or surface quality.

[0007] An example of such a waste plant material is draff, a byproduct of brewing and distillation. Draff is a fibrous, organic material primarily composed of cellulose, hemicellulose, lignin, proteins, and residual starches. A further example is chopped barley straw. While these waste plant materials have been utilized in various applications such as animal feed, biofuel production, and biodegradable composites, their high water absorption and / or typical fibre sizes limit their applicability in structural and packaging materials. In particular, fibres with too short a length and / or a high length to width ratio do not form effective structural webs due to inferior hydrogen bonding compared to those formed from paper pulp.To enhance the performance of waste plant material based composite materials, it is desirable to improve their strength, surface quality, and / or hydrophobicity. The present invention seeks to mitigate or ameliorate one or more of the above problems. This invention proposes a novel composite material that contains a low value starting material and overcomes water absorption issues, thereby expanding its usability in diverse applications.

[0008] Summary of the Invention

[0009] According to an aspect of the invention, there is provided a composite material. The composite material may comprise 20-80 wt% of paper pulp. The composite material may comprise 20-80 wt% of a waste plant material. The composite material may comprise 0.1-10 wt% of a plant-derived cellulose particulate material.

[0010] The inventors have found that incorporating a proportion of plant-derived cellulose particulate material into a composite material can improve the material properties of composites comprising waste plant materials, or mitigate a reduction in material properties due to the incorporation of waste plant materials. The corresponding composite materials can be formed with a high proportion of waste plant material, thereby reducing the cost of processing waste materials, reducing reliance on wood fibres, and / or improving the material properties. The resulting composite materials are low cost and biodegradable.

[0011] Plant-derived cellulose particulate material

[0012] Suitable plant-derived cellulose-containing particulate materials are available from the present applicant under the product name Curran®. The plant-derived cellulose particulate materials may be as described in the present applicant’s earlier applications WO2014 / 147392 and / or WO2014 / 147393 but also WO2015177548A1 and WO2017220777.

[0013] Without wishing to be bound by theory, it is believed that the plant-derived cellulose-containing particulate materials interact with other natural polymeric materials in the composite material creating increased hydrogen bonding and therefore strength. Once dried, the presence of the particulate materials leads to a high density and low porosity composite material due to the particulate materials bridging pores within the paper pulp and waste plant material matrix. This is understood to reduce the surface hydrophilicity and provide a surface which is better able to bind with surface coatings and / or decorations.

[0014] The plant-derived cellulose containing particulate material may be formed from a process comprising:(i) contacting herbaceous plant material with a peroxide reagent and optionally water; (ii) heating the mixture from (i) to a temperature of from 30 to 110°C and maintaining said mixture at a temperature of from 30 to 110°C until the pH of the mixture has reached a predetermined pH value; and

[0015] (iii) isolating the resulting cellulose-containing particulates.

[0016] The plant-derived cellulose-containing particulate materials comprise portions and fragments of the plant cell walls. The particulate material comprises a high proportion of cellulose and may comprise cellulose as the highest individual component.

[0017] The herbaceous plant material may comprise any non-woody plant material. "Herbaceous" is a well-defined botanical term that refers to annual, bi-annual or perennial vascular plants Preferably, the plant material is a vegetable or a fruit material. Useful examples include root vegetables such as sugar beet, carrot, turnip, parsnip, swede, fruits such as apple and pear, and citrus fruits such as oranges, lemons etc. The plant material may comprise a waste plant material, e.g. the waste remaining after a useful product has been extracted, such as postprocessing pulp from sugar or juice production.

[0018] The peroxide reagent may comprise hydrogen peroxide.

[0019] The temperature in step (ii) may comprise 40-110°C, 50-105°C, 60-100°C, 70-100°C, 80-100°C, 90-100°C, 95-100°C or approximately 97°C. Preferably the target heating temperature and the maintenance temperature are the same. The mixture may be maintained at the temperature for 20-60 minutes e.g. 25-50 minutes, or 30-45 minutes.

[0020] The predetermined pH value may comprise an absolute pH value, or a predetermined change in pH. The change in pH may comprise a change of about 1 to 2 pH units e.g. a drop in pH.

[0021] Isolating the cellulose-containing particulates may comprise one or more of: washing, filtering, and / or pressing the resulting material.

[0022] The process may comprise milling the resulting material e.g. to achieve a desired particle size. Milling may be carried out in a colloid mill with a gap size of 50 to 500 microns e.g. 75 to 400 microns, 100-300 microns, 125-275 microns, 150-250 microns, 175-225 microns, or 200 microns. The process may comprise drying the resulting material e.g. after milling.The plant-derived cellulose-containing particulate materials may be in the form of platelets. The platelets may comprise a mesh of nanocellulose fibres. The plant-derived cellulose particles may have a mean major dimension of from 1 to 250 microns. For example, the plant-derived cellulose particles may have a mean major dimension of from 10 to 240, 25-225, 50-200, 75-175, 100-150, or 125 microns. In one series of embodiments, the plant-derived cellulose particles may have a mean major dimension of 10 to 100 microns e.g. 20-90, 30-80, 40-70, 50-60 microns. Preferably they have a mean major dimension of from 10 to 70 m or from 30 to 70 pm.

[0023] The plant-derived cellulose-containing particulate materials may have an mean thickness of 0.1 to 10 microns. For example, the plant-derived cellulose-containing particulate materials may have an mean thickness of 0.2-9, 0.3-8, 0.4-7, 0.5-6, 0.6-4, 0.7-3, 0.8-2, 0.9-1.75, or 1-1.5 microns. Preferably, the platelets have an mean thickness of 0.5-2 microns.

[0024] The plant-derived cellulose-containing particulate materials may have a ratio of mean major dimension to mean thickness of from 200:1 to 50:1, for example 150:1, 125:1, 100:1, or 75:1.

[0025] The particulate dimensions can be measured by light microscopy. The particles are stained by adding a few drops of methylene blue to a dilute suspension of fully hydrated particles on a slide. The particles are viewed at 100X magnification, using a Dyno-eye camera (USB) on the eye piece of the microscope with Dynocapture 2.0 software on a computer connected to the camera. The largest particle dimension is measured using image analysis.

[0026] The plant-derived cellulose-containing particulate materials are typically not considered as nanocellulosic components, as these are usually composed of cellulose material that has been broken down to the nanoscale, i.e. thin fibres with an average length of from 1 nanometre to less than 100 nanometres, also known as nanofibrils.

[0027] The plant-derived cellulose-containing particulate material may comprise less than 60 wt% cellulose e.g. less than about 59 wt%, less than about 58 wt%, less than about 55 wt%, less than about 53 wt%, less than about 50 wt%, less than about 45 wt%, or less than about 40 wt% cellulose. In one series of embodiments, the cellulose-containing particles comprise cellulose in an amount greater than about 40 wt%, for example greater than about 45 wt%, greater than about 50 wt%, greater than about 53 wt%, greater than about 55 wt%, greater than about 58 wt%, greater than about 59 wt%, for example up to about 60 wt%.In one series of embodiments the plant-derived cellulose-containing particulate material comprises 40-60wt%, 42-58wt%, 44-56wt%, 45-55wt%, 46-54wt%, 48-52wt%, or 50wt% cellulose.

[0028] The plant-derived cellulose particulate material may comprise less than 30 wt% extractable glucose e.g. less than 25wt%, less than 20wt%, less than 19wt%, less than 18wt%, less than 17wt%, less than 16wt%, less than 15wt% extractable glucose.

[0029] The plant-derived cellulose particulate material may have a non-carbohydrate content of 20 to 50 % by dry weight. For example, the non-carbohydrate content may be 25-45%, 30-40%, or 35% by dry weight. The term “non-carbohydrate” herein refers to, among others, glycoproteins, but also other components that are not extractable sugars. Herein, the saccharide or oligosaccharide component of the glycoproteins is not accounted for as carbohydrate component.

[0030] Preferably the cellulose-containing particles contain polysaccharides other than cellulose in an amount of from 4 to 6 wt%.

[0031] Preferably the cellulose-containing particles contain hemicellulose in an amount of less than 2 wt % and pectin in amount of less than 10 wt %. The cellulose content and the content of the other polysaccharides may be measured using the following standard method: a sample of the material is converted into alcohol-insoluble residues and a portion of this is then subjected to acid hydrolysis using 2M trifluoroacetic acid for 1 hour at 120 °C. This produces a hydrolysate and a non-hydrolysable cellulosic / polysaccharide residue. The hydrolysate is dried and re-suspended in distilled water. This solution is then analysed for monosaccharide content using HPLC.

[0032] The cellulose-containing particulate material may contain extractable xylose in an amount of at least 5 % of the amount of extractable xylose in the starting plant material. The cellulose-containing particulate material may contain extractable xylose in an amount of at least 6%, at least 7%, at least 8%, at least 9%, at least 10 % of the amount of extractable xylose in the starting plant material, for example at least 20 %, at least 30 %, or at least 40 %.

[0033] In one series of embodiments, the cellulose particulate material may contain less than 70 % extractable xylose relative to the amount of extractable xylose in the starting plant material. Alternatively, the cellulose-containing particulate material may contain less than 60 % or 55% extractable xylose relative to the amount of extractable xylose in the starting plant material.In one series of embodiments, the cellulose-containing particulate material may contain extractable xylose in an amount of 5-70% of the amount of extractable xylose in the starting plant material e.g. 6-65%, 7-60%, 8-55%, 9-50%, 10-40%, or 20-30%.

[0034] In one series of embodiments, the cellulose-containing particulate material may be derived from sugar beet and contains at least about 1.5 wt% e.g. at least 1.6 wt%, at least about 1. 7 wt%, at least about 1.8 wt% at least about 1.9 wt%, for example about 2 wt% extractable xylose. The amount of extractable xylose in the starting sugar beet plant material may be about 20wt%. Alternatively, the cellulose-containing particulate material may be derived from carrot and may contain at least 0.8wt%, at least 0.9wt%, at least 1.0wt% extractable xylose. The amount of extractable xylose in the starting carrot plant material may be about 2.0wt%.

[0035] The cellulose-containing particles may be insoluble in water. By insoluble in water is meant that, at a concentration of 1 wt % (solids) or less in water, the cellulose-containing particles are discrete particles. A discrete particle is one that can be observed as such using light microscopy at 100X magnification.

[0036] The plant starting material for forming the cellulose-containing particulates may be a seed plant, ie. belonging to Magnoliaphyta. In a further embodiment the plant may be a monocotyledon, more specifically a member of Poales, typically a cereal. The plant material may be a waste product or side-stream from agricultural production.

[0037] The plant may be a member of eucotyledones, more specifically a crop plant, or a waste product or side-stream from agricultural production. Pulps remaining after production of sugar beet or potato starch are attractive agricultural side streams useful for the plant-derived cellulose-containing particulate matter. Root crops are in general relevant raw materials. A non-exhaustive list comprises carrot, swede, turnips, parsnips and radish. Pomace from fruit preserve, jam, juice production is another valuable waste product from which cellulose may be recovered.

[0038] The plant material used for the plant-derived cellulose-containing particulate matter is herbaceous plant material. These are further characterized by their aerial stems dying after each growth season. Regrowth in subsequent seasons for bi-annual and perennial species takes place from subterraneous organs, for example stem or root storage organs, tubers.The plant material may have a parenchymal cell content of higher than 30 % by volume, more preferably higher than 35 % by volume or higher than 50 % by volume and most preferably higher than 70 % based on the total volume of the plant material. The plant material may contain less than 20 wt % lignin, more preferably it contains from 1 to 10 wt % lignin, most preferably it contains from 1 to 5 wt % lignin. Lignin content can be measured by a standard method such as the Klason method. The plant material may comprise less than about 30 wt% lignocellulose e.g. less than 20wt%, less than 15 wt%, less than 10 wt%, less than 8wt%, less than 6wt%, less than 5wt%, less than 4wt%, less than 3wt%, less than 2wt%, less than 1wt%, or substantially no lignocellulose.

[0039] H / aste plant material

[0040] The waste plant material may comprise or consist primarily of particles having a mean size of 1 to 500 microns. Preferably, the waste plant material may comprise particles having a mean particle size of 1 to 250 microns. In some embodiments, the waste plant material may comprise material having a maximum particle size of 5mm, optionally 4mm, 3mm, 2mm or 1mm. In a further series of embodiments, the waste plant material may consist of particles having a mean particle size of 1 to 500 microns. For example, the waste plant material may comprise or consist of particles having a mean particle size of 1-200, 1-150, 1-100, 1-75, 1-50, 1-40, 1-30, 5-200, 10-200, 25-200, 50-200, 75-200 or 100-200 microns. The waste plant material may comprise less than 10% by weight of the total waste plant material of particles having a mean particle size greater than 250 microns. In some embodiments, the plant material may comprise less than 8wt%, 6wt%, 5wt%, 4wt%, 3wt% or 2 wt% of particles having a mean particle size greater than 250 microns. Preferably, the waste plant material may comprise 0.1 to 10wt%, 1-9wt%, 2-8wt%, 3-7wt%, 4-6wt%, or5wt% of particles having a mean particle size greater than 200 microns, by weight of the total waste plant material. The waste plant material may comprise less than 10% by weight of particles having a mean particle size greater than 250 microns, 225 microns, or 200 microns.

[0041] The waste plant material may comprise a dry waste plant material. Alternatively, the waste plant material may have a moisture content of 50 to 95%, 55-90%, 60-85%, 65-80%, or 70-75%. Low grade or low value waste plant materials often have a high moisture content, thus it is advantageous that the composite material of the present invention can be formed from such materials without requiring energy intensive pre-processing such as drying.The waste plant material may comprise an agricultural byproduct, food processing byproduct, and / or industrial byproduct. The waste plant material may comprise the retentate of biomass subjected to one or more of: mashing, fermentation, milling, and fi bril lating.

[0042] The waste plant material may comprise one or more of:

[0043] draff derived from cereals, such as barley, corn, oats, wheat, and such as distillers spent grain and / or brewers spent grain; and / or

[0044] chaff derived from grain, straw, and / or hay;

[0045] waste derived from plant oil extraction such as oil plant stems and heads, oilseed cake, and oilseed meal;

[0046] wood processing byproducts such as sawdust, shavings, and / or woodchip; and other plant fibres and byproducts comprising and / or derived from wood, sugar palms, nypa palm, cassava, milo, sorghum, sweet potatoes, molasses, tubers, roots, stems, sago, cassava, tapioca, rice peas, beans, potatoes, beets, fruits, pits, sorghum, sugar cane, rice, wheat straw, grass, hay, hemp, whole grains, rye, barley, bamboo, seeds, flower heads, algae, seaweed, and equisetum.

[0047] In a preferred series of embodiments, the waste plant material comprises draff (e.g. DSG and / or BSG). In a further preferred series of embodiments, the waste plant material comprises whisky draff.

[0048] The composite material may comprise two or more, three or more, or four or more waste plant materials from the above list. In one series of embodiments, the composite material may comprise draff and one or more further waste plant materials as described previously.

[0049] The waste plant material may comprise cellulose, hemicellulose, lignin, proteins, and residual starches.

[0050] Paper pulp

[0051] The paper pulp may comprise any conventional paper pulp, such as kraft pulp. The paper pulp may comprise virgin kraft pulp. The paper pulp may comprise recycled paper pulp. The paper pulp may be derived from wood fibres and / or non-wood fibres extracted by any method. Wood fibres may comprise fibres derived from hard or softwoods. Non-wood fibres may comprise those derived from hemp, grasses e.g. bamboo, or other sources. Preferable non-wood fibres are those with a length and strength comparable to wood fibres e.g. in contrast to the waste plant fibres described herein which are typically short and of lower strength. The paper pulp may comprise a combination of virgin and recycled paper pulp.Other components

[0052] The composite material may further comprise a binder. The binder may comprise a biopolymer resin and / or a natural adhesive.

[0053] The composite material may further comprise an additive.

[0054] The composite material may further comprise a surface coating. The surface coating may comprise a mineral-based surface coating, such as kaolinite, calcium carbonate, bentonite, or talc. The surface coating may be a polymer coating. The surface coating may comprise a polyethylene and / or polyolefin-based coating, polyethylene terephthalate (PET)-based coating, polyurethane-based coating, an acrylic based coating, PVA (polyvinylacetate) based coating, PVOH (polyvinyl alcohol) based coating, and / or other polymeric non-polymeric and / or resin-based barrier coatings. In one series of embodiments, the surface coating comprises a polyurethane-based coating. In a further series of embodiments, the surface coating comprises a coating based on the plant-derived cellulose particulate material described herein. The surface coating may be provided on a single surface of the composite material. Alternatively, the surface coating may be provided on two or more surfaces of the composite material e.g. on upper and lower and / or internal and external surfaces. The surface coating may be provided on all surfaces of the composite material.

[0055] In some embodiments, the surface coating may be configured to provide a barrier layer. In some embodiments, the composite material may comprise one or more layers within a laminate material.

[0056] Method

[0057] According to a second aspect of the invention, there is provided a method for producing a composite material as described above. The method may comprise mixing a waste plant material with paper pulp and a plant-derived cellulose particulate material to form a mixture. The method may comprise drying and / or compressing the mixture to form a solid composite material.

[0058] The method may further comprise drying the waste plant material e.g. to achieve a desired moisture content. The method may further comprise milling the waste plant material e.g. to a desired particle size. The drying and / or milling may be carried out prior to mixing the waste plant material with paper pulp and the plant-derived cellulose particulate material.The method may further comprise coating the solid composite material with a coating material, such as those described previously. The coating material may comprise a polyurethane based coating material or other type of barrier coating that can be applied onto standard paper as described with respect to the first aspect of the invention.

[0059] The resulting composite exhibits enhanced water resistance, increased durability, and improved mechanical properties, making it suitable for applications in biodegradable packaging, with high water resistance.

[0060] Increasing the amount of the plant-derived cellulose particulate material beyond 5% wt can further reduce porosity and hydrophilicity of the composite, leading to reduced water absorption and improved longevity. However, excessive amounts may affect mechanical performance, requiring an optimal balance tailored to specific applications.

[0061] Paper pulp substitute

[0062] According to a third aspect of the invention, there is provided a paper pulp substitute for use in forming composite materials. The paper pulp substitute may comprise 20 to 80 parts by weight of a waste plant material. The paper pulp substitute may comprise 0.1 to 10 parts by weight of a plant-derived cellulose-containing particulate material.

[0063] In one series of embodiments, the paper pulp substitute may comprise 25 to 75, 30 to 70, 35 to 65, 40 to 60, 45 to 55 or 50 parts by weight of a waste plant material. In other words, the paper pulp substitute may comprise from 66% to 99.5% waste plant material, relative to the weight of the paper pulp substitute as a whole. For example, the paper pulp substitute may comprise at least 66%, 70%, 75%, 80%, 85%, 90%, 95% or 99% waste plant material.

[0064] The paper pulp substitute may comprise 0.5 to 9.5, 1 to 9, 2 to 8, 3 to 7, 4 to 6, 4.5 to 5.5 or 5 parts by weight of a plant-derived cellulose-containing particulate material. In other words, the paper pulp substitute may comprise 0.1% to 50% CPM, relative to the weight of the waste plant material. Alternatively, the paper pulp substitute may comprise 0.1 to 33% CPM, relative to the weight of the paper pulp substitute as a whole. For example, the paper pulp substitute may comprise up to 0.5%, 1%, 5%, 10%, 15%, 20%, 25%, 30%, or 33% cellulose-containing particulate material.

[0065] The waste plant material and the cellulose-containing particulate material are as described previously with respect to the first aspect, and relevant sections of the first aspect are combinable with the third aspect herein.The waste plant material may comprise particles having a mean particle size of 1 to 500 microns. The paper pulp substitute may comprise particles having a mean particle size of 1 to 500 microns. The paper pulp substitute may comprise particles no greater than 5mm, preferably 4mm, 3mm, 2mm or 1mm.

[0066] According to a fourth aspect of the invention, there is provided the use of a mixture comprising 20 to 80 parts by weight of a waste plant material, and 0.1 to 10 parts by weight of a plant-derived cellulose-containing particulate material as a paper pulp substitute.

[0067] Brief Description of the Figures

[0068] Embodiments of the invention will now be described with reference to the drawings, in which:

[0069] Figure 1 is a graph showing the tensile strengths of a range of comparative composite materials;

[0070] Figure 2 is a particle size distribution (PSD) for a waste plant material;

[0071] Figure 3 is a particle size distribution (PSD) for a waste plant material;

[0072] Figure 4 is a graph showing the tensile strengths of a range of comparative composite materials;

[0073] Figure 4b is a particle size distribution (PSD) for a waste plant material;

[0074] Figure 4c is a graph showing the tensile strengths of a range of comparative and exemplary composite materials;

[0075] Figure 4d is a graph showing the hydrophobicity of a range of comparative and exemplary composite materials;

[0076] Figure 5 is a graph showing the hydrophobicity of a range of comparative and exemplary composite materials;

[0077] Figures 6 and 7 are graphs showing fluid loss of a range of comparative and exemplary composite materials;

[0078] Figures 8a and 8b are PSDs for waste plant materials;

[0079] Figures 9a and 9b are graphs showing the tensile strengths of a range of comparative and exemplary composite materials;

[0080] Figure 9c is a graph showing the hydrophobicity of a range of comparative and exemplary composite materials;

[0081] Figure 10a and 10b are graphs showing the tensile strength and hydrophobicity of comparative and exemplary composite materials;Figure 11a and 11b are graphs showing the tensile strength and hydrophobicity of comparative and exemplary composite materials;

[0082] Figure 12a and 12b are graphs showing the tensile strength and hydrophobicity of comparative and exemplary composite materials;

[0083] Figure 13a and 13b are graphs showing the tensile strength and hydrophobicity of comparative and exemplary composite materials;

[0084] Figure 14a and 14b are graphs showing the tensile strength and hydrophobicity of comparative and exemplary composite materials; and

[0085] Figure 15a and 15b are graphs showing the tensile strength and hydrophobicity of comparative and exemplary composite materials.

[0086] Detailed Description of the Invention

[0087] In addition to well known agricultural and industrial waste plant materials, a number of potential waste plant materials are produced as a byproduct of food processing.

[0088] For example, the main by-product resulting from the production of malt whisky is spent grain or draff, which is essentially the starch-depleted waste grains that remain after the mashing stage. Draff typically comprises peel, pericarp, and seeds with high levels of cellulose, hemicellulose, lignin, protein, fibres, residual starches and sugars, i.e. unfermented carbohydrates, alongside minor quantities of lipids, in particular fats and oils, and minerals, depending on the grain source. Cellulose and hemicellulose are structural polysaccharides that provide fibrous strength; lignin is a complex organic polymer that adds rigidity to plant cell walls. Due to its high moisture content, draff has a short shelf life and is prone to microbial contamination, which limits its use and suitability for long-distance transport.

[0089] The term “draff” herein refers to whisky draff and distillers' spent grain (DSG). Distillers' spent grain is a broader term that applies to all distilled grain spirits, whereas whisky draff is more specific to whisky production, particularly in Scotland. This byproduct is often used as animal feed, for biofuel production, or in sustainable packaging and agriculture.

[0090] The term “draff” herein also comprises spent grain from beer production (brewers' spent grain, or BSG) that has a similar composition to distillers' spent grain (DSG) from whisky production, but with some key differences. Both are by-products of mashing, consisting mainly of grain husks, fibre, protein, and residual starch, and both have high moisture content in a typical range of from 75 to 85% by weight, and both are rich in cellulose, hemicellulose, lignin, and proteins, making them useful as animal feed, biofuels, or in food applications. BSG oftenretains more fermentable sugars since it is often removed through a lautering step after the mash but before fermentation. Although lautering the mash is a very common method in beer production, it is not always employed and some beers undergo fermentation on the mash i.e. with the grain present and with a filtration step after fermentation. DSG usually comprises a lower sugars content than BSG since it has undergone fermentation directly, whereby a yeast strain has been employed to consume most of the available carbohydrates.

[0091] In addition, other sources of waste plant material may include the retentate of biomass that has been subjected to fermentation or at least mashing, such as draff derived from cereals, such as corn, wood, sugar palms, nypa palm, cassava, milo, sorghum, sweet potatoes, molasses, tubers, roots, stems, sago, cassava, tapioca, rice peas, beans, potatoes, beets, fruits, pits, sorghum, sugar cane, rice, wheat, whole grains, rye, barley, bamboo, seeds, oats, flower heads, algae, seaweed or a combination thereof, or a derivative or byproduct thereof. In some embodiments, the derivative or byproduct thereof comprises corn mash, bagasse, distiller's grains, distiller's dried solubles, distiller's dried grains, condensed distiller's solubles, distiller's wet grains, and / or distiller's dried grains with solubles.

[0092] The composite material is formulated by combining waste plant material with paper pulp and a plant-derived cellulose particulate material in a controlled manner. The steps of fabrication may include the pre-treatment of waste plant material: drying and milling the waste plant material to a specified particle size to ensure uniformity in the final composite; addition of the plant-derived cellulosic particulate either by direct blending, impregnation, or surface coating, depending on the additive.

[0093] Increasing the amount of plant-derived cellulose particulate material beyond 5% wt may result in improved water resistance but requires optimization to avoid compromising mechanical properties.

[0094] Compression and Curing: The mixture is subjected to heat and / or pressure to form a solid composite with desired mechanical properties.

[0095] Experiments and Examples

[0096] Methodology

[0097] In the following experiments, the following processes were followed unless otherwise described.Preparation of plant derived cellulose particulate material (CPM)

[0098] A feedstock consisting of either fresh pressed pulp (25%w / w solids) or dry pulp or pellets (89%w / w solids) of sugar beet was added to a mixing and heating vessel. Water was added to the vessel until a hydration level of 10-25% solids was reached. The content of the vessel was heated to 97°C while being mixed. Pre-heated water can be mixed with the feedstock to reduce heating demands within the vessel if available. Hydrogen peroxide (35% solution) at a ratio of 1 part peroxide to 10 parts feedstock solids is added to the vessel at the start of the heating phase, although no reaction occurs until the mixture reaches 85°C. Once 97°C was reached, the hot mixture is passed to a mixing screw whereby it is maintained at 97°C which being mixed thoroughly for an average residence time of 30-45 minutes. The exothermic nature of the reaction meant that minimal further heating was needed and any pressure buildup vented to remove e.g. gas products. The reacted mixture was then washed to remove any grit and soluble breakdown material - approximately 50% of the solid weight is removed compared to the starting feedstock. The material was then pressed to reduce the water content to the level desirable for milling. The washed and pressed material is then milled using a colloid mill with a gap size of 100-300 microns to achieve a particulate material (CPM) with a mean diameter of 50-100 microns. The CPM exiting the mill comprised a paste with a solids content of 10-25%. The milling process heated the CPM to 60-90°C, and thus the CPM was cooled and a food preservative (potassium sorbate) added by spraying before the material was packaged for storage.

[0099] Initial waste plant material processing

[0100] Waste plant material (draff barley, DSG) was obtained from the Holyrood Distillery, having been pre-treated with chemical preservative (ProSid™ Ml 700 CAS: 79-09-4; obtained from Perstorp Group) at source. ProSid™ Ml 700 comprises a combination of propionic acid glycerols and propionic acid. The chemical preservative is used to inhibit mould and yeasts growth in the draff. The waste plant material was frozen on receipt and allowed to defrost overnight prior to use.

[0101] The draff received consisted of a slurry comprising approximately 30% solids by weight and was diluted to approximately 15% by weight in water. The diluted slurry was milled using a high-shear colloidal mill for 2 minutes using a mill having a gap size set to 150|jm. Alternative waste plant materials were subjected to the same processing steps to ensure accurate comparisons.Alternatively, when using a Silverson high-shear mixer, the samples were blended for 10 minutes on each head at 7000rpm. The resulting material was then drained overnight to remove excess water before being stored in sealed containers in a fridge.

[0102] Sample composite material production

[0103] Discs comprising 9g of dry solids were made using various combinations of waste plant material, kraft pulp, and an additive comprising a plant-derived cellulose particulate material as discussed below.

[0104] Firstly, the kraft pulp was blended in 1L of water for 3 minutes on medium speed before incorporating the waste plant material and optional additive and blending for a further 3 minutes at the same speed. The mixture was allowed to stand for 2 minutes before vacuum filtering using a 100pm gap size mesh filter. The vacuum was operated for 2 minutes to ensure the samples were sufficiently drained. The discs of the drained mixture were then hot pressed between sponges at 0.5T constant pressure for 1 minute, having slowly ramped to this pressure to allow steam to release. Subsequently, the pressed discs were subjected to a 3 minute press at 2.5T between filter paper and hot plates. The final disc was removed from the press and dried at 160°C for 2 hours to yield the samples tested.

[0105] Tensile strength testing

[0106] Sample discs produced via the method above were cut into test strips in the shape of a dumbbell. Small tabs of coarse sandpaper were stuck to each end of the test strip using superglue and allowed to dry for 2 hours. The strips were then tested using an Instron™ 3342 Universal Testing System set to measure tensile strength.

[0107] Coating of sample discs

[0108] Sample discs were coated on a single side using a “pour and dump” method. The sample discs were held at an angle, the coating was poured over the surface, and allowed to drain off. Once the whole sample disc was covered, it was allowed to dry at an angle at room temperature overnight before curing in the oven for 5 minutes at the specified temperature for the coating used.

[0109] Liquid resistance testingSample discs were cut into small sections and placed over an end of an open nylon tube to close the opening. The sample was sealed to the surface using a silicone product, and left to cure for 24 hours before the tubes were filled with the test liquid. An aluminium plate was located over the open top of the tube and was also sealed with the silicone product. The weight of the sample was monitored over a set period of time. A control was also created comprising an aluminium plate over each end of the tube since theoretically no water vapour should escape through the plate. The observed results were normalised against the control in order to account for any vapour losses through the silicone seal or nylon tube.

[0110] Experiment 1 - Initial investigations

[0111] A series of tests was carried out to investigate the effect of incorporating a waste plant material consisting of draff into a composite material.

[0112] Samples of draff were initially prepared as discussed above using a small Silverson mixer to break up the fibrillar networks and disrupt bonding, as well as reduce particle size. The processed draff was then mixed with kraft pulp at the concentrations shown in Figure 1, with the kraft pulp forming the remainder of the composition, to form sample discs using the process as described above.

[0113] As shown in Figure 1, a sample disc comprising 100% draff material showed the poorest performance. Composite materials comprising a mixture of draff and kraft pulp all showed significantly higher tensile strengths than the pure draff comparison, and all but the highest draff loadings were equal or better than pure kraft pulp.

[0114] In particular, significantly higher tensile strength was observed in composites comprising 30, 40, and 50wt% of draff respectively, with tensile strengths far surpassing that of comparative samples comprising 100% kraft pulp (not shown), which has a strength of approximately 15MPa when prepared as described herein.

[0115] It was thus determined that a significant proportion of the kraft pulp in a material product could be replaced with draff without compromising material performance. This could significantly reduce the reliance on wood pulp for such products and aid with reducing carbon emissions and the sustainability the brewing and distilling industries.A further series of tests was carried out using draff that had not been treated with the chemical preservative. The samples showed a similar trend of increasing and then decreasing strength as the draff content in the composite material was increased, but with a slight overall decrease in tensile strength values compared to the samples tested above. Without wishing to be bound by theory, it is understood that the slight reduction in tensile strength is most likely due to partial breakdown of the material by microbial action.

[0116] The tests were further repeated using draff which had not been blended using the Silverson mixer and without any other processing. The resulting sample materials showed no significant change in tensile strength with draff content and the presence of significantly larger particles appeared to affect the structural integrity of the composites.

[0117] Subsequently, a particle size analysis was carried out on a sample of draff after processing with the Silverson mixer, and the results shown in Figure 2. Although the majority of particles have a diameter less than 100pm, a number of large diameter particles 21, 22 remained. It is suspected that the presence of the larger particles of draff within the composite material lead to a rough surface texture of the composite material and may affect the structural integrity of the material similar to the unprocessed samples. Furthermore, it was suspected that the rough texture would have a negative impact when coating the material with a coating product.

[0118] Experiment 2a - Milling

[0119] In order to avoid the variations in draff particle size observed in samples processed using the Silverson mixer, samples of draff were milled as described previously, other than the draff slurry having been diluted to 10% solids weight before milling rather than the 15% used as per subsequent experiments). After 2 minutes of milling, the particle size distribution (PSD) was measured and the results graphed in Figure 3. The PSD shows a larger proportion of finer particles and reduced content of particles having a diameter greater than 100pm. The difference in PSD was observable visually with composite materials formed therefrom having a smoother surface texture with no visible large particles.

[0120] The tensile strength of composite materials comprising the milled draff was measured using the same process as described above and in Experiment 1. Samples discs formed having varying content of the milled draff and kraft pulp were made and tested, and the results shown in Figure 4a.As shown in Figure 4a, it was found that increasing the content of milled draff in the composite material increased the maximum tensile strength of the composite material up to a maximum of 50% milled draff. Thereafter the tensile strength decreased back to the initial strength level. Furthermore, loading levels of 20-70% or milled draff equalled or surpassed the tensile strength equivalent for a material comprising solely kraft pulp (i.e. approx. 15MPa). Without wishing to be bound by theory, it is understood that by milling the draff there is no compromise in the strength properties of the composite material at 50% loading e.g. when compared to the high-shear mixer processing in Experiment 1. Although the maximum strength values observed were similar between the milled draff and the draff processed with the high-shear mixer, the milled draff produced a more consistent composite material with a smaller range of tensile strengths observed in repeat testing. A further advantage is that milling the draff would allow a significantly higher volume of material to be processed at one time without hindering performance, and could also be configured into a continuous process.

[0121] Experiment 2b - Single pass milling

[0122] A further series of tests were conducted to identify whether the waste plant material processing could be simplified and milled in a single pass, rather than being recirculated in the mill, in order to increase the material throughput. The particle size distribution of a single pass milling process at a gap size of 150 microns is shown in Figure 4b and the consequential tensile strengths are shown in Figure 4c alongside a kraft pulp only control. A range of compositions comprising 40% or 50% of the waste plant material (Distillers draff) and 0% or 5% of the cellulose-containing particulate material (CPM) were tested at a gap size of 100 microns and at 150 microns. The key of Figure 4c shows the gap size of the mill, draff percentage, and CPM percentage if present.

[0123] The testing identified a reduction in strength of the composite material when milling in a single pass compared to the previous recirculation method. The particle size distribution of single pass milled draff is similar to the recirculated equivalent but has a higher mean and is less homogenous - there are more large particles present in the single pass samples. In all samples and for both mill gap sizes tested, the samples comprising 5% CPM were found to have increased strength over those comprising 0% CPM, and significantly higher than the comparative example comprising kraft pulp only. Without wishing to be bound by theory adding CPM appears to stabilise the material so a higher draff loading dose can be achieved with no negative effect in the strength properties of the resulting composite material.Additional testing, as shown in Figure 4d, found the hydrophobicity and droplet contact angles of the composites formed from 40 to 60wt% of single pass milled waste plant material to be similar to those for samples subjected to recirculation in the mill, and in each case, the inclusion of 5% of CPM showed a significant improvement in the hydrophobicity over the 0% CPM samples with equivalent waste plant material content.

[0124] Without wishing to be bound by theory, it was suspected that the overprocessing of the waste plant material in earlier tests, both by with Silverson mixer and via recirculated milling, inadvertently formed particles of the waste plant material with similar strengthening properties to CPM. These tests suggest that although the single pass milling used in the experiment did not achieve the same increases in strength found previously, a product at which is at least comparable if not superior to the previous tests and to the kraft pulp control can be made by incorporating the CPM into the material along with the minimally processed waste plant material. The minimal processing of the waste plant material is particularly desirable due to the increased throughput and efficiency of such processes. As shown in Figure 4d, a further benefit of incorporating the CPM is the significant improvements in surface porosity and water absorbency of the resulting material.

[0125] Experiment 5 - Hydrophobicity testing

[0126] A further investigation was carried out to assess the impact of draff and CPM on the porosity of the composite material. A simple droplet absorption test was conducted on a range of composite materials: the first comprised 50wt% draff and 50wt% kraft pulp composite; the remainder comprised 50% by weight draff, up to 5% CPM, and with the balance comprising kraft pulp or recycled pulp. A water droplet was placed via pipette on the surface of the samples and timed until fully absorbed, with longer absorption times indicating greater hydrophobicity / lesser hydrophilicity of the resulting composite material. The results are shown in Figure 5.

[0127] It was found that adding 5% CPM to the composite material significantly increased the hydrophobicity compared to a lower content of 2.5% CPM or no CPM. The hydrophobicity for composite materials comprising recycled pulp at both 2.5% and 5% loading of CPM was far higher than for virgin kraft pulp, presumably due to additives (such as Alkylated ketene dimers) affecting the material properties. Nonetheless, there was a clear, observable trend toward increased hydrophobicity / reduced hydrophilicity with increasing CPM content. Such an increase could be used to achieve thinner coating layers on the composite material due to decreased absorption of the coating into the body of the material.Experiment 6 - Resistance testing

[0128] An investigation was carried out to find out the resistance of the composite materials to liquids, in particular ethanol containing liquids.

[0129] In a first test, a series of composite materials having various draff and CPM contents were prepared and tested alongside a first comparative example (61) material formed from only kraft pulp with no draff or CPM, and a second comparative material comprising 90wt% kraft pulp and 10wt% CPM (62). The composite materials and comparative examples were coated with a polyurethane-based coating material and then subjected to liquid resistance testing according to the processes described previously. In a first test, the liquid used was room temperature tap water, and the results shown in Figure 6. The weight loss of the water was measured over the course of one month and the results normalised to the control (i.e. an identical tube having an aluminium plate sealed to each end.

[0130] As shown in Figure 6, the samples of the composite materials containing draff showed no water loss through the polyurethane coating, with the paper pulp comparative example losing only a fractional amount. The negative weight loss for the draff-containing samples indicated that no water was being lost above the rate of the control i.e. the control losing more water at a higher rate. It was understood that the values observed for the four draff containing composite materials were within the error margins of the scale used.

[0131] In a second test, two samples of composite material were selected comprising 50% draff, 45% kraft pulp, and 5% CPM. A third sample comprising 50% draff, 45% recycled pulp material and 5% CPM was also prepared for testing. The samples were then tested against aqueous solutions of ethanol to assess the suitability of the composite material for storing alcoholic beverages. The samples were coated with a polyurethane-based material known to have good resistance to ethanol as described above, and the liquid resistance test was repeated with three concentrations of ethanol solution. The sample comprising recycled pulp material was used in the test with 60% ethanol solution. The weight loss of the ethanol solutions was measured over 1 month and the results are shown in Figure 7.

[0132] Without wishing to be bound by theory, it is understood that the addition of the CPM helps reduce the porosity and / or hydrophilicity of the composite materials which assists the formation of an effective polyurethane coating layer due to decreased absorption of the coating into the material. The coated composite materials were found to be effective at preventing theloss of the ethanol solutions at all concentrations tested, with a small increase of less than 1% of weight loss with a 20% increase in ethanol concentration. The observed liquid weight loss over a month would be acceptable for a product with limited shelf life, but was deemed insufficient for long term storage of high strength ethanol solutions. It is also understood that the test is a crude measure with potential for the ethanol interactions with the silicone to affect the results.

[0133] Experiment 7a - Alternative draff source

[0134] A series of tests were performed to identify whether there would be observable differences between distillers spent grain (DSG) and brewers spent grain (BSG). Samples BSG comprising malted barley and malted oats was processed as described in Experiment 2a with a mill gap size of 150 microns to ensure an accurate direct comparison, and the particle size distributions recorded in Figures 8a and 8b. Both processed draff samples showed a similar standard curve with the BSG particle size distribution slightly wider than for the DSG. The average particle size for DSG was 70.8pm compared to 59.6pm for BSG. DSG also had more large particles present than the BSG.

[0135] A series of sample discs of composite material were then formed from DSG (82-87) and BSG (92-97) at contents of 40-60wt% and either with or without 5% CPM. The tensile strengths of each of the samples were measured as described previously and are shown in Figures 9a and 9b against a control sample comprising only kraft pulp (81, 91). Similarly to Figures 1 and 4a, the incorporation of the draff results in an increase in tensile strength compared to the kraft pulp control, and are further improved with the addition of 5% CPM.

[0136] As shown in Figure 9c, a hydrophobicity test was carried out for each of the samples (82-87, 92-97). In all cases, the incorporation of 5% of CPM lead to a significant increase in the hydrophobicity of the composite material. Without wishing to be bound by theory, the incorporation of CPM is understood to reduce the porosity of the composite material and thus results in a more hydrophobic material, allowing thinner and more effective coatings to be applied.

[0137] Overall the properties of draff obtained from distilleries and breweries using malted barley (with the potential for small proportions of other malted grains) perform in a similar way and require no process or composition modifications to achieve the same outcome. The addition of CPM significantly increased the strength and hydrophobicity of composite materialscomprising both draff types. Moreover, the optimal loading level for both brewers and distillers draff was 50% draff + 5% CPM.

[0138] Experiment 7b - Alternative waste plant materials

[0139] A final series of experiments were carried out to determine whether the effects observed in composite materials comprising draff would be replicated with alternative sources for waste plant material. Samples were prepared, as described previously, using each of ryegrass, elephant grass, barley straw, rehydrated sugar beet pellets, sugar beet shreds (i.e. a secondary byproduct from sugar manufacturing which had not been compacted into pellet form), as well as samples with both dry and wet draff for comparison.

[0140] Figures 10a&b to 15a&b show the measured tensile strengths and the water absorption of sample composite materials comprising the waste plant materials produced according to a range of different kraft pulp to waste plant matter ratios and CPM contents.

[0141] Figure 10a and 10b show samples which incorporate powdered ryegrass (of the Lolium genus) at 30% and 50%. The ryegrass content resulted in tensile strength measurements that were less than or equal to kraft pulp alone. The addition of CPM to each composition resulted in an increase in strength, with a significant improvement at the higher 50% loading levels of waste plant material. When observing the particle size of the ryegrass material, the majority of particles were less than 100pm with an average particle size of 97.3pm due to the presence of some larger particles. Furthermore, as the loading level of ryegrass increased, the duration for a water droplet to fully absorb into the surface also increased. The addition of CPM significantly increases the absorption duration.

[0142] Figures 11a and 11b show samples which incorporate 50% of elephant grass (Pennisetum purpureum) both with and without CPM. The use of elephant grass resulted in a significant decrease in strength of the resulting composite material, with a subsequent increase due to the inclusion of the CPM. Without wishing to be bound by theory, it is understood that this was due to the pre-processing of the elephant grass - the average particle size of the powder was 53.7um with only a handful of large particle remaining above 150um. It is expected that this loss of strength could be resolved through milling at greater mill gap sizes and testing more loading levels. The hydrophobic test found a modest increase in absorption duration.

[0143] Figures 12a and 12b show samples comprising barley straw (Hordeum vulgare). The barley straw was cut up into small pieces less than 10mm in length and blended with water to breakdown into fine particles. The other components were then incorporated into the mixture and discs formed for testing. The average particle size of the barley straw was 84.5 microns, although there were significantly larger particles present and visible on the surface, some as large as 10mm. It is understood that this is the likely reason for the drop in strength due to the inclusion of the barley straw, and as previous, could be mitigated through better preprocessing and milling. In each case, the inclusion of 5% CPM increased the tensile strength to levels comparable to kraft pulp alone. There was a significant increase in the hydrophobicity of the samples, further increased with the addition of CPM.

[0144] Figures 13a and 13b show a further set of results for samples comprising draff as the waste plant material. Draff barley obtained from Holyrood distillery was incorporated wet or dry into discs and the properties tested. For the dry draff, the material was left in the oven to dry fully then blended into a powder before incorporating into the discs. For wet material this was incorporated directly into the discs with no further processing. It can be seen that drying the draff then attempting to incorporate it into the composite material results in a reduction in strength compared to kraft pulp alone, even with the addition of CPM into the composite. Incorporating the wet draff material significantly increases the tensile strength properties when CPM is present. There are however imperfections on the surface of the composite materials formed from wet draff without CPM that would result in an increased porosity. This is shown in Figure 13b in which only the wet draff and CPM composite material had a significant increase in hydrophobicity. As shown in prior experiments, milling the material can result in improved material properties.

[0145] Figures 14a and 14b show the results for composite materials comprising sugar beet pellets (SBP). French sugar beet pellets were rehydrated over night at approx. 1% and then incorporated directly into discs with and without CPM to mimic the conditions tested above. Incorporating sugar beet pellets at 30% loading level results in a material with equal strength to kraft pulp alone, whereas at 50% of sugar beet there is an increase in tensile strength of the composite material to an average of 22MPa. The addition of CPM improves the strength more in conjunction with a lower loading level of sugar beet than a higher level, suggesting that the increase in strength from incorporating CPM can be mitigated to an extent by high loading levels of sugar beet. Furthermore, there is a significant increase in the duration of water absorption in the composite materials comprising 30% of sugar beet material compared with the equivalent sample with CPM. Interestingly, the duration was similar for 30% sugar beet pellet with CPM and 50% sugar beet pellet.Lastly, Figures 15a and 15b shows the result for materials comprising sugar beet shreds. Shreds were sent from Minnesota (MN Shred) for testing to see if there is a difference in shreds processed in the early season (ESS) or late season (LSS). Addition of 50% early season shreds resulted in a significant increase in the tensile strength and reduction in porosity. An equivalent strength increase can be seen when using shreds from the late season but resulted in more porous material. The addition of CPM further increased the tensile strengths of both materials but only improved the porosity of the late season sample.

[0146] Conclusions

[0147] Overall, it was determined that variety of waste plant materials can be used as a replacement material for wood-derived paper pulp in a variety of composite materials. Said composite materials typically comprise properties that are improved or equal to materials formed from paper pulp alone. A preferred loading for waste plant material within the composite materials was deemed to be approximately 50% by weight, although useful composite materials from 20 to 80% loading of waste plant material were identified. For materials comprising draff and paper pulp, draff contents of 30-50% were preferred, with a 50% draff content being especially preferred.

[0148] Composite materials formed from both virgin paper pulp and recycled pulp were successfully formed having similar structural and material properties.

[0149] Importantly, the addition of CPM to the composite material was found to increase the strength. More significantly, the CPM inclusion was found to significantly reduce the porosity, and thus the water absorbance of the composite material, allowing for thinner, more effective coatings to be applied thereto. A waterproof coating was successfully achieved on composite materials comprising 5% CPM and 50% draff, although it is believed that similar results would be attainable for a range of waste plant material contents. Such coated composite materials showed an ethanol resistance suitable for products with limited shelf lives.

[0150] For composite materials comprising waste plant materials (other than draff) and paper pulp, the incorporation of CPM showed the same general trends as for the draff composites i.e. of increased overall strength and hydrophobicity over paper pulp materials. The Applicant has found that the combination of minimally processed waste plant material and cellulose-containing particulate material can be used as a paper pulp replacement achieving similar or better material properties to conventional paper pulp-derived products.

Claims

Claims1. A composite material comprising:- 20-80 wt% of paper pulp- 20-80 wt% of a waste plant material; and- 0.1-10 wt% of a plant-derived cellulose-containing particulate material.

2. The composite material according to claim 1, wherein the plant-derived cellulose- containing particulate material comprises less than 60 wt% cellulose.

3. The composite material according to claim 1 or claim 2, wherein the plant-derived cellulose-containing particulate material has a non-carbohydrate content of 20 to 50 % by dry weight.

4. The composite material according to any one of claims 1 to 3, wherein the plant-derived cellulose-containing particles have a mean major dimension of from 1 to 250 microns and preferably have a mean major dimension of 10 to 100 microns.

5. The composite material according to any one of the preceding claims, wherein the waste plant material comprises particles having a mean particle size of 1 to 500 microns.

6. The composite material according to any one of the preceding claims, wherein the waste plant material comprises an agricultural byproduct, food processing byproduct, and / or industrial byproduct.

7. The composite material according to claim 6, wherein the waste plant material comprises the retentate of biomass subjected to one or more of: mashing, fermentation, milling, and fibrillating.

8. The composite material according to any one of the preceding claims, wherein the waste plant material comprises one or more of:draff derived from cereals, such as barley, corn, oats, wheat, and such as distillers spent grain and / or brewers spent grain; and / orchaff derived from grain, straw, and / or hay;waste derived from plant oil extraction such as oil plant stems and heads, oilseed cake, and oilseed meal;wood processing byproducts such as sawdust, shavings, and / or woodchip; and other plant fibres and byproducts comprising and / or derived from wood, sugar palms, nypa palm, cassava, milo, sorghum, sweet potatoes, molasses, tubers, roots, stems, sago, cassava, tapioca, rice peas, beans, potatoes, beets, fruits, pits, sorghum, sugar cane, rice, wheat straw, grass, hay, hemp, whole grains, rye, barley, bamboo, seeds flower heads, algae, seaweed, and equisetum.

9. The composite material according to any one of the preceding claims, wherein the waste plant material comprises cellulose, hemicellulose, lignin, proteins, and residual starches.

10. The composite material according to any one of the preceding claims, wherein the paper pulp comprises one or more of: kraft pulp, optionally virgin kraft pulp; other pulp derived from wood fibres, pulp derived from non-wood fibres; and / or recycled paper pulp.

11. The composite material according to any one of the preceding claims, further comprising a binder, and optionally, wherein the binder is a biopolymer resin and / or a natural adhesive.

12. The composite material according to any one of the preceding claims, further comprising a surface coating, optionally, wherein the coating comprises a polyethylene, PET, acrylic, and / or polyurethane-based coating.

13. The composite material according to any one of the preceding claims, wherein the plant- derived cellulose containing particulate material may be formed from a process comprising: (i) contacting herbaceous plant material with a peroxide reagent and optionally water; (ii) heating the mixture from (i) to a temperature of from 30 to 110°C and maintaining said mixture at a temperature of from 30 to 110°C until the pH of the mixture has reached a predetermined pH value; and (iii) isolating the resulting cellulose- containing particulates.

14. A method for producing a composite material according to any one of the preceding claims, the method comprising:a) mixing a waste plant material with paper pulp and a plant-derived cellulose- containing particulate material to form a mixture; andb) drying and / or compressing the mixture to form a solid composite material.

15. The method according to claim 14, further comprising drying and milling the waste plant material to a desired particle size prior to mixing with paper pulp and the plant- derived cellulose-containing particulate material.

16. The method according to claim 14 or 15, further comprising coating the solid composite material with a coating material, optionally, a polyurethane based coating material.

17. A paper pulp substitute for use in forming composite materials according to any one of claims 1 to 13, the paper pulp substitute comprising:20 to 80 parts by weight of a waste plant material; and0.1 to 10 parts by weight of a plant-derived cellulose-containing particulate material.

18. The paper pulp substitute according to claim 17, wherein the waste plant material comprises particles having a mean particle size of 1 to 500 microns.

19. The use of a mixture comprising 20 to 80 parts by weight of a waste plant material, and 0.1 to 10 parts by weight of a plant-derived cellulose-containing particulate material as a paper pulp substitute.