A corundum-SiAlON-silicon nitride gradient brick for sulfur recovery reactor and its preparation process
By adopting the gradient design of corundum-SiAlON-silicon nitride gradient composite refractory bricks, the deformation and collapse of the inner lining material of the sulfur recovery reactor is solved, and high strength, thermal shock resistance and thermal insulation effect are achieved, reducing mold cost and transaction The freight construction period improves the versatility of bricks.
Patent Information
- Application Number
- CN201810800176.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2018-07-20
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2038-07-20
AI Technical Summary
The lining materials of existing sulfur recovery reactors are prone to deform during long-term thermal load operation, resulting in compaction collapse of the second and third layers of lightweight refractory materials, causing deformation of the lining structure and brick collapse risk, and arc-shaped bricks The customization cost is high and not versatile, and the mold is seriously wasted.
Corundum-SiAlON-silicon nitride gradient composite refractory bricks are used to design the raw material ratios between the working layer and the non-working layer through gradient design, forming isosceles trapezoidal bricks. The working layer and the non-working layer gradually transition from the gradient, combined with aluminum sol as The bonding agent improves the mechanical properties and thermal conductivity of the overall brick.
It achieves high strength and thermal shock resistance in high temperature, pressure and corrosion environments, and has good insulation effect, avoids deformation and collapse accidents of bricks, reduces mold costs and delivery periods, and improves the versatility of bricks. and inventory stocking capacity.
Smart Images

Figure CN110734042B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a corundum-SiAlON-silicon nitride gradient composite refractory brick for a sulfur recovery reactor and a preparation process thereof, belonging to the field of refractory materials. Background Art
[0002] A large amount of H2S toxic gas is produced during the crude oil refining process of petrochemical enterprises, which is extremely harmful to the human body and the environment. The sulfur recovery reactor converts the combined sulfur in sulfur-containing gases such as H2S into elemental sulfur, and burns the very small amount of residual H2S in the tail gas to recover sulfur dioxide, turning waste into treasure. The sulfur recovery reactor is used in a relatively harsh operating environment. There are dangerous factors such as high temperature, temperature fluctuation, pressure, corrosion, and explosion, and the flue gas composition is complex. Therefore, the refractory lining of the reactor is required to be high. Refractory materials with high strength, good corrosion resistance, and good thermal shock resistance are required. At present, the lining refractory materials used in sulfur recovery reactors are usually three layers: the first layer is heavy bricks, using zirconium corundum mullite bricks, and its volume density is 2.9~3.2g·cm -1 , compressive strength ≥ 100MPa, thermal conductivity ≤ 1.5W·m -1 ·K -1 , or chrome corundum bricks, with a volume density of about 3.0g cm -1 , compressive strength ≥ 80MPa, thermal conductivity ≤ 1.8W·m -1 ·K -1 The thickness is about 150mm; the second layer is lightweight bricks, using lightweight thermal insulation mullite bricks, with a volume density of 1.1~1.3g·cm -1 , compressive strength ≥ 8MPa, thermal conductivity ≤ 0.45W·m -1 ·K -1 , with a thickness of about 100~150mm; the third layer is a heat-insulating castable, which uses a high-aluminum lightweight castable with a bulk density of 0.95~1.1g·cm -1 , compressive strength ≥ 6MPa, thermal conductivity ≤ 0.25W·m -1 ·K -1 , with a thickness of about 100 mm. The schematic diagram of the refractory material lining of the sulfur recovery unit is shown in Figure 1 and Figure 2 As shown in the figure, the advantages of the three-layer refractory design are: the first layer of heavy refractory bricks has high strength, good wear resistance and corrosion resistance, and can withstand harsh working environments; the second layer of lightweight insulation bricks has low thermal conductivity, small heat capacity, and good thermal insulation effect; the third layer of lightweight castables has low thermal conductivity, good thermal insulation effect, and strong shape adaptability. However, this three-layer design still has obvious defects: due to the low strength of the second and third layers of lightweight refractory materials, in long-term heat load operation, the second and third layers at the bottom of the sulfur recovery reactor are often compacted and collapsed, causing the lining structure to deform from the original round to an elliptical shape, such as Figure 3 shown.
[0003] In order to eliminate the hidden danger of lining brick collapse caused by brick falling due to deformation, the refractory bricks are made of large curved bricks (such as Figure 4 ), the large angle slope surface extrusion stress and friction of the large volume curved brick can resist the gravity and load of the heavy brick (force analysis such as Figure 4 ), in order to eliminate the hidden dangers of brick falling and collapse. However, large curved bricks must be customized according to the diameter of each reactor. The slopes of curved bricks of different diameters are different. Therefore, different diameters must use molds that are suitable for the diameter, resulting in great waste of molds and high costs. And when there is an order, the mold must be opened before production, resulting in a very tight delivery schedule. When there is no order, the tunnel kiln used for sintering products runs idle, resulting in a great waste of fuel.
[0004] By using two or three small trapezoidal bricks (such as Figure 5 ) can adapt to different diameters without the need to open molds separately according to the diameter of each reactor, which can reduce mold costs and save delivery time. In addition, small trapezoidal bricks can adapt to the diameters of different kilns, solve the problem of variable diameters, and can be used as standard bricks. Even when there are no orders, they can be produced and kept in stock, so that the tunnel kiln will not run idle and waste fuel. However, since the current sulfur recovery reactor adopts a three-layer design, the second and third layers of the reactor lining are lightweight refractory materials, and deformation is inevitable. The extrusion stress and friction of the small-angle slope surface of the small trapezoidal bricks are not enough to resist the gravity and load of the heavy bricks (force analysis such as Figure 5 ), there are bound to be hidden dangers of falling bricks and kiln collapse accidents.
[0005] There is only one prerequisite to eliminate the falling of small trapezoidal bricks, that is, the second and third layers must not be deformed, the load base must be strong enough, and the lightweight refractory materials cannot meet the requirement of sufficiently high strength after long-term hot operation. Therefore, the solution can only be to abandon the idea of the currently commonly used three-layer design, that is, no longer adopt the design of the first layer of heavy bricks, the second layer of lightweight bricks, and the third layer of lightweight castables, but adopt an overall design method. To achieve the design of an overall brick, it is necessary to meet both the harsh process conditions of service and the effects of energy saving and heat preservation. The gradient material design idea can solve this problem. The present invention invented a corundum-SiAlON-silicon nitride gradient brick based on the gradient design idea. The performance of the working layer meets the harsh working conditions of the reactor, and has a good thermal insulation effect in the non-working layer. The working layer to the non-working layer of the whole brick gradually transitions by a gradient. Summary of the invention
[0006] The present invention is a corundum-SiAlON-silicon nitride gradient composite refractory brick for a sulfur recovery reactor. The refractory brick is a trapezoidal brick with an isosceles trapezoidal longitudinal section and a height of 300-400 mm. The upper bottom surface and the lower bottom surface are both rectangular or square, and the side lengths of the upper bottom surface and the lower bottom surface are 80-100 mm. There are a working layer, a transition layer 1, a transition layer 2, and a non-working layer in the vertical direction from the upper bottom surface to the lower bottom surface, wherein the raw material ratios of the working layer and the non-working layer are different, and the transition layer 1 is formed by mixing the raw materials of the working layer and the non-working layer in a weight ratio of 2:1; the transition layer 2 is formed by mixing the raw materials of the working layer and the non-working layer in a weight ratio of 1:2. The thickness ratio of the working layer, the transition layer 1, the transition layer 2, and the non-working layer arranged in the vertical direction from the upper bottom surface to the lower bottom surface is 2:1:1:2.
[0007] The raw materials used for the refractory bricks include: (1) plate-shaped corundum with a particle size of 4-2 mm and 2-1 mm, mesoporous alumina with a particle size of 1-0.5 mm and 0.5-0.088 mm, and silicon nitride with a particle size of 0.5-0.088 mm as a skeleton; (2) hollow alumina balls with a particle size of 3-2 mm and 2-1 mm; (3) plate-shaped corundum powder with a particle size of ≤0.045 mm and SiAlON powder with a particle size of ≤0.045 mm as a matrix; (4) silicon nitride powder with a particle size of ≤0.020 mm; (5) Suzhou white clay with a particle size of ≤0.010 mm; (6) magnesium carbonate powder with a particle size of ≤0.010 mm; and (7) aluminum sol binder.
[0008] The raw materials of the refractory brick working layer are calculated by weight percentage, and the formula is as follows:
[0009] (1) Tabular corundum with a particle size of 4 to 2 mm, 8 to 11%;
[0010] (2) Tabular corundum with a particle size of 2 to 1 mm, 12 to 22%;
[0011] (3) Mesoporous alumina with a particle size of 1 to 0.5 mm, 9 to 13%;
[0012] (4) Mesoporous alumina with a particle size of 0.5-0.088 mm, 15-20%;
[0013] (5) Silicon nitride with a particle size of 0.5~0.088mm, 5~8%;
[0014] (6) Tabular corundum with a particle size of ≤0.045 mm, 16-19%;
[0015] (7) SiAlON with a particle size of ≤0.045 mm, 5-10%;
[0016] (8) Silicon nitride powder with a particle size of ≤0.020 mm, 8-15%;
[0017] (9) Suzhou white mud with particle size ≤ 0.010 mm, 1~2%;
[0018] (10) Added aluminum sol, 2.5~3%.
[0019] The raw materials of the non-working layer of the refractory bricks are calculated by weight percentage and the formula is as follows:
[0020] (1) Alumina hollow balls with a particle size of 3~2mm, 9~12%;
[0021] (2) Hollow alumina balls with a particle size of 2~1 mm, 20~38%;
[0022] (3) Mesoporous alumina with a particle size of 1 to 0.5 mm, 9 to 21%;
[0023] (4) Mesoporous alumina with a particle size of 0.5-0.088 mm, 15-19%;
[0024] (5) Andalusite with particle size ≤ 0.045 mm, 12-15%;
[0025] (6) Suzhou white mud with particle size ≤ 0.010 mm, 8-13%;
[0026] (7) Magnesium carbonate with a particle size of ≤0.010 mm, 3-6%;
[0027] (8) Added aluminum sol, +2.5~3%.
[0028] The preparation process of the above refractory bricks is:
[0029] (1) Batching and mixing. Weigh the required raw materials in proportion, and batch and mix them separately according to the proportions of the working layer, gradient transition layer 1, gradient transition layer 2, and non-working layer.
[0030] Working layer: Pre-mix 98 plate-shaped corundum with a particle size of ≤0.045mm, SiAlON powder with a particle size of ≤0.045mm, andalusite with a particle size of ≤0.45mm, silicon nitride powder with a particle size of ≤0.020mm, and Suzhou white mud with a particle size of ≤0.010mm for 20 minutes, and record it as A powder for use. Mix 98 plate-shaped corundum with a particle size of 4~2mm and 2~1mm, mesoporous alumina with a particle size of 1~0.5mm and 0.5~0.088mm, and silicon nitride powder with a particle size of 0.5~0.088mm for 15~20 minutes, add aluminum sol as a binder, and then add the pre-mixed A powder, and wet-mill together for 30 minutes.
[0031] Non-working layer: Pre-mix andalusite with a particle size of ≤0.45mm, Suzhou white mud with a particle size of ≤0.010mm, and magnesium carbonate with a particle size of ≤0.010mm for 20 minutes, and record it as B powder for later use. Mix and grind 3~2mm and 2~1mm hollow alumina balls, mesoporous alumina with a particle size of 1~0.5mm, and mesoporous alumina with a particle size of 0.5~0.088 mm for 15~20 minutes, add aluminum sol as a binder, and then add the pre-mixed B powder, and wet grind together for 30 minutes.
[0032] Gradient transition layer 1: Mix 2 weights of material A and 1 weight of material B. The fine powder premixing and co-grinding process is the same as that of material A and material B.
[0033] Gradient transition layer two: Mix 1 weight of material A and 2 weights of material B, and premix and wet grind the fine powder in the same way as the process for material A and material B.
[0034] (2) Molding. Use cardboard to divide the mold into four areas. Pour material A, transition layer one, transition layer two, and B into the four areas in the order of working layer, gradient transition layer one, gradient transition layer two, and non-working layer. After spreading and flattening, pull out the cardboard and perform machine pressing or hydraulic molding.
[0035] (3) Drying: Dry the bricks at 120°C for 48 to 72 hours.
[0036] (4) Sintering: Sinter at 1450~1520℃ for 3~4h.
[0037] The performance of the refractory brick working layer of the present invention is: volume density 2.7~2.9g·cm -1 , compressive strength ≥ 80MPa, thermal conductivity ≤ 1.3W·m at 1100℃ -1 ·K -1 ; The performance of the non-working layer is: volume density 1.15~1.25g·cm -1 , compressive strength ≥ 20MPa, thermal conductivity ≤ 0.6W·m at 500℃ -1 ·K -1 .
[0038] The refractory bricks of the present invention adopt a gradient transition formula, the working layer, transition layer 1, transition layer 2 and non-working layer have high bonding strength, there is no interface shedding problem between layers, the overall performance of the bricks is good, and has outstanding technical effects.
[0039] (1) The invented corundum-SiAlON-silicon nitride gradient brick has high mechanical strength, good wear resistance, high load softening temperature, good corrosion resistance and good thermal shock resistance in the working layer, and can withstand the high temperature, temperature fluctuation, pressure, corrosion and other harsh working conditions in the sulfur recovery reactor. The non-working layer has high load softening temperature and low thermal conductivity, achieving both thermal insulation function and sufficient support strength without deformation.
[0040] (2) The working layer to the non-working layer gradually transitions by gradient, the interface bonding strength is good, and the integrity of the bricks is good.
[0041] (3) Compared with the heavy materials of the current working layer, zirconium corundum mullite bricks or chrome corundum mullite bricks, they are lower in cost because they do not contain zirconium and are more environmentally friendly because they do not contain chromium.
[0042] (4) The small-sized trapezoidal bricks of the invention have good versatility and can adapt to reactors of different diameters. They can be used as standard bricks for production and inventory, solving the problem that when there are orders for curved bricks, separate molds must be made, which increases costs and delays delivery schedules, while when there are no orders, the tunnel kiln idles, wasting fuel and causing high costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 This is a schematic diagram of the front cross-section (cylindrical) of a sulfur recovery reactor, where 1 is a heavy brick; 2 is a lightweight insulation brick; and 3 is a lightweight castable.
[0044] Figure 2 It is a schematic diagram of the side cross-section (circular ring) of the sulfur recovery reactor, where 1 is a heavy brick; 2 is a lightweight insulation brick; and 3 is a lightweight castable.
[0045] Figure 3 Schematic diagram of the side cross-section of the sulfur recovery reactor after deformation (oval ring), where 1 is a heavy brick; 2 is a lightweight insulation brick; 3 is a lightweight castable.
[0046] Figure 4 Schematic diagram of large curved bricks and their force analysis
[0047] Figure 5 Schematic diagram of small trapezoidal brick and its force analysis
[0048] Figure 6 Schematic diagram of gradient transition formula of gradient brick
[0049] Example 1
[0050] A corundum-SiAlON-silicon nitride gradient composite refractory brick for a sulfur recovery reactor. The refractory brick is a trapezoidal brick with an isosceles trapezoidal longitudinal section and a height of 400 mm. The upper bottom surface and the lower bottom surface are both rectangular or square. The side length of the upper bottom surface is 82 mm, and the side length of the lower bottom surface is 95 mm. There are four refractory layers composed of raw materials with different proportions in the vertical direction from the upper bottom surface to the lower bottom surface. The mass percentage formula of each raw material of the refractory brick working layer is: plate-shaped corundum with a particle size of 4-2 mm, 8%; plate-shaped corundum with a particle size of 2-1 mm, 22%; mesoporous alumina with a particle size of 1-0.5 mm, 9%; mesoporous alumina with a particle size of 0.5-0.088 mm, 15%; silicon nitride with a particle size of 0.5-0.088 mm, 8%; plate-shaped corundum with a particle size ≤0.045 mm, 16%; SiAlON with a particle size ≤0.045 mm, 5%; silicon nitride powder with a particle size ≤0.020 mm, 15%; Suzhou white mud with a particle size ≤0.010 mm, 2%; and added aluminum sol, 3%. The weight percentage formula of each raw material of the non-working layer is: hollow alumina balls with a particle size of 3~2mm, 9%; hollow alumina balls with a particle size of 2~1mm, 38%; mesoporous alumina with a particle size of 1~0.5 mm, 9%; mesoporous alumina with a particle size of 0.5~0.088 mm, 15%; andalusite with a particle size of ≤0.045mm, 15%; Suzhou white mud with a particle size of ≤0.010mm, 8%; magnesium carbonate with a particle size of ≤0.010mm, 6%; and additional aluminum sol, 3%. The transition layer 1 is mixed with the raw materials of the working layer and the non-working layer in a weight ratio of 2:1. The transition layer 2 is mixed with the raw materials of the working layer and the non-working layer in a weight ratio of 1:2. The ingredients are prepared and mixed according to the above proportions. Working layer material: Pre-mix 98 plate-shaped corundum with a particle size of ≤0.045mm, SiAlON powder with a particle size of ≤0.045mm, andalusite with a particle size of ≤0.45mm, silicon nitride powder with a particle size of ≤0.020mm, and Suzhou white mud with a particle size of ≤0.010mm for 20 minutes, and record it as A1 powder for later use. Mix 98 plate-shaped corundum with a particle size of 4~2mm and 2~1mm, mesoporous alumina with a particle size of 1~0.5mm and 0.5~0.088mm, and silicon nitride powder with a particle size of 0.5~0.088mm for 15 minutes, add aluminum sol as a binder, and then add the pre-mixed A1 powder, and wet-mill together for 30 minutes. Non-working layer B1 material: Pre-mix andalusite with a particle size of ≤0.45mm, Suzhou white mud with a particle size of ≤0.010mm, and magnesium carbonate with a particle size of ≤0.010mm for 20 minutes, and record it as B1 powder for standby. Mix 3~2mm and 2~1mm hollow alumina balls, mesoporous alumina with a particle size of 1~0.5 mm, and mesoporous alumina with a particle size of 0.5~0.088 mm for 15 minutes, add aluminum sol as a binder, and then add the premixed B1 powder, and wet-mill together for 30 minutes. Gradient transition layer 1: Mix 2 weights of A1 material and 1 weight of B1 material. The fine powder premixing and mixing process is the same as that of A1 material and B1 material.Gradient transition layer 2: Mix 1 weight of A1 material and 2 weights of B1 material, and premix and wet grind the fine powder in the same way as A1 and B1 materials. Use cardboard to divide the mold into four areas, and pour A1 material, transition layer 1 material, transition layer 2 material, and B1 material into the four areas in the order of working layer, gradient transition layer 1, gradient transition layer 2, and non-working layer. After spreading and flattening, pull out the cardboard, press or hydraulically form the bricks, dry the bricks at 120℃ for 48h, and sinter at 1450℃ for 4h. The performance parameters of the sintered refractory brick working layer are: volume density 2.89g·cm. -1 , room temperature compressive strength 92MPa, thermal conductivity 1.29W·m·K at 1100℃ -1 ; Non-working layer: volume density 1.17g·cm -1 , room temperature compressive strength 22MPa, thermal conductivity 0.55W·m·K at 500℃ -1 .
[0051] Example 2
[0052] A corundum-SiAlON-silicon nitride gradient composite refractory brick for a sulfur recovery reactor. The refractory brick is a trapezoidal brick with an isosceles trapezoidal longitudinal section and a height of 380 mm. The upper bottom surface and the lower bottom surface are both rectangular or square. The side length of the upper bottom surface is 87 mm, and the side length of the lower bottom surface is 99 mm. There are four refractory layers composed of raw materials with different proportions in the vertical direction from the upper bottom surface to the lower bottom surface. The mass percentage formula of each raw material of the refractory brick working layer is: plate-shaped corundum with a particle size of 4-2 mm, 8%; plate-shaped corundum with a particle size of 2-1 mm, 19%; mesoporous alumina with a particle size of 1-0.5 mm, 11%; mesoporous alumina with a particle size of 0.5-0.088 mm, 17%; silicon nitride with a particle size of 0.5-0.088 mm, 7%; plate-shaped corundum with a particle size ≤0.045 mm, 18%; SiAlON with a particle size ≤0.045 mm, 7%; silicon nitride powder with a particle size ≤0.020 mm, 12%; Suzhou white mud with a particle size ≤0.010 mm, 1%; and added aluminum sol, 3%. The weight percentage formula of each raw material of the non-working layer is as follows: hollow alumina balls with a particle size of 3~2mm, 10%; hollow alumina balls with a particle size of 2~1mm, 32%; mesoporous alumina with a particle size of 1~0.5 mm, 13%; mesoporous alumina with a particle size of 0.5~0.088 mm, 16%; andalusite with a particle size of ≤0.045mm, 14%; Suzhou white mud with a particle size of ≤0.010mm, 10%; magnesium carbonate with a particle size of ≤0.010mm, 5%; and additional aluminum sol, 3%. The transition layer 1 is formed by mixing the raw materials of the working layer and the non-working layer in a weight ratio of 2:1. The transition layer 2 is formed by mixing the raw materials of the working layer and the non-working layer in a weight ratio of 1:2. The ingredients and materials are prepared and mixed according to the above proportions. For the working layer material, 98 plate-shaped corundum with a particle size of ≤0.045mm, SiAlON powder with a particle size of ≤0.045mm, andalusite with a particle size of ≤0.45mm, silicon nitride powder with a particle size of ≤0.020mm, and Suzhou white mud with a particle size of ≤0.010mm are mixed vigorously for 20 minutes in advance and recorded as A2 powder for later use. 98 plate-shaped corundum with a particle size of 4~2mm and 2~1mm, mesoporous alumina with a particle size of 1~0.5mm and 0.5~0.088mm, and silicon nitride powder with a particle size of 0.5~0.088mm are mixed vigorously for 20 minutes, aluminum sol is added as a binder, and then the pre-mixed A2 powder is added, and wet-milled together for 30 minutes. Non-working layer material: Mix andalusite with a particle size of ≤0.45mm, Suzhou white mud with a particle size of ≤0.010mm, and magnesium carbonate with a particle size of ≤0.010mm for 20 minutes in advance, and record it as B2 powder for later use. Mix and grind 3~2mm and 2~1mm hollow alumina balls, mesoporous alumina with a particle size of 1~0.5mm, and mesoporous alumina with a particle size of 0.5~0.088mm for 20 minutes, add aluminum sol as a binder, and then add the pre-mixed B2 powder, and wet grind together for 30 minutes.Gradient transition layer 1: Mix 2 weights of A2 material and 1 weight of B2 material, and premix and wet grind the fine powder in the same way as A2 and B2 materials. Gradient transition layer 2: Mix 1 weight of A2 material and 2 weights of B2 material, and premix and wet grind the fine powder in the same way as A2 and B2 materials. Use cardboard to divide the mold into four areas, and pour A2 material, transition layer 1 material, transition layer 2 material, and B2 material into the four areas in the order of working layer, gradient transition layer 1, gradient transition layer 2, and non-working layer. After spreading and flattening, pull out the cardboard, press or hydraulically form, dry the bricks at 120℃ for 72h, and sinter at 1520℃ for 3h. The performance parameters of the sintered refractory brick working layer are: volume density 2.88g·cm. -1 , room temperature compressive strength 90MPa, thermal conductivity 1.29W·m·K at 1100℃ -1 ; Non-working layer: volume density 1.18g·cm -1 , room temperature compressive strength 28MPa, thermal conductivity 0.55W·m·K at 500℃ -1 .
[0053] Example 3
[0054] A corundum-SiAlON-silicon nitride gradient composite refractory brick for a sulfur recovery reactor. The refractory brick is a trapezoidal brick with an isosceles trapezoidal longitudinal section and a height of 350 mm. The upper bottom surface and the lower bottom surface are both rectangular or square. The side length of the upper bottom surface is 85 mm, and the side length of the lower bottom surface is 98 mm. There are four refractory layers composed of raw materials with different ratios in the vertical direction from the upper bottom surface to the lower bottom surface. The mass percentage formula of each raw material of the refractory brick working layer is: plate-shaped corundum with a particle size of 4-2 mm, 9%; plate-shaped corundum with a particle size of 2-1 mm, 16%; mesoporous alumina with a particle size of 1-0.5 mm, 12%; mesoporous alumina with a particle size of 0.5-0.088 mm, 18%; silicon nitride with a particle size of 0.5-0.088 mm, 6%; plate-shaped corundum with a particle size ≤0.045 mm, 19%; SiAlON with a particle size ≤0.045 mm, 8%; silicon nitride powder with a particle size ≤0.020 mm, 10%; Suzhou white mud with a particle size ≤0.010 mm, 2%; and added aluminum sol, 2.5%. The weight percentage formula of the non-working layer raw materials is: hollow alumina balls with a particle size of 3~2mm, 11%; hollow alumina balls with a particle size of 2~1mm, 26%; mesoporous alumina with a particle size of 1~0.5 mm, 17%; mesoporous alumina with a particle size of 0.5~0.088 mm, 17%; andalusite with a particle size of ≤0.045mm, 13%; Suzhou white mud with a particle size of ≤0.010mm, 12%; magnesium carbonate with a particle size of ≤0.010mm, 4%; and additional aluminum sol, 2.5%. The transition layer 1 is formed by mixing the working layer and non-working layer raw materials in a weight ratio of 2:1. The transition layer 2 is formed by mixing the working layer and non-working layer raw materials in a weight ratio of 1:2. The ingredients are prepared and mixed according to the above proportions. For the working layer material, 98 plate-shaped corundum with a particle size of ≤0.045mm, SiAlON powder with a particle size of ≤0.045mm, andalusite with a particle size of ≤0.45mm, silicon nitride powder with a particle size of ≤0.020mm, and Suzhou white mud with a particle size of ≤0.010mm are mixed vigorously for 20 minutes in advance and recorded as A3 powder for later use; 98 plate-shaped corundum with a particle size of 4~2mm and 2~1mm, 1~0.5mm, 0.5~0.08 Mesoporous alumina with a particle size of 8mm and silicon nitride powder with a particle size of 0.5~0.088mm are vigorously mixed and ground for 20 minutes, aluminum sol is added as a binder, and then the premixed A3 powder is added, and wet-ground for 30 minutes; non-working layer material: andalusite with a particle size ≤0.45mm, Suzhou white mud with a particle size ≤0.010mm, and magnesium carbonate with a particle size ≤0.010mm are vigorously mixed for 20 minutes in advance, recorded as B3 powder for later use, 3~2㎜, 2~1㎜ alumina hollow balls, mesoporous alumina with a particle size of 1~0.5 mm, and mesoporous alumina with a particle size of 0.5~0.088 mm are vigorously mixed and ground for 20 minutes, aluminum sol is added as a binder, and then the premixed B3 powder is added, and wet-ground for 30 minutes.Gradient transition layer 1: Mix 2 weights of A3 material and 1 weight of B3 material, and premix and co-mill the fine powder in the same way as A3 and B3 materials. Gradient transition layer 2: Mix 1 weight of A3 material and 2 weights of B3 material, and premix and wet-mill the fine powder in the same way as A3 and B3 materials. Use cardboard to divide the mold into four areas, and pour A3 material, transition layer 1 material, transition layer 2 material, and B3 material into the four areas in the order of working layer, gradient transition layer 1, gradient transition layer 2, and non-working layer. After spreading and flattening, pull out the cardboard, press or hydraulically form, dry the bricks at 120°C for 72 hours, and sinter at 1490°C for 3~4 hours. The performance parameters of the sintered refractory brick working layer are: A3 working layer: volume density 2.85g·cm. -1 , room temperature compressive strength 88MPa, thermal conductivity 1.28W·m·K at 1100℃ -1 ; Performance parameters of B3 non-working layer are: volume density 1.19g·cm -1 , room temperature compressive strength 24MPa, thermal conductivity 0.56W·m·K at 500℃ -1 .
[0055] Example 4
[0056] A corundum-SiAlON-silicon nitride gradient composite refractory brick for a sulfur recovery reactor. The refractory brick is a trapezoidal brick with an isosceles trapezoidal longitudinal section and a height of 300 mm. The upper bottom surface and the lower bottom surface are both rectangular or square. The side length of the upper bottom surface is 83 mm, and the side length of the lower bottom surface is 98 mm. There are four refractory layers composed of raw materials with different proportions in the vertical direction from the upper bottom surface to the lower bottom surface. The mass percentage formula of each raw material of the refractory brick working layer is: plate-shaped corundum with a particle size of 4-2 mm, 11%; plate-shaped corundum with a particle size of 2-1 mm, 12%; mesoporous alumina with a particle size of 1-0.5 mm, 13%; mesoporous alumina with a particle size of 0.5-0.088 mm, 20%; silicon nitride with a particle size of 0.5-0.088 mm, 5%; plate-shaped corundum with a particle size ≤0.045 mm, 19%; SiAlON with a particle size ≤0.045 mm, 10%; silicon nitride powder with a particle size ≤0.020 mm, 8%; Suzhou white mud with a particle size ≤0.010 mm, 2%; and additional aluminum sol, 2.5%. The weight percentage formula of the non-working layer raw materials is: hollow alumina balls with a particle size of 3~2mm, 12%; hollow alumina balls with a particle size of 2~1mm, 20%; mesoporous alumina with a particle size of 1~0.5mm, 21%; mesoporous alumina with a particle size of 0.5~0.088mm, 19%; andalusite with a particle size of ≤0.045mm, 12%; Suzhou white mud with a particle size of ≤0.010mm, 13%; magnesium carbonate with a particle size of ≤0.010mm, 3%; and aluminum sol, 2.5%. The transition layer 1 is formed by mixing the working layer and the non-working layer raw materials in a weight ratio of 2:1. The transition layer 2 is formed by mixing the working layer and the non-working layer raw materials in a weight ratio of 1:2. The ingredients are prepared and mixed according to the above proportions. For the working layer material, 98 plate-shaped corundum with a particle size of ≤0.045mm, SiAlON powder with a particle size of ≤0.045mm, andalusite with a particle size of ≤0.45mm, silicon nitride powder with a particle size of ≤0.020mm, and Suzhou white mud with a particle size of ≤0.010mm are vigorously mixed for 20 minutes in advance and recorded as A4 powder for later use. 98 plate-shaped corundum with a particle size of 4~2mm and 2~1mm, mesoporous alumina with a particle size of 1~0.5mm and 0.5~0.088mm, and silicon nitride powder with a particle size of 0.5~0.088mm are vigorously mixed and milled for 15 minutes, aluminum sol is added as a binder, and the premixed A4 powder is added, and wet-milled together for 30 minutes. Non-working layer material: Pre-mix andalusite with a particle size of ≤0.45mm, Suzhou white mud with a particle size of ≤0.010mm, and magnesium carbonate with a particle size of ≤0.010mm vigorously for 20 minutes, record it as B4 powder and set aside, vigorously mix and grind 3~2㎜ and 2~1㎜ alumina hollow balls, mesoporous alumina with a particle size of 1~0.5 mm, and mesoporous alumina with a particle size of 0.5~0.088 mm for 15 minutes, add aluminum sol as a binder, and then add the pre-mixed B4 powder, and wet-mill together for 30 minutes.Gradient transition layer 1: Mix 2 weights of A4 material and 1 weight of B4 material, and premix and mix and grind the fine powder in the same way as A4 and B4 materials. Gradient transition layer 2: Mix 1 weight of A4 material and 2 weights of B4 material, and premix and wet grind the fine powder in the same way as A4 and B4 materials. Use cardboard to divide the mold into four areas, and pour A4 material, transition layer 1 material, transition layer 2 material, and B4 material into the four areas in the order of working layer, gradient transition layer 1, gradient transition layer 2, and non-working layer. After spreading and flattening, pull out the cardboard, press or hydraulically form, dry the bricks at 120℃ for 72h, and sinter at 1500℃ for 3h. The performance parameters of the sintered refractory brick working layer are: volume density 2.84g·cm. -1 , room temperature compressive strength 88MPa, thermal conductivity 1.27W·m·K at 1100℃ -1 ; Non-working layer performance parameters: Volume density 1.22g·cm -1 , room temperature compressive strength 26MPa, thermal conductivity 0.58W·m·K at 500℃ -1 .
[0057] Table 1 Examples and performance list of corundum-SiAlON-silicon nitride gradient bricks for sulfur recovery reactors
[0058]
Claims
1. A corundum-SiAlON-silicon nitride gradient composite refractory brick for a sulfur recovery reactor, characterized in that: The overall gradient design is adopted, and the gradient distribution is as follows: 1 / 3L working layer A, 1 / 6L gradient transition layer 1, 1 / 6L gradient transition layer 2, 1 / 3L non-working layer B; The raw material formula characteristics of the corundum-SiAlON-silicon nitride gradient composite refractory brick for the sulfur recovery reactor are as follows: Said Working layer A: expressed in weight percentage, the raw materials are 8-11% of plate-shaped corundum with a particle size of 4-2mm, 12-22% of plate-shaped corundum with a particle size of 2-1mm, 9-13% of mesoporous alumina with a particle size of 1-0.5mm, 15-20% of mesoporous alumina with a particle size of 0.5-0.088mm, 5-8% of silicon nitride with a particle size of 0.5-0.088mm, 16-19% of plate-shaped corundum with a particle size ≤0.045mm, 5-10% of SiAlON with a particle size ≤0.045mm, 8-15% of silicon nitride powder with a particle size ≤0.020mm, 1-2% of Suzhou white mud with a particle size ≤0.010mm, and 2.5-3% of aluminum sol; The non-working layer B is characterized by: expressed in weight percentage, the raw materials are 9-12% of hollow alumina balls with a particle size of 3-2 mm, 20-38% of hollow alumina balls with a particle size of 2-1 mm, 9-21% of mesoporous alumina with a particle size of 1-0.5 mm, 15-19% of mesoporous alumina with a particle size of 0.5-0.088 mm, 12-15% of andalusite with a particle size of ≤0.045 mm, 8-13% of Suzhou white mud with a particle size of ≤0.010 mm, 3-6% of magnesium carbonate with a particle size of ≤0.010 mm, and 2.5-3% of aluminum sol. The gradient transition layer 1 is characterized by: a mixed ratio of 2 / 3A and 1 / 3B expressed in weight percentage; The second gradient transition layer is characterized by a mixed ratio of 1 / 3A and 2 / 3B expressed in weight percentage.
2. A method for preparing the corundum-SiAlON-silicon nitride gradient composite refractory brick for the sulfur recovery reactor according to claim 1, comprising weighing raw materials, wet grinding, molding, drying and high-temperature sintering, characterized in that: Weigh the required raw materials in proportion, and separately mix and grind the working layer material A, the non-working layer material B, the gradient transition layer material 1 2 / 3A+1 / 3B, and the gradient transition layer material 2 1 / 3A+2 / 3B; pour the working layer material A, the transition layer material 1, the transition layer material 2, and the non-working layer material B into the mold in sequence, and press or hydraulically form the bricks; dry the bricks at 120℃ for 48-72h; and sinter at 1450-1520℃ for 3-4h; The working layer A material: Premixing of fine powder: Premix 98 plate-shaped corundum with a particle size of ≤0.045mm, SiAlON powder with a particle size of ≤0.045mm, andalusite with a particle size of ≤0.45mm, silicon nitride powder with a particle size of ≤0.020mm, and Suzhou white mud with a particle size of ≤0.010mm vigorously for 20 minutes and set aside, which is recorded as A powder; Mixing and grinding: Mix and grind 98 plate-shaped corundum with particle size of 4-2mm and 2-1mm, mesoporous alumina with particle size of 1-0.5mm and 0.5-0.088mm, and silicon nitride powder with particle size of 0.5-0.088mm vigorously for 15-20 minutes, add aluminum sol as a binder, and then add pre-mixed A powder, and wet grind together for 30 minutes; The non-working layer B material: Premixing of fine powder: Premix andalusite with a particle size of ≤0.45mm, Suzhou white mud with a particle size of ≤0.010mm, and magnesium carbonate with a particle size of ≤0.010mm vigorously for 20 minutes and set aside, which is recorded as B powder; Mixing and grinding: Mix and grind 3-2mm and 2-1mm hollow alumina balls, mesoporous alumina with a particle size of 1-0.5mm, and mesoporous alumina with a particle size of 0.5-0.088mm for 15-20 minutes, add aluminum sol as a binder, and then add the premixed B powder, and wet grind together for 30 minutes; The gradient transition layer: The first material of the gradient transition layer 2 / 3A+1 / 3B is a mixture of 2 / 3 weight of material A and 1 / 3 weight of material B, and the premixing and co-grinding of fine powder are the same as those of material A and material B; similarly, the second material of the gradient transition layer 1 / 3A+2 / 3B is a mixture of 1 / 3 weight of material A and 2 / 3 weight of material B, and the premixing and wet-grinding of fine powder are the same as those of material A and material B.