A method for preparing a nitrogen-doped carbon framework material coated with an iron-cobalt-nickel ternary alloy

Through ball milling method and melamine pyrolysis technology, a nitrogen-doped carbon frame material coated with iron-cobalt-nickel ternary alloy was prepared, which solved the problems of high preparation cost, insufficient catalytic activity and limited specific surface area in the prior art, and achieved high efficiency electrocatalytic activity and low-cost new battery materials.

CN111921551BActive Publication Date: 2024-11-26NANCHANG UNIV

Patent Information

Application Number
CN202010722663.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-07-24
Publication Date
2024-11-26
Estimated Expiration
2040-07-24

AI Technical Summary

Technical Problem

The preparation of existing transition metal alloy-optimized nitrogen-doped carbon materials has problems such as high equipment dependence, high cost, insufficient catalytic activity and limited specific surface area, which is difficult to meet the needs of new battery materials.

Method used

The ellagic acid-iron-cobalt nickel complex was prepared by ball milling, and the co-pyrolysis of melamine was used to form a carbon nanosheet nanoframe grafted with nitrogen-doped carbon nanotubes, which was coated with iron-cobalt nickel ternary transition metal alloy Nanoparticles realize low cost, high specific surface area and dual-function electrocatalytic activity of materials.

Benefits of technology

It realizes the low cost, high specific surface area and dual-function electrocatalytic activity of the material. It is suitable for electrochemical energy storage and conversion devices such as zinc-air batteries and fuel cells, and improves the catalytic efficiency and application breadth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111921551B_ABST
    Figure CN111921551B_ABST
Patent Text Reader

Abstract

A method for preparing a nitrogen-doped carbon framework material coated with an iron-cobalt-nickel ternary alloy, wherein ellagic acid-iron-cobalt-nickel complex is obtained by ball milling, and then melamine is added for co-pyrolysis to obtain a carbon nanosheet nanoframe grafted with nitrogen-doped carbon nanotubes, wherein the framework is coated with iron-cobalt-nickel ternary transition metal alloy nanoparticles. The method is simple and easy to implement, low in cost, and the prepared material has a high specific surface area and oxygen reduction and oxygen evolution dual-functional electrocatalytic activity, and can be applied to electrochemical energy storage and conversion devices such as zinc-air batteries, fuel cells, and water electrolysis hydrogen production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of new materials and nanocatalysis, and specifically relates to a method for preparing a nitrogen-doped carbon framework material coated with an iron-cobalt-nickel ternary alloy. Background Art

[0002] Transition metal alloy optimized nitrogen-doped carbon materials can be widely used as oxygen reduction catalysts in metal-air batteries and fuel cells as new cathode materials, with the advantages of high catalytic performance and strong stability. However, there are still many difficulties in the preparation of transition metal alloy optimized nitrogen-doped carbon materials. First, supercritical reactions are often used to prepare this material, resulting in equipment dependence and increased costs. Second, the transition metal alloys in this material are mostly binary alloys, and the intrinsic catalytic activity of oxygen reduction needs to be improved. Third, the specific surface area of ​​this material is usually limited, resulting in the inability to fully utilize its high intrinsic catalytic activity in practical applications. Therefore, it is very important to develop a new technology for transition metal alloy optimized nitrogen-doped carbon materials with a simple preparation process and a high specific surface area. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a nitrogen-doped carbon framework material coated with an iron-cobalt-nickel ternary alloy. The method uses a ball milling method to obtain an ellagic acid-iron-cobalt-nickel complex, and then adds melamine for co-pyrolysis to obtain a nitrogen-doped carbon nanotube-grafted carbon nanosheet nanoframe, in which iron-cobalt-nickel ternary transition metal alloy nanoparticles are coated. The method is simple and easy to implement, low in cost, and the prepared material has a high specific surface area and oxygen reduction and oxygen evolution dual-functional electrocatalytic activity, and can be applied to electrochemical energy storage and conversion devices such as zinc-air batteries, fuel cells, and water electrolysis hydrogen production.

[0004] The present invention is achieved through the following technical solutions.

[0005] The method for preparing a nitrogen-doped carbon framework material coated with an iron-cobalt-nickel ternary alloy described in the present invention is characterized by comprising the following steps.

[0006] (1) Mix ellagic acid, cobalt acetate tetrahydrate, nickel acetate tetrahydrate, and ferric chloride hexahydrate in a weight ratio of 1:1:1:1:1 to 4:1:1:1.

[0007] (2) Using a planetary ball mill, the mixed system obtained in step (1) is ball milled to obtain a black solid, wherein the process parameters of the ball milling are: using a 100 mL zirconia ball mill with a 5 mm zirconia grinding ball, a ball-to-material ratio of 1:1 to 8:1, a motor speed of 100 to 300 rpm, and a ball milling time of 240 to 1440 min.

[0008] (3) The black solid obtained in step (2) is washed with deionized water and freeze-dried to obtain a ternary transition metal ellagic acid complex flaky powder EA-FeCoNi.

[0009] (4) Add melamine to the ternary transition metal ellagic acid complex powder obtained in step (3), and grind and mix them in a mortar; wherein the amount of melamine added is 1 to 3 times the weight of EA-FeCoNi.

[0010] (5) The mixed solid powder obtained in step (4) is placed in a porcelain boat, and the porcelain boat is placed in a high-temperature tube furnace, and a black solid powder is obtained by high-temperature pyrolysis; wherein the process parameters of the pyrolysis are: under the protection of nitrogen flow or argon flow, the temperature is increased to 700°C~900°C at a rate of 5°C / min, and the temperature is kept for 2 hours.

[0011] (6) The black solid powder obtained in step (5) is pickled to obtain a nitrogen-doped carbon framework material (FeCoNi-NC) coated with an iron-cobalt-nickel ternary alloy; the pickling process is as follows: the solid powder is placed in 0.5-1 mol / L sulfuric acid or hydrochloric acid, heated to 40-80 °C, stirred for 12-24 h, filtered, washed with deionized water for several times, and dried in an oven at 60 °C for 12 h.

[0012] The mass ratio of ellagic acid, cobalt acetate tetrahydrate, nickel acetate tetrahydrate and ferric chloride hexahydrate in step (1) is preferably 4:1:1:1.

[0013] The ball milling process in step (2) uses a 100 mL zirconia ball milling jar with 5 mm zirconia grinding balls, a ball-to-material ratio of 8:1, a motor speed of 255 rpm, and a ball milling time of 1440 min.

[0014] The amount of melamine added in step (4) is 3 times that of EA-FeCoNi.

[0015] The pyrolysis process in step (5) is preferably carried out under the protection of an argon gas flow with a flow rate of 40 sccm, with the temperature being increased to 775°C at a heating rate of 5°C / min, maintained for 120 min, and then cooled naturally.

[0016] The acid washing process in step (6) is to put the solid powder into 1 mol / L hydrochloric acid, heat it to 80°C, stir it for 24 hours, filter it, wash the obtained solid with deionized water several times, and dry it in an oven at 60°C for 12 hours.

[0017] The invention has the following benefits: the phenolic hydroxyl group of ellagic acid is mixed with Fe by ball milling. 3+ ,Co 2+ , Ni 2+The complex precursor is formed, and then melamine is added for uniform blending, followed by high-temperature pyrolysis. During the high-temperature pyrolysis process, the ellagic acid matrix is ​​carbonized to form carbon nanosheets, and the transition metal ions are thermally reduced to iron-cobalt-nickel ternary transition metal alloys; while melamine is decomposed into nitrogen-containing carbon-based fragments at high temperatures, which nucleate and grow in situ under the catalysis of transition metal nanoparticles, and transform into nitrogen-doped carbon nanotubes grafted on the carbon nanosheets, and finally generate a nitrogen-doped carbon framework material coated with an iron-cobalt-nickel ternary alloy. This material has the following advantages: first, the preparation method is simple and can be prepared in large quantities; second, it has a multi-level pore structure and a large specific surface area, which can effectively expose more active sites and improve the material transmission rate and charge transfer rate; third, the iron-cobalt-nickel alloy nanoparticles coated under the nitrogen-doped carbon layer can optimize the charge distribution on the surface of the material and reduce the reaction free energy required for oxygen electrocatalysis. Therefore, the material has a high oxygen reduction and oxygen evolution dual-functional catalytic activity, which can effectively improve the efficiency of electrochemical energy storage and conversion devices such as rechargeable zinc-air batteries, proton exchange membrane fuel cells, and water electrolysis hydrogen production systems. Compared with the prior art, the material prepared by the present invention has a low price, a simple process, excellent performance, and a wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a scanning electron microscope image of the ternary metal-ellagic acid complex synthesized in Example 1 of the present invention.

[0019] Figure 2 This is a scanning electron microscope image of the framework material FeCoNi-NC synthesized in Example 1 of the present invention.

[0020] Figure 3 This is a high-angle annular dark field image-scanning transmission electron microscope image of the framework material FeCoNi-NC synthesized in Example 1 of the present invention.

[0021] Figure 4 This is the X-ray energy spectrum analysis of the C element of the framework material FeCoNi-NC synthesized in Example 1 of the present invention under a scanning transmission electron microscope.

[0022] Figure 5 This is the X-ray energy spectrum analysis of the N element of the framework material FeCoNi-NC synthesized in Example 1 of the present invention under a scanning transmission electron microscope.

[0023] Figure 6 This is the X-ray energy spectrum analysis of the Fe element of the framework material FeCoNi-NC synthesized in Example 1 of the present invention under a scanning transmission electron microscope.

[0024] Figure 7 This is the X-ray energy spectrum analysis of the Co element of the framework material FeCoNi-NC synthesized in Example 1 of the present invention under a scanning transmission electron microscope.

[0025] Figure 8 This is the X-ray energy spectrum analysis of the Ni element of the framework material FeCoNi-NC synthesized in Example 1 of the present invention under a scanning transmission electron microscope. Fig. 9 It is the nitrogen adsorption-desorption curve and pore size distribution diagram of the framework material FeCoNi-NC synthesized in Example 1 of the present invention.

[0026] Fig.10 It is a diagram of oxygen reduction and oxygen precipitation polarization curves of the framework material FeCoNi-NC synthesized in Example 1 of the present invention.

[0027] Fig.11 The framework material FeCoNi-NC synthesized in Example 1 of the present invention is applied to the air electrode of a zinc-air battery, and the charge and discharge polarization curve of the battery. DETAILED DESCRIPTION

[0028] The present invention will be further illustrated by the following examples.

[0029] Example 1.

[0030] (1) Weigh 1.00 g of ellagic acid, 0.25 g of cobalt acetate tetrahydrate, 0.25 g of nickel acetate tetrahydrate, and 0.25 g of ferric chloride hexahydrate, and place them in a 100 mL zirconia ball mill. Add five 5 mm and one 10 mm zirconia grinding balls.

[0031] (2) In a planetary ball mill, the ball milling mixture obtained in (1) was ball milled to obtain a black solid; wherein the ball milling parameters were set as follows: motor speed of 255 rpm, ball milling time of 1440 min.

[0032] (3) The black solid obtained in step (2) is washed with deionized water and freeze-dried to obtain a black flaky powder.

[0033] (4) Melamine and the black flaky powder obtained in (3) were ground and mixed in a mortar at a weight ratio of 3:1 until they were uniform.

[0034] (5) The mixed powder obtained in step (4) is placed in a porcelain boat and placed in a tubular furnace to obtain a black powder by pyrolysis; wherein the process parameters of the pyrolysis are: argon gas flow rate of 40 sccm, heating rate of 5 °C / min, target temperature of 775 °C, target temperature holding time of 120 min, and natural cooling program.

[0035] (6) The black powder obtained in step (5) is pickled, washed with deionized water, and dried to obtain a final product of a nitrogen-doped carbon framework material (FeCoNi-NC) coated with an iron-cobalt-nickel ternary alloy; wherein the pickling process is: using 1 mol / L hydrochloric acid, the temperature is 80 °C, and the pickling time is 24 h.

[0036] Example 2.

[0037] (1) Weigh 1.00 g of ellagic acid, 0.50 g of cobalt acetate tetrahydrate, 0.50 g of nickel acetate tetrahydrate, and 0.50 g of ferric chloride hexahydrate, and place them in a 100 mL zirconia ball mill. Add five 5 mm zirconia grinding balls.

[0038] (2) In a planetary ball mill, the ball milling mixture obtained in (1) was ball milled to obtain a black solid; wherein the ball milling parameters were set as follows: motor speed of 300 rpm, ball milling time of 240 min.

[0039] (3) The black solid obtained in step (2) is washed with deionized water and freeze-dried to obtain a black flaky powder.

[0040] (4) Melamine and the black flaky powder obtained in (3) were ground and mixed in a mortar at a weight ratio of 1:1 until they were uniform.

[0041] (5) The mixed powder obtained in step (4) is placed in a porcelain boat and placed in a tubular furnace to obtain a black powder by pyrolysis; wherein the process parameters of the pyrolysis are: argon gas flow rate of 40 sccm, heating rate of 5 °C / min, target temperature of 800 °C, target temperature holding time of 120 min, and natural cooling program.

[0042] (6) The black powder obtained in step (5) is pickled, washed with deionized water, and dried to obtain a final product of a nitrogen-doped carbon framework material (FeCoNi-NC) coated with an iron-cobalt-nickel ternary alloy; wherein the pickling process is: using 1 mol / L sulfuric acid, the temperature is 80°C, and the pickling time is 12 h.

[0043] Example 3.

[0044] (1) Weigh 1.00 g of ellagic acid, 1.00 g of cobalt acetate tetrahydrate, 1.00 g of nickel acetate tetrahydrate, and 1.00 g of ferric chloride hexahydrate, and place them in a 100 mL zirconia ball mill. Add five 5 mm and two 10 mm zirconia grinding balls.

[0045] (2) In a planetary ball mill, the ball milling mixture obtained in (1) was ball milled to obtain a black solid; wherein the ball milling parameters were set as follows: motor speed of 100 rpm, ball milling time of 720 min.

[0046] (3) The black solid obtained in step (2) is washed with deionized water and freeze-dried to obtain a black flaky powder.

[0047] (4) Melamine and the black flaky powder obtained in (3) were ground and mixed in a mortar at a weight ratio of 2:1 until they were uniform.

[0048] (5) The mixed powder obtained in step (4) is placed in a porcelain boat and placed in a tube furnace to obtain a black powder by pyrolysis; wherein the process parameters of the pyrolysis are: argon gas flow rate of 40 sccm, heating rate of 5 °C / min, target temperature of 700 °C, target temperature holding time of 120 min, and natural cooling program.

[0049] (6) The black powder obtained in step (5) is pickled, washed with deionized water, and dried to obtain a final product of a nitrogen-doped carbon framework material (FeCoNi-NC) coated with an iron-cobalt-nickel ternary alloy; wherein the pickling process is: using 0.5 mol / L hydrochloric acid, the temperature is 25°C, and the pickling time is 24 h.

[0050] The ellagic acid-ternary transition metal complex precursor obtained in the preparation process of Example 1 was observed using a scanning electron microscope (SEM). It can be seen that the microscopic morphology of the precursor prepared by the ball milling method is nano-flower particles assembled by nano-sheets, such as Figure 1 The final product FeCoNi-NC obtained in Example 1 was characterized by transmission electron microscopy (TEM). The results showed that the precursor and melamine were mixed and pyrolyzed, and then acid-washed to obtain a carbon nanotube-grafted nanosheet framework structure, and metal nanoparticles were coated in the framework structure, such as Figure 2 To further analyze the chemical composition of FeCoNi-NC, the sample was subjected to energy dispersive spectroscopy (EDS) analysis under a scanning transmission electron microscope. The results showed that C and N elements were evenly distributed on the surface of the sample, while Fe, Co, and Ni elements were evenly distributed within the metal nanoparticles of the sample, proving that the material is a Fe-Co-Ni ternary nanoalloy coated with a nitrogen-doped carbon framework, as shown in Figure 2. Figure 3-Figure 8 In order to further characterize the pore structure of the sample, nitrogen adsorption-desorption analysis was performed on the sample. The results showed that the sample showed a type IV adsorption isotherm with an H4 type hysteresis loop. Combined with the pore size distribution curve, it was proved that the sample had a micro-mesoporous multi-level pore structure, as shown in Figure 2. Fig. 9The sample was evenly dropped onto a rotating disk electrode, and a linear voltammetry (LSV) scan was performed on the sample film in a 0.1 mol / L potassium hydroxide solution saturated with dissolved oxygen at a speed of 1600 rpm. The polarization curve obtained showed that the sample had two electrocatalytic activities: oxygen reduction and oxygen evolution. Fig.10 The sample was loaded on hydrophobic porous carbon paper as the air electrode of the zinc-air battery, and the battery was charged-discharged and cycled. The results showed that the zinc-air battery with FeCoNi-NC as the catalytic layer had stable charge-discharge cycle performance, such as Fig.11 shown.

Claims

1. A method for preparing a nitrogen-doped carbon framework material coated with an iron-cobalt-nickel ternary alloy, It is characterized in that The following steps are involved: (1) Mix ellagic acid, cobalt acetate tetrahydrate, nickel acetate tetrahydrate, and ferric chloride hexahydrate in a weight ratio of 1:1:1:1:1 to 4:1:1:1; (2) using a planetary ball mill to ball mill the mixed system obtained in step (1) to obtain a black solid, wherein the process parameters of the ball milling are: using a 100 mL zirconia ball milling jar with a 5 mm zirconia grinding ball, a ball-to-material ratio of 1:1 to 8:1, a motor speed of 100 to 300 rpm, and a ball milling time of 240 to 1440 min; (3) washing the black solid obtained in step (2) with deionized water and freeze-drying to obtain a ternary transition metal ellagic acid complex flaky powder EA-FeCoNi; (4) adding melamine to the ternary transition metal ellagic acid complex powder obtained in step (3), grinding and mixing in a mortar; wherein the amount of melamine added is 1 to 3 times the weight of EA-FeCoNi; (5) placing the mixed solid powder obtained in step (4) into a porcelain boat, and placing the porcelain boat in a high-temperature tube furnace, and subjecting the mixture to high-temperature pyrolysis to obtain a black solid powder; wherein the pyrolysis process parameters are: under the protection of nitrogen or argon flow, heating the mixture to 700°C to 800°C at a rate of 5°C / min, and keeping the temperature for 2 hours; (6) The black solid powder obtained in step (5) is stirred in sulfuric acid or hydrochloric acid for 12 to 24 h, the concentration of sulfuric acid or hydrochloric acid is 0.5 to 1 mol / L, and the temperature is controlled at 80 °C. The solid is then filtered and washed with deionized water several times, and dried in an oven at 60 °C for 12 h to finally obtain a nitrogen-doped carbon framework material FeCoNi-NC coated with an iron-cobalt-nickel ternary alloy.

2. A method for preparing a nitrogen-doped carbon framework material coated with an iron-cobalt-nickel ternary alloy according to claim 1, It is characterized in that The mass ratio of ellagic acid, cobalt acetate tetrahydrate, nickel acetate tetrahydrate and ferric chloride hexahydrate in step (1) is 4:1:1:

1.

3. The method for preparing a nitrogen-doped carbon framework material coated with an iron-cobalt-nickel ternary alloy according to claim 1, It is characterized in that The ball milling process in step (2) uses a 100 mL zirconia ball milling jar with 5 mm zirconia grinding balls, a ball-to-material ratio of 8:1, a motor speed of 255 rpm, and a ball milling time of 1440 min.

4. The method for preparing a nitrogen-doped carbon framework material coated with an iron-cobalt-nickel ternary alloy according to claim 1, It is characterized in that The amount of melamine added in step (4) is 3 times that of EA-FeCoNi.

5. The method for preparing a nitrogen-doped carbon framework material coated with an iron-cobalt-nickel ternary alloy according to claim 1, It is characterized in that The pyrolysis process in step (5) is preferably carried out under the protection of an argon gas flow with a flow rate of 40 sccm, with the temperature being increased to 775°C at a heating rate of 5°C / min, maintained for 120 min, and then cooled naturally.

Citation Information

Patent Citations

  • Method for preparing metal-carbon composite catalytic material and its application

    CN109718822A

  • Nitrogen-doped carbon nanotube-loaded nitrogen-doped carbon-coated iron-cobalt alloy bifunctional catalyst and preparation method and application thereof

    CN110783582A

  • Preparation method of heteroatom doped hollow carbon nanotube

    CN111056547A

  • Preparation method and application of nitrogen-doped carbon nanotube coated cobalt nanoparticle composite material

    CN111146458A

  • Air electrode catalyst for metal-air secondary battery

    JP2018067494A

Cited By

  • Preparation method of nitrogen-doped carbon nanosheet-cobalt-nickel-iron three-transition-metal composite material and application of nitrogen-doped carbon nanosheet-cobalt-nickel-iron three-transition-metal composite

    CN119663347A

  • Preparation method of nitrogen-doped carbon nanosheet@cobalt-nickel-iron transition metal composite material and its application in water electrolysis and hydrogen evolution

    CN119663347B